Continuous selective leaching process, leaching apparatus and two-stage leaching device for crude cobalt hydroxide, and production process and production system for cobalt product

By gradually increasing the pH value with acidic solution in the selective leaching process of crude cobalt hydroxide, selective precipitation of divalent cobalt is achieved, solving the problem of impurities introduced in traditional processes, and improving the purity and production efficiency of cobalt products.

WO2024239283A1PCT designated stage expired Publication Date: 2024-11-28YICHANG BRUNP CONTEMPORARY AMPEREX CO LTD +3

Patent Information

Application Number
PCT/CN2023/096095
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The traditional crude cobalt hydroxide selective leaching process has the problem of leaching divalent cobalt and trivalent cobalt at the same time, resulting in the introduction of impurities, affecting the purification quality of cobalt. The use of reducing agents and oxidants increases impurities, making it difficult to be at low pH. Precipitation affects the purity of the leachate.

Method used

A continuous selective leaching process is adopted to gradually increase the pH value by mixing acid solution with crude cobalt hydroxide slurry, and selective precipitation of divalent cobalt ions is achieved, avoiding the use of reducing agents and oxidizing agents, and simplifying the subsequent The treatment improves the quality of cobalt products.

Benefits of technology

It achieves efficient purification of divalent cobalt, reduces the content of impurities, improves the purity and production efficiency of cobalt products, simplifies the subsequent processing process, and ensures the excellent quality of cobalt products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023096095_28112024_PF_FP_ABST
    Figure CN2023096095_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided herein is a continuous selective leaching process for crude cobalt hydroxide. The continuous selective leaching process comprises the following steps: preparing a crude cobalt hydroxide slurry; mixing some of the crude cobalt hydroxide slurry with an acid solution until the crude cobalt hydroxide slurry is dissolved in the acid solution, so as to obtain a primary leachate; adding the rest of the crude cobalt hydroxide slurry to the primary leachate, and mixing same, so as to obtain an adjusted leachate; subjecting the adjusted leachate to a selective precipitation operation, so as to form a precipitate and a selective leachate; and subjecting the precipitate and the selective leachate to a solid-liquid separation operation, so as to respectively obtain a first-stage leachate and acid leaching residues.
Need to check novelty before this filing date? Find Prior Art

Description

Continuous selective leaching process for crude cobalt hydroxide, leaching device and two-stage leaching equipment, cobalt product production process and production system Technical Field

[0001] This article relates to a continuous selective leaching process for crude cobalt hydroxide, a leaching device and two-stage leaching equipment, a cobalt product production process and a production system. Background Art

[0002] Non-ferrous metals are basic materials for the development of the national economy. With the rapid development of my country's economy, the demand for non-ferrous metals is increasing, and non-ferrous metal extraction and metallurgical technology should also continue to innovate with the development of science and technology.

[0003] Since cobalt has similar chemical properties to nickel, iron, manganese and copper, it is often found together in natural minerals, and minerals often contain these elements at the same time. There are many different cobalt-containing mineral raw materials, and there are many methods and processes for extracting cobalt. They can be classified according to different mineral types, mainly oxidized minerals, arsenic minerals and sulfide minerals. They are usually processed by the process of pyrometallurgical enrichment and hydrometallurgical smelting. The research and application of the full hydrometallurgical process is currently under development.

[0004] Hydrometallurgy is an important technical approach in the metallurgical field. It involves transferring ore, concentrated ore, or other raw materials through a leaching agent into a liquid phase, thereby achieving metal separation, enrichment, and extraction. Hydrometallurgy encompasses processes such as leaching, metal enrichment, and solution purification. Leaching is a key step in hydrometallurgy, and different leaching agents have unique applications within the leaching process. Cyanide leaching is the oldest method for extracting gold and silver. Metals such as copper sulfate, which are directly soluble in water, are leached directly with water. Copper, nickel, cobalt, zinc, and phosphorus oxides can be leached using sulfuric acid; chalcopyrite can be leached using hydrochloric acid; niobium and tantalum can be leached using hydrofluoric acid; scheelite and uranium ore can be leached using sodium carbonate; copper, nickel, and cobalt sulfides can be leached using ammonia; and copper, cobalt, and manganese can also be leached using bacterial leaching agents.

[0005] Crude cobalt hydroxide is a cobalt intermediate, which includes Co, Mn, Cu, Ni, Ca, Mg, Fe, Al and water. Cobalt in the crude cobalt hydroxide can be selectively leached.

[0006] Traditional selective leaching processes present the following challenges: The two-stage leaching process not only extracts divalent cobalt but also uses a reducing agent to leach trivalent cobalt. The addition of the reducing agent introduces a significant amount of impurities, which in turn affects the quality of the cobalt purification. Furthermore, the reducing agent reduces ferric ions to ferrous ions, which are difficult to precipitate at low pH levels. Therefore, an oxidizing agent must be added after the reduction leaching process to oxidize the ferrous ions to ferric ions. The addition of the oxidizing agent further introduces a significant amount of impurities. The reducing agent is at least one of sodium metabisulfite, sodium sulfite, sulfur dioxide, and sulfur; the oxidizing agent is at least one of sodium chlorate and manganese dioxide.

[0007] For example, the Chinese patent with patent publication number CN112359225A proposes a selective leaching process for crude cobalt hydroxide ore, which includes the following steps: the raw ore is stirred and slurried at a ratio of ore: water = 1:3, and after slurrying, the temperature is raised to 60°C to 70°C, concentrated sulfuric acid is added to make the slurry pH 0.45 to 0.5, and a first-stage leaching is performed to preferentially dissolve divalent cobalt and trivalent iron, and the mixture is stirred for 5min to 10min and filtered; the acid leaching liquid is directly fed into the transfer tank for iron removal, and the acid leaching residue is slurried for the second time at a ratio of acid leaching residue: water = 1:2; after the second slurrying of the acid leaching residue, the temperature is raised to 50°C to 60°C, sodium metabisulfite is added for second-stage reduction leaching, and the slurry pH is maintained at 1.0 to 1.5 until the reduction potential is lower than 240mV. The slurry after the above treatment is pre-oxidized by adding manganese dioxide ore, and manganese dioxide will reduce Fe 2+ Oxidized to Fe 3+ , when Fe in the slurry 2+ When the content falls below 0.05 g / L, the slurry is transferred to the transfer tank for iron removal. The reducing agent is sodium metabisulfite, or Na2S2O5. The addition of this reducing agent introduces sodium ions. Similarly, the oxidizing agent is manganese dioxide, or MnO2. This introduces manganese ions, reducing the purity of the selective leaching solution and, in turn, affecting the quality of the cobalt extraction.

[0008] Summary of the Invention

[0009] Based on this, it is necessary to provide a continuous selective leaching process for crude cobalt hydroxide with good purification effect on divalent cobalt ions, a leaching device and a two-stage leaching equipment, a cobalt product production process and a production system.

[0010] A continuous selective leaching process for crude cobalt hydroxide comprises the following steps:

[0011] preparing a crude cobalt hydroxide slurry;

[0012] mixing a portion of the crude cobalt hydroxide slurry and the acidic solution until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a primary leachate;

[0013] adding another portion of the crude cobalt hydroxide slurry to the preliminary leachate and mixing them to obtain an adjusted leachate;

[0014] performing a selective precipitation operation on the adjusted leachate to form a precipitate and a selective leachate;

[0015] The precipitate and the selective leaching liquid are subjected to a solid-liquid separation operation to obtain a first-stage leaching liquid and an acid leaching residue respectively.

[0016] In one embodiment, the step of preparing the crude cobalt hydroxide slurry is specifically: preparing the crude cobalt hydroxide slurry by mixing crude cobalt hydroxide and water in a mass ratio of 1:(2.5-4).

[0017] In one embodiment, the step of preparing the crude cobalt hydroxide slurry by mixing crude cobalt hydroxide and water in a mass ratio of 1: (2.5-4) is specifically as follows: under stirring, mixing crude cobalt hydroxide and water in a mass ratio of 1: (2.5-4) to prepare the crude cobalt hydroxide slurry.

[0018] In one embodiment, the acidic solution is at least one of sulfuric acid or hydrochloric acid.

[0019] In one embodiment, the pH of the preliminary leachate is 2.0-2.5.

[0020] In one embodiment, a portion of the crude cobalt hydroxide slurry and an acidic solution are mixed under heating conditions until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a primary leachate.

[0021] In one embodiment, another portion of the crude cobalt hydroxide slurry is added to the preliminary leachate under heating conditions and mixed to obtain an adjusted leachate.

[0022] In one embodiment, a portion of the crude cobalt hydroxide slurry and the acidic solution are mixed at 60° C. to 70° C. until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a primary leachate.

[0023] In one embodiment, another portion of the crude cobalt hydroxide slurry is added to the preliminary leachate at 60° C. to 70° C. and mixed to obtain an adjusted leachate.

[0024] In one embodiment, the time for the steps of mixing a portion of the crude cobalt hydroxide slurry with the acidic solution until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain the preliminary leachate is 0.8 h to 1.2 h.

[0025] In one embodiment, the time for the steps of mixing a portion of the crude cobalt hydroxide slurry with the acidic solution until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain the preliminary leachate is 1 hour.

[0026] In one embodiment, the step of mixing a portion of the crude cobalt hydroxide slurry with an acidic solution until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a preliminary leachate is specifically:

[0027] A portion of the crude cobalt hydroxide slurry and the acidic solution are subjected to at least two mixing and stirring leaching operations to obtain the primary leachate.

[0028] In one embodiment, the step of performing at least two mixing and stirring leaching operations on a portion of the crude cobalt hydroxide slurry and the acidic solution to obtain the preliminary leachate is specifically as follows:

[0029] performing a first leaching operation on a portion of the crude cobalt hydroxide slurry and the acidic solution to obtain a primary leachate;

[0030] performing a second leaching operation on the primary leachate to obtain a secondary leachate;

[0031] The secondary leachate is subjected to a third leaching operation to obtain a preliminary leachate.

[0032] In one embodiment, the pH of the primary leachate is 1.0-1.5.

[0033] In one embodiment, the pH of the secondary leachate is 1.5-2.0.

[0034] In one embodiment, the pH of the preliminary leachate is 2.0-2.5.

[0035] In one embodiment, the sum of the time for the step of adding another portion of the crude cobalt hydroxide slurry to the preliminary leachate to obtain an adjusted leachate and the step of performing a selective precipitation operation on the adjusted leachate to form a precipitate and a selective leachate is 0.8h to 1.2h.

[0036] In one embodiment, the sum of the time for the step of adding another portion of the crude cobalt hydroxide slurry to the preliminary leachate to obtain an adjusted leachate and the step of performing a selective precipitation operation on the adjusted leachate to form a precipitate and a selective leachate is 1 hour.

[0037] In one embodiment, the step of performing a selective precipitation operation on the adjusted leachate to form a precipitate and a selective leachate is specifically:

[0038] The adjusted leachate is subjected to at least one selective precipitation operation to form a precipitate and a selective leachate.

[0039] In one embodiment, the step of performing a selective precipitation operation on the adjusted leachate to form a precipitate and a selective leachate is specifically:

[0040] performing a first selective precipitation operation on the adjusted leachate to obtain a primary selective leachate and a first precipitate;

[0041] performing a second selective precipitation operation on the primary selective leachate to obtain a secondary selective leachate and a second precipitate;

[0042] The secondary selective leaching solution is subjected to a third selective precipitation operation to obtain a selective leaching solution and a third precipitate.

[0043] In one embodiment, the pH of the primary selective leaching solution is 3.5-4.0.

[0044] In one embodiment, the pH of the secondary selective leaching solution is 4.0-4.5.

[0045] In one embodiment, the pH of the selective leaching solution is 5.0-5.5.

[0046] In one embodiment, the pH of the primary selective leaching solution is 3.2-3.4.

[0047] In one embodiment, the pH of the secondary selective leachate is 4.7.

[0048] In one embodiment, the pH of the selective leaching solution is 5.0-6.7.

[0049] In one embodiment, the step of mixing a portion of the crude cobalt hydroxide slurry and the acidic solution is specifically:

[0050] A portion of the crude cobalt hydroxide slurry and the acidic solution are added simultaneously and mixed.

