Terbium-containing paramagnetic garnet-type transparent ceramic, production method therefor, raw-material mixture therefor, and magneto-optical device obtained using same and production method therefor

The terbium-containing paramagnetic garnet-type transparent ceramic addresses thermal lensing and reproducibility issues in high-power laser applications by maintaining beam shape integrity and transparency at 160 W, utilizing a specific composition and sintering aid to enhance its performance in optical isolators.

WO2024237198A1PCT designated stage expired Publication Date: 2024-11-21SHIN ETSU CHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017408
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-05-10
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Current magneto-optical materials for high-power laser applications, such as optical isolators, face challenges with thermal lensing and manufacturing reproducibility, particularly when exposed to high incident powers, leading to beam distortion and reduced transparency.

Method used

A terbium-containing paramagnetic garnet-type transparent ceramic with a specific composition (Tb1-x-yYxScy)(Al1-zScz)O12, where 0.35≦x≦0.45, 0

Benefits of technology

The ceramic ensures a maximum change in incident laser beam diameter of 10% or less at 160 W, maintaining beam shape integrity and enhancing the material's suitability for high-power laser applications with improved manufacturing reproducibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017408_21112024_PF_FP_ABST
    Figure JP2024017408_21112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a terbium-containing paramagnetic garnet-type transparent ceramic which has a property that, when laser light having a wavelength of 1,064 nm and a beam diameter of 1.6 mm is caused to strike thereon at an incidence power elevated even to 160 W, the maximum change in the diameter of the incident laser beam can be kept below 10%; and others. The terbium-containing paramagnetic garnet-type transparent ceramic includes a sintered object of a composite oxide represented by formula (1) and has a total light transmittance of 84.8% or higher at a wavelength of at 600 nm. (1) (Tb1-x-yYxScy)3(Al1-zScz)5O12 (In the formula, 0.35≤x≤0.45, 0<y<0.03, 0.5<1-x-y<0.65, 0.001<z<0.03, and 0<y+z<0.06.) A magneto-optical element according to the present invention is an optical isolator which is equipped with the transparent ceramic as a Faraday rotator 110 and is also equipped with a polarizer 120 and an analyzer 130 respectively arranged on the front and back of the Faraday rotator on the optical axis 102 thereof, and which is utilizable in the wavelength band of 0.9-1.1 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Terbium-containing paramagnetic garnet-type transparent ceramics, their manufacturing method, raw material mixture therefor, and magneto-optical device using the same and its manufacturing method

[0001] The present invention relates to terbium-containing paramagnetic garnet-type transparent ceramics, a method for producing the same, a raw material mixture therefor, and a magneto-optical device using the same and a method for producing the same. More specifically, the present invention relates to terbium-containing paramagnetic garnet-type transparent ceramics suitable for constituting magneto-optical devices such as optical isolators, a method for producing the same, a raw material mixture therefor, and a magneto-optical device using the same and a method for producing the same.

[0002] In recent years, as it has become possible to achieve higher output, the use of laser processing machines using fiber lasers has become increasingly common. However, when external light enters the laser light source built into the laser processing machine, the resonance state becomes unstable, causing the oscillation state to be disrupted. In particular, when the oscillated light is reflected by the optical system along the way and returns to the light source, the oscillation state is significantly disrupted. To prevent this, an optical isolator is usually installed before the light source.

[0003] An optical isolator consists of a Faraday rotator, a polarizer placed on the light input side of the Faraday rotator, and an analyzer placed on the light output side of the Faraday rotator. The Faraday rotator is used by applying a magnetic field parallel to the light's direction of propagation. The polarization of the light rotates in only one direction, whether it is traveling forward or backward through the Faraday rotator. Furthermore, the Faraday rotator is adjusted to a length that rotates the polarization of the light exactly 45 degrees. If the polarization planes of the polarizer and analyzer are offset 45 degrees from the direction of rotation of the forward light, the polarization of the forward light will be aligned at the polarizer and analyzer positions, allowing it to pass through. On the other hand, the polarization of the backward light will be rotated 45 degrees in the opposite direction to the polarizer's polarization plane, which is offset 45 degrees from the analyzer position. In this case, the polarization plane of the returning light at the polarizer position will be offset by 45 degrees - (-45 degrees) = 90 degrees from the polarizer's polarization plane, preventing it from passing through the polarizer. In this way, it functions as an optical isolator that transmits and emits forward-moving light and blocks backward-moving returning light.

[0004] Among the materials used for the Faraday rotator that constitutes the optical isolator, TGG crystal (Tb 3 Ga 5 O 12 ) and TSAG crystal ((Tb (3-x) Sc x ) Sc 2 Al 3 O 12 ) is known (Japanese Patent Laid-Open No. 2011-213552 (Patent Document 1), Japanese Patent Laid-Open No. 2002-293693 (Patent Document 2)). TGG crystals are currently widely used in standard fiber laser devices. On the other hand, the Verdet constant of TSAG crystals is said to be about 1.3 times that of TGG crystals, making them suitable for use in fiber laser devices. However, because Sc is an extremely expensive raw material, their adoption has not progressed due to manufacturing costs.

[0005] In addition to the above, TAG crystal (Tb3Al5O 12 ) is also known. However, because TAG crystals are decomposed melting crystals, there is a restriction that the perovskite phase is generated first at the solid-liquid interface, followed by the TAG phase. In other words, the garnet and perovskite phases of TAG crystals can only be grown in a mixed state, and the growth of high-quality, large-sized TAG crystals has not yet been realized.

[0006] However, recently, WO 2018 / 193848 (Patent Document 3) discloses a paramagnetic garnet-type transparent ceramic, which is a sintered body of a complex oxide represented by the following formula, and which is characterized in that the linear transmittance at a wavelength of 1064 nm with an optical path length of 15 mm is 83% or more. 1-x-y Sc x Ce y ) 3 (Al 1-z Sc z ) 5 O 12 (wherein 0<x<0.08, 0≦y≦0.01, 0.004<z<0.16) was disclosed.

[0007] Furthermore, the composition is (Tb x Y1-x ) 3 Al 5 O 12 It was disclosed that a dense ceramic sintered body with x = 0.5 to 1.0 has a higher extinction ratio than existing TGG crystals (improving from the existing 35 dB to 39.5 dB or more) and can also reduce insertion loss (improving from the existing 0.05 dB to 0.01 to 0.05 dB) (Non-Patent Document 1).

[0008] Subsequently, Japanese Patent Laid-Open No. 2019-199386 (Patent Document 4) disclosed a sintered body of a composite oxide represented by the following formula, in which SiO 2 a paramagnetic garnet-type transparent ceramic containing more than 0 mass % and 0.1 mass % or less of (Tb 1-x-y Y x Sc y ) 3 (Al 1-z Sc z ) 5 O 12 (wherein 0.05≦x<0.45, 0<y<0.1, 0.5<1−x−y<0.95, 0.004<z<0.2) has been disclosed.

[0009] JP 2011-213552 A JP 2002-293693 A WO 2018 / 193848 JP 2019-199386 A

[0010] Yan Lin Aung, Akio Ikesue, “Development of optical grade (TbxY1-x)3Al5O12 ceramics as Faraday rotator material”, J. Am. Ceram. Soc. , (2017), 100(9), 4081-4087

[0011] In Patent Document 3, the Verdet constant is comparable to that of TAG, and the linear transmittance is improved to be 83% or more even with an optical path length of 15 mm, so it can be said that it has almost reached a practical level. However, although not specified in Patent Document 3, when the inventors of the present application actually adjusted laser light with a wavelength of 1064 nm to a beam diameter of 1.6 mm and incident it with an input power of 100 W onto a sample that reproduced the example in the patent document, it became clear that the maximum change in the diameter of the incident laser beam due to the occurrence of thermal lensing exceeded 15%.

