Electrolyte additive comprising metal nitrate, lithium metal battery using same, and manufacturing method therefor

The use of a polymer nanofiber structure with metal nitrate as an electrolyte additive addresses the stability issues in lithium metal batteries by forming a stable SEI, enhancing electrochemical performance and battery stability.

WO2024237719A1PCT designated stage expired Publication Date: 2024-11-21KOREA ADVANCED INST OF SCI & TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/006694
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-05-16
Filing Date
2024-05-17
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Lithium metal batteries face stability issues due to low solubility of existing electrolyte additives in carbonate solvents, leading to early exhaustion and inadequate formation of a stable solid electrolyte interphase (SEI), which affects the battery's lifespan and performance.

Method used

A polymer nanofiber structure with metal nitrate, such as lithium nitrate or rubidium nitrate, is used as an electrolyte additive, supported on the nanofibers, which forms a stable SEI through electrospinning, enhancing ionic conductivity and uniform lithium deposition.

Benefits of technology

The solution significantly improves the electrochemical performance and stability of lithium metal batteries by forming a stable SEI with improved ionic conductivity and uniform lithium deposition, extending the battery's lifespan and maintaining high capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006694_21112024_PF_FP_ABST
    Figure KR2024006694_21112024_PF_FP_ABST
Patent Text Reader

Abstract

An embodiment of the present invention provides a lithium metal battery having remarkably excellent electrochemical performance and stability compared to a lithium metal battery using an existing commercial carbonate electrolyte by providing an intermediate layer prepared from an electrolyte additive, in which a large amount of metal nitrate is supported through electrospinning of a polymer solution having a metal nitrate dissolved therein, and by allowing the intermediate layer to be further included in a lithium metal battery using a carbonate electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte additive containing metal nitrate, lithium metal battery using the same, and method for manufacturing the same

[0001] Cross-citation with related application(s)

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0063582, filed May 17, 2023, and Korean Patent Application No. 10-2024-0063612, filed May 16, 2024, the entire contents of which are incorporated herein by reference.

[0003] The present invention relates to an electrolyte additive containing a metal nitrate, a lithium metal battery using the same, and a method for manufacturing the same. More specifically, the present invention relates to an electrolyte additive for an intermediate layer capable of inducing uniform lithium desorption and simultaneously forming a stable solid electrolyte interphase (SEI) to increase the stability of a carbonate electrolyte for a high-capacity lithium metal battery, a lithium metal battery using the same, and a method for manufacturing the same.

[0004] Lithium metal batteries are secondary batteries that use lithium metal as an anode material, boasting high energy density. Compared to the graphite anodes used in conventional lithium-ion batteries, they offer a higher operating voltage and a theoretical capacity more than 10 times higher (372 mAh / g vs. 203860 mAh / g), enabling them to store more energy.

[0005] However, lithium metal anodes pose a high risk of short circuits and fire, requiring improved stability for commercialization. Lithium reacts with the electrolyte, consuming the electrolyte and forming a solid electrolyte interphase (SEI). When deposited on the electrode, it forms dendrites. The thick SEI, formed during charge / discharge processes due to the increased surface area caused by the dendrites, and the lithium released from the electrode increase the overvoltage, leading to electrode deterioration.

[0006] To achieve high capacity in lithium-ion batteries, metal oxide cathodes have been used, and carbonate electrolytes, which have a wide voltage window and are relatively inexpensive, have been commercialized. However, the carbonate electrolytes used in lithium metal batteries have low stability, and thus, ether electrolytes, which have a narrow voltage window but high stability, have been used in conjunction with cathode materials with low operating voltages.

[0007] Recently, various electrolyte additive technologies have been developed to address these issues. However, most utilize high-concentration ether electrolytes, resulting in high costs and difficulties with high-voltage applications. This not only increases battery costs but also complicates full-cell operation using various cathode materials.

[0008] Therefore, for stable full-cell operation of lithium metal batteries, it is necessary to induce uniform lithium deposition and desorption by adding additives to the carbonate electrolyte while simultaneously forming a stable SEI. However, previously known electrolyte additives have low solubility in carbonate solvents and electrolytes, which makes it difficult to form a stable SEI due to premature depletion during battery charging and discharging, and there was a problem that the life characteristics of lithium metal batteries could not be sufficiently improved.

