Ultrahigh-strength spring steel and preparation method therefor

By adopting the chemical composition and optimization process of manganese-aluminum-nitrogen microalloyation in spring steel, the problems of insufficient strength and high cost of existing spring steel are solved, and high-strength and low-cost ultra-high-strength spring steel are realized. Suitable for high-end equipment manufacturing industry.

WO2024239303A1PCT designated stage expired Publication Date: 2024-11-28SHANDONG JIANZHU UNIV +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/096184
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2023-05-25
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing spring steel is insufficient in strength, which cannot meet the needs of high-performance, high-speed engines and aerospace fields, and has high production costs, resulting in a small share of domestic spring products in the high-end market, unstable performance, and a short service life.

Method used

Ultra-high strength spring steel containing manganese-aluminum-nitrogen microalloy is used, with chemical compositions of C: 0.45-0.60%, Si: 0.15-0.35%, Mn: 6.0-12.0%, Al: 1.0-3.0%, Cr: 0.30-0.50%, Mo: 0.10-0.25%, V: 0.10-0.50%, Nb: 0.025-0.04%, N: 0.005-0.015%, improve the mechanical strength of spring steel by solid solution strengthening and refining grain structure , elongation and fatigue resistance, and reduce production costs through optimized processes.

Benefits of technology

It has achieved the effect of high mechanical strength, high elongation and good fatigue resistance of ultra-high strength spring steel, and the cost is lower than that of market-based spring steel. It is suitable for industrial production and is suitable for high-demand industries, such as equipment manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023096184_28112024_PF_FP_ABST
    Figure CN2023096184_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides ultrahigh-strength spring steel, comprising the following chemical components: C: 0.45-0.60%, Si: 0.15-0.35%, Mn: 6.0-12.0%, Al: 1.0-3.0%, Cr: 0.30-0.50%, Mo: 0.10-0.25%, V: 0.10-0.50%, Nb: 0.025-0.04%, N: 0.005-0.015%, Pb≤0.03%, Sn≤0.03%, Zn≤0.03%, Sb≤0.03%, Bi≤0.03%, O2≤15 ppm, H2≤15 ppm, S≤0.02%, P≤0.02%, Cu≤0.2%, Ni≤0.35%, and the balance of iron and inevitable impurities. The spring steel has high mechanical strength, large elongation, high percentage reduction of area and good anti-fatigue performance, and is suitable for manufacturing and production of weight-reduced few-leaf springs.
Need to check novelty before this filing date? Find Prior Art

Description

Ultra-high strength spring steel and preparation method thereof Technical Field

[0001] The present invention belongs to the technical field of special steel production, and in particular relates to an ultra-high strength (2GPa) spring steel and a preparation method thereof. Background Art

[0002] Springs, along with bolts and gears, constitute the three fundamental components of machinery. They come in a wide variety of varieties and are widely used in industries such as automotive, machinery, light industry, electric power, aerospace, and rail transit. Springs play a vital role in various types of machinery, performing complex tasks such as cushioning, shock absorption, energy storage, connection, support, and force transmission. Their excellent overall performance is essential for the safe operation of machinery, and improving spring quality is a prerequisite for ensuring the performance of the mainframe machinery. Springs operate under alternating stresses such as cyclical bending and torsion, enduring tension, compression, torsion, impact, fatigue, and corrosion. They sometimes operate in extremely harsh and complex environments, such as high and low temperatures, corrosion, and static loads. In recent years, with the rapid development of industries such as automotive and rail transit, particularly in the context of the dual carbon strategies of achieving peak carbon emissions and achieving carbon neutrality, the demand for spring weight reduction, such as lightweight design in automobiles and rail transit, to conserve energy and resources, has become increasingly urgent, leading to a growing demand for ultra-high-strength springs. However, the current strength of domestic spring steel is only around 1350 MPa, severely hindering the development of new energy vehicles and the reduction of weight and emissions across various types of vehicles. It also fails to meet the demands of high-performance, high-speed engines, particularly in the aviation and aerospace sectors. Developing high-performance spring steel with ultra-high strength, high elongation, high reduction of area, and fatigue resistance is an inevitable trend in improving my country's independent production capabilities for high-end equipment parts and effectively replacing imports.