[0051] In one embodiment, the step of mixing a portion of the crude cobalt hydroxide slurry with the acidic solution is specifically as follows: the volume ratio of the portion of the crude cobalt hydroxide slurry to the acidic solution is 14-16.

[0052] In one embodiment, the step of adding another portion of the crude cobalt hydroxide slurry to the preliminary leachate to obtain the adjusted leachate is specifically as follows: the volume ratio of the portion of the crude cobalt hydroxide slurry to the acidic solution is 15.

[0053] A cobalt product production process comprises performing at least the following steps on the first-stage leachate obtained by any of the above embodiments:

[0054] Obtaining a section of leachate;

[0055] performing extraction treatment on the first stage leachate;

[0056] The first-stage leaching liquid that has undergone the extraction treatment is processed to obtain a first-stage leached cobalt product.

[0057] A continuous selective leaching device for crude cobalt hydroxide, which performs leaching operations using the continuous selective leaching process for crude cobalt hydroxide described in any of the above embodiments, and comprises:

[0058] A leaching mechanism, the leaching mechanism comprising at least a slurry dissolving component, a slurry replenishing component, and a selective precipitation component, the slurry dissolving component being provided with a first overflow port, the first overflow port being connected to the slurry replenishing component, the slurry replenishing component being provided with a second overflow port, the second overflow port being connected to the selective precipitation component, and the selective precipitation component being provided with a third overflow port;

[0059] A transfer mechanism is connected to the third overflow port, and is used to be connected to the primary leachate storage mechanism and the leachate residue pulping device respectively.

[0060] In one embodiment, the selective precipitation component is connected to the slurry dissolving component.

[0061] In one embodiment, the slurry dissolving component is connected to the transfer component.

[0062] In one embodiment, the grouting component is connected to the transfer component.

[0063] In one embodiment, the slurry dissolving component comprises at least a primary slurry dissolving kettle and a secondary slurry dissolving kettle that are connected to each other, and the first overflow port is formed in the secondary slurry dissolving kettle.

[0064] In one embodiment, the slurry dissolving component further includes an intermediate slurry dissolving kettle, and the intermediate slurry dissolving kettle is respectively connected to the primary slurry dissolving kettle and the secondary slurry dissolving kettle.

[0065] In one embodiment, the selective precipitation component comprises at least a first hydrolysis precipitation tank and a second hydrolysis precipitation tank that are connected to each other, and the third overflow port is formed in the second hydrolysis precipitation tank.

[0066] In one embodiment, the crude cobalt hydroxide continuous selective leaching device further includes a filter press mechanism, which is connected to the transfer mechanism and is used to be connected to the leaching residue slurrying device.

[0067] In one embodiment, the leaching mechanism further includes a heating component, and the active end of the heating component acts on the slurry component.

[0068] In one embodiment, the heating component is a steam heating component, and the steam heating component is provided with a steam output end, and the steam output end is connected to the slurry dissolving component.

[0069] In one embodiment, the slurry dissolving component is provided with a first pH measuring component.

[0070] In one embodiment, the grouting component is provided with a second pH measuring component.

[0071] In one embodiment, the selective precipitation component is provided with a third pH measurement component.

[0072] In one embodiment, the leaching mechanism further includes at least a first stirring component, and the stirring end of the first stirring component is disposed in the slurry component.

[0073] In one embodiment, the slurry dissolving component is formed with a slurry inlet trough and a slurry inlet port that are connected to each other, and the slurry inlet trough is connected to the first overflow port.

[0074] In one embodiment, the leaching mechanism further includes a first slurry supply component, and the first slurry supply component is connected to the slurry dissolving component.

[0075] In one embodiment, the first slurry supply component includes a first pH meter, a first flow rate monitor, a first movable partition and a first slurry supply trough body, the first slurry supply trough body is connected to the slurry dissolving component, the first movable partition is arranged at the connection point between the first slurry supply trough body and the slurry dissolving component, the detection end of the first pH meter is arranged in the slurry dissolving component, and the active end of the first flow rate monitor is arranged at the first overflow port.

[0076] In one embodiment, the first slurry supply component is used to set the flow rate of the crude cobalt hydroxide slurry to 1m 3 / h~3m 3 / h.

[0077] In one embodiment, the slurry feeding component is provided with a slurry holding tank and a feeding port that are connected to each other, and the slurry holding tank is connected to the first overflow port and the selective precipitation component respectively.

[0078] In one embodiment, the leaching mechanism further includes a second slurry supply component, and the second slurry supply component is connected to the slurry replenishment component.

[0079] In one embodiment, the second slurry supply component

[0080] This article also provides a two-stage leaching equipment for crude cobalt hydroxide, comprising a first-stage leachate storage mechanism, a leach residue slurrying device, and the crude cobalt hydroxide continuous selective leaching device described in any of the above embodiments, wherein the filter press mechanism is respectively connected to the first-stage leachate storage mechanism and the leach residue slurrying device.

[0081] In one embodiment, the leached residue slurrying device includes a two-stage leaching mechanism and a two-stage leachate storage mechanism that are connected.

[0082] A cobalt product production system comprises a first-stage leachate treatment device, a second-stage leachate treatment device, and the crude cobalt hydroxide second-stage leaching device described in any of the above embodiments, wherein the first-stage leachate treatment device is connected to the first-stage leachate storage mechanism, and the second-stage leachate treatment device is connected to the second-stage leachate storage device.

[0083] The details of one or more embodiments of the present invention are set forth in the following drawings and description. Compared with the prior art, the present invention has at least the following advantages:

[0084] 1) In the continuous selective leaching process of crude cobalt hydroxide herein, an acidic solution is used to leach divalent cobalt ions, trivalent iron ions, aluminum ions, copper ions, and impurity ions in the crude cobalt hydroxide slurry to obtain a preliminary leachate, and then the added crude cobalt hydroxide slurry is gradually dissolved in the acidic solution to gradually increase the pH value until the pH value is within a range in which divalent cobalt ions are not precipitated and most impurity ions are precipitated, so that the divalent cobalt ions exist in ionic form and most impurities exist in the precipitate, thereby separating the divalent cobalt ions from most impurities in the solid-liquid state, thereby achieving selective leaching of crude cobalt hydroxide.

[0085] 2) The continuous selective leaching process for crude cobalt hydroxide in this article not only avoids the problem of introducing sodium ions by adding a reducing agent, introducing sodium ions or tetravalent manganese ions by adding an oxidant, and introducing sodium ions or potassium ions by adding an alkaline auxiliary material in the traditional crude cobalt hydroxide selective leaching process, but also simplifies the subsequent treatment process for sodium ions, tetravalent manganese ions and potassium ions, thereby improving production efficiency, and reducing the concentrations of sodium ions, tetravalent manganese ions and potassium ions, ensuring the quality of the cobalt products produced subsequently. BRIEF DESCRIPTION OF THE DRAWINGS

[0086] In order to more clearly illustrate the technical solutions in the embodiments of this article or the prior art, the following briefly introduces the drawings that may be used in the description of the embodiments or the prior art.

[0087] FIG1 is a flow chart of the method steps of a continuous selective leaching process for crude cobalt hydroxide according to one embodiment;

[0088] FIG2 is a flow chart of the method steps of a cobalt product production process according to an embodiment. DETAILED DESCRIPTION

[0089] To facilitate understanding of this document, a more comprehensive description of this document will be provided below with reference to the accompanying drawings. Optional embodiments of this document are shown in the accompanying drawings. However, this document can be implemented in many different forms and is not limited to the embodiments described herein. Rather, the purpose of providing these embodiments is to provide a more thorough and comprehensive understanding of the disclosure herein. When an element is referred to as being "fixed to" another element, it can be directly attached to the other element or there can be an intermediate element. When an element is considered to be "connected to" another element, it can be directly connected to the other element or there can be an intermediate element. The terms "vertical," "horizontal," "left," "right," and similar expressions used herein are for illustrative purposes only and do not represent the only embodiments. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this document pertains. The terms used herein in this specification are for the purpose of describing specific embodiments only and are not intended to limit this document. The term "and / or" as used herein includes any and all combinations of one or more of the relevant listed items.

[0090] This article provides a continuous selective leaching process for crude cobalt hydroxide. In order to better understand the continuous selective leaching process for crude cobalt hydroxide in this article, the following further explains the continuous selective leaching process for crude cobalt hydroxide in this article:

[0091] As shown in FIG1 , further, the continuous selective leaching process of crude cobalt hydroxide includes some or all of the following steps:

[0092] S100, preparing crude cobalt hydroxide slurry.

[0093] It can be understood that crude cobalt hydroxide and water are weighed, mixed and stirred to obtain crude cobalt hydroxide slurry.

[0094] S200: A portion of the crude cobalt hydroxide slurry and the acidic solution are mixed until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a primary leachate.

[0095] The crude cobalt hydroxide slurry and the acidic solution are added simultaneously, and the acidic solution can be sulfuric acid or hydrochloric acid, which alleviates the problem of long feeding time and reduced production efficiency caused by adding the crude cobalt hydroxide slurry first and then adding the acidic solution in the traditional crude cobalt hydroxide selective leaching process. In other embodiments, the cobalt hydroxide slurry and the acidic solution are not limited to being added simultaneously, that is, the cobalt hydroxide slurry and the acidic solution are added separately.

[0096] S300, adding another portion of the crude cobalt hydroxide slurry to the preliminary leachate for mixing to obtain an adjusted leachate.

[0097] It can be understood that the crude cobalt hydroxide slurry includes metal hydroxides and metal oxides, and the metals refer to Co, Mn, Cu, Ni, Ca, Mg, Fe and Al. The addition of alkaline substances avoids the problem of introducing sodium ions or potassium ions by adding alkaline auxiliary materials in the traditional crude cobalt hydroxide selective leaching process, thereby avoiding the need to increase the number of extraction treatments and extend the extraction time, thereby reducing production efficiency. It also avoids the need to subsequently treat the sodium in the P507 raffinate, which increases the wastewater treatment process. The problem, that is, the production process is reduced, thereby improving production efficiency and reducing labor intensity; and since no impurities are introduced into the first-stage leaching solution, the quality of subsequent cobalt products is improved. For example, the national standard for the sodium content of superior cobalt sulfate is less than or equal to 0.001%, and the sodium content of first-grade products is less than or equal to 0.002%. Since no sodium ions are introduced into the first-stage leaching solution, the subsequent cobalt product can easily reach the grade of superior cobalt sulfate, that is, the quality of the cobalt product is ensured.

[0098] S400, performing a selective precipitation operation on the adjusted leachate to form a precipitate and a selective leachate.

[0099] It can be understood that as the crude cobalt hydroxide slurry gradually dissolves, the pH gradually increases during the dissolution process, so that the impurity ions with a lower precipitation pH gradually precipitate as precipitates, while ensuring that the divalent cobalt ions are present in the selective leachate in the form of ions, that is, a selective leachate containing divalent cobalt ions is obtained.

[0100] S500, performing a solid-liquid separation operation on the precipitate and the selective leaching liquid to obtain a first-stage leaching liquid and an acid leaching residue respectively.

[0101] It can be understood that the first-stage leachate is stored in the first-stage leachate storage mechanism, and the second-stage reduction leachate obtained by the subsequent second-stage reduction leaching of the acid leaching residue is stored in an independent mechanism, thereby avoiding the problem that the first-stage leachate with higher purity is affected by the second-stage reduction leachate with lower purity, thereby ensuring the purity of the first-stage leachate. Moreover, since the acid leaching residue is less, the acid leaching residue can be batch processed subsequently to improve production efficiency.

[0102] In the above-mentioned continuous selective leaching process of crude cobalt hydroxide, the acidic solution leach the divalent cobalt ions, trivalent iron ions, aluminum ions, copper ions and impurity ions in the crude cobalt hydroxide slurry to obtain a primary leachate, and then the added crude cobalt hydroxide slurry is gradually dissolved in the acidic solution to gradually increase the pH value until the pH value is within a range in which the divalent cobalt ions do not precipitate and most of the impurity ions precipitate, so that the divalent cobalt ions exist in ionic form and most of the impurities exist in the precipitate, thereby separating the divalent cobalt ions from most of the impurities in the solid-liquid state, thereby achieving selective leaching of the crude cobalt hydroxide.

