Solid electrolyte, solid electrolyte layer, and solid electrolyte battery

The development of halide-based solid electrolytes with specific compositions addresses the low sodium ion conductivity and stability issues in existing electrolytes, achieving high conductivity and stability for all-solid-state sodium ion batteries through compression molding and a glassy or defective double perovskite structure.

WO2024237345A1PCT designated stage expired Publication Date: 2024-11-21KYUSHU UNIV

Patent Information

Application Number
PCT/JP2024/018413
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-17
Filing Date
2024-05-17
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Current solid electrolytes for all-solid-state sodium ion batteries have insufficient sodium ion conductivity, and existing halide-based electrolytes require high temperatures for stability, while sulfide-based electrolytes lack chemical and electrochemical stability.

Method used

Development of halide-based solid electrolytes with specific compositions, such as Na3α+2β+1cM1M2M3ChX6-2α and Na3α+2β+1cM1M2M3X6, which can be compression molded at room temperature and exhibit high sodium ion conductivity, using elements like Y, Sc, Al, Ga, In, Zr, Hf, Nb, Ta, and halogens like Cl, Br, I, to form a glassy or defective double perovskite structure.

Benefits of technology

The new solid electrolytes demonstrate high sodium ion conductivity (1 × 10−6 S/cm or more) at 25°C and maintain conductivity over a wide temperature range, even after heat treatment, with a relative density of 80% or more, enhancing the performance and stability of all-solid-state sodium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018413_21112024_PF_FP_ABST
    Figure JP2024018413_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a solid electrolyte which has high sodium ion conductivity. This solid electrolyte contains a compound represented by formula (1) or formula (2). Formula (1): Na3a+2b+1cM1 aM2 bM3 cChαX6-2α Formula (2): Na3a+2b+1cM1 aM2 bM3 cX6 In formulae (1) and (2), M1 is selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof; M2 is selected from the group consisting of Zr, Hf, Ti, Si, Ge, Sn, and combinations thereof; and M3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi, and combinations thereof. Ch is selected from the group consisting of O, S, Se, Te and combinations thereof, and X is selected from the group consisting of F, Cl, Br, I, and combinations thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Solid electrolyte, solid electrolyte layer and solid electrolyte battery

[0001] The present invention relates to a solid electrolyte, a solid electrolyte layer, and a solid electrolyte battery.

[0002] Lithium-ion secondary batteries have traditionally been installed in a wide range of electronic and electrical devices, including mobile phones, laptops, digital cameras and videos, and portable music players. There is a strong demand for batteries, which serve as the power source for these devices, to be smaller and thinner, as well as safer. In the currently widely used lithium-ion secondary batteries, charging and discharging are achieved by lithium ions moving between the positive and negative electrodes via an electrolyte, which contains an organic solvent. Because the electrolyte contains a flammable organic solvent, ensuring safety against leakage and other issues is a challenge.

[0003] For this reason, development of all-solid-state lithium-ion secondary batteries in which a solid electrolyte layer is provided between a positive electrode and a negative electrode is underway. Known solid electrolytes include oxide-based solid electrolytes, sulfide-based solid electrolytes, and complex hydride-based solid electrolytes. In recent years, the use of halide solid electrolytes as the solid electrolyte has also been considered (Patent Documents 1 and 2).

[0004] For example, Patent Document 1 discloses a solid electrolyte made of a compound represented by the following formula [1]: 2+a E 1-b+α G b X d ... [1] In formula [1], A is one element selected from the group consisting of Li, K, and Na, E is at least one element selected from the group consisting of Zr, Hf, Ti, and Sn, G is at least one element selected from the group consisting of Mg, Ca, Sr, Cs, Ba, Y, Al, Sc, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Cu, Ag, Au, Pb, Bi, In, Sn, Sb, Nb, Ta, and W, and X is at least one element selected from the group consisting of F, Cl, Br, and I. Note that Patent Document 1 evaluates battery performance only when A is Li.

[0005] In addition, Patent Document 2 states that 4-2x-y-z B x Sn 3-y M y O 8-z N z A solid electrolyte characterized by having a crystal structure represented by the formula (1≦4−2x-y-z<4, A: Li, Na, B: Mg, Ca, Sr, Ba, M: V, Nb, Ta, N: F, Cl) is disclosed.

[0006] Sodium is more abundant than lithium, and there is no concern about uneven distribution of production areas. For this reason, in recent years, there has been hope for the practical application of all-solid-state sodium-ion batteries to replace all-solid-state lithium-ion batteries. To make all-solid-state sodium-ion batteries practical, the development of solid electrolyte materials that exhibit high sodium ion conductivity is required.

[0007] As sodium ion conductive solid electrolytes, oxide-based solid electrolytes, sulfide-based solid electrolytes, and the like are known, similar to lithium ion conductive solid electrolyte materials. In addition, in recent years, the use of halide solid electrolytes as solid electrolytes has also been considered. Although oxide-based solid electrolytes have excellent chemical and electrochemical stability, they require heat treatment at high temperatures to achieve high ionic conductivity. On the other hand, sulfide-based solid electrolytes can achieve high ionic conductivity by compression molding alone, but they are poor in chemical and electrochemical stability. Therefore, expectations are growing for halide-based solid electrolytes that can be compression molded at room temperature and have higher electrochemical stability than sulfide-based solid electrolytes. For example, Non-Patent Document 1 describes Na as a solid electrolyte for high-voltage, long-life all-solid-state sodium ion batteries. 3-x Y 1-x Zr x Cl 6 has been reported.

[0008] International Publication No. 2021 / 024783 International Publication No. 2014 / 141456

[0009] Nature Communications volume 12, Article number: 1256 (2021)

[0010] As mentioned above, halide-based solid electrolytes for all-solid-state sodium-ion secondary batteries have been reported, but their sodium ion conductivity is insufficient, and there is a need to develop halide-based solid electrolyte materials that exhibit higher sodium ion conductivity.

[0011] Therefore, in order to solve the problems of the conventional technology, the present inventors have carried out investigations with the aim of providing a solid electrolyte having high sodium ion conductivity.

[0012] Examples of specific embodiments of the present invention are given below.