[0003] In the global research and development and production of high-performance spring steel, industry giants such as Kobe Steel of Japan lead the way. my country's spring production is large and diverse, but its market share in high-end springs is small. This has long led to a passive structure in the Chinese spring industry, characterized by an oversupply of low-end, standard springs and a shortage of high-end products (those with high strength, high stress, special features, and specialized materials). Spring products no longer fully meet the needs of the high-end equipment manufacturing industry. Suspension springs, valve springs, and clutch springs for passenger cars, as well as high-end springs for locomotives, machinery, power generation, and military applications, still require imports. Furthermore, the performance of Chinese spring products currently lags behind that of similar foreign products, particularly in load accuracy and verticality. These differences manifest in unstable performance, high variability in some key quality indicators, and an uncertain service life. This discrepancy is particularly pronounced when the main engine requires the springs to operate under high-speed and high-stress conditions.

[0004] Spring steel is categorized by chemical composition into non-alloy spring steel (carbon spring steel) and alloy spring steel. Currently, springs used in various countries primarily consist of high-quality carbon steel with a carbon content of 0.3-0.9 wt.%, as well as alloy spring steels containing alloys such as Cr-Si, Cr-Mn, Si-Mn, and Cr-V. Carbon spring steel is primarily used in springs such as scroll springs and leaf springs, while most other springs, such as suspension springs and valve springs, are made of alloy spring steel. Si-Mn spring steel offers excellent resistance to elastic degradation and low production costs, making it the primary spring steel production system in my country. However, Si-Mn spring steel also has certain limitations, such as surface decarburization during heat treatment and insufficient hardenability, which have limited its development. Internationally, most countries use Cr-Mn and Cr-V alloy steels for spring steel production. This is because these alloy spring steels offer excellent hardenability during heat treatment and resist surface decarburization. Based on the above system, various countries are further developing spring steel with better performance. The main idea is to add alloying elements such as Mo, W, and V. The main purpose is to improve the hardenability of spring steel, refine the grains, and reduce the grain size, so as to achieve the purpose of improving the structure and performance of spring steel.

[0005] In recent years, with the high-quality development of the dual-carbon economy and equipment manufacturing industry, spring products need to achieve not only high mechanical properties and excellent fatigue performance, but also low production costs. Therefore, the main development directions of spring steel are: first, continue to develop the existing spring steel system, adopt different processes or add trace elements to further tap its potential; second, develop new spring steel systems. Developing new spring steel systems requires a lot of time and cost, so relatively few countries and regions have carried out research and development. Currently, the widely used springs such as SAE9254 and 54SiCrV6 are too low in strength, and the production cost of 54SiCrV6 is high; UHS2000 springs are higher in strength, but their cost is extremely high. In response to the pain points and difficulties in the industry, the present invention invents an ultra-high-strength spring steel containing manganese-aluminum-nitrogen microalloying, which has the advantages of high mechanical strength, large elongation, high cross-sectional reduction rate, and good fatigue resistance; at the same time, the preparation method of this ultra-high-strength spring steel is simple and easy, the production cost is low, and it is suitable for industrial production. Summary of the Invention

[0006] In response to the current problem of lack of high-strength spring steel products, the present invention provides an ultra-high-strength spring steel with the advantages of high mechanical strength, large elongation, high cross-sectional shrinkage and good fatigue resistance.

[0007] Another object of the present invention is to provide a method for preparing the above-mentioned ultra-high strength spring steel, which is simple, easy to implement and suitable for industrial production.

[0008] To achieve the above objectives, the present invention adopts the following technical solutions.

[0009] An ultra-high strength spring steel, belonging to a manganese-aluminum-nitrogen microalloyed spring steel, comprising the following chemical components in percentage by mass:

[0010] The main chemical composition is: C: 0.45-0.60%, Si: 0.15-0.35%, Mn: 6.0-12.0%, Al: 1.0-3.0%, Cr: 0.30-0.50%, Mo: 0.10-0.25%, V: 0.10-0.50%, Nb: 0.025-0.04%, N: 0.005-0.015%;

[0011] The chemical composition of impurities is: Pb≤0.03%, Sn≤0.03%, Zn≤0.03%, Sb≤0.03%, Bi≤0.03%, O2≤15ppm, H2≤15ppm; S≤0.02%, P≤0.02%, Cu≤0.2%, Ni≤0.35%;

[0012] The balance is iron and unavoidable impurities.

