Cathode material, cathode comprising same, and lithium secondary battery

The cathode material with controlled single-particle lithium nickel-based oxide and optional coatings addresses the structural and performance issues of conventional lithium nickel cobalt manganese oxide, improving battery lifespan and output by reducing particle breakage and electrolyte interactions, and maintaining high energy density.

WO2024237716A1PCT designated stage expired Publication Date: 2024-11-21LG CHEM LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/006691
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-14
Filing Date
2024-05-17
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional lithium nickel cobalt manganese oxide cathode materials in lithium secondary batteries face issues such as particle breakage, reduced lifespan, and poor output characteristics due to their secondary particle structure, which leads to increased gas generation and electrolyte interactions, and higher nickel content exacerbates these problems.

Method used

A cathode material with single-particle lithium nickel-based oxide particles, where the primary particle shape is controlled to achieve specific circularity, aspect ratio, and curvature values, and optionally coated with elements like Al, Ti, or Co, to enhance structural stability and lithium mobility.

Benefits of technology

The controlled single-particle cathode material improves lifespan and output characteristics by reducing particle breakage and electrolyte interactions, while maintaining high energy density and mechanical stability, thus enhancing the overall performance of lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006691_21112024_PF_FP_ABST
    Figure KR2024006691_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a cathode material comprising a plurality of discrete-particle-based cathode active material particles. Each of the discrete-particle-based cathode active material particles comprises 1 to 30 primary particles, the ratio of the arithmetic average value of the circularities of the primary particles to the average aspect ratio of the primary particles, which is measured from a segmentation image segmented by primary particle unit and obtained through processing of a scanning electron microscope (SEM) image of the cathode active material, is 0.45 or more, the circularity is defined by the relation 1, and the discrete-particle-based cathode active material comprises a lithium nickel-based oxide having the composition represented by [chemical formula 1]. [Relation 1] Circularity = 4πA / P2 In relation 1, A is the area of each primary particle measured in the segmentation image, and P is the circumferential length of each primary particle measured in the segmentation image. [Chemical formula 1] Lia[NixCoyM1 zM2 1-x-y-z]O2 In chemical formula 1, M1 includes Mn, Al or a combination thereof, M2 includes at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, Al, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P and Sr, 1,0≤a≤1.3, 0.5≤x<1.0, 0<y<0.5 and 0<z<0.5.
Need to check novelty before this filing date? Find Prior Art

Description

Cathode material, cathode containing same, and lithium secondary battery

[0001] Cross-citation with related applications

[0002] This application claims the benefit of priority to Korean Patent Application Nos. 10-2023-0064596, 10-2023-0064597, filed May 18, 2023, and 10-2023-0076140, filed June 14, 2023, the entire disclosure of which is incorporated herein by reference.

[0003] Technology field

[0004] The present invention relates to a cathode material, a cathode including the same, and a lithium secondary battery, and more particularly, to a cathode material including a single-particle cathode active material in which the shape of the primary particles is controlled to satisfy specific conditions, and a cathode including the same and a lithium secondary battery.

[0005]

[0006] A lithium secondary battery is generally composed of a positive electrode, a negative electrode, a separator, and an electrolyte, and the positive electrode and negative electrode include an active material capable of intercalating and deintercalating lithium ions.

[0007] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMnO4, etc.), and lithium iron phosphate compound (LiFePO4) have been used as cathode active materials for lithium secondary batteries. Among these, lithium cobalt oxide has the advantages of high operating voltage and excellent capacity characteristics, but the high price of cobalt, which is the raw material, and its supply are unstable, making it difficult to commercially apply it to large-capacity batteries. Lithium nickel oxide has poor structural stability, making it difficult to achieve sufficient cycle life characteristics. On the other hand, lithium manganese oxide has excellent stability but has the problem of poor capacity characteristics. Therefore, lithium composite transition metal oxides containing two or more transition metals have been developed to complement the problems of lithium transition metal oxides containing only Ni, Co, or Mn. Among these, lithium nickel cobalt manganese oxides containing Ni, Co, and Mn are widely used in the field of electric vehicle batteries.

[0008] Conventional lithium nickel cobalt manganese oxides were generally in the form of spherical secondary particles formed by agglomeration of tens to hundreds of primary particles. However, in the case of lithium nickel cobalt manganese oxides formed in the form of secondary particles formed by agglomeration of many primary particles, there is a problem in that the primary particles are easily broken during the rolling process during the manufacture of the positive electrode, and cracks occur inside the particles during the charge and discharge process. When the positive electrode active material particles are broken or cracked, the contact area with the electrolyte increases, which increases gas generation and active material degradation due to side reactions with the electrolyte, and this causes problems in that the life characteristics are reduced.

[0009] Furthermore, demand for high-power, high-capacity batteries, such as those for electric vehicles, is increasing, leading to a gradual increase in the nickel content of cathode active materials. While increased nickel content improves initial capacity characteristics, repeated charge / discharge cycles can lead to structural collapse of the cathode active material, accelerating its degradation rate and reducing cycle life and battery safety.

[0010] To address the above issues, a technology has been proposed for producing single-particle positive electrode active materials rather than secondary particles by increasing the sintering temperature during the production of lithium nickel cobalt manganese oxide. Single-particle positive electrode active materials have a smaller contact area with the electrolyte than conventional secondary-particle positive electrode active materials, resulting in less side reactions with the electrolyte and superior particle strength, which reduces particle breakage during electrode production. Therefore, the application of single-particle positive electrode active materials offers the advantages of superior gas generation and cycle life characteristics.

[0011] However, in the case of conventional single particle type positive electrode active materials, there is a problem that the interface between primary particles that serve as a passage for lithium ions to move within the particles is small, so lithium mobility is low, resistance is high, and output characteristics are low, and compared to positive electrode active materials in the form of secondary particles, the rolling property is low, so the rolling density is low, and the energy density is low.

[0012]

[0013] The present invention is intended to solve the above problems, and to provide a single-particle cathode material having superior capacity characteristics and resistance characteristics compared to conventional single-particle cathode active materials by controlling the primary particle shape of cathode material powder to satisfy specific conditions.

[0014] In addition, the present invention seeks to provide a cathode and a lithium secondary battery having excellent life characteristics and output characteristics, including the cathode material as described above.

[0015]

[0016] To solve the above problem, the present invention provides a cathode material, a cathode including the cathode material, and a lithium secondary battery including the same.

[0017] (1) The present invention provides a cathode material comprising a plurality of single-particle cathode active material particles, wherein the single-particle cathode active material particles comprise 1 to 30 primary particles, and a ratio of an arithmetic mean value of circularity of the primary particles to an average aspect ratio of the primary particles, which is measured from a segmentation image obtained by image processing a scanning electron microscope (SEM) image of the cathode material and divided into primary particle units, is 0.45 or more, and the circularity is defined by the following formula 1, and the single-particle cathode active material comprises a lithium nickel-based oxide having a composition represented by the following [chemical formula 1].

[0018] [Formula 1] Circularity = 4πA / P 2

[0019] In the above equation 1, A is the area of ​​each primary particle measured in the segmentation image, P is the perimeter of each primary particle measured in the segmentation image,

[0020] [Chemical Formula 1]

[0021] Li a [Ni x Co y M 1 z M 2 1-x-y-z ]O2

[0022] In the above chemical formula 1, M 1 contains Mn, Al or a combination thereof, and M 2It includes at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, Al, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P and Sr, and 1,0≤a≤1.3, 0.5≤x<1.0, 0 <y<0.5, 0<z<0.5이다.

[0023] (2) The present invention provides a cathode material in which the arithmetic mean value of the circularity of the primary particles in the above (1) is 0.65 or more.

[0024] (3) The present invention provides a cathode material in which the average aspect ratio of the primary particles in (1) or (2) is 1.2 to 4.0.

[0025] (4) The present invention provides a cathode material in which the ratio of the arithmetic mean value of the circularity of the primary particles to the average aspect ratio of the primary particles is 0.45 to 0.95 in any one of (1) to (3).

[0026] (5) The present invention provides a cathode material comprising, in any one of (1) to (4) above, a lithium nickel-based oxide having a single particle system and a coating layer formed on the lithium nickel-based oxide, wherein the single particle system cathode active material comprises 1 to 30 primary particles;

[0027] (6) The present invention provides a cathode material in the above (5), wherein the coating layer includes at least one coating element selected from the group consisting of Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb. Mo, Sr, Sb, Bi, Si and S.

[0028] (7) In any one of the above (1) to (6), the cathode material is D 50 This provides a cathode material having a diameter of 2 to 15㎛.

[0029] (8) The present invention provides a cathode material in which the average particle diameter of the primary particles is 1 µm to 6 µm in any one of the above (1) to (7).

