Method for manufacturing anion exchange membrane water electrolysis system
The use of NiMo-based alloy catalysts with specific molar ratios and activation conditions in anion exchange membrane water electrolysis systems addresses the low catalytic activity and durability issues, enhancing efficiency and stability, and reducing costs by achieving performance comparable to platinum catalysts.
Patent Information
- Application Number
- PCT/KR2024/005474
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-04-23
- Publication Date
- 2024-11-21
AI Technical Summary
Current anion exchange membrane water electrolysis systems face challenges with low catalytic activity and durability of non-platinum catalysts, leading to inefficient hydrogen production and increased costs due to the use of platinum-based catalysts in cation exchange membrane systems, and issues with alkaline electrolyte leakage and resistance in alkaline electrolysis.
A method for manufacturing an anion exchange membrane water electrolysis system using NiMo-based alloy catalysts with a molar ratio of Ni to Mo between 6:1 to 101:1 and an oxidation number of Mo as 5+ or 6+, activated by applying a current at 25 to 200 mA/cm² and maintaining at 50 to 60°C for 90 to 360 minutes, which enhances catalytic activity and durability.
The method produces an anion exchange membrane water electrolysis system with improved durability and efficiency, achieving water electrolysis performance comparable to platinum catalysts while reducing long-term performance degradation and Mo loss, thus lowering costs and increasing system stability.
Smart Images

Figure KR2024005474_21112024_PF_FP_ABST
Abstract
Description
Manufacturing method of an anion exchange membrane water electrolysis system
[0001] Cross-citation with related application(s)
[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0061678, filed May 12, 2023, the entire contents of which are incorporated herein by reference.
[0003] The present invention relates to a method for manufacturing an anion exchange membrane electrolysis system that exhibits excellent electrolysis performance, as well as improved durability and efficiency.
[0004]
[0005] The importance of technology that can produce hydrogen, a next-generation energy source that can solve fossil fuel depletion and environmental pollution, in an environmentally friendly manner is being highlighted.
[0006] Accordingly, active research is being conducted on water electrolysis technologies using electrolysis. Representative water electrolysis technologies include proton exchange membrane water electrolysis (PEMWE), anion exchange membrane water electrolysis (AEMWE), and alkaline water electrolysis (AWE).
[0007] In alkaline electrolysis, nickel-based oxides and cobalt-based oxides are commonly used as reduction and oxidation electrode catalysts, respectively, and an alkaline aqueous solution such as KOH is used as the electrolyte. Alkaline electrolysis has the advantages of not requiring precious metal catalysts and operating at relatively low temperatures. However, it suffers from low hydrogen production rates and the large size of the design system for hydrogen production. Furthermore, liquid alkaline electrolytes are prone to leakage, which increases resistance, reduces current density, and ultimately reduces electrolysis efficiency.
[0008] Meanwhile, cation exchange membrane electrolysis (CEM) is a water electrolysis system that uses a solid electrolyte membrane, such as Nafion, instead of a liquid electrolyte. Because the volume occupied by the solid electrolyte membrane is smaller than that of a liquid electrolyte, the system can be reduced in size and provide high current density. However, because it operates in an acidic environment, platinum-based catalysts, such as IrO2 and Pt, that can withstand the strong corrosiveness of acidic environments are required for the reduction and oxidation electrode catalyst materials. The use of expensive PEM catalysts increases the cost of hydrogen production, posing a significant obstacle to the commercialization of CEM.
[0009] In contrast, anion exchange membrane electrolysis utilizes the advantages of existing systems while overcoming their shortcomings. Because it operates in an alkaline environment, it can utilize non-platinum metals as catalysts, achieving a satisfactory energy density in a compact system. However, non-platinum metal catalysts exhibit lower catalytic activity than platinum metal catalysts, resulting in lower electrolysis efficiency.
[0010] Accordingly, research and development are being conducted on catalysts and anion exchange membrane electrolysis systems that can improve electrolysis efficiency by exhibiting superior catalytic activity. Research on catalysts is primarily focused on applying previously developed alkaline half-cell catalysts to anion exchange membrane systems. However, these applied catalysts still suffer from low catalytic activity and deteriorated durability.
[0011]
[0012] The present invention aims to solve the problems of the prior art as described above and provide a method for manufacturing an anion exchange membrane electrolysis system that exhibits excellent electrolysis performance along with improved durability and efficiency.
[0013] The present invention also seeks to provide an anion exchange membrane electrolysis system manufactured by the above manufacturing method.
[0014] The present invention also seeks to provide an activation method capable of improving the performance of an anion exchange membrane electrolysis system.
[0015]
[0016] A method for manufacturing an anion exchange membrane electrolysis system according to one embodiment of the present invention is as follows:
[0017] A step of manufacturing a preliminary reduction electrode and an oxidation electrode, respectively;
[0018] A step of manufacturing a preliminary membrane-electrode assembly by interposing an anion exchange membrane between the preliminary reduction electrode and the oxidation electrode; and
[0019] A step of supplying an alkaline aqueous solution to the preliminary membrane-electrode assembly and activating the preliminary reduction electrode;
[0020] The above preliminary reduction electrode comprises NiMo alloy particles in which the molar ratio of Ni and Mo is 1:1 to 6:1 and the oxidation number of Mo is 4+, 5+ or 6+,
[0021] The above activation is performed by applying a current at a current density of 25 to 200 mA / ㎠ and maintaining it at 50 to 60°C for 90 to 360 minutes.
[0022] In addition, an anion exchange membrane electrolysis system according to another embodiment of the present invention is manufactured by the method for manufacturing the anion exchange membrane electrolysis system described above, and includes a reduction electrode including a particulate NiMo-based alloy catalyst; an oxidation electrode; an anion exchange membrane interposed between the reduction electrode and the oxidation electrode; and an alkaline aqueous solution; wherein the NiMo-based alloy catalyst includes Ni and Mo in a molar ratio of 6:1 to 101:1, and the oxidation number of Mo is 5+ or 6+.
[0023] According to another embodiment of the present invention, a method for activating an anion exchange membrane electrolysis system includes a preliminary reduction electrode, an oxidation electrode, and an anion exchange membrane interposed between the preliminary reduction electrode and the oxidation electrode, wherein the preliminary reduction electrode includes NiMo-based alloy particles containing Ni and Mo in a molar ratio of 1:1 to 6:1 and wherein Mo has an oxidation number of 4+, 5+, or 6+, and the step of activating the preliminary reduction electrode includes supplying an alkaline aqueous solution to the preliminary anion exchange membrane electrolysis system, applying a current at a current density of 25 to 200 mA / cm2, and maintaining the current at 50 to 60°C for 90 to 360 minutes.
[0024]
[0025] The manufacturing method according to the present invention enables the manufacture of an anion exchange membrane electrolysis system exhibiting improved durability and efficiency along with excellent electrolysis performance.
[0026]
[0027] Figure 1a is Ni 24 This is a graph showing the adsorption energies of H2O, MoO2, and H2O / MoO2 clusters on the surface of a Mo4 alloy, and Fig. 1b is a graph showing the adsorption energies according to the adsorption site of the hydrogen intermediate H*.
[0028] Figure 2 is a schematic diagram schematically showing the hydrogen production reaction mechanism of NiMo alloy in an alkaline atmosphere.
[0029] FIG. 3 is a schematic diagram of an anion exchange membrane electrolysis system including an alkaline aqueous solution circulation device of a dual feeding type according to one embodiment of the present invention.
[0030] FIG. 4 is a schematic diagram of an anion exchange membrane electrolysis system including an alkaline aqueous solution circulation device of a both feeding method according to another embodiment of the present invention.
[0031] FIG. 5 is a schematic diagram of an anion exchange membrane electrolysis system including an alkaline aqueous solution circulation device of an anode feeding type according to another embodiment of the present invention.
[0032] Figures 6a to 6d are graphs showing the BET analysis results for NiMo-based alloy particles of Manufacturing Examples 1, 2, 3, and 4, respectively.
[0033] Figure 7 is a graph showing the results of evaluating the activity change for the hydrogen evolution reaction according to the molar ratio of Ni and Mo in a NiMo alloy using linear scanning potential (LSV).
[0034] Figure 8 is a graph showing the results of analyzing the initial oxidation number of Mo in the NiMo alloys of Manufacturing Examples 1 to 4 using X-ray photoelectron spectroscopy (XPS).
[0035] Figure 9 is a graph showing the results of XPS analysis of the change in Mo oxidation number in the Ni3Mo alloy before and after activation.
[0036] Figure 10 is a graph showing the results of observing the change in current according to voltage control in an anion exchange membrane electrolysis system activated by increasing and decreasing the applied voltage.
[0037] Figure 11 is a graph showing the results of observing the change in current according to voltage control in an anion exchange membrane electrolysis system activated by applying current at a constant current density and maintaining it for a constant period of time.
[0038] Figure 12 shows the current density of 25 mA / cm 2 , 50 mA / cm 2 , 100 mA / cm 2 and 200 mA / cm 2 This is a graph showing the polarization evaluation results for each activated anion exchange membrane electrolysis system under the conditions.
[0039] Figure 13 shows the current density of 25 mA / cm 2 , 50 mA / cm 2 , 100 mA / cm 2 and 200 mA / cm 2 This is a graph showing the durability evaluation results for each activated anion exchange membrane electrolysis system under the conditions.
[0040] Figure 14 is a phase diagram of Mo according to pH, disclosed in the literature "Anatolyevich, Pavel. "The Revised Pourbaix Diagram for Molybdenum." HMo 2.10: 3."
[0041] Figure 15 shows the current density of 25 mA / cm 2 , 50 mA / cm 2 , 100 mA / cm 2 and 200 mA / cm 2 This is a graph showing the results of analyzing the Mo residual amount in an anion exchange membrane electrolysis system activated under each condition using X-ray fluorescence analysis (XRF).
[0042] Figure 16 is a graph showing the results of evaluating the effect of activation time on the performance development of NiMo alloys.
[0043] Figure 17 is a graph showing the polarization evaluation results of an anion exchange membrane electrolysis system according to an alkaline aqueous solution circulation method.
[0044] Figure 18 is a graph showing the results of a durability evaluation of an anion exchange membrane electrolysis system.
[0045]
[0046] In the present invention, terms such as first, second, etc. are used to describe various components, and the terms are used only for the purpose of distinguishing one component from another.
[0047] Furthermore, the terminology used herein is merely for the purpose of describing exemplary embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this specification, it should be understood that the terms "comprise," "include," or "have" indicate the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0048] Additionally, in the present invention, when each layer or element is referred to as being formed “on” or “over” each layer or element, it means that each layer or element is formed directly on each layer or element, or that other layers or elements may be additionally formed between each layer, on the object, or on the substrate.
[0049] Also, in the present invention, “reduction electrode,” “membrane-electrode assembly,” and “anion exchange membrane electrolysis system” mean a reduction electrode, a membrane-electrode assembly, and anion exchange membrane electrolysis system after activation, respectively, and “preliminary reduction electrode,” “preliminary membrane-electrode assembly,” and “preliminary anion exchange membrane electrolysis system” mean a reduction electrode, a membrane-electrode assembly, and anion exchange membrane electrolysis system before activation, respectively.
