Micro-led chip, and preparation method therefor and application thereof

By integrating the metasurface conductive structural layer on the light-extrusion surface of the Micro-LED chip, the problems of large light divergence angle and low luminous efficiency are solved, and efficient and low-cost light extraction and full-color display are achieved, which is suitable for high-resolution display needs.

WO2024239403A1PCT designated stage expired Publication Date: 2024-11-28SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI

Patent Information

Application Number
PCT/CN2023/101034
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2023-06-19
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing Micro-LED chips have problems such as large light divergence angle, low luminous efficiency, complex color display technology and high cost, especially in high-resolution display applications.

Method used

The metasurface conductive structure layer is integrated on the light-exit surface of the Micro-LED chip. Through the metasurface structure composed of metal or non-metal conductive layer and specific pattern structure, the light exit angle and wavelength are regulated, thereby improving the light extraction efficiency and collimation. , and realizes simple and low-cost technology for full color display.

Benefits of technology

It significantly improves the light extraction efficiency and collimation of Micro-LED chips, reduces production costs and process difficulty, is suitable for ultra-high resolution display applications, and achieves efficient full-color display effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023101034_28112024_PF_FP_ABST
    Figure CN2023101034_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present application are a Micro-LED chip, and a preparation method therefor and an application thereof. The Micro-LED chip comprises an LED chip structure and a first metasurface conductive structure layer, the first metasurface conductive structure layer comprising: a first conductive layer, which is electrically bonded to a light emergent surface of the LED chip structure; and a metasurface structure, which is arranged, in a stacked manner and / or an integrated manner, with the first conductive layer, wherein the metasurface structure is at least used for adjusting and controlling an emergent angle or wavelength of light emitted from the light emergent surface. On the basis of the technical solution of the present application, full-color of a Micro-LED chip can be realized, the light emergent rate and the collimation can be increased, and the preparation of the Micro-LED chip and the integration of a Micro-LED pixel and a display unit can be realized by using a large-scale standard semiconductor process, thereby improving the production efficiency and yield of the Micro-LED chip and reducing the cost.
Need to check novelty before this filing date? Find Prior Art

Description

Micro-LED chip and its preparation method and application

[0001] This application is based on and claims priority from the Chinese patent application number 2023105800924 filed on May 22, 2023, entitled “Micro-LED Chip, Preparation Method and Application Thereof”. Technical Field

[0002] The present application relates to a semiconductor optoelectronic device, specifically to a Micro-LED chip and its preparation method and application, belonging to the field of semiconductor optoelectronic technology. Background Art

[0003] Micro-LEDs (micro light-emitting diodes) offer exceptional performance in brightness, contrast, luminous efficiency, resolution, response speed, energy consumption, impact resistance, operating temperature, and lifespan. They are an indispensable technology for the next generation of displays, boasting broad applications in ultra-high-definition large-screen displays, microdisplays, flexible displays, head-mounted displays, and augmented and virtual reality. Among current display applications, LED-based display technology holds a significant position in our lives. Among these, the novel gallium nitride (GaN) Micro-LED display technology holds the greatest potential and is poised to gradually replace other display technologies, ultimately becoming the mainstream technology in the display field.

[0004] The light emission characteristic of the active region of a GaN LED is isotropic, emitting light in all directions with a wide divergence angle. Consequently, very little light actually reaches the emission window, severely impacting the LED's effective luminous efficiency. The most common display applications require a wider viewing angle, as well as improved light saturation and contrast. Furthermore, industrial exposure and image projection applications are limited by the numerical aperture of projection lenses. Consequently, the light emitted by Micro-LED devices and their arrays must exhibit a smaller divergence angle, higher light extraction efficiency, and higher luminous quality.

[0005] At present, the main solutions for improving the light output efficiency and direction of Micro-LEDs include resonant cavity structures and lens systems. The resonant cavity structure is to prepare two reflective structures at the bottom and top of the Micro-LED active area. By forming a microcavity structure, the light emitted by the active area is reflected back and forth under the action of the resonant cavity, achieving constructive interference, thereby enhancing the output efficiency and collimation of the light emitted by the active area, and achieving enhanced optical characteristics of the device. However, this solution is complex and the bottom preparation process is difficult. The Micro-LED material needs to be removed from the original substrate before the bottom reflective layer can be added. It is only suitable for Micro-LED device structures with a peeling structure. The lens system mainly changes the optical path of the emitted light through specific microlenses to improve the collimation of the device's light emission. However, its preparation is difficult and generally requires complex photolithography, etching and other processes before a lens system can be added on top of the Micro-LED. In addition, the lens system is large in size, not suitable for lightweight applications, and the cost is also high.

[0006] On the other hand, color-enhancing micro-LED displays often require wavelength conversion of monochromatic micro-LEDs. Common solutions currently include mass transfer and quantum dot film color conversion. Mass transfer technology involves placing different-color micro-LED units onto a single substrate using methods such as mechanical transfer. Due to the extremely high pixel density and the large amount of transfer required, specialized, large-scale equipment is typically required. Furthermore, the transfer process requires extremely high precision control of the adsorption and placement of micro-LED pixels, and the success rate of adsorption during the transfer process directly impacts product yield. Furthermore, the pixel pitch after transfer and placement is relatively large, making it unsuitable for ultra-high-resolution display applications. Quantum dot color conversion technology typically uses quantum dot films, such as zinc sulfide, cadmium selenide, and perovskite, to convert the blue light emitted by conventional GaN micro-LEDs into green and red light, achieving color conversion. However, existing quantum dot technology is not yet mature, and controlling the uniformity of quantum dots is difficult. Variation in the size of the dots can affect color purity and color quality. At the same time, existing quantum dots generally cannot withstand high temperatures, so they must be properly insulated from the Micro-LED chip. Ensuring color uniformity during the spraying process and avoiding interference between quantum dots of different colors also require further solutions. Furthermore, quantum dots are produced using chemical methods, which are not environmentally friendly.

[0007] Application Contents

[0008] The main purpose of this application is to provide a Micro-LED chip and its preparation method and application to overcome the shortcomings of the existing technology.

[0009] To achieve the aforementioned application objectives, the technical solutions adopted in this application include:

[0010] One aspect of the present application provides a Micro-LED chip, comprising an LED chip structure and a first supersurface conductive structure layer, wherein the first supersurface conductive structure layer comprises:

[0011] A first conductive layer electrically coupled to the light emitting surface of the LED chip structure;

[0012] The metasurface structure is stacked and / or integrated with the first conductive layer and is at least used to regulate the emission angle and / or wavelength of light emitted from the light-emitting surface.

[0013] Another aspect of the present application provides a method for manufacturing the Micro-LED chip, comprising:

[0014] Making LED chip structure;

[0015] A first conductive layer and a super-surface structure are arranged on the light-emitting surface of the LED chip structure, and the super-surface structure and the first conductive layer are stacked and / or integrally arranged.

[0016] Another aspect of the present application provides a use of the Micro-LED chip in preparing optoelectronic devices, including but not limited to display devices, microdisplay devices, etc.

[0017] Compared with the existing technology, this application integrates a metasurface structure in the Micro-LED chip, which can not only give full play to the excellent performance of GaN-based Micro-LED, but also realize the full color of Micro-LED in a simple and low-cost manner, and significantly increase its light output and collimation. At the same time, the preparation of Micro-LED chips and the integration of Micro-LED pixels and display units can be achieved through large-scale standard semiconductor process technology, effectively improving the production efficiency and yield of Micro-LED chips, greatly reducing their costs, and promoting the development and application of Micro-LED display fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The drawings in the specification, which constitute a part of this application, are used to provide further understanding of this application. The illustrative embodiments of this application and their descriptions are used to explain this application and do not constitute improper limitations on this application.

[0019] FIG1 is a schematic structural diagram of a Micro-LED chip in Example 1;

[0020] FIG2 is a schematic diagram of a first supersurface conductive structure layer in Example 1;

[0021] FIG3 is a schematic structural diagram of an epitaxial wafer of a Micro-LED chip in Example 1;

[0022] FIG4 is a schematic diagram of a first supersurface conductive structure layer in Example 4;

[0023] FIG5 is a schematic diagram of a first supersurface conductive structure layer in Example 8;

[0024] FIG6 is a schematic structural diagram of a Micro-LED chip in Example 10;

[0025] FIG7 is a schematic diagram of a first supersurface conductive structure layer in Example 11;

[0026] FIG8 is a schematic diagram of a third metasurface structure in Example 12;

[0027] FIG9 is a schematic structural diagram of a Micro-LED chip in Example 13;

[0028] FIG10 is a partial enlarged schematic diagram of area A in FIG9 ;

[0029] FIG11 is a test diagram of the reflectivity of a heat-conducting medium layer for light of different wavelengths in Example 12. DETAILED DESCRIPTION

[0030] This application integrates a metasurface structure into a Micro-LED chip, specifically a conductive metasurface structure on the light-emitting surface of the Micro-LED chip, to optimize the light emission angle, improve light extraction efficiency, and reduce the difficulty and cost of colorization. The technical solution of this application is further described below.

[0031] In this specification, the metasurface structure is a two-dimensional plane graphic composed of materials with special electromagnetic properties arranged in a certain way. It is mainly composed of sub-wavelength nanometer-sized microstructure units, which can achieve flexible control of the amplitude, phase, polarization, etc. of the incident light.

[0032] Some embodiments of the present application provide a Micro-LED chip including an LED chip structure and a first super-surface conductive structure layer, wherein the first super-surface conductive structure layer includes:

[0033] A first conductive layer electrically coupled to the light emitting surface of the LED chip structure;

[0034] A metasurface structure is stacked and / or integrally arranged with the first conductive layer and is at least used to regulate the emission angle and / or wavelength of light emitted from the light-emitting surface, thereby achieving at least one or more of the following effects, including: optimizing the collimation of light emitted by the Micro-LED chip, improving the light extraction efficiency of the Micro-LED chip, and changing the color of the light emitted by the Micro-LED chip.

[0035] In one embodiment, the supersurface structure includes a first supersurface structure, the first conductive layer includes a plurality of first graphic structures, the plurality of first graphic structures are distributed along a direction parallel to the light-emitting surface, and form the first supersurface structure; wherein, the first conductive layer includes a metal conductive layer or a non-metallic conductive layer.

