Coordinated recovery method for waste lithium ion battery material and high-grade nickel matte
Through the coordinated roasting process of waste lithium-ion battery materials and high ice nickel, the problems of low lithium element extraction rate and complex process of high ice nickel preparation of nickel sulfate in lithium-ion battery materials recycling are solved, and efficient separation of lithium and valuable metals is achieved, and the process flow is simplified. And reduces costs and is suitable for large-scale production.
Patent Information
- Application Number
- PCT/CN2023/127623
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2023-10-30
- Publication Date
- 2024-11-28
AI Technical Summary
The prior art has problems such as low extraction rate of lithium element, complex process, high safety risks, high cost and waste of resources in the recycling of retired lithium-ion battery materials, especially in the process of preparing nickel sulfate with high ice nickel.
Co-rotating process of waste lithium-ion battery materials and high ice nickel is adopted to generate water-soluble lithium sulfate through baking, and convert metals such as nickel, cobalt, manganese, etc. into water-insoluble form. Combined with the atmospheric acid leaching process, lithium is achieved. Priority for extraction and efficient separation.
It realizes efficient separation of more than 92% of lithium and valuable metals, simplifies the process flow, reduces costs, is suitable for the recycling of a variety of retired lithium-ion battery materials, avoids high temperature and high pressure conditions, and is suitable for large-scale production.
Smart Images

Figure CN2023127623_28112024_PF_FP_ABST
Abstract
Description
A method for collaboratively recovering waste lithium-ion battery materials and high-grade nickel matte Technical Field
[0001] The present invention belongs to the field of solid waste recycling and metallurgical technology, and in particular relates to a method for the coordinated recovery of waste lithium-ion battery materials and high-grade nickel matte. Background Art
[0002] In recent years, with the global promotion of electric vehicles, market demand for lithium-ion batteries has rapidly increased. Ternary cathode materials, due to their excellent cycling performance, high conductivity, and high energy density, have become the preferred cathode material for electric vehicle power batteries. The rapid development of the power battery sector has also led to high demand for lithium carbonate and nickel sulfate. On the one hand, the price of battery-grade lithium carbonate has soared from 41,000 yuan / ton in 2019 to 600,000 yuan / ton in 2022. On the other hand, global nickel sulfate demand is projected to increase from 640,000 tons to 3.67 million tons between 2020 and 2035, with the new energy sector, the largest consumer of nickel sulfate, accounting for a share of this increase from 59% to 79%. However, my country's dependence on foreign lithium and nickel resources exceeds 70%. Therefore, developing technologies to recover valuable metals from retired lithium-ion batteries can help alleviate the shortage of lithium and nickel resources.
[0003] In order to give priority to lithium extraction from retired lithium-ion batteries, a combined pyrometallurgical and hydrometallurgical process is currently mainly used. Due to the large differences in the physical and chemical properties of different metal elements, it is difficult to efficiently recover lithium elements from powder waste by simple pyrometallurgy and hydrometallurgy. The combined pyrometallurgical and hydrometallurgical process first selectively converts the lithium in the powder waste into soluble lithium compounds, such as LiCl, Li2CO3, LiNO3, Li2SO4, LiOH, etc., while other metals such as nickel, cobalt, and manganese form water-insoluble metal elements or oxides during the roasting process. For the leached residue after lithium extraction, inorganic acid and hydrogen peroxide are generally used to leach and recover the remaining metal elements. This method avoids the loss of lithium caused by traditional pyrometallurgical processes, and greatly reduces the generation of wastewater and acidic waste compared to hydrometallurgical processes.
[0004] Nickel matte is an intermediate product from the pyrometallurgical smelting of nickel ore. Traditionally, nickel sulfate is produced from nickel matte using staged pressurized acid leaching. However, this process requires high equipment requirements, consumes a lot of energy, produces a wide variety of impurity ions in the leachate, and poses certain safety risks. The common process of dissolving nickel metal in sulfuric acid and producing nickel sulfate by evaporation and crystallization is complex, resulting in excessively high costs for nickel sulfate. Therefore, it is necessary to develop a low-cost, easy-to-operate, and easily industrializable method for preparing nickel sulfate to achieve the rational utilization of nickel matte resources.