[0050] Also, “NiMo alloy particles” are alloy particles before activation used in the manufacture of a preliminary reduction electrode, and “NiMo alloy catalyst” or “NiMo alloy catalyst in particle form” means alloy particles after activation.
[0051] The present invention is susceptible to various modifications and takes various forms. Specific embodiments are illustrated and described in detail below. However, this is not intended to limit the present invention to specific disclosed forms, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.
[0052] Hereinafter, a method for manufacturing an anion exchange membrane electrolysis system according to embodiments of the invention, an anion exchange membrane electrolysis system manufactured thereby, and an activation method capable of improving the performance of an anion exchange membrane electrolysis system will be described in detail.
[0053]
[0054] A method for manufacturing an anion exchange membrane electrolysis system according to one embodiment of the present invention is
[0055] Step 1 for manufacturing a preliminary reduction electrode and an oxidation electrode, respectively;
[0056] A step (step 2) of manufacturing a preliminary membrane-electrode assembly by interposing an anion exchange membrane between the preliminary reduction electrode and the oxidation electrode; and
[0057] A step (step 3) of supplying an alkaline aqueous solution into the preliminary membrane-electrode assembly and activating the preliminary reduction electrode;
[0058] At this time, the preliminary reduction electrode includes NiMo-based alloy particles, the NiMo-based alloy particles include Ni and Mo in a molar ratio of 1:1 to 6:1, and the oxidation number of Mo is 4+, 5+, or 6+.
[0059] The above activation is performed by applying a current at a current density of 25 to 200 mA / ㎠ and maintaining it at 50 to 60°C for 90 to 360 minutes.
[0060] As a result of activation of the above-described preliminary reduction electrode, a reduction electrode is manufactured. The reduction electrode comprises a particulate NiMo-based alloy catalyst derived from the NiMo-based alloy particles, wherein the NiMo-based alloy catalyst comprises Ni and Mo in a molar ratio of 6:1 to 101:1, and the oxidation number of Mo is 5+ or 6+.
[0061] The present inventors have discovered a problem in that, in the case of a NiMo-based alloy catalyst developed as a conventional non-platinum catalyst for anion exchange membrane electrolysis, Mo is lost in an alkaline atmosphere when the anion exchange membrane electrolysis system is operated, resulting in a decrease in electrolysis performance. By elucidating the performance expression mechanism of the NiMo-based alloy, the molar ratio and oxidation number of the NiMo alloy, the activation method of the electrolysis system, and further, the electrolyte supply method are controlled and optimized, thereby confirming that the manufactured anion exchange membrane electrolysis system can exhibit excellent electrolysis performance at the level of a platinum catalyst even though it includes a non-platinum catalyst, and furthermore, the durability and efficiency of the anion exchange membrane electrolysis system are improved, so that performance decrease is small even after long-term operation, and thus the present invention has been completed.
[0062] Specifically, NiMo-based alloy particles containing Ni and Mo in various molar ratios were manufactured, and a pre-reduction electrode and a pre-anion exchange membrane electrolysis system containing the same were manufactured, activated, and cell performance was confirmed. As a result, it was confirmed that a significant loss of Mo in the NiMo-based alloy occurred in an alkaline atmosphere when the electrolysis system was operated, and accordingly, the molar ratio of Ni and Mo in the alloy and the oxidation number of Mo were changed.
[0063] Afterwards, the mechanism for Mo loss was elucidated through thermodynamic calculations. Specifically, Ni 24 When calculating the energy required for the loss of individual Mo atoms from a Mo8 alloy, all of the energy shifts toward stabilization (see Table 3 in Experimental Example 3 below). Furthermore, computational chemistry confirmed that the NiMo alloy is stable in an alkaline environment when all Mo atoms present on the surface are lost.
[0064] Figure 1a is Ni 24 This is a graph showing the adsorption energies of H2O, MoO2, and H2O / MoO2 clusters on the surface of a Mo4 alloy, and Fig. 1b is a graph showing the adsorption energies according to the adsorption site of the hydrogen intermediate H*.
[0065] Through the adsorption energy calculation in Fig. 1a, it was confirmed that the Mo lost during the activation of the water electrolysis system adsorbs water and exists in the form of H2O / MoO2 clusters. In addition, from the adsorption energy calculation results according to the adsorption site in Fig. 1b, it was confirmed that the intermediate product, hydrogen, is more stable when adsorbed on the Ni side than on the Mo site. From these results, it is possible to predict the mechanism by which H2O / MoO2 clusters are adsorbed on the Ni surface, and after water decomposition, hydrogen moves to the Ni surface to generate hydrogen.
[0066] Figure 2 is a schematic diagram schematically illustrating the hydrogen production reaction mechanism of a NiMo alloy, specifically a Ni3Mo alloy, in an alkaline atmosphere. Figure 2 is merely an example for explaining the present invention, and the present invention is not limited thereto.
[0067] Referring to Fig. 2, the hydrogen production reaction of a NiMo alloy in an alkaline atmosphere consists of the following mechanisms: (1) loss of all Mo on the surface of the NiMo alloy, (2) formation of Mo oxide of the lost Mo, (3) re-adsorption on the bare Ni surface in the form of H2O / Mo oxide, (4) dissociation reaction of water and adsorption of hydrogen intermediate H* at Ni site (dual active site), and (5) H2 production by Heyrovsky or Tafel reaction.
[0068] Therefore, the structure of a NiMo alloy catalyst that is stable and highly active in an alkaline atmosphere is a structure in which the catalyst surface is composed of Ni, Mo is dissolved to become MoO2, and then is adsorbed on the Ni surface in a state of forming H2O and H2O / Mo oxide clusters. In addition, the molar ratio of Ni and Mo in the alloy catalyst is 6:1 to 101:1, and the oxidation number of Mo is 5+ or 6+.
[0069] When the above molar ratio conditions are satisfied, only Mo on the surface of the NiMo alloy is selectively dissolved, and the Mo oxide generated thereafter forms clusters with water and can be sufficiently adsorbed on the Ni surface. If only Mo exists on the surface of the alloy catalyst as in the past, it is difficult to control the molar ratio of Ni and Mo and the oxidation number of Mo to satisfy the above conditions.
[0070] The present invention is based on the performance expression mechanism of the NiMo alloy identified above, and implements a NiMo alloy catalyst structure that is stable and exhibits high activity by controlling and optimizing the molar ratio of Ni and Mo in the NiMo alloy, the oxidation number of Mo, the activation method of the water electrolysis system, and further the electrolyte supply method.
[0071] Accordingly, the reduction electrode in the anion exchange membrane electrolysis system manufactured by the method for manufacturing the anion exchange membrane electrolysis system according to the present invention includes a NiMo-based alloy catalyst having a structure that is stable and exhibits high activity.
[0072] Specifically, an anion exchange membrane electrolysis system manufactured by the method for manufacturing an anion exchange membrane electrolysis system according to the present invention comprises: a reduction electrode including a particulate NiMo-based alloy catalyst; an oxidation electrode; an anion exchange membrane interposed between the reduction electrode and the oxidation electrode; and an alkaline aqueous solution; wherein the NiMo-based alloy catalyst includes Ni and Mo in a molar ratio of 6:1 to 101:1, and the oxidation number of Mo is 5+ or 6+.
[0073] In the present invention, the molar ratio of Ni and Mo in the NiMo alloy catalyst can be determined through XRF analysis. The specific analysis method and conditions are as described in the experimental examples below.
[0074] Additionally, the oxidation number of Mo in the NiMo alloy catalyst can be determined through XPS analysis. The specific analysis method and conditions are as described in the experimental examples below.
[0075] In addition, the NiMo-based alloy catalyst includes a Ni layer on the surface.
[0076] The above Ni layer is formed due to loss of Mo from the surface of the NiMo alloy particles during the activation process.
[0077] Meanwhile, the loss rate of each element in the NiMo alloy before and after activation can be confirmed through XRF analysis of the alloy. The specific analysis method and conditions are described in the experimental examples below.
[0078] In addition, the NiMo-based alloy catalyst is manufactured from NiMo-based alloy particles, and the NiMo-based alloy particles may be manufactured by a powder method using a co-precipitation reaction. Accordingly, the NiMo-based alloy catalyst has a particle form (powder), and has a relatively small average particle diameter and a large specific surface area compared to NiMo-based alloys manufactured by conventional methods such as electroplating or deposition.
[0079] In addition, the NiMo-based alloy catalyst is a porous particle having multiple pores within the particle.
[0080] Furthermore, when manufacturing electrodes using conventional alloy catalysts having an average particle size in the nanometer range, the specific surface area of the manufactured electrodes was not large because the catalyst layer was formed on the electrode substrate through electroplating or deposition. On the other hand, in the present invention, a particulate alloy is dispersed in a solvent to manufacture a slurry for forming a preliminary reduction electrode, which is then applied to a release film, dried, and separated to manufacture a catalyst layer, which is then used as a reduction electrode itself. Accordingly, the manufactured reduction electrode has a larger specific surface area than the conventional one, and as a result, can exhibit excellent catalytic activity.
[0081] In addition, the NiMo alloy catalyst is 1.0 mg / cm in the reduction electrode. 2 It can be included with high loading amounts above.
[0082] Meanwhile, the anion exchange membrane electrolysis system according to the present invention includes a membrane electrode assembly (MEA) comprising a reduction electrode (cathode) including the above-described particulate NiMo-based alloy catalyst, an oxidation electrode (anode), and an anion exchange membrane interposed between the reduction electrode and the oxidation electrode, as a unit cell.
[0083] The above anion exchange membrane electrolysis system may include a plurality of membrane-electrode assemblies, and the number of membrane-electrode assemblies may be appropriately determined depending on the performance required for the electrolysis system.
[0084] The above plurality of membrane-electrode assemblies are connected and stacked to form a stack.
[0085] Accordingly, the anion exchange membrane electrolysis system includes a plurality of the above membrane-electrode assemblies, and includes a stack that electrolyzes an alkaline aqueous solution to generate hydrogen and oxygen, and may further optionally include an alkaline aqueous solution circulation device that supplies the alkaline aqueous solution to the stack, a generated gas discharge device for discharging oxygen and hydrogen generated within the stack, and a power supply device that applies and controls voltage and current to the stack.
[0086] In the above membrane-electrode assembly, a hydrogen evolution reaction (HER) occurs at the reduction electrode by a reduction catalyst, resulting in the production of hydrogen (H2) and hydroxide ions (OH-). At this time, the above-described particulate NiMo-based alloy catalyst is included as the reduction catalyst.
[0087] Typically, the electrodes of a water electrolysis system include a catalyst layer containing a catalyst and an electrode substrate for supporting the catalyst layer, but the reduction electrode of the present invention does not include an electrode substrate and is composed only of a catalyst layer containing the NiMo-based alloy catalyst.
[0088] Meanwhile, the oxidation electrode causes an oxygen evolution reaction (OER) by an oxidation catalyst, and hydroxide ions generated at the reduction electrode and diffused through the anion exchange membrane are oxidized to produce water and oxygen.
[0089] As the above oxidation catalyst, at least one selected from the group consisting of Ni, NiCoFe, Ir, and NiFe-layered double hydroxide (LDH) can be used.
[0090] The above oxidation electrode may further include an electrode substrate for supporting the catalyst layer together with a catalyst layer including the oxidation catalyst. The electrode substrate is a conductive porous body.