[0036] Furthermore, the thickness of the metal conductive layer can be less than 20 nm and have the first metasurface structure. This first metasurface structure can not only improve the light transmittance of the metal conductive layer and enhance the ability to control the emission angle and / or wavelength of light, but also form an array electrode. For example, the thickness of the metal conductive layer can be 0.1, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 nm to provide good light transmittance.

[0037] Furthermore, the thickness of the metal conductive layer can be greater than 20nm and have the first metasurface structure, so that on the one hand the metal conductive layer has better current expansion capability, and on the other hand the first metasurface structure is used to maintain good light transmittance, while allowing the first metasurface structure to give full play to its performance of regulating the output angle and / or wavelength of light, thereby improving at least one of the light output efficiency, collimation and full colorization of the Micro-LED chip. In addition, array electrodes can be formed, and each array electrode corresponds to a corresponding light-emitting pixel point, which is conducive to the precise control of the light field of each pixel unit.

[0038] In particular, when the first conductive layer is a metal layer and the first patterned structures have nanoscale dimensions, they also exhibit a strong light-field localized surface plasmon resonance effect as metal nanostructures. When light emitted by the LED chip structure enters the first conductive layer and the frequency of the light matches the vibration frequency of the metal nanostructure's conduction electrons, the first patterned structures strongly absorb the photon energy, exhibiting a strong resonant absorption peak in the spectrum. Furthermore, when multiple first patterned structures form the first metasurface structure, due to the plasmon resonance effect of the metal nanostructures and the relatively compact arrangement of these metal nanostructures, mutual coupling occurs between the nanostructures, increasing the overall resonance intensity and ultimately improving the color rendering efficiency of the Micro-LED chip.

[0039] In one embodiment, the first conductive layer includes a metal conductive layer or a non-metal conductive layer; the metal conductive layer has a thickness of less than 20 nm and extends continuously in a direction parallel to the light emitting surface.

[0040] Furthermore, the material of the metal conductive layer includes any one or more combinations of indium, tin, silver, platinum, gold, titanium, aluminum, nickel, chromium, molybdenum and copper, but is not limited thereto.

[0041] In one embodiment, the material of the non-metallic conductive layer includes ITO (indium tin oxide) or other transparent conductive materials, such as graphene, carbon nanotubes, conductive polymers, etc. or a combination thereof, but is not limited thereto.

[0042] In one embodiment, the thickness of the non-metallic conductive layer is 1 nm to 500 nm.

[0043] Furthermore, in a direction parallel to the light-emitting surface, the size of the first graphic structure is 0.1 nm to 1 μm, preferably 80 nm to 800 nm, and more preferably 100 nm to 600 nm.

[0044] Furthermore, the first graphic structure includes an X-shaped graphic structure and a variant Y-shaped graphic structure; in a specified direction parallel to the light-emitting surface, the variant Y-shape is a shape formed by rotating the Y-shape 90° clockwise; and the X-shaped graphic structure and the variant Y-shaped graphic structure are alternately arranged along the specified direction, and each X-shaped graphic structure and an adjacent Y-shaped graphic structure are spaced 1 to 500 nm apart and form a unit, and multiple units are arranged periodically, and the period in the specified direction and the direction perpendicular to the specified direction is 1 nm to 1 μm. Preferably, the X-shaped graphic structure and the Y-shaped graphic structure in a unit are spaced 10 to 100 nm apart, more preferably 30 to 50 nm. Preferably, the period is 50 to 500 nm, more preferably 100 to 300 nm. The size of the first graphic structure is particularly preferably 450 to 550 nm.

[0045] In some cases, the first metasurface structure may include multiple identical first graphic structures. The first metasurface structure may also be a non-periodic structure. However, it is preferred to use the aforementioned X-shaped graphic structure and variant Y-shaped graphic structure and periodic arrangement.

[0046] In one embodiment, the first supersurface conductive structure layer further includes a transparent dielectric layer stacked on the first conductive layer.

[0047] In one embodiment, the metasurface structure includes a second metasurface structure, the transparent medium layer includes a plurality of second graphic structures, and the plurality of second graphic structures are distributed along a direction parallel to the light emitting surface to form a second metasurface structure.

[0048] Furthermore, in a direction parallel to the light-emitting surface, a size of the second graphic structure is 1 nm to 1 μm, preferably 50 nm to 900 nm, and more preferably 50 nm to 500 nm.

[0049] In some cases, the second pattern structure includes a circular pattern structure with a modified F-shaped through-hole embedded in the center. In a specified direction parallel to the light-emitting surface, the modified F-shape is a shape formed by rotating the F-shape 30° clockwise. The size of the modified F-shape is 1 to 200 nm, preferably 10 to 100 nm, and more preferably 10 to 50 nm. Multiple circular pattern structures are arranged periodically, and the period in the specified direction and the direction perpendicular to the specified direction is 1 nm to 1 μm, preferably 5 to 300 nm, and more preferably 10 to 100 nm. Particularly preferably, the diameter of the circular pattern structure is 50 to 150 nm.

[0050] Alternatively, in some cases, the second graphic structure includes a variant K-shaped graphic structure and a variant L-shaped graphic structure. In a specified direction parallel to the light-emitting surface, the variant K-shape is a shape formed by rotating the K-shape 45° counterclockwise, and the variant L-shape is a shape formed by mirror-inverting the L-shape. The variant K-shaped graphic structures and the variant L-shaped graphic structures are alternately arranged along the specified direction. Each variant K-shaped graphic structure and an adjacent variant L-shaped graphic structure are separated by 1 to 200 nm (preferably 10 to 100 nm, more preferably 10 to 50 nm) to form a unit. Multiple units are periodically arranged, and the period in the specified direction and the direction perpendicular to the specified direction is 1 to 500 nm, preferably 50 to 200 nm, and more preferably 100 to 200 nm. Particularly preferably, the size of the variant K-shaped graphic structure and the variant L-shaped graphic structure is 50 to 150 nm.

[0051] Alternatively, in some cases, the second graphic structure includes a regular hexagonal graphic structure with an H-shaped through hole embedded in the center, the size of the H-shaped through hole is 1 to 200 nm, preferably 10 to 100 nm, and more preferably 10 to 50 nm. In a specified direction parallel to the light-emitting surface, every two adjacent regular hexagonal graphic structures are separated by 1 to 200 nm (preferably 10 to 100 nm, more preferably 50 to 100 nm) and form a unit. Multiple units are arranged periodically, and the period in the specified direction and the direction perpendicular to the specified direction is 1 to 1000 nm, preferably 50 to 500 nm, and particularly preferably 100 to 200 nm. Particularly preferably, the diameter of the regular hexagonal graphic structure is 50 to 100 nm.

[0052] Alternatively, in some cases, the second graphic structure includes an elliptical graphic structure, the major axis of the ellipse is 1 to 1000 nm (preferably 50 to 500 nm, more preferably 100 to 200 nm) and is parallel to a specified direction on the light-emitting surface, the minor axis is 1 to 1000 nm (preferably 10 to 500 nm, more preferably 10 to 200 nm, and particularly preferably 50 to 100 nm), and a V-shaped through hole and an X-shaped through hole are respectively formed on both sides of the minor axis, and the sizes of the V-shaped and X-shaped are 1 to 500 nm (preferably 10 to 10 0nm, more preferably 10-50nm), the interval between the V-shaped through holes and the X-shaped through holes is 1-500nm (preferably 10-200nm, more preferably 30-80nm), every two adjacent elliptical graphic structures are spaced 1-500nm (preferably 10-200nm, more preferably 50-100nm) and constitute a unit, a plurality of the units are periodically arranged, and the period in the specified direction and the direction perpendicular to the specified direction is 1-1000nm, preferably 10-500nm, more preferably 100-200nm.

[0053] Alternatively, in some cases, the second graphic structure includes a variant Z-shaped graphic structure, a variant T-shaped graphic structure, a variant M-shaped graphic structure and a P-shaped graphic structure, the variant Z-shaped graphic structure and the variant T-shaped graphic structure are alternately arranged along a specified direction parallel to the light-emitting surface, the variant M-shaped graphic structure and the P-shaped graphic structure are also alternately arranged along the specified direction, the P-shaped graphic structure and the variant Z-shaped graphic structure are alternately arranged in a direction perpendicular to the specified direction, and the variant M-shaped graphic structure and the variant T-shaped graphic structure are alternately arranged in a direction perpendicular to the specified direction. Each variant Z-shaped pattern structure and an adjacent variant T-shaped pattern structure, a variant M-shaped pattern structure, and a P-shaped pattern structure form a unit. The spacing between any two pattern structures in each unit in the specified direction and the direction perpendicular to the specified direction is 1 to 200 nm (preferably 10 to 100 nm, more preferably 30 to 80 nm). Multiple units are arranged periodically, and the period in the specified direction and the direction perpendicular to the specified direction is 1 to 1000 nm, preferably 10 to 500 nm, and more preferably 100 to 300 nm. Particularly preferably, the size of the variant Z-shaped pattern structure, the variant T-shaped pattern structure, the variant M-shaped pattern structure, and the P-shaped pattern structure is 100 to 200 nm.

[0054] In some cases, the second metasurface structure may also be a non-periodic structure.

[0055] In one embodiment, the metasurface structure comprises:

[0056] a first metasurface structure formed in the first conductive layer and configured to adjust at least one of an emission angle and a wavelength of light emitted from the light-emitting surface;

[0057] The second metasurface structure is at least used to regulate the other of the emission angle and the wavelength of the light emitted from the light-emitting surface.

[0058] Exemplarily, in the first case, the first metasurface structure is used to control the emission angle of the light emitted from the light-emitting surface to improve the collimation of the light emitted by the Micro-LED chip; at the same time, the second metasurface structure is used to control the wavelength of the light emitted from the light-emitting surface, that is, to change the wavelength of the light emitted, thereby achieving a color-changing effect on the Micro-LED chip. Alternatively, it can also be the second case, that is, the first metasurface structure is used to control the wavelength of the light emitted from the light-emitting surface, and the second metasurface structure is used to control the emission angle of the light emitted from the light-emitting surface. Surprisingly, compared with the first case, in the second case, the structure of the Micro-LED chip can be simpler, and while forming wavelength color control and improving the emission brightness, it can increase the color gamut, have higher color saturation, and obtain a more uniform observation effect.