[0005] Chinese patent CN112111651B discloses a pyrometallurgical process for recovering valuable metals from retired lithium-ion batteries using sulfate for sulfation and roasting. The process involves mixing powdered waste with sulfate and roasting it to convert lithium into lithium sulfate. The lithium sulfate is then converted to lithium carbonate or lithium bicarbonate by leaching it with alkali and introducing carbon dioxide. The lithium carbonate is then evaporated to obtain the lithium carbonate, and the leached residue is further leached with sulfuric acid. While this method can selectively leach lithium, the sulfate used contains sodium or potassium ions, making separation difficult and affecting the purity of the lithium carbonate.
[0006] Chinese patent CN114574705A discloses a method for separating lithium and valuable metals from powdered waste materials containing positive and negative electrodes of retired ternary lithium-ion batteries using concentrated sulfuric acid for sulfation roasting. The method mainly involves mixing the positive and negative electrode powders with a certain amount of sulfuric acid and deionized water, drying them, and then ball milling them. The mixture is then roasted under an inert atmosphere to convert the lithium into lithium sulfate. The lithium-containing aqueous solution is then obtained by water immersion, and after impurity removal, it is used to prepare high-purity lithium carbonate. Although this method achieves preferential lithium extraction, concentrated sulfuric acid is used during the roasting and aging process. The amount of concentrated sulfuric acid used affects the lithium extraction rate. The sulfuric acid and powder are easily mixed unevenly during the mixing process, and high requirements are placed on the corrosion resistance of the device, posing certain safety risks.
[0007] Chinese patent application CN114959252A discloses a method for producing nickel sulfate by oxidative roasting of high nickel matte. It oxidatively roasts high nickel matte to convert the metal elements therein into oxides. The roasted product is sequentially leached with sulfuric acid, subjected to multi-stage impurity removal, and concentrated crystallization to obtain a nickel sulfate product. This method realizes the process technology of directly producing nickel sulfate from high nickel matte, so that nickel disulfide is roasted to form oxides, which can be better applied to wet processes of different systems. Although this method has strong properties, it will produce acidic tail gas and wastewater during the treatment process, resulting in a waste of resources, and improper handling will also pose a risk of environmental pollution.
[0008] Chinese patent application CN114892001A discloses a three-stage leaching process for producing nickel sulfate from high-grade nickel matte. This process involves atmospheric pressure leaching, a first oxygen pressure leaching process with gradually increasing temperature and pressure, and a second oxygen pressure leaching process, effectively separating the nickel. This method converts sulfur into sulfate ions during the oxygen pressure leaching process, without generating harmful gases. However, the process involves numerous steps, making it difficult to operate and reduce costs.
[0009] Summary of the Invention
[0010] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a method for the coordinated recovery of waste lithium-ion battery materials and high-grade nickel matte.
[0011] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0012] A method for collaboratively recovering waste lithium-ion battery materials and high-grade nickel matte comprises the following steps:
[0013] (1) mixing waste lithium-ion battery materials with high nickel matte to obtain a mixture;
[0014] (2) calcining the mixture obtained in step (1) to obtain a co-calcined solid product;
[0015] (3) leaching the solid product obtained in step (2) with deionized water to obtain a lithium-containing aqueous solution and aqueous leaching residue;
[0016] (4) acid dissolving the water-leached residue obtained in step (3) to obtain an acidic leachate; and the leachate is subjected to precipitation, impurity removal, extraction and separation to obtain metal sulfate;
[0017] (5) Purifying the lithium-containing aqueous solution obtained in step (3) to obtain lithium carbonate.
[0018] The present invention proposes a brand-new process method, which realizes the preferential extraction of lithium from retired lithium-ion batteries and the preparation of nickel sulfate by atmospheric pressure acid leaching of high-pressure nickel matte. After coordinated roasting, the lithium is selectively reacted to generate lithium sulfate that is easily soluble in water, and the nickel, cobalt, manganese, aluminum, copper and other metals contained in the lithium battery are converted into a water-insoluble form.
[0019] Preferably, the waste lithium-ion battery material in step (1) has a lithium content of 1 to 7 wt%.
[0020] Preferably, the waste lithium-ion battery material is a retired lithium-ion battery positive electrode material or a mixed powder of positive / negative electrode materials, and the retired lithium-ion battery positive electrode material or the positive / negative electrode material contains lithium and one or more of graphite, manganese, nickel, cobalt, copper, aluminum, phosphorus or fluorine.
[0021] Furthermore, the retired lithium-ion battery positive electrode material or positive / negative electrode material is one or more of lithium cobalt oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide.