[0013] In the present invention, the addition amount and function of each chemical component are as follows:

[0014] Carbon (C) improves spring steel's elastic strength, hardness, and wear resistance through solid solution strengthening, but reduces its plasticity, toughness, and fatigue strength. Controlling C within a range of 0.45-0.60 wt.% and, when combined with other alloying elements, achieves an optimal combination of strength, fatigue life, and economic benefits. The present invention utilizes a lower C content than conventional spring steel. Within this range, it modifies the martensitic microstructure and improves the toughness of the spring steel.

[0015] Silicon (Si) strengthens ferrite through solid solution, improving the elasticity of steel. However, it weakens the steel's plasticity and toughness, significantly increases the tendency to decarburize and graphitize, creates inclusions, and deteriorates the fatigue performance of springs. Therefore, the present invention has found that controlling the silicon content within 0.15-0.35 wt.% minimizes the impact on fatigue strength. The Si content used in this invention is lower than that of conventional spring steel, which reduces carbon rejection and reduces decarburization.

[0016] Manganese (Mn) improves steel's strength and hardenability through solid solution, while also reducing carbon rejection and minimizing decarburization. The present invention utilizes a much higher Mn content than conventional spring steel to leverage its interaction with aluminum and nitrogen to enhance dislocation migration, thereby significantly increasing strength without compromising toughness. However, excessive Mn can promote temper brittleness, so the Mn content should be controlled within a range of 6.0-12.0 wt.%.

[0017] Aluminum (Al) refines the grain structure of steel, inhibits aging in low-carbon steel, reduces notch sensitivity, and particularly lowers the ductile-brittle transition temperature, improving steel's toughness at low temperatures. This invention introduces Al into spring steel for the first time, leveraging its affinity for nitrogen to deoxidize and nitrogenate, refine grains, and significantly improve strength, low-temperature toughness, and fatigue strength. However, excessive Al can affect the hot workability of steel. Experiments have determined that the optimal Al content should be between 1.0 and 3.0 wt.%.

[0018] Chromium (Cr) increases the strength of steel through solid solution, and can also improve the hardenability and tempering stability of steel, which is beneficial to improving the performance and dispersion precipitation of spring steel. However, the Cr content used in the present invention is much lower than that of conventional spring steel. The purpose is to prevent excessive chromium from easily forming chromium carbide and reducing the plasticity and toughness of the steel. Therefore, the Cr content is controlled at 0.30-0.50wt.%.

[0019] Molybdenum (Mo) improves the strength of steel through solid solution, strongly improves the hardenability of steel, stabilizes carbon elements, and is beneficial to improving the strength of spring steel. However, excessive Mo will change the quenching curve of steel, tending to the formation of feathery bainite, which is not conducive to the fatigue strength of spring steel. Therefore, the Mo content needs to be controlled at 0.10-0.25wt.%.

[0020] Vanadium (V) and niobium (Nb) form dispersed, fine vanadium carbide (VC), niobium carbide (NbC), vanadium nitride (VN), or niobium nitride (NbN) in steel, which dramatically strengthens the matrix while refining grain boundaries and preventing grain growth. This results in a dense, high-strength structure, significantly improving the strength and fatigue properties of spring steel. However, excessive amounts of either element can lead to particle coarsening and loss of their excellent properties. Therefore, the present invention utilizes the combined functions of the two elements, and after optimization, the optimal content is 0.10-0.50wt.% for V and 0.025-0.04wt.% for Nb.

[0021] Cr, Mo, V and Nb are precious elements and are used in very small amounts in the present invention to reduce production costs.

[0022] Nitrogen (N) plays a similar role in steel as carbon. It can improve the elasticity, strength and hardness of steel through stronger solid solution strengthening, but it weakens the plasticity, toughness and fatigue strength of spring steel less than carbon. In particular, the martensite formed has an Fe-CN structure and has higher fatigue strength. Microalloyed spring steel with nitrogen addition can have higher strength, toughness and fatigue life. The optimal N content determined by the present invention is 50-150ppm.

[0023] Sulfur (S) or phosphorus (P) forms inclusions with alloying elements, such as MnS, which not only offsets the beneficial effects of the alloying elements, but also causes S and P to segregate, weakening the toughness of the steel and becoming a source of fatigue cracks, seriously reducing the fatigue strength of the spring. Therefore, the S and P content in spring steel should be strictly controlled within 0.02wt.%.