[0013] [1] A solid electrolyte containing a compound represented by formula (1) or formula (2). Formula (1) Na 3a+2b+1c M 1 a M 2 b M 3 c Ch α X 6-2α (In formula (1), M 1 is selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof; M 2 is selected from the group consisting of Zr, Hf, Ti, Si, Ge, Sn, and combinations thereof; M 3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi and combinations thereof, Ch is selected from the group consisting of O, S, Se, Te and combinations thereof, X is selected from the group consisting of F, Cl, Br, I and combinations thereof, and a+b+c=1, 0≦a≦1, 0≦b≦1, 0≦c≦1, 0.1≦α≦2.9. Formula (2) Na 3a+2b+1c M 1 a M 2 b M 3 c X 6 (In formula (2), M 1is selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof; M 2 is selected from the group consisting of Zr, Hf, Ti, Si, Ge, Sn, and combinations thereof; M 3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi and combinations thereof, and X is selected from the group consisting of F, Cl, Br, I and combinations thereof, and a+b+c=1, 0≦a≦0.9, 0≦b≦0.9, 0.1≦c≦1. [2] In formula (2), M 3 is selected from the group consisting of Ta and Nb. [3] The solid electrolyte according to [1], wherein X is Cl in formula (1). [4] The solid electrolyte according to [1], wherein X is Cl in formula (2). [5] The solid electrolyte according to [1], wherein when compression-molded at room temperature under a pressure of 170 MPa, the sodium ion conductivity at 25°C is 1×10 -6 [6] The solid electrolyte according to any one of [1] to [4], which has a relative density of 80% or more when compression-molded at room temperature under a pressure of 170 MPa. [7] A solid electrolyte comprising a compound represented by formula (1'). This embodiment may also relate to a solid electrolyte comprising a compound represented by formula (1'). Formula (1') Na3a+2b+1c-γ+δM 1 a M 2 b M 3 c Ch ε X ζ (In formula (1'), M 1 is selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof; M 2 is selected from the group consisting of Zr, Hf, Ti, Si, Ge, Sn, and combinations thereof; M 3is selected from the group consisting of Nb, Ta, V, P, Sb, Bi and combinations thereof, Ch is selected from the group consisting of O, S, Se, Te and combinations thereof, X is selected from the group consisting of F, Cl, Br, I and combinations thereof, and a+b+c=1, 0≦a≦1, 0≦b≦1, 0≦c≦1, 0≦γ<≦1, 0≦δ≦2, 0≦ε≦2 and 4≦ζ≦8. [8] A solid electrolyte according to [7], wherein X is Cl in formula (1'). [9] A solid electrolyte according to [7], wherein when compression-molded at room temperature under a pressure of 170 MPa, the sodium ion conductivity at 25°C is 1×10 -6

[10] The solid electrolyte according to any one of [7] to [9], which has a relative density of 80% or more when compression-molded at room temperature under a pressure of 170 MPa.

[11] A solid electrolyte layer comprising the solid electrolyte according to any one of [1] to

[10] .

[12] A solid electrolyte battery comprising the solid electrolyte layer according to

[11] .

[0014] According to the present invention, a solid electrolyte having high sodium ion conductivity can be provided. Furthermore, according to the present invention, a solid electrolyte layer and a solid electrolyte battery (all-solid-state sodium ion secondary battery) exhibiting high sodium ion conductivity can be provided.

[0015] NaNbCl 6 This is the result of energy X-ray diffraction analysis of NaTaCl 6 The results are obtained by energy X-ray diffraction analysis of Na 3 YCl 6 The results are obtained by energy X-ray diffraction analysis of NaNbOCl. 4 This is the analysis result of energy X-ray diffraction of NaTaOCl 4 1 shows the results of energy X-ray diffraction analysis of NaNbCl after heat treatment. 6 The results of energy X-ray diffraction analysis of NaTaCl after heat treatment are shown. 6 The results of energy X-ray diffraction analysis of Na after heat treatment are shown. 3 YCl 61 shows the results of energy X-ray diffraction analysis of the solid electrolytes obtained in Examples and Comparative Examples. 6 This is the analysis result of energy X-ray diffraction of NaNbCl 6 This is the result of diffuse reflectance measurement of NaTaCl 6 This is the result of diffuse reflectance measurement of NaTaOCl 4 This is the result of diffuse reflectance measurement of NaNbOCl. 4 This is the result of diffuse reflectance measurement of Na 1+x Ta 1-x Zr x Cl 6 (x<1.0) shows the results of X-ray diffraction and impedance measurement. 1+x Ta 1-x Zr x Cl 6 (x<1.0) shows the measurement results of sodium ion conductivity. 2 O 5 Using NaTa 1/5(3+2x) O x Cl 4 The results of X-ray diffraction and impedance measurement are shown for the synthesis of Ta as an oxygen source. 2 O 5 Using NaTa 1/5(3+2x) O x Cl 4 The results are shown in Table 1. The sodium ion conductivity was measured when Ta was used as an oxygen source. 2 O 5 Using Na 1+x TaOCl 4+x The results of X-ray diffraction and impedance measurement are shown for the synthesis of Ta as an oxygen source. 2 O 5 Using Na 1+x TaOCl 4+x The results are shown in Table 1. The sodium ion conductivity was measured when Ta was used as an oxygen source. 2 O 5 The process time was changed using NaTaOCl 4 The results are shown in Table 1. The sodium ion conductivity was measured when Ta was used as an oxygen source. 2 O 5 The process time was changed using NaTaOCl4 The results are shown in Table 1. The sodium ion conductivity was measured when Na was used as an oxygen source. 2 Na using O 2x TaO x Cl 5 The results of X-ray diffraction and impedance measurement are shown for the synthesis of Na as an oxygen source. 2 Na using O 2x TaO x Cl 5 1 shows the measurement results of sodium ion conductivity when synthesized.

[0016] The present invention will be described in detail below. The following description of the constituent elements may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0017] (Solid Electrolyte) The present embodiment relates to a solid electrolyte containing a compound represented by formula (1) or formula (2). Formula (1) Na 3a+2b+1c M 1 a M 2 b M 3 c Ch α X 6-2α (In formula (1), M 1 is selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof; M 2 is selected from the group consisting of Zr, Hf, Ti, Si, Ge, Sn, and combinations thereof; M 3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi and combinations thereof, Ch is selected from the group consisting of O, S, Se, Te and combinations thereof, X is selected from the group consisting of F, Cl, Br, I and combinations thereof, and a+b+c=1, 0≦a≦1, 0≦b≦1, 0≦c≦1, 0.1≦α≦2.9. Formula (2) Na 3a+2b+1c M 1a M 2 b M 3 c X 6 (In formula (2), M 1 is selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof; M 2 is selected from the group consisting of Zr, Hf, Ti, Si, Ge, Sn, and combinations thereof; M 3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi and combinations thereof, X is selected from the group consisting of F, Cl, Br, I and combinations thereof, and a+b+c=1, 0≦a≦0.9, 0≦b≦0.9, 0.1≦c≦1.