[0103] Furthermore, the above-mentioned continuous selective leaching process for crude cobalt hydroxide does not require the addition of a reducing agent for leaching, thereby saving the time of the reduction reaction and improving production efficiency.

[0104] Furthermore, the first-stage leachate not only avoids the problems of introducing sodium ions by adding a reducing agent, introducing sodium ions or tetravalent manganese ions by adding an oxidant, and introducing sodium ions or potassium ions by adding an alkaline auxiliary material in the traditional selective leaching process of crude cobalt hydroxide, but also simplifies the subsequent treatment process of sodium ions, tetravalent manganese ions and potassium ions, thereby improving production efficiency, and reduces the concentrations of sodium ions, tetravalent manganese ions and potassium ions, ensuring the quality of the cobalt products produced subsequently.

[0105] Furthermore, the crude cobalt hydroxide slurry and the acidic solution are added to the slurry dissolving component at the same time, thereby avoiding the problem of low production efficiency caused by the traditional crude cobalt hydroxide selective leaching process of first adding the slurry and heating it before adding sulfuric acid, thereby improving production efficiency.

[0106] Furthermore, the traditional crude cobalt hydroxide selective leaching process transfers the divalent cobalt leachate and the trivalent cobalt reduction leachate to the transfer tank for iron removal. The purity of the divalent cobalt leachate is relatively high. The trivalent cobalt reduction leachate introduces sodium ions and manganese ions respectively because the reducing agent is first added to the trivalent cobalt reduction leachate for reduction reaction and then the oxidant is added for oxidation reaction. The sodium ions are difficult to hydrolyze and precipitate. At the same temperature, the precipitation pH of manganese ions is higher than the precipitation pH of divalent cobalt. It is also difficult to precipitate manganese ions under the condition that divalent cobalt is not precipitated. That is, the impurity ions introduced by the reducing agent and the oxidant are difficult to remove. Therefore, the trivalent cobalt reduction leachate reduces the purity of the divalent cobalt leachate, thereby reducing the subsequent purification quality of the divalent cobalt leachate. In order to improve the quality of the cobalt product obtained subsequently, the crude cobalt hydroxide selective leaching process in this article treats the divalent cobalt leachate and the acid leaching residue separately, and the divalent cobalt leachate does not add a reducing agent, an oxidizing agent and an alkaline auxiliary material, thereby ensuring the quality of the cobalt product obtained subsequently.

[0107] Furthermore, in the crude cobalt hydroxide, the content of divalent cobalt is high and the content of trivalent cobalt is low, and the trivalent cobalt needs to be added with a reducing agent to be leached. After the divalent cobalt is leached, it is transferred to the transfer tank for iron removal. It is necessary to wait for the trivalent cobalt to be reduced and leached before being transferred to the transfer tank for iron removal. Therefore, the traditional crude cobalt hydroxide selective leaching process reduces production efficiency. In order to improve the quality of the cobalt products obtained subsequently and further improve production efficiency, the crude cobalt hydroxide selective leaching process in this article treats the divalent cobalt leachate and the acid leaching residue separately, and collects the acid leaching residue and processes it in batches.

[0108] In one embodiment, the step of preparing the crude cobalt hydroxide slurry is specifically: preparing the crude cobalt hydroxide slurry by mixing crude cobalt hydroxide and water in a mass ratio of 1:(2.5-4).

[0109] In one embodiment, the step of preparing a crude cobalt hydroxide slurry by mixing crude cobalt hydroxide and water in a mass ratio of 1:(2.5-4) is specifically as follows: mixing crude cobalt hydroxide and water in a mass ratio of 1:(2.5-4) and stirring to prepare a crude cobalt hydroxide slurry.

[0110] In one embodiment, the acidic solution is at least one of sulfuric acid or hydrochloric acid.

[0111] In one embodiment, the pH of the preliminary leachate is 2.0 to 2.5. It is understood that when the preliminary leachate is obtained, the crude cobalt hydroxide slurry is fully dissolved in the acidic solution, that is, a solution is obtained in which a large amount of divalent cobalt ions are leached.

[0112] In one embodiment, a portion of the crude cobalt hydroxide slurry and an acidic solution are mixed under heating conditions until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a primary leachate.

[0113] In one embodiment, another portion of the crude cobalt hydroxide slurry is added to the preliminary leachate under heating conditions and mixed to obtain an adjusted leachate.

[0114] In one embodiment, a portion of the crude cobalt hydroxide slurry and an acidic solution are mixed at 60°C to 70°C until the crude cobalt hydroxide slurry dissolves in the acidic solution, thereby obtaining a preliminary leachate. It is understood that increasing the temperature can activate the reaction, accelerate the movement between particles, and promote the two-phase contact reaction between sulfuric acid and the material powder liquid. The increase in temperature increases the internal energy of the reactants, increases the chance of collision between the two, and thus improves the cobalt leaching rate and leaching reaction rate, shortening the time required for leaching to reach equilibrium.

[0115] In one embodiment, another portion of the crude cobalt hydroxide slurry is added to the preliminary leachate at 60°C to 70°C and mixed to obtain a conditioned leachate. It is understood that increasing the temperature can activate the reaction, accelerate the movement between particles, and promote the two-phase contact reaction between sulfuric acid and the material powder liquid. The increase in temperature increases the internal energy of the reactants, increases the chance of collision between the two, and thus improves the cobalt leaching rate and leaching reaction rate, shortening the time required for leaching to reach equilibrium.

[0116] In one embodiment, a portion of the crude cobalt hydroxide slurry and the acidic solution are mixed until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a preliminary leachate, and the total time of the steps is 0.8 h to 1.2 h. In this embodiment, a portion of the crude cobalt hydroxide slurry and the acidic solution are mixed until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a preliminary leachate, and the total time of the steps is 1 h.

[0117] In one embodiment, the step of mixing a portion of the crude cobalt hydroxide slurry with an acidic solution until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a preliminary leachate is specifically as follows: performing a mixing and stirring leaching operation on the portion of the crude cobalt hydroxide slurry and the acidic solution at least twice to obtain a preliminary leachate. It is understood that the crude cobalt hydroxide slurry is fully dissolved in the acidic solution, thereby obtaining relatively sufficient leaching of divalent cobalt ions.

[0118] In one embodiment, the steps of performing at least two mixing and stirring leaching operations on a portion of the crude cobalt hydroxide slurry and the acidic solution to obtain a preliminary leachate are specifically as follows:

[0119] performing a first leaching operation on a portion of the crude cobalt hydroxide slurry and the acidic solution to obtain a primary leachate;

[0120] performing a second leaching operation on the primary leachate to obtain a secondary leachate;

[0121] The secondary leachate is subjected to a third leaching operation to obtain a preliminary leachate.

[0122] In one embodiment, the pH of the primary leachate is 1.0 to 1.5. In this embodiment, the pH of the primary leachate is 1.2.

[0123] In one embodiment, the pH of the secondary leachate is 1.5 to 2.0. In this embodiment, the pH of the secondary leachate is 1.8.

[0124] In one embodiment, the pH of the preliminary leachate is 2.0 to 2.5. In this embodiment, the pH of the preliminary leachate is 2.3.

[0125] In one embodiment, the sum of the time for the step of adding another portion of the crude cobalt hydroxide slurry to the preliminary leachate to obtain the conditioned leachate and the step of subjecting the conditioned leachate to selective precipitation to form a precipitate and a selective leachate is 0.8 h to 1.2 h. In this embodiment, the sum of the time for the step of adding another portion of the crude cobalt hydroxide slurry to the preliminary leachate to obtain the conditioned leachate and the step of subjecting the conditioned leachate to selective precipitation to form a precipitate and a selective leachate is 1 h.

[0126] In one embodiment, the steps of performing a selective precipitation operation on the adjusted leachate to form a precipitate and a selective leachate are specifically as follows:

[0127] The adjusted leachate is subjected to at least one selective precipitation operation to form a precipitate and a selective leachate.

[0128] In one embodiment, the steps of performing a selective precipitation operation on the adjusted leachate to form a precipitate and a selective leachate are specifically as follows:

[0129] performing a first selective precipitation operation on the adjusted leachate to obtain a primary selective leachate and a precipitate;

[0130] It can be understood that the conditioned leachate contains divalent cobalt ions, iron ions, aluminum ions, copper ions and impurity ions. As the pH increases, the easily precipitated iron ions are first hydrolyzed and precipitated, that is, the precipitate in this step is ferric hydroxide, and the primary selective leachate is a conditioned leachate from which most of the iron ions have been removed.

[0131] performing a second selective precipitation operation on the primary selective leachate to obtain a secondary selective leachate and a precipitate;

[0132] It can be understood that as the pH further increases, aluminum ions are hydrolyzed and precipitated, that is, the precipitate added in this step is aluminum hydroxide and a trace amount of iron hydroxide, and the secondary selective leachate is an adjusted leachate with iron ions and aluminum ions removed.

[0133] The secondary selective leaching solution is subjected to a third selective precipitation operation to obtain a selective leaching solution and a precipitate.

[0134] It can be understood that as the pH further increases, copper ions are hydrolyzed and precipitated, that is, the precipitate added in this step is copper hydroxide, a small amount of aluminum hydroxide and a trace amount of iron hydroxide, thereby achieving copper enrichment. The secondary selective leachate is a regulated leachate from which iron ions, aluminum ions and part of the copper ions are removed.

[0135] In one embodiment, the pH of the primary selective leaching solution is 3.5 to 4.0. It is understood that the reaction between the crude cobalt hydroxide slurry and the acidic solution lowers the pH of the mixed solution. When the pH is greater than 3.5, the iron ions are easily completely hydrolyzed and precipitated.

[0136] In one embodiment, the pH of the secondary selective leaching solution is 4.0 to 4.5. It can be understood that the reaction between the crude cobalt hydroxide slurry and the acidic solution lowers the pH of the mixed solution. When the pH is 4.0 to 4.5, most of the aluminum ions are hydrolyzed and precipitated.

[0137] In one embodiment, the pH of the selective leachate is 5.0-5.5. It is understood that the reaction between the crude cobalt hydroxide slurry and the acidic solution lowers the pH of the mixed solution. When the pH is 5.0-5.5, a small amount of aluminum ions and some copper ions are hydrolyzed and precipitated, thereby reducing the impurity ions in the selective leachate and achieving copper enrichment.

[0138] In one embodiment, the pH of the primary selective leachate is 3.2-3.4. It is understood that when the pH of the primary selective leachate is 3.2-3.4, the iron ions are fully hydrolyzed and precipitated, while the aluminum ions have not yet begun to hydrolyze and precipitate. In other words, the resulting first precipitate is primarily ferric hydroxide precipitate, which is of high quality and has a high recovery value. For example, it can be used to make pigments, medicines, and arsenic antidotes, or it can be treated with a reducing agent at high temperature to convert it into ferrosoferric oxide.

[0139] In one embodiment, the pH of the secondary selective leachate is 4.7. It is understood that when the pH of the secondary selective leachate is 4.7, iron ions have been fully precipitated in the previous step, aluminum ions have been fully hydrolyzed and precipitated in this step, and copper ions have not yet begun to hydrolyze and precipitate. That is, the second precipitate obtained in this step is mainly aluminum hydroxide precipitate, which has a high grade and high recovery value. For example, it can be used to prepare antacids to treat stomach pain, excessive stomach acid, heartburn, and gastric acid. It can also be used to reduce phosphate levels in people with kidney problems.

[0140] In one embodiment, the pH of the selective leachate is 5.0-6.7. It is understood that when the pH of the selective leachate is 5.0-6.7, the iron and aluminum ions have been fully precipitated in the previous step, and the divalent cobalt ions have not yet begun to hydrolyze and precipitate. That is, the third precipitate obtained in this step is primarily copper hydroxide precipitate, which is of high grade and has a high recovery value. For example, it can be used to prepare mordants, catalysts, fungicides, and pigments, and for dyeing paper, etc., as an analytical reagent; as a raw material for preparing copper salts, a mordant, and as a component of fungicides and antifouling paint for ship bottoms.

[0141] In one embodiment, the pH of the selective leachate is 6.7. It can be understood that when the pH of the selective leachate is 5.0-6.7, the copper ions are fully hydrolyzed and precipitated, while the divalent cobalt ions do not begin to hydrolyze and precipitate. In other words, the sedimentation rate of the copper ions can be increased while reducing the loss of divalent cobalt ions, thereby more fully achieving the enrichment and recovery of copper.