[0024] Copper (Cu) will seriously reduce the thermoplasticity of the material. Since the spring will undergo subsequent hot processing, a high Cu content is prone to microcracks, which seriously affects the strength of the spring. Therefore, the Cu content should be strictly controlled to ≤0.2wt.%.

[0025] Nickel (Ni) can improve the strength and toughness of steel, lower the brittle transition temperature, and especially improve hardenability. However, nickel is extremely expensive, so other alloys are used as much as possible to meet performance requirements. Within the content range of other elements, the present invention can meet the strength and toughness requirements without the need for additional Ni addition. The Ni content of the raw materials is ≤0.35wt.% mainly due to the inevitable introduction of Ni into the raw materials.

[0026] The method for preparing the ultra-high strength spring steel comprises the following steps:

[0027] The spring steel raw materials are sequentially smelted, refined, RH vacuum degassed, continuously cast into steel ingots, the steel ingots are peeled, continuously hot rolled, and controlled cooling is performed to obtain ultra-high strength spring steel.

[0028] In order to reduce costs, the above-mentioned spring steel raw materials can use some scrap steel, but scrap steel contains impurities such as copper. Therefore, the amount of scrap steel needs to be controlled within 20% of the total mass of the spring steel raw materials.

[0029] Specifically, the ultra-high-strength spring steel production process involves feeding raw materials into a converter and controlling the percentage of scrap steel in the raw materials. To control impurity levels, electromagnetic stirring and RH vacuum degassing are used throughout the secondary refining process, resulting in a uniform fiber structure with fewer bubbles and pores and a denser structure. After vacuum degassing, continuous casting is performed to form a stable macrostructure, followed by continuous heating and rolling to ensure uniform dimensional structure. Controlled cooling temperature reduces the decarburization layer and ensures shear hardness. After cooling to room temperature, the steel is obtained.

[0030] Furthermore, the optimized process parameters in the above process are as follows:

[0031] The smelting temperature is 1630-1700°C for 25-60 minutes. The refining temperature is 1500-1550°C for 20-60 minutes. In order to homogenize the microstructure and prevent the segregation of alloy elements, electromagnetic stirring is used in the refining process.

[0032] The parameters of RH vacuum degassing are: vacuum degree ≤ 130Pa, time is 20-60 minutes.

[0033] The rolling reduction ratio of the continuous casting ingot to the spring steel size is greater than 15:1. The continuous casting cooling process requires cooling at a rate of 25-35°C / min to below 1150°C, followed by natural cooling to room temperature. This minimizes inclusions from forming on the ingot's centerline, minimizing the impact on product performance after rolling.

[0034] The depth of ingot peeling is not less than 3.0mm.

[0035] The starting rolling temperature of continuous hot rolling is 900℃-1000℃, and the finishing rolling temperature is 780℃-900℃. Continuous hot rolling needs to be carried out in the austenite region to maximize the material's deformation properties and provide favorable conditions for subsequent cooling.

[0036] The specific steps of controlled cooling are: rapid cooling to 600°C at a rate of no less than 30°C / min, followed by slow cooling to room temperature at a rate of no more than 10°C / min. This prevents surface decarburization and maintains a low hardness to facilitate subsequent shearing.

[0037] The ultra-high strength spring steel obtained by the above preparation method has a hardness of ≤HB350, a semi-decarburized layer of ≤0.20 mm, and no fully decarburized layer.

[0038] To further enhance the performance of spring steel, after processing and forming, the finished product requires heat treatment. This process involves oil quenching at a temperature of 840-890°C (1.0-1.3 min / mm) and a holding time of 1.0-1.3 min / mm. Tempering is performed at a temperature of 380-500°C. After this heat treatment, metallographic examination revealed that the spring steel's microstructure consists of >95% troostite and a small amount of ferrite, with no other structures present.

[0039] After heat treatment, the finished product has a tensile strength of more than 2000MPa, a yield strength of more than 1850MPa, an elongation of ≥7%, a cross-sectional shrinkage of ≥25%, a fatigue cycle of more than 350,000 cycles, and a grain size greater than ASTM grade 9.0.

[0040] The ultra-high strength spring steel obtained by the above preparation method has an application thickness of 6-50 mm or an application diameter of 6-35 mm.