[0009] The technical problem to be achieved by the present invention is to provide an electrolyte additive for manufacturing an intermediate layer capable of increasing the stability of a carbonate electrolyte, inducing uniform lithium desorption and formation of a stable SEI, and a lithium metal battery using the same, and a manufacturing method thereof, for a high-capacity lithium metal battery capable of overcoming the limited solubility of nitrate.

[0010] The technical problems to be solved by the present invention are not limited to the technical problems mentioned above, and other technical problems not mentioned can be clearly understood by a person having ordinary skill in the technical field to which the present invention belongs from the description below.

[0011] In order to achieve the above technical task, one embodiment of the present invention provides an electrolyte additive comprising a polymer nanofiber structure; and a metal nitrate supported on the polymer nanofiber structure, wherein the metal nitrate comprises lithium nitrate or rubidium nitrate.

[0012] In an embodiment of the present invention, the polymer nanofiber structure includes polyvinylpyrrolidone (PVP), polyvinylidene fluoride (PVDF) or polyacrylonitrile (PAN), and may include fibers obtained by electrospinning these polymers.

[0013] In an embodiment of the present invention, the polymer nanofiber structure may have a fiber diameter of 100 to 500 nm.

[0014] In an embodiment of the present invention, the metal nitrate may be included in an amount of 10 to 70 wt% based on the total weight of the electrolyte additive.

[0015] In order to achieve the above technical task, another embodiment of the present invention provides a lithium metal battery comprising: a lithium metal negative electrode; an intermediate layer in the form of nanofibers, positioned on the negative electrode and made from an electrolyte and an electrolyte additive; a separator positioned on the intermediate layer; and a positive electrode positioned on the separator.

[0016] In an embodiment of the present invention, a solid electrolyte interphase (SEI) having improved ionic conductivity can be formed on the intermediate layer by nitrate anions formed through decomposition of metal nitrate.

[0017] Additionally, the intermediate layer may have a thickness of 10 to 40 μm.

[0018] In order to achieve the above technical task, another embodiment of the present invention provides a method for manufacturing a lithium metal battery, comprising the steps of: preparing an electrolyte additive which is a mixture of a polymer and a metal nitrate; preparing an intermediate layer from the electrolyte and the electrolyte additive; and arranging a lithium metal negative electrode under the intermediate layer and sequentially arranging a separator and a positive electrode over the intermediate layer.

[0019] In an embodiment of the present invention, in the step of preparing the electrolyte additive, the mixing weight ratio of the metal nitrate and the polymer may be 1:2 to 3:1.

[0020] In an embodiment of the present invention, the step of manufacturing the intermediate layer may be characterized in that it is performed through an electrospinning method.

[0021] In an embodiment of the present invention, the electrospinning method can be performed under a voltage of 8 kV to 25 kV.

[0022] According to an embodiment of the present invention, an intermediate layer supporting a large amount of metal nitrate can be manufactured using an electrolyte additive, which is a polymer solution containing an electrolyte and a predetermined metal nitrate, through electrospinning. This provides a lithium metal battery with significantly superior electrochemical performance and stability compared to lithium metal batteries using existing commercial carbonate electrolytes.

[0023] In a lithium metal battery according to the present invention, anions can form a solid electrolyte interphase (SEI) composed of a large amount of inorganic compounds through an intermediate layer manufactured from an additive containing nitrate, and at the same time, cations can induce uniform lithium deposition through a nucleation seed or charge shielding effect.

[0024] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the detailed description of the present invention or the composition of the invention described in the claims.

[0025] FIG. 1 schematically illustrates the structure of a lithium metal battery including a PAN intermediate layer loaded with a metal nitrate according to one embodiment of the present invention.

[0026] FIG. 2 schematically illustrates an example of a method for manufacturing a PAN intermediate layer loaded with a metal nitrate and an electrospinning device according to one embodiment of the present invention.

[0027] Figure 3 shows a schematic diagram of the expected effect when the manufactured intermediate layer is applied to a lithium metal battery.

[0028] Figure 4 shows a scanning electron microscope (SEM) analysis photograph according to Example 1.

[0029] Figure 5 shows a scanning electron microscope (SEM) analysis photograph according to Example 2.

[0030] Figure 6 shows an SEM analysis photograph of an intermediate layer (CsPAN) formed with a PAN nanofiber layer loaded with CsNO3 according to Example 3.