[0022] Preferably, the nickel matte in step (1) is an intermediate product nickel matte produced in the nickel metallurgical production process, and the nickel matte contains the main elements Ni, S and one or more other metal elements of Cu, Fe or Co.
[0023] Preferably, the high nickel matte in step (1) includes nickel sulfide as a main component and one or more valuable metals such as copper, cobalt or iron, with a nickel content of 40 to 70 wt% and a sulfur content of 20 to 35 wt%.
[0024] Preferably, the molar ratio of Li in the waste lithium-ion battery material and S in the high nickel matte in step (1) is 2:1 to 2:3.
[0025] Preferably, the calcination temperature in step (2) is 550-750° C., and the calcination time is 0.5-3 h.
[0026] Preferably, the mixture is laid with a thickness of 3 mm to 30 mm during the roasting process.
[0027] Preferably, the deionized water in step (3) is mixed with the solid product obtained by roasting at a solid-liquid ratio of 1:3 to 1:10 g / mL, the water immersion temperature is 20 to 90° C., and the leaching time is 0.5 to 3 h.
[0028] Preferably, the solution used in the acid leaching in step (4) is one or more of sulfuric acid, hydrochloric acid or nitric acid, and the acid solution [H + ] concentration is greater than 0.1 mol / L, the water leaching residue and the acid leaching solution are mixed at a solid-liquid ratio of 1:5 to 1:20 g / mL, the acid leaching temperature is 20 to 90° C., and the leaching time is 0.5 to 3 h.
[0029] Furthermore, the metal sulfate is one or more of nickel sulfate, cobalt sulfate or manganese sulfate.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The present invention uses high-grade nickel matte to co-roast retired lithium-ion battery powder waste, which simply and efficiently achieves a lithium leaching rate of more than 92% and efficient separation of valuable metals, providing a guarantee for the subsequent preparation of high-purity lithium carbonate and battery-grade nickel / cobalt / manganese sulfate.
[0032] (2) The present invention uses nickel matte as an additive, based on the fact that the metal elements in the powdered waste of retired lithium-ion batteries are almost identical to the common impurity metals (cobalt, copper, iron, aluminum, etc.) in the nickel matte raw material. By controlling appropriate conditions, the nickel, cobalt, manganese, and copper in the powdered waste are converted into corresponding metal oxides or metals, and the nickel sulfide in the nickel matte is converted into nickel oxide after roasting. This innovatively achieves the coupling of the atmospheric pressure acid leaching process of retired lithium-ion batteries and the valuable metals in the nickel matte.
[0033] (3) The present invention converts the lithium in the raw material into a soluble substance under appropriate conditions by means of coordinated roasting, so as to preferentially extract the lithium element in the subsequent water leaching process; this technology can separate lithium from other metal elements, thereby making the subsequent acid leaching treatment more efficient.
[0034] (4) The process of the present invention has strong adaptability to raw materials and is suitable for the recovery of a variety of retired lithium-ion battery materials; the process is simple and easy to implement, and the loss of valuable metals during the recovery process is small, providing a reliable technical guarantee for the large-scale and efficient recovery of valuable metals in retired lithium-ion batteries.
[0035] (5) The advantages of the present invention are that it avoids the high temperature and high pressure acid leaching conditions required by the traditional process of preparing nickel sulfate from high-grade nickel matte, realizes the coupling of the recovery of nickel, cobalt and manganese in the leaching residue after preferential lithium extraction and the recovery process of nickel in high-grade nickel matte, and opens up a new and efficient process technology of high-grade nickel matte-assisted preferential lithium extraction and direct production of short-range efficient leaching, which is suitable for large-scale process production and has broad application value and development prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0037] FIG1 is a process flow chart of comprehensive recovery of valuable metals from in-service lithium-ion battery powder waste in an embodiment of the present invention. DETAILED DESCRIPTION
[0038] To facilitate understanding of the present invention, the present invention will be described in more comprehensive and detailed form below in conjunction with the accompanying drawings and preferred embodiments. However, the protection scope of the present invention is not limited to the following specific embodiments.
[0039] Unless otherwise defined, all technical terms used hereinafter have the same meanings as those generally understood by those skilled in the art. The technical terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0040] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0041] Example 1:
[0042] A method for the coordinated recovery of waste lithium-ion battery materials and high-grade nickel matte, the process flow diagram of which is shown in FIG1 , comprises the following steps:
[0043] (1) 5 g of retired lithium-ion battery powder waste (lithium content 3%) and 2.6 g of high-sulfur nickel matte (sulfur content 26%) were mixed in a molar ratio of n(Li):n(S)=1:1, stirred thoroughly and spread evenly in an alumina crucible with a material layer thickness of 10 mm. The alumina crucible was placed in a high-temperature furnace and co-calcined in an air atmosphere with an air flow rate of 600 mL / min in the furnace, a reaction temperature of 600°C, and a reaction time of 120 min to obtain a solid product.