[0012] Furthermore, the material disclosed in Non-Patent Document 1, by substituting some of the Tb ions with Y ions, enables even lower loss than the material disclosed in Patent Document 3, and is a material from which an extremely high-quality garnet-type Faraday rotator can be obtained. Specifically, when a 1064 nm laser beam was adjusted to a beam diameter of 1.6 mm and incident at an input power of 100 W onto a sample that reproduced the material described in Non-Patent Document 1, it was found that the maximum change in the incident laser beam diameter due to the occurrence of thermal lensing was less than 10%.

[0013] However, the material described in Non-Patent Document 1 has very low manufacturing reproducibility, and when the inventors of the present application actually adjusted laser light with a wavelength of 1064 nm to a beam diameter of 1.6 mm and applied it with an incident power of 100 W to a sample that reproduced the example described in the document, it became clear that there was a very high probability that the maximum change in the incident laser beam diameter due to the occurrence of thermal lensing would exceed 15%.

[0014] The material disclosed in Patent Document 4 is a material that can obtain a garnet-type Faraday rotator of the same high quality as that of Non-Patent Document 1 by substituting some of the Tb ions with Y ions, as in Non-Patent Document 1. In fact, when a 1064 nm laser beam was adjusted to a beam diameter of 1.6 mm and incident at an output of 100 W on a sample that reproduced the material described in the patent document, the maximum change in the incident laser beam diameter due to the occurrence of thermal lensing was less than 10%, as in Non-Patent Document 1. Furthermore, the material described in Patent Document 4 also had significantly improved manufacturing reproducibility.

[0015] Therefore, the incident power was further increased to 160 W, and the light was incident on samples that reproduced the material described in Patent Document 4. As a result, many of the samples exceeded the maximum change in incident laser beam diameter of 15% due to the occurrence of thermal lensing. In other words, it can be said that the complex oxide sintered body material for an incident power of 100 W has reached a practical level, but it cannot be said that the complex oxide sintered body material for an incident power of 160 W has yet reached a practical level.

[0016] The present invention has been made in view of the above circumstances, and aims to provide a terbium-containing paramagnetic garnet-type transparent ceramic, which is a sintered body of a paramagnetic garnet-type oxide containing at least yttrium, terbium, and aluminum as main components, with the volume molar concentration of terbium being equal to or higher than that of yttrium, and which is capable of keeping the maximum change in incident laser beam diameter to 10% or less even when a laser beam having a wavelength of 1064 nm and a beam diameter of 1.6 mm is incident at an input power of up to 160 W; a method for producing the same; a raw material mixture therefor; and a magneto-optical device using the same and a method for producing the same.

[0017] In order to achieve the above object, the present invention provides, as a first aspect, a terbium-containing paramagnetic garnet-type transparent ceramic comprising a sintered body of a composite oxide containing terbium, yttrium, scandium, and aluminum, represented by the following formula (1): (Tb 1-x-y Y x Sc y ) 3 (Al 1-z Sc z ) 5 O 12 (1) (wherein 0.35≦x≦0.45, 0<y<0.03, 0.5<1−x−y<0.65, 0.001<z<0.03, 0<y+z<0.06) The total light transmittance at a wavelength of 600 nm is 84.8% or more.

[0018] The terbium-containing paramagnetic garnet-type transparent ceramic of the present invention contains SiO as a sintering aid. 2 may further be contained in the range of more than 0 mass % and 0.1 mass % or less.

[0019] The terbium-containing paramagnetic garnet-type transparent ceramic of the present invention may have both optical end faces precision mirror-polished to a length of 14 mm or more, and the average roughness of each of the polished optical end faces is in the range of arithmetic mean height Sa≦0.70 nm or root mean square height Sq≦0.89 nm.

[0020] The total light transmittance of the paramagnetic garnet-type transparent ceramic of the present invention is preferably 84.6% or more at a wavelength of 540 nm and 85.25% or more at a wavelength of 1064 nm.

[0021] A second aspect of the present invention is a magneto-optical material comprising the above-mentioned terbium-containing paramagnetic garnet-type transparent ceramic.

[0022] A third aspect of the present invention is a magneto-optical device comprising the above-described magneto-optical material.

[0023] The magneto-optical device of the present invention may be an optical isolator that includes the above-mentioned terbium-containing paramagnetic garnet-type transparent ceramic as a Faraday rotator and has polarizing materials in front of and behind the optical axis of the Faraday rotator and is usable in the wavelength band of 0.9 μm or more and 1.1 μm or less.

[0024] In a fourth aspect, the present invention provides a method for producing a terbium-containing paramagnetic garnet-type transparent ceramic comprising a sintered body of a composite oxide containing terbium, yttrium, scandium, and aluminum, represented by the following formula (1): (Tb 1-x-y Y x Sc y ) 3 (Al 1-z Sc z ) 5 O 12(1) (wherein, 0.35≦x≦0.45, 0<y<0.03, 0.5<1−x−y<0.65, 0.001<z<0.03, 0<y+z<0.06) A method for producing a sintered body having a relative sintering density of 93.8% or more, 97.2% or more, comprising the steps of: mixing terbium oxide and yttrium oxide or a coprecipitated oxide of terbium and yttrium with aluminum oxide and scandium oxide to prepare a mixed raw material; calcining or heat-drying the mixed raw material with a thermal history of 950°C or less, and then shaping the mixed raw material to obtain a molded body; degreasing the molded body to obtain a degreased body; and sintering the degreased body under reduced pressure by first holding the degreased body at a hold temperature of 1000°C or less to degas the degreased body while maintaining a state in which the degreased body exhibits a brown color derived from the tetravalent terbium, and then heating the degreased body to a sintering temperature, so that the relative sintering density is 93.8% or more, 97.2% or more. The method includes the steps of obtaining a sintered body within the range below, further densifying the sintered body by hot isostatic pressing (HIP) until the relative sintered density is 99.9% or more, subjecting the densified sintered body to a decolorizing annealing treatment at a temperature lower than that of the HIP treatment to bleach the brown color of the densified sintered body derived from the tetravalent terbium, additionally sintering the bleached sintered body under reduced pressure at a temperature higher than both the sintering temperature and the temperature of the HIP treatment, and subjecting the additionally sintered sintered body to an oxidation annealing treatment in an oxygen atmosphere or in the air at a temperature lower than that of the HIP treatment.

[0025] In the mixed raw material, the weight ratio of the residue that does not pass through a mesh with 20 μm openings to the total weight of the mixed raw material is preferably 0.5% or less.

[0026] In a fifth aspect, the present invention provides a mixed raw material for producing a terbium-containing paramagnetic garnet-type transparent ceramic, comprising a sintered body of a composite oxide containing terbium, yttrium, scandium, and aluminum, represented by the following formula (1): (Tb 1-x-y Y x Sc y ) 3 (Al 1-z Sc z ) 5 O 12(1) (Wherein, 0.35≦x≦0.45, 0<y<0.03, 0.5<1−x−y<0.65, 0.001<z<0.03, 0<y+z<0.06) The mixed raw material is a mixture of terbium, yttrium, scandium, and aluminum oxides in an uncombined state, and the weight ratio of the residue that does not pass through a 20 μm mesh to the total weight of the mixed raw material is 0.5% or less.

[0027] A sixth aspect of the present invention is a method for manufacturing a magneto-optical device, in which the magneto-optical device is constructed using the paramagnetic garnet-type transparent ceramic obtained by the above-described method for manufacturing a paramagnetic garnet-type transparent ceramic.

[0028] The present invention provides a terbium-containing paramagnetic garnet-type transparent ceramic that is truly transparent and fully suitable for use in high-power laser applications, capable of suppressing the maximum change in incident laser beam diameter to 10% or less even when high-power laser light, such as a laser light with a wavelength of 1064 nm, a beam diameter of 1.6 mm, and an incident power of 160 W, is incident, and the shape of the incident beam is not distorted. Furthermore, by using the terbium-containing paramagnetic garnet-type transparent ceramic, it is possible to provide magneto-optical materials applicable to high-power laser devices, magneto-optical devices such as optical isolators, and methods for manufacturing magneto-optical devices.