[0059] Furthermore, the material of the transparent medium layer includes any one or more of silicon oxide, silicon nitride, aluminum nitride, aluminum oxide, gallium oxide, titanium oxide, and hafnium oxide, but is not limited thereto.

[0060] Furthermore, the thickness of the transparent dielectric layer is 0.1 nm to 1 μm, preferably 20 nm to 600 nm, and more preferably 100 nm to 400 nm. In the first case, if the transparent dielectric layer of the preferred thickness is used, the brightness and color hue saturation of the Micro-LED chip will be higher, and the light uniformity will be better.

[0061] In one embodiment, the Micro-LED chip further includes a second super-surface conductive structure layer, the LED chip structure has a first surface and a second surface opposite to the first surface, the first surface is the light-emitting surface, and the second surface is electrically connected to the LED driving mechanism through a second conductive layer.

[0062] In one embodiment, the second surface of the LED chip structure is electrically connected to the LED driving mechanism through a second super-surface conductive structure layer. The second super-surface conductive structure layer includes the second conductive layer and a third super-surface structure. The third super-surface structure is arranged on a side surface of the second conductive layer close to the LED chip structure or on the second surface of the LED chip structure, and is at least used to reflect light emitted by the LED chip structure to the second super-surface conductive structure layer.

[0063] Furthermore, the third metasurface structure includes a plurality of third graphic structures distributed along a direction parallel to the second surface, and in the direction parallel to the second surface, the size of the third graphic structure is 1 nm to 1 μm, preferably 80 nm to 800 nm, and more preferably 150 nm to 650 nm.

[0064] Furthermore, the third graphic structure includes an equilateral triangle graphic structure and a variant equilateral triangle graphic structure, and the equilateral triangle graphic structure and the variant equilateral triangle graphic structure are alternately arranged along a specified direction parallel to the second surface, wherein the center of the equilateral triangle graphic structure is embedded with a variant X-shaped through hole, and the variant X-shape is the shape of the X-shape rotated 45° clockwise, and the center of the variant equilateral triangle graphic structure is embedded with a variant Z-shaped through hole, and the variant equilateral triangle is the shape of the equilateral triangle rotated 90° clockwise around a specified point, and the variant Z-shape is the shape of the Z-shape rotated 45° clockwise. The shape of the variant X-shape and the variant Z-shape has a line length of 1nm to 500nm, preferably 10 to 200nm, and more preferably 50 to 100nm; the midpoint of one side of each of the equilateral triangle graphic structures and a vertex of an adjacent variant equilateral triangle graphic structure intersect at the designated point and form a unit, and a plurality of the units are periodically arranged, and the period in the designated direction is 1nm to 1μm, preferably 50 to 500nm, and more preferably 100 to 500nm, and the period in the direction perpendicular to the designated direction is 1nm to 1μm, preferably 50 to 500nm, and more preferably 100 to 500nm.

[0065] Furthermore, the third metasurface structure comprises a plurality of third graphic structures that are the same or different, and the third metasurface structure is a periodic or non-periodic structure.

[0066] Furthermore, the LED driving mechanism may include but is not limited to a CMOS or TFT driving mechanism, etc., which may be integrated with a driving substrate, etc.

[0067] Furthermore, the second conductive layer may be made of a metal material, such as any one or more of indium, tin, silver, platinum, gold, titanium, aluminum, nickel, chromium, molybdenum, and copper, or a non-metallic material such as ITO, graphene, carbon nanotubes, or a conductive polymer, without limitation. Preferably, the second conductive layer is formed of a metal material having excellent thermal conductivity, electrical conductivity, and light reflectivity, such as aluminum, indium, tin, silver, or gold.

[0068] Furthermore, the thickness of the second conductive layer can be set according to actual needs, for example, it can be greater than 1nm, greater than 10nm, greater than 100nm, greater than 500nm or greater than 1μm, but it should not be too thick to avoid a significant increase in the overall thickness and cost of the Micro-LED chip.

[0069] In one embodiment, the LED chip structure includes a first doped semiconductor layer, an active layer, and a second doped semiconductor layer stacked in sequence along a set direction, and a surface of the first doped semiconductor layer or the second doped semiconductor layer away from the active layer is the light emitting surface.

[0070] In one embodiment, the first conductive layer forms an ohmic contact with the light-emitting surface of the LED chip structure, for example, forms an ohmic contact with the first doped semiconductor layer or the second doped semiconductor layer.

[0071] In one embodiment, the Micro-LED chip may include multiple LED chip structures, and the multiple LED chip structures are arranged in an array, that is, forming an LED chip array. Each LED chip structure can be used as a pixel, or multiple adjacent LED chip structures can be used as a pixel. Exemplarily, the multiple LED chip structures are divided into multiple groups, each group includes three blue light LED chip structures, and by respectively setting different first super-surface conductive structure layers on the three LED chip structures, the three pixel points corresponding to the three LED chip structures respectively present blue, red and green colors. Compared with the Micro-LED full-color display solution based on mass transfer technology and quantum dot thin film color conversion technology, the full-color display solution of the present application has many advantages such as simple structure, low cost, high yield, good process controllability, and environmental protection.

[0072] Furthermore, the Micro-LED chip may also include an optical isolation structure to better eliminate optical crosstalk between adjacent LED chip structures and improve the contrast and brightness of the Micro-LED chip. Taking the surface of the second doped semiconductor layer as the light-emitting surface as an example, the optical isolation structure may include an ion implantation region, an isolation groove, and a light-blocking structure distributed within the Micro-LED chip; the ion implantation region at least continuously extends from the top surface of the second doped semiconductor layer to the interior of the first doped semiconductor layer, and is used to electrically isolate any two adjacent LED chip structures from each other; the isolation groove is entirely located within the ion implantation region, the groove opening is provided on the top surface of the second doped semiconductor layer, and the bottom surface of the groove is located within the first doped semiconductor layer and is higher than the bottom surface of the ion implantation region; the light-blocking structure is provided within the isolation groove and is used to prevent light from being transmitted between any two adjacent LED chip structures through the second doped semiconductor layer and the active layer.

[0073] Among them, by adopting ion implantation isolation to realize LED chip array, and by opening isolation grooves in the ion implantation area and setting light-blocking structures in the isolation grooves, it is possible to better realize chip miniaturization, avoid chip sidewall damage and dangling bonds caused by the etching process, ensure and improve the quantum efficiency and effective use area of ​​the chip, and make it have better optical and electrical characteristics. At the same time, it can also effectively prevent light from being transmitted between adjacent chips in the LED chip array, eliminate optical crosstalk, and thus improve the contrast and brightness of the LED chip array and other display effects. By placing the isolation groove as a whole in the ion implantation area, on the one hand, it can further reduce the risk of damaging the semiconductor material due to over-etching during the process of making the isolation groove, and on the other hand, it can also use the ion implantation area to electrically isolate the conductive filling material in the isolation groove from the semiconductor material in the structural layers such as the second doped semiconductor layer and the active layer, thereby ensuring the normal operation performance of the device.

[0074] The implanted ions used to form the ion implantation area include H ions, F ions, N ions, or O ions, and are not limited thereto. Furthermore, the ion implantation area may be one or more. Exemplarily, on the surface of the Micro-LED chip, the ion implantation area may be in a grid-like shape, and the area surrounded by each grid is a non-ion implantation area for fabricating the LED chip structure. Accordingly, the isolation trench may also be one or more, and exemplarily, it may also be in a grid-like structure on the surface of the Micro-LED chip.

[0075] The ion implantation area may be arranged around the corresponding non-ion implantation area, and the corresponding non-ion implantation area is formed with an LED chip structure. The sizes of the ion implantation area and the LED chip structure may be determined according to actual needs. For example, the sizes of the ion implantation area and the LED chip structure are 1 μm to 50 μm. The sizes of the ion implantation area and the LED chip structure mainly refer to their sizes in the direction parallel to the layer plane of the LED chip structure, and can also be considered as their length and width or their diameter.

[0076] There is a certain distance between the inner wall of the isolation groove and the outer wall of the corresponding ion implantation region, that is, the ion implantation region has a certain wall thickness, which can be 100 nm to 20 μm, for example.

[0077] The Micro-LED chip may further include at least one thermally conductive medium layer, the thermally conductive medium layer continuously covering at least the sidewalls of the isolation groove and being located between the sidewalls of the isolation groove and the light-blocking structure; and the light-blocking structure may include a metal light-isolating layer continuously covering at least the sidewalls of the isolation groove. By providing the thermally conductive medium layer, on the one hand, the sidewalls of the isolation groove can be protected, and on the other hand, the conductive filling material in the isolation groove can be further electrically isolated from the semiconductor materials in the second doped semiconductor layer and the active layer and other structural layers. Furthermore, by utilizing the thermally conductive medium layer, when the metal light-isolating layer is manufactured by processes such as evaporation, the escape of ions from the ion-implanted area can be prevented, thereby better ensuring the performance of the device.

[0078] The material of the thermal conductive medium layer includes, but is not limited to, silicon oxide, silicon nitride, aluminum nitride, aluminum oxide, gallium oxide, titanium oxide, or hafnium oxide. The thickness of the thermal conductive medium layer may be 5 nm to 500 nm.

[0079] Preferably, the Micro-LED chip includes multiple thermally conductive medium layers with different refractive indices, and the multiple thermally conductive medium layers are stacked at least sequentially on the sidewalls of the isolation trench and combined with the ion implantation region to form a distributed Bragg reflector structure (DBR). The definition of the distributed Bragg reflector structure is well known in the art, and is mainly an optical film composed of a low refractive index material and a high refractive index material through different stacking combinations. Exemplarily, the low refractive index material can be selected from but not limited to SiO2, and the high refractive index material can be selected from but not limited to TiO2, Ta2O5, ZrO2, etc. The greater the refractive index difference between the materials, the smaller the thickness required to achieve the desired reflectivity.

