Tread rubber composition achieving low noise, low rolling resistance and wear resistance, mixing method, and tire
By using a combination of modified carbon black W31 and white carbon black in the tread rubber composition, combined with a specific process and composition ratio, the problem of difficult to take into account both the rolling resistance and the wear performance in the prior art is achieved, and the low Noise, low roll resistance and wear resistance, especially under harsh road conditions.
Patent Information
- Application Number
- PCT/CN2023/122261
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2023-09-27
- Publication Date
- 2024-11-28
AI Technical Summary
While improving the rolling resistance and wear performance, existing tread rubber compositions are difficult to take into account low noise, especially under harsh road conditions, and the low Vickers hardness of carbon black leads to poor grip in wetlands.
By using the combination of modified carbon black W31 and white carbon black, by adjusting the modulus of the rubber composition and adding components such as sulfur powder, vulcanization accelerator, zinc oxide, microcrystalline wax, environmentally friendly oil, stearic acid and anti-aging agent, the The mixing process of the series-connected mixer and the F370 shear mixer optimizes the physical and noise performance of the rubber composition.
A tread rubber composition with low noise, low roll resistance and wear resistance is achieved, improving the noise performance of the tire on demanding road surfaces and wetland grip, ensuring the roll resistance and physical properties of the rubber composition.
Smart Images

Figure PCTCN2023122261-FTAPPB-I100001 
Figure PCTCN2023122261-FTAPPB-I100002 
Figure PCTCN2023122261-FTAPPB-I100003
Abstract
Description
Tread rubber composition, mixing method and tire with low noise, low rolling resistance and wear resistance
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to Chinese patent application number 202310599019.1 filed with the State Intellectual Property Office of China on May 25, 2023, entitled “A tread rubber composition, mixing method and tire with low noise, low rolling resistance and wear resistance,” the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present disclosure relates to the technical field of tire manufacturing, and in particular to a tread rubber composition, a mixing method, and a tire that are low-noise, low-rolling-resistance, and wear-resistant. Background Art
[0004] In rubber processing, carbon black or white carbon black is usually added during mixing as a reinforcing agent to enhance the mechanical properties of rubber, giving rubber special properties such as magnetism, conductivity, flame retardancy, and color. It also helps to improve the processability of rubber (reducing the shrinkage of semi-finished products, improving the surface flatness of semi-finished products, etc.) and reduce costs.
[0005] Adding carbon black to rubber maintains excellent physical properties and wear resistance in the tread rubber composition. However, due to the gelled physical bond between carbon black and rubber, slippage occurs under external forces. This leads to high friction between the carbon black itself and between carbon black and rubber, resulting in significant hysteresis losses in the rubber composition and increased rolling resistance. Furthermore, due to the low Vickers hardness of carbon black, it is covered by the rubber and rarely exposed, resulting in poor wet grip.
[0006] In the 1950s, scientists invented silica white carbon black, known in the industry as a "green filler." Compared to carbon black, it has lower rolling resistance and better wet grip. This is mainly because silica and rubber form chemical cross-links through coupling agents, resulting in low friction between silica and rubber, low hysteresis loss, and low rolling resistance of the tire, but poor wear. Due to its polarity, silica interacts strongly with water and weakly with rubber. Furthermore, due to silica's higher Vickers hardness, when sliding on wet roads, the rubber on the silica surface is easily rubbed off, exposing the silica to the surface of the rubber composition, which can puncture the water film and increase wet grip.
[0007] To better balance tire rolling resistance and wear performance, it is urgent to develop a new filler to compensate for the shortcomings of existing fillers. In addition to using new fillers to develop a rubber composition that balances rolling resistance and wear performance, tire noise, especially harsh road noise, must also be taken into account.
[0008] Summary of the Invention
[0009] The present disclosure provides a rubber composition, wherein the rubber composition is composed of raw materials including the following components based on 100 parts by weight of the rubber component:
[0010] Optionally, the modified carbon black satisfies:
[0011] The oil absorption value is 100-120*10 -5 cm 3 / g, nitrogen adsorption surface area is 70-90m 2 / g, iodine absorption value 80-90g / kg, total specific surface area 75-85*10 3 m 2 / kg, tinting strength 95-110%.
[0012] Optionally, the modified carbon black is carbon black W31, obtained from Jiangxi Black Cat Carbon Black Co., Ltd.