[0030] (9) The present invention provides a cathode material, wherein the arithmetic mean value of the curvature of primary particles measured from a segmentation image divided by primary particle unit obtained by image processing a scanning electron microscope image of the cathode material in any one of the above (1) to (8) is 0.92 or more, and the curvature is defined by the following equation 2.

[0031] [Formula 2] Curvature = P c / P r

[0032] In the above equation 2, P r is the actual perimeter of each primary particle measured in the above segmentation image, and P c is the perimeter of a virtual shape obtained by connecting the outermost points of each primary particle measured in the above segmentation image.

[0033] (10) The present invention relates to a cathode material, wherein the arithmetic mean value of the hardness of primary particles measured from a segmentation image divided by primary particle units obtained by image processing a scanning electron microscope image of the cathode material in any one of the above (1) to (9) is 0.85 or more, and the hardness is defined by the following equation 3:

[0034] [Formula 3] Hardness = A r / A c

[0035] In the above equation 3, A r is the actual area of ​​each primary particle measured in the above segmentation image, and A c is the area of ​​a virtual shape obtained by connecting the outermost points of each primary particle measured in the above segmentation image.

[0036] (11) The present invention provides a cathode comprising any one of the cathode materials (1) to (10).

[0037] (12) The present invention provides a lithium secondary battery including the positive electrode of (11).

[0038]

[0039] The cathode material according to the present invention includes a single-particle cathode active material controlled so that the ratio of the arithmetic mean value of the circularity of the primary particles to the average aspect ratio of the primary particles satisfies 0.45 or more, and has superior lithium mobility and rolling characteristics compared to a conventional single-particle cathode active material. Accordingly, when the cathode material according to the present invention is applied, a lithium secondary battery having superior capacity characteristics and life characteristics compared to a conventional battery can be realized.

[0040]

[0041] Figure 1 is a drawing for explaining the curvature according to the present invention.

[0042] Figure 2 is a drawing for explaining the robustness according to the present invention.

[0043] Figure 3 is a scanning electron microscope (SEM) image (A) of a cathode material manufactured by Example 1 and a segmentation image (B) obtained by image processing the SEM image.

[0044] Figure 4 is a scanning electron microscope (SEM) image (A) of a cathode material manufactured by Example 2 and a segmentation image (B) obtained by image processing the SEM image.

[0045] Figure 5 is a scanning electron microscope (SEM) image (A) of a cathode material manufactured by Example 3 and a segmentation image (B) obtained by image processing the SEM image.

[0046] Figure 6 is a scanning electron microscope (SEM) image (A) of a cathode material manufactured by Example 4 and a segmentation image (B) obtained by image processing the SEM image.

[0047] Figure 7 is a scanning electron microscope (SEM) image (A) of a cathode material manufactured by Comparative Example 1 and a segmentation image (B) obtained by image processing the SEM image.

[0048] Figure 8 is a scanning electron microscope (SEM) image (A) of a cathode material manufactured by Comparative Example 2 and a segmentation image (B) obtained by image processing the SEM image.

[0049] Figure 9 is a scanning electron microscope (SEM) image (A) of a cathode material manufactured by Comparative Example 3 and a segmentation image (B) obtained by image processing the SEM image.

[0050]

[0051] Terms or words used in this specification and claims should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical spirit of the present invention, based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best possible manner.

[0052] In the present invention, “primary particle” means a particle unit that has no apparent grain boundary when observed at a magnification of 5,000 to 20,000 times using a scanning electron microscope.

[0053] In the present invention, a "secondary particle" is a particle formed by the aggregation of multiple primary particles. In the present invention, to distinguish it from conventional secondary particles formed by the aggregation of tens to hundreds of primary particles, secondary particles formed by the aggregation of 30 or fewer primary particles are referred to as single-particle cathode active materials.

[0054] In the present invention, “single-particle positive electrode active material” means a positive electrode active material having an average primary particle diameter of 1 µm or more, preferably 1 µm to 5 µm, and composed of 1 to 30 primary particles.

[0055] In the present invention, "D 50" means the particle size at the 50% point of the cumulative volume distribution according to particle size. The above D 50 The particle size distribution can be calculated by dispersing the target powder (e.g., cathode material powder) in a dispersion medium, introducing it into a commercially available laser diffraction particle size measuring device (e.g., Microtrac's S3500), transmitting a laser beam to measure the difference in diffraction pattern according to particle size, and calculating the particle diameter at the point where the volume cumulative distribution according to particle size is 50%.

[0056] In the present invention, “circularity” is an indicator indicating the degree to which the cross-sectional shape of a particle is close to a circle, and is a value defined by the following equation 1.

[0057] [Formula 1] Circularity = 4πA / P 2

[0058] In the above equation 1, A is the area of ​​the cross-section of the particle to be measured, and P is the perimeter length of the cross-section of the particle to be measured.

[0059] In the present invention, “curvature” is an indicator indicating the surface roughness of a particle to be measured, and is a value defined by the following equation 2.

[0060] [Formula 2] Curvature = P c / P r

[0061] In the above equation 2, P r is the actual circumference of the particle being measured, and P c is the perimeter of the virtual shape obtained by connecting the outermost points of the particle to be measured.

[0062] In the present invention, “hardness” is an indicator indicating the surface roughness of a particle to be measured, and is a value defined by the following equation 3.

[0063] [Formula 3] Hardness = A r / A c

[0064] In the above equation 3, A ris the actual area of ​​the particle to be measured, and A c is the area of ​​a virtual shape obtained by connecting the outermost points of the particle to be measured.

[0065] Figure 1 is a drawing for explaining the meaning of curvature according to the present invention. As shown in Figure 1, P r represents the actual circumference of the primary particle, P C represents the circumference of the virtual plane obtained by connecting the outermost points of the primary particles. When the particle surface is formed smoothly without any irregularities, the values ​​of Pr and Pc become similar, so the tortuosity approaches 1. On the other hand, when the particle surface has many irregularities and is rough, the Pr value increases, so the tortuosity decreases. In other words, the smaller the arithmetic mean value of the tortuosity of the primary particles constituting the single-particle positive electrode active material, the more irregularities there are on the primary particle surface.

[0066] Figure 2 is a drawing to explain the meaning of robustness according to the present invention. As shown in Figure 2, A r is the actual area of ​​the primary particle, and A c represents the area of ​​the virtual shape obtained by connecting the outermost points of the primary particle. If the particle surface is formed smoothly without any irregularities, A r and A c As the values ​​of A become similar, the hardness approaches 1. On the other hand, when the particle surface has many irregularities and thus has high roughness, A r As the value decreases, the hardness decreases. That is, the smaller the arithmetic mean value of the hardness of the primary particles constituting the single-particle positive electrode active material, the more unevenness there is on the surface of the primary particles.

[0067] Meanwhile, as particle surface roughness increases, the contact area with the electrolyte increases, and the uneven portions of the particle surface become more susceptible to cracking during electrode rolling, increasing particle breakage and degrading the life characteristics. Therefore, to improve the life characteristics of the cathode material, it is necessary to control the surface shape of the primary particles.

[0068] In the present invention, “aspect ratio” means the ratio of the major diameter to the minor diameter of a particle to be measured.

[0069] In the present invention, the circularity of the primary particles, the curvature of the primary particles, the hardness of the primary particles, the average particle diameter of the primary particles, and the average aspect ratio of the primary particles can be measured from a segmentation image segmented by primary particle unit obtained by image processing a scanning electron microscope (SEM) image of the cathode material using an artificial intelligence model. Specifically, the segmentation image can be obtained by: obtaining a scanning electron microscope (SEM) image of the cathode material powder to be measured; inputting the obtained scanning electron microscope image into a U-NET structure to generate a binary image; converting the binary image into a distance-converted image based on a distance-converted algorithm; filtering the binary image using a threshold value set based on the distance-converted image; identifying a plurality of objects included in the filtered binary image; and segmenting the SEM image by primary particle unit based on the plurality of objects.

[0070]

[0071] Hereinafter, the present invention will be described in more detail.

[0072]

[0073] cathode material

[0074] The cathode material according to the present invention comprises a plurality of single-particle cathode active material particles, wherein the single-particle cathode active material particles comprise 1 to 30 primary particles.

[0075] Single-particle cathode active materials exhibit higher particle strength than conventional secondary particle-type cathode active materials, which consist of tens to hundreds of primary particles aggregated together. Consequently, they are less prone to particle breakage during rolling. Furthermore, because single-particle cathode active materials comprise fewer primary particles, their volumetric expansion and contraction during charge and discharge are minimal, significantly reducing the occurrence of cracks within the particles.

[0076] Therefore, by using the cathode material according to the present invention including a single particle system cathode active material, the electrochemical performance degradation due to particle breakage and crack occurrence can be minimized.

[0077] Meanwhile, the single particle positive electrode active material includes a lithium nickel oxide containing nickel and cobalt.