[0080] Specifically, after ion implantation forms an ion implantation zone in a selected area of ​​the LED chip structure, the refractive index of the semiconductor material therein will also change, thereby forming a light refraction interface with the semiconductor material in the chip. Then, by alternately stacking multiple dielectric layers with different refractive indices on the sidewalls of the isolation groove, a DBR structure can be formed. It can not only achieve sidewall passivation to better ensure the electrical performance stability and long-term reliability of the optoelectronic chip, but also cooperate with the light-blocking structure to optically isolate and fully reflect the light emitted from the sidewall of the optoelectronic chip, so that more light energy inside the optoelectronic chip can be emitted from the front, thereby better eliminating the problem of optical crosstalk and further improving the photoelectric conversion efficiency of the chip.

[0081] Wherein, the material of the metal light isolation layer may include gold, titanium, aluminum, nickel, chromium, molybdenum or copper, and is not limited thereto. Preferably, the metal light isolation layer is formed of a metal or alloy such as Al that has both excellent reflective properties and conductive properties. The metal light isolation layer may be a single layer or multilayer structure. More preferably, the thermal expansion coefficient of the heat-conducting medium material used to form the heat-conducting medium layer is between the thermal expansion coefficient of the material constituting the metal light isolation layer and the thermal expansion coefficient of the material constituting the ion isolation region, and / or the heat-conducting medium material has good bonding properties with the material constituting the metal light isolation layer and the material constituting the ion isolation region. This is not only conducive to transferring the heat generated by the chip more quickly, but also makes the metal light isolation layer more firmly bonded to the chip, avoiding the metal light isolation layer from being separated from the chip structure under the influence of the heat generated after the chip has been working for a long time. The heat-conducting medium material can be selected from silicon nitride, aluminum nitride, etc., and is not limited thereto.

[0082] More preferably, the dielectric layer used to form the distributed Bragg reflector structure is formed of the thermal conductive dielectric material to have both light reflection and heat conduction functions.

[0083] The Micro-LED chip may also include a thermally conductive passivation layer, which covers the surface of the LED chip structure and is thermally connected to the metal optical isolation layer. This thermally conductive passivation layer not only protects the surface of the LED chip array but also forms a thermal conduction path with the metal optical isolation layer, further helping to reduce the temperature of the LED chip array and ensure its operating performance and stability. The thermally conductive passivation layer may be made of, but is not limited to, aluminum nitride, boron nitride, or diamond.

[0084] In some cases, a local area of ​​the thermally conductive passivation layer fills the isolation groove and directly contacts the metal optical isolation layer. In some cases, the thermally conductive passivation layer may also have windows for forming electrodes that match the structures of the LED chips.

[0085] In some cases, the metal light isolation layer further extends to cover the surface of the LED chip structure and forms a current spreading layer.

[0086] In the present application, the material of the LED chip structure includes a III-V compound, preferably a III-V nitride, such as Al x In y Ga 1-x-yN, 1≥x≥0, 1≥y≥0, 1≥(1-xy)≥0. Wherein, the first doped semiconductor layer and the second doped semiconductor layer have different conductivity types. For example, the first doped semiconductor layer and the second doped semiconductor layer can be an N-type semiconductor layer and a P-type semiconductor layer, respectively, or vice versa. The active layer can be a multi-quantum well layer. In addition, the LED chip structure can also include other structural layers commonly known in the art, such as a buffer layer, etc. The materials, thicknesses, etc. of these structural layers can be selected or set in a manner known in the art, and will not be described here one by one. Exemplarily, the LED chip structure can be a GaN-based LED chip structure.

[0087] In the present application, the Micro-LED chip may further include a substrate, such as, but not limited to, a sapphire, Si, SiC, or GaN substrate. In some cases, such as when the Micro-LED chip is a flip-chip structure, the substrate may also be removed.

[0088] Some embodiments of the present application further provide a method for preparing the Micro-LED chip, comprising:

[0089] Making LED chip structure;

[0090] A first conductive layer and a super-surface structure are arranged on the light-emitting surface of the LED chip structure, and the super-surface structure and the first conductive layer are stacked and / or integrally arranged.

[0091] In one embodiment, a first doped semiconductor layer, an active layer, and a second doped semiconductor layer can be grown sequentially on a substrate using processes such as metal organic chemical vapor epitaxy (MOCVD) or molecular beam epitaxy (MBE), thereby forming an epitaxial structure of the Micro-LED chip, and then one or more LED chip structures can be manufactured in the epitaxial structure using processes such as photolithography and etching.

[0092] In one embodiment, the metasurface structure includes a first metasurface structure, and the preparation method specifically includes: when making a first conductive layer on the light-emitting surface of the LED chip structure, a plurality of first graphic structures are formed in the first conductive layer, and the plurality of first graphic structures are distributed in a direction parallel to the light-emitting surface, thereby forming the first metasurface structure.

[0093] Furthermore, a continuous transparent dielectric layer may be formed on the first conductive layer by atomic layer deposition (ALD) or other physical / chemical deposition methods.

[0094] In one embodiment, the metasurface structure includes a second metasurface structure, and the preparation method specifically includes: providing a transparent medium layer on the first conductive layer, and forming a plurality of second graphic structures in the transparent medium layer, and distributing the plurality of second graphic structures along a direction parallel to the light-emitting surface, thereby forming the second metasurface structure.

[0095] For example, a continuous metal layer with a thickness of less than 20 nm can be made on the light-emitting surface of the LED chip structure by evaporation or sputtering as the first conductive layer, and then a dielectric layer with a second metasurface structure is formed on the first conductive layer by atomic layer deposition (ALD) or other physical / chemical deposition methods.

[0096] In one embodiment, the metasurface structure includes a first metasurface structure and a second metasurface structure, and the preparation method specifically includes:

[0097] When manufacturing a first conductive layer on the light-emitting surface of the LED chip structure, a plurality of first graphic structures are formed in the first conductive layer, and the plurality of first graphic structures are distributed in a direction parallel to the light-emitting surface, thereby forming the first metasurface structure;

[0098] Furthermore, a transparent dielectric layer is provided on the first conductive layer, and a plurality of second graphic structures are formed in the transparent dielectric layer, and the plurality of second graphic structures are distributed along a direction parallel to the light emitting surface, thereby forming the second metasurface structure.

[0099] In the present application, a patterned mask can be pre-set on the light-emitting surface of the LED chip structure, and then a metal or non-metallic conductive material can be directly deposited on the light-emitting surface of the LED chip structure by physical / chemical deposition, thereby obtaining a first conductive layer having a first metasurface structure. Alternatively, a metal or non-metallic conductive material can be directly deposited on the light-emitting surface of the LED chip structure by physical / chemical deposition, thereby forming a continuous first conductive layer. The first conductive layer can then be processed by photolithography, etching, or other processes, thereby giving the first conductive layer a first metasurface structure. A similar method can be used for the transparent dielectric layer to provide it with a second metasurface structure.

[0100] In the present application, after the first conductive layer is produced, the first conductive layer can also be made to form an ohmic contact with the light-emitting surface of the LED chip structure, that is, the surface of the first doped semiconductor layer or the second doped semiconductor layer, through processes such as rapid annealing.

[0101] In one embodiment, the preparation method may further include: electrically connecting a surface of the second surface of the LED chip structure opposite to the light emitting surface to an LED driving mechanism via a second conductive layer.

[0102] Furthermore, the side surface (second surface) of the LED chip structure opposite to the light emitting surface (first surface) can be electrically coupled to the LED driving mechanism via a second metasurface conductive structure layer, wherein the second metasurface conductive structure layer includes the second conductive layer and a third metasurface structure, and the third metasurface structure is formed on a side surface of the second conductive layer close to the LED chip structure or on the second surface of the LED chip structure.

[0103] For example, a second conductive layer can be pre-formed on the surface of the LED driver mechanism, and a third metasurface structure can be fabricated on the second conductive layer. The second conductive layer can then be bonded to the second surface of the LED chip structure. Alternatively, the third metasurface structure can be fabricated on the second surface of the LED chip structure, and the second surface of the LED chip structure can then be bonded to the LED driver mechanism via the second conductive layer. The latter approach is preferred from the perspective of process controllability.

[0104] The second conductive layer can also be referred to as a metal bonding layer or metal adhesion layer, and its material includes, but is not limited to, one or more combinations of In, Sn, Ag, and Au. Alternatively, the second conductive layer can be formed using a conductive adhesive. However, to ensure bonding strength and thermal conductivity, the former approach will achieve better results.

[0105] In one embodiment, the preparation method may further include:

[0106] First, ion implantation is performed on the LED chip structure at least from the top surface of the second doped semiconductor layer, and the ion implantation depth reaches the interior of the first doped semiconductor layer, thereby forming an ion implantation region, so as to utilize the ion implantation region to electrically isolate multiple LED chip structures arranged in an array within the epitaxial structure, wherein the implanted ions include but are not limited to H ions, F ions, N ions or O ions. Generally speaking, the ion implantation region is arranged around the non-ion implantation region, and the LED chip structure is made in the non-ion implantation region. The sizes of the ion implantation region and the non-ion implantation region can be set to 1μm to 50μm. In order to increase the effective utilization area of ​​the epitaxial structure, the size of the non-ion implantation region should be as large as possible, and the size of the ion implantation region should be as small as possible within a reasonable range. This reasonable range should meet the following conditions, namely, it can achieve electrical isolation between adjacent chip structures and is conducive to the opening of isolation grooves.

[0107] Secondly, the ion implantation area is etched to a depth less than the ion implantation depth and reaching the interior of the first doped semiconductor layer to form an isolation groove in the ion implantation area, thereby isolating at least the second doped semiconductor layer and the active layer of any two adjacent LED chip structures from each other.

[0108] Then, a light blocking structure is provided in the isolation groove to prevent light from being transmitted between any two adjacent LED chip structures through the second doped semiconductor layer and the active layer.