[0031] Figure 7 is a graph showing the coulombic efficiency per cycle of a half-cell cell to evaluate lithium reversibility according to comparative examples and examples.

[0032] Figure 8 is an image obtained through scanning electron microscopy and focused ion beam (FIB) cross-sectional analysis to evaluate the electrodeposition morphology of lithium electrodes according to comparative examples and examples.

[0033] Figure 9 shows the results of capacity and coulombic efficiency per cycle for evaluating the overall battery performance according to comparative examples and examples.

[0034] Hereinafter, the present invention will be described with reference to the attached drawings. However, the present invention can be implemented in various different forms and is therefore not limited to the embodiments described herein. In the drawings, irrelevant parts have been omitted for clarity of description, and similar parts have been designated with similar reference numerals throughout the specification.

[0035] Throughout the specification, when a part is said to be "connected (connected, contacted, or coupled)" to another part, this includes not only cases where it is "directly connected," but also cases where it is "indirectly connected" with another part in between. Furthermore, when a part is said to "include" a component, this does not exclude other components, but rather implies that it may include other components, unless otherwise specifically stated.

[0036] The terminology used herein is merely used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this specification, it should be understood that the terms "comprises" or "has" indicate the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but do not exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0037]

[0038] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings.

[0039] “LiPAN” refers to an intermediate layer formed of a PAN nanofiber layer loaded with lithium nitrate (LiNO3).

[0040] “RbPAN” refers to an intermediate layer formed of a PAN nanofiber layer loaded with rubidium nitrate (RbNO3).

[0041]

[0042] An electrolyte additive according to one embodiment of the present invention comprises a polymer nanofiber structure; and a metal nitrate supported on the polymer nanofiber structure, wherein the metal nitrate may include lithium nitrate or rubidium nitrate. Since the polymer intermediate layer prepared from the electrolyte additive is located between the lithium anode and the separator in a lithium metal battery, the metal nitrate supported on the polymer nanofiber structure readily reacts with the lithium anode and functions as an additive.

[0043] The above polymer nanofiber structure may include a polymer selected from the group consisting of polyvinylpyrrolidone (PVP), polyvinylidene fluoride (PVDF), and polyacrylonitrile (PAN), and these polymers may be electrospun to form a polymer nanofiber structure having a fiber shape.

[0044] In these polymer nanofiber structures, each fiber may have a fiber diameter of, for example, 100 to 500 nm, or 150 to 450 nm, and these nanofibers may have an entangled form.

[0045] The above metal nitrate may be included in an amount of 10 to 70 wt% relative to the total weight of the intermediate layer or electrolyte additive.

[0046] FIG. 1 schematically illustrates the structure of a lithium metal battery including a PAN intermediate layer loaded with a metal nitrate according to one embodiment of the present invention.

[0047] A lithium metal battery according to another embodiment of the present invention is described with reference to FIG. 1.

[0048] A lithium metal battery according to one embodiment of the present invention may include a lithium metal anode; an intermediate layer in the form of a nanofiber structure, positioned on the anode and made from an electrolyte and an electrolyte additive; a separator positioned on the intermediate layer; and a cathode positioned on the separator.

[0049] FIG. 2 schematically illustrates an example of a method for manufacturing a PAN intermediate layer loaded with a metal nitrate according to one embodiment of the present invention and an electrospinning device applied thereto.

[0050] Referring to FIG. 2, a method for manufacturing a lithium metal battery according to another embodiment of the present invention is described below.

[0051] A method for manufacturing a lithium metal battery according to one embodiment of the present invention may include the steps of preparing an electrolyte additive which is a mixture of a polymer and a metal nitrate; preparing an intermediate layer from the electrolyte and the electrolyte additive; and arranging a lithium metal negative electrode under the intermediate layer and sequentially arranging a separator and a positive electrode over the intermediate layer.

[0052] First, a step is to prepare an electrolyte additive, which is a mixture of a polymer and a metal nitrate. A mixture is prepared by dissolving and dispersing the metal nitrate and a polymer selected from the group consisting of, for example, polyvinylpyrrolidone (PVP), polyvinylidene fluoride (PVDF), or polyacrylonitrile (PAN) in a solvent. The solvent used here may be dimethyl formamide (DMF).