[0078] At this time, the lower limit of the nickel content among all metals excluding lithium in the lithium nickel-based oxide may be 50 mol% or more, 55 mol% or more, 60 mol% or more, 80 mol% or more, 85 mol% or more, or 88 mol% or more, and the upper limit of the nickel content among all metals excluding lithium may be less than 100 mol%, 99 mol% or less, or 95 mol% or less. When the nickel content in the lithium nickel-based oxide satisfies the above range, high energy density can be realized.

[0079] Specifically, the lithium nickel-based oxide may have a composition represented by the following [chemical formula 1].

[0080] [Chemical Formula 1]

[0081] Li a [Ni x Co y M 1 z M 2 1-x-y-z ]O2

[0082] In the above chemical formula 1, M 1 contains Mn, Al or a combination thereof, and M 2It may include at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, Al, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P and Sr. Preferably, the M 1 It can be Mn or a combination of Mn and Al, and the above M 2 may include Al, Zr, Y, Mg, Ti, Ba, Sr, Mo or a combination thereof, and more preferably may include Zr, Y or a combination thereof. M 2 Although the element is not essential, when included in an appropriate amount, it can play a role in promoting grain growth or improving crystal structure stability during sintering of lithium nickel-based oxides.

[0083] The above a represents the molar ratio of lithium in the lithium nickel-based oxide, and may be 1.0≤a≤1.3, 1.0≤a≤1.2, or 1.0≤a≤1.07. When the molar ratio of lithium satisfies the above range, the crystal structure of the lithium nickel-based oxide can be stably formed.

[0084] The above x represents the molar ratio of nickel among the total metals excluding lithium in the lithium nickel-based oxide, and is 0.5≤x<1.0, 0.55≤x<1.0, 0.60≤x<1.0, 0.80≤x<1.0, 0.85≤x<1.0, 0.88≤x<1.0, 0.5≤x≤0.99, 0.55≤x≤0.99, 0.60≤x≤0.99, 0.80≤x≤0.99, 0.85≤x≤0.99, 0.88≤x≤0.99, 0.5≤x≤0.95, 0.55≤x≤0.95, 0.60≤x≤0.95, 0.80≤x≤0.95, 0.85≤x≤0.95, or It can be 0.88≤x≤0.95. The higher the nickel molar ratio, the more advantageous it is for high capacity implementation.

[0085] The above y represents the molar ratio of cobalt among all metals excluding lithium in the lithium nickel oxide, and is 0. <y<0.5, 0<y<0.45, 0<y<0.4, 0<y<0.2, 0<y<0.15 또는 0<y<0.12일 수 있다.

[0086] The above z is M of all metals except lithium in lithium nickel oxide. 1 It represents the molar ratio of 0 <z<0.5, 0<z<0.45, 0<z<0.4, 0<z<0.2, 0<z<0.15 또는 0<z<0.12일 수 있다.

[0087]

[0088] More specifically, the lithium nickel-based oxide may have a composition represented by the following [Chemical Formula 1-1].

[0089] [Chemical Formula 1-1]

[0090] Li a [Ni x Co y Mn z-w Al w M 2 1-x-y-z ]O2

[0091] In the above chemical formula 1-1, M 2 , a, x, y, z are the same as in chemical formula 1.

[0092] Meanwhile, w represents the molar ratio of Al among metals other than lithium in lithium nickel oxide, and is 0. <w<0.2, 0<w≤0.1, 0<w≤0.05, 0<w≤0.03, 또는 0<w≤0.02일 수 있다. 리튬 니켈계 산화물이 상기 [화학식 1-1]의 조성을 가질 경우, 양극 활물질의 구조 안정성 및 용량 특성이 우수하게 나타난다.

[0093]

[0094] Meanwhile, the single particle positive electrode active material may further include a coating layer formed on the lithium nickel oxide, if necessary.

[0095] At this time, the coating layer may include at least one coating element selected from the group consisting of Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb. Mo, Sr, Sb, Bi, Si and S, and preferably, may include at least one coating element selected from the group consisting of Co, Al, B, W, Ti and Zr.

[0096] When a coating layer exists on the surface of a lithium nickel-based oxide, contact between the electrolyte and the lithium nickel-based oxide is suppressed by the coating layer, thereby reducing the elution of transition metals or gas generation due to side reactions with the electrolyte.

[0097] In particular, when Co, Al or a combination thereof is included as a coating element, the effects of improving output and reducing resistance can be obtained along with the effect of suppressing side reactions with the electrolyte.

[0098]

[0099] The cathode material according to the present invention has a ratio of the arithmetic mean value of the circularity of the primary particles to the average aspect ratio of the primary particles, as measured from a segmentation image obtained by image processing a scanning electron microscope (SEM) image and divided by primary particle unit, of 0.45 or more, specifically 0.45 to 0.95, more specifically 0.45 to 0.90. According to a study by the present inventors, it was shown that when a cathode material in which the ratio of the arithmetic mean value of the circularity of the primary particles to the average aspect ratio of the primary particles satisfies the above range is used, the life characteristics are significantly improved.

[0100] At this time, the circularity of the primary particle is a value defined by the following equation 1.

[0101] [Formula 1] Circularity = 4πA / P 2

[0102] In the above equation 1, A is the area of ​​each primary particle measured in the segmentation image, P is the perimeter of each primary particle measured in the segmentation image,

[0103]

[0104] Analysis of the particle shape of positive electrode active materials is performed using images of positive electrode active material powder obtained through a scanning electron microscope (SEM). However, in the case of SEM images of positive electrode material powder, it is difficult to distinguish aggregated primary particles in the image due to factors such as image resolution, particle agglomeration, and surface roughness. Therefore, a method was previously used in which a person selected individual positive electrode material particles and / or primary particles from the SEM image and manually measured the circumference, aspect ratio, particle size, etc. of the selected particles. However, in this case, quantitative analysis of a large number of positive electrode active material particles is difficult, and the measured values ​​may vary depending on the measurer, which reduces the analysis accuracy. Therefore, it has been difficult to accurately analyze the surface shape of the primary particles of positive electrode active materials in the past, and thus it has been difficult to derive a correlation between the surface shape of the primary particles and battery performance.

[0105] Accordingly, the inventors of the present invention developed a method capable of quantitatively analyzing the surface shape of primary particles in cathode material powder through image analysis using an artificial intelligence model, and found that when the ratio of the arithmetic mean value of the circularity of the primary particles to the average aspect ratio of the primary particles measured according to the analysis method is 0.45 or more, the life characteristics of the single-particle cathode material are significantly improved, thereby completing the present invention.

[0106] The method for analyzing the shape of the cathode material particles according to the present invention is as follows.

[0107] First, a scanning electron microscope image of the cathode material powder to be measured is acquired, and then the acquired scanning electron microscope image is input into an artificial intelligence model to generate a binary image. At this time, the artificial intelligence model may be a model trained to convert an active material image into a binary image. At this time, the training data uses an SEM image of the cathode material powder as a raw image, and a binary image obtained by binarizing the SEM image is used as a label image. The binary image is an image obtained by binarizing the SEM image using a computer vision technique or an image obtained by manually drawing on the SEM image. In addition, in order to train various cases, additional images are generated by applying an image augmentation algorithm (e.g., rotation, tilt, shear, brightness adjustment, contrast adjustment, enlargement, reduction, or a combination thereof) to the raw image and the label image, and these are used as training data.

[0108] Meanwhile, the sizes of the Raw image and Label images may be the same. The image size may be defined as the number of horizontal pixels X the number of vertical pixels, and for example, the sizes of the Raw image and Label image may be 256 X 256.

[0109] Meanwhile, the artificial intelligence model uses a U-NET structure that can reflect the input image by adding a skip connection during the encoding and decoding processes. The artificial intelligence model has a structure in which multiple layers are sequentially connected, and the input of the sequentially connected layers can be the output of the layer connected immediately before, and the output of the sequentially connected layers can be the input of the layer connected immediately after. The layer included in the encoding area has a structure in which a 2D convolution layer, a batch normalization layer, an activation layer, and a max pooling layer are sequentially connected, and the layer included in the decoding area has a structure in which a 2D convolution layer, a batch normalization layer, an activation layer, and an upsampling layer are sequentially connected.

[0110] The training of the artificial intelligence model was done using the deep learning backpropagation algorithm, and the binary cross entropy loss function was used as the loss function. If necessary, the binary cross entropy loss function used a function with a weight between 1 and 1000 applied to one of the two colors (or classes) (e.g., white among black and white).

[0111] Next, the binary image generated from the artificial intelligence model was converted into a distance-transformed image based on a distance-transformation algorithm. The distance-transformation algorithm may be a max-min normalization, Z-score normalization, L1 normalization, or L2 normalization algorithm.