[0142] The traditional selective leaching process for crude cobalt hydroxide simultaneously leaches iron hydroxide, aluminum hydroxide, and copper hydroxide, that is, a precipitate containing iron hydroxide, aluminum hydroxide, and copper hydroxide is obtained. When the precipitate is recovered, iron, aluminum, and copper need to be separated before they can be recovered, which reduces production efficiency and increases production costs. In order to precipitate iron hydroxide, aluminum hydroxide, and copper hydroxide separately, in one embodiment, the pH of the primary selective leaching solution is 3.2-3.4, the pH of the secondary selective leaching solution is 4.7, and the pH of the selective leaching solution is 5.0-6.7. It can be understood that this makes the content of iron hydroxide in the first precipitate higher, the content of aluminum hydroxide in the second precipitate higher, and the content of copper hydroxide in the third precipitate higher, thereby enabling iron hydroxide, aluminum hydroxide, and copper hydroxide to be recovered separately, and improving the production convenience and production efficiency of the subsequent recovery process, and reducing production costs.

[0143] In one embodiment, the step of mixing a portion of the crude cobalt hydroxide slurry and the acidic solution is specifically as follows: simultaneously adding a portion of the crude cobalt hydroxide slurry and the acidic solution and mixing them. It can be understood that simultaneously adding a portion of the crude cobalt hydroxide slurry and the acidic solution and mixing them alleviates the problem of long production time caused by the traditional method of first adding the crude cobalt hydroxide slurry and then adding the acidic solution, thereby improving production efficiency.

[0144] Please refer to Figures 1 and 2 together. This article also provides a cobalt product production process. The above cobalt product production process includes performing at least the following steps on a first-stage leachate obtained by any of the above embodiments:

[0145] S501, obtaining a section of leachate;

[0146] In this embodiment, the primary leachate prepared by the above-mentioned continuous selective leaching process for crude cobalt hydroxide is used, i.e., no reducing agent, oxidizing agent, or alkaline auxiliary material is added to the primary leachate, thereby avoiding the problem of sodium ions, sulfide, tetravalent manganese ions, and potassium ions introduced into the conventional primary leachate due to the addition of reducing agents, oxidizing agents, and alkaline auxiliary materials.

[0147] S600, extracting a section of the leachate;

[0148] In this embodiment, although the first-stage leachate has hydrolyzed and precipitated iron ions, aluminum ions, and some copper ions, the first-stage leachate still contains impurity ions, specifically tetravalent manganese ions, nickel ions, calcium ions, magnesium ions, and some copper ions, which need to be removed by extraction treatment. The concentration of the impurity ions after treatment is inversely proportional to the quality of the cobalt product obtained subsequently.

[0149] S700, processing the first-stage leaching liquid that has undergone extraction treatment to obtain a first-stage leaching cobalt product.

[0150] The traditional selective leaching process for crude cobalt hydroxide introduces sodium ions or sulfides by adding a reducing agent, sodium ions or tetravalent manganese ions by adding an oxidizing agent, and sodium ions or potassium ions by adding an alkaline auxiliary material. Therefore, extraction and other treatments are required to remove impurity ions, and the following problems exist:

[0151] Sodium and potassium ions will seriously affect the quality of subsequent cobalt products. Therefore, it is necessary to increase the number of subsequent extraction treatments and extend the extraction time to reduce the ion concentration to 0.01g / L to achieve the purpose of impurity removal, which makes the production process more complicated and reduces production efficiency. Similarly, the treatment of sulfides requires the use of gas stripping, chemical precipitation or oxidation methods, which require more chemicals and precipitate treatment, have high energy consumption and high costs, and are not environmentally friendly. In particular, gas stripping will produce a large amount of H2S-containing air, so the H2S-containing air needs to be treated subsequently, further complicating the production process and reducing production efficiency. In addition, since the oxidant introduces tetravalent manganese ions, the concentration of tetravalent manganese ions is higher, which means that more extractants are needed to remove the tetravalent manganese ions, the number of extractions is increased, and the extraction time is extended, thereby reducing production efficiency.

[0152] The above-mentioned cobalt product production process uses a primary leachate prepared by the above-mentioned continuous selective leaching process for crude cobalt hydroxide, thereby avoiding the problem of sodium ions, sulfides, tetravalent manganese ions, and potassium ions being introduced into the conventional primary leachate, reducing the number of extraction treatments and shortening the extraction time, thereby improving production efficiency. Furthermore, since the primary leachate does not introduce impurities, the quality of subsequent cobalt products is improved. For example, the national standard for the sodium content of premium cobalt sulfate is less than or equal to 0.001%, and the sodium content of first-class cobalt sulfate is less than or equal to 0.002%. Since the primary leachate does not introduce sodium ions, the subsequent cobalt product can easily reach the grade of premium cobalt sulfate, thus ensuring the quality of the cobalt product.

[0153] The present invention also provides a continuous selective leaching device for crude cobalt hydroxide, which uses the continuous selective leaching process for crude cobalt hydroxide of any of the above embodiments to perform leaching operations. The continuous selective leaching device for crude cobalt hydroxide comprises:

[0154] The leaching mechanism includes at least a slurry dissolving component, a slurry replenishing component, and a selective precipitation component. The slurry dissolving component is provided with a first overflow port, the first overflow port is connected to the slurry replenishing component, the slurry replenishing component is provided with a second overflow port, the second overflow port is connected to the selective precipitation component, and the selective precipitation component is provided with a third overflow port;

[0155] The transfer mechanism is connected to the third overflow port and is used to be connected to the primary leachate storage mechanism and the leachate residue pulping device respectively.

[0156] In the above-mentioned continuous selective leaching device for crude cobalt hydroxide, the dissolving component is used to hold the crude cobalt hydroxide slurry and the acidic solution. The acidic solution leach the divalent cobalt ions, trivalent iron ions, aluminum ions and copper ions in the crude cobalt hydroxide slurry in the dissolving component to obtain a leachate. The leachate then overflows into the slurry replenishing component through the first overflow port. The slurry replenishing component is used to hold the leachate and the added crude cobalt hydroxide slurry. The added crude cobalt hydroxide slurry gradually dissolves in the acidic solution to gradually increase the pH value of the liquid in the slurry replenishing component and the selective precipitation component until the pH value is within a range in which the divalent cobalt ions do not precipitate and most impurity ions precipitate, so that the divalent cobalt ions exist in ionic form and most impurities exist in the precipitate, thereby separating the divalent cobalt ions from most impurities in solid and liquid form, thereby achieving selective leaching of crude cobalt hydroxide.

[0157] Furthermore, the first-stage leachate and precipitate obtained by selective leaching in the selective precipitation assembly are both overflowed to the transfer mechanism through the third overflow port, and then the first-stage leachate flows to the first-stage leachate storage mechanism, and the precipitate is transported to the leach residue slurrying device; the first-stage leachate not only avoids the problem of introduction of impurities caused by adding reducing agents and oxidizing agents to the leachate in the traditional crude cobalt hydroxide selective leaching process, but also avoids the problem of introduction of impurities caused by adding alkaline auxiliary materials by using crude cobalt hydroxide slurry as a regulator to increase pH, thereby ensuring the purity of the first-stage leachate, that is, improving the purification quality of cobalt.

[0158] Furthermore, the above-mentioned crude cobalt hydroxide continuous selective leaching device adds the crude cobalt hydroxide slurry and the acidic solution into the slurry dissolving component at the same time, thereby avoiding the low production efficiency problem caused by the traditional crude cobalt hydroxide selective leaching process of first adding the slurry and heating it before adding sulfuric acid, thereby improving production efficiency.

[0159] Furthermore, the crude cobalt hydroxide slurry and the acidic solution overflow from the dissolving assembly through the first overflow port to the slurry feeding assembly, then overflow from the slurry feeding assembly through the second overflow port to the selective precipitation assembly, and then overflow from the selective precipitation assembly through the third overflow port to the transfer mechanism, thereby reducing the use of machine pumps, ensuring the automation of the crude cobalt hydroxide continuous selective leaching device, simplifying the operating process, and avoiding the problem of transferring the leachate to a transfer tank in the traditional crude cobalt hydroxide selective leaching process, thereby reducing labor intensity.

[0160] Furthermore, in the conventional selective leaching process for crude cobalt hydroxide, the divalent cobalt leachate and the trivalent cobalt reduction leachate are successively transferred to a transfer tank for iron removal. The purity of the divalent cobalt leachate is relatively high. Since the reducing agent is first added to the trivalent cobalt reduction leachate for reduction reaction and then the oxidant is added for oxidation reaction, sodium ions and manganese ions are introduced respectively. The sodium ions are difficult to hydrolyze and precipitate. At the same temperature, the precipitation pH of the manganese ions is higher than the precipitation pH of the divalent cobalt. It is also difficult to precipitate the manganese ions while ensuring that the divalent cobalt is not precipitated. That is, the impurity ions introduced by the reducing agent and the oxidant are difficult to remove. Therefore, the trivalent cobalt reduction leachate reduces the purity of the divalent cobalt leachate, thereby reducing the subsequent purification quality of the divalent cobalt leachate.

[0161] Furthermore, in the crude cobalt hydroxide, the content of divalent cobalt is high, while the content of trivalent cobalt is low and requires the addition of a reducing agent for leaching. After the divalent cobalt is leached, it is transferred to a transfer tank for iron removal. It is necessary to wait for the trivalent cobalt to be reduced and leached before it is transferred to the transfer tank for iron removal, which reduces production efficiency.

[0162] In one embodiment, the selective precipitation module is connected to the slurry dissolving module. It can be understood that the slurry dissolving component is provided with a first overflow port, the first overflow port is connected to the slurry replenishing component, the slurry replenishing component is provided with a second overflow port, the second overflow port is connected to the selective precipitation component, and the selective precipitation component is connected to the slurry dissolving component, that is, the slurry dissolving component, the slurry replenishing component and the selective precipitation component form a circular connection; and the selective precipitation component is not limited to being used only for selective precipitation, but can also be used for slurry dissolving or slurry replenishing. Similarly, the slurry dissolving component is not limited to being used only for slurry dissolving, but can also be used for selective precipitation or slurry replenishing. Similarly, the slurry replenishing component is not limited to being used only for slurry replenishing, but can also be used for selective precipitation or slurry dissolving; therefore, when the slurry in the selective precipitation component is not fully dissolved, the selective precipitation component with more slurry accumulated in this round can be used as the slurry dissolving component of the next round, and other components are also adjusted in coordination so that the slurry that is not fully dissolved in this round can be dissolved again in the next round, thereby improving the full utilization of the crude cobalt hydroxide slurry, and reducing the problem of manual cleaning and transfer of the slurry, which causes high labor intensity, and saving time for cleaning and transfer of the slurry, thereby improving production efficiency.

[0163] In order to improve the subsequent purification quality of the divalent cobalt leachate and improve production efficiency, in one embodiment, the transfer mechanism is used to be connected to a leachate storage mechanism and a leach residue slurrying device respectively. It can be understood that the transfer mechanism performs solid-liquid separation on the divalent cobalt leachate and the precipitate. The divalent cobalt leachate is a first-stage leachate, and the first-stage leachate flows to a first-stage leachate storage mechanism. The first-stage leachate storage mechanism is only used to store a first-stage leachate, and is not used to store the trivalent cobalt leachate of the subsequent precipitation reduction leaching, thereby ensuring the purity of the first-stage leachate; and since the amount of precipitate is small, the precipitate will be concentrated in batches for leaching later, and the batch processing of the precipitate saves energy, reduces the use of the leaching residue pulping device, thereby reducing the damage and maintenance of the leaching residue pulping device, thereby increasing the service life of the leaching residue pulping device, and greatly improving the production efficiency; and since the traditional crude cobalt hydroxide selective leaching process avoids the problem of transferring the divalent cobalt to the transfer tank for iron removal after leaching, and needing to wait for the trivalent cobalt reduction leachate to be iron removed together, thereby reducing the phenomenon of equipment being occupied but not used, that is, ensuring the utilization rate of the equipment, thereby reducing the equipment footprint.