[0053] The step of preparing the above electrolyte additive may be performed under an inert gas atmosphere. This is to prevent moisture from being contained in the mixture during the process of dissolving and dispersing the metal nitrate and polymer in the solvent.

[0054] In the step of preparing the above electrolyte additive, the mixing ratio of the metal nitrate and the polymer may be 1:2 to 3:1.

[0055] The following is a step for manufacturing an intermediate layer. This step for manufacturing the intermediate layer can be performed using electrospinning. Through this electrospinning method, the polymer nanofiber structure can be obtained from the polymer.

[0056] Electrospinning is a method for manufacturing nanofibers by dissolving or melting a polymer and extruding it through a spinneret. This method can produce nanofibers with a large surface area per unit weight, high porosity, and thinness. The intermediate layer according to an embodiment of the present invention can be obtained in the form of a polymer nanofiber structure by transforming a PAN polymer dissolved in a solvent into a nanofiber form using electrospinning. The surface area of ​​the metal nitrate can increase depending on the degree of dispersion.

[0057] When the above electrospinning method is performed, the applied voltage range may be 8 kV to 25 kV. If the voltage range is lower than 8 kV, electrospinning may not occur, and if it is higher than 25 kV, spinning may not occur in the form of nanofibers. However, the voltage range is not limited thereto and may vary depending on the concentration of the mixture, additives, or spinning distance.

[0058] An additional step of drying the intermediate layer may be included. After electrospinning is completed, drying in a vacuum oven can be performed to confirm the final synthesis of the intermediate layer in the form of nanofibers.

[0059] Finally, a lithium metal negative electrode can be placed on the lower portion of the intermediate layer, and a separator and a positive electrode can be sequentially placed on the upper portion of the intermediate layer to manufacture a lithium metal battery.

[0060]

[0061] The polymer nanofiber structure and the polymer intermediate layer containing the metal nitrate are manufactured through electrospinning. Additives with low solubility, which are difficult to apply to electrolytes, can be loaded in large quantities through the polymer intermediate layer. The loaded additives slowly dissolve in the electrolyte, exerting their effects over a long period of time, thereby enhancing the stability of lithium metal when used in lithium metal batteries.

[0062]

[0063] Figure 3 shows a schematic diagram of the expected effect when the manufactured intermediate layer is applied to a lithium metal battery.

[0064] Referring to Fig. 3, a solid electrolyte interphase (SEI) with improved ionic conductivity can be formed by nitrate anions generated through the decomposition of the metal nitrate in the intermediate layer. Meanwhile, the metal cations generated through the decomposition of the metal nitrate in the intermediate layer can be reduced to a metallic form on the lithium surface and act as nucleation seeds, thereby inducing uniform lithium deposition.

[0065] When an intermediate layer is applied to a lithium metal anode in this way, a stable SEI can be formed through the decomposition of metal nitrate, and the metal ions exhibit a uniform lithium deposition shape depending on their type.

[0066] Meanwhile, the lithium metal battery may follow the configuration of a general lithium metal secondary battery, except that it includes a lithium metal negative electrode and an intermediate layer including the polymer nanofiber structure and metal nitrate.

[0067] In such lithium metal batteries, an electrolyte including a non-aqueous organic solvent and a lithium salt may be supported in the intermediate layer.

[0068] The lithium salt included in the above electrolyte is used as a medium for transferring ions within the secondary battery. The lithium salt is, for example, Li as a cation. + Including, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO2 - , PF6 - , CF3SO3 - , CH3CO2 -, CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - , BF2C2O4 - , BC4O8 - , PF4C2O4 - , PF2C4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - and SCN - It may include an anion selected from the group consisting of .

[0069] Specifically, the lithium salt is LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 , LiAlCl4, LiAlO2, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiFSI (Lithium bis(fluorosulfonyl) imide, LiN(SO2F)2), LiBF2(C2O4), LiBETI (lithium bis(perfluoroethanesulfonyl) imide, LiN(SO2CF2CF3)2) and LiTFSI (lithium bis(trifluoromethanesulfonyl) imide, LiN(SO2CF3)2).

[0070] The concentration of the above lithium salt can be appropriately changed within a commonly usable range, and can be included in the electrolyte at a concentration of 0.4 M to 6 M, or a concentration of 0.5 M to 5 M.