[0029] FIG. 1 is a cross-sectional schematic diagram showing an example of the configuration of an optical isolator using the magneto-optical material according to the present invention as a Faraday rotator. FIG. 2 is a photograph showing the amount of gritty particles generated when a mixed raw material for the terbium-containing paramagnetic garnet-type transparent ceramic according to the present invention is calcined at 900°C. FIG. 3 is a photograph showing the amount of gritty particles generated when a mixed raw material for the terbium-containing paramagnetic garnet-type transparent ceramic according to the present invention is calcined at 950°C. FIG. 4 is a photograph showing the amount of gritty particles generated when a mixed raw material for the terbium-containing paramagnetic garnet-type transparent ceramic according to the present invention is calcined at 1000°C. FIG. 5 is a photograph showing the appearance of the sintered body after HIP treatment of Example 3. FIG. 6 is a photograph showing the appearance of the sintered body after decolorization annealing of Example 3. FIG. 7 is a graph showing the total light transmittance of the sintered bodies after oxidation annealing of Example 3, Comparative Example 6, and Comparative Example 7.

[0030] [1. Terbium-containing paramagnetic garnet-type transparent ceramics] First, one embodiment of the terbium-containing paramagnetic garnet-type transparent ceramics according to the present invention will be described. The terbium-containing paramagnetic garnet-type transparent ceramics of this embodiment includes a sintered body of a composite oxide containing terbium, yttrium, scandium, and aluminum, represented by the following formula (1): (Tb 1-x-y Y x Sc y ) 3 (Al 1-z Sc z ) 5 O 12 (1) (wherein, 0.35≦x≦0.45, 0<y<0.03, 0.5<1−x−y<0.65, 0.001<z<0.03, 0<y+z<0.06) The total light transmittance at a wavelength of 600 nm is 84.8% or more.

[0031] By having the composition of the composite oxide represented by the above formula (1), the beam does not collapse even when a laser beam having a wavelength of 1064 nm, a beam diameter of 1.6 mm, and an incident power of 160 W is incident.

[0032] The terbium-containing paramagnetic garnet-type transparent ceramic further contains SiO as a sintering aid. 2It is preferable that the content of SiO is more than 0 mass % and 0.1 mass % or less. 2 When the content is within this range, the transparency of the resulting paramagnetic garnet-type ceramic sintered body is improved to a practically usable level and is stable, which is preferable.

[0033] In this embodiment, it is essential that the hexacoordinated sites and tetracoordinated sites in the garnet structure are primarily composed of aluminum (Al). If these sites are primarily composed of aluminum, the bonding strength of the crystal is improved, and the average value of dn / dt at a wavelength of 1064 nm and at 30°C ± 10°C can be reduced. If the ratio of aluminum occupying the hexacoordinated sites and tetracoordinated sites is 1-z (0.001 < z < 0.03), the average value of dn / dt at a wavelength of 1064 nm and at 30°C ± 10°C can be reduced to 9.0 × 10 -6 K -1 It can be managed as follows:

[0034] In this embodiment, terbium (Tb) and yttrium (Y) are selected as the main components of the octacoordinated site, and the terbium concentration is set to the range of 1-x-y (0.5<1-x-y<0.65), and the yttrium concentration is set to x (0.35≦x≦0.45). By setting the terbium concentration within the above range, a Verdet constant of 30 rad / (T·m) or more at a wavelength of 1064 nm is ensured. Furthermore, by setting the terbium concentration and the yttrium concentration within the above range, the beam does not collapse even when laser light with a wavelength of 1064 nm, a beam diameter of 1.6 mm, and an incident power of 160 W is incident. Note that when these two main components simultaneously satisfy the above ranges, the two properties can be simultaneously satisfied.

[0035] In this embodiment, scandium (Sc) is added within the range of the above formula (1). In the above formula (1), the range of y is 0 < y < 0.03, preferably 0.001 < y < 0.008, and more preferably 0.002 < y < 0.004. When y is within this range, the perovskite-type heterophase can be reduced to a level that is not detectable by X-ray diffraction (XRD) analysis. Furthermore, excessive decreases in thermal conductivity due to the homogeneity of the sintered body and grain boundary scattering can be prevented. Furthermore, the range of z in the above formula (1) is 0.001 < z < 0.03, more preferably 0.002 < z < 0.004. When z is within this range, the perovskite-type heterophase can be reduced to a level that is not detectable by X-ray diffraction (XRD) analysis. Furthermore, excessive decreases in thermal conductivity due to the homogeneity of the sintered body and grain boundary scattering can be prevented. By adding scandium in such a range that y is greater than 0 and less than 0.03, and z is greater than 0.001 and less than 0.03, it becomes possible to stably produce a highly transparent sintered body.

[0036] The terbium-containing paramagnetic garnet-type transparent ceramic of this embodiment contains the component represented by formula (1) above as a main component. Here, "containing as a main component" means that the composite oxide represented by formula (1) above is contained in an amount of 90 mass% or more. The content of the composite oxide represented by formula (1) above is preferably 99 mass% or more, more preferably 99.9 mass% or more, even more preferably 99.99 mass% or more, and particularly preferably 99.999 mass% or more.

[0037] The terbium-containing paramagnetic garnet-type transparent ceramic of this embodiment is composed of the above-mentioned main component and a sintering aid as a secondary component, but may further contain other elements. Examples of other elements include rare earth elements such as lutetium (Lu) and cerium (Ce), and various impurities such as sodium (Na), calcium (Ca), magnesium (Mg), phosphorus (P), tungsten (W), and molybdenum (Mo). The content of the other elements is preferably 10 parts by mass or less, more preferably 0.1 parts by mass or less, and particularly preferably 0.001 parts by mass or less (substantially zero), based on 100 parts by mass of the total amount of Tb and Y.

[0038] The terbium-containing paramagnetic garnet-type transparent ceramic of this embodiment has a total light transmittance of 84.8% or more at a wavelength of 600 nm, which indicates that the oxygen vacancies in the sintered body are extremely small. It has been confirmed that if oxygen vacancies exist in the sintered body, absorption due to oxygen vacancies occurs near the wavelength of 600 nm, causing the total light transmittance to fall below 84.8%. In other words, a total light transmittance of 84.8% or more at a wavelength of 600 nm means that absorption due to oxygen vacancies is minimized, and therefore indicates a truly transparent and practical sintered body in which the shape of the incident beam is not distorted even when high-power laser light with a wavelength of 1064 nm, a beam diameter of 1.6 mm, and an incident power of 160 W is incident.

[0039] The terbium-containing paramagnetic garnet-type transparent ceramic of this embodiment preferably has a total light transmittance of 84.8% or more at a wavelength of 540 nm and 85.3% or more at a wavelength of 1064 nm. This indicates that the sintered body is truly transparent, free from minute bubbles of 1 μm or less that would slightly reduce the total light transmittance at a wavelength of 540 nm, and free from various defects such as residual strain that would reduce the total light transmittance at a wavelength of 1064 nm.

[0040] The terbium-containing paramagnetic garnet-type transparent ceramic of this embodiment is processed to a length of 14 mm or more and used as the target magneto-optical material. A length of 14 mm or more is preferable because, although it depends on the configuration and size of the external magnet, by properly designing the magnetic circuit, it is possible to rotate incident light in the wavelength range of 0.9 μm to 1.1 μm by 45 degrees.

[0041] The optical end faces of the terbium-containing paramagnetic garnet-type transparent ceramic of this embodiment are preferably optically polished so that their average roughness falls within the range of arithmetic mean height Sa≦0.70 nm or root mean square height Sq≦0.89 nm. When the average roughness of the optical end faces is within the above range, the laser damage threshold is 10 J / cm even when a high-power laser is incident. 2 At the same time, it is also preferable because unintended scattering loss on the optical surface can be suppressed to an extremely small level.