[0112] Next, a filtered binary image is obtained by filtering the binary image using a threshold value set based on the distance transformation image. At this time, the threshold value may be a value obtained by multiplying the normalized maximum distance of the distance transformation image by a specified ratio (e.g., 0 to 0.1). The filtering may be performed by selecting pixels having a distance value lower than the specified threshold value among pixels included in the distance transformation image, and setting the color values ​​of pixels corresponding to the pixels selected from the distance change image among pixels included in the binary image to a specified color value. Through the above method, a filtered image including a plurality of objects is obtained.

[0113] Next, after identifying multiple objects included in the filtered image, the SEM image is segmented based on the multiple objects to obtain a segmented image divided into primary particle units. At this time, the segmentation is performed using the Watershed algorithm.

[0114] Since the segmentation image obtained by the above method represents the positive electrode active material particles in the positive electrode material by dividing them into primary particle units, by using this, various shape information related to the primary particles of the positive electrode active material particles (e.g., circularity of the primary particle, perimeter of the primary particle, area of ​​the primary particle, aspect ratio of the primary particle, convexity of the primary particle, solidity of the primary particle, etc.) can be quantitatively obtained.

[0115] In addition, since the above-described analysis method utilizes an artificial intelligence model that minimizes user input, the problem of measurement values ​​varying depending on the user is minimized, resulting in excellent accuracy and reproducibility.

[0116]

[0117] In the cathode material according to the present invention, the arithmetic mean of the circularity of the primary particles may be 0.65 or more, specifically 0.65 to 0.98, more specifically 0.65 to 0.90, or 0.65 to 0.85. When the arithmetic mean of the circularity of the primary particles is within the above range, lithium ions can diffuse more smoothly into the particles, and the contact area between the single-particle cathode active material and the electrolyte increases, thereby improving battery chemical performance. In addition, since the distance between the particles within the electrode is maintained relatively constant, the flow of current within the electrode is smooth, and the particle arrangement is uniform, the mechanical stability is improved, thereby improving the cycle life of the battery. In addition, it is possible to prevent the friction between single particles within the above range from increasing and the distribution of the single particle positive electrode active material from becoming uneven, thereby reducing the capacity and / or life characteristics of the battery, and at the same time, it is possible to suppress the need for additional processes for excessive crushing or circularization, or the occurrence of particle damage or particle breakage.

[0118]

[0119] In the cathode material according to the present invention, the average aspect ratio of the primary particles may be 1.2 to 4.0, preferably 1.2 to 3.0. Here, the aspect ratio refers to the ratio of the major axis to the minor axis of the primary particles. If the average aspect ratio of the primary particles is too small, the contact between particles may not be good, which may reduce lithium mobility, and if it is too large, the diffusion distance of lithium ions within the particles may increase, which may reduce electrochemical performance, and the distance between particles may become large, which may hinder lithium ion diffusion within the electrode.

[0120]

[0121] In the cathode material according to the present invention, the arithmetic mean value of the curvature of the primary particles may be 0.92 or more, specifically 0.92 to 1.0, and more specifically 0.92 to 0.98.

[0122] At this time, the curvature of the primary particle is a value defined by Equation 2 below.

[0123] [Formula 2] Curvature = P c / P r

[0124] In the above equation 2, P r is the actual perimeter of each primary particle measured in the above segmentation image, and P c is the perimeter of a virtual shape obtained by connecting the outermost points of each primary particle measured in the above segmentation image.

[0125] The anode material according to the present invention may have an arithmetic mean value of the hardness of the primary particles, measured from a segmentation image obtained by processing a scanning electron microscope (SEM) image and divided into primary particle units, of 0.85 or more, specifically 0.85 to 1.0, and more specifically 0.85 to 0.98.

[0126] At this time, the hardness of the primary particle is a value defined by the following equation 3.

[0127] [Formula 3] Hardness = A r / A c

[0128] In the above equation 1, A r is the actual area of ​​each primary particle measured in the above segmentation image, and A c is the area of ​​a virtual shape obtained by connecting the outermost points of each primary particle measured in the above segmentation image.

[0129] When the arithmetic mean of the curvature of the primary particles and / or the arithmetic mean of the hardness of the primary particles are within the above range, the particle surface roughness increases, the contact area with the electrolyte increases, and the uneven portion is prevented from breaking during electrode rolling, thereby increasing particle breakage, and thus the life characteristics of the battery can be improved.

[0130]

[0131] In the cathode material according to the present invention, the single particle cathode active material is D 50 This may be 2㎛ to 15㎛, preferably 3㎛ to 10㎛, more preferably 3㎛ to 8㎛. D of the positive electrode active material 50 If this is too small, it is difficult to form an active material layer during electrode manufacturing, the electrolyte impregnation property is poor, and the electrochemical properties are deteriorated. 50 If this is too large, there is a problem that the resistance increases and the output characteristics deteriorate.

[0132]

[0133] In addition, in the cathode material according to the present invention, the average particle diameter of the primary particles may be 1 μm to 6 μm, preferably 1 μm to 5 μm, and more preferably 1 μm to 4 μm. When the average particle diameter of the primary particles satisfies the above range, a single-particle cathode active material having excellent electrochemical properties can be formed. If the average particle diameter of the primary particles is too small, the number of agglomerates of the primary particles forming the lithium nickel-based oxide particles increases, which reduces the effect of suppressing particle breakage during rolling, and if the average particle diameter of the primary particles is too large, the lithium diffusion path within the primary particles becomes long, which may increase resistance and deteriorate output characteristics.

[0134]

[0135] Method for manufacturing cathode material

[0136] Next, a method for manufacturing a cathode material according to the present invention will be described.

[0137] The method for manufacturing a cathode material according to the present invention comprises: (1) a step of mixing a transition metal precursor and a first lithium raw material and then performing a first firing to form a first fired product including a single-particle lithium nickel-based oxide including 1 to 30 primary particles; (2) a first crushing step of crushing the first fired product; (3) a step of mixing the crushed first fired product and a second lithium raw material and then performing a second firing to form a second fired product; and (4) a second crushing step of crushing the second fired product.

[0138]

[0139] (1) Step of forming the first plastic product

[0140] First, the transition metal precursor and the first lithium raw material are mixed and then calcined for the first time to form the first calcined product.

[0141] At this time, the transition metal precursor may be purchased and used as a commercially available precursor such as nickel-cobalt-manganese hydroxide, or may be manufactured according to a precursor manufacturing method known in the art.

[0142] Preferably, the transition metal precursor may be a transition metal hydroxide represented by the following [chemical formula 2].

[0143] [Chemical Formula 2]

[0144] [Ni x1 Co y1 M 1 z1 M 2 1-x1-y1-z1](OH)2

[0145] In the above chemical formula 2, M 1 and M 2 is the same as defined in chemical formula 1. That is, M 1 contains Mn, Al or a combination thereof, and M 2It includes at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, Al, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P and Sr.

[0146] Meanwhile, x1 represents the molar ratio of nickel among all metal elements in the transition metal precursor, 0.5≤x1<1.0, 0.55≤x1<1.0, 0.60≤x1<1.0, 0.80≤x1<1.0, 0.85≤x1<1.0, 0.88≤x1<1.0, 0.5≤x1≤0.99, 0.55≤x1≤0.99, 0.60≤x1≤0.99, 0.80≤x1≤0.99, 0.85≤x1≤0.99, 0.88≤x1≤0.99, 0.5≤x1≤0.95, 0.55≤x1≤0.95, 0.60≤x1≤0.95, 0.80≤x1≤0.95, It can be 0.85≤x1≤0.95, or 0.88≤x1≤0.95.

[0147]

[0148] The above y1 represents the molar ratio of cobalt among the total metals in the transition metal precursor, 0 <y1<0.5, 0<y1<0.45, 0<y1<0.4, 0<y1<0.2, 0<y1<0.15 또는 0<y1<0.12일 수 있다.

[0149] The above z1 is M among all metals in the transition metal precursor. 1 It represents the molar ratio of 0 <z1<0.5, 0<z1<0.45, 0<z1<0.4, 0<z1<0.2, 0<z1<0.15 또는 0<z1<0.12일 수 있다.

[0150]

[0151] The above transition metal precursor can be prepared, for example, by introducing a transition metal aqueous solution and an ammonium cation complex forming and basic compound into a reactor and performing a co-precipitation reaction while stirring.

[0152] The above transition metal aqueous solution can be prepared by dissolving a transition metal-containing raw material in a solvent such as water, and for example, it can be prepared by dissolving a nickel-containing raw material or a cobalt-containing raw material in water. In addition, if necessary, the above transition metal aqueous solution can be prepared by dissolving M 1 Raw materials and / or M 2 It may further include metal-containing raw materials.

[0153] Meanwhile, the above transition metal-containing raw material may be an acetate, carbonate, nitrate, sulfate, halite, sulfide, or oxide of the transition metal.