[0071] Meanwhile, the type of non-aqueous organic solvent that can be included in the electrolyte is not particularly limited, and any organic solvent previously known to be applicable to electrolytes of lithium ion batteries, etc., can be used. Examples of such organic solvents include at least one selected from the group consisting of carbonate solvents, ether solvents, nitrile solvents, phosphate solvents, and sulfone solvents.

[0072] More specifically, as the carbonate solvent, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, methyl propyl carbonate, ethyl methyl carbonate, ethyl propyl carbonate or methyl (2,2,2-trifluoroethyl) carbonate can be used, and as the phosphate solvent, trimethyl phosphate, triethyl phosphate or 2-(2,2,2-trifluoroethoxy)-1,3,2-dioxaphosphorane 2-oxide can be used.

[0073] In addition, as the ether solvent, dibutyl ether, tetraglyme, diglyme, dimethoxy ethane, or tetrahydrofuran derivatives such as 2-methyl tetrahydrofuran can be used, and as the nitrile solvent, succinonitrile, adiponitrile, sebaconitrile, acetonitrile, or propionitrile can be used. In addition, as the sulfone solvent, dimethyl sulfone, ethylmethyl sulfone, or sulforane can be used.

[0074] Meanwhile, in the lithium metal battery, the positive electrode may include a positive electrode current collector and a positive electrode active material layer positioned on the positive electrode current collector.

[0075] These positive electrodes can be manufactured by mixing an active material and a binder, and in some cases, a conductive material, a filler, etc. in a solvent to prepare a positive electrode slurry composition, and applying the composition to a positive electrode current collector.

[0076] The positive electrode current collector may generally have a thickness of 3 to 500 μm. In addition, the positive electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. The current collector may also form fine unevenness on its surface to increase the adhesive strength of the positive electrode active material, and various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric are possible.

[0077] And, in the case of the above positive electrode active material, it may include a compound capable of reversible intercalation and deintercalation of lithium, specifically a lithium metal oxide containing one or more metals such as iron, cobalt, manganese, nickel, or aluminum and lithium.

[0078] Specifically, the lithium metal oxide is a lithium-manganese oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-cobalt oxide (e.g., LiCoO2, etc.), a lithium-nickel oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese oxide (e.g., LiNi 1-Y Mn Y O2 (here, 0 <Y<1), LiMn 2-Z Ni Z O4 (where 0<Z<2), etc.), lithium-nickel-cobalt oxides (e.g., LiNi 1-Y1 CoY1 O2 (here, 0 <Y1<1) 등), 리튬-망간-코발트계 산화물(예를 들면, LiCo 1-Y2 Mn Y2 O2 (here, 0 <Y2<1), LiMn 2-Z1 Co Z1 O4 (wherein, 0<Z1<2) etc.), lithium-nickel-manganese-cobalt oxides (e.g., Li(Ni p Co q Mn r )O2(wherein, 0<p<1, 0<q<1, 0<r<1, p+q+r=1) or Li(Ni p1 Co q1 Mn r1 )O4 (wherein, 0<p1<2, 0<q1<2, 0<r1<2, p1+q1+r1=2) etc.), lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r2 M s2 )O2 (wherein, M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg and Mo, and p2, q2, r2 and s2 are atomic fractions of independent elements, respectively, 0<p2<1, 0<q2<1, 0<r2<1, 0<s2<1, p2+q2+r2+s2=1), etc.), or lithium iron phosphate (e.g., Li 1+a Fe 1-x M x (PO 4-b )X b (Here, M is at least one selected from Al, Mg, and Ti, X is at least one selected from F, S, and N, -0.5≤a≤+0.5, 0≤x≤0.5, 0≤b≤0.1), and any one or two or more compounds thereof may be included.

[0079] Among these, the positive electrode active material includes a lithium metal oxide including lithium and two or more metals selected from the group consisting of nickel, manganese, cobalt, and aluminum, and the lithium metal oxide may include nickel in an amount of 50 mol% or more, or 60 to 99 mol%, or 70 to 95 mol%, based on the total metal content excluding lithium. Such a lithium metal oxide may be represented by, for example, the following chemical formula 1:

[0080] [Chemical Formula 1]

[0081] Li x Ni a Co b M 1 c M 2 d O2

[0082] In the above chemical formula 1, the M 1 Mn and Al may be one or more selected from or a combination thereof, and M 2 may be at least one selected from the group consisting of Zr, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, F, P and S, and may be 0.90≤x≤1.1, or 0.95≤x≤1.08, or 1.0≤x≤1.08, and may be 0.50≤a<1.0, or 0.60≤a≤0.99, or 0.70≤a≤0.95. In addition, 0 <b≤0.3이고, 0<c≤0.3이고, 0≤d≤0.1일 수 있다.