[0041] The present invention has the following advantages:

[0042] The spring steel provided by this invention has high mechanical strength, large elongation, high cross-sectional reduction, and excellent fatigue resistance, making it suitable for use in demanding industries such as equipment manufacturing. Its cost is lower than that of currently commercially available spring steel. The preparation method provided by this invention is scientific, rational, simple, and suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 is a metallographic diagram of spring steel that has not been heat treated;

[0044] FIG2 is a metallographic diagram of Example 1;

[0045] FIG3 is a metallographic diagram of Example 2;

[0046] FIG4 is a metallographic diagram of Example 3. DETAILED DESCRIPTION

[0047] The present invention will be further described below with reference to the following examples and accompanying drawings, but the present invention is not limited by the following examples. Unless otherwise specified, all raw materials used in the examples are commercially available.

[0048] Example 1 Preparation of ultra-high strength spring steel

[0049] The chemical composition weight percentage of the steel in this embodiment is shown in Table 1.

[0050] Ultra-high strength spring steel is produced by the following steps:

[0051] The molten iron was added to a 25-ton induction heating furnace and smelted at 1680°C. After 45 minutes, the steel was tapped and 18.0wt.% scrap steel was added to adjust the temperature to 1600°C. The steel was then transferred to a refining furnace. Under electromagnetic stirring, alloy materials such as ferrosilicon, ferromanganese, ferrochromium-molybdenum, ferrovanadium, ferroniobium and manganese nitride were added. Pure aluminum wire was fed at 1535±15°C and the chemical composition was adjusted for 40 minutes before RH vacuum degassing (vacuum degree ≤ 130Pa) was performed. The steel was then continuously cast into 200×200 mm ingots, cooled to 1150°C at a rate of 28°C / min, and then air-cooled to room temperature. The ingots were then peeled to a depth of 3.2 mm, then reheated to 1150°C and continuously rolled into 24×89 mm spring strip steel. The rolling temperature was set at 1050°C and the final rolling temperature was 860°C. After rolling, the steel was rapidly cooled to 600°C at a rate of 37°C / min, followed by slow cooling to room temperature at 8°C / min. The 24×89 mm strip steel produced by the above method had its chemical composition shown in Table 1. The metallographic diagram is shown in Figure 1. The microstructure of the unheat-treated spring steel is primarily pearlite and ferrite.

[0052] The steel strip obtained in Example 1 was further processed into a single leaf spring. After being held at 880°C for 20 minutes, the spring was oil-quenched and tempered at 460°C for 45 minutes to obtain a leaf spring product. Samples were taken from the leaf spring product obtained in Example 1 and metallographic specimens were prepared. The metallographic structure is shown in Figure 2. Figure 2 shows that the microstructure of the spring steel prepared in Example 1 contains a uniform sorbite structure and a small amount of ferrite, with the sorbite structure exceeding 95%. Compared with Figure 1, the microstructure of the spring steel obtained in Example 1 is significantly improved. Furthermore, the prepared leaf spring product was subjected to tensile specimen processing and tensile testing in accordance with GB / T228-2002, and the yield strength, elongation, and reduction of area were measured. The assembled leaf spring was then fatigue tested in accordance with GB / T228-2002. The test results are shown in Table 2, showing a tensile strength of 2193 MPa.

[0053] Example 2 Preparation of ultra-high strength spring steel

[0054] The chemical composition weight percentage of the steel in this embodiment is shown in Table 1.

[0055] Ultra-high strength spring steel is produced by the following steps:

[0056] Molten iron was added to a 60-ton converter and smelted at 1630°C. After 60 minutes, the steel was tapped and 15.0% scrap steel was added to adjust the temperature to 1650°C before being transferred to a refining furnace. Under electromagnetic stirring, alloying materials such as ferrosilicon, ferromanganese, ferrochromium-molybdenum, ferrovanadium, ferroniobium, and manganese nitride were added. The chemical composition was adjusted at 1515±15°C for 60 minutes, followed by vacuum degassing (under vacuum conditions of ≤130Pa). The steel was then continuously cast into 200×200mm ingots, cooled to 1150°C at a rate of 30°C / min, and then air-cooled to room temperature. The ingots were then peeled to a depth of 3.5mm, reheated to 1200°C, and finally continuously rolled into 24×89mm spring strip steel with a starting rolling temperature of 950°C and a finishing rolling temperature of 850°C. After rolling, the steel was rapidly cooled to 600°C at a rate of 35°C / min, and then slowly cooled to room temperature at a rate of 10°C / min. According to the above method, 24×89 mm strip steel was produced, and its chemical composition was shown in Table 1.