[0018] In formula (1), M 1 is selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof. 1 is preferably one selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu, and more preferably one selected from the group consisting of Y, Sc and In. 1 In the above, when referring to a combination of elements, for example, a solid solution of two or more of the above elements can be mentioned.

[0019] In formula (1), 0≦a≦1, preferably 0≦a≦0.9, more preferably 0≦a≦0.7, and further preferably 0≦a≦0.5. In formula (1), it is also preferable that a=0, and when a is 0, M 1 is not included.

[0020] In formula (1), M 2 is selected from the group consisting of Zr, Hf, Ti, Si, Ge, Sn and combinations thereof. 2is preferably one selected from the group consisting of Zr, Hf, Ti, Si, Ge and Sn, and more preferably one selected from the group consisting of Zr and Hf.

[0021] In formula (1), 0≦b≦1, preferably 0≦b≦0.9, more preferably 0≦b≦0.7, and further preferably 0≦b≦0.5. In formula (1), it is also preferable that b=0, and when b is 0, M 2 is not included.

[0022] In formula (1), M 3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi and combinations thereof. 3 is preferably one selected from the group consisting of Nb, Ta, V, P, Sb, and Bi, more preferably one selected from the group consisting of Nb, Ta, and V, and particularly preferably Nb or Ta.

[0023] In formula (1), 0≦c≦1, preferably 0.1≦c≦1, and more preferably 0.2≦c≦1. In formula (1), a+b+c=1.

[0024] In formula (1), Ch is selected from the group consisting of O, S, Se, Te, and combinations thereof. Among them, Ch is preferably one selected from the group consisting of O, S, Se, and Te, more preferably O or S, and particularly preferably O. As in the compound represented by formula (1), by introducing an element selected from the group consisting of O, S, Se, Te, and combinations thereof into Ch, the conductivity of the solid electrolyte can be more effectively improved.

[0025] In formula (1), X is selected from the group consisting of F, Cl, Br, I, and combinations thereof. Among these, X is preferably one selected from the group consisting of F, Cl, Br, and I, more preferably Cl or Br, and particularly preferably Cl. When Ch in formula (1) is O, the compound represented by formula (1) becomes an acid halide compound, and in this embodiment, it is preferable to use an acid halide compound that can exhibit high sodium ion conductivity.

[0026] In formula (1), 0.1≦α≦2.9, preferably 0.2≦α≦2.0, and more preferably 0.5≦α≦1.5. Of these, it is particularly preferable that α is 1.

[0027] The present embodiment may also relate to a solid electrolyte containing a compound represented by formula (1'): Na3a+2b+1c-γ+δM 1 a M 2 b M 3 c Ch ε X ζ (In formula (1'), M 1 is selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof; M 2 is selected from the group consisting of Zr, Hf, Ti, Si, Ge, Sn, and combinations thereof; M 3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi, and combinations thereof; Ch is selected from the group consisting of O, S, Se, Te, and combinations thereof; X is selected from the group consisting of F, Cl, Br, I, and combinations thereof; and a+b+c=1, 0≦a≦1, 0≦b≦1, 0≦c≦1, 0≦γ<≦1, 0≦δ≦2, 0≦ε≦2, and 4≦ζ≦8.

[0028] In addition, M in formula (1′) 1 , M 2 , M 3 Examples and preferred ranges of Ch and X are as follows: M1 , M 2 , M 3 , Ch and X. The preferred numerical ranges of a, b and c in formula (1') are the same as the preferred numerical ranges of a, b and c in formula (1). γ is preferably 0.2 or less, and more preferably 0. Furthermore, (-γ+δ) is preferably 0 or more and 2 or less. Furthermore, (3a+2b+1c-γ+δ) is preferably 1 or more and 3 or less. Furthermore, ε is preferably 0.3 or more and 1 or less. Furthermore, ε is preferably 4 or more and 7 or less, and more preferably 4 or more and 6 or less.

[0029] The compound represented by formula (1) is preferably a compound represented by the following formula (11): Formula (11) NaM 3 Ch α X 6-2α (In formula (11), M 3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi and combinations thereof, Ch is selected from the group consisting of O, S, Se, Te and combinations thereof, and X is selected from the group consisting of F, Cl, Br, I and combinations thereof, and 0.1≦α≦2.9.

[0030] In addition, M in formula (11) 3 Examples and preferred ranges of Ch and X are as follows: M 3 , Ch and X.

[0031] When diffuse reflectance measurement is performed on the compound represented by formula (1), the band gap value calculated from the absorption coefficient obtained by converting the measured data using a Kubelka-Munk function is preferably 2 eV or more, more preferably 2.5 eV or more, and even more preferably 3 eV or more. By setting the band gap value within the above range, the compound represented by formula (1) can exhibit high electronic insulating properties.

[0032] In formula (2), M 1 is selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof. 1is preferably one selected from the group consisting of Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, and more preferably one selected from the group consisting of Y, Sc, and In.

[0033] In formula (2), 0≦a≦0.9, preferably 0≦a≦0.8, more preferably 0≦a≦0.7, and further preferably 0≦a≦0.5. In formula (2), it is also preferable that a=0, and when a is 0, M 1 is not included.

[0034] In formula (2), M 2 is selected from the group consisting of Zr, Hf, Ti, Si, Ge, Sn and combinations thereof. 2 is preferably one selected from the group consisting of Zr, Hf, Ti, Si, Ge and Sn, and more preferably one selected from the group consisting of Zr and Hf. 2 is also preferably Si or Ge.

[0035] In formula (2), 0≦b≦0.9, preferably 0≦b≦0.8, more preferably 0≦b≦0.7, and further preferably 0≦b≦0.5. In formula (2), it is also preferable that b=0, and when b is 0, M 2 is not included.

[0036] In formula (2), M 3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi and combinations thereof. 3 is preferably one selected from the group consisting of Nb, Ta, V, P, Sb, and Bi, more preferably one selected from the group consisting of Nb, Ta, and V, and particularly preferably Nb or Ta.

[0037] In formula (2), 0≦c≦1, preferably 0.1≦c≦1, and more preferably 0.2≦c≦1. Note that in formula (2), a+b+c=1.