[0091] The above oxidation electrode can be manufactured according to a conventional method, and for example, the oxidation electrode can be manufactured by a manufacturing method including a step of applying a slurry for forming an oxidation electrode, including an oxidation catalyst, a binder, and a solvent, onto a release film, drying it, and then separating it from the release film, or can be manufactured by a manufacturing method including a step of applying, plating, or depositing an oxidation catalyst on an electrode substrate.
[0092] In addition, the anion exchange membrane plays a role in moving OH- ions from the reduction electrode to the oxidation electrode. As the anion exchange membrane, any membrane commonly used in anion exchange membrane water electrolysis systems, such as Trimethyl ammonium functionalized polystyrenes, can be used without any particular restrictions. It can also be obtained commercially and used, and in this case, an example is Sustainion™ X37-50 grade RT anion exchange membrane from Sustainion.
[0093] In addition, the membrane-electrode assembly may optionally further include a gasket that seals and fixes the edges of the membrane-electrode assembly together with the oxidation electrode, reduction electrode, and anion exchange membrane.
[0094] A plurality of membrane-electrode assemblies having the above structure are connected in series and stacked to form a stack.
[0095] In addition, in the anion exchange membrane electrolysis system, the stack may further include, together with the membrane-electrode assembly, at least one of a porous transport layer and a separator (or bipolar plate).
[0096] The porous transport layer is located on the electrode side that does not come into contact with the anion exchange membrane in the membrane-electrode assembly, and serves to conduct electricity, move the alkaline aqueous solution to the electrode, and also discharge the generated gas to the outside. The porous transport layer may be located on either the reduction electrode or the oxidation electrode, or on both. Nickel foam may be used as the porous transport layer for the reduction electrode, which is located on the reduction electrode side. Carbon paper may be used as the porous transport layer for the oxidation electrode, which is located on the oxidation electrode side.
[0097] In addition, the separator plates are located on both sides of the membrane-electrode assembly and serve to support and connect two adjacent membrane-electrode assemblies in series.
[0098] In addition, the separator is a metal plate such as nickel, and thus can conduct electricity applied from a power supply. Furthermore, a flow path is formed on the separator, allowing the alkaline solution supplied from the alkaline solution circulation device to be transported to the porous transport layer. Furthermore, the separator can discharge generated gas to the outside and transfer heat generated by the reaction.
[0099] In addition, the anion exchange membrane electrolysis system according to the present invention may further include an alkaline solution circulation device that supplies and discharges an alkaline solution to the stack.
[0100] The above alkaline aqueous solution may contain one or more types of alkali metal hydroxides, such as potassium hydroxide and sodium hydroxide. More specifically, the alkaline aqueous solution may contain the alkali metal hydroxides at a concentration of 0.1 M to 1 M. Even more specifically, the alkaline aqueous solution may be a potassium hydroxide aqueous solution at a concentration of 0.1 M to 1 M.
[0101] The above alkaline aqueous solution circulation device may further include a tank specifically for storing the alkaline aqueous solution, a temperature control device for controlling the temperature through heat supply to the water electrolysis system, and a flow control device such as a pump for controlling the supply flow rate of the alkaline aqueous solution to keep it constant.
[0102] Additionally, one or more of the alkaline aqueous solution circulation devices may be included in the water electrolysis system.
[0103] The above alkaline solution circulation device can be classified into a both feeding method, an anode feeding method, and a dual feeding method according to the supply method of the alkaline solution. Specifically, the both feeding method is a method in which an alkaline solution is supplied to both an oxidation electrode and a reduction electrode from one alkaline solution circulation device, and one alkaline solution circulation device is included in the anion exchange membrane electrolysis system. The alkaline nucleus circulation device of the above-mentioned boss feeding method is connected to both the oxidation electrode and the reduction electrode, and supplies the alkaline solution to both the oxidation electrode and the reduction electrode. In addition, the anode feeding method is a method in which an alkaline solution is supplied to the oxidation electrode, and in this case, one alkaline solution circulation device is included in the electrolysis system. The alkaline solution circulation device of the above-mentioned anode feeding method is connected to the oxidation electrode, and supplies the alkaline solution to the oxidation electrode. Meanwhile, the dual feeding method is a method of supplying an alkaline solution to each electrode from an alkaline solution circulation device equipped for each of the oxidation electrode and reduction electrode, and the alkaline solution circulation device of the dual feeding method is composed of an alkaline solution circulation device for the oxidation electrode and an alkaline solution circulation device for the reduction electrode, which are respectively connected to the oxidation electrode and reduction electrode.
[0104] FIG. 3 is a schematic diagram showing an anion exchange membrane electrolysis system including a dual-feeding type alkaline aqueous solution circulation device according to one embodiment of the present invention, FIG. 4 is a schematic diagram showing an anion exchange membrane electrolysis system including a boss-feeding type alkaline aqueous solution circulation device according to another embodiment of the present invention, and FIG. 5 is a schematic diagram showing an anion exchange membrane electrolysis system including an anode-feeding type alkaline aqueous solution circulation device according to still another embodiment of the present invention. FIGS. 3 to 5 are merely examples for explaining the present invention, and the present invention is not limited thereto.
[0105] Meanwhile, the circulation method of alkaline aqueous solution in an anion exchange membrane electrolysis system affects the Mo loss and the performance, especially durability, of the anion exchange membrane electrolysis system.
[0106] Specifically, the boss feeding method involves the simultaneous dissolution of Mo by direct contact of the NiMo alloy particles with an alkaline solution, and the dissolution of Mo by anionization and migration to the reduction electrode. In contrast, the anode feeding method does not involve direct contact of the NiMo alloy particles with an alkaline solution. Therefore, the anode feeding method exhibits a lower Mo loss rate than the boss feeding method.
[0107] In addition, in terms of the performance of the electrolysis system, hydrogen can be produced at a lower voltage when using a dual feeding method in which two alkaline solution circulation devices supply alkaline solution to the oxidation electrode and reduction electrode, respectively, than when using a boss feeding method in which one alkaline solution circulation device supplies alkaline solution to both the oxidation electrode and reduction electrode.
[0108] In addition, the anion exchange membrane electrolysis system according to the present invention may further include a generated gas discharge device and a power supply device together with the above-described stack and alkaline aqueous solution circulation device.
[0109] In addition, the above-mentioned generated gas discharge device is connected to the discharge port of the alkaline aqueous solution circulation device, so that the gas generated within the electrolysis system can be discharged mixed with the alkaline aqueous solution or discharged independently. In addition, the above-mentioned generated gas discharge device can remove gas at atmospheric pressure (1±0.1) and can pressurize by controlling the flow rate.
[0110] The above-mentioned generated gas discharge device may include a generated gas discharge system for an oxidation electrode (or a generated gas discharge unit for an oxidation electrode) for discharging oxygen generated at an oxidation electrode of an anion exchange membrane electrolysis system, and a generated gas discharge system for a reduction electrode (or a generated gas discharge unit for a reduction electrode) for discharging hydrogen generated at a reduction electrode.
[0111] In addition, the power supply outputs the voltage required for electrolysis to the stack of the anion exchange membrane electrolysis system, specifically, the oxidation electrode and the reduction electrode, and also controls the current and voltage within the system by consuming and removing the residual voltage within the stack.
[0112] Accordingly, when an alkaline aqueous solution is supplied from the alkaline electrolyte circulation device to the anion exchange membrane, and a direct current voltage is applied to the oxidation electrode and reduction electrode from the power supply, hydroxide ions (OH) which are decomposition products of the alkaline aqueous solution in the anion exchange membrane - ) is oxidized by an oxidation catalyst on the surface of the oxidation electrode to generate oxygen, water, and electrons, and the electrons move to the reduction electrode along the external conductor, and then the electrons and water react catalytically on the surface of the reduction electrode to generate hydrogen and hydroxide ions (OH - ) is generated. The oxygen generated at the oxidation electrode and the hydrogen generated at the reduction electrode are discharged out of the anion exchange membrane electrolysis system through the generation gas discharge system for the oxidation electrode and the generation gas discharge system for the reduction electrode, respectively.
[0113] The anion exchange membrane electrolysis system according to the present invention having the above-described structure is manufactured through a process of circulation and activation of an alkaline aqueous solution after manufacturing a preliminary membrane-electrode assembly including a preliminary reduction electrode, an oxidation electrode, and an anion exchange membrane interposed between the preliminary reduction electrode and the oxidation electrode, and during the activation process, the molar ratio of Ni and Mo in the NiMo alloy particles in the preliminary reduction electrode and the oxidation number of Mo are changed through the above-described mechanism.
[0114] As described above, the method for manufacturing the anion exchange membrane electrolysis system specifically includes the steps of manufacturing a preliminary reduction electrode and an oxidation electrode (step 1); manufacturing a preliminary membrane-electrode assembly by interposing an anion exchange membrane between the preliminary reduction electrode and the oxidation electrode (step 2); and supplying an alkaline aqueous solution into the preliminary membrane-electrode assembly and activating the preliminary reduction electrode (step 3); wherein the preliminary reduction electrode includes NiMo-based alloy particles, the NiMo-based alloy particles include Ni and Mo in a molar ratio of 1:1 to 6:1, and the oxidation number of Mo is 4+, 5+, or 6+, and the activation is performed by applying a current at a current density of 25 to 200 mA / cm2 and maintaining the current at 50 to 60°C for 90 to 360 minutes.
[0115] Hereinafter, each step will be described. Step 1 is a step for manufacturing a preliminary reduction electrode and an oxidation electrode, respectively.
[0116] The above-mentioned preliminary reduction electrode can be manufactured by a manufacturing method including a step of applying a slurry for forming a preliminary reduction electrode, including the NiMo-based alloy particles, a binder, and a solvent, onto a release film, drying the slurry, and then separating the slurry from the release film.
[0117] The NiMo alloy particles included in the above-mentioned preliminary reduction electrode specifically contain Ni and Mo in a molar ratio of 1:1 to 6:1, and the oxidation number of Mo is 4+, 5+, or 6+.
[0118] More specifically, the NiMo-based alloy particles may include Ni6Mo, Ni4Mo, Ni3Mo, or NiMo, and any one or a mixture of two or more thereof may be used. Even more specifically, the NiMo-based alloy particles may be a Ni3Mo alloy containing Ni and Mo in a molar ratio of 3:1, and in which the oxidation number of Mo is 4+, 5+, or 6+.
[0119] The above-mentioned NiMo alloy particles can be manufactured by a powder method, specifically, a manufacturing method including a step of co-precipitating a Ni precursor and a Mo precursor under alkaline conditions and then heat-treating the resulting product.
[0120] As the Ni precursor, a carbonate, nitrate, sulfate, acetate, hydroxide, chloride, or hydrate containing Ni may be used. A specific example may include nickel (II) chloride hexahydrate (NiCl2·6H2O). In addition, as the Mo precursor, a carbonate, nitrate, sulfate, acetate, hydroxide, or chloride containing Mo may be used. A specific example may include MoCl5.
[0121] The mixing ratio of the above Ni precursor and Mo precursor can be appropriately determined depending on the molar ratio of elements in the alloy to be manufactured.