[0109] For example, a patterned ion implantation mask can be pre-placed on the surface of the LED chip structure, and the ion implantation can be performed using the mask. The ion implantation mask can be pre-fabricated and then transferred to the surface of the LED chip structure, or it can be formed by coating a photoresist layer on the surface of the LED chip structure and then using a photolithography process. The pattern and size of the ion implantation mask correspond to the shape and size of the ion implantation area, which can be determined according to actual needs. For example, the ion implantation area can be circular, square, or other regular or irregular shapes.

[0110] For example, the ion implantation area can be etched using etching methods such as RIE, ECR, and ICP to form the isolation groove. Furthermore, by setting an etching mask on the ion implantation area and performing the etching operation using the etching mask, the position, size, and shape of the isolation groove can be more accurately controlled to avoid damage to the sidewalls of the chip structure. Preferably, the distance between the edge of the opening on the etching mask and the edge of the ion implantation area can be controlled to be 100nm to 20μm, so that the distance between the inner wall of the etched isolation groove and the outer wall of the corresponding ion implantation area is 100nm to 20μm. In actual production, the spacing of the high-resistance ion implantation area can be precisely adjusted by changing the size of the aforementioned ion implantation mask and etching mask, thereby flexibly defining the characteristic size of the chip and realizing the preparation of devices with sizes ranging from several microns to hundreds of microns.

[0111] Furthermore, the preparation method may further include:

[0112] Making at least one heat-conducting medium layer, and making the heat-conducting medium layer continuously cover at least the sidewalls of the isolation groove;

[0113] A metal light isolation layer is manufactured, and the metal light isolation layer is made to at least continuously cover the heat conducting medium layer to form the light blocking structure.

[0114] In the above embodiments of the present application, the thermal conductive medium layer may be grown by a process such as atomic layer deposition (ALD), and its thickness may be set to be 5 nm to 500 nm.

[0115] Preferably, a plurality of alternately stacked heat-conducting medium layers with different refractive indices may be formed at least on the sidewalls of the isolation trench, and the plurality of heat-conducting medium layers may be combined with the ion implantation region to form a distributed Bragg reflector structure.

[0116] Furthermore, a thermally conductive passivation layer can be formed on the surface of the LED chip structure, and the thermally conductive passivation layer can be thermally connected to the metal light isolation layer. The thermally conductive passivation layer can also be grown by a process such as atomic layer deposition (ALD). Preferably, the thermally conductive passivation layer can cover the entire surface of the LED chip structure. Of course, if electrodes are to be formed, corresponding windows can also be opened in the thermally conductive passivation layer.

[0117] Furthermore, the metal light isolation layer can be extended to cover the surface of the LED chip structure to form a current spreading layer, which is also beneficial to improving the light emission uniformity of the LED chip array.

[0118] By adopting the above solution, the device optical crosstalk problem can be effectively eliminated and the device luminous efficiency can be improved. At the same time, it can achieve the effects of increasing the effective use area of ​​the chip and reducing the sidewall damage effect of the material, so as to obtain Micro-LED chips with smaller size, better optical properties (such as resolution and brightness, etc.) and electrical properties.

[0119] Furthermore, electrodes that match the LED chip structure can be manufactured using solutions well known in the art, so that the Micro-LED chip can operate normally.

[0120] Obviously, compared with the solution of improving the light output efficiency and light output direction of Micro-LED chips through resonant cavity structure or lens system, and the solution of achieving full-color display through mass transfer or quantum dot thin film color conversion technology, the method of this application is compatible with large-scale standard semiconductor process technology, the process difficulty is significantly reduced, the controllability is higher, it is safer and more environmentally friendly, and the structural changes to the device are small, making it suitable for lightweight applications, low cost, high yield, better device quality, and can better meet the application requirements for ultra-high resolution display.

[0121] In addition, the solution of the present application is also suitable for the production of micro-nano sized optoelectronic devices such as Mini-LED chips.

[0122] Some embodiments of the present application further provide a Micro-LED device comprising the aforementioned Micro-LED chip. The Micro-LED device may be a lighting device, a display device, etc., but is not limited thereto.

[0123] The following describes the embodiments of the present application through specific examples. Those skilled in the art will readily understand the other advantages and benefits of the present application from the disclosure herein. The present application may also be implemented or applied through various other specific embodiments, and the details in this specification may be modified or altered based on different viewpoints and applications without departing from the spirit of the present application.

[0124] For example, when describing the embodiments of this application, cross-sectional views of device structures may be partially enlarged to a different scale for ease of explanation. Furthermore, these schematic views are merely illustrative and should not limit the scope of protection of this application. Furthermore, in actual production, three-dimensional dimensions, including length, width, and depth, should be included.

[0125] For convenience, spatially relative terms such as "under," "below," "below," "below," "above," and "on" may be used herein to describe the relationship of one element or feature to other elements or features shown in the drawings. It will be understood that these spatially relative terms are intended to encompass orientations of the device in use or operation in addition to the orientation depicted in the drawings. Additionally, when a layer is referred to as being "between" two layers, it can be the only layer between the two layers, or one or more intervening layers may also be present.

[0126] In the context of the present application, a structure described as a first feature being "above" a second feature may include embodiments where the first and second features are in direct contact, and may also include embodiments where additional features are formed between the first and second features, such that the first and second features may not be in direct contact.

[0127] It should be noted that the illustrations provided in this embodiment only illustrate the basic concept of the present application in a schematic manner. Therefore, the illustrations only show components related to the present application and are not drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component can be changed at will, and the component layout type may also be more complicated.

[0128] Example 1

[0129] Please refer to FIG1 , this embodiment provides a Micro-LED chip, which includes a sapphire substrate 10 and an LED chip structure 11. The LED chip structure includes Al2O3, Al2O4, and Al2O6 grown on the substrate in sequence from bottom to top. x Ga 1-xAn N (0≤x≤1) buffer layer 111, an N-type GaN layer 112, a GaN multi-quantum well active layer (GaN MQWs) 113, and a P-type GaN layer 114. The GaN MQWs layer 113 emits blue light with a wavelength of approximately 450 nm. Furthermore, the surface of the P-type GaN layer 114 is the light-emitting surface of the LED chip structure, and a first supersurface conductive structure layer is also provided on the surface of the P-type GaN layer 114. The first supersurface conductive structure layer is a p-type electrode 115, that is, an Au / Ni metal layer (the aforementioned first conductive layer), which has a thickness of about 50 nm and has a first supersurface structure composed of a plurality of first graphic structures 1151 periodically arranged on the surface of the P-type GaN layer 114. As shown in Figure 2, there are two types of first graphic structures. In a specified direction parallel to the light-emitting surface, one is X-shaped (referred to as the X-shaped graphic structure), and the other is a shape formed by rotating the Y-shape 90° clockwise (referred to as the variant Y-shaped graphic structure). The sizes of the X-shaped graphic structure and the variant Y-shaped graphic structure are both about 500 nm, and the two are alternately arranged along the specified direction. An X-shaped graphic structure and an adjacent Y-shaped graphic structure are separated by 40 nm and form a unit. Multiple units are periodically arranged, and the period in the specified direction and the direction perpendicular to it is about 140 nm. The Au / Ni metal layer forms an ohmic contact with the p-type GaN layer 114. The LED chip structure 11 also has a mesa structure, and its n-type electrode 116 can be a Ti / Al / Ni / Au layer, or a conductive layer made of materials such as indium tin oxide (ITO), indium (In), tin (Sn), silver (Ag), platinum (Pt), gold (Au), titanium (Ti), aluminum (Al), nickel (Ni), chromium (Cr), molybdenum (Mo), or copper (Cu), forming an ohmic contact with the n-type GaN layer 112. Compared to Micro-LED chips that use a continuous ITO conductive layer or a continuous Au / Ni metal layer with a thickness of less than 20nm as the p-type electrode, the Micro-LED chip of this embodiment, due to the use of the first super-surface conductive structure layer, emits green light with a wavelength of approximately 550nm.

[0130] A method for manufacturing the Micro-LED chip includes the following steps:

[0131] S1. An AlN buffer layer 111, an N-type GaN layer 112, a multi-quantum well active layer 113 and a P-type GaN layer 114 are sequentially grown on a sapphire substrate by MOCVD, MBE or PECVD to obtain the epitaxial wafer shown in FIG3.

[0132] S2. Patterning the P-type GaN layer 114, the GaN MQWs layer 113, and a portion of the N-type GaN layer 112 is performed by photolithography, dry or wet etching, etc., so that the P-type GaN layer 114 and the N-type GaN layer 112 are exposed after patterning to form a mesa structure. Then, an ohmic contact is formed on the surface of the N-type GaN layer 112 through processes such as metal film deposition and rapid annealing. The ohmic contact metal, i.e., the n-type electrode 116, can be Ti / Al / Ni / Au or a similar structure. The thickness of each layer does not exceed 500 nm. The rapid annealing temperature is 500°C to 1000°C, and the annealing time does not exceed 180 seconds.

[0133] S3. A patterned evaporation mask is provided on the top surface of the P-type GaN layer 114, and Au / Ni metal is deposited on the top surface of the P-type GaN layer 114 by evaporation to form a p-type electrode 115 having a first metasurface structure.

[0134] Example 2

[0135] The structure of a Micro-LED chip provided in this embodiment is basically the same as that in Example 1, except that: the p-type electrode adopts an Au / Ni metal layer with a thickness of approximately 10 nm, and the size and period of the first graphic structure in the first supersurface structure of the p-type electrode are also the same as those in Example 1.

[0136] Compared to a Micro-LED chip using a continuous Au / Ni metal layer with a thickness of approximately 10 nm as the p-type electrode, the Micro-LED chip of this embodiment, due to its use of the first metasurface conductive structure layer, emits green light with a wavelength of approximately 550 nm. Furthermore, compared to the Micro-LED chip of Example 1, the Micro-LED chip of this embodiment exhibits significantly improved luminance.

[0137] Example 3

[0138] The structure of a Micro-LED chip provided in this embodiment is basically the same as that in Example 2, except that a continuous transparent silicon oxide (SiO2) film with a thickness of about 1 μm is also covered on the p-type electrode.

[0139] Compared with the Micro-LED chip of Example 2, the Micro-LED chip of this embodiment has better light emission uniformity.