[0038] In formula (2), X is selected from the group consisting of F, Cl, Br, I, and combinations thereof. Among these, X is preferably one selected from the group consisting of F, Cl, Br, and I, more preferably Cl or Br, and particularly preferably Cl.

[0039] The compound represented by formula (2) is preferably a compound represented by the following formula (12): Formula (12) NaM 3 X 6 (In formula (12), M 3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi and combinations thereof, and X is selected from the group consisting of F, Cl, Br, I and combinations thereof.

[0040] In addition, M in formula (12) 3 Examples and preferred ranges of X are M in formula (2). 3 and X.

[0041] When diffuse reflectance measurement is performed on the compound represented by formula (2), the band gap value calculated from the absorption coefficient obtained by converting the measured data using a Kubelka-Munk function is preferably 2 eV or more, more preferably 2.5 eV or more, and even more preferably 3 eV or more. By setting the band gap value within the above range, the compound represented by formula (2) can exhibit high electronic insulating properties.

[0042] In the compounds represented by formula (1) and formula (2), the metal element and the halogen element preferably form an octahedron with six-coordination, and the octahedron serves as the basic structure of the anion sublattice. More preferably, the compounds have a glassy or defective double perovskite structure. The compounds represented by formula (1) and formula (2) are novel compounds as solid electrolytes, and are halide solid electrolytes that exhibit high sodium ion conductivity.

[0043] The present embodiment has the above-described configuration, and therefore has high sodium ion conductivity. For example, when the solid electrolyte is compression molded at room temperature under a pressure of 170 MPa, the sodium ion conductivity at 25°C is 1×10 -6S / cm or more, and 5×10 -6 S / cm or more is more preferable, and 1×10 -5 S / cm or more is more preferable, and 1×10 -4 As described above, since the solid electrolyte of the present embodiment has high sodium ion conductivity, a solid electrolyte battery including a solid electrolyte layer formed from the above solid electrolyte material can exhibit excellent battery performance.

[0044] In this specification, the sodium ion conductivity of the solid electrolyte is measured after the solid electrolyte is compression-molded at room temperature under a pressure of 170 MPa. The solid electrolyte of this embodiment can exhibit high sodium ion conductivity by compression molding at room temperature, and therefore can reduce energy input during use.

[0045] Furthermore, the solid electrolyte of this embodiment, having the above-described structure, can exhibit high conductivity over a wide temperature range. For example, the solid electrolyte of this embodiment can exhibit high conductivity even in a relatively high temperature range (e.g., about 50 to 600°C), and even in this case, the decrease in its sodium ion conductivity is suppressed.

[0046] Furthermore, even when the solid electrolyte of this embodiment is heat-treated, the sodium ion conductivity is suppressed from decreasing. For example, even when the solid electrolyte of this embodiment is heat-treated at 200° C. for 12 hours, the conductivity is hardly decreased, and high sodium ion conductivity is maintained. Therefore, when the solid electrolyte of this embodiment is used, it is also possible to adjust the interface state by heat treatment.

[0047] In addition, the solid electrolyte of this embodiment has high moldability. The solid electrolyte of this embodiment has a high relative density even when compression molded. Specifically, when the solid electrolyte is compression molded at room temperature under a pressure of 170 MPa, the relative density is preferably 80% or more. Note that the relative density is relative to the theoretical density, and the theoretical density is a value theoretically determined from the crystal structure.

[0048] In the solid electrolyte of this embodiment, for example, by containing Ta or Nb, the electrostatic repulsion between cations in the structure is strengthened, making it possible to realize a structure in which octahedra share corners, and as a result, it is expected that the free volume required for sodium ion conduction will increase (Pauling's third law). This is thought to be why high sodium ion conductivity is exhibited. In addition, M 3 It is believed that the inclusion of a higher valence element, such as that represented by formula (1), results in vacancies at sodium sites formed by the use of structural cations. The formation energy of sodium vacancies leads to a decrease in the activation energy of sodium ion conduction. In particular, in compounds represented by formula (1), the introduction of elements such as oxygen into the halogen-based structural framework stabilizes the corner-sharing structure between octahedra, the basic structural blocks, and allows for the construction of a structure that ensures a larger free volume. This is thought to contribute to improved sodium ion conduction. Furthermore, the introduction of different anions into the structure distorts the structure, resulting in a dispersion in the energy of the Na sites. This is thought to enable the construction of a percolation network of Na sites with similar energy levels with a smaller activation energy. In particular, when solid electrolytes contain elements such as Nb or Ta, a double perovskite structure with large vacancies is formed, which is thought to ensure sodium ion conduction paths even in thermodynamically stable phases where sodium ion conductivity was previously thought to be reduced. It is therefore believed that this will enable the realization of halogen-based solid electrolytes whose sodium ion conductivity does not decrease even after heat treatment.

[0049] The solid electrolyte of this embodiment may contain one compound having a single composition, or may contain two or more compounds having different compositions. The shape of the solid electrolyte is not particularly limited, and may be, for example, powder, granules, or blocks, or may be pellets or plates.

[0050] (Method for Producing Solid Electrolyte) When the solid electrolyte of this embodiment is in a powder state, the solid electrolyte can be produced, for example, by mixing materials containing predetermined elements in a predetermined molar ratio. Although care must be taken to prevent the generation of HCl gas, oxyhydrides can also be used as the material.

[0051] Solid electrolytes can be produced, for example, by a mechanochemical method. To induce a mechanochemical reaction, a planetary ball mill, for example, is used. A planetary ball mill is a device that places media (balls for pulverizing or promoting the mechanochemical reaction) and materials in a sealed container, rotates and revolves, and applies kinetic energy to the materials to induce pulverization or a mechanochemical reaction. A planetary ball mill can use, for example, a sealed container made of zirconia and zirconia media (balls). When reacting materials using a planetary ball mill, the materials are less likely to reach high temperatures during the reaction, making phase separation less likely to occur. The solid electrolyte production method of this embodiment can also be applied to the production of thermodynamically metastable phases. Furthermore, because the propagation of energy due to the impact of the media contributes to the generation and persistence of defects, the solid electrolyte production method of this embodiment can also be used to produce solid electrolytes that exhibit a structure containing a large number of defects or a glass phase.

[0052] The synthesis of solid electrolytes using mechanochemical methods is necessary for the vitrification of materials, and the longer the reaction time, the higher the conductivity tends to be. For example, when reacting materials using a planetary ball mill, the reaction time is preferably 5 to 200 hours, more preferably 10 to 150 hours, and even more preferably 25 to 100 hours.