[0013] Optionally, the rubber composition satisfies M10≤0.5Mpa and M300≥8.0Mpa.
[0014] Optionally, the rubber composition has a shore A hardness of 55-62, and optionally a shore A hardness of 55-60.
[0015] The present disclosure provides a tire tread rubber composition that is low-noise, low-rolling-resistance, and wear-resistant, wherein the rubber composition is prepared by mixing raw materials including the following components based on 100 parts of the rubber component:
[0016] The modified carbon black is carbon black W31, produced by Jiangxi Black Cat Carbon Black Co., Ltd., with an oil absorption value of 100-120*10 -5 cm 3 / g, nitrogen adsorption surface area is 70-90m 2 / g, iodine absorption value 80-90g / kg, total specific surface area 75-85*10 3 m 2 / kg, tinting strength 95-110%; and the rubber composition has M10 ≤ 0.5 MPa, M300 ≥ 8.0 MPa, and hardness shore A 55-60.
[0017] Optionally, the rubber composition is prepared by mixing raw materials including the following components based on 100 parts of the rubber component:
[0018] Optionally, the rubber is selected from a mixture of natural rubber or butadiene rubber and one or two solution-polymerized styrene-butadiene rubbers.
[0019] Optionally, the mixture contains 10-30 phr of natural rubber or butadiene rubber and 70-90 phr of solution-polymerized styrene-butadiene rubber.
[0020] Optionally, the butadiene rubber is neodymium-based butadiene rubber.
[0021] Optionally, the neodymium-based butadiene rubber satisfies the following conditions: the weight average molecular weight is between 380 kg / mol<Mw<460 kg / mol.
[0022] Optionally, the solution-polymerized styrene-butadiene rubber is selected from two solution-polymerized styrene-butadiene rubbers and used in combination. The solution-polymerized styrene-butadiene rubber 1 must meet the following requirements: the percentage S of styrene in the solution-polymerized styrene-butadiene rubber must be 30%<S<42%; the solution-polymerized styrene-butadiene rubber 2 must meet the following requirements: the percentage S of styrene in the solution-polymerized styrene-butadiene rubber must be S>40%.
[0023] Optionally, the rubber composition further comprises one or more of oil-extended sulfur powder, a vulcanization accelerator, zinc oxide, microcrystalline wax, environmentally friendly oil, stearic acid, and an antioxidant;
[0024] Optionally, the oil-extended sulfur powder comprises 1.0-2.5 phr, a vulcanization accelerator comprises 1.0-5.0 phr, zinc oxide comprises 1.0-4.0 phr, microcrystalline wax comprises 1.0-4.0 phr, environmentally friendly oil comprises 2-10 phr, stearic acid comprises 1.5-4.0 phr and an antioxidant comprises 2.0-5.0 phr.
[0025] Optionally, the antioxidant is antioxidant TMQ or antioxidant 6PPD.
[0026] Optionally, the antioxidant is TMQ 1.0-2.0 phr, or 6PPD 2.0-4.0 phr.
[0027] Optionally, the vulcanization accelerator is accelerator NS, and the oil-extended sulfur powder is 10% oil-extended.
[0028] Optionally, the rubber is selected from a mixture of natural rubber or butadiene rubber and one or two solution polymerized styrene-butadiene rubbers; the natural rubber or the butadiene rubber is 10-30 phr, and the solution polymerized styrene-butadiene rubber is 70-90 phr.
[0029] Optionally, the butadiene rubber is neodymium-based butadiene rubber, and the neodymium-based butadiene rubber satisfies: a weight-average molecular weight of 380 kg / mol < Mw < 460 kg / mol.
[0030] Optionally, the solution-polymerized styrene-butadiene rubber is selected from two solution-polymerized styrene-butadiene rubbers, and the solution-polymerized styrene-butadiene rubber 1 needs to meet the following conditions: the percentage S of styrene in the solution-polymerized styrene-butadiene rubber in the solution-polymerized styrene-butadiene rubber meets 30%<S<42%, and the solution-polymerized styrene-butadiene rubber 2 needs to meet the following conditions: the percentage S of styrene in the solution-polymerized styrene-butadiene rubber in the solution-polymerized styrene-butadiene rubber meets S>40%.
[0031] Optionally, the oil absorption value of the white carbon black is 2-3.5cm 3 / g, nitrogen adsorption surface area is 150-170m 2 / g.