[0083] By using a lithium metal oxide containing such a high nickel content as a positive electrode active material and combining it with an anode of one embodiment, the output and capacity characteristics, life characteristics, etc. of a lithium metal battery can be further improved.

[0084] The above-described positive electrode active material may be included in an amount of 60 to 99 wt%, or 70 to 99 wt%, or 80 to 98 wt% based on the total weight of the positive electrode active material layer.

[0085] Meanwhile, the conductive material included in the positive electrode active material layer is a component for further improving the conductivity of the positive electrode active material. The conductive material is not particularly limited as long as it has conductivity without causing chemical changes in the battery. For example, carbon powder such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, or graphite with a highly developed crystal structure; conductive nanomaterials such as carbon nanofibers or carbon nanotubes; fluorinated carbon powder; conductive powder such as aluminum powder or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc. can be used. Among these, the conductive material can further lower the resistance of the lithium metal battery and improve the output characteristics, etc. by including a conductive nanomaterial such as carbon nanotubes or carbon nanofibers.

[0086] Typically, the conductive material may be included in an amount of 1 to 20 wt%, or 1 to 15 wt%, or 1 to 10 wt% based on the total weight of the positive electrode active material layer.

[0087] The binder optionally included in the above-described positive electrode active material layer is a component that assists in the bonding of the positive electrode active material and the conductive material, and in the bonding to the current collector. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene (PE), polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, nitrile rubber, styrene-butadiene rubber, or fluororubber, and a mixture or copolymer of two or more selected from these may also be used.

[0088] Typically, the binder may be included in an amount of 1 to 20 wt%, or 1 to 15 wt%, or 1 to 10 wt% based on the total weight of the positive electrode active material layer.

[0089] Meanwhile, the lithium metal battery described above may further include a porous separator interposed between the positive electrode and the negative electrode. More specifically, the separator may be positioned between the intermediate layer and the positive electrode.

[0090] These porous separators can be made of olefin polymers such as polyethylene and polypropylene, glass fibers, etc. in the form of sheets, multi-layer films, microporous films, woven fabrics, and non-woven fabrics, but are not necessarily limited thereto. However, it may be preferable to use porous polyethylene or porous glass fiber non-woven fabric (glass filter) as the separator, and it may be more preferable to use porous glass filter (glass fiber non-woven fabric) as the separator. The separator may be an insulating thin film having high ion permeability and mechanical strength, and the pore diameter of the separator may generally be in the range of 0.01 to 10 ㎛, and the thickness may generally be in the range of 5 to 300 ㎛, but is not limited thereto.

[0091]

[0092] Hereinafter, the embodiments, comparative examples, and experimental examples of the invention will be described in detail.

[0093] Comparative Example 1 represents a lithium metal battery using a carbonate electrolyte (1M LiPF6in EC / DEC / FEC) without an intermediate layer and a lithium metal negative electrode, Example 1 comprises a PAN intermediate layer without a metal nitrate, Example 2 comprises a LiPAN nanofiber intermediate layer with lithium nitrate added as the metal nitrate, and Example 3 represents a lithium metal battery comprising a RbPAN nanofiber intermediate layer with rubidium nitrate added as the metal nitrate, respectively.

[0094]

[0095] Comparative Example 1: Carbonate electrolyte without metal nitrate additive (1M LiPF6in EC / DEC / FEC, 45:45:10)

[0096] A commercially available 1M LiPF6in EC / DEC / FEC electrolyte with 10 vol% FEC added to a conventional lithium ion battery electrolyte (1M LiPF6in EC / DEC) was used.

[0097]

[0098] Example 1: Polymer nanofiber (PAN) interlayer without metal nitrate addition

[0099] 7 wt% polyacrylonitrile (PAN) was mixed with DMF solvent and stirred for 12 hours to prepare a completely dissolved mixture (PAN / DMF). The mixture was transferred to a Luer lock syringe and equipped with an electrospinning needle. The electrospinning conditions were a voltage of 15–20 kV, a flow rate of 0.5–1 ml / hr, and a spinning distance of approximately 15 cm. The electrospun aluminum foil was dried in a vacuum oven at a temperature of approximately 60°C under a vacuum atmosphere for more than 12 hours.