[0140] Example 4

[0141] The structure of a Micro-LED chip provided in this embodiment is basically the same as that of Example 1, with the following difference: referring to Figure 4, a transparent silicon oxide (SiO2) film 117 with a thickness of about 1 μm is also covered on the p-type electrode 115. The SiO2 film has a second metasurface structure composed of a plurality of second graphic structures 1171 periodically arranged on the upper surface of the p-type electrode. The second graphic structure is a circular graphic structure with a variant F-shaped through-hole embedded in the center. The diameter of the circular graphic structure is 100 nm. In a specified direction parallel to the light-emitting surface, the shape of the variant F-shaped through-hole is a shape formed by rotating the F-shape 30° clockwise. Its lateral dimension is about 30 nm and the longitudinal dimension is about 40 nm. The period in the specified direction and the direction perpendicular thereto is about 50 nm.

[0142] A method for manufacturing the Micro-LED chip is also substantially the same as that of Example 1, except that it further includes the following steps:

[0143] S4. Depositing a continuous SiO2 film on the p-type electrode using ALD or other processes, and then patterning the SiO2 film using photolithography and dry etching processes to form the second metasurface structure.

[0144] Compared with Example 1, the Micro-LED chip of this embodiment adopts the first metasurface structure and the second metasurface structure. Not only does it emit green light with a wavelength of about 550nm, but the collimation and light extraction efficiency of the device are also significantly improved. In particular, the color saturation and contrast presented by the device are higher.

[0145] Example 5

[0146] The structure of a Micro-LED chip provided in this embodiment is basically the same as that in Example 4, except that: the first supersurface structure is the same as the second supersurface structure in Example 4, and the second supersurface structure is the same as the first supersurface structure in Example 4.

[0147] The operating performance of the Micro-LED chip of this embodiment is similar to that of Example 4, but the saturation and contrast of the colors presented during operation are reduced to a certain extent.

[0148] Example 6

[0149] The structure of a Micro-LED chip provided in this embodiment is substantially the same as that of Example 4, except that the second pattern structure comprises two shapes: a modified K-shape and a modified L-shape. In the specified direction, the modified K-shape is formed by rotating the K-shape 45° counterclockwise, and the modified L-shape is formed by mirroring the L-shape. Both patterns are approximately 100 nm in size and are arranged alternately along the specified direction. A modified K-shaped pattern structure and an adjacent modified L-shaped pattern structure are spaced approximately 30 nm apart and form a unit. Multiple units are arranged periodically, with a period of approximately 130 nm in both the specified direction and the perpendicular direction. Light emitted by this Micro-LED chip is primarily green light with a wavelength of approximately 550 nm, but the device's collimation and light extraction efficiency are inferior to those of the device in Example 4.

[0150] Example 7

[0151] The structure of a Micro-LED chip provided in this embodiment is basically the same as that of Example 2, except that: a transparent silicon oxide (SiO2) film with a thickness of about 1 μm is also covered on the p-type electrode, and the SiO2 film has a second metasurface structure composed of a plurality of second graphic structures periodically arranged on the upper surface of the p-type electrode, and the second graphic structure is a regular hexagonal graphic structure with an H-shaped through hole embedded in the center. The diameter of the regular hexagonal graphic structure is 80 nm, and the lateral and longitudinal dimensions of the H-shaped through hole are both about 35 nm. In the specified direction, every two adjacent regular hexagonal graphic structures are spaced approximately 60 nm apart and form a unit. The multiple units are arranged periodically, and the period in the specified direction and the direction perpendicular thereto is approximately 140 nm.

[0152] Compared with Examples 2 and 3, the Micro-LED chip of this embodiment adopts the first metasurface structure and the second metasurface structure. Not only does it emit green light with a wavelength of about 550nm, but the collimation and light extraction efficiency of the device are also significantly improved. In particular, the saturation and contrast of the colors presented by the device are also higher.

[0153] Example 8

[0154] The structure of a Micro-LED chip provided in this embodiment is basically the same as that of Example 4, except that: referring to Figure 5, the Au / Ni metal layer 115' is continuous and has a thickness of approximately 10nm; and, in the second metasurface structure of the SiO2 film 117', in a specified direction parallel to the light-emitting surface, the second graphic structure 1171' is elliptical, with a major axis of approximately 120nm and parallel to the specified direction, and a minor axis of approximately 80nm. A V-shaped through hole and an X-shaped through hole are formed on both sides of the minor axis, respectively. The size of the V-shaped through hole is approximately 25nm, the size of the X-shaped through hole is approximately 40nm, and the spacing between the V-shaped through hole and the X-shaped through hole is approximately 50nm. Two adjacent ellipses are spaced approximately 60nm apart and form a unit. Multiple units are arranged periodically, with a period in the specified direction of approximately 180nm and a period in a direction perpendicular to the specified direction of approximately 140nm. The Micro-LED chip of this embodiment uses the second metasurface structure, and thus emits red light with a wavelength of approximately 650nm. The light energy emitted from the active area has low loss, directional emission, high collimation and light extraction efficiency.

[0155] Example 9

[0156] The structure of a Micro-LED chip provided in this embodiment is substantially the same as that of Example 8, except that: The second metasurface structure of the SiO2 film has four shapes in a specified direction parallel to the light-emitting surface: a modified Z-shaped, a modified T-shaped, a modified M-shaped, and a P-shaped structure. The dimensions of each of these four structures are approximately 150 nm. The modified Z-shaped and modified T-shaped structures are arranged alternately along the specified direction, the modified M-shaped and P-shaped structures are also arranged alternately along the specified direction, the P-shaped and modified Z-shaped structures are arranged alternately in a direction perpendicular to the specified direction, and the modified M-shaped and modified T-shaped structures are arranged alternately in a direction perpendicular to the specified direction. Four adjacent modified Z-shaped, modified T-shaped, modified M-shaped, and P-shaped structures, totaling four structures, form a unit. The spacing between adjacent structures in the specified direction and the spacing between adjacent structures in a direction perpendicular thereto are both approximately 50 nm. Multiple units are arranged periodically, with a period of approximately 200 nm in both the specified direction and the direction perpendicular thereto. Because the Micro-LED chip of this embodiment adopts the second metasurface structure, although it still emits blue light, its collimation, brightness and luminous uniformity are significantly improved compared with the control product that does not adopt the second metasurface structure.

[0157] Example 10

[0158] Referring to Figures 6 and 7, a Micro-LED chip provided in this embodiment includes an LED chip structure 21, which includes an N-type GaN layer 211, a GaN multi-quantum well active layer (GaN MQWs) 212, and a P-type GaN layer 213. The GaN MQWs layer 212 emits blue light with a wavelength of approximately 450nm. Furthermore, the surface of the N-type GaN layer 211 is the light-emitting surface of the LED chip structure, and a first super-surface conductive structure layer 214 is also provided on the surface of the N-type GaN layer 211. The first super-surface conductive structure layer includes an n-type electrode 2141 and a transparent silicon oxide layer 2142 stacked on the n-type electrode 2141. The n-type electrode 2141 and the transparent silicon oxide layer 2142 respectively have the same first super-surface structure and second super-surface structure as in Example 4, and the n-type electrode 2141 forms an ohmic contact with the N-type GaN layer 211. At the same time, the P-type GaN layer 213 is bonded to the driving substrate 216 through the metal adhesion layer 215 (ie, the aforementioned second conductive layer), and is electrically connected to the CMOS (complementary metal oxide semiconductor) or TFT (thin film field effect transistor) driving circuit in the driving substrate.

[0159] A method for manufacturing the Micro-LED chip includes the following steps:

[0160] S1. An AlN buffer layer, an N-type GaN layer, a multi-quantum well active layer, and a P-type GaN layer are sequentially grown on a silicon substrate by MOCVD, MBE, or PECVD to obtain an epitaxial wafer having a structure similar to that shown in FIG3 .

[0161] S2. The P-type GaN layer of the epitaxial wafer is adhered to a temporary substrate of the same size through a temporary bonding process. The temporary substrate can be a silicon or sapphire substrate. The adhesion force includes but is not limited to electrostatic force, adhesion provided by adhesive materials such as photoresist that can be released without loss, so that the epitaxial wafer and the temporary substrate can be separated without damage through a debonding process.

[0162] S3. Use laser stripping, thinning and grinding to remove the silicon substrate in the epitaxial wafer, then use dry etching or wet etching to remove the AlN buffer layer and part of the N-type GaN layer.

[0163] S4. Prepare a first supersurface conductive structure layer on the surface of the remaining N-type GaN layer in a manner similar to Example 4.

[0164] S5, separating the LED chip structure in the device structure obtained in step S4 from the temporary substrate through a debonding process;

[0165] S6. Bonding the P-type GaN layer to the driving substrate through the metal adhesion layer.

[0166] When the Micro-LED chip is in use, the brightness of the Micro-LED chip can be controlled by applying different electrical signals to the CMOS or TFT driving circuit.

[0167] Example 11

[0168] Referring to FIG. 8 , the structure of a Micro-LED chip provided in this embodiment is substantially identical to that of Example 9, except that a third metasurface structure 217 is further formed on the surface of the P-type GaN layer 213 facing away from the N-type GaN layer. This metasurface structure is configured to reflect light emitted from the active region toward the P-type GaN layer. This third metasurface structure comprises a plurality of periodically arranged third graphic structures 2171. These third graphic structures are either regular triangles or modified regular triangles, each with a side length of approximately 100 nm. These third graphic structures are arranged alternately along a specified direction parallel to the surface of the P-type GaN layer 213 facing away from the N-type GaN layer. A modified X-shaped through-hole is embedded in the center of the regular triangle graphic structure. This modified X-shaped through-hole is an X-shaped through-hole rotated 45° clockwise, with each line of the X-shaped through-hole being approximately 60 nm long. A variant Z-shaped through-hole is embedded in the center of the variant equilateral triangle structure. The variant equilateral triangle is formed by rotating the equilateral triangle 90° clockwise around a designated point. The variant Z-shaped through-hole is formed by rotating the Z-shape 45° clockwise. The length of each Z-shaped line is also approximately 60nm. The midpoint of one side of each equilateral triangle structure and a vertex of an adjacent variant equilateral triangle structure intersect at the designated point and form a unit. Multiple units are arranged periodically, with a period of approximately 300nm in the designated direction and approximately 200nm in the direction perpendicular to the designated direction. Compared to Examples 4 and 10, the Micro-LED chip of this embodiment has higher brightness and more significantly improved collimation.