[0164] In order to improve the subsequent purification quality of the divalent cobalt leachate and improve production efficiency, in one embodiment, the transfer mechanism is used to be connected to a leachate storage mechanism and a leach residue slurrying device respectively. It can be understood that the transfer mechanism performs solid-liquid separation on the divalent cobalt leachate and the precipitate. The divalent cobalt leachate is a first-stage leachate, and the first-stage leachate flows to a first-stage leachate storage mechanism. The first-stage leachate storage mechanism is only used to store a first-stage leachate, and is not used to store the trivalent cobalt leachate of the subsequent precipitation reduction leaching, thereby ensuring the purity of the first-stage leachate; and since the amount of precipitate is small, the precipitate will be concentrated in batches for leaching later, and the batch processing of the precipitate saves energy, reduces the use of the leaching residue pulping device, thereby reducing the damage and maintenance of the leaching residue pulping device, thereby increasing the service life of the leaching residue pulping device, and greatly improving the production efficiency; and since the traditional crude cobalt hydroxide selective leaching process avoids the problem of transferring the divalent cobalt to the transfer tank for iron removal after leaching, and needing to wait for the trivalent cobalt reduction leachate to be iron removed together, thereby reducing the phenomenon of equipment being occupied but not used, that is, ensuring the utilization rate of the equipment, thereby reducing the equipment footprint.

[0165] In one embodiment, the slurry dissolving assembly includes at least a primary slurry dissolving kettle and a secondary slurry dissolving kettle that are connected to each other, and the first overflow port is formed in the secondary slurry dissolving kettle. It is understood that the process from the addition of the crude cobalt hydroxide slurry and the acidic solution to the filling of the primary slurry dissolving kettle is a process that takes time. Similarly, the overflow from the primary slurry dissolving kettle to the secondary slurry dissolving kettle also takes time. During this period, the crude cobalt hydroxide slurry is relatively fully dissolved in the acidic solution, that is, the divalent cobalt in the crude cobalt hydroxide is relatively fully leached, thereby ensuring the leaching rate of the divalent cobalt in the crude cobalt hydroxide.

[0166] In one embodiment, the slurry dissolving assembly further includes an intermediate slurry dissolving kettle, which is connected to the primary slurry dissolving kettle and the secondary slurry dissolving kettle, respectively. It is understood that the process from the crude cobalt hydroxide slurry and the acidic solution being added to the primary slurry dissolving kettle to filling the primary slurry dissolving kettle is a process that takes time. Similarly, it takes time for the primary slurry dissolving kettle to overflow into the intermediate slurry dissolving kettle, and similarly, it takes time for the intermediate slurry dissolving kettle to overflow into the secondary slurry dissolving kettle. During this period, the crude cobalt hydroxide slurry is more fully dissolved in the acidic solution, that is, the divalent cobalt in the crude cobalt hydroxide is more fully leached, thereby ensuring the leaching rate of divalent cobalt in the crude cobalt hydroxide.

[0167] In one embodiment, the selective precipitation component includes at least a first hydrolysis precipitation tank and a second hydrolysis precipitation tank that are connected to each other, and a third overflow port is formed in the second hydrolysis precipitation tank. It is understood that the added crude cobalt hydroxide slurry requires a certain amount of time to dissolve. In the process of flowing from the slurry supply component to the first hydrolysis precipitation tank and the second hydrolysis precipitation tank in sequence, the added crude cobalt hydroxide slurry is relatively fully dissolved and gradually consumes the acidic solution, causing the pH to gradually increase, thereby causing the trivalent iron ions, aluminum ions, and copper ions to gradually hydrolyze and precipitate, thereby achieving continuous selective leaching of the crude cobalt hydroxide and ensuring the leaching effect, that is, ensuring the purification effect of divalent cobalt.

[0168] In one embodiment, the selective precipitation component is connected to the slurry dissolving component. It can be understood that the slurry dissolving component is provided with a first overflow port, the first overflow port is connected to the slurry replenishing component, the slurry replenishing component is provided with a second overflow port, the second overflow port is connected to the selective precipitation component, the selective precipitation component is connected to the slurry dissolving component, that is, the slurry dissolving component, the slurry replenishing component and the selective precipitation component form a loop connection; and the selective precipitation component is not limited to being used only for selective precipitation, but can also be used for slurry dissolving or slurry replenishing, similarly, the slurry dissolving component is not limited to being used only for slurry dissolving, but can also be used for selective precipitation or slurry replenishing, similarly, the slurry replenishing component is not limited to being used only for slurry replenishing, but can also be used for selective precipitation or slurry replenishing. Selective precipitation or dissolution; therefore, when the slurry in the selective precipitation component is not fully dissolved due to a malfunction of the leaching mechanism or other reasons, the selective precipitation component with more slurry accumulated in the current round can be used as the dissolution component in the next round, and other components are also adjusted in a coordinated manner so that the slurry that is not fully dissolved accumulated in the current round can be dissolved again in the next round, thereby improving the full utilization of the crude cobalt hydroxide slurry, reducing the need for manual cleaning and transfer of the slurry, and reducing the labor intensity caused by the high labor intensity, and saving time for cleaning and transfer of the slurry, thereby improving production efficiency.

[0169] In one embodiment, the selective precipitation component is connected to the slurry dissolving component, and the slurry replenishing component is connected to the transfer component. It can be understood that the slurry dissolving component is provided with a first overflow port, the first overflow port is connected to the slurry replenishing component, the slurry replenishing component is provided with a second overflow port, the second overflow port is connected to the selective precipitation component, and the selective precipitation component is connected to the slurry dissolving component, that is, the slurry dissolving component, the slurry replenishing component and the selective precipitation component form a loop connection; and the selective precipitation component is not limited to being used only for selective precipitation, but can also be used for slurry dissolving or slurry replenishing, similarly, the slurry dissolving component is not limited to being used only for slurry dissolving, but can also be used for selective precipitation or slurry replenishing, similarly, the slurry replenishing component is not limited to being used only for slurry replenishing, but can also be used for selective precipitation or slurry dissolving; therefore, when the leaching mechanism fails or other reasons occur, the slurry in the selective precipitation component is not fully dissolved. During the decomposition, the selective precipitation component with more slurry accumulation in this round can be used as the dissolving component in the next round, the dissolving component in this round can be used as the slurry replenishing component in the next round of production, and the slurry replenishing component in this round can be used as the selective precipitation component in the next round of production. Then, the selective leaching liquid obtained by processing the slurry replenishing component in this round in the next round of production flows to the transfer component. There is no need to transfer the slurry or move the position of the leaching mechanism, so that the slurry that is not fully dissolved in this round can be dissolved again in the next round, thereby improving the full utilization of the crude cobalt hydroxide slurry, reducing the problem of high labor intensity caused by manual cleaning and transfer of the slurry, saving time for cleaning and transfer of the slurry, and thus improving production efficiency.

[0170] In one embodiment, the selective precipitation component is connected to the slurry dissolving component, and the slurry dissolving component is connected to the transfer component. It can be understood that the slurry dissolving component is provided with a first overflow port, the first overflow port is connected to the slurry replenishing component, the slurry replenishing component is provided with a second overflow port, the second overflow port is connected to the selective precipitation component, and the selective precipitation component is connected to the slurry dissolving component, that is, the slurry dissolving component, the slurry replenishing component and the selective precipitation component form a circular connection; and the selective precipitation component is not limited to being used only for selective precipitation, but can also be used for slurry dissolving or slurry replenishing, similarly, the slurry dissolving component is not limited to being used only for slurry dissolving, but can also be used for selective precipitation or slurry replenishing, similarly, the slurry replenishing component is not limited to being used only for slurry replenishing, but can also be used for selective precipitation or slurry dissolving; therefore, when the leaching mechanism fails or other reasons occur, the slurry in the slurry replenishing component has more slurry. When it is not dissolved, the slurry replenishment component with more slurry accumulation in this round can be used as the slurry dissolving component in the next round, the slurry dissolving component in this round can be used as the selective precipitation component in the next round, and the selective precipitation component in this round can be used as the slurry replenishment component in the next round. Then, the selective leaching liquid obtained by processing the slurry replenishment component in this round in the next round of production flows to the transfer component. There is no need to transfer the slurry or move the position of the leaching mechanism, so that the slurry that is not fully dissolved accumulated in this round can be dissolved again in the next round, thereby improving the full utilization of the crude cobalt hydroxide slurry, reducing the problem of high labor intensity caused by manual cleaning and transfer of the slurry, saving time for cleaning and transfer of the slurry, and thus improving production efficiency.

[0171] In one embodiment, the third overflow port is connected to the primary dissolving slurry kettle, and the primary dissolving slurry kettle, the intermediate dissolving slurry kettle, the secondary dissolving slurry kettle, the slurry replenishing assembly, the first hydrolysis precipitation kettle and the second hydrolysis precipitation kettle are respectively connected to the transfer assembly. It can be understood that the primary dissolving slurry kettle, the primary dissolving slurry kettle, the secondary dissolving slurry kettle, the slurry replenishing assembly, the first hydrolysis precipitation kettle and the second hydrolysis precipitation kettle form a circular connection; and the selective precipitation assembly is not limited to being used only for selective precipitation, but can also be used for dissolving slurry or slurry replenishing. Similarly, the dissolving slurry assembly is not limited to being used only for dissolving slurry, but can also be used for selective precipitation or slurry replenishing. Similarly, the slurry replenishing assembly is not limited to being used only for slurry replenishing, but can also be used for selective precipitation or dissolving slurry. Therefore, when the leaching mechanism fails or for other reasons, for example, when a large amount of undissolved crude cobalt hydroxide slurry is accumulated in the second hydrolysis precipitation kettle, there is no need to transfer the slurry or move the position of the leaching mechanism, so that the second hydrolysis precipitation kettle of this round can be used as the primary dissolving slurry kettle of the next round. The primary dissolving kettle of this round serves as the intermediate dissolving kettle of the next round, the intermediate dissolving kettle of this round serves as the secondary dissolving kettle of the next round, the secondary dissolving kettle of this round serves as the slurry replenishing component of the next round, the slurry replenishing component of this round serves as the first hydrolysis precipitation kettle of the next round, the first hydrolysis precipitation kettle of this round serves as the second hydrolysis precipitation kettle of the next round, and the selective leachate obtained by the first hydrolysis precipitation kettle of this round in the next round of production flows to the transfer component, so that the incompletely dissolved slurry accumulated in this round can be dissolved again in the next round, thereby improving the full utilization of the crude cobalt hydroxide slurry, reducing the need for manual cleaning and transfer of the slurry, and reducing the labor intensity caused by manual cleaning and transfer of the slurry, saving time for cleaning and transfer of the slurry, and thus improving production efficiency.

[0172] The traditional leaching process is carried out in a single reactor. When problems arise during production, it is difficult to analyze which step caused the problem, and even if analyzed, it is difficult to make timely adjustments. The traditional leaching process also requires reduction and oxidation reactions, which means the process is relatively complex, making the reactor structure more complex and occupying a large area. In order to simplify the structure of the continuous selective leaching device for crude cobalt hydroxide while making it easier to analyze and adjust production problems, in one embodiment, the leaching mechanism includes a primary slurry reactor, an intermediate slurry reactor, a secondary slurry reactor, a slurry replenishment assembly, a first hydrolysis precipitation reactor, and a second hydrolysis precipitation reactor, which are connected in sequence. It can be understood that the crude cobalt hydroxide used in this article is a cobalt intermediate, which includes 34.7% Co, 1.75% Mn, 1.83% Cu, 0.08% Ni, 0.88% Ca, 5.3% Mg, 1.22% Fe, 0.23% Al and 15% water. Therefore, the amount of precipitate obtained in each step of the process is predictable, and the production of each step can be observed based on the amount, color and morphology of the precipitate to see whether there is a problem. When problems are found in the process links, corresponding adjustments and improvements are made quickly to ensure normal production, thereby ensuring production efficiency and improving the quality of the leachate and the quality of subsequent cobalt products. After it is observed that a problem occurs in a certain link in the process, the intermediate product before this step can be saved and wait for adjustment and improvement to continue production. For the link and subsequent links where problems occur, targeted adjustments are made, and the intermediate products that cannot be adjusted are discarded to avoid the problem of subsequent cobalt products being unqualified due to unqualified intermediate products, which causes greater losses.

[0173] In one embodiment, the crude cobalt hydroxide continuous selective leaching device further includes a filter press mechanism, which is connected to the transfer mechanism and is used to be connected to the leaching residue slurry making device.