[0053] The solid electrolyte may be produced by firing. The firing temperature is preferably, for example, 150 to 600°C, and the firing time is preferably 10 minutes to 48 hours. Furthermore, firing is preferably carried out in a vacuum or an inert atmosphere.

[0054] The solid electrolyte may be produced by liquid phase synthesis, for example, in a predetermined organic solvent or aqueous solvent.

[0055] (Solid Electrolyte Layer) This embodiment relates to a solid electrolyte layer containing the above-described solid electrolyte. The solid electrolyte layer preferably contains 50 mass % or more of the above-described solid electrolyte, more preferably 60 mass % or more, even more preferably 70 mass % or more, still more preferably 80 mass % or more, and particularly preferably 90 mass % or more. Furthermore, the solid electrolyte layer may contain 100 mass % of the above-described solid electrolyte, or may be a layer consisting only of the above-described solid electrolyte.

[0056] The sodium ion conductivity of the solid electrolyte layer at 25°C is 1 x 10 -6 S / cm or more, and 5×10 -6 S / cm or more is more preferable, and 1×10 -5 S / cm or more is more preferable, and 1×10 -4 It is particularly preferable that the viscosity is 25 S / cm or more.

[0057] The relative density of the solid electrolyte layer is preferably 80% or more. The relative density is relative to the theoretical density, and the theoretical density is a value theoretically determined from the crystal structure.

[0058] The thickness of the solid electrolyte layer is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. The thickness of the solid electrolyte layer is preferably 1 mm or less. By setting the thickness of the solid electrolyte layer within the above range, sodium ion conductivity can be more effectively increased.

[0059] The solid electrolyte layer may contain optional components other than the solid electrolyte described above, as long as the optional components do not deviate from the spirit of the present invention. Examples of optional components include a binder resin. In this case, the content of the optional components is preferably 10% by mass or less, and more preferably 1% by mass or less, based on the total mass of the solid electrolyte.

[0060] (Method for manufacturing solid electrolyte layer) The solid electrolyte layer is obtained by compressing and molding the obtained powder solid electrolyte. In this case, for example, the powder solid electrolyte may be compressed at room temperature to form a molded body, or may be compressed using a hot press method to form a molded body.

[0061] The solid electrolyte layer of this embodiment can be obtained by compression molding at room temperature. The molding pressure at this time is preferably 50 to 500 MPa. When the solid electrolyte layer of this embodiment is compression molded at room temperature, energy consumption during production can be reduced, and the burden on the environment can also be reduced.

[0062] The solid electrolyte layer may be a sintered body obtained by sintering the obtained powdered solid electrolyte. When the solid electrolyte layer is formed by sintering, the sintering temperature is preferably about 200 to 500°C, and the sintering time is preferably about 5 to 60 minutes.

[0063] (Solid Electrolyte Battery) This embodiment relates to a solid electrolyte battery including the above-described solid electrolyte layer. The solid electrolyte battery in this embodiment is an all-solid-state sodium ion secondary battery.

[0064] The solid electrolyte battery is preferably an all-solid-state sodium ion secondary battery having a positive electrode, a solid electrolyte layer, and a negative electrode. In this embodiment, the solid electrolyte layer is provided between the positive electrode and the negative electrode. In the all-solid-state sodium ion secondary battery, a positive electrode current collector may be laminated on the positive electrode, or a negative electrode current collector may be laminated on the negative electrode. Furthermore, the all-solid-state sodium ion secondary battery may be housed in a battery case.

[0065] <Positive Electrode> The positive electrode has a positive electrode active material. The positive electrode active material is preferably a compound capable of absorbing and releasing sodium. Examples of the positive electrode active material include a complex compound containing sodium and a transition metal, such as a complex oxide or a phosphate compound. Examples of the complex compound include a complex oxide containing sodium and a transition metal, and a phosphate compound containing sodium and a transition metal. For example, Na 2 Fe 2 (SO 4 ) 3 , NaNi0.5 Mn 0.5 O 2 , NaFe 0.5 Mn 0.5 O 2 , NaFe 0.5 Co 0.5 O 2 transition metal oxides such as Na 3 V 2 (P.O. 4 ) 3 Examples of phosphoric acid-based positive electrodes include those described above.

[0066] The positive electrode is also preferably a composite positive electrode. In this case, a composite positive electrode is formed containing the above-mentioned positive electrode active material and the above-mentioned solid electrolyte. In the composite positive electrode, a positive electrode layer in which the positive electrode active material and the solid electrolyte are mixed substantially uniformly may be formed, or a layer containing the positive electrode active material as a main component may be laminated on a layer in which the positive electrode active material and the solid electrolyte are mixed substantially uniformly.

[0067] The positive electrode may contain optional components in addition to the active materials described above. Examples of optional components include a conductive additive, glass, etc. In this case, the content of the optional components is preferably 20% by volume or less, and more preferably 5% by volume or less, based on the total volume of the positive electrode.

[0068] <Negative Electrode> The negative electrode includes a negative electrode active material. Examples of the negative electrode active material include compounds capable of absorbing and releasing sodium. Examples include sodium metal, sodium alloys (alloys of sodium with metals such as tin, aluminum, and antimony), inorganic compounds such as tin compounds, carbon materials, silicon-based materials (Si and SiO), and conductive polymers.

[0069] The negative electrode may contain optional components in addition to the active materials described above. Examples of optional components include a binder resin and a negative electrode conductive agent. In this case, the content of the optional components is preferably 10% by volume or less, and more preferably 1% by volume or less, based on the total volume of the negative electrode.

[0070] The negative electrode is also preferably a composite negative electrode. In this case, a composite negative electrode containing the above-mentioned negative electrode active material and a solid electrolyte is formed. Note that the composite negative electrode may have a negative electrode layer in which the negative electrode active material and the solid electrolyte are mixed substantially uniformly, or may have a configuration in which a layer containing the negative electrode active material as a main component is laminated on a layer in which the negative electrode active material and the solid electrolyte are mixed substantially uniformly.

[0071] <Positive Electrode Current Collector> The all-solid-state sodium ion secondary battery may have a positive electrode current collector on the positive electrode. The positive electrode current collector is electrically connected to the positive electrode. Examples of materials for the positive electrode current collector include aluminum, stainless steel, and titanium. Examples of the form of the positive electrode current collector include a metal plate, a metal foil, a foam metal plate, and an expanded metal.