[0169] A method for manufacturing the Micro-LED chip is substantially the same as that of Example 10, except that it further includes the following steps:

[0170] S5X: After completing step S5, the exposed surface of the P-type GaN layer is patterned by photolithography and dry etching processes to form a third metasurface structure, and then step S6 is performed.

[0171] Example 12

[0172] Referring to FIG. 9 , this embodiment provides an epitaxial structure of a Micro-LED chip, comprising an AlN buffer layer 311, an N-type GaN layer 312, a multi-quantum well active layer 313, and a P-type GaN layer 314, sequentially grown on a sapphire substrate 310. The multi-quantum well active layer can emit blue light with a central wavelength of approximately 450 nm. The epitaxial structure includes an ion-implanted region 315 and multiple non-ion-implanted regions distributed along the layer plane. Any two adjacent non-ion-implanted regions are electrically isolated by the ion-implanted region. An LED chip structure 316 is fabricated within each non-ion-implanted region, and each LED chip structure 316 can serve as a pixel, meaning that the Micro-LED chip contains multiple pixels. Furthermore, an isolation trench 317 is provided within the ion-implanted region to isolate the P-type GaN layer and the multi-quantum well active layer of two adjacent LED chip structures from each other. Furthermore, a light-blocking structure is provided within the isolation trench to prevent light from transmitting between the two adjacent Micro-LED chip structures through the P-type GaN layer 314 and the multi-quantum well active layer 313. The light-blocking structure includes one or more layers of opaque metal light isolation layers 318, made of gold (Au), titanium (Ti), aluminum (Al), nickel (Ni), chromium (Cr), molybdenum (Mo), copper (Cu), or their alloys. The metal light isolation layer covers the inner wall of the isolation groove and is primarily used to block and reflect light reflected by the multi-quantum well active layer, thereby blocking the light transmission path between adjacent Micro-LED chip structures. A thermal conductive medium layer 319 is also provided between the metal light isolation layer and the inner wall of the isolation groove. As shown in FIG10 , the thermal conductive medium layer comprises eight pairs of TiO2 / SiO2 composite layers. The total thickness of the thermal conductive medium layer is approximately 895.2 nm, wherein TiO2 layers 3191 and SiO2 layers 3192 are alternately stacked to form a distributed Bragg reflector structure. The thickness of each TiO2 layer is approximately 41.1 nm, and the thickness of each SiO2 layer is approximately 70.8 nm. The reflectivity of the thermal conductive medium layer for light of different wavelengths is shown in FIG11 . On the one hand, the thermal conductive medium layer can passivate the inner wall of the isolation groove and electrically isolate the metal optical isolation layer from the inner wall of the isolation groove. On the other hand, it can cooperate with the metal optical isolation layer (such as a metal aluminum layer) to more thoroughly eliminate the problem of optical crosstalk. At the same time, it can also serve as a transition layer between the ion injection area of ​​the doped GaN material and the metal optical isolation layer, strengthen the bonding force between the metal optical isolation layer and the isolation groove wall, and cooperate with the metal optical isolation layer to construct a new thermal conductive channel for the Micro-LED chip. At the same time, the metal optical isolation layer also continuously extends to cover the surface of the adjacent LED chip structure, thereby forming a current expansion layer. In addition, a transparent medium layer 320 is also covered on the current expansion layer, which is in direct contact with the metal optical isolation layer. Its material can include but is not limited to silicon oxide, titanium oxide, etc. The current expansion layer and the transparent medium layer on the surface of each LED chip structure cooperate to form a first super surface conductive structure.Furthermore, the first metasurface conductive structure layers on the surfaces of three adjacent LED chip structures are different. For example, the first metasurface conductive structure layers on the surfaces of the three LED chip structures are the same as those in Examples 1, 7, and 8, respectively, emitting green, red, and blue light, thereby achieving full-color display. To achieve the same first metasurface conductive structure layer as in Example 1, the current spreading layer on the surface of the corresponding LED chip structure can be patterned. To achieve the same first metasurface conductive structure layer as in Examples 7 and 8, the thickness of the current spreading layer on the surface of the corresponding LED chip structure can be reduced to less than 20 nm.

[0173] As an improved solution, referring to Examples 9 and 10, the sapphire substrate or the sapphire substrate and the AlN buffer layer can be removed, and the substrate can be bonded to the drive substrate via a metal adhesion layer 215 (i.e., the aforementioned second conductive layer). Furthermore, the N-type GaN layer can be electrically connected to the CMOS (complementary metal oxide semiconductor) or TFT (thin film field effect transistor) drive circuit in the drive substrate. By applying different electrical signals to the CMOS or TFT drive circuit to control the brightness of different pixels, the three pixel units of red, green, and blue with different brightness levels can be mixed into a single color unit, thereby enabling full-color display applications.

[0174] A method for preparing the Micro-LED chip may include the following steps:

[0175] S1. Using MOCVD, MBE, PECVD and other methods, an AlN buffer layer, an N-type GaN layer, a multi-quantum well active layer and a P-type GaN layer are sequentially grown on a sapphire substrate to obtain an epitaxial wafer.

[0176] S2. A patterned ion implantation mask is formed by photolithography and other processes. The materials of the ion implantation mask include but are not limited to photoresist, silicon oxide, silicon nitride, metal, etc. Using the ion implantation mask as a barrier layer, ion implantation is performed on the epitaxial structure in the epitaxial wafer to control the area and / or shape of the light-emitting area of ​​the Micro-LED chip. The depth of the ion implantation must at least penetrate the P-type GaN layer, preferably reaching the inside of the N-type GaN layer. The types of ions implanted include but are not limited to H ions, F ions, N ions, O ions, etc. The size of the ion implantation area finally formed is 1μm to 50μm, and the size of the non-ion implantation area is 1μm to 50μm. From a top-down perspective, the ion implantation area is preferably arranged around the non-ion implantation area, and each non-ion implantation area is used to form an LED chip structure. This step uses ion implantation for electrical isolation, which has the advantages of less damage and high control accuracy compared to the method of using an etching process for electrical isolation.

[0177] S3. An etching mask is set on the ion implantation area, and a through hole is opened on the etching mask. The size of the through hole is smaller than the size of the ion implantation area. Preferably, the distance between the edge of the through hole and the edge of the ion implantation area is 100nm to 20μm, so as to minimize the damage to the side wall of the chip. Then, a dry etching process such as atomic layer etching (ALE), ion beam etching (IBE), and inductively coupled plasma etching (ICP) is used to etch the ion implantation area through the through hole of the etching mask. The etching depth is less than or equivalent to the ion implantation depth, but preferably less than the ion implantation depth, and especially preferably enters the interior of the N-type GaN layer, thereby forming an isolation groove. This step can not only effectively avoid the damage to the side wall caused by the etching process and improve the photoelectric conversion efficiency by performing dry etching in the ion implantation area, but also the formed etched isolation area can be narrower, especially it can effectively isolate the light between the pixels in the Micro-LED chip and eliminate the optical crosstalk effect.

[0178] S4. A thermally conductive medium layer is formed on the side wall of the isolation groove by atomic layer deposition (ALD) and other processes. In some cases, the inner wall of the isolation groove can also be completely covered with a thermally conductive medium layer. Further, an opaque metal material is deposited on the thermally conductive medium layer to form a metal light isolation layer. The light-blocking structure formed mainly by the metal light isolation layer can effectively reduce the light crosstalk between each pixel point. Among them, the isolation groove can also be filled with a metal light isolation layer. Then, the metal light isolation layer is continuously extended to cover the surface of the adjacent LED chip structure, thereby forming a current expansion layer. And for the current expansion layer on the surface of different LED chip structures, they can be thinned, patterned, etc. respectively. Then, a transparent dielectric layer is deposited on the metal light isolation layer as a passivation layer, so that it passivates the surface of the metal light isolation layer and serves as a thermal conductive layer of the Micro-LED chip. In particular, the transparent dielectric layer on the surface of some LED chip structures can also be patterned, so that the current expansion layer and the transparent dielectric layer on the surface of each LED chip structure cooperate to form the aforementioned first super-surface conductive structure layer.

[0179] The above embodiments are merely illustrative of the principles and effects of this application and are not intended to limit this application. Anyone skilled in the art may modify or alter the above embodiments without departing from the spirit and scope of this application. Therefore, all equivalent modifications or alterations made by one of ordinary skill in the art without departing from the spirit and technical concepts disclosed in this application shall be covered by the claims of this application.

Claims

1. A Micro-LED chip, comprising an LED chip structure, characterized in that: The Micro-LED chip further includes a first super-surface conductive structure layer, and the first super-surface conductive structure layer includes: A first conductive layer electrically coupled to the light emitting surface of the LED chip structure; The super surface structure is stacked and / or integrated with the first conductive layer and is at least used to adjust the emission angle and / or wavelength of light emitted from the light emitting surface.

2. The Micro-LED chip according to claim 1, characterized in that: The supersurface structure includes a first supersurface structure, the first conductive layer includes a plurality of first graphic structures, the plurality of first graphic structures are distributed along a direction parallel to the light emitting surface, and form the first supersurface structure; wherein the first conductive layer includes a metal conductive layer or a non-metal conductive layer.

3. The Micro-LED chip according to claim 1, wherein: The first conductive layer includes a metal conductive layer or a non-metal conductive layer; the metal conductive layer has a thickness of less than 20 nm and extends continuously in a direction parallel to the light emitting surface.

4. The Micro-LED chip according to any one of claims 2 to 3, characterized in that: The material of the metal conductive layer includes any one or more combinations of indium, tin, silver, platinum, gold, titanium, aluminum, nickel, chromium, molybdenum and copper; and / or the thickness of the metal conductive layer is 0.1nm-20nm, or the thickness of the metal conductive layer is greater than 20nm; And / or, the material of the non-metallic conductive layer includes ITO; and / or, the thickness of the non-metallic conductive layer is 1 nm to 500 nm.