[0122] In addition, the coprecipitation reaction of the Ni precursor and the Mo precursor is performed under alkaline conditions. For this purpose, one or more basic substances such as sodium hydroxide (NaOH), sodium carbonate (Na2CO3), lithium hydroxide (LiOH), or potassium hydroxide (KOH) may be added. The basic substance may be added in an amount that maintains a pH range appropriate for the coprecipitation reaction to occur, specifically, pH 11 to 12.
[0123] Additionally, the above basic substances can be introduced in the form of a solution dissolved in water.
[0124] In addition, the co-precipitation reaction of the Ni precursor and the Mo precursor can be performed in a solvent. At this time, ultrapure water (DI water) or the like can be used as the solvent.
[0125] Specifically, a first solution is prepared by mixing a Ni precursor and a Mo precursor, a second solution of a basic substance is prepared by dissolving a basic substance in water, and then water is placed in a separate reactor, and the first and second solutions are added thereto to cause a co-precipitation reaction. After the co-precipitation reaction of the Ni precursor and the Mo precursor, a reaction product is generated in the form of a precipitate.
[0126] The generated reaction product is separated and then heat-treated at 300 to 500°C or 350 to 450°C under a mixed gas atmosphere of hydrogen and an inert gas.
[0127] The reaction product is reduced by the above heat treatment. In addition, the alloying degree and the size of the alloy particles can be controlled by controlling the heat treatment temperature. In the present invention, by performing the heat treatment under the above-mentioned temperature conditions, NiMo-based alloy particles satisfying the above-mentioned molar ratio conditions, oxidation number conditions, and further particle size conditions can be produced.
[0128] In addition, during the heat treatment, hydrogen may be included in an amount of 10 to 25 vol% based on the total volume of the mixed gas. In addition, nitrogen, argon (Ar), etc. may be used as the inert gas. More specifically, the heat treatment may be performed in an H2 / N2 atmosphere containing 10 vol% of hydrogen based on the total volume of the mixed gas of hydrogen and nitrogen.
[0129] When manufactured using the above-described manufacturing method, it is obtained in the form of particles and has a relatively small average particle diameter and a large specific surface area compared to NiMo alloys manufactured by conventional methods such as electroplating or atomic deposition.
[0130] Specifically, the NiMo alloy particles have a BET specific surface area of 30 to 100 m 2 / g, more specifically 35 to 70 m 2 / g is.
[0131] In the present invention, the BET specific surface area of the NiMo alloy particles can be measured using a Micromeritics Tristar II 3020 device according to the BET (Brunauer-Emmett-Teller) method, and the specific measurement method and conditions are described in the following experimental examples.
[0132] In addition, the NiMo alloy particles are porous particles having multiple pores.
[0133] Specifically, the NiMo-based alloy particles have an average pore size of 5 to 20 nm, more specifically 9 to 16 nm, and a pore volume within the alloy particles of 0.1 to 0.5 cm 3 / g, more specifically 0.12 to 0.2 cm 3 / g is.
[0134] Meanwhile, the average pore size and pore volume of the NiMo alloy particles can be calculated from the amount of adsorbed nitrogen gas measured according to the BET method, and the specific measurement method and conditions are described in the following experimental examples.
[0135] In general, NiMo alloys have a structure in which Mo is located on the Ni surface, and the higher the content of Mo present on the Ni surface, the higher the catalytic activity can be exhibited when used as a reduction catalyst in an anion exchange membrane electrolysis system. However, in the case of NiMo alloys manufactured by conventional plating or deposition methods, the Ni particle size is large, so the surface area is small, and as a result, the content of Mo present on the Ni surface is low. In contrast, the alloy particles of the present invention manufactured by the above-described manufacturing method have a smaller Ni particle size than in the conventional method, so the specific surface area of Ni is relatively large, and as a result, much more Mo can be present on the surface. Accordingly, when Mo is lost due to contact with an alkaline aqueous solution thereafter, the surface area of Ni can become larger, and as a result, better catalytic activity can be exhibited.
[0136] Meanwhile, binders that can be used in the manufacture of a slurry for forming a preliminary reduction electrode include PTFE (Polytetrafluoroethylene), PFSA (perfluorosulfonic acid), anion exchange resin, or cation exchange resin, and one or a mixture of two or more of these may be used.
[0137] The above binder can be used in an amount of 20 to 50 parts by weight per 100 parts by weight of NiMo-based alloy particles.
[0138] In addition, when preparing the slurry for forming the above-mentioned preliminary reduction electrode, water; or an alcohol-based solvent such as isopropyl alcohol, propyl alcohol, or ethanol; etc. may be used as a solvent.
[0139] The slurry for forming the above-mentioned preliminary reduction electrode is applied onto a release film, dried, and then separated to manufacture a preliminary reduction electrode. The preliminary reduction electrode used in the water electrolysis system of the present invention is composed only of a catalyst layer including NiMo-based alloy particles, and does not typically include an electrode substrate for supporting the catalyst layer.
[0140] Meanwhile, the oxidation electrode includes an oxidation catalyst as described above.
[0141] The above-mentioned oxidation electrode can be manufactured by a conventional oxidation electrode manufacturing method. Specifically, as in the above-mentioned reduction electrode, it can be manufactured by a manufacturing method including a step of mixing an oxidation catalyst with a binder and a solvent to manufacture a slurry for forming an oxidation electrode, applying the slurry for forming an oxidation electrode including the oxidation catalyst, binder and solvent onto a release film, drying it and then separating it from the release film, or it can be manufactured by a manufacturing method including a step of applying, plating or depositing an oxidation catalyst on an electrode substrate.
[0142] Next, step 2 is a step of manufacturing a preliminary membrane-electrode assembly by interposing an anion exchange membrane between the preliminary reduction electrode and oxidation electrode manufactured in step 1.
[0143] Specifically, the preliminary membrane-electrode assembly can be manufactured by interposing an anion exchange membrane between an oxidation electrode and a preliminary reduction electrode so that the anion exchange membrane and the catalyst layer of each electrode are in contact with each other, and then bonding them by applying heat and pressure. At this time, the bonding process by heat and pressure can be performed by a conventional method.
[0144] In addition, when the manufactured preliminary membrane-electrode assembly further includes a gasket, a step of bonding the gasket to the manufactured assembly may be additionally performed after the bonding process using heat and pressure.
[0145] Meanwhile, the heterofilm used in the manufacture of the oxidation electrode and the preliminary reduction electrode may be separated after the bonding process is completed.
[0146] Meanwhile, the anion exchange membrane is as described above.
[0147] In addition, when the anion exchange membrane electrolysis system includes a plurality of membrane electrode assemblies, the method may further include a step of manufacturing a stack by repeatedly performing the manufacturing process of the membrane-electrode assembly at least twice, stacking the manufactured plurality of membrane-electrode assemblies, and fastening them by applying pressure.
[0148] In addition, when the stack further includes a porous transport layer and a separator together with the membrane-electrode assembly, the stack may further include a step of manufacturing the stack by sequentially positioning the porous transport layer and the separator on the electrode surface side of the membrane-electrode assembly that does not come into contact with the anion exchange membrane, and then applying pressure to fasten them.
[0149] Next, step 3 is a step of supplying an alkaline aqueous solution to the preliminary membrane-electrode assembly manufactured in step 2 and activating it.
[0150] The above alkaline aqueous solution can be supplied to at least one of the preliminary reduction electrode and the oxidation electrode of the preliminary membrane-electrode assembly.
[0151] As described above, the alkaline aqueous solution can be supplied by an alkaline circulation device connected to a preliminary membrane-electrode assembly, and accordingly, the manufacturing method according to the present invention may further include a step of connecting an alkaline circulation device to the preliminary membrane-electrode assembly after the step of manufacturing the preliminary membrane-electrode assembly in step 2.
[0152] For example, after the step of manufacturing the preliminary membrane-electrode assembly, the step of connecting an alkaline aqueous solution circulation device to the oxidation electrode of the preliminary membrane-electrode assembly may further be included, wherein the alkaline aqueous solution may be supplied from the alkaline aqueous solution circulation device to the oxidation electrode of the preliminary membrane-electrode assembly.
[0153] As another example, after manufacturing the preliminary membrane-electrode assembly, the method may further include a step of connecting an alkaline aqueous solution circulation device for the preliminary reduction electrode and an alkaline aqueous solution circulation device for the oxidation electrode to the preliminary reduction electrode and the oxidation electrode of the preliminary membrane-electrode assembly, respectively, wherein the alkaline aqueous solution may be supplied from the alkaline aqueous solution circulation device for the preliminary reduction electrode and the alkaline aqueous solution circulation device for the oxidation electrode to the preliminary reduction electrode and the oxidation electrode of the preliminary membrane-electrode assembly, respectively.
[0154] As another example, after manufacturing the preliminary membrane-electrode assembly, the method may further include a step of installing an alkaline circulation device so as to be connected to both the preliminary reduction electrode and the oxidation electrode of the preliminary membrane-electrode assembly, wherein an alkaline aqueous solution may be supplied from the alkaline circulation device to the preliminary reduction electrode and the oxidation electrode of the preliminary membrane-electrode assembly.
[0155] In the present invention, since the preliminary reduction electrode becomes a reduction electrode after activation, the alkaline aqueous solution circulation device for the preliminary reduction electrode connected to the preliminary reduction electrode is called an alkaline circulation device for the reduction electrode after activation.
[0156] The above alkaline aqueous solution is as described above, and more specifically, it may be a potassium hydroxide aqueous solution having a concentration of 0.1 to 1 M.
[0157] The molar ratio of Ni and Mo and the oxidation number of Mo in the NiMo alloy particles are changed by the above-described activation process, and the activation conditions during the activation process, specifically the current and time, affect the performance development mechanism of the NiMo alloy described above. Accordingly, in the present invention, the composition of a NiMo alloy exhibiting excellent performance was confirmed, and the activation conditions capable of realizing such an alloy composition were discovered and optimized.
[0158] Specifically, the above activation can be performed by applying a current at a current density of 25 to 200 mA / cm2 and maintaining it at 50 to 60°C for 90 to 360 minutes. More specifically, the activation can be performed by applying a current at a current density of 50 to 100 mA / cm2 and maintaining it at 50 to 60°C for 300 to 360 minutes.
[0159] When activation is performed under the above conditions, a NiMo-based alloy catalyst satisfying the molar ratio and oxidation number conditions described above is produced, and as a result, excellent water electrolysis performance can be exhibited.
[0160] Specifically, the molar ratio of Ni and Mo in the NiMo-based alloy particles before activation is 1:1 to 6:1 (Ni:Mo), but Mo is lost during activation, so the molar ratio of Ni and Mo in the NiMo-based alloy catalyst after activation becomes 6:1 to 101:1.
[0161] In addition, the oxidation number of Mo in the NiMo alloy particles before activation is 4+, 5+, or 6+, but after activation, it becomes 5+ or 6+. This is because the oxidation number of Mo changes during activation through the mechanism described above.
[0162] In addition, due to the loss of Mo during activation, a Ni layer composed of Ni is formed on the surface of the alloy catalyst after activation and on the surface of the reduction electrode including the catalyst.
[0163] In addition, the manufacturing method of the present invention may further include a cell performance verification step for verifying the performance of the anion exchange membrane electrolysis system after the activation.
[0164] Specifically, the above cell performance verification step can be performed by measuring the current density for each section by maintaining it for 10 seconds in 0.05 V units from 1.45 to 1.9 V.