[0154] Specifically, the nickel-containing raw material may be, for example, NiO, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, nickel halide, or a combination thereof.

[0155] The above cobalt-containing raw material is, for example, CoSO 4, It can be Co(OCOCH3)2ㆍ4H2O, Co(NO3)2ㆍ6H2O, CoSO4ㆍ7H2O, or a combination thereof.

[0156] Above M 1 The containing raw material may be a manganese-containing raw material and / or an aluminum-containing raw material. The manganese-containing raw material may be, for example, Mn2O3, MnO2, Mn3O4MnCO3, Mn(NO3)2, MnSO4ㆍH2O, manganese acetate, manganese halides, or combinations thereof, and the aluminum-containing raw material may be, for example, Al2O3, Al(OH)3, Al(NO3)3, Al2(SO4)3, (HO)2AlCH3CO2, HOAl(CH3CO2)2, Al(CH3CO2)3aluminum halides, or combinations thereof. However, in the case of Al, instead of being added to the transition metal aqueous solution, it may be introduced together with the lithium raw material in the calcination step described later.

[0157] M 2 Contains raw materials M 2 It may be an acetate, carbonate, nitrate, sulfate, halite, sulfide or oxide of the metal.

[0158] The input amount of each of the above transition metal-containing raw materials can be determined by considering the molar ratio of the transition metal in the positive electrode active material to be ultimately produced.

[0159] Meanwhile, the ammonium cation complex forming agent may include at least one compound selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and NH4CO3, and may be introduced into the reactor in the form of a solution in which the compound is dissolved in a solvent. At this time, the solvent may be water or a mixture of water and an organic solvent (specifically, alcohol, etc.) that can be uniformly mixed with water.

[0160] The basic compound may be at least one compound selected from the group consisting of NaOH, KOH, and Ca(OH)2, and may be introduced into the reactor in the form of a solution in which the compound is dissolved in a solvent. At this time, the solvent may be water, or a mixture of water and an organic solvent (specifically, alcohol, etc.) that can be uniformly mixed with water.

[0161] As described above, when a transition metal aqueous solution, an ammonium cation complex forming agent, and a basic compound are introduced into a reactor and stirred, the transition metals in the transition metal aqueous solution coprecipitate, generating precursor particles in the form of transition metal hydroxides.

[0162] At this time, the above transition metal aqueous solution, ammonium cation complex forming agent, and basic compound are added in an amount such that the pH of the reaction solution becomes within the desired range.

[0163] Once precursor particles are formed as described above, the particles are separated from the reaction solution to obtain a transition metal precursor. For example, the reaction solution may be filtered to separate the transition metal precursor, and then the separated transition metal precursor may be washed and dried to obtain the transition metal precursor. Processes such as grinding and / or classification may also be performed as needed.

[0164]

[0165] Next, the transition metal precursor and the first lithium raw material are mixed and then fired for the first time to form a first fired product including a single-particle lithium nickel oxide including 1 to 30 primary particles. At this time, if necessary, an aluminum-containing raw material and / or M 2 Metal-containing raw materials can be mixed and fired together.

[0166] As the first lithium raw material, lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide or oxyhydroxide may be used, and for example, Li2CO3, LiNO3, LiNO2, LiOH, LiOHㆍH2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, Li3C6H5O7 or a mixture thereof may be used.

[0167] Meanwhile, the first lithium raw material may be mixed so that the molar ratio of lithium to the total molar ratio of transition metals included in the transition metal precursor is 0.9 to 1.1, preferably 0.95 to 1.07, and more preferably 1 to 1.05. When the molar ratio of the transition metal precursor and the first lithium raw material satisfies the above range, the layered crystal structure of the positive electrode active material is well developed, so that a positive electrode material with excellent electrochemical performance can be manufactured.

[0168]

[0169] Meanwhile, the above primary calcination is performed under conditions in which the primary particles grow to 1 μm or more to form single-particle lithium nickel oxide.

[0170] The appropriate first firing temperature may vary depending on the metal composition in the precursor, and for example, when the nickel (Ni) content is 80 mol% or more, the first firing may be performed at a temperature of 800°C to 950°C, preferably 820°C to 950°C, and more preferably 850°C to 950°C.

[0171] Additionally, the first firing time may be 5 to 35 hours, preferably 5 to 20 hours, and more preferably 5 to 15 hours.

[0172] Additionally, the above-mentioned primary firing may be performed in an oxygen atmosphere. In the present specification, the term "oxygen atmosphere" refers to an atmosphere containing oxygen sufficient for firing, including an atmospheric atmosphere. In particular, it is preferable to perform the firing in an atmosphere with a higher oxygen partial pressure than an atmospheric atmosphere.

[0173] When the first sintering is performed under the above conditions, a single-particle lithium nickel oxide with excellent electrochemical properties can be formed. If the first sintering temperature and time are too low, the primary particles do not grow sufficiently, resulting in the production of a cathode active material in the form of secondary particles. If the temperature and time are too high, an excessive amount of electrically inactive rock-salt phase is formed during the sintering process, resulting in a structurally unstable sintered product with low crystallinity, which may result in deterioration of the electrochemical properties.

[0174]

[0175] (2) First crushing stage

[0176] When a primary fired product is formed through the primary firing as described above, a first crushing step of crushing the primary fired product is performed.

[0177] The above first crushing step is intended to crush the agglomerated positive electrode active materials and to appropriately control the particle size and shape of the particles in the positive electrode material, and can be performed using a crushing device well known in the art, such as a jet-mill crusher or a ball-mill crusher.

[0178]

[0179] By appropriately controlling the grinding conditions such as grinding pressure, classification speed, etc. in the first grinding step, the particle size distribution (D50) and primary particle shape and aspect ratio of the lithium nickel oxide particles can be controlled.

[0180] For example, the first crushing step may be performed under crushing pressure conditions of 1.5 bar to 2.5 bar, preferably 1.5 bar to 2.4 bar, and more preferably 1.5 bar to 2.3 bar. When the crushing pressure of the first crushing step satisfies the above range, it is easy to manufacture a cathode material having the desired arithmetic mean value of the curvature of the primary particles.

[0181] In addition, the first crushing step may be performed at a classification speed of 800 rpm to 1800 rpm, preferably 900 rpm to 1800 rpm, and more preferably 900 rpm to 1700 rpm. When the classification speed of the first crushing step satisfies the above range, the D of the positive electrode material 50 And / or it is easy to control the average particle diameter of the primary particles within a desired range.

[0182]

[0183] (3) Step of forming a secondary plastic product

[0184] Next, the primary calcined product crushed through the first crushing step is mixed with the secondary lithium raw material and then subjected to a secondary calcination.

[0185] At this time, lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide or oxyhydroxide may be used as the second lithium raw material, and for example, Li2CO3, LiNO3, LiNO2, LiOH, LiOHㆍH2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, Li3C6H5O7 or a mixture thereof may be used. The second lithium raw material may be the same as or different from the first lithium raw material.

[0186]

[0187] Meanwhile, the second lithium raw material may be mixed so that the molar ratio of lithium to the total molar ratio of transition metals included in the transition metal precursor is 0.005 to 0.1, preferably 0.005 to 0.05, and more preferably 0.005 to 0.04. When the amount of the second lithium raw material input satisfies the above range, it is easy to manufacture a cathode material having primary particles of a desired shape without deteriorating the properties of the cathode material. If the secondary calcination is performed without inputting the second lithium raw material, there is a problem that the reaction speed is slow, requiring high temperature and long-term calcination, and even if the second lithium raw material is input, if the amount input is too little, the effect of reducing the rock salt structure on the surface of the single-particle lithium nickel-based oxide is minimal, and if the amount input is too much, lithium byproducts may increase, which may deteriorate the electrochemical performance.

[0188] As described above, when a secondary lithium raw material is additionally added and secondary calcination is performed, lithium is inserted into the rock salt structure that can be formed on the surface of a single-particle lithium nickel oxide, and the layered structure is restored, thereby improving crystallinity, and the surface of the primary particle is formed smoothly during the secondary calcination process, making it easy to manufacture a cathode material having the desired degree of curvature.

[0189] Meanwhile, the secondary firing may be performed at a temperature 50°C to 100°C lower than the primary firing temperature. If the secondary firing temperature is higher than the primary firing temperature, an excessive amount of rock salt phase may occur on the surface of the lithium nickel-based oxide, causing the surface to deteriorate and lithium byproducts to remain, which may result in a decrease in electrochemical properties. In addition, if the secondary firing temperature is 100°C or more lower than the primary firing temperature, the lithium insertion rate may be slowed down, resulting in a decrease in electrochemical performance and a minimal improvement in primary particle curvature. For example, the secondary firing temperature may be 700°C to 850°C, preferably 750°C to 850°C, and more preferably 750°C to 840°C.