[0042] [2. Manufacturing Method of Terbium-Containing Paramagnetic Garnet-Type Transparent Ceramics] Next, one embodiment of the manufacturing method of the terbium-containing paramagnetic garnet-type transparent ceramics according to the present invention will be described. The manufacturing method of this embodiment includes the steps of mixing oxides of terbium, yttrium, aluminum, and scandium to prepare a mixed raw material, calcining or heating and drying the mixed raw material under a predetermined thermal history and then molding it to obtain a green body, degreasing the green body to obtain a degreasing body, sintering the degreasing body under reduced pressure by first maintaining it at a predetermined temperature to degas the degreasing body while maintaining a state in which the degreasing body exhibits a brown color derived from the tetravalent terbium, and then raising the temperature to the sintering temperature to sinter the degreasing body to obtain a sintered body having a predetermined relative sintered density, densifying the sintered body by hot isostatic pressing (HIP), subjecting the densified sintered body to decolorization annealing to decolorize the brown color derived from the tetravalent terbium, additionally sintering the decolorized sintered body, and subjecting the additionally sintered sintered body to oxidation annealing. Each step will be described below.

[0043] [2-1. Mixed Raw Material Preparation Step] As the raw materials used in the manufacturing method of this embodiment, for example, oxide powders of terbium, yttrium, scandium, and aluminum can be used. In this case, the raw material purity is preferably 99.9% by mass or more, and particularly preferably 99.99% by mass or more. Co-precipitated oxides of terbium and yttrium can also be used. Then, predetermined amounts of each raw material are weighed and mixed so as to obtain the composite oxide composition represented by the above formula (1), thereby obtaining a mixed raw material. In this specification, the term "mixed raw material" refers to a mixture in which the oxides of terbium, yttrium, scandium, and aluminum are mixed in an uncombined state.

[0044] This mixed raw material contains silicon oxide (SiO 2 The mixed raw materials may be mixed using a wet ball mill, a bead mill, or a jet mill, as appropriate.

[0045] Of the above raw materials, terbium oxide and yttrium oxide, or the coprecipitated oxide of terbium and yttrium, are preferably pre-calcined at 1000° C. or higher. By pre-calcining at 1000° C. or higher, the BET value of each raw material is 35m 2 This is preferable because the weight loss can be suppressed to 1 / g or less, preventing ultrafine powder from flying around during handling. In addition, it is possible to remove the moisture adsorbed in the raw material powder, so the accuracy of weighing the raw material after calcination treatment is improved.

[0046] The mixed raw material (when the terbium and yttrium oxides are previously calcined, the mixed raw material is mixed with aluminum oxide and scandium oxide) is preferably subjected to a calcination treatment or a heat-drying treatment. The thermal history of the mixed raw material that has been calcined or heat-drying treated is preferably kept at 950°C or less, more preferably at 920°C or less, and even more preferably at 900°C or less. When the thermal history of the mixed raw material is controlled within the above range, it is possible to reduce the possibility that the rare earth oxide component and aluminum oxide will react and combine to form a monoclinic phase and / or a perovskite phase and / or a garnet phase, and it is also possible to prevent the highly active aluminum oxide fine powder from undergoing a necking reaction and agglomerating to form agglomerates.

[0047] In fact, when the thermal history of the mixed raw material is controlled within the above range, it is possible to suppress the amount of residues (hereinafter simply referred to as "grit") that do not pass through a 20 μm mesh, among the gritty, clumps, aggregates, and coarse powder derived from reaction compounds and necking aggregates, to 0.5% or less in terms of weight ratio to the total weight of the mixed raw material. The lower limit of the thermal history in the calcination treatment or heat drying treatment of the mixed raw material is not particularly limited, but may be, for example, 800° C. or higher.

[0048] Furthermore, when the mixed raw materials are managed as described above, the amount of quasi-lump components that barely pass through a 20 μm mesh is small, and the entire mixed raw material is maintained in a fine, smooth powder state. Therefore, the granules granulated by spray drying or the like are soft, easily crushed, and smooth and highly fluid, resulting in good packing and crushing properties during the molding process. Good packing and crushing properties during the molding process make it difficult for unintended voids to form inside the molded body, and the overall molding density is also likely to be increased. Furthermore, when such a molded body is put into the sintering process, it is possible to obtain a highly transparent sintered body with very few residual bubbles.

[0049] Furthermore, when the mixed raw materials are managed in the above-mentioned state, the reactivity of the mixed raw materials is maintained at a high level, which promotes densification during the sintering process and enables uniform sintering throughout the sintered body. This makes it possible to obtain a high-quality, heterophase-free sintered body that is highly transparent and has little compositional irregularity.

[0050] Various organic additives may be added to the mixed raw material for the purpose of improving the quality stability and yield in subsequent processes. In this embodiment, these are not particularly limited, and various dispersants, binders, lubricants, plasticizers, etc. can be suitably used. However, it is preferable to select high-purity organic additives that do not contain unnecessary metal ions. Furthermore, the order of addition of each organic additive must be appropriately designed so as not to interfere with the control of the properties (particle size distribution, etc.) of the mixed raw material to be produced.

[0051] [2-2. Molding Process] In the manufacturing method of this embodiment, a typical press molding process can be suitably used. That is, a very common uniaxial pressing process in which a mold is filled and pressurized from a certain direction, a cold isostatic pressing (CIP) process in which a molded body is sealed and placed in a deformable, waterproof container and pressurized with isostatic pressure, or a warm isostatic pressing (WIP) process can be suitably used. The applied pressure can be adjusted appropriately while checking the relative density of the resulting molded body, and is not particularly limited. For example, controlling the pressure within a pressure range of approximately 300 MPa or less, which can be handled by commercially available CIP or WIP equipment, can reduce manufacturing costs. Alternatively, a hot pressing process, a spark plasma sintering process, a microwave heating process, or the like can be suitably used, which not only performs the molding process but also sintering at once during molding. Furthermore, molded bodies can also be produced by a slip casting method instead of a press molding method. Other molding methods, such as pressure casting, centrifugal casting, and extrusion, can also be employed by optimizing the shape and size of the raw material oxide powder and the combination of various organic additives. To produce the high-quality terbium-containing paramagnetic garnet-type transparent ceramics of the present invention, it is preferable to apply as little pressure as possible during uniaxial press molding without causing the compact to collapse.

[0052] [2-3. Debinding Process] In the manufacturing method of this embodiment, a conventional debinding process can be suitably used. That is, it is possible to perform temperature-raised debinding using a heating furnace. The type of atmospheric gas used is not particularly limited, and air, oxygen, hydrogen, etc. can be suitably used. The debinding temperature is preferably a temperature above which the organic components of the added organic additives can be sufficiently decomposed and removed, and is preferably kept below 900°C. Controlling the debinding temperature within this range is preferable because it prevents unintended thermal shrinkage (a situation in which densification progresses while retaining adsorbed gases) caused by heating the debound body in an atmosphere other than a reduced-pressure environment. It is more preferable to keep the debinding temperature below 800°C. The lower limit of the debinding temperature is not particularly limited, but may be, for example, 300°C or higher.

[0053] [2-4. Sintering Step] In the manufacturing method of this embodiment, the sintering step is a step in which the degreased body obtained in the degreasing step is sintered under reduced pressure, and the temperature is temporarily held in a temperature range of 1000°C or less during the temperature rise to degas the degreased body in a state in which the brown color derived from the tetravalent terbium oxide remains, and then the temperature is raised to the sintering temperature to obtain a sintered body with a relative sintered density of 93.8% or more, and 97.2% or less.

[0054] The reason for temporarily holding the temperature at 1000°C or below is to thoroughly discharge adsorbed components such as water vapor and nitrogen from the system before full-scale densification begins. This holding (hereinafter also referred to as "holding") allows for efficient discharge of oxygen gas components, which are released in large quantities when the terbium oxide component's Tb(IV) is converted to trivalent by heating. However, it was found that at the same time, oxygen bound to the yttrium oxide is also released, gradually causing oxygen deficiency. Furthermore, it was also found that if the Tb(IV) is completely converted to trivalent, the degree of oxygen deficiency in the yttrium oxide becomes serious, and the amount of oxygen deficiency in the entire sintered body increases to the extent that the appearance becomes black after the HIP process in the subsequent process.