[0032] Optionally, the silane coupling agent is bis-[γ-(triethoxysilyl)propyl]tetrasulfide.
[0033] Optionally, the rubber composition further comprises one or more of oil-extended sulfur powder, vulcanization accelerator, zinc oxide, microcrystalline wax, environmentally friendly oil, stearic acid, and antioxidant; optionally, 1.0-2.5 phr of oil-extended sulfur powder, 1.0-5.0 phr of vulcanization accelerator, 1.0-4.0 phr of zinc oxide, 1.0-4.0 phr of microcrystalline wax, 2-10 phr of environmentally friendly oil, 1.5-4.0 phr of stearic acid, and 2.0-5.0 phr of antioxidant;
[0034] Optionally, the antioxidant is selected from TMQ 1.0-2.0 phr, and the antioxidant 6PPD 2.0-4.0 phr; the vulcanization accelerator is selected from accelerator NS, and the oil-extended sulfur powder is 10% oil-extended.
[0035] The present disclosure provides a method for preparing a rubber composition, which is a mixing method, including a mixing stage and a final mixing stage, and includes the following steps:
[0036] Mixing section: adopts tandem internal mixer;
[0037] Add rubber, carbon black W31, white carbon black, and other raw materials except environmentally friendly oil, sulfur, and accelerator to the series upper machine and raise the temperature to between 110-125°C; add environmentally friendly oil and pressurize to raise the temperature to 145-148°C; maintain a constant temperature of 145-148°C for 30-60 seconds to drain the glue;
[0038] In the serial lower computer, after receiving the rubber material from the upper computer, the temperature is raised to 145℃-148℃; the rubber is discharged at a constant temperature of 145℃-148℃ for 120-160 seconds to obtain the masterbatch;
[0039] Final mixing stage: put the masterbatch into the internal mixer, and simultaneously add sulfur and accelerator; pressurize for 30-60 seconds and raise the temperature to 95-105℃; discharge the rubber to obtain the rubber composition.
[0040] The present disclosure provides a mixing method for a rubber composition, the method comprising the following steps:
[0041] Mixing section: adopts tandem internal mixer, and the rotor speed of internal mixer can be controlled at 10-55rpm;
[0042] Series upper computer masterbatch process: add rubber, carbon black W31, white carbon black and other raw materials except sulfur and accelerator, press the top bolt for 30-45 seconds to bring the temperature to between 110-125℃; lift the top bolt, add environmentally friendly oil and pressurize again to 145-148℃; control the constant temperature at 145-148℃ for 30-60 seconds to drain the glue;
[0043] Series lower machine masterbatch process: after receiving the upper machine rubber material, the temperature is raised to 145℃-148℃; the rubber is discharged at 145℃-148℃ under constant temperature control for 120-160 seconds; after the rubber is bonded, a twin-screw extruder is used to produce the sheet to obtain the masterbatch;
[0044] Final mixing section: F370 shear mixer, rotor speed 20-35rpm, all mixers upper bolt pressure 45-60N / cm 2 , the cooling water temperature of the internal mixer is controlled between 30-45℃; the masterbatch obtained from the series internal mixer is accurately weighed and put into the internal mixer, and the corresponding proportion of sulfur and accelerator are simultaneously added; pressurize for 30-60 seconds, lift the top bolt to allow the rubber to turn over; press the top bolt again to raise the temperature to 95-105℃; discharge the rubber to the twin-screw extruder to produce sheets to obtain a rubber composition.
[0045] The present disclosure also provides a tire tread, which is prepared using the rubber composition.
[0046] The present disclosure also provides a tire that is low-noise, low-rolling-resistance, and wear-resistant, wherein the tread of the tire is prepared by vulcanizing the rubber composition.
[0047] Detailed Description of the Invention
[0048] The present invention provides a tread rubber composition that is low in noise, low in rolling resistance and wear-resistant. The rubber composition uses a new type of carbon black reinforcement material to ensure the rolling resistance and physical properties of the rubber composition.
[0049] The modulus of the rubber composition of the present disclosure is adjusted and optimized to determine a suitable modulus to improve the noise performance of the rubber composition, especially the performance on harsh noise roads.