[0190] Meanwhile, the secondary firing time may be, for example, 5 to 35 hours, preferably 5 to 20 hours, and more preferably 5 to 15 hours, in order to increase the crystallinity of the internal crystal structure of the positive electrode active material.

[0191] Additionally, the secondary firing can be performed in an oxygen atmosphere.

[0192] When secondary firing is performed under the above conditions, a cathode material having excellent electrochemical properties and the desired primary particle shape can be easily formed.

[0193]

[0194] (4) Second crushing stage

[0195] Next, a second crushing step is performed to crush the secondary sintered product obtained through the secondary sintering. At this time, the crushing pressure of the second crushing step is preferably lower than that of the first crushing step. If the crushing pressure of the second crushing step is higher than that of the first crushing step, excessive crushing occurs, making it difficult to form the surface shape of the primary particles within the desired range, and in severe cases, fracture surfaces may occur in the single-particle lithium nickel-based oxide particles.

[0196] For example, the second crushing step may be performed under crushing pressure conditions of 0.4 bar to 1.4 bar, 0.5 bar to 1.4 bar, or 0.6 bar to 1.3 bar.

[0197] In addition, the second crushing step may be performed at a classification speed of 800 rpm to 1800 rpm, preferably 900 rpm to 1800 rpm, and more preferably 900 rpm to 1700 rpm. When the classification speed of the second crushing step satisfies the above range, it is easy to control the D50 and / or the average particle diameter of the primary particles within a desired range.

[0198]

[0199] (5) Coating step

[0200] Meanwhile, the method for manufacturing a cathode material according to the present invention may further include, if necessary, a step of mixing the pulverized second sintered product and the coating raw material after the second pulverization step and then performing heat treatment to form a coating layer.

[0201] The above coating raw material may be an acetate, carbonate, nitrate, sulfate, halite, sulfide or oxide containing a coating element.

[0202] Meanwhile, the above mixing may be performed as a solid-state mixing or a liquid-state mixing, and the heat treatment may be performed at an appropriate temperature depending on the type of element to be coated. For example, the heat treatment may be performed at a temperature of 200°C to 800°C, preferably 400°C to 750°C. In addition, the heat treatment may be performed in two or more stages at different temperatures.

[0203] The above heat treatment can be performed for 1 to 10 hours, specifically 2 to 8 hours, and more specifically 3 to 6 hours, in order to increase the crystallinity of the coating portion.

[0204]

[0205] The cathode material manufactured by the above method comprises a plurality of single-particle cathode active material particles. In addition, when measured from a segmented image obtained by image processing a scanning electron microscope (SEM) image of the cathode material and divided into primary particle units, the ratio of the arithmetic mean of the circularity of the primary particles to the average aspect ratio of the primary particles may be 0.45 or more. In addition, other physical properties of the cathode material according to the present invention may be satisfied.

[0206]

[0207] anode

[0208] Next, the anode according to the present invention will be described.

[0209] The positive electrode according to the present invention comprises a positive electrode active material layer comprising a positive electrode material according to the present invention. Specifically, the positive electrode comprises a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and comprising the positive electrode material.

[0210] In the above positive electrode, the positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 ㎛, and fine unevenness may be formed on the surface of the positive electrode current collector to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.

[0211]

[0212] In addition, the positive electrode active material layer may include a conductive material and a binder together with the positive electrode material described above.

[0213] The conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any particular limitation. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotube; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used. The conductive material may typically be included in an amount of 1 to 30 wt%, preferably 1 to 20 wt%, and more preferably 1 to 10 wt%, based on the total weight of the positive electrode active material layer.

[0214] The above binder serves to improve adhesion between positive electrode active material particles and adhesion between the positive electrode active material and the positive electrode current collector. Specific examples thereof include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof. The above binder may be included in an amount of 1 to 30 wt%, preferably 1 to 20 wt%, and more preferably 1 to 10 wt%, based on the total weight of the positive electrode active material layer.

[0215] The above positive electrode can be manufactured according to a conventional positive electrode manufacturing method. For example, the positive electrode can be manufactured by mixing a positive electrode material, a binder, and / or a conductive material in a solvent to manufacture a positive electrode slurry, applying the positive electrode slurry onto a positive electrode current collector, and then drying and rolling.

[0216] The solvent may be a solvent generally used in the relevant technical field, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water. One of these may be used alone or a mixture of two or more thereof may be used. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode material, conductive material, and binder, taking into account the coating thickness and manufacturing yield of the slurry, and to have a viscosity that can exhibit excellent thickness uniformity when applied thereafter for manufacturing the positive electrode.

[0217] Alternatively, the positive electrode may be manufactured by casting the positive electrode slurry onto a separate support, then peeling the resulting film from the support and laminating it onto a positive electrode current collector.

[0218]

[0219] lithium secondary battery

[0220] Next, a lithium secondary battery according to the present invention will be described.

[0221] The lithium secondary battery of the present invention comprises the positive electrode according to the present invention. Specifically, the lithium secondary battery comprises a positive electrode, a negative electrode positioned opposite the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode is as described above. In addition, the lithium secondary battery may optionally further comprise a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0222]

[0223] In the above lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer positioned on the negative electrode current collector.

[0224] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. In addition, the negative electrode current collector can typically have a thickness of 3 to 500 ㎛, and like the positive electrode current collector, fine unevenness can be formed on the surface of the current collector to strengthen the bonding strength of the negative electrode active material. For example, it can be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven fabric, etc.

[0225] The above negative electrode active material layer optionally includes a binder and a conductive material together with the negative electrode active material.

[0226] As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; SiO β (0 <β< 2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the above metal compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used.

[0227] In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbon material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include amorphous, plate-like, flaky, spherical or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.

[0228] The conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any particular limitation. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotube; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used. The conductive material may typically be included in an amount of 1 to 30 wt%, preferably 1 to 20 wt%, and more preferably 1 to 10 wt%, based on the total weight of the negative electrode active material layer.

[0229] The above binder serves to improve adhesion between negative electrode active material particles and adhesion between the negative electrode active material and the negative electrode current collector. Specific examples thereof include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof may be used. The above binder may be included in an amount of 1 to 30 wt%, preferably 1 to 20 wt%, and more preferably 1 to 10 wt%, based on the total weight of the negative electrode active material layer.

[0230] The above-described negative electrode active material layer may be manufactured by, for example, applying a negative electrode slurry containing a negative electrode active material and optionally a binder and a conductive material onto a negative electrode current collector and drying it, or by casting the negative electrode slurry onto a separate support and then laminating the resulting film onto a negative electrode current collector by peeling it off from the support.

[0231]

[0232] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in lithium secondary batteries can be used without special restrictions, and in particular, one having low resistance to ion movement of the electrolyte and excellent electrolyte moisture retention capacity is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. can also be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength can be used, and can optionally be used in a single-layer or multi-layer structure.

[0233]

[0234] In addition, examples of the electrolyte used in the present invention include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.

[0235]

[0236] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0237] The organic solvent may be used without any particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; Carbonate solvents such as dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (wherein R is a C2 to C20 linear, branched, or cyclic hydrocarbon group, and may include a double-bonded aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, a carbonate solvent is preferable, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery and a linear carbonate compound having low viscosity (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate, etc.) is more preferable.

[0238]

[0239] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl04, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2. LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within the range of 0.1 to 5.0 M, and preferably 0.1 to 3.0 M. When the concentration of the lithium salt is within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.

[0240]

[0241] In addition to the electrolyte components, the electrolyte may further include additives for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery. For example, the additives may include haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexamethylphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, either singly or in mixtures, but are not limited thereto. The additives may be included in an amount of 0.1 to 10 wt%, preferably 0.1 to 5 wt%, based on the total weight of the electrolyte.

[0242]

[0243] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement them. However, the present invention may be implemented in various different forms and is not limited to the embodiments described herein.

[0244]

[0245] Example 1

[0246] D 50 This 4.20㎛ transition metal precursor Ni 0.885 Co 0.035 Mn 0.08 (OH)2 and LiOH were mixed so that the molar ratio of Ni+Co+Mn:Li was 1:1.03, and Al(OH)3, Y2O3, and ZrO2 were mixed in amounts of 1470 ppm, 1000 ppm, and 1500 ppm, respectively, based on the total weight of the transition metal precursor, to prepare a mixture. Then, the mixture was first fired at 890°C to 900°C for 6 hours to obtain a first fired product.

[0247] Then, the above primary sintered product was pulverized using a jet-mill pulverizer at room temperature under the conditions of a pulverizing pressure of 2.1 bar and a classification speed of 1600 rpm (first pulverization stage).

[0248] Next, the crushed primary calcined product and LiOH were mixed so that the molar ratio of Ni+Co+Mn:Li was 1:0.01, and the secondary calcined product was obtained by secondary calcination at 820°C for 9 hours.