[0055] Therefore, if the hold temperature for changing Tb(IV) to Tb(III) is controlled to 1000°C or less while desorbing the adsorbed components, a small amount of Tb(IV) will remain, causing the sintered body to have a light brown color, but instead the amount of oxygen deficiency in the yttrium oxide can be suppressed to an extremely small level. As a result, the appearance of the sintered body after the HIP treatment in the subsequent process can be finished as a light brown (close to orange) sintered body with no black tinge, i.e., with very little oxygen deficiency.

[0056] On the other hand, if the hold temperature is set to a temperature exceeding 1000°C, the light brown color will completely disappear, but a large amount of oxygen deficiency will occur, causing the sintered body to appear black after the subsequent HIP treatment. The lower limit of the hold temperature is not particularly limited as long as it is a temperature that can change Tb tetravalent to Tb trivalent, but for example, 850°C or higher is preferable, and 900°C or higher is more preferable. Note that the hold time during which the degassing is performed by holding at a hold temperature of 1000°C or lower is sufficient for several hours, but it is preferable to set it to 8 hours or more in order to sufficiently degas from the inside of the degreased body. The upper limit of the hold time is not particularly limited, but may be, for example, 30 hours or less.

[0057] In the sintering process, the body is held at the hold temperature to degas, and then heated to a predetermined sintering temperature. It is essential that the predetermined sintering temperature be set within a temperature range where the oxides of terbium, yttrium, and scandium combine with aluminum oxide to stably produce only the garnet phase. After the degassing process is fully completed, it is preferable to heat the transparent ceramic sintered body as quickly as possible to a temperature range where only the garnet phase is produced, since this minimizes the rate of unintended production of heterogeneous phases such as monoclinic phases and perovskite phases.

[0058] For example, this predetermined sintering temperature is preferably 1400 to 1780°C, and particularly preferably 1450 to 1700°C. If the sintering temperature is within this range, as described above, densification is promoted while suppressing heterophase precipitation, which is preferable. Furthermore, the temperature rise rate from the hold temperature to the sintering temperature is preferably 100°C / hr or more, more preferably 200°C / hr or more, and even more preferably a high-speed temperature rise of 250°C / hr or more. The upper limit of the temperature rise rate is not particularly limited, but may be, for example, 300°C / hr or less.

[0059] In the sintering process, the relative sintered density of the resulting sintered body is controlled to be in the range of 93.8% or more and 97.2% or less. Control of the relative sintered density can be performed by conducting several preliminary experiments. Sintering is more preferably performed while controlling the relative sintered density to be in the range of 93.8% or more and 96.5% or less, and even more preferably while controlling the relative sintered density to be in the range of 93.8% or more and 96.0% or less. If the resulting sintered body is controlled within this density range, the residual bubbles inside the sintered body can be converted into closed pores, while the sintered grain size can be controlled without being excessively large, which is preferable because the closed pores can be firmly crushed in the subsequent HIP treatment.

[0060] The sintering process can be suitably carried out by general heating sintering methods such as resistance heating and induction heating. The atmosphere during this process is a reduced pressure environment (vacuum). By carrying out the sintering process in a reduced pressure atmosphere, components such as water vapor and nitrogen adsorbed inside the degreased body can be efficiently volatilized and discharged, and oxygen gas, which is desorbed in large quantities when Tb(IV) is converted to Tb(III) by heating, can also be efficiently discharged and volatilized outside the sintered body. The vacuum level is 1×10 -3 If the degree of vacuum is controlled within this range, the sintered body can be uniformly and sufficiently discharged from the degreased body to the center thereof, which is preferable.

[0061] [2-5. Hot Isostatic Pressing (HIP) Treatment Step] In the manufacturing method of this embodiment, after the sintering step, a hot isostatic pressing (HIP) treatment is performed to densify the sintered body until the relative sintered density is 99.9% or more. If the relative sintered density in the sintering step is properly managed, that is, if the HIP treatment can be performed without the sintered grain size becoming excessively large, the HIP stress is transmitted widely and uniformly from the outer periphery to the center of the sintered body, the closed pores are crushed, and the sintered body is firmly densified. In other words, a substantially ideal sintered body can be obtained that has no stress unevenness, no unintended void unevenness, and few remaining small bubbles.

[0062] In the manufacturing method of this embodiment, the conditions are controlled so that the sintered body intentionally exhibits a light brown appearance due to residual Tb tetravalent after HIP treatment. This suppresses the generation of oxygen vacancies in the easily reduced yttrium oxide, making it possible to produce a terbium-containing paramagnetic garnet-type transparent ceramic sintered body with a total light transmittance of 84.8% or more at a wavelength of 600 nm. It has been confirmed that the presence of oxygen vacancies in yttrium oxide causes absorption due to oxygen vacancies near the wavelength of 600 nm, resulting in a total light transmittance below 84.8%. Conversely, a total light transmittance of 84.8% or more at a wavelength of 600 nm means that absorption due to oxygen vacancies is minimized, and thus a truly transparent and practical sintered body can be provided, in which the shape of the incident beam is not distorted even when high-power laser light with a wavelength of 1064 nm, a beam diameter of 1.6 mm, and an incident power of 160 W is incident.

[0063] The type of pressurized gas medium used in HIP treatment is an inert gas such as argon or nitrogen, or Ar—O 2 can be suitably used. The pressure applied by the pressurized gas medium is preferably 50 to 300 MPa, more preferably 100 to 300 MPa. If the pressure is less than 50 MPa, the transparency improvement effect may not be obtained, and if the pressure exceeds 300 MPa, further improvement in transparency cannot be obtained even if the pressure is increased, and the load on the device becomes excessive, which may damage the device. For convenience, it is preferable that the applied pressure be 196 MPa or less, which can be processed with a commercially available HIP device.

[0064] The treatment temperature for the HIP treatment is preferably 1100 to 1780°C, more preferably 1200 to 1730°C. Treatment temperatures above 1780°C are not preferred because they increase the risk of oxygen vacancies. Treatment temperatures below 1100°C do not provide much of an effect of improving the transparency of the sintered body. There are no particular restrictions on the holding time at the treatment temperature, but holding for too long a time is not preferred because it increases the risk of oxygen vacancies. Typically, the holding time is preferably set in the range of 1 to 3 hours.

[0065] The heater material, heat insulating material, and treatment vessel for HIP treatment are not particularly limited, but graphite, molybdenum (Mo), tungsten (W), and platinum (Pt) can be suitably used, and yttrium oxide and gadolinium oxide can also be suitably used for the treatment vessel. In particular, when the treatment temperature is 1500°C or less, platinum can be used for the heater material, heat insulating material, and treatment vessel, and Ar—O can be used as the pressurized gas medium. 2 When the treatment temperature exceeds 1500°C, graphite is preferred as the heater material and heat insulating material, but in this case, it is preferred to select any one of graphite, molybdenum, and tungsten as the treatment container, and further select any one of yttrium oxide and gadolinium oxide as a double container inside the treatment container, and fill the container with an oxygen release material, since this can minimize the amount of oxygen vacancies that occur during the HIP treatment.

[0066] [2-6. Decolorization Annealing Treatment Step] In the manufacturing method of this embodiment, the sintered body after the HIP treatment has a light brown appearance. Therefore, in order to decolorize it and make it approximately white, a decolorization annealing treatment is performed in an oxygen atmosphere or in the air at a temperature equal to or lower than the treatment temperature of the HIP treatment, typically 1200 to 1400°C. This is because if the additional sintering treatment described below is performed without this step, a large number of bubbles will remain in the sintered body. The sintered body that has been subjected to the decolorization annealing treatment can discharge excess oxygen derived from terbium tetravalent to the outside of the system while at the same time minimizing oxygen deficiency derived from yttrium oxide, making it possible to obtain a garnet-type oxide sintered body with extremely low defect absorption.

[0067] The time for which the color removal annealing treatment is held at the above temperature does not need to be very long, and typically, holding for 2 hours is sufficient.