[0050] In some embodiments, the present disclosure provides a rubber composition, wherein the rubber composition may include raw materials of the following components based on 100 parts by weight of the rubber component:
[0051] Optionally, the modified carbon black satisfies: the oil absorption value is between 100-120*10 -5 cm 3 / g, nitrogen adsorption surface area is 70-90m 2 / g, iodine absorption value 80-90g / kg, total specific surface area 75-85*10 3 m 2 / kg, tinting strength 95-110%.
[0052] Optionally, the modified carbon black is carbon black W31, obtained from Jiangxi Black Cat Carbon Black Co., Ltd.
[0053] Optionally, the rubber composition has an M10 of ≤0.5 MPa, an M300 of ≥8.0 MPa, and a shore A hardness of 55-60.
[0054] In some embodiments, the present disclosure provides a tire tread rubber composition that is low-noise, low-rolling-resistance, and wear-resistant. The rubber composition is prepared by mixing raw materials including the following components, based on 100 parts of the rubber component:
[0055] Among them, the modified carbon black uses carbon black W31, produced by Jiangxi Black Cat Carbon Black Co., Ltd., with an oil absorption value of 100-120*10 -5 cm 3 / g, nitrogen adsorption surface area is 70-90m 2 / g, iodine absorption value 80-90g / kg, total specific surface area 75-85*10 3 m 2 / kg, tinting strength 95-110%; and the rubber composition has M10 ≤ 0.5 MPa, M300 ≥ 8.0 MPa, and hardness shore A 55-60.
[0056] Optionally, the rubber composition is prepared by mixing raw materials including the following components based on 100 parts of the rubber component:
[0057] In some optional embodiments, the rubber is selected from a mixture of natural rubber or butadiene rubber and one or two solution polymerized styrene-butadiene rubbers; the natural rubber or butadiene rubber comprises 10-30 phr, and the solution polymerized styrene-butadiene rubber comprises 70-90 phr. For example, the natural rubber or butadiene rubber may comprise 10 phr, 15 phr, 20 phr, 25 phr, or 30 phr, with the remainder being solution polymerized styrene-butadiene rubber.
[0058] For example, the solution polymerized styrene butadiene rubber can be 70 phr, 75 phr, 80 phr, 85 phr, 90 phr, and the rest is natural rubber or butadiene rubber.
[0059] In some optional embodiments, the butadiene rubber is neodymium-based butadiene rubber, and the neodymium-based butadiene rubber satisfies: a weight-average molecular weight of 380 kg / mol < Mw < 460 kg / mol.
[0060] In some optional embodiments, two types of solution-polymerized styrene-butadiene rubber are used in combination, and the solution-polymerized styrene-butadiene rubber 1 must meet the following requirements: the percentage S of styrene in the solution-polymerized styrene-butadiene rubber in the solution-polymerized styrene-butadiene rubber must meet 30%<S<42%; the solution-polymerized styrene-butadiene rubber 2 must meet the following requirements: the percentage S of styrene in the solution-polymerized styrene-butadiene rubber must meet S>40%.
[0061] In some optional embodiments, the oil absorption value of white carbon black is 2-3.5 cm 3 / g, nitrogen adsorption surface area is 150-170m 2 / g.
[0062] In some optional embodiments, the silane coupling agent is bis-[γ-(triethoxysilyl)propyl]tetrasulfide.
[0063] In some optional embodiments, the rubber composition further comprises one or more of oil-extended sulfur powder, vulcanization accelerator, zinc oxide, microcrystalline wax, environmentally friendly oil, stearic acid, and antioxidant; optionally, the oil-extended sulfur powder is 1.0-2.5 phr, the vulcanization accelerator is 1.0-5.0 phr, the zinc oxide is 1.0-4.0 phr, the microcrystalline wax is 1.0-4.0 phr, the environmentally friendly oil is 2-10 phr, the stearic acid is 1.5-4.0 phr, and the antioxidant is 2.0-5.0 phr; optionally, the antioxidant is selected from antioxidant TMQ 1.0-2.0 phr and antioxidant 6PPD 2.0-4.0 phr; the vulcanization accelerator is selected from accelerator NS, and the oil-extended sulfur powder is oil-extended by 10%.
[0064] In some optional embodiments, the method is a mixing method, including a mixing section and a final mixing section, and includes the following steps:
[0065] Mixing section: adopts tandem internal mixer;
[0066] Add rubber, carbon black W31, white carbon black, and other raw materials except environmentally friendly oil, sulfur, and accelerator to the tandem upper machine and raise the temperature to between 110-125°C. Add environmentally friendly oil and pressurize until the temperature reaches 145-148°C. Maintain a constant temperature of 145-148°C for 30-60 seconds to drain the glue.