[0249] Then, the above secondary sintered product was pulverized using a jet-mill pulverizer at room temperature under the conditions of pulverizing pressure of 0.9 bar and classification speed of 1600 rpm to obtain single particle lithium nickel oxide LiNi. 0.8784 Co 0.0347 Mn 0.0794 Al 0.005 Zr 0.0015 Y 0.001 O2 was obtained (second crushing stage)

[0250] Next, the single-particle lithium nickel-based oxide obtained above and Co(OH)2, Al(OH)3 were uniformly mixed, heat-treated at 700°C for 5 hours in an oxygen atmosphere, and then heat-treated at 500°C for 3 hours to manufacture a cathode material having a coating layer formed thereon. At this time, the Co(OH)2 was mixed in an amount such that the ratio (B / A) of the number of moles of Co (B) in Co(OH)2 to the total number of moles (A) of the remaining metals excluding lithium in the lithium nickel-based oxide was 0.02, and the Al(OH)3 was mixed in an amount of 0.05 parts by weight per 100 parts by weight of the lithium nickel-based oxide.

[0251]

[0252] Example 2

[0253] A cathode material was manufactured in the same manner as in Example 1, except that the first crushing step was performed at a crushing pressure of 1.6 bar.

[0254]

[0255] Example 3

[0256] D 50 This 4.2㎛ transition metal precursor Ni 0.885 Co 0.035 Mn 0.08 (OH)2 and LiOH were mixed so that the molar ratio of Ni+Co+Mn:Li was 1:1, and Al(OH)3, Y2O3, and ZrO2 were mixed in amounts of 1470 ppm, 1000 ppm, and 1500 ppm, respectively, based on the total weight of the transition metal precursor, to prepare a mixture. Then, the mixture was first fired at 850°C for 12 hours to obtain a first fired product.

[0257] Then, the above primary sintered product was pulverized using a jet-mill pulverizer at room temperature under the conditions of a pulverizing pressure of 2.1 bar and a classification speed of 1600 rpm (first pulverization stage).

[0258] Next, the crushed primary calcined product and LiOH were mixed so that the molar ratio of Ni+Co+Mn:Li was 1:0.05, and the secondary calcined product was obtained by secondary calcination at 800°C for 12 hours.

[0259] Then, the above secondary sintered product was pulverized using a jet-mill pulverizer at room temperature under the conditions of pulverizing pressure of 0.9 bar and classification speed of 1600 rpm to obtain single particle lithium nickel oxide LiNi. 0.8784 Co 0.0347 Mn 0.0794 Al 0.005 Zr 0.0015 Y 0.001 O2 was obtained (second crushing stage)

[0260] Next, the single-particle lithium nickel-based oxide obtained above and Co(OH)2 were uniformly mixed, and then heat-treated at 700°C for 5 hours in an oxygen atmosphere to form a Co coating layer on the surface of the single-particle lithium nickel-based oxide. Then, the Co-coated single-particle lithium nickel-based oxide and Al(OH)3 were uniformly mixed, and then heat-treated at 500°C for 5 hours in an oxygen atmosphere to form a Co and Al-coated single-particle lithium nickel-based oxide. At this time, the Co(OH)2 was mixed in an amount such that the ratio (B / A) of the number of moles of Co in Co(OH)2 to the total number of moles (A) of the remaining metals excluding lithium in the lithium nickel-based oxide was 0.02, and the Al(OH)3 was mixed in an amount of 0.05 parts by weight per 100 parts by weight of the lithium nickel-based oxide.

[0261]

[0262] Example 4

[0263] D 50 This 5.50㎛ transition metal precursor Ni 0.905 Co 0.085 Mn 0.01(OH)2 and LiOH were mixed so that the molar ratio of Ni+Co+Mn:Li was 1:1, and Al(OH)3, Y2O3, and ZrO2 were mixed thereto in amounts of 1470 ppm, 1000 ppm, and 1500 ppm, respectively, based on the total weight of the transition metal precursor, to prepare a mixture. Then, the mixture was first fired at 820°C for 12 hours to obtain a first fired product.

[0264] Then, the above primary sintered product was pulverized using a jet-mill pulverizer at room temperature under the conditions of a pulverizing pressure of 1.5 bar and a classification speed of 1250 rpm (first pulverization stage).

[0265] Next, the crushed primary calcined product and LiOH were mixed so that the molar ratio of Ni+Co+Mn:Li was 1:0.03, and the secondary calcined product was obtained by secondary calcination at 770°C for 12 hours.

[0266] Then, the above secondary sintered product was pulverized using a jet-mill pulverizer at room temperature under the conditions of pulverizing pressure of 0.6 bar and classification speed of 1250 rpm to obtain single particle lithium nickel oxide LiNi. 0.8982 Co 0.0844 Mn 0.0099 Al 0.005 Zr 0.0015 Y 0.001 O2 was obtained (second crushing stage)

[0267] Next, the single-particle lithium nickel-based oxide obtained above and Co(OH)2, Al(OH)3 were uniformly mixed, heat-treated at 700°C for 5 hours in an oxygen atmosphere, and then heat-treated at 500°C for 3 hours to manufacture a cathode material having a coating layer formed thereon. At this time, the Co(OH)2 was mixed in an amount such that the ratio (B / A) of the number of moles of Co (B) in Co(OH)2 to the total number of moles (A) of the remaining metals excluding lithium in the lithium nickel-based oxide was 0.02, and the Al(OH)3 was mixed in an amount of 0.05 parts by weight per 100 parts by weight of the lithium nickel-based oxide.

[0268]

[0269] Comparative Example 1 - Manufacturing OS instead of TS

[0270] D 50 This 4.20㎛ transition metal precursor Ni 0.885 Co 0.035 Mn 0.08 (OH)2 and LiOH were mixed so that the molar ratio of Ni+Co+Mn:Li was 1:1.05, and Al(OH)3, Y2O3, and ZrO2 were mixed in amounts of 1470 ppm, 1000 ppm, and 1500 ppm, respectively, relative to the total weight of the transition metal precursor, to prepare a mixture.

[0271] Then, the mixture was calcined at 880°C for 3 hours, then calcined again at 800°C for 9 hours, and then D was calcined at room temperature using a jet-mill pulverizer at a pulverizing pressure of 2.1 bar and a grading speed of 1600 rpm. 50 LiNi is a single particle lithium nickel oxide that is pulverized to 3.8㎛. 0.8784 Co 0.0347 Mn 0.0794 Al 0.005 Zr 0.0015 Y 0.001 Got O2.

[0272] Next, the single-particle lithium nickel-based oxide obtained above and Co(OH)2, Al(OH)3 were uniformly mixed, heat-treated at 700°C for 5 hours in an oxygen atmosphere, and then heat-treated at 500°C for 3 hours to manufacture a cathode material having a coating layer formed thereon. At this time, the Co(OH)2 was mixed in an amount such that the ratio (B / A) of the number of moles of Co (B) in Co(OH)2 to the total number of moles (A) of the remaining metals excluding lithium in the lithium nickel-based oxide was 0.02, and the Al(OH)3 was mixed in an amount of 0.05 parts by weight per 100 parts by weight of the lithium nickel-based oxide.

[0273]

[0274] Comparative Example 2 - Second crushing is performed at a higher crushing pressure than the first crushing.

[0275] A cathode material was manufactured in the same manner as in Example 1, except that the first crushing step was performed at a crushing pressure of 1.6 bar and the second crushing step was performed at a crushing pressure of 2.1 bar.

[0276]

[0277] Comparative Example 3 - Performing only the second crushing without the first crushing

[0278] A cathode material was manufactured in the same manner as in Example 1, except that the secondary firing was performed without crushing the primary fired product and the secondary fired product was crushed at a crushing pressure of 2.1 bar.

[0279]

[0280] 1st firing 1st crushing 2nd firing 2nd crushing Example 1890~900℃, 6hr 2.1bar, 1600rpm 820℃, 9hr 0.9bar, 1600rpm Example 2890~900℃, 6hr 1.6bar, 1600rpm 820℃, 9hr 0.9bar, 1600rpm Example 3850℃, 12hr 2.1bar, 1600rpm 800℃, 12hr 0.9bar, 1600rpm Example 4820℃, 12hr 1.5bar, 1250rpm 770℃, 12hr 0.6bar, 1250rpm Comparative Example 1890℃, 3hr, 800℃, 9hr 2.1bar, 1600rpm XX Comparative Example 2890~900℃, 6hr1.6bar, 1600rpm820℃, 9hr2.1bar, 1600rpmComparative example 3890~900℃, 6hrX820℃, 8hr2.1bar, 1600rpm

[0281]

[0282] Experimental Example 1 - Measurement of circularity and curvature

[0283] After obtaining scanning electron microscope images of the cathode materials manufactured by Examples 1 to 4 and Comparative Examples 1 to 3 through a scanning electron microscope, each image was image-processed using the particle shape analysis method described above to obtain segmentation images divided by primary particle unit. The SEM images and segmentation images of each cathode material manufactured by Examples 1 to 4 and Comparative Examples 1 to 3 are illustrated in FIGS. 3 to 9. In FIGS. 3 to 9, (A) is an SEM image, and (B) is a segmentation image obtained by image-processing the SEM image.