[0072] <Negative electrode current collector> The all-solid-state sodium ion secondary battery may have a negative electrode current collector on the negative electrode. The negative electrode current collector is electrically connected to the negative electrode. Examples of materials for the negative electrode current collector include copper, stainless steel, titanium, and nickel. The negative electrode current collector may be in the form of a metal plate, metal foil, foam metal plate, expanded metal, or the like.

[0073] <Battery Case> The battery case accommodates the laminate of the positive electrode current collector, positive electrode, solid electrolyte layer, negative electrode, and negative electrode current collector described above. The shape of the battery case is not particularly limited and can be appropriately selected depending on various applications. Examples of the shape of the battery case include a cylindrical shape, a flattened oval shape, a flattened elliptical shape, and a rectangular shape. Examples of materials constituting the battery case include aluminum, stainless steel, nickel-plated steel, various resins, and the like.

[0074] The features of the present invention will be explained in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, treatment contents, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the specific examples shown below.

[0075] Example 1: NaNbCl 6 Preparation of NaNbCl 6 NaCl and NbCl5 The material was synthesized by a mechanochemical method using the reagents. Specifically, the above powder reagents, weighed in the stoichiometric ratio, were filled into an 80 mL planetary ball mill cup made of zirconia together with Zr milling media, and mechanochemical synthesis was carried out using a Fritsche Planetary Ball Mill P-7 at 500 rpm for 33 hours. During this process, the mechanical mixing of the ball mill was repeated 198 times for 10 minutes at 10-minute intervals to avoid the inside of the ball mill becoming too hot. The obtained powder (solid electrolyte) was collected in a glove box, and its properties were verified by X-ray diffraction and impedance measurement.

[0076] Example 2: NaTaCl 6 Preparation of NaTaCl 6 was synthesized by mechanochemical synthesis using NaCl and TaCl5 reagents. Specifically, the above powder reagents, weighed in stoichiometric ratios, were loaded into an 80 mL zirconia planetary ball mill cup along with Zr milling media, and mechanochemical synthesis was carried out using a Fritsche Planetary Ball Mill P-7 at 500 rpm for 33 hours. During this process, mechanical mixing in the ball mill was repeated 198 times for 10 minutes at 10-minute intervals to prevent the inside of the ball mill from becoming too hot. The resulting powder was collected in a glove box, and its properties were verified by X-ray diffraction and impedance measurement.

[0077] Example 3: NaTaOCl 4 Preparation of NaTaOCl 4 , NaCl, TaCl 5 and Ta 2 O 5 The compound was synthesized by a mechanochemical method using the reagents. Specifically, the above powder reagents, weighed in the stoichiometric ratio, were filled into an 80 mL planetary ball mill cup made of zirconia together with Zr milling media, and mechanochemical synthesis was carried out using a Fritsche Planetary Ball Mill P-7 at 500 rpm for 80 hours. During this process, the mechanical mixing of the ball mill was repeated 480 times, with 10-minute operations every 10 minutes, to avoid the inside of the ball mill becoming too hot. The obtained powder was collected in a glove box, and its properties were verified by X-ray diffraction and impedance measurement.

[0078] Example 4: NaNbOCl4 Preparation of NaTaOCl 4 , NaCl, TaCl 5 and Nb 2 O 5 The compound was synthesized by a mechanochemical method using the reagents. Specifically, the above powder reagents, weighed in the stoichiometric ratio, were filled into an 80 mL planetary ball mill cup made of zirconia together with Zr milling media, and mechanochemical synthesis was carried out using a Fritsche Planetary Ball Mill P-7 at 500 rpm for 80 hours. During this process, the mechanical mixing of the ball mill was repeated 480 times, with 10-minute operations every 10 minutes, to avoid the inside of the ball mill becoming too hot. The obtained powder was collected in a glove box, and its properties were verified by X-ray diffraction and impedance measurement.

[0079] (Comparative Example 1: Na 3 YCl 6 As a comparative example, Na 3 YCl 6 NaCl and YCl 5 The compound was synthesized by a mechanochemical method using the reagents. Specifically, the powdered reagents, weighed in the stoichiometric ratio, were filled into an 80 ml planetary ball mill cup made of zirconia together with Zr milling media, and mechanochemical synthesis was carried out using a Fritsche Planetary Ball Mill P-7 at 500 rpm for 33 hours. During this process, mechanical mixing in the ball mill was repeated 198 times for 10 minutes at 10-minute intervals to prevent the inside of the ball mill from becoming too hot. The resulting powder was collected in a glove box, and its properties were verified by X-ray diffraction and impedance measurement.

[0080] (Measurement and Evaluation) <Confirmation of Crystallization> For the solid electrolytes obtained in the examples and comparative examples, X-ray diffraction was performed using a holder that allows measurement of samples without exposure. Specifically, energy X-ray diffraction (XRD) analysis was performed using a Brucker D8 advanced instrument. The XRD patterns were obtained with 2θ of 12 to 75 degrees. NaNbCl 6 has unique peaks at 15.9, 16.7, 18.9, and 31.1. 6 Then NaNbCl 6The pattern was almost the same as that of the crystal lattice, but each peak appeared at a lower angle of about 0.1 to 0.5 due to the size effect of the crystal lattice (Figs. 1 and 2). 3 YCl 6 is the previously reported crystal structure pattern P2 1 A pattern with the space group NaNbOCl / c was observed (Fig. 3). It was confirmed that the introduction of oxygen changed the crystal structure. 4 In the case of NaNbCl 6 In addition to a small peak attributable to , peaks at 13.9 and 16.3 were particularly characteristic (Fig. 4). 4 is NaTaCl 6 and Ta 2 O 5 A glassy pattern was obtained except for a small peak attributable to (Fig. 5).

[0081] <Ionic Conductivity (1)> A press cell was prepared in which electrochemical measurements could be performed while applying pressure to the sample without exposure. The solid electrolytes obtained in the Examples and Comparative Examples were sealed therein and molded at a pressure of 170 MPa. SUS rods were used as electrodes, and temperature-dependent AC impedance measurements were performed using a VMP3 impedance analyzer manufactured by BioLogic. The obtained frequency response data was fitted using an equivalent circuit with Relaxis3 software to determine the resistance value at each temperature. The ionic conductivity was obtained from the resistance value and the cell constant of the sample, and the activation energy was obtained from its temperature dependence. The conductivity of the solid electrolyte obtained in the Examples was significantly improved compared to the solid electrolyte obtained in the Comparative Examples. Na in Comparative Example 1 3 YCl 6 In the previous study, it was confirmed that conductivity improved by reducing the amount of Na in the structure, but in the system of the example, where high ionic conductivity was achieved due to the low amount of Na and high mobility, conductivity was improved by increasing the amount of Na. Furthermore, by introducing oxygen group elements, a dramatic improvement in conductivity was observed in both samples using Nb and Ta, and in particular in NaTaOCl 4 In this study, conductivity comparable to that of sulfides was achieved without elemental sulfur (Figure 6).