[0165] The above cell performance verification step is intended to verify the performance of the anion exchange membrane electrolysis system and does not affect the activation results and cell performance.
[0166] The anion exchange membrane electrolysis system manufactured by the above-described manufacturing method exhibits excellent electrolysis performance, as well as improved durability and efficiency.
[0167] According to another embodiment of the present invention, an activation method capable of improving the performance of an anion exchange membrane electrolysis system is provided.
[0168] Specifically, the method for activating the anion exchange membrane electrolysis system includes a step of supplying an alkaline aqueous solution to the anion exchange membrane electrolysis system, wherein the anion exchange membrane comprises a pre-reduction electrode, an oxidation electrode, and an anion exchange membrane interposed between the pre-reduction electrode and the oxidation electrode, wherein the pre-reduction electrode comprises NiMo-based alloy particles containing Ni and Mo in a molar ratio of 1:1 to 6:1 and wherein the oxidation number of Mo is 4+, 5+, or 6+, and applying a current at a current density of 25 to 200 mA / cm2 and maintaining the current at 50 to 60°C for 90 to 360 minutes, thereby activating the pre-reduction electrode.
[0169] The details of the above-mentioned preliminary anion exchange membrane electrolysis system, the alkaline aqueous solution and its injection method, and the activation process are as described above.
[0170] In addition, as a result of activation of the above-mentioned preliminary reduction electrode, a reduction electrode is manufactured, and the reduction electrode includes a NiMo-based alloy catalyst in which the molar ratio of Ni and Mo is 6:1 to 101:1 and the oxidation number of Mo is 5+ or 6+.
[0171]
[0172] Below, preferred embodiments are presented to aid understanding of the invention. However, the following embodiments are intended only to illustrate the invention and are not intended to limit the invention to these embodiments.
[0173] <NiMo계 합금 입자의 제조>
[0174] Manufacturing Example 1
[0175] The first solution was prepared by dissolving NiCl2·6H2O and MoCl5 in 20 ml of DI water so that the total content was 15 mmol. At this time, NiCl2·6H2O and MoCl5 were used so that the molar ratio of Ni:Mo was 1:1.
[0176] Separately, a second solution was prepared by dissolving 34.2 mmol of NaOH solution and 10.7 mmol of Na2CO3 in 20 ml of DI water.
[0177] 40 ml of DI water was placed in a vial, and the first and second solutions were added dropwise while stirring to mix. The mixing was performed at room temperature (23±2°C), and the pH of the mixture was maintained at 8.5 or lower.
[0178] The above mixed solution was stirred and reacted for 24 hours, and the resulting metal precipitate was obtained by centrifugation. The obtained metal precipitate was washed three times with water and ethanol and dried overnight at 50°C in a convection oven.
[0179] 300 mg of the resulting dried product was reduced in a 10% H2 / N2 atmosphere at 400°C for 1 hour to produce NiMo alloy particles.
[0180]
[0181] Manufacturing Example 2
[0182] Ni3Mo alloy particles were manufactured in the same manner as in Manufacturing Example 1, except that in the manufacturing of the first solution in Manufacturing Example 1, NiCl2·6H2O and MoCl5 were used so that the molar ratio of Ni:Mo was 3:1.
[0183]
[0184] Manufacturing Example 3
[0185] Ni4Mo alloy particles were manufactured using the same method as in Manufacturing Example 1, except that in the manufacturing of the first solution in Manufacturing Example 1, NiCl2·6H2O and MoCl5 were used so that the molar ratio of Ni:Mo was 4:1.
[0186]
[0187] Manufacturing Example 4
[0188] Ni6Mo alloy particles were manufactured using the same method as in Manufacturing Example 1, except that in the manufacturing of the first solution in Manufacturing Example 1, NiCl2·6H2O and MoCl5 were used so that the molar ratio of Ni:Mo was 6:1.
[0189]
[0190] <Manufacturing of water electrolysis system>
[0191] Example 1
[0192] An anion exchange membrane electrolysis system was manufactured using the NiMo alloy particles manufactured in Manufacturing Example 1 above.
[0193] In detail, it was manufactured in the following order: electrode manufacturing step, membrane-electrode assembly manufacturing step, KOH solution feeding system configuration step, and activation step.
[0194] Electrode manufacturing steps
[0195] The NiMo alloy particles and binder manufactured in the above Manufacturing Example 1 were dispersed in a solvent, and then ultrasonic waves were applied for 30 minutes, and then dispersed at least 1 by using a ball mill to manufacture a slurry for forming a preliminary reduction electrode. At this time, the NiMo alloy particles and the binder were used at a weight ratio of 1:0.2, and a 60 wt% PTFE (Polytetrafluoroethylene) aqueous dispersion was used as the binder. In addition, a mixed solvent of water and IPA (isopropyl alcohol) at a weight ratio of 5:5 was used as the solvent, and the solvent was used so that the solid content in the slurry for forming a preliminary reduction electrode was 20 wt%.
[0196] The slurry for forming the preliminary reduction electrode prepared above was dried so that the loading amount of NiMo was 1.0 mg / cm 2 The pre-reduction electrode was manufactured by applying the NiMo to the release film using a bar coater and drying it in an 80°C convection oven for 1 hour. The loading amount of NiMo was 1.0 mg / cm through XRF analysis. 2 I checked if it was abnormal.
[0197] Separately, an oxidation electrode was prepared in the same manner as above, except that NiFe-layered double hydroxide (NiFe LDH) was used as a catalyst.
[0198]
[0199] Membrane-electrode assembly manufacturing steps
[0200] It was manufactured by bonding an electrode to an anion exchange membrane using the CCM (catalyst coated membrane) method.
[0201] The preliminary reduction electrode and oxidation electrode manufactured in the above electrode manufacturing step were cut into 3 cm wide and 3 cm long pieces, respectively, and then a Sustainion™ X37-50 grade RT anion exchange membrane from Sustainion was interposed between the preliminary reduction electrode and the oxidation electrode, and roll pressed at 130°C, 30 MPa of pressure, and 0.1 m / min of speed to manufacture a preliminary membrane-electrode assembly. Thereafter, the release film on the preliminary reduction electrode and the oxidation electrode was removed. A sub-gasket having a thickness of 200 μm was bonded to the manufactured preliminary membrane-electrode assembly to prevent cell leakage and facilitate handling.
[0202]
[0203] Activation phase
[0204] A lower end plate made of SUS (Steel Use Stainless) was prepared, and on top of that, a nickel foam having a thickness of 300 μm as a nickel foam porous transport layer (PTL) for the oxidation electrode, and the pre-membrane electrode assembly manufactured above were laminated so that the oxidation electrode was in contact with the porous transport layer. On the reduction electrode side of the pre-membrane electrode assembly, a carbon paper having a thickness of 250 μm as a nickel foam porous transport layer for the oxidation electrode, a nickel-based separation plate for the oxidation electrode, and an upper end plate made of SUS were sequentially positioned and fastened by applying a torque of 7 Nm to manufacture a stack.
[0205] A preliminary anion exchange membrane electrolysis system was manufactured using a dual feeding method in which two KOH tanks were prepared as alkaline aqueous solution circulation devices and connected to the oxidation electrode and reduction electrode of the stack, respectively, to supply KOH to the oxidation electrode and reduction electrode, respectively. At this time, a 1 M KOH aqueous solution was used as the alkaline aqueous solution.
[0206] For the manufactured preliminary anion exchange membrane electrolysis system, KOH was supplied as a dual feeding. The temperature of the KOH aqueous solution was 50°C and it was circulated at 10 cc / min. When the preliminary anion exchange membrane electrolysis system reached 50°C, the power supply was used to supply 50 mA / cm to the preliminary anion exchange membrane electrolysis system. 2 After activating the cell by applying a current density of 1 for 6 hours, the cell performance was confirmed by measuring the current density at each section while maintaining the voltage from 1.45 V to 1.9 V in 0.05 V increments for 10 seconds using a power supply, and an anion exchange membrane electrolysis system was manufactured.
[0207]
[0208] Examples 2 to 4
[0209] An anion exchange membrane electrolysis system was manufactured in the same manner as in Example 1, except that the alloy particles manufactured in Manufacturing Examples 2 to 4 were used as the alloy particles.
[0210]
[0211] Experimental Example 1
[0212] The BET specific surface area, average pore size, and average pore volume of the alloy particles manufactured in the above manufacturing examples 1 to 4 were measured using the following method.
[0213] According to the BET (Brunauer-Emmett-Teller) method, nitrogen gas was adsorbed on the alloy particles manufactured in Manufacturing Examples 1 to 4 at liquid nitrogen temperature (77 K) using Micromeritics Tristar II 3020, and the amount of adsorbed nitrogen gas was measured, and the specific surface area, pore volume, and pore size were calculated. The measurement results are shown in Table 1 and FIGS. 6a to 6d below.
[0214] Figures 6a to 6d are graphs showing the BET analysis results for NiMo-based alloy particles of Manufacturing Examples 1, 2, 3, and 4, respectively.
[0215]
[0216] NiMo alloy particle composition BET specific surface area [m 2 / g]Pore volume[cm 3 / g]Pore size[nm] Manufacturing example 1 NiMo 3 8.13 10.149 15.731 Manufacturing example 2 Ni3Mo 6 5.49 50.159 9.724 Manufacturing example 3 Ni4Mo 5 6.67 50.197 13.923 Manufacturing example 4 Ni6Mo 3 7.65 20.149 15.731
[0217]
[0218] As a result of the experiment, the NiMo alloy particles manufactured in Manufacturing Examples 1 to 4 had a BET specific surface area of 37 to 66 m 2 / g, and the pore size was 9 to 16 nm, and it had an increased pore size and pore volume along with a wide BET specific surface area compared to alloys manufactured by conventional deposition or plating methods.
[0219]
[0220] Experimental Example 2
[0221] The activity change for the hydrogen evolution reaction according to the molar ratio of Ni and Mo in NiMo alloys was evaluated using linear sweep voltammetry (LSV).
[0222] LSV was performed in a three-electrode cell using a CHE760E Bipotentiostat from CH Instruments.
[0223] A catalyst slurry for a working electrode was prepared by mixing 10 mg of NiMo-based alloy particles, 1 ml of deionized water, 1.5 ml of 2-propanol, and 60 μl of a 5 wt% Nafion solution. At this time, the alloy particles prepared in Preparation Examples 1 to 4 were used as the NiMo-based alloy. 10 μl of the prepared catalyst slurry was applied to a glassy carbon rotating disk electrode (RDE) at a concentration of 0.2 mg / cm. 2 The amount of loading was , and the LSV was measured with a RHE (Reversible hydrogen electrode) from 0.15 V to -0.3 V in a 1 M KOH solution.
[0224] Also, for comparison, the loading amount was set to 0.04 mg / cm for 40 wt% Pt / C, which is used as a conventional oxidation electrode catalyst. 2 and 0.2mg / cm 2 The activity change for the hydrogen evolution reaction was evaluated in the same manner as above, except that each was changed to .
[0225]
[0226] In addition, the initial oxidation number of Mo in the NiMo alloys of Manufacturing Examples 1 to 4 used in this experimental example was confirmed through X-ray photoelectron spectroscopy (XPS).