[0174] In one embodiment, the leaching mechanism further includes a heating component, and the active end of the heating component acts on the slurry component.

[0175] In one embodiment, the heating component is a steam heating component, and the steam heating component is provided with a steam output end, which is connected to the slurry dissolving component.

[0176] In one embodiment, the slurry dissolving component is provided with a first pH measuring component.

[0177] In one embodiment, the grouting assembly is provided with a second pH measuring assembly.

[0178] In one embodiment, the selective precipitation component is provided with a third pH measurement component.

[0179] In one embodiment, the leaching mechanism further includes at least a first stirring component, and the stirring end of the first stirring component is disposed in the slurry component.

[0180] In one embodiment, the slurry dissolving component is formed with a slurry inlet trough and a slurry inlet port which are connected to each other, and the slurry inlet trough is connected to the first overflow port.

[0181] In one embodiment, the leaching mechanism further includes a first slurry supply component, and the first slurry supply component is connected to the slurry dissolving component.

[0182] In one embodiment, the first slurry supply component includes a first pH meter, a first flow rate monitor, a first movable partition and a first slurry supply tank body. The first slurry supply tank body is connected to the slurry dissolving component. The first movable partition is arranged at the connection between the first slurry supply tank body and the slurry dissolving component. The detection end of the first pH meter is arranged in the slurry dissolving component, and the action end of the first flow rate monitor is arranged at the first overflow port. It can be understood that the first pH meter is used to add an acidic solution to the slurry dissolving component and monitor the pH of the mixed material body in the slurry dissolving component, and adjust the addition rate of the acidic solution according to the pH. The first flow rate monitor is used to monitor the flow rate of the mixed material body, change the opening of the first movable partition according to the flow rate, and then change the flow rate of the crude cobalt hydroxide slurry, thereby ensuring the leaching effect of the crude cobalt hydroxide slurry in the acidic solution, that is, ensuring the leaching rate of divalent cobalt ions.

[0183] In one embodiment, the first slurry supply assembly is used to set the flow rate of the crude cobalt hydroxide slurry to 1m 3 / h~3m 3 / h.

[0184] In one embodiment, the slurry feeding component is provided with a slurry holding tank and a feeding port which are connected to each other, and the slurry holding tank is connected to the first overflow port and the selective precipitation component respectively.

[0185] In one embodiment, the leaching mechanism further includes a second slurry supply component, and the second slurry supply component is connected to the slurry replenishment component.

[0186] In one embodiment, the second slurry supply component includes a second pH meter, a second flow rate monitor, a second movable partition and a second slurry supply tank body. The second slurry supply tank body is connected to the slurry dissolving component. The second movable partition is arranged at the connection point between the second slurry supply tank body and the slurry dissolving component. The detection end of the second pH meter is arranged in the slurry dissolving component, and the active end of the second flow rate monitor is arranged at the second overflow port.

[0187] This article also provides a two-stage leaching equipment for crude cobalt hydroxide, including a first-stage leachate storage mechanism, a leach residue slurrying device, and a crude cobalt hydroxide continuous selective leaching device according to any of the above embodiments, wherein the filter press mechanism is respectively connected to the first-stage leachate storage mechanism and the leach residue slurrying device.

[0188] The above-mentioned crude cobalt hydroxide two-stage leaching equipment collects precipitates in batches for leaching, saves energy for batch processing of precipitates, reduces the use of leaching residue pulping equipment, and thus reduces damage and maintenance of the leaching residue pulping equipment, thereby increasing the service life of the leaching residue pulping equipment and significantly improving production efficiency; and because it avoids the problem of transferring divalent cobalt to a transfer tank for iron removal after leaching, and having to wait for trivalent cobalt reduction leachate to be removed together, the phenomenon of equipment being occupied but not used is reduced, that is, the utilization rate of the equipment is ensured, and the equipment footprint is reduced.

[0189] In one embodiment, the leached residue slurrying apparatus includes a two-stage leaching mechanism and a two-stage leachate storage mechanism, wherein the two-stage leaching mechanism is connected to a filter press mechanism. It is understood that the second-stage reduced leachate is stored in the second-stage leachate storage mechanism, i.e., it is stored in a separate storage mechanism from the first-stage leachate.

[0190] This article also provides a cobalt product production system, including a first-stage leachate treatment device, a second-stage leachate treatment device and a crude cobalt hydroxide second-stage leaching device according to any of the above embodiments, wherein the first-stage leachate treatment device is connected to the first-stage leachate storage mechanism, and the second-stage leachate treatment device is connected to the second-stage leachate storage device.

[0191] In the above-mentioned cobalt product production system, the first-stage leachate treatment equipment is used to treat the first-stage leachate, and the second-stage leachate treatment equipment is used to treat the second-stage reduction leachate. That is, the first-stage leachate and the second-stage reduction leachate are treated separately, which ensures the quality of the cobalt product obtained from the first-stage leachate, simplifies the process of treating the first-stage leachate, and improves production convenience and efficiency.

[0192] The following examples illustrate some specific embodiments, where percentages are expressed by weight. It should be noted that the following examples do not exhaust all possible situations, and that the materials used in the following examples, unless otherwise specified, can be obtained from commercial sources.

[0193] Example 1

[0194] Crude cobalt hydroxide is a cobalt intermediate product, which includes 34.7% Co, 1.75% Mn, 1.83% Cu, 0.08% Ni, 0.88% Ca, 5.3% Mg, 1.22% Fe, 0.23% Al and 15% moisture.

[0195] Weighing 1 ton of crude cobalt hydroxide and 3 tons of water, mixing and stirring to obtain 4 tons of crude cobalt hydroxide slurry, adding concentrated sulfuric acid and 3.85 tons of crude cobalt hydroxide slurry simultaneously, mixing and stirring, and then heating to 60° C. to make the pH value of the mixed solution of the crude cobalt hydroxide slurry and concentrated sulfuric acid slurry 1.0, and then reacting for 1 hour to obtain a preliminary leachate with a pH of 2.0 to 2.5 and an acid leaching residue;

[0196] gradually adding the remaining 0.15 tons of crude cobalt hydroxide slurry to the preliminary leachate to obtain an adjusted leachate; then subjecting the adjusted leachate to a selective precipitation operation for 1 hour to sequentially obtain a first precipitate and a primary selective leachate with a pH of 3.5 to 4.0, a second precipitate and a secondary selective leachate with a pH of 4.0 to 4.5, and a third precipitate and a selective leachate with a pH of 5.0 to 5.5;

[0197] A filter press was used to perform solid-liquid separation, obtaining a section of leachate and 0.19 tons of solid matter;

[0198] Then, the first leachate was extracted once with P204 for 30 min to obtain P204 raffinate.

[0199] Then, the P204 raffinate was extracted once with P507, and each extraction time was 20 minutes to obtain a cobalt-containing organic phase and a P507 raffinate;

[0200] Then, the cobalt-containing organic phase is stripped with sulfuric acid to obtain a cobalt sulfate solution;

[0201] performing an evaporation and crystallization operation on the cobalt sulfate solution to obtain cobalt sulfate crystals;

[0202] The solid matter is collected and waits for batch secondary reduction leaching treatment.

[0203] Example 2

[0204] Crude cobalt hydroxide is a cobalt intermediate product, which includes 34.7% Co, 1.75% Mn, 1.83% Cu, 0.08% Ni, 0.88% Ca, 5.3% Mg, 1.22% Fe, 0.23% Al and 15% moisture.

[0205] Weighing 1 ton of crude cobalt hydroxide and 4 tons of water, mixing and stirring to obtain 5 tons of crude cobalt hydroxide slurry, adding concentrated sulfuric acid and 4.84 tons of crude cobalt hydroxide slurry simultaneously, mixing and stirring, and then heating to 65° C. to make the pH value of the mixed solution of the crude cobalt hydroxide slurry and concentrated sulfuric acid slurry 1.3, and then reacting for 1 hour to obtain a preliminary leachate with a pH of 2.0 to 2.5 and an acid leaching residue;

[0206] 0.16 tons of crude cobalt hydroxide slurry is gradually added to the preliminary leachate to obtain an adjusted leachate; the adjusted leachate is then subjected to a selective precipitation operation for 1 hour to sequentially obtain a first precipitate and a primary selective leachate with a pH of 3.5 to 4.0, a second precipitate and a secondary selective leachate with a pH of 4.0 to 4.5, and a third precipitate and a selective leachate with a pH of 5.0 to 5.5;

[0207] A filter press was used to perform solid-liquid separation, obtaining a section of leachate and 0.21 tons of solid matter;

[0208] Then, the first leachate was extracted once with P204 for 30 min to obtain P204 raffinate.

[0209] Then, the P204 raffinate was extracted once with P507, and each extraction time was 20 minutes to obtain a cobalt-containing organic phase and a P507 raffinate;

[0210] Then, the cobalt-containing organic phase is stripped with sulfuric acid to obtain a cobalt sulfate solution;

[0211] performing an evaporation and crystallization operation on the cobalt sulfate solution to obtain cobalt sulfate crystals;

[0212] The solid matter is collected and waits for batch secondary reduction leaching treatment.

[0213] Example 3

[0214] Crude cobalt hydroxide is a cobalt intermediate product, which includes 34.7% Co, 1.75% Mn, 1.83% Cu, 0.08% Ni, 0.88% Ca, 5.3% Mg, 1.22% Fe, 0.23% Al and 15% moisture.

[0215] Weighing 1 ton of crude cobalt hydroxide and 2.5 tons of water, mixing and stirring to obtain 3.5 tons of crude cobalt hydroxide slurry, adding 3.39 tons of crude cobalt hydroxide slurry and concentrated sulfuric acid simultaneously, mixing and stirring, and then heating to 70° C. to make the pH value of the mixed solution of the crude cobalt hydroxide slurry and concentrated sulfuric acid 1.5, and then reacting for 1 hour to obtain a preliminary leachate with a pH of 2.0 to 2.5 and an acid leaching residue;

[0216] 0.11 tons of crude cobalt hydroxide slurry is gradually added to the preliminary leachate to obtain an adjusted leachate; the adjusted leachate is then subjected to a selective precipitation operation for 1 hour to sequentially obtain a first precipitate and a primary selective leachate with a pH of 3.5 to 4.0, a second precipitate and a secondary selective leachate with a pH of 4.0 to 4.5, and a third precipitate and a selective leachate with a pH of 5.0 to 5.5;

[0217] A filter press was used to perform solid-liquid separation to obtain a leachate and 0.18 tons of acid leaching residue.

[0218] Then, the first leachate was extracted once with P204 for 30 min to obtain P204 raffinate.

[0219] Then, the P204 raffinate was extracted once with P507, and each extraction time was 20 minutes to obtain a cobalt-containing organic phase and a P507 raffinate;

[0220] Then, the cobalt-containing organic phase is stripped with sulfuric acid to obtain a cobalt sulfate solution;

[0221] performing an evaporation and crystallization operation on the cobalt sulfate solution to obtain cobalt sulfate crystals;

[0222] The solid matter is collected and waits for batch secondary reduction leaching treatment.

[0223] Example 4

[0224] Crude cobalt hydroxide is a cobalt intermediate product, which includes 34.7% Co, 1.75% Mn, 1.83% Cu, 0.08% Ni, 0.88% Ca, 5.3% Mg, 1.22% Fe, 0.23% Al and 15% moisture.

[0225] Weighing 1 ton of crude cobalt hydroxide and 3 tons of water, mixing and stirring to obtain 4 tons of crude cobalt hydroxide slurry, adding concentrated sulfuric acid and 3.87 tons of crude cobalt hydroxide slurry simultaneously, mixing and stirring, and then heating to 70° C. to make the pH value of the mixed solution of the crude cobalt hydroxide slurry and concentrated sulfuric acid slurry 1.0, and then reacting for 1 hour to obtain a preliminary leachate with a pH of 2.0 to 2.5 and an acid leaching residue;

[0226] The remaining 0.13 tons of crude cobalt hydroxide slurry was gradually added to the preliminary leachate to obtain an adjusted leachate; the adjusted leachate was then subjected to a selective precipitation operation for 1 hour to obtain, in sequence, a first precipitate and a primary selective leachate with a pH of 3.2 to 3.4, a second precipitate and a secondary selective leachate with a pH of 4.7, and a third precipitate and a selective leachate with a pH of 5.0 to 5.5;

[0227] A filter press was used to perform solid-liquid separation operations, and a first-stage leachate, 0.16 tons of acid leaching residue, 27.82 kg of the first precipitate, 7.06 kg of the second precipitate, and 13.86 kg of the third precipitate were obtained respectively;

[0228] Then, the first leachate was extracted once with P204 for 30 min to obtain P204 raffinate.