[0067] In the serial lower computer, after receiving the rubber material from the upper computer, the temperature is raised to 145℃-148℃; the rubber is discharged at a constant temperature of 145℃-148℃ for 120-160 seconds to obtain the masterbatch;
[0068] Final mixing stage: put the masterbatch into the internal mixer, and simultaneously add sulfur and accelerator; pressurize for 30-60 seconds and raise the temperature to 95-105°C; discharge the masterbatch to obtain the rubber composition. The present disclosure also provides a mixing method for the rubber composition, which includes the following steps:
[0069] 1) Mixing section: adopts tandem internal mixer, and the rotor speed of internal mixer can be controlled at 10-55rpm;
[0070] Series upper computer masterbatch process: add rubber, carbon black W31, white carbon black and other raw materials except sulfur and accelerator, press the top bolt for 30-45 seconds to bring the temperature to between 110-125℃; lift the top bolt, add environmentally friendly oil and pressurize again to 145-148℃; control the constant temperature at 145-148℃ for 30-60 seconds to drain the glue;
[0071] 2) Masterbatch process in series with the lower machine: after receiving the rubber material from the upper machine, the temperature is raised to 145-148°C; the rubber is discharged at a constant temperature of 145-148°C for 120-160 seconds; after the rubber is bonded, a twin-screw extruder is used to produce the sheet to obtain the masterbatch;
[0072] 3) Final mixing section: F370 shear mixer, rotor speed 20-35rpm, all mixers with top bolt pressure 45-60N / cm 2 , the cooling water temperature of the internal mixer is controlled between 30-45℃; the masterbatch obtained from the series internal mixer is accurately weighed and put into the internal mixer, and the corresponding proportion of sulfur and accelerator are simultaneously added; pressurize for 30-60 seconds, lift the top bolt to allow the rubber to turn over; press the top bolt again to raise the temperature to 95-105℃; discharge the rubber to the twin-screw extruder to produce sheets to obtain a rubber composition.
[0073] In some optional embodiments, the present disclosure further provides a tire that is low-noise, low-rolling-resistance, and wear-resistant, wherein the tread of the tire is prepared by vulcanizing the rubber composition.
[0074] The present disclosure adopts the above-mentioned technical solution, and the rubber composition uses a new type of carbon black as a reinforcing material to ensure the rolling resistance and physical properties of the rubber composition. Furthermore, through research, it is found that noise is mainly affected by the small strain modulus. The smaller the small strain modulus, the lower the noise, while control is mainly affected by the large strain modulus. The larger the large strain modulus, the better the control. For this reason, the present application adjusts and optimizes the modulus of the rubber composition, determines a suitable modulus, to improve the noise performance of the rubber composition, especially the harsh noise road performance. Example
[0075] The following is a clear and complete description of the technical solutions in the embodiments of the present disclosure. Obviously, the embodiments described are only part of the embodiments of the present disclosure, not all of them. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present disclosure without making any creative efforts are within the scope of protection of the present disclosure.
[0076] The raw materials used in the comparative examples and examples 1-5 are shown in Table 1.
[0077] The rubber compositions in Table 1 were all mixed using the same mixing method, which is as follows:
[0078] 1) Mixing section: adopts tandem internal mixer, and the rotor speed of internal mixer can be controlled at 10-55 rpm (revolutions / min);
[0079] Series upper computer masterbatch process: add rubber, W31 carbon black, white carbon black and other raw materials except environmentally friendly oil, sulfur and accelerator, press the top bolt for 30-45 seconds to bring the temperature to between 110-125℃; lift the top bolt, add environmentally friendly oil and pressurize again to 145-148℃; control the temperature at 145-148℃ for 30-60 seconds to drain the glue;
[0080] The masterbatch process of serial lower machine: after receiving the rubber material from the upper machine, the temperature is raised to 145℃-148℃; the rubber is discharged at 145℃-148℃ under constant temperature control for 120-160 seconds; after the rubber is bonded, a twin-screw extruder is used to produce the sheet to obtain the masterbatch;
[0081] 2) Final mixing section: F370 shear mixer is used, the rotor speed is controllable at 20-35rpm, and the top bolt pressure on all mixers is 45-60N / cm 2 , the cooling water temperature of the internal mixer is controlled between 30-45℃; the masterbatch obtained from the tandem internal mixer is accurately weighed and fed into the F370 internal mixer, and sulfur and accelerator in corresponding proportions are simultaneously fed into the mixer; pressurize for 30-60 seconds, lift the top bolt to allow the rubber to flip; press the top bolt again to raise the temperature to 95-105℃; discharge the rubber to the twin-screw extruder to produce sheets to obtain the rubber composition.