5. The Micro-LED chip according to claim 2, wherein: The first graphic structure includes an X-shaped graphic structure and a variant Y-shaped graphic structure; in a specified direction parallel to the light-emitting surface, the variant Y-shape is a shape formed by rotating the Y-shape 90° clockwise, and the sizes of the X-shaped graphic structure and the variant Y-shaped graphic structure are both 1nm~1μm; and the X-shaped graphic structure and the variant Y-shaped graphic structure are alternately arranged along the specified direction, each X-shaped graphic structure and an adjacent Y-shaped graphic structure are spaced 1~500nm apart and form a unit, and multiple units are periodically arranged, and the period in the specified direction and the direction perpendicular to the specified direction is 1nm~1μm.

6. The Micro-LED chip according to any one of claims 1 to 3, characterized in that: The first super-surface conductive structure layer also includes a transparent medium layer stacked on the first conductive layer.

7. The Micro-LED chip according to claim 6, wherein: The super-surface structure includes a second super-surface structure, and the transparent medium layer includes a plurality of second graphic structures. The plurality of second graphic structures are distributed along a direction parallel to the light emitting surface to form a second super-surface structure.

8. The Micro-LED chip according to claim 7, characterized in that: The super surface structure comprises: A first metasurface structure is formed in the first conductive layer and is used to at least adjust one of an emission angle and a wavelength of light emitted from the light-emitting surface; A second metasurface structure is used to at least adjust the other of an emission angle and a wavelength of light emitted from the light-emitting surface; and / or, in a direction parallel to the light emitting surface, a size of the second graphic structure is 1 nm to 1 μm; And / or, the second graphic structure includes a circular graphic structure with a variant F-shaped through hole embedded in the center, in a specified direction parallel to the light-emitting surface, the variant F-shape is a shape formed by rotating the F-shape 30° clockwise, the size of the variant F-shape is 1 to 200 nm, a plurality of the circular graphic structures are periodically arranged, and the periods in the specified direction and in a direction perpendicular to the specified direction are both 1 nm to 1 μm; Alternatively, the second graphic structure includes a variant K-shaped graphic structure and a variant L-shaped graphic structure. In a specified direction parallel to the light-emitting surface, the variant K-shape is a shape formed by rotating the K-shape counterclockwise by 45°, and the variant L-shape is a shape formed by flipping the L-shape in a mirror image. The variant K-shaped graphic structure and the variant L-shaped graphic structure are alternately arranged along the specified direction. Each variant K-shaped graphic structure and an adjacent variant L-shaped graphic structure are spaced 1 to 200 nm apart and form a unit. A plurality of the units are periodically arranged, and the periods in the specified direction and in a direction perpendicular to the specified direction are both 1 to 500 nm. Alternatively, the second graphic structure comprises a regular hexagonal graphic structure with an H-shaped through hole embedded in the center, the size of the H-shaped through hole is 1 to 200 nm, and in a specified direction parallel to the light-emitting surface, every two adjacent regular hexagonal graphic structures are spaced 1 to 200 nm apart and form a unit, a plurality of the units are arranged periodically, and the periods in the specified direction and in a direction perpendicular to the specified direction are both 1 to 1000 nm; Alternatively, the second graphic structure includes an elliptical graphic structure, the major axis of the ellipse is 1-1000nm and is parallel to a specified direction on the light-emitting surface, the minor axis is 1-1000nm, a V-shaped through hole and an X-shaped through hole are formed on both sides of the minor axis, the sizes of the V-shaped and X-shaped are 1-500nm, the interval between the V-shaped through hole and the X-shaped through hole is 1-500nm, every two adjacent elliptical graphic structures are spaced 1-500nm apart and form a unit, a plurality of the units are periodically arranged, and the period in the specified direction and the direction perpendicular to the specified direction is 1-1000nm; Alternatively, the second graphic structure includes a variant Z-shaped graphic structure, a variant T-shaped graphic structure, a variant M-shaped graphic structure and a P-shaped graphic structure, wherein the variant Z-shaped graphic structure and the variant T-shaped graphic structure are alternately arranged along a specified direction parallel to the light exiting surface, the variant M-shaped graphic structure and the P-shaped graphic structure are also alternately arranged along the specified direction, the P-shaped graphic structure and the variant Z-shaped graphic structure are alternately arranged in a direction perpendicular to the specified direction, and the variant The M-shaped graphic structure and the variant T-shaped graphic structure are alternately arranged in a direction perpendicular to the specified direction, each of the variant Z-shaped graphic structures and an adjacent variant T-shaped graphic structure, a variant M-shaped graphic structure and a P-shaped graphic structure form a unit, and the spacing between any two graphic structures in each of the units in the specified direction and the direction perpendicular to the specified direction is 1 to 200 nm; multiple units are periodically arranged, and the period in the specified direction and the direction perpendicular to the specified direction is 1 to 1000 nm.

9. The Micro-LED chip according to claim 6, wherein: The material of the transparent medium layer includes any one or more combinations of silicon oxide, silicon nitride, aluminum nitride, aluminum oxide, gallium oxide, titanium oxide, and hafnium oxide; and / or the thickness of the transparent medium layer is 0.1 nm to 1 μm.

10. The Micro-LED chip according to claim 1, characterized in that: It also includes a second super-surface conductive structure layer, the LED chip structure has a first surface and a second surface opposite to the first surface, the first surface is the light emitting surface, and the second surface is electrically connected to the LED driving mechanism through a second conductive layer.

11. The Micro-LED chip according to claim 10, characterized in that: The second surface of the LED chip structure is electrically combined with the LED driving mechanism via the second supersurface conductive structure layer, the second supersurface conductive structure layer includes the second conductive layer and the third supersurface structure, the third supersurface structure is arranged on a side surface of the second conductive layer close to the LED chip structure or on the second surface of the LED chip structure, and is at least used to reflect light emitted from the LED chip structure to the second supersurface conductive structure layer; The third supersurface structure includes a plurality of third graphic structures distributed in a direction parallel to the second surface, and the size of the third graphic structure is 1nm~1μm; and the third graphic structure includes an equilateral triangle graphic structure and a variant equilateral triangle graphic structure, and the equilateral triangle graphic structure and the variant equilateral triangle graphic structure are alternately arranged in a specified direction parallel to the second surface, wherein a variant X-shaped through hole is embedded in the center of the equilateral triangle graphic structure, and the variant X-shape is the shape of the X-shape rotated 45° clockwise, and a variant Z-shaped through hole is embedded in the center of the variant equilateral triangle graphic structure, and the variant equilateral triangle is the shape of the equilateral triangle rotated 90° clockwise around a specified point, and the variant Z-shape is the shape of the Z-shape rotated 45° clockwise, and the line lengths of the variant X-shape and the variant Z-shape are 1nm~500nm; the midpoint of one side of each of the equilateral triangle graphic structures and a vertex of an adjacent variant equilateral triangle graphic structure intersect at the specified point and form a unit, and a plurality of the units are periodically arranged, and the period in the specified direction and the direction perpendicular to the specified direction is 1nm~1μm.

12. The Micro-LED chip according to claim 1, wherein: The LED chip structure comprises a first doped semiconductor layer, an active layer and a second doped semiconductor layer stacked in sequence along a set direction, and a surface of the first doped semiconductor layer or the second doped semiconductor layer away from the active layer is the light emitting surface; And / or, the first conductive layer forms an ohmic contact with the light emitting surface of the LED chip structure; and / or, the LED chip structure includes a GaN-based LED chip structure.

13. The method for preparing a Micro-LED chip according to any one of claims 1 to 12, characterized in that: include: Making LED chip structure; A first conductive layer and a super surface structure are arranged on the light emitting surface of the LED chip structure, and the super surface structure and the first conductive layer are stacked and / or integrally arranged.

14. The method for preparing a Micro-LED chip according to claim 13, characterized in that: The supersurface structure includes a first supersurface structure, and the preparation method specifically includes: when making a first conductive layer on the light-emitting surface of the LED chip structure, a plurality of first graphic structures are formed in the first conductive layer, and the plurality of first graphic structures are distributed in a direction parallel to the light-emitting surface, thereby forming the first supersurface structure; Alternatively, the supersurface structure includes a second supersurface structure, and the preparation method specifically includes: providing a transparent medium layer on the first conductive layer, and forming a plurality of second graphic structures in the transparent medium layer, and distributing the plurality of second graphic structures along a direction parallel to the light emitting surface, thereby forming the second supersurface structure; Alternatively, the supersurface structure includes a first supersurface structure and a second supersurface structure, and the preparation method specifically includes: When manufacturing a first conductive layer on the light emitting surface of the LED chip structure, a plurality of first graphic structures are formed in the first conductive layer, and the plurality of first graphic structures are distributed in a direction parallel to the light emitting surface, thereby forming the first super surface structure; And, a transparent medium layer is arranged on the first conductive layer, and a plurality of second graphic structures are formed in the transparent medium layer, and the plurality of second graphic structures are distributed along a direction parallel to the light emitting surface, so as to form the second super surface structure.

15. The method for preparing a Micro-LED chip according to any one of claims 13 to 14, characterized in that: Also includes: The side surface of the LED chip structure opposite to the light emitting surface is electrically connected to the LED driving mechanism through a second supersurface conductive structure layer; wherein the second supersurface conductive structure layer includes a second conductive layer and a third supersurface structure, and the third supersurface structure is formed on the side surface of the second conductive layer close to the LED chip structure or on the side surface of the LED chip structure opposite to the light emitting surface.

16. A Micro-LED device, characterized in that A Micro-LED chip comprising any one of claims 1-12.

Citation Information

Patent Citations

  • Fabrication technique of double-layer nano imaging LED

    CN103227249A

  • LED chip and manufacturing method thereof

    CN110783434A

  • Display substrate, manufacturing method thereof and display device

    CN113990908A

  • Micro-LED display chip, manufacturing method thereof and related equipment

    CN114759058A

  • LED structure, preparation method thereof and light field display system

    CN114824043A

Cited By

  • On-chip integrated system of Micro LED optical waveguide AR glasses

    CN120195800A