[0229] Then, the P204 raffinate was extracted once with P507, and each extraction time was 20 minutes to obtain a cobalt-containing organic phase and a P507 raffinate;

[0230] Then, the cobalt-containing organic phase is stripped with sulfuric acid to obtain a cobalt sulfate solution;

[0231] performing an evaporation and crystallization operation on the cobalt sulfate solution to obtain cobalt sulfate crystals;

[0232] The acid leaching residue is collected and waits for batch secondary reduction leaching treatment.

[0233] Comparative Example 1

[0234] Crude cobalt hydroxide is a cobalt intermediate product, which includes 34.7% Co, 1.75% Mn, 1.83% Cu, 0.08% Ni, 0.88% Ca, 5.3% Mg, 1.22% Fe, 0.23% Al and 15% moisture.

[0235] 1) Weighing 1 ton of crude cobalt hydroxide and 3 tons of water, mixing and stirring to form a slurry, heating to 60° C. to 70° C. to obtain a crude cobalt hydroxide slurry, gradually adding concentrated sulfuric acid to the crude cobalt hydroxide slurry to obtain a reaction mixture of the crude cobalt hydroxide slurry and concentrated sulfuric acid with a pH of 0.45 to 0.5, stirring for 1 hour, and filtering; obtaining a first-stage leachate and 0.20 tons of acid leaching residue; the first-stage leachate is directly fed into a transfer tank for iron removal; and performing a secondary slurrying operation on 0.20 tons of acid leaching residue and twice the amount of water;

[0236] 2) Secondary reduction leaching: After the acid leaching residue is secondary slurried, the temperature is raised to 50°C to 60°C, sodium metabisulfite is added, and the slurry pH is maintained at 1.0 to 1.5 until the reduction potential is lower than 240mV;

[0237] Pre-oxidation: After step 2), add manganese dioxide ore to 2+ Oxidized to Fe 3+ , when Fe in the slurry 2+ The content is lower than 0.05 g / L, and the obtained second-stage reduction leaching solution is transferred to the transfer tank for iron removal to obtain a mixture of the first-stage leaching solution and the second-stage reduction leaching solution;

[0238] The mixed solution is subjected to selective precipitation treatment to obtain a leachate and a precipitate; and the concentration of tetravalent manganese ions in Comparative Example 1 is higher than that in Examples 1 to 4;

[0239] Then, the leachate was extracted once with P204 for 30 min to obtain P204 raffinate.

[0240] The P204 raffinate was then extracted twice with P507, each extraction time being 30 min, to obtain a cobalt-containing organic phase and a P507 raffinate;

[0241] Then, the cobalt-containing organic phase is stripped with sulfuric acid to obtain a cobalt sulfate solution;

[0242] performing an evaporation and crystallization operation on the cobalt sulfate solution to obtain cobalt sulfate crystals;

[0243] The sodium ions in the P507 raffinate are treated.

[0244] Comparative Example 2

[0245] Crude cobalt hydroxide is a cobalt intermediate product, which includes 34.7% Co, 1.75% Mn, 1.83% Cu, 0.08% Ni, 0.88% Ca, 5.3% Mg, 1.22% Fe, 0.23% Al and 15% moisture.

[0246] 1) Weighing 1 ton of crude cobalt hydroxide and 3 tons of water, mixing and stirring to form a slurry, heating to 60° C. to 70° C. to obtain a crude cobalt hydroxide slurry, gradually adding concentrated sulfuric acid to the crude cobalt hydroxide slurry to obtain a reaction mixture of the crude cobalt hydroxide slurry and concentrated sulfuric acid with a pH of 0.45 to 0.5, stirring for 1 hour, and filtering; obtaining a first-stage leachate and 0.20 tons of acid leaching residue; the first-stage leachate is directly fed into a transfer tank for iron removal; and performing a secondary slurrying operation on 0.20 tons of acid leaching residue and twice the amount of water;

[0247] 2) Secondary reduction leaching: After the acid leaching residue is secondary slurried, the temperature is raised to 50°C to 60°C, sulfur dioxide is added, and the slurry pH is maintained at 1.0 to 1.5 until the reduction potential is lower than 240mV;

[0248] Pre-oxidation: After step 2), sodium chlorate is added to 2+ Oxidized to Fe 3+ , when Fe in the slurry 2+ The content is lower than 0.05 g / L, and the obtained second-stage reduction leaching solution is transferred to the transfer tank for iron removal to obtain a mixture of the first-stage leaching solution and the second-stage reduction leaching solution;

[0249] The mixed solution is subjected to selective precipitation treatment to obtain a leachate and a precipitate; and the concentration of tetravalent manganese ions in Comparative Example 1 is higher than that in Examples 1 to 4;

[0250] Then, the leachate was extracted once with P204 for 30 min to obtain P204 raffinate.

[0251] The P204 raffinate was then extracted twice with P507, each extraction time being 30 min, to obtain a cobalt-containing organic phase and a P507 raffinate;

[0252] Then, the cobalt-containing organic phase is stripped with sulfuric acid to obtain a cobalt sulfate solution;

[0253] performing an evaporation and crystallization operation on the cobalt sulfate solution to obtain cobalt sulfate crystals;

[0254] The sodium ions in the P507 raffinate are treated.

[0255] The contents of iron ions, aluminum ions, copper ions, tetravalent manganese ions, nickel ions, calcium ions, magnesium ions, and sodium ions in the first-stage leachates of Examples 1 to 4 and the leachates of Comparative Examples 1 to 2 were measured, and the results are shown in Table 1 below:

[0256] Table 1: Metal ion content

[0257] Since the amount of crude cobalt hydroxide added in Examples 1 to 4 and Comparative Examples 1 to 2 is the same, but the amount of water added is different, the amount of 3 tons of water added in Example 1 is used as the standard to convert the metal ion content in Examples 1 to 4 and Comparative Examples 1 to 2 to obtain Table 2.

[0258] Table 2: Metal ion content

[0259] The contents of cobalt, iron, aluminum, copper, manganese, nickel, calcium, magnesium and sodium in the first-stage leached cobalt products obtained in Examples 1 to 4, and the contents of cobalt, iron, aluminum, copper, manganese, nickel, calcium, magnesium and sodium in the cobalt products obtained in Comparative Examples 1 to 2 were measured respectively. The results are shown in Table 3 below:

[0260] Table 3: Metal ion content and sulfur content in cobalt products

[0261] 1) As can be seen from Table 2, in the selective leachates of Examples 1 to 4, the content of tetravalent manganese ions is significantly lower than that of Comparative Examples 1 to 2, the content of sodium ions in Examples 1 to 4 is equal to 0, the content of sodium ions and tetravalent manganese ions in Comparative Example 1 is significantly higher than those in Examples 1 to 4, and the content of sodium ions in Comparative Example 2 is significantly higher than that in Examples 1 to 4.

[0262] 2) As shown in 1), the sodium ion content in the first-stage leachate of Examples 1 to 4 is equal to 0. Therefore, in the subsequent extraction process, the number of extraction processes and the time for each extraction process are less than those in Comparative Examples 1 to 2, thereby improving production efficiency and saving the use of extraction agent. In addition, the subsequently obtained P507 raffinate does not contain sodium ions, and there is no need to remove sodium ions from the P507 raffinate.

[0263] Similarly, the content of tetravalent manganese ions in the first-stage leachate of Examples 1 to 4 was significantly lower than that in Comparative Example 1. Therefore, in the subsequent extraction process, the number of extraction processes and the time for each extraction process were both shorter than those in Comparative Examples 1 to 2, thereby improving production efficiency and saving the use of extraction agents.

[0264] 3) As can be seen from Table 3, the cobalt products of the first-stage leaching of Examples 1 to 4 meet the national standard for superior cobalt sulfate; the cobalt products of Comparative Examples 1 to 2 meet the national standard for first-class cobalt sulfate. That is, the quality of the cobalt products of the first-stage leaching of Examples 1 to 4 is significantly higher than that of the cobalt products of Comparative Examples 1 to 2.

[0265] 4) 27.82 kg of the first precipitate obtained in Example 4 was dissolved with 100 L of dilute hydrochloric acid to obtain a first dissolution solution and 5.27 kg of acid leaching residue, and the concentration of iron ions in the first dissolution solution was determined to be 2.085 mol / L. It can be seen that the mass proportion of iron hydroxide in the first precipitate is 80.2%, and the proportion of iron hydroxide in the soluble matter is 98.9%, which shows that the recovery value of the first precipitate is high;

[0266] 7.06 kg of the second precipitate obtained in Example 4 was dissolved with 100 L of dilute hydrochloric acid to obtain a second dissolution solution and 0.99 kg of acid leaching residue. The concentration of aluminum ions in the second dissolution solution was determined to be 0.771 mol / L. It can be seen that the mass proportion of aluminum hydroxide in the second precipitate is 85.1%, and the proportion of aluminum hydroxide in the soluble matter is 99.01%. It can be seen that the recovery value of the second precipitate is high;

[0267] 13.86 kg of the third precipitate obtained in Example 4 was dissolved with 100 L of dilute hydrochloric acid to obtain a third dissolution solution and 0.04 kg of acid leaching residue. The concentration of copper ions in the third dissolution solution was determined to be 1.413 mol / L. It can be seen that the mass proportion of copper hydroxide in the third precipitate is 99.42%, and the proportion of aluminum hydroxide in the soluble matter is 99.71%. It can be seen that the recovery value of the third precipitate is high.

[0268] Compared with the existing technology, this paper has at least the following advantages:

[0269] 1) In the continuous selective leaching process of crude cobalt hydroxide herein, an acidic solution is used to leach divalent cobalt ions, trivalent iron ions, aluminum ions, copper ions, and impurity ions in the crude cobalt hydroxide slurry to obtain a preliminary leachate, and then the added crude cobalt hydroxide slurry is gradually dissolved in the acidic solution to gradually increase the pH value until the pH value is within a range in which divalent cobalt ions are not precipitated and most impurity ions are precipitated, so that the divalent cobalt ions exist in ionic form and most impurities exist in the precipitate, thereby separating the divalent cobalt ions from most impurities in the solid-liquid state, thereby achieving selective leaching of crude cobalt hydroxide.

[0270] 2) The continuous selective leaching process for crude cobalt hydroxide in this article not only avoids the problem of introducing sodium ions by adding a reducing agent, introducing sodium ions or tetravalent manganese ions by adding an oxidant, and introducing sodium ions or potassium ions by adding an alkaline auxiliary material in the traditional crude cobalt hydroxide selective leaching process, but also simplifies the subsequent treatment process for sodium ions, tetravalent manganese ions and potassium ions, thereby improving production efficiency, and reducing the concentrations of sodium ions, tetravalent manganese ions and potassium ions, ensuring the quality of the cobalt products produced subsequently.

Claims

1. A continuous selective leaching process for crude cobalt hydroxide, characterized in that: The steps include: preparing a crude cobalt hydroxide slurry; Mixing a portion of the crude cobalt hydroxide slurry and the acidic solution until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a primary leaching solution; adding another portion of the crude cobalt hydroxide slurry to the preliminary leachate for mixing to obtain an adjusted leachate; performing a selective precipitation operation on the adjusted leachate to form a precipitate and a selective leachate; The precipitate and the selective leaching solution are subjected to a solid-liquid separation operation to obtain a first-stage leaching solution and acid leaching residue respectively.

2. The continuous selective leaching process for crude cobalt hydroxide according to claim 1, characterized in that: The step of preparing the crude cobalt hydroxide slurry is specifically: preparing the crude cobalt hydroxide slurry by mixing crude cobalt hydroxide and water in a mass ratio of 1:(2.5-4).