[0057] The steel strip obtained in Example 2 was further processed into a single leaf spring. After being held at 850°C for 20 minutes, the spring was oil-quenched and tempered at 480°C for 45 minutes to obtain a leaf spring product. Samples were taken from the leaf spring product obtained in Example 2, and metallographic specimens were prepared. The metallographic structure is shown in Figure 3. Figure 3 shows that the microstructure of the spring steel prepared in Example 2 contains a uniform sorbite structure and a small amount of ferrite, with the sorbite structure exceeding 95%. Compared with Figure 1, the microstructure of the spring steel obtained in Example 2 was significantly improved. Furthermore, tensile specimens were processed and tested in accordance with GB / T 228-2002, and yield strength, elongation, and reduction of area were measured. The assembled leaf springs were then fatigue tested in accordance with GB / T 228-2002. The test results are shown in Table 2, showing a tensile strength of 2183 MPa.

[0058] Example 3 Preparation of ultra-high strength spring steel

[0059] The chemical composition weight percentage of the steel in this embodiment is shown in Table 1.

[0060] Ultra-high strength spring steel is produced by the following steps:

[0061] Molten iron was added to a 120-ton converter and smelted at 1700°C. After 25 minutes, the steel was tapped and 16% scrap steel was added to adjust the temperature to 1650°C before being transferred to a refining furnace. Under electromagnetic stirring, alloy materials such as ferrosilicon, ferromanganese, ferrochromium-molybdenum, ferrovanadium, ferroniobium and manganese nitride were added. After adjusting the chemical composition at 1535±15°C for 30 minutes, vacuum degassing was carried out (under vacuum conditions of ≤130Pa). Subsequently, the steel was continuously cast into 200×200mm ingots, cooled to 1150°C at a rate of 35°C / min, and then air-cooled to room temperature. The ingots were then peeled to a depth of 3.0mm and then heated to 1200°C. Finally, the steel was continuously rolled into 24×89mm spring strips with a starting rolling temperature of 900°C and a finishing rolling temperature of 900°C. After rolling, the steel was rapidly cooled to 600°C at a rate of 40°C / min and then slowly cooled to room temperature at a rate of 9°C / min. According to the above method, 24×89 mm strip steel was produced, and its chemical composition was shown in Table 1.

[0062] The steel strip obtained in Example 3 was further processed into a single leaf spring. After being held at 900°C for 20 minutes, the spring was oil-quenched and tempered at 500°C for 45 minutes to obtain a leaf spring product. Samples were taken from the leaf spring product obtained in Example 3, and metallographic specimens were prepared. The metallographic structure is shown in Figure 4. Figure 4 shows that the microstructure of the spring steel prepared in Example 3 contains a uniform sorbite structure and a small amount of ferrite, with the sorbite structure exceeding 95%. Compared with Figure 1, the microstructure of the spring steel obtained in Example 3 is significantly improved. Furthermore, tensile specimens were processed and tested in accordance with GB / T 228-2002, and yield strength, elongation, and reduction of area were measured. The assembled leaf springs were then fatigue tested in accordance with GB / T 228-2002. The test results are shown in Table 2, showing a tensile strength of 2156 MPa.

[0063] Comparative Example

[0064] Table 1 lists the chemical compositions of three commonly used spring steels: standard steel SAE9260, standard steel SAE5160, and standard steel SAE6150. These three standard steels were then processed into single-leaf leaf springs according to the process described in Application Example 3. This involves holding at 900°C for 20 minutes, oil quenching, and tempering at 500°C for 45 minutes to produce leaf spring products. Tensile specimens were processed and tested according to GB / T228-2002, and yield strength, elongation, and reduction of area were measured. The assembled leaf springs were then fatigue tested according to GB / T228-2002. The test results are shown in Table 2.