[0284] From the above segmentation image, the arithmetic mean of the circularity of the primary particles, the arithmetic mean of the curvature of the primary particles, the average particle diameter of the primary particles, and the average aspect ratio of the primary particles were measured.

[0285] In addition, 0.01 g of the cathode powder manufactured by Examples 1 to 4 and Comparative Examples 1 to 3 was collected, placed in a vial containing 30 ml of ultrapure water and 500 μl of dispersant, dispersed for 1 minute using a sonicator, and then placed in a particle size analyzer (PSA) (Microtrac, S3500) to measure the D of the cathode powder. 50 was measured.

[0286] The measurement results are shown in Table 2 below.

[0287]

[0288] Arithmetic mean of circularityAverage aspect ratio of primary particlesArithmetic mean of circularity of primary particles to the average aspect ratio of primary particlesAverage particle diameter of primary particles (㎛)D 50(㎛) Arithmetic mean of curvature Arithmetic mean of hardness Example 10.72 26 1.38 7 30.5 15 9 3.0 6 23 3.8 20.9 36 4 0.9 12 1 Example 20.7 15 31.40 7 9 0.50 47 2.99 0 23.70 0.93 6 20.90 78 Example 30.67 9 11.40 9 30.48 19 2.73 6 9 3.87 0.92 7 4 0.88 45 Example 40.68 0 7 1.43 8 30.47 3 34.0 25 26.17 0.92 7 9 0.88 8 Comparative example 10.56471.54730.38272.82363.780.87260.8402Comparative Example 20.61161.47680.41422.31343.410.91140.8387Comparative Example 30.62661.46300.42662.38374.070.91130.8328

[0289]

[0290] Experimental Example 2

[0291] Each of the cathode materials, conductive material (FX35), and binder (a mixture of KF9700 and BM730H in a weight ratio of 2.8:0.2) manufactured by Examples 1 to 4 and Comparative Examples 1 to 3 was mixed in N-methylpyrrolidone in a weight ratio of 95:2:3 to manufacture a cathode slurry. The cathode slurry was applied to one surface of an aluminum current collector, dried at 130°C, and then rolled to manufacture a cathode.

[0292] An electrode assembly was manufactured by interposing a porous polyethylene separator between each manufactured positive electrode and a lithium metal disk, and then positioning this inside a battery case, and injecting an electrolyte to manufacture a half-cell. The electrolyte was manufactured by dissolving LiPF6 at a concentration of 1 M in a mixed organic solvent containing ethylene carbonate: ethyl methyl carbonate: and diethyl carbonate in a volume ratio of 3:3:4.

[0293]

[0294] (1) Initial capacity

[0295] For each lithium secondary battery manufactured above, the battery was charged to 4.25 V in CC / CV mode at 25°C with 0.1 C and 0.5 C cut-off conditions, and then discharged to 2.5 V in CC mode to measure the initial discharge capacity.

[0296]

[0297] (2) Life characteristics

[0298] For each lithium secondary battery manufactured above, 50 cycles of charge and discharge were repeated at 45°C in a voltage range of 2.5 to 4.25 V, and the capacity retention rate and resistance increase rate at 50 cycles were measured. At this time, the charge was performed in CCCV mode to 4.25 V, and cut-off was performed when the voltage reached 0.05 C, and the discharge was performed in CC mode until the voltage reached 2.5 V.

[0299] The capacity retention rate was measured as the percentage of the discharge capacity after 50 cycles to the discharge capacity after 1 cycle ((discharge capacity after 50 cycles / discharge capacity after 1 cycle) × 100), and the resistance increase rate was measured as the percentage of the resistance after 50 cycles to the resistance after 1 cycle ({(resistance after 50 cycles - resistance after 1 cycle) / resistance after 1 cycle)} × 100).

[0300] The measurement results are shown in Table 3 below.

[0301]

[0302] Initial charge capacity (mAh / g) Initial discharge capacity (mAh / g) Initial efficiency (%) Capacity retention rate (%) Resistance increase rate (%) Example 1 231.4 206.5 89.29 6.54 0.3 Example 2 230.9 205.9 89.29 6.34 2.0 Example 3 232.0 205.0 88.49 6.34 6.8 Example 4 233.1 206.3 88.5 96.0 5 0.5 Comparative example 1 230.7 201.8 87.5 95.264.2 Comparative example 2 230.3 203.4 88.394.75 8.1 Comparative example 3 228.8 201.287.9 ​​95.667.4

[0303] Through the above Table 3, it can be confirmed that the batteries using the positive electrode materials of Examples 1 to 4, in which the ratio of the arithmetic mean value of the circularity of the primary particles to the average aspect ratio of the primary particles is 0.45 or more, have a superior capacity retention rate after 50 cycles and a smaller increase in resistance than the batteries using the positive electrode materials of Comparative Examples 1 to 3.

Claims

1. A cathode material comprising a plurality of single-particle cathode active material particles, The above single particle positive electrode active material particles include 1 to 30 primary particles, The ratio of the arithmetic mean of the circularity of the primary particles to the average aspect ratio of the primary particles, measured from a segmentation image obtained by image processing a scanning electron microscope (SEM) image of the above cathode material, is 0.45 or more, The above circularity is defined by the following equation 1, The above single particle positive electrode active material is a positive electrode material including a lithium nickel oxide having a composition represented by the following [chemical formula 1]: [Formula 1] Circularity = 4πA / P 2 In the above equation 1, A is the area of ​​each primary particle measured in the segmentation image, P is the perimeter of each primary particle measured in the segmentation image, [Chemical Formula 1] Li a [Ni x Co y M 1 z M 2 1-x-y-z ]O2 In the above chemical formula 1, M 1 contains Mn, Al or a combination thereof, and M 2 It includes at least one selected from the group consisting of B, Ba, Ce, Cr, F, Mg, Al, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P and Sr, and 1,0≤a≤1.3, 0.5≤x<1.0, 0 <y<0.5, 0<z<0.5이다.

2. In claim 1, A cathode material having an arithmetic mean of the circularity of the above primary particles of 0.65 or more.

3. In claim 1, A cathode material having an average aspect ratio of the above primary particles of 1.2 to 4.

0.

4. In claim 1, A cathode material wherein the ratio of the arithmetic mean value of the circularity of the primary particles to the average aspect ratio of the primary particles is 0.45 to 0.

95.

5. In claim 1, A cathode material comprising a lithium nickel-based oxide having 1 to 30 primary particles, wherein the single-particle cathode active material comprises a coating layer formed on the lithium nickel-based oxide.

6. In claim 5, A cathode material, wherein the coating layer comprises at least one coating element selected from the group consisting of Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb. Mo, Sr, Sb, Bi, Si and S.

7. In claim 1, The above cathode material is D 50 This cathode material is 2 to 15㎛.

8. In claim 1, A cathode material having an average particle diameter of the primary particles of 1 ㎛ to 6 ㎛.

9. In claim 1, A cathode material, wherein the arithmetic mean value of the curvature of primary particles measured from a segmentation image obtained by image processing a scanning electron microscope image of the cathode material and divided by primary particle unit is 0.92 or more, and the curvature is defined by the following equation 2: [Formula 2] Curvature = P c / P r In the above equation 2, P r is the actual perimeter of each primary particle measured in the above segmentation image, and P c is the perimeter of a virtual shape obtained by connecting the outermost points of each primary particle measured in the above segmentation image.

10. In claim 1, A cathode material, wherein the arithmetic mean value of the hardness of primary particles measured from a segmentation image obtained by image processing a scanning electron microscope image of the cathode material and divided into primary particle units is 0.85 or more, and the hardness is defined by the following equation 3: [Formula 3] Hardness = A r / A c In the above equation 3, A r is the actual area of ​​each primary particle measured in the above segmentation image, and A c is the area of ​​a virtual shape obtained by connecting the outermost points of each primary particle measured in the above segmentation image.

11. A cathode comprising the cathode material of any one of claims 1 to 10.

12. A lithium secondary battery comprising the positive electrode of claim 11.

Citation Information

Patent Citations

  • Positive electrode material, positive electrod and lithium secondary battery comprising the same

    KR102833612B1

  • Active material, battery, and method for manufacturing electrode

    JP2010262826A

  • Electroactive materials for metal-ion batteries

    KR1020170128491A

  • Apparatus for Massaging whole body with a Plural of Rotational Balls

    KR1020210100579A

  • Foldable support scaffold to aid in bowel movement

    KR1020220155008A