[0227] Specifically, the composition of Ni3Mo alloy particles in the preparatory anion exchange membrane electrolysis system and the composition of the electrode surface in the anion exchange membrane electrolysis system were measured using a Thermo Scientific K-alpha X-ray photoelectron spectrometer from Thermo Fisher Scientific, respectively. To calibrate the binding energy, the C 1s peak was set to 284.6 eV as the reference.
[0228] The measurement results are shown in Figs. 7 and 8.
[0229] Fig. 7 is a graph showing the results of evaluating the activity change for the hydrogen evolution reaction according to the molar ratio of Ni and Mo in the NiMo-based alloy using linear scanning potential (LSV), and Fig. 8 is a graph showing the results of analyzing the initial oxidation number of Mo in the NiMo-based alloys of Manufacturing Examples 1 to 4 using XPS.
[0230] As a result of the experiment, it was confirmed that the NiMo alloy particles exhibited the best catalytic activity when the ratio of Ni and Mo was 3:1 to 4:1, and that the oxidation number of Mo at this time was 4+, 5+, or 6+.
[0231]
[0232] Experimental Example 3
[0233] In order to confirm the loss of Mo in a NiMo alloy in an alkaline atmosphere, an anion exchange membrane electrolysis system was manufactured using the Ni3Mo alloy particles manufactured in Manufacturing Example 2, and the change in the molar ratio of Ni and Mo in the alloy before and after activation was evaluated.
[0234] Specifically, 10 preliminary anion exchange membrane electrolysis systems were manufactured in the same manner as in Example 1, except that the Ni3Mo alloy particles manufactured in Manufacturing Example 2 were used as the NiMo-based alloy particles (Sample no. 1 to 10). The NiMo content in the manufactured preliminary anion exchange membrane electrolysis systems and the contents of Ni and Mo in the alloy were each measured.
[0235] For each of the preliminary anion exchange membrane electrolysis systems manufactured above, 50°C, 1M KOH solution was circulated, and 25 mA / cm 2 After activation was performed by maintaining the current for 6 hours, the cell performance was confirmed by measuring the current density at each section by maintaining the current at 0.05 V increments from 1.45 to 1.9 V for 10 seconds using a power supply, and an anion exchange membrane electrolysis system was manufactured.
[0236] The content of the NiMo alloy catalyst and the contents of Ni and Mo in the alloy were measured for the manufactured anion exchange membrane electrolysis system.
[0237]
[0238] The above NiMo content and the contents of Ni and Mo in the alloy were measured through X-ray fluorescence analysis (XRF).
[0239] Specifically, Olympus' VANTA S was used as the XRF equipment, and the elemental analysis was performed by analyzing the peak that appears after irradiating the material with X-rays of 0 to 40 keV. In addition, the X-ray irradiation time was maintained for 10 seconds, and a calibration curve was drawn for the peak that appears at this time to analyze the content. Each calibration curve utilized the software built into the XRF equipment.
[0240] The results are shown in Table 2 below.
[0241]
[0242] Sample No. Content of pre-activated alloy particles (mg / cm2) Content of activated alloy catalyst (mg / cm2) Molar ratio of Ni:Mo in activated alloy catalyst 12.02 (Ni: 1.42, Mo: 0.60) 1.59 (Ni: 1.30, Mo: 0.29) 7.3:12 2.02 (Ni: 1.65, Mo: 0.37) 1.54 (Ni: 1.43, Mo: 0.11) 21.3:13 1.42 (Ni: 1.21, Mo: 0.21) 1.10 (Ni: 1.03, Mo: 0.07) 24.1:14 1.56 (Ni: 1.31, Mo: 0.24) 1.28 (Ni: 1.18, Mo: 0.10)19.3:152.16(Ni: 1.87, Mo: 0.29)1.77(Ni: 1.69, Mo: 0.08)34.5:161.52(Ni: 1.32, Mo: 0.20)1.32(Ni: 1.25, Mo: 0.07)29.2:172.37(Ni: 1.68, Mo: 0.69)1.71(Ni: 1.54, Mo: 0.17)14.8:182.73(Ni: 1.20, Mo: 1.53)1.56(Ni: 1.22, Mo: 0.34)5.9:190.68(Ni: 0.51, Mo: 0.17)0.52(Ni: 0.51, Mo: 0.01)83.4:1101.92(Ni: 1.34, Mo: 0.58)1.25(Ni: 1.23, Mo: 0.02)100.5:1
[0243]
[0244] Experimental results confirmed that a significant loss of Mo occurred after activation. In addition, it was confirmed that this resulted in a change in the molar ratio of Ni and Mo in the NiMo alloy.
[0245] In addition, the reason for the loss of the above Mo was clarified through thermodynamic calculations.
[0246] Table 3 below shows the loss energy of Mo in NiMo-based alloy catalysts.
[0247]
[0248] Mo dissolutionE des Ni 24 Mo8→ Ni 24Mo7-0.60Ni 24 Mo7→ Ni 24 Mo6-0.51Ni 24 Mo6→ Ni 24 Mo5-0.72Ni 24 Mo5→ Ni 24 Mo4-0.67
[0249]
[0250] As shown in Table 3 above, Ni 24 When calculating the energy when Mo is lost one by one in the Mo8 alloy, it can be seen that everything progresses in the direction of stabilization, and also, through computational chemistry, it can be seen that the NiMo alloy is stable when all Mo present on the surface is lost in an alkaline atmosphere.
[0251] Ni 24 The adsorption energies of H2O, MoO2, and H2O / MoO2 clusters on the surface of Mo8 alloy were calculated, and the results showed that the lost Mo adsorbed with water and existed in the form of H2O / MoO2.
[0252] In addition, the adsorption energy of the hydrogen intermediate H* according to the adsorption site was calculated, and it was found that the hydrogen intermediate was stabilized when adsorbed on the Ni site rather than the Mo site. Therefore, it can be expected that clusters of MoO2 and H2O are adsorbed on the Ni surface, and that after water decomposition, hydrogen moves to the Ni surface to generate hydrogen.
[0253] From the above results, it can be seen that the hydrogen production reaction mechanism of the Ni-Mo alloy in an alkaline environment is that all Mo on the surface of the Ni-Mo alloy is lost, the lost Mo forms Mo oxide, and is then re-adsorbed on the bare Ni surface in the form of H2O / Mo oxide, followed by a dissociation reaction of water and adsorption of the hydrogen intermediate H* on the Ni site (dual active site), and H2 is produced through the Heyrovsky or Tafel reaction.
[0254] Therefore, a stable and highly active NiMo alloy structure in an alkaline environment must have a surface composed of Ni by selectively dissolving only the Mo on the surface, and the dissolved Mo must be in the form of Mo oxide of MoO2, forming a cluster with H2O and being adsorbed on the Ni surface. It was confirmed that the molar ratio of Ni and Mo was 6:1 to 101:1.
[0255]
[0256] Experimental Example 4
[0257] The change in oxidation number of Mo in NiMo alloy before and after activation was evaluated.
[0258] Specifically, a preliminary anion exchange membrane electrolysis system was manufactured in the same manner as in Example 1, except that the Ni3Mo alloy particles manufactured in Manufacturing Example 2 were used as the NiMo alloy particles. The Mo oxidation number of the Ni3Mo alloy particles in the manufactured preliminary anion exchange membrane electrolysis system was measured.
[0259] Circulate 1M KOH solution at 50℃ for the preliminary anion exchange membrane electrolysis system manufactured above, and 50 mA / cm 2 After activation was performed by maintaining the current for 6 hours, the cell performance was confirmed by measuring the current density at each section by maintaining it at 0.05 V increments from 1.45 to 1.9 V for 10 seconds using a power supply, and an anion exchange membrane electrolysis system was manufactured. The oxidation number of Mo of the alloy catalyst in the manufactured anion exchange membrane electrolysis system was measured.
[0260] The above Mo oxidation number was measured through X-ray photoelectron spectroscopy (XPS), and the measurement method and conditions were the same as in Experimental Example 2. The results are shown in Fig. 9.
[0261] Figure 9 is a graph showing the results of XPS analysis of the change in Mo oxidation number in the Ni3Mo alloy before and after activation.
[0262] Experimental results showed that the oxidation numbers of Mo in the Ni3Mo alloy before activation were 4+, 5+, and 6+, but after activation, they were 5+ and 6+. From this, it was confirmed that the oxidation number of Mo in the NiMo alloy changes in an alkaline atmosphere.
[0263]
[0264] Experimental Example 5
[0265] The effect of activation method on the performance of an anion exchange membrane electrolysis system was evaluated.
[0266] Specifically, a preliminary anion exchange membrane electrolysis system was manufactured in the same manner as in Example 1 except that the Ni3Mo alloy particles manufactured in Manufacturing Example 2 were used as the NiMo-based alloy particles, and then activation was performed by injecting an alkaline aqueous solution into the manufactured preliminary anion exchange membrane electrolysis system while increasing and decreasing the applied voltage as in the prior art (hereinafter referred to as “Comparative Example”) and by applying a current while maintaining a constant current density as in the present invention (hereinafter referred to as “Example”).
[0267]
[0268] (1) Activation method 1 (Comparative example A)
[0269] For the preliminary anion exchange membrane electrolysis system manufactured above, a 1M KOH solution at 60°C was circulated, and the voltage was increased from 1.45 to 1.9 V in 0.05 V increments while maintaining it for 5 seconds, and then decreased from 1.9 to 1.45 V in 0.05 V increments while maintaining it for 5 seconds. At this time, the number of activations through the voltage increases and decreases was fixed at 20 to maintain the current density.
[0270]
[0271] (2) Activation method 2 (Example A)
[0272] Circulate 1M KOH solution at 60℃ for the preliminary anion exchange membrane electrolysis system manufactured above, and 100mA / cm 2 Activation was performed by maintaining the current for 6 hours.
[0273] After activation by the above method, for each anion exchange membrane electrolysis system, the cell performance was confirmed by measuring the current density at each section while maintaining the voltage from 1.45 V to 1.9 V in 0.05 V increments for 10 seconds using a power supply. During the cell performance confirmation, the current change according to voltage control was observed, and the results are shown in Figs. 10 and 11.
[0274] Fig. 10 is a graph showing the results of observing the change in current according to voltage control in an anion exchange membrane electrolysis system activated by increasing and decreasing the applied voltage (Comparative Example A), and Fig. 11 is a graph showing the results of observing the change in current according to voltage control in an anion exchange membrane electrolysis system activated by applying current at a constant current density and maintaining it for a constant time (Example A).
[0275] As a result of the experiment, the activation method (comparative example A) of increasing and decreasing the applied voltage as in the past accelerated the loss of Mo when the voltage was changed, and as a result, the electrolysis performance deteriorated rapidly. On the other hand, when the voltage was increased to 100 mA / cm 2 The activation method (Example A) of applying current at a current density and maintaining it for 6 hours confirmed that the performance was maintained constant without change even when the voltage change was repeated 10 or more times as Mo was lost at the initial stage of activation and then redeposited on the Ni surface.
[0276]
[0277] Experimental Example 6
[0278] The effect of activation method on Mo loss in an anion exchange membrane electrolysis system was evaluated.