[0068] [2-7. Additional Sintering Process] In the manufacturing method of this embodiment, after the decolorization annealing process, additional sintering is performed under reduced pressure at a temperature that exceeds the sintering temperature and also exceeds the HIP processing temperature. However, if the additional sintering temperature exceeds 1780°C, the risk of oxygen deficiency increases, which is not preferable. This makes it possible to more thoroughly eliminate any remaining internal strains or bubbles. The degree of vacuum in the additional sintering process can be the same as in the sintering process.

[0069] A processing time of 8 hours or more for the additional sintering is preferable because it can recover even residual strain and defects inside the sintered body. A processing time of 10 hours or more is even more preferable. A sufficiently long processing time for the additional sintering is preferable because it can eliminate residual strain and residual bubbles sufficiently and uniformly from the periphery to the center of the sintered body. The additional sintering process is essential, especially when using garnet-type transparent oxide ceramic materials in an environment where a high-power laser of 160 W or more is incident.

[0070] [2-8. Oxidation Annealing Treatment Step] In the manufacturing method of this embodiment, after the additional sintering treatment is completed, it is preferable to perform an oxidation annealing treatment (oxygen deficiency recovery treatment) in an oxygen atmosphere or in the air at a temperature equal to or lower than the HIP treatment temperature, typically 1000 to 1500°C, in order to recover oxygen deficiencies in the obtained transparent ceramic sintered body. The oxidation annealing temperature is more preferably 1300°C or higher and 1450°C or lower. This makes it possible to recover oxygen deficiencies even in sintered bodies in which oxygen deficiencies have accumulated due to sintering, HIP treatment, additional sintering, etc., and to finish the body into a colorless, transparent, terbium-containing paramagnetic garnet-type transparent ceramic that is free of defect absorption.

[0071] The treatment time of the oxidation annealing treatment is preferably 8 hours or more, more preferably 20 hours or more, and even more preferably 30 hours or more. If the treatment time of the oxidation annealing treatment is sufficiently long, it becomes possible to sufficiently recover oxygen vacancies remaining particularly in the central part of the sintered body.

[0072] [2-9. Optical Polishing Step] In the manufacturing method of this embodiment, it is preferable to optically polish both end faces of the terbium-containing paramagnetic garnet-type transparent ceramic that has undergone the above series of steps, which are located on the optically utilized axis. The optical surface precision at this time is preferably λ / 2 or less, and particularly preferably λ / 8 or less, when the measurement wavelength λ is 633 nm. Furthermore, the average roughness of both optical end faces is preferably an arithmetic mean height Sa of 0.70 nm or less and a root-mean-square height Sq of 0.89 nm or less, and more preferably Sa≦0.55 nm and Sq≦0.70 nm, respectively. It is also possible to further reduce optical loss by appropriately forming an anti-reflection film (AR coating film) on the optically polished surface as described above.

[0073] As described above, a terbium-containing paramagnetic garnet-type transparent ceramic can be produced, which includes a sintered body of a composite oxide containing terbium, yttrium, scandium, and aluminum, as represented by the above formula (1), and has a total light transmittance of 84.8% or more at a wavelength of 600 nm. Furthermore, by producing the ceramic under the above-described manufacturing conditions, it is possible to achieve a high total light transmittance of 84.8% or more at a wavelength of 540 nm and 85.3% or more at a wavelength of 1064 nm. This suggests that a truly transparent sintered body is produced, free of minute bubbles of 1 μm or less that would slightly reduce the total light transmittance at a wavelength of 540 nm, and free of various defects such as residual strain that would reduce the total light transmittance at a wavelength of 1064 nm. Furthermore, by controlling the total light transmittance within the above range, a truly transparent sintered body can be provided, in which the shape of the incident beam does not become distorted even when high-power laser light with a wavelength of 1064 nm, a beam diameter of 1.6 mm, and an incident power of 160 W is incident thereon.

[0074] [3. Magneto-optical Material, Magneto-optical Device, and Manufacturing Method Thereof] Further, one embodiment of the magneto-optical material, magneto-optical device, and manufacturing method thereof according to the present invention will be described. The magneto-optical material of this embodiment includes the above-mentioned terbium-containing paramagnetic garnet-type transparent ceramic. Furthermore, the magneto-optical device of this embodiment is constructed using the above-mentioned terbium-containing paramagnetic garnet-type transparent ceramic. Specifically, it is preferable to construct and use a magneto-optical device by applying a magnetic field parallel to the optical axis of the above-mentioned terbium-containing paramagnetic garnet-type transparent ceramic, and then setting a polarizer and an analyzer so that their optical axes are offset by 45 degrees from each other. In particular, the above-mentioned terbium-containing paramagnetic garnet-type transparent ceramic is suitable for use as a Faraday rotator in an optical isolator for a wavelength of 0.9 to 1.1 μm as a magneto-optical device.

[0075] FIG. 1 is a cross-sectional view schematically illustrating an example of an optical isolator, which is a magneto-optical device including a Faraday rotator made of the paramagnetic garnet-type transparent ceramic according to the present embodiment as an optical element. As shown in FIG. 1 , the optical isolator 100 includes, within its housing 102, a Faraday rotator 110 made of the above-described paramagnetic garnet-type transparent ceramic, a polarizer 120 made of a polarizing material, and an analyzer 130. These components are arranged in this order along the optical axis 104 of the Faraday rotator: the polarizer 120, the Faraday rotator 110, and the analyzer 130. The polarization plane of the polarizer 120 and the polarization plane of the analyzer 130 are arranged so that the relative angle is 45°. The optical isolator 100 also includes, within the housing 102, a magnet 140 for applying a magnetic field to the Faraday rotator 110, attached to at least one of the side surfaces of the Faraday rotator 110.

[0076] Such an optical isolator 100 can be suitably used in an industrial fiber laser device (not shown). The optical isolator can prevent the laser light emitted from the laser light source from being reflected back to the light source, causing oscillation instability.

[0077] EXAMPLES The present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0078] [Examples 1 and 2, Comparative Examples 1 to 8] Terbium oxide powder, yttrium oxide powder, and scandium oxide powder manufactured by Shin-Etsu Chemical Co., Ltd., and aluminum oxide powder manufactured by Taimei Chemical Co., Ltd. were obtained. In addition, tetraethyl orthosilicate (TEOS) liquid manufactured by Kishida Chemical Co., Ltd. The purity of the powder raw materials was 99.95% by mass or more, and the purity of the liquid raw materials was 99.999% by mass or more.

[0079] Using the above raw materials, the mixing ratio was adjusted to prepare composite oxide raw materials with two types of final compositions shown in Table 1. The mixing ratio was adjusted by weighing and mixing each oxide powder so that the mole numbers of terbium, yttrium, aluminum, and scandium were in the molar ratios of each composition in Table 1. Next, TEOS was added, and the amount of SiO 2 The raw materials were weighed out so as to be converted into the mass % shown in Table 1 and added to each raw material.

[0080]

[0081] The individual components were then dispersed and mixed in ethanol using an alumina ball mill, taking care to prevent mixing of each other, for 15 hours.

[0082] The mixed raw materials were then spray-dried to dryness, and each mixed raw material was calcined at varying calcination temperatures as shown in Table 2. Again, each sample was dispersed and mixed in ethanol using an alumina ball mill, taking care to prevent contamination. The processing time was 20 hours. After 20 hours of mixing, each raw material slurry was filtered through a 20 μm mesh, and the weight of the residue (grit) remaining on the mesh was measured and recorded as a percentage of the total weight of the mixed raw materials. These results are summarized in Table 2.

[0083]

[0084] Photographs showing the amount of gritty material remaining after Samples 1, 2, and 3 were calcined, mixed and ground in ethanol for 20 hours, and then passed through a mesh with 20 μm openings are shown in Figures 2A to 2C.