[0082] The physical properties of the tread rubber composition are measured according to the general method of the national standard.
[0083] Tire noise testing: Objective testing using the Siemens LMS sound and vibration acquisition system
[0084] Tire wear test: Taxi road tests in Hangzhou. After driving 60,000 kilometers, the tires are recycled and the actual tire wear is estimated based on the wear conditions.
[0085] Tire rolling resistance and noise testing: Tire rolling resistance is tested according to ISO2850. In the table, the rolling resistance and noise results of Comparative Example 1 are set as 100, and the tires in other groups are scored according to the percentage of Comparative Example 1; the higher the score, the better the performance.
[0086] Table 1 Comparison of the formulation and performance tests of the comparative example and Examples 1-5
[0087] The sources of the raw materials in Table 1 are as follows:
[0088] Natural rubber: Vietnamese product
[0089] Solution Polystyrene Butadiene Rubber 1: LG Chemical Co., Ltd., oil-extended 37.5phr, the percentage of styrene in solution polystyrene butadiene rubber (S) satisfies 30%<S<42%;
[0090] Solution Polystyrene Butadiene Rubber 2: Product of Zeon Corporation, oil-extended 25phr, the percentage of styrene in solution polystyrene butadiene rubber (S) satisfies S>40%;
[0091] Neodymium-based butadiene: a product of Synthos, Poland, with a weight-average molecular weight of 380 kg / mol<Mw<460 kg / mol;
[0092] N234 carbon black: product of Shanghai Carbon Chemical Co., Ltd.
[0093] W31 carbon black: a product of Jiangxi Black Cat Carbon Black Co., Ltd., with an oil absorption value of 100-120*10 -5 cm 3 / g, nitrogen adsorption surface area is 70-90m 2 / g, iodine absorption value 80-90g / kg, total specific surface area 75-85*10 3 m 2 / kg, tinting strength 95-110%;
[0094] White carbon black: a product of Fujian Sanming Zhengyuan Chemical Co., Ltd., the oil absorption value of white carbon black is 2-3.5cm 3 / g, nitrogen adsorption surface area is 150-170m 2 / g;
[0095] Bis-[γ-(triethoxysilyl)propyl]tetrasulfide: product of Jiangxi Hongbai New Materials Co., Ltd.
[0096] α-Methylstyrene resin: a product of Kraton Chemical Company, with a molecular weight distribution satisfying 4<Mw / Mn<5;
[0097] Other undeclared raw materials are purchased from the market.
[0098] The above is a description of the embodiments of the present disclosure. Through the above description of the disclosed embodiments, professionals and technicians in this field can implement or use the present disclosure. Various modifications to these embodiments will be apparent to professionals and technicians in this field. The general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present disclosure. Therefore, the present disclosure will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel points disclosed herein. Industrial Applicability
[0099] The present disclosure provides a tire tread rubber composition that combines low noise, low rolling resistance, and wear resistance. The rubber composition is prepared by mixing the following raw materials, based on 100 parts of the rubber component: 100 phr of rubber; 30-80 phr of modified carbon black; 0-50 phr of white carbon black; 0-5.0 phr of silane coupling agent; 2.0-15 phr of α-methylstyrene resin; the modified carbon black is carbon black W31. The rubber composition of the present disclosure uses a new type of carbon black reinforcement material to ensure the rolling resistance and physical properties of the rubber composition. The modulus of the rubber composition is adjusted and optimized to determine a suitable modulus to improve the noise performance of the rubber composition, especially the performance on harsh noise roads, and has excellent industrial applicability.
Claims
1. A rubber composition, characterized in that: The rubber composition comprises the following raw materials based on 100 parts by weight of the rubber component:
2. The rubber composition according to claim 1, wherein The modified carbon black satisfies: The oil absorption value is between 100-120*10 -5 cm 3 / g, nitrogen adsorption surface area is 70-90m 2 / g, iodine absorption value 80-90g / kg, total specific surface area 75-85*10 3 m 2 / kg, color strength 95-110%; Optionally, the rubber composition has M10 ≤ 0.5 MPa and M300 ≥ 8.0 MPa; Optionally, the rubber composition has a shore A hardness of 55-62, and optionally, a shore A hardness of 55-60.