[0044] (2) The solid product obtained in step (1) was subjected to water leaching at a leaching temperature of 50° C., a leaching time of 0.5 h, and a solid-liquid ratio of 1:5 (g / mL) to obtain a lithium-containing water leaching solution and leaching residue.
[0045] (3) The lithium-containing aqueous solution obtained in step (2) is evaporated and concentrated, and the pH value of the aqueous solution is adjusted to 11 with a 2 mol / L NaOH solution, and impurities are removed by precipitation to obtain impurity-removed residue and impurity-removed liquid.
[0046] (4) directly leaching the leached residue obtained in step (2) and the impurity-removed residue obtained in step (3) with a sulfuric acid solution, dissolving the filter residue to obtain an acidic leachate.
[0047] (5) The impurity-removed liquid obtained in step (3) is added to a saturated Na2CO3 solution (the molar amount of Na2CO3 is approximately twice the molar amount of lithium element in the raw material) to precipitate Li2CO3, which is filtered to obtain solid Li2CO3. The solid Li2CO3 is washed with hot water to remove residual sodium ions to obtain lithium carbonate with a purity greater than 99.5%.
[0048] (6) The nickel, cobalt and manganese-containing leaching solution obtained in step (4) is subjected to deep purification steps such as extraction and stripping to obtain battery-grade nickel / cobalt / manganese sulfate, which can be used for the preparation of ternary precursors.
[0049] According to calculation, the lithium leaching rate in this embodiment reaches 93.40%, and the leaching rates of nickel, cobalt and manganese in the acidic leaching solution reach 99.99%, 99.81% and 99.94% respectively.
[0050] Example 2:
[0051] A method for the coordinated recovery of waste lithium-ion battery materials and high-grade nickel matte, the process flow diagram of which is shown in FIG1 , comprises the following steps:
[0052] (1) 5 g of retired lithium-ion battery powder waste (lithium content 5%) and 3.9 g of high-sulfur nickel matte (sulfur content 26%) were mixed in a molar ratio of n(Li):n(S) = 2:1.5, stirred thoroughly and spread evenly in an alumina crucible with a material layer thickness of 5 mm. The alumina crucible was placed in a high-temperature furnace and co-calcined in an air atmosphere with an air flow rate of 600 mL / min in the furnace, a reaction temperature of 650°C, and a reaction time of 180 min to obtain a solid product.
[0053] (2) The solid product obtained in step (1) was subjected to water leaching at a leaching temperature of 25° C., a leaching time of 1 h, and a solid-liquid ratio of 1:5 (g / mL) to obtain a lithium-containing water leaching solution and leaching residue.
[0054] (3) The lithium-containing aqueous solution obtained in step (2) is evaporated and concentrated, and the pH value of the aqueous solution is adjusted to 11 with a 2 mol / L NaOH solution, and impurities are removed by precipitation to obtain impurity-removed residue and impurity-removed liquid.
[0055] (4) directly leaching the leached residue obtained in step (2) and the impurity-removed residue obtained in step (3) with a sulfuric acid solution, dissolving the filter residue to obtain an acidic leachate.
[0056] (5) The impurity-removed liquid obtained in step (3) is added to a saturated Na2CO3 solution (the molar amount of Na2CO3 is approximately twice the molar amount of lithium element in the raw material) to precipitate Li2CO3, which is filtered to obtain solid Li2CO3. The solid Li2CO3 is washed with hot water to remove residual sodium ions to obtain lithium carbonate with a purity greater than 99.5%.
[0057] (6) The nickel, cobalt and manganese-containing leaching solution obtained in step (3) is subjected to deep purification steps such as extraction and stripping to obtain battery-grade nickel / cobalt / manganese sulfate, which can be used for the preparation of ternary precursors.
[0058] According to calculation, the leaching rate of lithium in this embodiment reaches 92.63%, and the leaching rates of nickel, cobalt and manganese in the acidic leaching solution reach 99.86%, 98.11% and 98.26% respectively.