[0279] (1) Activation method 1 (comparative example B)
[0280] A preliminary anion exchange membrane electrolysis system was manufactured in the same manner as in Example 1, except that the Ni3Mo alloy particles manufactured in Manufacturing Example 2 were used as the NiMo alloy particles. Then, a 60°C, 1M KOH solution was circulated through the manufactured preliminary anion exchange membrane electrolysis system, and the voltage was increased from 1.45 to 1.9 V in 0.05 V increments for 5 seconds, and then decreased from 1.9 to 1.45 V in 0.05 V increments for 5 seconds. The number of cycles was fixed so as to maintain the current density.
[0281] After the activation, for each anion exchange membrane electrolysis system, the cell performance was confirmed by measuring the current density at each section by maintaining the voltage from 1.45 V to 1.9 V in 0.05 V increments for 10 seconds using a power supply, and the anion exchange membrane electrolysis system was manufactured.
[0282]
[0283] (2) Activation method 2 (Example B)
[0284] A preliminary anion exchange membrane electrolysis system was manufactured in the same manner as in Example 1, except that the Ni3Mo alloy particles manufactured in Manufacturing Example 2 were used as NiMo alloy particles, and then a 60°C, 1M KOH solution was circulated through the manufactured preliminary anion exchange membrane electrolysis system at 50 mA / cm. 2 Activation was performed by maintaining the current for 6 hours. Thereafter, the cell performance was confirmed by measuring the current density at each section by maintaining the voltage from 1.45 V to 1.9 V in 0.05 V increments for 10 seconds using a power supply, and an anion exchange membrane electrolysis system was manufactured.
[0285]
[0286] The NiMo alloy content and Mo content in the pre-activation anion exchange membrane electrolysis system, and the NiMo alloy content and Mo content remaining in the electrode of the anion exchange membrane electrolysis system after activation were measured using X-ray fluorescence analysis (XRF).
[0287] At this time, X-ray fluorescence analysis (XRF) and content measurement were performed using the same method as in Experimental Example 3.
[0288] Experimental results show that the initial Mo content in the NiMo alloy before activation is initially 0.75 mg / cm 2 In (catalytic reaction area 5cm) 2 ), when activated by activation method 1 (comparative example B), the Mo content after activation was 0.07 mg / cm 2 , about 9% remained. On the other hand, when activated by activation method 2 (Example B), the initial Mo content was 0.75 mg / cm 2 After activation at 0.18 mg / cm 2 , about 24% remained.
[0289] From this, it was confirmed that the activation method of the present invention is more advantageous in reducing the amount of Mo loss, and as a result, can improve the life characteristics of the water electrolysis system.
[0290]
[0291] Experimental Example 7
[0292] To evaluate the effect of current conditions during activation on the performance development mechanism of NiMo alloys, the current density was set to 25 mA / cm 2 , 50 mA / cm 2 , 100 mA / cm 2 and 200 mA / cm 2 Each was activated by changing it and the cell performance was evaluated.
[0293] Specifically, a preliminary anion exchange membrane electrolysis system was manufactured in the same manner as in Example 1, except that the Ni3Mo alloy particles of Manufacturing Example 2 were used. A 50°C, 1M KOH solution was circulated through the manufactured preliminary anion exchange membrane electrolysis system at a current density of 25 mA / cm. 2 , 50 mA / cm 2 , 100 mA / cm 2 and 200 mA / cm 2 The cells were activated by applying current for 6 hours under the conditions of . Afterwards, the cell performance was confirmed by measuring the current density at each section by maintaining the voltage from 1.45 V to 2.5 V in 0.05 V increments for 10 seconds using a power supply, and an anion exchange membrane electrolysis system was manufactured.
[0294] For comparison, a preliminary anion exchange membrane electrolysis system was manufactured in the same manner as in Example 1 using a 40 wt Pt / C catalyst as a catalyst for the reduction electrode. Activation was performed by circulating a 1 M KOH solution at 50°C for the manufactured preliminary anion exchange membrane electrolysis system, increasing the voltage from 1.45 to 1.9 V in 0.05 V increments for 5 seconds, and then decreasing it from 1.9 to 1.45 V in 0.05 V increments for 5 seconds. The number of cycles was fixed so as to maintain the current density. Thereafter, the cell performance was confirmed in the same manner as described above, and an anion exchange membrane electrolysis system was manufactured.
[0295]
[0296] For the anion exchange membrane electrolysis system manufactured above, the voltage change according to the current density was measured using linear scanning voltammetry (LSV), and a polarization curve was obtained as a result.
[0297] Specifically, for each anion exchange membrane electrolysis system manufactured above, the voltage change according to the current density was measured under LSV conditions using a CHE760E Bipotentiostat device from CH Instruments. The results are shown in Fig. 12.
[0298]
[0299] In addition, the durability of the anion exchange membrane electrolysis system manufactured above was evaluated using the chronoamperometry method.
[0300] Specifically, for each anion exchange membrane electrolysis system manufactured above, a power supply of 1 A / cm is used. 2 The voltage was measured while maintaining the current density. Durability was judged to be excellent if the voltage remained unchanged, and durability was judged to be low if the voltage increased. The results are shown in Fig. 13.
[0301]
[0302] Figure 12 shows the current density of 25 mA / cm 2 , 50 mA / cm 2 , 100 mA / cm 2 and 200 mA / cm 2 This is a graph showing the polarization evaluation results for the anion exchange membrane electrolysis system activated under the conditions of , and Fig. 13 shows the current density of 25 mA / cm 2 , 50 mA / cm 2 , 100 mA / cm 2 and 200 mA / cm 2 This is a graph showing the durability evaluation results for each activated anion exchange membrane electrolysis system under the conditions.
[0303] Experimental results show that the current density is 25 to 200 mA / cm 2 When activated in the range of , it exhibited excellent performance characteristics, especially at a current density of 50 mA / cm. 2It was confirmed that when activated, it exhibited better performance and durability than platinum.
[0304]
[0305] Meanwhile, the reason for the above experimental results can be understood through the pourbaix diagram.
[0306] Figure 14 is a phase diagram of Mo according to pH, disclosed in the literature "Anatolyevich, Pavel. "The Revised Pourbaix Diagram for Molybdenum." HMo 2.10: 3."
[0307] As shown in Fig. 14, in an alkaline atmosphere and at a specific current section, Mo is MoO4 2- Or it can be seen that it exists in the form of MoO2. Also, under conditions of pH 12 or higher, Mo is MoO4. 2- It is dissolved and lost in the form of MoO2. However, looking at line 26, we can see that it can exist in the form of MoO2 in a specific voltage range between pH 9 and 12. Through this experiment and computational chemistry, we can see that the activation in a specific current range is MoO2. It indicates that it can exist in the form of 50mA / cm 2 It was predicted that when activated, it would likely exist as MoO2.
[0308]
[0309] Additionally, the effect of current conditions during activation on the loss of Mo in NiMo alloys in an alkaline atmosphere was evaluated.
[0310] For this purpose, the current density is 25 mA / cm 2 , 50 mA / cm 2 , 100 mA / cm 2 and 200 mA / cm 2 The residual Mo was measured using X-ray fluorescence analysis (XRF) in the same manner as in Experimental Example 3 for the activated anion exchange membrane electrolysis system, which was changed to each of .
[0311] The results are shown in Figure 15.
[0312] Figure 15 shows the current density of 25 mA / cm 2 , 50 mA / cm 2 , 100 mA / cm 2 and 200 mA / cm 2 This is a graph showing the results of analyzing the Mo residual amount in an anion exchange membrane electrolysis system activated under each condition using X-ray fluorescence analysis (XRF).
[0313] Experimental results, current density 50mA / cm 2 When activated, the largest amount of Mo remained on the cathode. From this, it can be predicted that the Mo lost through activation is re-adsorbed on the Ni surface.
[0314]
[0315] Experimental Example 8
[0316] To evaluate the effect of activation time on the performance development mechanism of NiMo alloys, activation was performed at 90, 180, and 360 minutes, respectively, and cell performance was evaluated.
[0317] Specifically, a preliminary anion exchange membrane electrolysis system was manufactured in the same manner as in Example 1, except that the Ni3Mo alloy particles of Manufacturing Example 2 were used. A 50°C, 1M KOH solution was circulated through the manufactured preliminary anion exchange membrane electrolysis system, and a current density of 50 mA / cm was applied. 2 The cell was activated by applying current for 90 minutes, 3 hours, and 6 hours, respectively, under the conditions. Afterwards, the cell performance was confirmed by measuring the current density at each section by maintaining the voltage from 1.45 V to 1.9 V in 0.05 V increments for 10 seconds using a power supply, and an anion exchange membrane electrolysis system was manufactured.
[0318] Also, for comparison, a preliminary anion exchange membrane electrolysis system was manufactured in the same manner as in Example 1 using a 40 wt Pt / C catalyst as a catalyst for the reduction electrode. Activation was performed by circulating a 1 M KOH solution at 50°C for the manufactured preliminary anion exchange membrane electrolysis system, increasing the voltage from 1.45 to 1.9 V in 0.05 V increments while maintaining it for 5 seconds, and decreasing it from 1.9 to 1.45 V in 0.05 V increments while maintaining it for 5 seconds. At this time, the number of cycles was fixed at 10 to maintain the current density. Afterwards, the cell performance was confirmed by measuring the current density at each section while maintaining it from 1.45 V to 1.9 V in 0.05 V increments for 10 seconds using a power supply, and the anion exchange membrane electrolysis system was manufactured.
[0319] For the anion exchange membrane electrolysis system manufactured above, 1 A / cm using the chronoamperometry method 2 The voltage value was measured while maintaining the conditions. The results are shown in Fig. 16.
[0320] Figure 16 is a graph showing the results of evaluating the effect of activation time on the performance development of NiMo alloys.
[0321] Experimental results showed that the performance was better than platinum when the activation time was 180 minutes or longer, and it became stable when the activation time was 360 minutes or longer.
[0322]
[0323] Experimental Example 9
[0324] The change in Mo loss according to the alkaline aqueous solution circulation method in an anion exchange membrane electrolysis system was evaluated.
[0325] Using the Ni3Mo alloy particles manufactured in the above Manufacturing Example 2, a preliminary anion exchange membrane electrolysis system including an alkaline aqueous solution circulation device of the both feeding type as in Fig. 4 and a preliminary anion exchange membrane electrolysis system including an alkaline aqueous solution circulation device of the anode feeding type as in Fig. 5 were manufactured, respectively. The NiMo content in the manufactured preliminary anion exchange membrane electrolysis system and the contents of Ni and Mo in the alloy were each measured.
[0326] Next, 60°C, 1M KOH solution is circulated through the above-mentioned preliminary anion exchange membrane electrolysis system, and 25 mA / cm 2 Activation was performed by applying a current of 1.45 to 1.9 V and maintaining it for 6 hours, and the cell performance was confirmed by measuring the current density at each section by maintaining it for 10 seconds in 0.05 V increments from 1.45 to 1.9 V using a power supply, thereby manufacturing an anion exchange membrane electrolysis system. The content of the NiMo alloy catalyst in the manufactured anion exchange membrane electrolysis system and the contents of Ni and Mo in the alloy were measured.
[0327] The above NiMo content and the contents of Ni and Mo in the alloy were measured through X-ray fluorescence analysis (XRF) using the same method as in Experimental Example 3. The results are shown in Table 4 below.