[0085] As shown in Figure 2C, calcining the mixed raw material at 1000 °C produces a large amount of coarse granules that cannot pass through a 20 μm mesh. Furthermore, there is a significant amount of coarse powder that can barely pass through a 20 μm mesh. As a result, the resulting raw material has large size variations, is very hard, and is extremely difficult to handle. Naturally, even after granulation, the mixed raw material has poor granular hardness and large crushability variations. Furthermore, when a compact is produced using such heterogeneous raw materials, uneven stress transmission occurs within the compact, and the generation of unintended coarse voids cannot be prevented. Furthermore, when such a heterogeneous compact is sintered, uneven stress and void-induced final composition variations and localized internal defects inevitably remain within the sintered body. On the other hand, as shown in Figure 2B, when the mixed raw material was calcined at 950°C, the amount of granular material was significantly reduced, and as shown in Figure 2A, when the mixed raw material was calcined at 900°C, almost no granular material was observed.

[0086] The six samples (oxide raw materials) were then subjected to uniaxial press molding and CIP molding to obtain nine CIP compacts for each sample. All of the compacts were degreased in a muffle furnace at 800°C for three hours to obtain degreased compacts.

[0087] Next, the degreased compacts of Samples 1, 2, and 4, 5 were divided into three groups of three each. Six of the compacts from Samples 1 to 6 were vacuum sintered at a temperature of 1000°C for 12 hours, and three were vacuum sintered at 1080°C for 12 hours, as shown in Table 3. The six samples that were vacuum sintered at 1000°C for 12 hours were vacuum sintered at different sintering temperatures, as shown in Table 3, to achieve different post-sintered densities. Samples 3 and 6 were vacuum sintered at a temperature of 1000°C for 12 hours, with the relative sintered density ranging from 93.8% to 97.2%.

[0088]

[0089] The resulting sintered bodies were placed in a carbon heater HIP furnace and subjected to HIP treatment in Ar at 200 MPa, 1600°C, and 3 hours. All of the resulting sintered bodies had a relative density of 99.9% or higher. The sintered bodies obtained at a holding temperature of 1000°C were light brown (coloration due to Tb tetravalent), while the sintered bodies obtained at a holding temperature of 1080°C were completely black (massive oxygen deficiency absorption).

[0090] Therefore, all of the samples of Examples 1 to 4 and Comparative Examples 2, 4, 5, 7, 9, and 10, which had a light brown appearance, were subjected to decolorization annealing treatment in an atmospheric heating furnace at 1300°C for 2 hours. The resulting annealed products were all transparent or translucent, i.e., decolorized.

[0091] Fig. 3A is a photograph showing the appearance of the sintered body of Example 3 after HIP treatment, which was light brown in color. Fig. 3B is a photograph showing the appearance of the sintered body of Example 3 after further decolorizing annealing at 1300°C for 2 hours, which was transparent. On the other hand, Fig. 3C is a photograph showing the appearance of the sintered body of Comparative Example 6, which was held at a hold temperature of 1080°C for 12 hours, heated to the sintering temperature, sintered, and then HIP-treated, which was black in color.

[0092] Thereafter, all samples, including the HIP-treated sintered bodies that had turned black, were subjected to additional sintering in a vacuum sintering furnace at a sintering temperature of 1720°C for 15 hours in an attempt to eliminate residual bubbles throughout the entire area, including the center of the sintered body.

[0093] Next, each of the obtained sintered bodies was subjected to oxidation annealing treatment at 1400°C for 40 hours in an atmospheric heating furnace while managing each lot (Example number, Comparative example number), to sufficiently recover distortion and oxygen deficiency. In this way, a total of 14 types of sintered body sets, including Examples and Comparative examples, were prepared, each set consisting of at least three sintered bodies and up to nine sintered bodies.

[0094] Thereafter, all of the obtained sintered body samples were cut and precision polished to a length of 20 mm, and it was confirmed that both optical end faces of all of the sintered body samples had an optical surface precision of λ / 8 or more (when the measurement wavelength λ=633 nm), and that the average roughness was processed under the conditions of an arithmetic mean height Sa of 0.70 nm or less and a root mean square height Sq of 0.89 nm or less.

[0095] For each of the sintered body samples obtained as described above, the total light transmittance and forward scattering coefficient were measured as follows.

[0096] (Method for measuring total light transmittance and forward scattering) Total light transmittance and forward scattering were measured with reference to JIS K7105 (ISO 13468-2:1999) and JIS K7136 (ISO 14782:1999). Measurements were performed at wavelengths of 540 nm, 600 nm, 760 nm, 930 nm, and 1064 nm using a spectrophotometer V-670 manufactured by JASCO Corporation.

[0097] First, to measure the total light transmittance, the spectrophotometer V-670 is irradiated with light separated by a spectroscope without setting a workpiece (sample), the light is received by an integrating sphere set in the device in advance, and the collected light is received by a detector. The obtained illuminance is I 0 Next, the workpiece is set in the device, and this time the dispersed light is incident on the workpiece. The transmitted light is again collected by an integrating sphere and received by a detector. The obtained illuminance is defined as I and is calculated using the following formula: Total light transmittance (% / 25mm) = I / I 0 ×100

[0098] Next, to measure forward scattering, the same measurement system is used except that the reflector on the back of the integrating sphere is removed from the state where the workpiece is set. The dispersed light is again incident on the workpiece, and the transmitted light is again collected by the integrating sphere and received by the detector. The obtained illuminance represents the scattered components other than the linear transmitted component, and this is called I S The forward scattering rate was calculated using the following formula: Generally, forward scattering is almost flat in the visible range and has no wavelength dependency, so the value at a wavelength of 1064 nm was recorded as a representative value. Forward scattering rate (% / 25 mm) = I S / I 0 ×100

[0099] To account for reproducibility and variations, measurements were taken on three or nine samples under each condition, and the average values ​​were calculated to determine the total light transmittance and forward scattering values ​​for each sample. The beam diameter was 2 mm, regardless of the diameter of the sintered body, and the incident position was adjusted to approximately the center of the optically effective surface. The results are summarized in Table 4, showing the total light transmittance at wavelengths of 540 nm, 600 nm, 760 nm, 930 nm, and 1064 nm, as well as the forward scattering coefficient at a wavelength of 1064 nm. A graph of the total light transmittance for Example 3, Comparative Example 6, and Comparative Example 7 is shown in Figure 4.

[0100]

[0101] From the results in Table 4, it was confirmed that, among the groups in which the calcination temperature of the starting mixed raw materials was controlled to 950°C or less when producing the complex oxide sintered body of the present invention, that is, the groups in which the uncompounded raw material ratio was less than half, and further the group in which the hold temperature during the temperature rise in the sintering step was set to 1000°C, and the groups in which the sintering was carried out so that the relative sintered density was less than 98.9%, preferably 97.2% or less, and then the HIP treatment was carried out, that is, the samples of Examples 1 to 4, all had a total light transmittance of 84.8% or more at a wavelength of 600 nm, a total light transmittance of 84.6% or more at a wavelength of 540 nm, and a total light transmittance of 85.25% or more at a wavelength of 1064 nm, and were finished as truly transparent terbium-containing paramagnetic garnet-type transparent ceramics with no noticeable absorption over a wide wavelength band.

[0102] On the other hand, in the case of the samples in the group in which the calcination temperature of the mixed raw material was set to 1000°C (Comparative Examples 5 and 10), the total light transmittance at a wavelength of 600 nm did not reach 84.8%, the total light transmittance at a wavelength of 540 nm did not reach 84.6%, and the total light transmittance at a wavelength of 1064 nm did not reach 85.25%.

[0103] In addition, in the groups in which the calcination temperature of the mixed raw materials was controlled to 950°C or less, but the hold temperature during the temperature rise in the sintering process was set to 1080°C (Comparative Examples 1, 3, 6, and 8), and in the groups in which the relative sintered density exceeded 97.2% (Comparative Examples 2, 4, 7, and 9), the total light transmittance at a wavelength of 600 nm did not reach 84.8%, the total light transmittance at a wavelength of 540 nm did not reach 84.6%, and further the total light transmittance at a wavelength of 1064 nm did not reach 85.25%.