[0082] <Ionic Conductivity (2)> Changes in the structure and transport of solid electrolytes due to sintering were investigated. As shown in Figures 7 to 9, it was found that the peak intensity of samples with crystalline structures increased with annealing, improving the degree of crystallinity. The open symbols in Figure 10 indicate the conductivity of samples after heat treatment at 200°C for 12 hours. All samples were pelletized and vacuum sealed in quartz tubes, and all operations were carried out in a glove box filled with inert gas. After heat treatment, the samples were powdered again and placed in the press cell for electrochemical measurement described above, and the conductivity was measured. Na in Comparative Example 1 3 YCl 6 In the case of NaTaCl, the conductivity was significantly reduced after heat treatment (sintering) (dotted arrow in Figure 10), whereas in the samples containing Ta and Nb of the example, the decrease in conductivity due to heat treatment (sintering) was significantly suppressed. 6 In the case of Ta and Nb, high conductivity was observed even when heat treatment was performed over a wide temperature range (200°C, 500°C, or 600°C) (Fig. 11). This suggests that the high conductivity is maintained over a wide temperature range in the samples containing Ta and Nb, and that the interface state can be adjusted by heat treatment.

[0083] <Calculation of relative density (relative to theoretical density)> The relative density was calculated using the dimensional density relative to the theoretical density. 2 to 300 mg of sample was placed in an electrochemical measurement cell and compressed under a pressure of 170 MPa. The dimensional density was calculated from the surface area and thickness of the compressed pellet and the weight of the sample. The theoretical density was a value theoretically determined from the crystal structure. The relative density relative to the theoretical density was 80 to 90% for all compositions, regardless of before or after heat treatment.

[0084] <Calculation of Band Gap Value> To investigate the electronic properties of the solid electrolytes obtained in Examples 1 to 4, the band gap size was measured by diffuse reflectance measurement using an ultraviolet-visible spectrometer. Solid electrolyte powder was used as the sample, and a Shimadzu UV-3600 Plus was used as the instrument. To perform measurements without exposure to the atmosphere, the solid electrolyte powder was placed on a sample holder with a window inside a glove box, and the window was sealed with vacuum grease. Measurements were performed at room temperature. The band gap value was calculated from the absorption coefficient converted from the measurement data using a Kubelka-Munk function (Figures 12 to 15). As shown in Figure 12, 6 The band gap of NaTaCl is 3.1 eV, as shown in FIG. 6 The band gap of NaTaOCl is 3.7 eV, as shown in FIG. 4 The band gap of NaNbOCl is 3.8 eV, as shown in FIG. 4 The band gaps of the solid electrolytes obtained in the examples were 3.3 eV, and all of the values ​​were greater than 3 eV. This result indicates that the solid electrolytes obtained in the examples had low electronic conductivity (high electronic insulation).

[0085] Example 101: The effect of carrier concentration in a solid electrolyte on ionic conduction was investigated by substituting Zr for Na. 1+x Ta 1-x Zr x Cl 6 was synthesized and verified. 1+x Ta 1-x Zr x Cl 6 are NaCl and TaCl 5 , ZrCl 4The powder was synthesized by a mechanochemical method using the reagents. Specifically, the above powder reagents, weighed in the stoichiometric ratio, were filled into an 80 mL planetary ball mill cup made of zirconia together with Zr milling media, and mechanochemical synthesis was carried out using a Fritsche planetary ball mill P-7 at 500 rpm for 33 hours. During this process, the mechanical mixing of the ball mill was repeated 198 times for 10 minutes at 10-minute intervals to avoid the inside of the ball mill becoming too hot. The obtained powder was collected in a glove box, and its properties were verified by X-ray diffraction and impedance measurement (Figure 16). Note that Na 1+x Ta 1-x Zr x Cl 6 is NaTaCl in the range of x < 1.0 6 This indicates that the material has a similar crystal structure to that of the material shown in Figure 17, and that the amount of Na in the crystal structure can be modulated. As shown in Figure 17, it was found that higher ionic conductivity can be achieved when a trace amount of Zr is included. This result indicates that adjusting the amount of Na affects ionic conductivity, suggesting that increasing the amount of Na ions strengthens the electrostatic repulsion between conductive ions, thereby improving Na ion conduction.

[0086] (Test Example 1: NaTa 1/5(3+2x) O x Cl 4 Preparation of NaTa shown in the table below 1/5(3+2x) O x Cl 4 , NaCl, TaCl 5 and Ta 2 O 5 The compound was synthesized by a mechanochemical method using the reagents. Specifically, the above powder reagents, weighed in the stoichiometric ratio, were filled into an 80 mL planetary ball mill cup made of zirconia together with Zr milling media, and mechanochemical synthesis was carried out using a Fritsche Planetary Ball Mill P-7 at 600 rpm for 100 hours. During this process, the mechanical mixing of the ball mill was repeated 600 times, with 10-minute operations every 10 minutes, to avoid the inside of the ball mill becoming too hot. The obtained powder was collected in a glove box, and its properties were verified by X-ray diffraction and impedance measurement.

[0087]

[0088] Ta as an oxygen source 2 O 5 Using Ta 2 O 5 The remaining phases were largely amorphous (Fig. 18). Although it was shown that not all of the introduced oxygen was used, a significant improvement in conductivity was confirmed by increasing the amount of introduced oxygen (Figs. 19(a) and (b)).

[0089] (Test Example 2: Na 1+x TaOCl 4+x Preparation of Na shown in the table below 1+x TaOCl 4+x , NaCl, TaCl 5 and Ta 2 O 5 The compound was synthesized by a mechanochemical method using the reagents. Specifically, the above powder reagents, weighed in the stoichiometric ratio, were filled into an 80 mL planetary ball mill cup made of zirconia together with Zr milling media, and mechanochemical synthesis was carried out using a Fritsche Planetary Ball Mill P-7 at 600 rpm for 100 hours. During this process, the mechanical mixing of the ball mill was repeated 600 times, with 10-minute operations every 10 minutes, to avoid the inside of the ball mill becoming too hot. The obtained powder was collected in a glove box, and its properties were verified by X-ray diffraction and impedance measurement.