[0065] Table 1 Comparison of chemical composition of different steels (wt.%)

[0066]

[0067] Table 2 Performance test results of different finished products

[0068]

[0069] From the results in Table 2, it can be seen that, while maintaining the same levels of plasticity, toughness, cross-sectional reduction rate Z, and elongation A, the strength of the leaf spring products of the spring steel prepared in Examples 1 to 3 is greatly improved; compared with the standard steel 9260, the yield strength (Rp 0.2 ) is increased by up to approximately 1.05 times, the tensile strength (Rm) is increased by up to approximately 1.02 times, and the fatigue strength is increased by more than 4 times. Therefore, the ultra-high-strength spring steel of this invention is particularly suitable for the production of lightweight leaf springs.

Claims

1. [Corrected 15.01.2024 in accordance with Rule 91] An ultra-high strength (2 GPa) spring steel, characterized in that: The chemical composition includes the following mass ratios: The main chemical components are: C: 0.45-0.60%, Si: 0.15-0.35%, Mn: 6.0-12.0%, Al: 1.0-3.0%, Cr: 0.30-0.50%, Mo: 0.10-0.25%, V: 0.10-0.50%, Nb: 0.025-0.04%, N: 0.005-0.015%; Controlled impurity chemical composition: Pb≤0.03%, Sn≤0.03%, Zn≤0.03%, Sb≤0.03%, Bi≤0.03%, O2≤15ppm, H2≤15ppm; S≤0.02%, P≤0.02%, Cu≤0.2%, Ni≤0.35%; The balance is iron and unavoidable impurities.

2. A method for preparing the ultra-high strength (2 GPa) spring steel as claimed in claim 1, characterized in that: The following steps are involved: The spring steel raw materials are sequentially smelted, refined, RH vacuum degassed, continuously cast into steel ingots, the steel ingots are peeled, continuously hot rolled, and controlled cooled to obtain ultra-high strength spring steel.

3. The preparation method according to claim 2, characterized in that: The smelting temperature is 1630-1700°C, and the time is 25-60 minutes; the refining temperature is 1500-1550°C, and the time is 20-60 minutes; The vacuum degree of RH vacuum degassing is ≤130Pa; the vacuum time is 20-60 minutes.

4. The preparation method according to claim 2, characterized in that: Electromagnetic stirring is used in the refining process.

5. The preparation method according to claim 2, characterized in that: The cooling process of continuous casting is to first cool down to below 1150℃ at 25℃-35℃ / min, and then cool naturally to room temperature; The specific steps of controlled cooling are: rapidly cooling to 600°C at a speed of not less than 30°C / min, and then slowly cooling to room temperature at a speed of not more than 10°C / min; The starting temperature of hot rolling is 900-1000℃, and the final rolling temperature is 780-900℃.

6. The preparation method according to claim 2, characterized in that: The peeling depth of the steel ingot is at least 3.0 mm; and the compression ratio of continuous hot rolling is greater than 15:

1.

7. The preparation method according to any one of claims 2 to 6, characterized in that: The hardness of the obtained spring steel is ≤HB350, the semi-decarburized layer is less than or equal to 0.20 mm, and there is no full decarburized layer.

8. The preparation method according to claim 2, characterized in that: It also includes heat treatment; the heat treatment method is quenching + tempering; the quenching method is oil quenching, the quenching temperature is 840-890℃, and the holding time is 1.0-1.3min / mm; the tempering temperature is 380℃-500℃.

9. The preparation method according to claim 8, characterized in that: The microstructure of the obtained spring steel is >95% troostite and a small amount of ferrite, and only troostite and ferrite, without other tissues; The obtained spring steel has a tensile strength of ≥2000MPa, a yield strength of ≥1850MPa, an elongation of ≥7%, a cross-sectional shrinkage of ≥25%, a fatigue cycle of more than 350000; and a grain size greater than ASTM grade 9.

0.

10. The preparation method according to claim 8, characterized in that: The obtained spring steel has an application thickness of 6-50 mm and an application diameter of 6-35 mm.

Citation Information

Patent Citations

  • High-strength stainless steel wire having excellent heat deformation resistance, high-strength spring, and method for manufacturing same

    CN104136645A

  • Valve spring stainless steel and steel wire preparation method thereof

    CN110607479A

  • Steel wire rod for deep drawing of cold-drawn spring steel wire and preparation method thereof

    CN111197140A

  • High-stress spring steel and preparation process thereof

    CN111705261A

  • Preparation method of 17-7PH stainless steel spring steel wire and steel wire

    CN115710678A