[0328]
[0329] Sample No. Alkali aqueous solution feeding method Alloy type Alloy particle content before activation (mg / cm2) Alloy catalyst content after activation (mg / cm2) 11 Anode (60℃) Ni3Mo2.02 (Ni: 1.42, Mo: 0.60) 1.59 (Ni: 1.30, Mo: 0.29) 12 Both (60℃) Ni3Mo2.34 (Ni: 1.59 Mo: 0.75) 1.60 (Ni: 1.53, Mo: 0.07)
[0330]
[0331] The experimental results showed that the anode feeding method, which supplies KOH solution only to the oxidation electrode, showed a lower Mo loss rate than the both feeding method, which supplies KOH solution simultaneously.
[0332] In the case of the both-feeding method, Mo dissolution occurs simultaneously when the KOH solution directly contacts the NiMo catalyst, and Mo dissolution occurs when the NiMo catalyst is anionized and moves to the anode. On the other hand, anode feeding shows a lower dissolution rate than both-feeding because the NiMo catalyst does not come into direct contact with KOH.
[0333]
[0334] Experimental Example 10
[0335] The effect of the alkaline aqueous solution circulation method in an anion exchange membrane electrolysis system on the performance of the electrolysis system was evaluated.
[0336] Using the Ni3Mo alloy particles manufactured in the above Manufacturing Example 2, a preliminary anion exchange membrane electrolysis system including an alkaline aqueous solution circulation device of a both feeding type as in Fig. 4 and a preliminary anion exchange membrane electrolysis system including an alkaline aqueous solution circulation device of a dual feeding type as in Fig. 6 were manufactured, respectively.
[0337] Next, 60°C, 1M KOH solution is circulated through the above-mentioned preliminary anion exchange membrane electrolysis system, and 25 mA / cm 2 Activation was performed by maintaining the current for 6 hours, and the cell performance was confirmed by measuring the current density at each section by maintaining the current at 0.05 V increments from 1.45 to 1.9 V for 10 seconds using a power supply, and an anion exchange membrane electrolysis system was manufactured.
[0338]
[0339] For each anion exchange membrane electrolysis system manufactured above, the voltage change according to the current density was measured using linear scanning voltammetry (LSV), and a polarization curve was obtained as a result.
[0340] Specifically, for each anion exchange membrane electrolysis system manufactured above, a device (CHE760E Bipotentiostat manufactured by CH Instruments) was used to measure the voltage change according to the current density under the conditions of LSV.
[0341]
[0342] In addition, the durability of the anion exchange membrane electrolysis system manufactured above was evaluated using the chronoamperometry method.
[0343] Specifically, for each anion exchange membrane electrolysis system manufactured above, a power supply of 1 A / cm is used. 2 The voltage was measured while maintaining the current density. If the voltage remained unchanged, it was judged to have excellent durability, and if the voltage increased, it was judged to have low durability. The results are shown in Figs. 17 and 18, respectively.
[0344]
[0345] Figure 17 is a graph showing the polarization evaluation results of an anion exchange membrane electrolysis system according to an alkaline aqueous solution circulation method, and Figure 18 is a graph showing the durability evaluation results of an anion exchange membrane electrolysis system.
[0346] Experimental results showed that the two-feeding method, which uses a single tank to supply KOH aqueous solution, produced hydrogen at a lower voltage than the dual-feeding method, which uses separate tanks to supply KOH aqueous solution. In other words, it was confirmed that configuring the anode and cathode with separate KOH aqueous solutions resulted in higher system efficiency.
Claims
1. A step of manufacturing a preliminary reduction electrode and an oxidation electrode, respectively; A step of manufacturing a preliminary membrane-electrode assembly by interposing an anion exchange membrane between the preliminary reduction electrode and the oxidation electrode; and A step of supplying an alkaline aqueous solution to the preliminary membrane-electrode assembly and activating the preliminary reduction electrode; The above preliminary reduction electrode comprises NiMo-based alloy particles in which the molar ratio of Ni and Mo is 1:1 to 6:1 and the oxidation number of Mo is 4+, 5+ or 6+, The above activation is performed by applying a current at a current density of 25 to 200 mA / ㎠ and maintaining it at 50 to 60℃ for 90 to 360 minutes. A method for manufacturing an anion exchange membrane electrolysis system.
2. In paragraph 1, The above activation is performed by applying a current at a current density of 50 to 100 mA / ㎠ and maintaining it at 50 to 60℃ for 300 to 360 minutes. A method for manufacturing an anion exchange membrane electrolysis system.
3. In paragraph 1, The above alkaline aqueous solution is supplied to at least one of the preliminary reduction electrode and the oxidation electrode of the preliminary membrane-electrode assembly. A method for manufacturing an anion exchange membrane electrolysis system.
4. In paragraph 1, After the step of manufacturing the preliminary membrane-electrode assembly, a step of connecting an alkaline aqueous solution circulation device to the oxidation electrode of the preliminary membrane-electrode assembly is further included. An alkaline aqueous solution is supplied from the alkaline aqueous solution circulation device to the oxidation electrode of the preliminary membrane-electrode assembly, A method for manufacturing an anion exchange membrane electrolysis system.
5. In paragraph 1, After manufacturing the above preliminary membrane-electrode assembly, a step of connecting an alkaline aqueous solution circulation device for the preliminary reduction electrode and an alkaline aqueous solution circulation device for the oxidation electrode to the preliminary reduction electrode and oxidation electrode of the preliminary membrane-electrode assembly is further included, respectively. An alkaline aqueous solution is supplied from the alkaline aqueous solution circulation device for the preliminary reduction electrode and the alkaline aqueous solution circulation device for the oxidation electrode to the preliminary reduction electrode and oxidation electrode of the preliminary membrane-electrode assembly, respectively. A method for manufacturing an anion exchange membrane electrolysis system.
6. In paragraph 1, After manufacturing the above preliminary membrane-electrode assembly, a step of installing an alkaline circulation device so as to be connected to both the preliminary reduction electrode and the oxidation electrode of the preliminary membrane-electrode assembly is further included. An alkaline aqueous solution is supplied from the alkaline circulation device to the preliminary reduction electrode and oxidation electrode of the preliminary membrane-electrode assembly, A method for manufacturing an anion exchange membrane electrolysis system.
7. In paragraph 1, The above alkaline aqueous solution is a potassium hydroxide aqueous solution having a concentration of 0.1 to 1 M. A method for manufacturing an anion exchange membrane electrolysis system.
8. In paragraph 1, The above NiMo alloy particles have a molar ratio of Ni and Mo of 3:1 and an oxidation number of Mo of 4+, 5+ or 6+. A method for manufacturing an anion exchange membrane electrolysis system.
9. In paragraph 1, The above NiMo alloy particles are manufactured by a manufacturing method including a step of co-precipitating a Ni precursor and a Mo precursor under alkaline conditions and then heat-treating the resulting product. A method for manufacturing an anion exchange membrane electrolysis system.
10. In paragraph 1, The above-mentioned preliminary reduction electrode is manufactured by a manufacturing method including the step of applying a slurry for forming a preliminary reduction electrode including the NiMo-based alloy particles, a binder, and a solvent onto a release film, drying the slurry, and then separating the slurry from the release film. A method for manufacturing an anion exchange membrane electrolysis system.
11. In paragraph 10, The above binder is at least one selected from the group consisting of polytetrafluoroethylene, perfluorosulfonic acid, anion exchange resin, and cation exchange resin. A method for manufacturing an anion exchange membrane electrolysis system.
12. In paragraph 1, As a result of the above activation, a reduction electrode is manufactured, The above reduction electrode comprises a NiMo-based alloy catalyst in which the molar ratio of Ni and Mo is 6:1 to 101:1 and the oxidation number of Mo is 5+ or 6+. A method for manufacturing an anion exchange membrane electrolysis system.
13. In paragraph 12, The above NiMo alloy catalyst comprises a Ni layer on the surface. A method for manufacturing an anion exchange membrane electrolysis system.
14. In paragraph 1, The above oxidation electrode is, It is manufactured by a manufacturing method including a step of applying a slurry for forming an oxidation electrode including an oxidation catalyst, a binder and a solvent onto a release film, drying it and then separating it from the release film, or Manufactured by a manufacturing method including a step of applying, plating or depositing an oxidation catalyst on an electrode substrate. A method for manufacturing an anion exchange membrane electrolysis system.
15. In paragraph 14, The above oxidation catalyst comprises at least one selected from the group consisting of Ni, NiCoFe, Ir, and NiFe-layered double hydroxides. A method for manufacturing an anion exchange membrane electrolysis system.
16. In paragraph 1, After the above activation, the step of checking the cell performance by measuring the current density for each section by maintaining it for 10 seconds in 0.05 V units from 1.45 to 1.9 V is further included. A method for manufacturing an anion exchange membrane electrolysis system.
17. Manufactured using the manufacturing method according to Article 1, A reduction electrode comprising a particulate NiMo alloy catalyst; an oxidation electrode; an anion exchange membrane interposed between the reduction electrode and the oxidation electrode; and an alkaline aqueous solution; The above NiMo alloy catalyst contains Ni and Mo in a molar ratio of 6:1 to 101:1, and the oxidation number of Mo is 5+ or 6+. Anion exchange membrane electrolysis system.
18. In paragraph 17, The above anion exchange membrane electrolysis system, A device comprising an anode-feeding type alkaline solution circulation device connected to the oxidation electrode and supplying an alkaline solution to the oxidation electrode; or a boss-feeding type alkaline solution circulation device connected to both the oxidation electrode and the reduction electrode and supplying an alkaline solution to both the oxidation electrode and the reduction electrode; or a dual-feeding type alkaline solution circulation device for the oxidation electrode, which is composed of an alkaline solution circulation device for the oxidation electrode and an alkaline solution circulation device for the reduction electrode, which are connected to the oxidation electrode and the reduction electrode, respectively. Anion exchange membrane electrolysis system.
19. A pre-anion exchange membrane electrolysis system comprising a pre-reduction electrode, an oxidation electrode, and an anion exchange membrane interposed between the pre-reduction electrode and the oxidation electrode, wherein the pre-reduction electrode comprises NiMo-based alloy particles containing Ni and Mo in a molar ratio of 1:1 to 6:1 and wherein the oxidation number of Mo is 4+, 5+, or 6+. A step of supplying an alkaline aqueous solution, applying a current at a current density of 25 to 200 mA / cm2, and maintaining the current at 50 to 60°C for 90 to 360 minutes to activate the preliminary reduction electrode, Method for activating an anion exchange membrane electrolysis system.
20. In paragraph 19. As a result of the above activation, a reduction electrode is manufactured, The above reduction electrode comprises a NiMo-based alloy catalyst in which the molar ratio of Ni and Mo is 6:1 to 101:1 and the oxidation number of Mo is 5+ or 6+. Method for activating an anion exchange membrane electrolysis system.
Citation Information
Patent Citations
Method for preparing anion exchange membrane water electrolysis sysyem
KR1020240164172A
Method for activating cathode for electrolysis and electrolysis method
JP2007107089A
Method for activating of water electrolysis cell based on anion exchange membrane
KR1020180128562A
Method for electrolyzing alkaline water
US20180334751A1
Water Electrolyzers Employing Anion Exchange Membranes
US20190085471A1