[0104] Finally, for the samples with forward scattering of 0.5% or more (Comparative Examples 2, 4, 5, 7, 9, and 10), the scattered light would scatter in all directions when a high-power laser beam with an incident power of 160 W was incident, making the evaluation dangerous, so the evaluation of high-power resistance was abandoned.The other eight groups, Examples 1 to 4 and Comparative Examples 1, 3, 6, and 8, were coated with an antireflection film for a wavelength of 1064 nm on both optical end faces, and the rate of change in beam diameter when a high-power laser beam with an incident power of 160 W was incident thereon, was evaluated.

[0105] (Evaluation of Beam Diameter Change Rate) The beam diameter change rate was measured using a collimated CW laser beam manufactured by IPG Inc., having a wavelength of 1070 nm, an output power of 160 W, and a diameter of 1.6 mm, using a ModeMaster PCM manufactured by Coherent Corporation. 2 The beam diameter at the reference plane (full bezel) of the profiler was measured using a beam propagation analyzer. However, since the output power after passing through the sample was very high, the intensity of the output laser light was first attenuated to 1 / 1000 or less using a beam separator before being introduced into the beam profiler. The distance between the reference plane (full bezel) of the beam profiler and the sample holder was 1.9 m, and the distance between the reference plane and the collimator was 2.1 m. First, the beam diameter of the original beam was measured, and this value was used as r 0 Next, each of the samples with a length of 20 mm was placed in the optical path, and the beam diameter of each transmitted light was measured and defined as r. The beam diameter change rate in the present invention is |(1-r / r 0 )|×100, and a value of 10% or less was evaluated as pass, and a value of more than 10% was evaluated as fail. The evaluation results are shown in Table 5.

[0106]

[0107] From the results in Table 5, in the groups of Examples in which the total light transmittance at a wavelength of 600 nm was 84.8% or more, the total light transmittance at a wavelength of 540 nm was 84.6% or more, and the total light transmittance at a wavelength of 1064 nm was 85.25% or more, the beam diameter change rate when a high-power laser beam with an incident power of 160 W was incident was 10% or less. Conversely, in the groups of Comparative Examples 1, 3, 6, and 8 in which the total light transmittance values ​​did not reach these levels, the beam diameter change rate when a high-power laser beam with an incident power of 160 W was incident was more than 10%, which deteriorated.

[0108] Although the present invention has been described using the above-mentioned embodiment, the present invention is not limited to this embodiment, and can be modified within the scope of what a person skilled in the art can conceive, such as other embodiments, additions, changes, deletions, etc., and any aspect is included in the scope of the present invention as long as it achieves the effects of the present invention.

[0109] 100 Optical isolator 102 Housing 110 Faraday rotator 120 Polarizer 130 Analyzer 140 Magnet

Claims

1. A terbium-containing paramagnetic garnet-type transparent ceramic comprising a sintered body of a composite oxide containing terbium, yttrium, scandium and aluminum represented by the following formula (1), (Tb 1-x-y Y x S.C. y ) 3 (Al 1-z S.C. z ) 5 O 12 (1) (wherein 0.35≦x≦0.45, 0<y<0.03, 0.5<1-x-y<0.65, 0.001<z<0.03, and 0<y+z<0.06) A terbium-containing paramagnetic garnet-type transparent ceramic having a total light transmittance of 84.8% or more at a wavelength of 600 nm.

2. SiO as a sintering aid 2 2. The terbium-containing paramagnetic garnet-type transparent ceramic according to claim 1, further comprising:

3. The terbium-containing paramagnetic garnet-type transparent ceramic according to claim 1 or 2, wherein both optical end faces are precisely mirror-polished so that the length of the terbium-containing paramagnetic garnet-type transparent ceramic is 14 mm or more, and the average roughness of each of the polished optical end faces is in the range of arithmetic mean height Sa≦0.70 nm or root mean square height Sq≦0.89 nm.

4. The terbium-containing paramagnetic garnet-type transparent ceramic according to claim 1 or 2, wherein the total light transmittance of said paramagnetic garnet-type transparent ceramic is 84.6% or more at a wavelength of 540 nm and 85.25% or more at a wavelength of 1064 nm.

5. A magneto-optical material comprising the terbium-containing paramagnetic garnet-type transparent ceramic according to claim 1 or 2.

6. A magneto-optical device comprising the magneto-optical material according to claim 5.

7. The magneto-optical device according to claim 6, which is an optical isolator usable in the wavelength range of 0.9 μm or more and 1.1 μm or less, comprising the terbium-containing paramagnetic garnet-type transparent ceramic as a Faraday rotator and having polarizing materials in front of and behind the optical axis of the Faraday rotator.

8. A method for producing a terbium-containing paramagnetic garnet-type transparent ceramic comprising a sintered body of a composite oxide containing terbium, yttrium, scandium and aluminum represented by the following formula (1), comprising: (Tb 1-x-y Y x S.C. y ) 3 (Al 1-z S.C. z ) 5 O 12 (1) (wherein, 0.35≦x≦0.45, 0<y<0.03, 0.5<1-x-y<0.65, 0.001<z<0.03, 0<y+z<0.06) A process for preparing a mixed raw material by mixing terbium oxide and yttrium oxide or a coprecipitated oxide of terbium and yttrium with aluminum oxide and scandium oxide; A process for calcining or heating and drying the mixed raw material with a thermal history of 950°C or less, and then shaping the mixed raw material to obtain a molded body; A process for degreasing the molded body to obtain a degreased body; A process for sintering the degreased body under reduced pressure, first maintaining a hold temperature of 1000°C or less to degas the degreased body while maintaining a state in which the degreased body exhibits a brown color derived from the tetravalent terbium, and then heating the degreased body to a sintering temperature to obtain a sintered body having a relative sintered density in the range of 93.8% to 97.2%; a step of further densifying the sintered body by hot isostatic pressing (HIP) until the relative sintered density becomes 99.9% or more; a step of subjecting the densified sintered body to a decolorizing annealing treatment at a temperature lower than the temperature in the HIP treatment to decolorize the brown color derived from the tetravalent terbium exhibited by the densified sintered body; a step of additionally sintering the decolorized sintered body under reduced pressure at a temperature higher than both the sintering temperature and the temperature in the HIP treatment; and a step of subjecting the additionally sintered sintered body to an oxidation annealing treatment in an oxygen atmosphere or in the air at a temperature lower than the temperature in the HIP treatment.

9. A method for producing terbium-containing paramagnetic garnet-type transparent ceramics as set forth in claim 8, wherein the weight ratio of the residue that does not pass through a mesh having an opening of 20 μm to the total weight of the mixed raw material is 0.5% or less.

10. A mixed raw material for producing a terbium-containing paramagnetic garnet-type transparent ceramic, comprising a sintered body of a composite oxide containing terbium, yttrium, scandium and aluminum represented by the following formula (1), (Tb 1-x-y Y x S.C. y ) 3 (Al 1-z S.C. z ) 5 O 12 (1) (Wherein, 0.35≦x≦0.45, 0<y<0.03, 0.5<1-x-y<0.65, 0.001<z<0.03, 0<y+z<0.06) The mixed raw material is a mixture in which the oxides of terbium, yttrium, scandium, and aluminum are mixed in an uncombined state, and the weight ratio of the residue that does not pass through a 20 μm mesh to the total weight of the mixed raw material is 0.5% or less.

11. A method for producing a magneto-optical device, comprising the steps of: forming a magneto-optical device using the paramagnetic garnet-type transparent ceramic obtained by the method for producing paramagnetic garnet-type transparent ceramic according to claim 8 or 9.

Citation Information

Patent Citations

  • Terbium-aluminum-garnet single crystal and method of manufacturing for the same

    JP2002293693A

  • Garnet crystal for magnetooptical element

    JP2011213552A

  • Paramagnetic garnet transparent ceramic, magnetic optical material and magnetic optical device

    JP2019199386A

  • Paramagnetic garnet-type transparent ceramic, magneto-optical material, and magneto-optical device

    WO2018193848A1

  • Method for manufacturing transparent ceramics for faraday rotator

    JP2019207340A