3. A tire tread rubber composition having low noise, low rolling resistance and wear resistance, characterized in that: The rubber composition is prepared by mixing raw materials including the following components based on 100 parts of the rubber component: The modified carbon black is carbon black W31, produced by Jiangxi Black Cat Carbon Black Co., Ltd., with an oil absorption value of 100-120*10 -5 cm 3 / g, nitrogen adsorption surface area is 70-90m 2 / g, iodine absorption value 80-90g / kg, total specific surface area 75-85*10 3 m 2 / kg, tinting strength 95-110%; and the M10 of the rubber composition meets ≤0.5Mpa, M300 ≥8.0Mpa, and the hardness shore A meets 55-60.
4. The rubber composition according to any one of claims 1 to 3, characterized in that The rubber composition is prepared by mixing raw materials including the following components based on 100 parts of the rubber component:
5. The rubber composition according to any one of claims 1 to 4, characterized in that The rubber is selected from a mixture of natural rubber or butadiene rubber and one or two solution-polymerized styrene-butadiene rubbers; Optionally, in the mixture, natural rubber or butadiene rubber is 10-30 phr, and solution-polymerized styrene-butadiene rubber is 70-90 phr; Optionally, the butadiene rubber is neodymium-based butadiene rubber; Optionally, the neodymium-based butadiene rubber satisfies: a weight average molecular weight of 380 kg / mol<Mw<460 kg / mol; Optionally, the solution polymerized styrene butadiene rubber is selected from two solution polymerized styrene butadiene rubbers, and the solution polymerized styrene butadiene rubber must meet the following requirements: The percentage S of styrene in the solution polymerized styrene butadiene rubber satisfies 30%<S<42%; the solution polymerized styrene butadiene 2 rubber must satisfy: the percentage S of styrene in the solution polymerized styrene butadiene rubber satisfies S>40%.
6. The rubber composition according to any one of claims 1 to 5, characterized in that The rubber composition further comprises one or more of oil-extended sulfur powder, a vulcanization accelerator, zinc oxide, microcrystalline wax, environmentally friendly oil, stearic acid, and an antioxidant; Optionally, the oil-extended sulfur powder 1.0-2.5 phr, vulcanization accelerator 1.0-5.0 phr, zinc oxide 1.0-4.0 phr, microcrystalline wax 1.0-4.0 phr, environmentally friendly oil 2-10 phr, stearic acid 1.5-4.0 phr and antioxidant 2.0-5.0 phr; Optionally, the antioxidant is antioxidant TMQ or antioxidant 6PPD; Optionally, the antioxidant is antioxidant TMQ 1.0-2.0phr, antioxidant 6PPD 2.0-4.0phr; Optionally, the vulcanization accelerator is accelerator NS, and the oil-filled sulfur powder is 10% oil-filled.
7. The rubber composition according to any one of claims 1 to 6, characterized in that The rubber is selected from a mixture of natural rubber or butadiene rubber and one or two solution polymerized styrene-butadiene rubbers; the natural rubber or the butadiene rubber is 10-30 phr, and the solution polymerized styrene-butadiene rubber is 70-90 phr.
8. The rubber composition according to any one of claims 1 to 7, characterized in that The butadiene rubber is neodymium-based butadiene rubber, and the neodymium-based butadiene rubber satisfies: a weight average molecular weight of 380kg / mol<Mw<460kg / mol.
9. The rubber composition according to any one of claims 1 to 8, characterized in that The solution polymerized styrene butadiene rubber is selected from two solution polymerized styrene butadiene rubbers, the solution polymerized styrene butadiene 1 rubber needs to satisfy: the percentage S of styrene in the solution polymerized styrene butadiene rubber to the solution polymerized styrene butadiene rubber meets 30%<S<42%, and the solution polymerized styrene butadiene 2 rubber needs to satisfy: the percentage S of styrene in the solution polymerized styrene butadiene rubber to the solution polymerized styrene butadiene rubber meets S>40%.
10. The rubber composition according to any one of claims 1 to 9, characterized in that The oil absorption value of the white carbon black is between 2 and 3.5 cm 3 / g, nitrogen adsorption surface area is 150-170m 2 / g.