[0100] Fig. 4 shows a scanning electron microscope (SEM) analysis photograph according to Example 1. Referring to Fig. 4, it can be confirmed that a nanofiber-shaped intermediate layer is synthesized through the electrospinning method of the above example.

[0101]

[0102] Example 2: LiPAN nanofiber interlayer

[0103] In Example 2, a polymer nanofiber (PAN) intermediate layer carrying lithium nitrate (LiNO3) in the intermediate layer of Example 1 was used.

[0104] In Example 2, a mixture containing an additive (LiNO3-PAN / DMF) was prepared by additionally dissolving lithium nitrate and PAN in a weight ratio of 2:3 to 4:5 in the PAN-DMF mixture prepared as in Example 1. To prevent moisture from being contained during the dissolution and dispersion process, the process was performed in an argon atmosphere glove box and stirred for about 12 hours. The mixture was transferred to a Luer lock syringe and equipped with an electrospinning needle. The electrospinning conditions were a voltage of 15 to 20 kV, a flow rate of 0.3 to 0.5 ml / hr, and a spinning distance of about 15 cm. The aluminum foil on which electrospinning was completed was dried in a vacuum oven at a temperature of about 60 °C under a vacuum atmosphere for more than 12 hours.

[0105] Fig. 5 shows a scanning electron microscope (SEM) analysis photograph according to Example 2. Referring to Fig. 5, it can be confirmed that a nanofiber-shaped intermediate layer was synthesized through the electrospinning method of Example 2, and that an intermediate layer uniformly loaded with LiNO3 was synthesized.

[0106]

[0107] Example 3: RbPAN nanofiber interlayer

[0108] In Example 3, a polymer nanofiber (PAN) intermediate layer containing rubidium nitrate (RbNO3) was used as the intermediate layer in Example 1.

[0109] In Example 3, the particle size of rubidium nitrate was reduced through a ball milling process using a stainless steel ball-milling bottle and zirconia balls.

[0110] In Example 3, RbPAN particles of about 5 μm, obtained through a ball milling process for about 2 hours in the PAN-DMF mixture prepared as in Example 1, were dissolved and dispersed together with PAN in a DMF solvent at a weight ratio of about 1:1. To prevent moisture from being contained during the dissolution and dispersion process, the process was performed in a glove box with an argon atmosphere, and after stirring for about 12 hours, the PAN polymer was completely dissolved and the RbNO3 particles were uniformly dispersed to prepare a suspension (RbNO3-PAN / DMF).

[0111] Afterwards, the particle dispersion of RbNO3 was further increased through ultrasonic treatment. The prepared suspension was transferred to a Luer lock syringe and equipped with an electrospinning needle. Electrospinning was performed on an aluminum foil substrate in two steps. To prevent the RbNO3 particles from sticking to the aluminum foil, 1 ml of the PAN / DMF solution was electrospun in the first step. In the second step, approximately 6 ml of the RbNO3-PAN / DMF suspension was electrospun. The electrospinning conditions were a voltage of 15–20 kV, a flow rate of 0.5–1.0 ml / hr, and a spinning distance of approximately 15 cm.

[0112] The aluminum foil after electrospinning was dried in a vacuum oven at a temperature of about 60°C for more than 12 hours under a vacuum atmosphere.

[0113] Fig. 6 shows a SEM analysis photograph of an intermediate layer (RbPAN) formed with a PAN nanofiber layer loaded with RbNO3 according to Example 3. Referring to Fig. 6, it can be confirmed that a nanofiber-shaped intermediate layer is synthesized through the electrospinning method of Example 3, and that the dispersed RbNO3 particles are uniformly synthesized together.

[0114]

[0115] Experimental example

[0116] Below, the electrochemical activity, etc. of the lithium metal battery of Comparative Example 1 and the lithium metal battery using the intermediate layer of Examples 1 to 3 were evaluated.

[0117] FIG. 7 is a graph showing the coulomb efficiency per cycle of a copper-lithium half-cell cell to evaluate lithium reversibility according to comparative examples and embodiments of the present invention.