[0059] Example 3:
[0060] A method for the coordinated recovery of waste lithium-ion battery materials and high-grade nickel matte, the process flow diagram of which is shown in FIG1 , comprises the following steps:
[0061] (1) 5 g of retired lithium-ion battery powder waste (lithium content 7%) and 3.7 g of high-sulfur nickel matte (sulfur content 26%) were mixed in a molar ratio of n(Li):n(S)=2:1.2, stirred thoroughly and spread evenly in an alumina crucible with a material layer thickness of 5 mm. The alumina crucible was placed in a high-temperature furnace and co-calcined in an air atmosphere with an air flow rate of 600 mL / min in the furnace, a reaction temperature of 550°C, and a reaction time of 180 min to obtain a solid product.
[0062] (2) The solid product obtained in step (1) was subjected to water leaching at a leaching temperature of 25° C., a leaching time of 0.5 h, and a solid-liquid ratio of 1:10 (g / mL) to obtain a lithium-containing water leaching solution and leaching residue.
[0063] (3) The lithium-containing aqueous solution obtained in step (2) is evaporated and concentrated, and the pH value of the aqueous solution is adjusted to 11 with a 2 mol / L NaOH solution, and impurities are removed by precipitation to obtain impurity-removed residue and impurity-removed liquid.
[0064] (4) directly leaching the leached residue obtained in step (2) and the impurity-removed residue obtained in step (3) with a sulfuric acid solution, dissolving the filter residue to obtain an acidic leachate.
[0065] (5) The impurity-removed liquid obtained in step (3) is added to a saturated Na2CO3 solution (the molar amount of Na2CO3 is approximately twice the molar amount of lithium element in the raw material) to precipitate Li2CO3, which is filtered to obtain solid Li2CO3. The solid Li2CO3 is washed with hot water to remove residual sodium ions to obtain lithium carbonate with a purity greater than 99.5%.
[0066] (6) The nickel, cobalt and manganese-containing leaching solution obtained in step (3) is subjected to deep purification steps such as extraction and stripping to obtain battery-grade nickel / cobalt / manganese sulfate, which can be used for the preparation of ternary precursors.
[0067] According to calculation, the leaching rate of lithium in this embodiment reaches 93.28%, and the leaching rates of nickel, cobalt and manganese in the acidic leaching solution reach 98.28%, 98.23% and 98.69% respectively.
[0068] Example 4:
[0069] A method for the coordinated recovery of waste lithium-ion battery materials and high-grade nickel matte, the process flow diagram of which is shown in FIG1 , comprises the following steps:
[0070] (1) 20 g of retired lithium-ion battery powder waste (lithium content 3%) and 7.9 g of high-sulfur nickel matte (sulfur content 26%) were mixed in a molar ratio of n(Li):n(S)=2:1.5, stirred thoroughly and spread evenly in an alumina crucible with a material layer thickness of 20 mm. The alumina crucible was placed in a high-temperature furnace and co-calcined in an air atmosphere with an air flow rate of 600 mL / min in the furnace, a reaction temperature of 650°C, and a reaction time of 120 min to obtain a solid product.
[0071] (2) The solid product obtained in step (1) was subjected to water leaching at a leaching temperature of 50° C., a leaching time of 0.5 h, and a solid-liquid ratio of 1:5 (g / mL) to obtain a lithium-containing water leaching solution and leaching residue.
[0072] (3) The lithium-containing aqueous solution obtained in step (2) is evaporated and concentrated, and the pH value of the aqueous solution is adjusted to 11 with a 2 mol / L NaOH solution, and impurities are removed by precipitation to obtain impurity-removed residue and impurity-removed liquid.
[0073] (4) directly leaching the leached residue obtained in step (2) and the impurity-removed residue obtained in step (3) with a sulfuric acid solution, dissolving the filter residue to obtain an acidic leachate.
[0074] (5) The impurity-removed liquid obtained in step (3) is added to a saturated Na2CO3 solution (the molar amount of Na2CO3 is approximately twice the molar amount of lithium element in the raw material) to precipitate Li2CO3, which is filtered to obtain solid Li2CO3. The solid Li2CO3 is washed with hot water to remove residual sodium ions to obtain lithium carbonate with a purity greater than 99.5%.
[0075] (6) The nickel, cobalt and manganese-containing leaching solution obtained in step (3) is subjected to deep purification steps such as extraction and stripping to obtain battery-grade nickel / cobalt / manganese sulfate, which can be used for the preparation of ternary precursors.