3. The continuous selective leaching process for crude cobalt hydroxide according to claim 1, characterized in that: The step of preparing the crude cobalt hydroxide slurry by mixing crude cobalt hydroxide and water in a mass ratio of 1:(2.5-4) is specifically as follows: preparing the crude cobalt hydroxide slurry by mixing crude cobalt hydroxide and water in a mass ratio of 1:(2.5-4) under stirring.

4. The continuous selective leaching process for crude cobalt hydroxide according to claim 3, characterized in that: The acidic solution is at least one of sulfuric acid or hydrochloric acid.

5. The continuous selective leaching process for crude cobalt hydroxide according to claim 4, characterized in that: The pH of the preliminary leaching solution is 2.0-2.

5.

6. The continuous selective leaching process for crude cobalt hydroxide according to claim 1, characterized in that: Under heating conditions, a portion of the crude cobalt hydroxide slurry and the acidic solution are mixed until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a preliminary leachate; and / or, Under heating conditions, another portion of the crude cobalt hydroxide slurry is added to the preliminary leaching solution for mixing to obtain an adjusted leaching solution.

7. The continuous selective leaching process for crude cobalt hydroxide according to claim 6, characterized in that: Under the condition of 60° C. to 70° C., a portion of the crude cobalt hydroxide slurry and the acidic solution are mixed until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a preliminary leaching solution; and / or, Under the condition of 60° C. to 70° C., another portion of the crude cobalt hydroxide slurry is added to the preliminary leaching solution for mixing to obtain an adjusted leaching solution.

8. The continuous selective leaching process for crude cobalt hydroxide according to claim 1, characterized in that: The time for the steps of mixing a portion of the crude cobalt hydroxide slurry with the acidic solution until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a preliminary leaching solution is 0.8 h to 1.2 h.

9. The continuous selective leaching process for crude cobalt hydroxide according to claim 8, characterized in that: The time for the steps of mixing a portion of the crude cobalt hydroxide slurry and the acidic solution until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a preliminary leaching solution is 1 hour.

10. The continuous selective leaching process for crude cobalt hydroxide according to claim 1, characterized in that: The step of mixing a portion of the crude cobalt hydroxide slurry with the acidic solution until the crude cobalt hydroxide slurry is dissolved in the acidic solution to obtain a preliminary leachate is specifically: A portion of the crude cobalt hydroxide slurry and the acidic solution are subjected to at least two mixing and stirring leaching operations to obtain the preliminary leaching solution.

11. The continuous selective leaching process for crude cobalt hydroxide according to claim 10, characterized in that: The step of performing at least two mixing and stirring leaching operations on a portion of the crude cobalt hydroxide slurry and the acidic solution to obtain the preliminary leachate is specifically: performing a first leaching operation on a portion of the crude cobalt hydroxide slurry and the acidic solution to obtain a primary leaching solution; performing a second leaching operation on the primary leaching solution to obtain a secondary leaching solution; The secondary leaching solution is subjected to a third leaching operation to obtain a preliminary leaching solution.

12. The continuous selective leaching process for crude cobalt hydroxide according to claim 11, characterized in that: The pH of the primary leaching solution is 1.0 to 1.

5.

13. The continuous selective leaching process for crude cobalt hydroxide according to claim 11, characterized in that: The pH of the secondary leaching solution is 1.5-2.

0.

14. The continuous selective leaching process for crude cobalt hydroxide according to claim 11, characterized in that: The pH of the preliminary leaching solution is 2.0-2.

5.

15. The continuous selective leaching process for crude cobalt hydroxide according to claim 1, characterized in that: The sum of the time for adding another portion of the crude cobalt hydroxide slurry to the preliminary leaching solution for mixing and the time for performing the selective precipitation operation on the adjusted leaching solution is 0.8h to 1.2h.

16. The continuous selective leaching process for crude cobalt hydroxide according to claim 1, characterized in that: The step of performing a selective precipitation operation on the adjusted leachate is specifically: The adjusted leachate is subjected to at least one selective precipitation operation to form a precipitate and a selective leachate.

17. The continuous selective leaching process for crude cobalt hydroxide according to claim 1, characterized in that: The step of performing a selective precipitation operation on the adjusted leachate comprises: performing a first selective precipitation operation on the adjusted leachate to obtain a primary selective leachate and a first precipitate; performing a second selective precipitation operation on the first selective leaching solution to obtain a second selective leaching solution and a second precipitate; The secondary selective leaching solution is subjected to a third selective precipitation operation to obtain a selective leaching solution and a third precipitate.

18. The continuous selective leaching process for crude cobalt hydroxide according to claim 17, characterized in that: The pH of the primary selective leaching solution is 3.5-4.0; and / or, The pH of the secondary selective leaching solution is 4.0-4.5; and / or, The pH of the selective leaching solution is 5.0-5.

5.

19. The continuous selective leaching process for crude cobalt hydroxide according to claim 17, characterized in that: The pH of the primary selective leaching solution is 3.2 to 3.4; and / or, The pH of the secondary selective leaching solution is 4.7; and / or, The pH of the selective leaching solution is 5.0-6.

7.

20. The continuous selective leaching process for crude cobalt hydroxide according to claim 17, characterized in that: The step of mixing a portion of the crude cobalt hydroxide slurry and the acidic solution is specifically as follows: A portion of the crude cobalt hydroxide slurry and the acidic solution are added simultaneously and mixed.

21. The continuous selective leaching process for crude cobalt hydroxide according to claim 1, characterized in that: The volume ratio of the portion of the crude cobalt hydroxide slurry to the acidic solution is 14-16.

22. A cobalt product production process, characterized in that: The steps include: The first stage leachate is obtained by the continuous selective leaching process for crude cobalt hydroxide according to claims 1 to 22; the first stage leachate is subjected to extraction treatment; The first-stage leaching solution that has undergone the extraction treatment is processed to obtain a first-stage leaching cobalt product.

23. A continuous selective leaching device for crude cobalt hydroxide, characterized in that: The leaching operation is performed by using the continuous selective leaching process for crude cobalt hydroxide according to any one of claims 1 to 23, wherein the continuous selective leaching device for crude cobalt hydroxide comprises: A leaching mechanism, the leaching mechanism at least comprising a slurry dissolving component, a slurry replenishing component and a selective precipitation component, the slurry dissolving component is provided with the first overflow port, the first overflow port is connected to the slurry replenishing component, the slurry replenishing component is provided with the second overflow port, the second overflow port is connected to the selective precipitation component, and the selective precipitation component is provided with the third overflow port; A transfer mechanism, the transfer mechanism is connected to the third overflow port, and the transfer mechanism is used to be connected to the primary leachate storage mechanism and the leachate residue pulping device respectively.

24. The continuous selective leaching device for crude cobalt hydroxide according to claim 23, characterized in that: The selective precipitation component is connected to the slurry dissolving component.

25. The continuous selective leaching device for crude cobalt hydroxide according to claim 24, characterized in that: The slurry dissolving component is connected to the transfer component; and / or, The grouting component is connected to the transfer component.

26. The continuous selective leaching device for crude cobalt hydroxide according to claim 23, characterized in that: The slurry dissolving component at least comprises a primary slurry dissolving kettle and a secondary slurry dissolving kettle which are connected to each other, and the first overflow port is formed in the secondary slurry dissolving kettle.

27. The continuous selective leaching device for crude cobalt hydroxide according to claim 26, characterized in that: The slurry dissolving component further comprises an intermediate slurry dissolving kettle, and the intermediate slurry dissolving kettle is respectively connected to the primary slurry dissolving kettle and the secondary slurry dissolving kettle.

28. The continuous selective leaching device for crude cobalt hydroxide according to claim 23, characterized in that: The crude cobalt hydroxide continuous selective leaching device also includes a filter press mechanism, which is connected to the transfer mechanism and is used to be connected to the leached residue slurry making device.

29. The continuous selective leaching device for crude cobalt hydroxide according to claim 23, characterized in that: The selective precipitation component at least includes a first hydrolysis precipitation tank and a second hydrolysis precipitation tank that are connected to each other, and the third overflow port is formed in the second hydrolysis precipitation tank.

30. The continuous selective leaching device for crude cobalt hydroxide according to claim 23, characterized in that: The leaching mechanism also includes a heating component, and the action end of the heating component acts on the slurry component.

31. The continuous selective leaching device for crude cobalt hydroxide according to claim 30, characterized in that: The heating component is a steam heating component, and the steam heating component is provided with a steam output end, and the steam output end is connected to the slurry dissolving component.

32. The continuous selective leaching device for crude cobalt hydroxide according to claim 23, characterized in that: The slurry dissolving component is provided with a first pH measuring component; and / or, The grouting component is provided with a second pH measuring component; and / or, The selective precipitation component is provided with a third pH measurement component.

33. The continuous selective leaching device for crude cobalt hydroxide according to claim 23, characterized in that: The leaching mechanism at least further comprises a first stirring component, wherein a stirring end of the first stirring component is disposed in the slurry dissolving component; and / or, The slurry dissolving component is formed with a slurry inlet groove and a slurry inlet port which are connected to each other, and the slurry inlet groove is connected to the first overflow port.

34. The continuous selective leaching device for crude cobalt hydroxide according to claim 23, characterized in that: The leaching mechanism also includes a first slurry supply component, which is connected to the slurry dissolving component.

35. The continuous selective leaching device for crude cobalt hydroxide according to claim 23, characterized in that: The first slurry supply component includes a first pH meter, a first flow rate monitor, a first movable baffle and a first slurry supply tank body, the first slurry supply tank body is connected to the slurry dissolving component, the first movable baffle is arranged at the connection between the first slurry supply tank body and the slurry dissolving component, the detection end of the first pH meter is arranged in the slurry dissolving component, and the action end of the first flow rate monitor is arranged at the first overflow port; and / or, The first slurry supply assembly is used to set the flow rate of the crude cobalt hydroxide slurry to 1m 3 / h~3m 3 / h.

36. The continuous selective leaching device for crude cobalt hydroxide according to claim 23, characterized in that: The slurry replenishment component is provided with a slurry storage tank and a feeding port which are connected to each other. The slurry storage tank is connected to the first overflow port and the selective precipitation component respectively.

37. The continuous selective leaching device for crude cobalt hydroxide according to claim 23, characterized in that: The leaching mechanism further includes a second slurry supply component, and the second slurry supply component is connected to the slurry replenishment component.

38. The continuous selective leaching device for crude cobalt hydroxide according to claim 37, characterized in that: The second slurry supply component includes a second pH meter, a second flow rate monitor, a second movable baffle and a second slurry supply trough body. The second slurry supply trough body is connected to the slurry dissolving component. The second movable baffle is arranged at the connection point between the second slurry supply trough body and the slurry dissolving component. The detection end of the second pH meter is arranged in the slurry dissolving component, and the active end of the second flow rate monitor is arranged at the second overflow port.

39. A crude cobalt hydroxide two-stage leaching equipment, characterized in that: The invention comprises a leachate storage mechanism, a leachate slurry making device and a crude cobalt hydroxide continuous selective leaching device according to any one of claims 23 to 38, wherein the filter press mechanism is connected to the leachate storage mechanism and the leachate slurry making device respectively.

40. The crude cobalt hydroxide two-stage leaching equipment according to claim 39, characterized in that: The leached residue pulping device comprises a two-stage leaching mechanism and a two-stage leaching liquid storage mechanism which are connected to each other, and the two-stage leaching mechanism is connected to the filter press mechanism.

41. A cobalt product production system, characterized in that: It comprises a first-stage leachate treatment device, a second-stage leachate treatment device and a crude cobalt hydroxide second-stage leaching device according to any one of claims 39 to 40, wherein the first-stage leachate treatment device is connected to the first-stage leachate storage mechanism, and the second-stage leachate treatment device is connected to the second-stage leachate storage device.

Citation Information

Patent Citations

  • Method for two-stage leaching of nickel and cobalt from crude nickel and cobalt hydroxide

    CN111910075A

  • Selective leaching process of crude cobalt hydroxide ore

    CN112359225A

  • Method for manufacturing nickel and cobalt-containing solution from hydroxide containing nickel and cobalt

    CN113474069A

  • Method for continuously enriching nickel and cobalt from low-concentration nickel-cobalt solution

    CN114427037A

  • Production method of cobaltous sulfate for high-performance lithium ion power battery

    CN115057481A

Cited By

  • Method for enriching and separating nickel, cobalt and scandium

    CN121496170A