[0118] Referring to Figure 7, the evaluation condition is 1 mA·cm -2 and 1 mAh·cm -2 And, the ratio of lithium deposition capacity to lithium desorption capacity is expressed as Coulomb efficiency, and it can be seen that Comparative Example 1 and Example 1 have relatively low Coulomb efficiency and lifespan, and it can be confirmed that Examples 2 and 3 show high Coulomb efficiency and excellent lifespan compared to Comparative Example 1 and Example 1.

[0119] Figure 8 is an image obtained through scanning electron microscopy and focused ion beam (FIB) cross-sectional analysis to evaluate the electrodeposition morphology of a lithium electrode according to comparative examples and examples of the present invention.

[0120] Referring to Fig. 8, it was confirmed that lithium was deposited in the form of dendrites on the local surface in Comparative Example 1 and Example 1, which also appears as a thick, porous lithium layer in the cross-sectional image. In the case of Examples 2 and 3, in which lithium nitrate or rubidium nitrate was added, it was confirmed that a lithium deposition shape with suppressed dendrites and a relatively thin lithium layer was formed accordingly.

[0121] Figure 9 shows the results of capacity and coulombic efficiency per cycle for evaluating the overall battery performance according to comparative examples and embodiments of the present invention. At this time, the working electrode is NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 O2) electrode was used, and 20 μm lithium foil was used as the counter electrode and reference electrode, and the evaluation condition was 1 mA·cm -2(0.29C), charge and discharge tests were conducted under conditions of a cut-off voltage of 3 V to 4.3 V.

[0122] Referring to FIG. 9, it can be seen that Examples 2 and 3 maintained high coulombic efficiency and stable capacity for 100 cycles, confirming that they can be utilized even in full batteries.

[0123]

[0124] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will readily appreciate that the present invention can be readily modified into other specific forms without altering the technical spirit or essential characteristics of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single entity may be implemented in a distributed manner, and similarly, components described as distributed may be implemented in a combined manner.

[0125] The scope of the present invention is indicated by the claims described below, and all changes or modifications derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.

Claims

1. Polymer nanofiber structure; and Containing a metal nitrate supported on the above polymer nanofiber structure, The above metal nitrate is an electrolyte additive containing lithium nitrate or rubidium nitrate.

2. In paragraph 1, The above polymer nanofiber structure is an electrolyte additive comprising at least one selected from the group consisting of polyvinylpyrrolidone (PVP), polyvinylidene fluoride (PVDF), and polyacrylonitrile (PAN).

3. In the first paragraph, the polymer nanofiber structure is an electrolyte additive having a fiber diameter of 100 to 500 nm.

4. An electrolyte additive according to claim 1, wherein the metal nitrate is contained in an amount of 10 to 70 wt% based on the total weight of the electrolyte additive.

5. Lithium metal cathode; An intermediate layer in the form of nanofibers positioned on the cathode and manufactured from an electrolyte and an electrolyte additive according to claim 1; a separator positioned on the intermediate layer; and A lithium metal battery comprising a positive electrode positioned on the above separator.

6. In paragraph 5, A lithium metal battery in which a solid electrolyte interphase (SEI) having improved ionic conductivity is formed on the intermediate layer by nitrate anions formed through decomposition of metal nitrate.

7. A lithium metal battery according to claim 5, wherein the intermediate layer has a thickness of 10 to 40 μm.

8. Step of preparing an electrolyte additive which is a mixture of a polymer and a metal nitrate; A step of manufacturing an intermediate layer from an electrolyte and the electrolyte additive; A method for manufacturing a lithium metal battery, comprising the steps of placing a lithium metal negative electrode under the intermediate layer and sequentially placing a separator and a positive electrode over the intermediate layer.

9. In paragraph 8, A method for manufacturing a lithium metal battery, wherein the mixing weight ratio of the metal nitrate and the polymer in the step of preparing the electrolyte additive is 1:2 to 3:

1.

10. In paragraph 8, A method for manufacturing a lithium metal battery, wherein the step of manufacturing the above intermediate layer is performed using an electrospinning method.

11. In paragraph 10, A method for manufacturing a lithium metal battery, wherein the above electrospinning method is performed under an applied voltage of 8 kV to 25 kV.

Citation Information

Patent Citations

  • Complex fibrous separator, manufacturing method thereof and secondary battery using the same

    KR101576151B1

  • Battery module with improved flame-retardant connector

    KR1020230063235A