[0090]

[0091] The effect of varying the amount of NaCl on conductivity was investigated, but there was almost no effect, and it was possible to synthesize materials with conductivity exceeding 1 mS / cm in all cases (Figures 20 and 21).

[0092] (Test Example 3: NaTaOCl 4 Preparation of NaCl, TaCl 5 and Ta 2 O 5The reagents were synthesized by a mechanochemical method using a mass ratio of 5:3:1. Specifically, the weighed powder reagents were filled into an 80 mL planetary ball mill cup made of zirconia together with Zr milling media, and mechanochemical synthesis was carried out using a Fritsche planetary ball mill P-7 at 600 rpm for 25 hours, 50 hours, 75 hours, and 100 hours, respectively. At this time, the mechanical mixing of the ball mill was repeated 150, 300, 450, and 600 times, with 10-minute operations every 10 minutes to avoid the inside of the ball mill becoming too hot. The powder obtained at each synthesis time was collected in a glove box, and its properties were verified by X-ray diffraction and impedance measurement.

[0093] As a result, it was found that the conductivity improved with an extension of the processing time, but that the conductivity did not change significantly even with a relatively short milling time of about 25 hours (Figures 22 and 23).

[0094] (Test Example 4: Na 2x TaO x Cl 5 Preparation of Na shown in the table below 2x TaO x Cl 5 Na 2 O and TaCl 5 The compound was synthesized by a mechanochemical method using the reagents. Specifically, the above powder reagents, weighed in the stoichiometric ratio, were filled into an 80 mL planetary ball mill cup made of zirconia together with Zr milling media, and mechanochemical synthesis was carried out using a Fritsche Planetary Ball Mill P-7 at 600 rpm for 100 hours. During this process, the mechanical mixing of the ball mill was repeated 600 times, with 10-minute operations every 10 minutes, to avoid the inside of the ball mill becoming too hot. The obtained powder was collected in a glove box, and its properties were verified by X-ray diffraction and impedance measurement.

[0095]

[0096] The precursor reagent was Ta 2 O 5 From Na 2By changing the cation exchange rate to O, we succeeded in synthesizing a more homogeneous glass. It is believed that the use of a precursor reagent that is highly reactive and soft, with mechanical properties similar to those of other precursors, is required for the synthesis of a homogeneous compound. This resulted in the reproducibility of a high conductivity of 3.7 mS / cm (Figures 24 and 25(a) and (b)).

Claims

1. A solid electrolyte containing a compound represented by formula (1) or formula (2). Formula (1) Na 3a+2b+1c M 1 a M 2 b M 3 c Ch α X 6-2α (In formula (1), M 1 is selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof; M 2 is selected from the group consisting of Zr, Hf, Ti, Si, Ge, Sn, and combinations thereof; M 3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi, and combinations thereof; Ch is selected from the group consisting of O, S, Se, Te, and combinations thereof; X is selected from the group consisting of F, Cl, Br, I, and combinations thereof; a + b + c = 1, 0 ≦ a ≦ 1, 0 ≦ b ≦ 1, 0 ≦ c ≦ 1, 0.1 ≦ α ≦ 2.9.) Formula (2) Na 3a+2b+1c M 1 a M 2 b M 3 c X 6 (In formula (2), M 1 is selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and combinations thereof; M 2 is selected from the group consisting of Zr, Hf, Ti, Si, Ge, Sn, and combinations thereof; M 3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi, and combinations thereof; X is selected from the group consisting of F, Cl, Br, I, and combinations thereof; a + b + c = 1, 0 ≦ a ≦ 0.9, 0 ≦ b ≦ 0.9, 0.1 ≦ c ≦ 1.) 2. In formula (2), M 3 is selected from the group consisting of Ta and Nb, the solid electrolyte according to claim 1.

3. The solid electrolyte according to claim 1, wherein X is Cl in formula (1).

4. The solid electrolyte according to claim 1, wherein X is Cl in formula (2).

5. When compression molding is performed at room temperature and under a pressure of 170 MPa, the sodium ion conductivity at 25 °C is 1 × 10 -6 S / cm or more, and the solid electrolyte according to claim 1.

6. The solid electrolyte according to claim 1, having a relative density of 80% or more when compression-molded at room temperature and under a pressure of 170 MPa.

7. A solid electrolyte containing a compound represented by the formula (1'). The formula (1'): Na3a + 2b + 1c - γ + δM 1 a M 2 b M 3 c Ch ε X ζ (In the formula (1'), M 1 is selected from the group consisting of Y, Sc, Al, Ga, In, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu and combinations thereof, M 2 is selected from the group consisting of Zr, Hf, Ti, Si, Ge, Sn and combinations thereof, M 3 is selected from the group consisting of Nb, Ta, V, P, Sb, Bi and combinations thereof, Ch is selected from the group consisting of O, S, Se, Te and combinations thereof, X is selected from the group consisting of F, Cl, Br, I and combinations thereof, a + b + c = 1, 0 ≦ a ≦ 1, 0 ≦ b ≦ 1, 0 ≦ c ≦ 1, 0 ≦ γ < ≦ 1, 0 ≦ δ ≦ 2, 0 ≦ ε ≦ 2 and 4 ≦ ζ ≦ 8.) 8. The solid electrolyte according to claim 7, wherein X is Cl in formula (1').

9. When compression molding is carried out at room temperature and under a pressure of 170 MPa, the sodium ion conductivity at 25 °C is 1 × 10 -6 S / cm or more, and the solid electrolyte according to claim 7.

10. The solid electrolyte according to claim 7, having a relative density of 80% or more when compression-molded at room temperature and under a pressure of 170 MPa.

11. A solid electrolyte layer containing the solid electrolyte according to any one of claims 1 to 10.

12. A solid electrolyte battery comprising the solid electrolyte layer according to claim 11.

Citation Information

Patent Citations

  • Solid electrolytes for sodium batteries.

    JP2021510905A

  • Solid electrolytes for all solid state rechargeable lithium battery, methods for manufacturing the same, and all solid state rechargeable lithium battery including the same

    KR1020170112033A

  • Chlorine-Based Sodium Solid Electrolyte

    US20230115956A1

Cited By

  • Solid electrolyte, electrode, and secondary battery

    WO2026071004A1

  • Solid electrolyte, electrochemical device, and sodium battery

    WO2026204865A1