11. The rubber composition according to any one of claims 1 to 10, characterized in that The silane coupling agent is bis-[γ-(triethoxysilyl)propyl]tetrasulfide.
12. The rubber composition according to any one of claims 1 to 11, characterized in that The rubber composition further comprises one or more of oil-extended sulfur powder, vulcanization accelerator, zinc oxide, microcrystalline wax, environmentally friendly oil, stearic acid, and antioxidant; optionally, 1.0-2.5 phr of oil-extended sulfur powder, 1.0-5.0 phr of vulcanization accelerator, 1.0-4.0 phr of zinc oxide, 1.0-4.0 phr of microcrystalline wax, 2-10 phr of environmentally friendly oil, 1.5-4.0 phr of stearic acid, and 2.0-5.0 phr of antioxidant; Optionally, the antioxidant is selected from TMQ 1.0-2.0phr, and the antioxidant 6PPD 2.0-4.0phr; the vulcanization accelerator is selected from accelerator NS, and the oil-extended sulfur powder is 10% oil-extended.
13. A method for preparing a rubber composition according to any one of claims 1 to 12, wherein the method is a mixing method, comprising a mixing section and a final mixing section, and comprising the following steps: Mixing section: using tandem internal mixer; In the serial upper machine, add rubber, carbon black W31, white carbon black and other raw materials except environmentally friendly oil, sulfur and accelerator, and make the temperature reach between 110-125℃; add environmentally friendly oil and pressurize to make the temperature reach 145℃-148℃; control the temperature at 145℃-148℃ for 30-60 seconds to drain the glue; In the serial lower machine, after receiving the rubber material from the upper machine, the temperature is raised to 145℃-148℃; the rubber is discharged at a constant temperature of 145℃-148℃ for 120-160 seconds to obtain the masterbatch; Final mixing stage: put the masterbatch into the internal mixer, and simultaneously add sulfur and accelerator; pressurize for 30-60 seconds and raise the temperature to 95-105℃; discharge the masterbatch to obtain the rubber composition.
14. A method for mixing a rubber composition according to any one of claims 1 to 12, the method comprising the following steps: Mixing section: adopts tandem internal mixer, the rotor speed of internal mixer can be controlled at 10-55rpm; Series upper computer masterbatch process: add rubber, carbon black W31, white carbon black and other raw materials except sulfur and accelerator, press the top bolt for 30-45 seconds to make the temperature reach between 110-125℃; lift the top bolt, add environmentally friendly oil and pressurize again to 145℃-148℃; control the constant temperature at 145℃-148℃ for 30-60 seconds to discharge the glue; The process of connecting the lower machine masterbatch in series: after receiving the rubber material from the upper machine, the temperature is raised to 145℃-148℃; the rubber is discharged at a constant temperature of 145℃-148℃ for 120-160 seconds; after the rubber is bonded, a twin-screw extruder is used to produce the sheet to obtain the masterbatch; Final mixing section: F370 shear mixer, rotor speed 20-35rpm, top bolt pressure 45-60N / cm 2 , the cooling water temperature of the internal mixer is controlled between 30-45℃; the masterbatch obtained from the series internal mixer is accurately weighed and put into the internal mixer, and the corresponding proportion of sulfur and accelerator are simultaneously added; pressurize for 30-60 seconds, lift the top bolt to let the rubber compound turn over; press the top bolt again to raise the temperature to 95-105℃; discharge the rubber to the twin-screw extruder to produce sheets to obtain a rubber composition.
15. A tire tread, prepared using the rubber composition according to any one of claims 1 to 12.
16. A tire with low noise, low rolling resistance and wear resistance, characterized in that: The tread of the tire is prepared by vulcanizing the rubber composition described in any one of claims 1 to 12.
Citation Information
Patent Citations
Tire tread rubber with ultra-low rolling resistance and ultra-high wet grapping performance and preparation method thereof and tire
CN106750668A
High-performance tire tread rubber material, preparation method thereof and tire
CN109134978A
Rubber composition for tire tread and tire including same
CN110317376A
Tire with low rolling resistance, high wet grabbing and good controllability
CN115124773A
Electric vehicle tire tread rubber composition, mixing method thereof and tire
CN115584068A
Cited By
Rubber magnet with self-repairing function and preparation method thereof
CN122325859A