[0076] According to calculation, the leaching rate of lithium in this embodiment reaches 93.03%, and the leaching rates of nickel, cobalt and manganese in the acidic leaching solution reach 98.86%, 99.14% and 99.72% respectively.
[0077] Example 5:
[0078] A method for the coordinated recovery of waste lithium-ion battery materials and high-grade nickel matte, the process flow diagram of which is shown in FIG1 , comprises the following steps:
[0079] (1) 5 g of retired lithium-ion battery powder waste (lithium content 5%) and 6.6 g of high-sulfur nickel matte (sulfur content 26%) were mixed in a molar ratio of n(Li):n(S)=2:3, stirred thoroughly and spread evenly in an alumina crucible with a material layer thickness of 10 mm. The alumina crucible was placed in a high-temperature furnace and co-calcined in an air atmosphere with an air flow rate of 600 mL / min in the furnace, a reaction temperature of 550°C, and a reaction time of 180 min to obtain a solid product.
[0080] (2) The solid product obtained in step (1) was subjected to water leaching at a leaching temperature of 25° C., a leaching time of 0.5 h, and a solid-liquid ratio of 1:5 (g / mL) to obtain a lithium-containing water leaching solution and leaching residue.
[0081] (3) The lithium-containing aqueous solution obtained in step (2) is evaporated and concentrated, and the pH value of the aqueous solution is adjusted to 11 with a 2 mol / L NaOH solution, and impurities are removed by precipitation to obtain impurity-removed residue and impurity-removed liquid.
[0082] (4) directly leaching the leached residue obtained in step (2) and the impurity-removed residue obtained in step (3) with a sulfuric acid solution, dissolving the filter residue to obtain an acidic leachate.
[0083] (5) The impurity-removed liquid obtained in step (3) is added to a saturated Na2CO3 solution (the molar amount of Na2CO3 is approximately twice the molar amount of lithium element in the raw material) to precipitate Li2CO3, which is filtered to obtain solid Li2CO3. The solid Li2CO3 is washed with hot water to remove residual sodium ions to obtain lithium carbonate with a purity greater than 99.5%.
[0084] (6) The nickel, cobalt and manganese-containing leaching solution obtained in step (3) is subjected to deep purification steps such as extraction and stripping to obtain battery-grade nickel / cobalt / manganese sulfate, which can be used for the preparation of ternary precursors.
[0085] According to calculation, the leaching rate of lithium in this embodiment reaches 92.80%, and the leaching rates of nickel, cobalt and manganese in the acidic leaching solution reach 99.59%, 98.30% and 98.63% respectively.
[0086] Example 6:
[0087] A method for the coordinated recovery of waste lithium-ion battery materials and high-grade nickel matte, the process flow diagram of which is shown in FIG1 , comprises the following steps:
[0088] (1) 5 g of retired lithium-ion battery powder waste (lithium content 3%) and 1.6 g of high-sulfur nickel matte (sulfur content 26%) were mixed in a molar ratio of n(Li):n(S)=2:1.2, stirred thoroughly and spread evenly in an alumina crucible with a material layer thickness of 5 mm. The alumina crucible was placed in a high-temperature furnace and co-calcined in an air atmosphere with an air flow rate of 600 mL / min in the furnace, a reaction temperature of 700°C, and a reaction time of 180 min to obtain a solid product.
[0089] (2) The solid product obtained in step (1) was subjected to water leaching at a leaching temperature of 25° C., a leaching time of 2 h, and a solid-liquid ratio of 1:5 (g / mL) to obtain a lithium-containing water leaching solution and a leaching residue.
[0090] (3) The lithium-containing aqueous solution obtained in step (2) is evaporated and concentrated, and the pH value of the aqueous solution is adjusted to 11 with a 2 mol / L NaOH solution, and impurities are removed by precipitation to obtain impurity-removed residue and impurity-removed liquid.
[0091] (4) directly leaching the leached residue obtained in step (2) and the impurity-removed residue obtained in step (3) with a sulfuric acid solution, dissolving the filter residue to obtain an acidic leachate.
[0092] (5) The impurity-removed liquid obtained in step (3) is added to a saturated Na2CO3 solution (the molar amount of Na2CO3 is approximately twice the molar amount of lithium element in the raw material) to precipitate Li2CO3, which is filtered to obtain solid Li2CO3. The solid Li2CO3 is washed with hot water to remove residual sodium ions to obtain lithium carbonate with a purity greater than 99.5%.
[0093] (6) The nickel, cobalt and manganese-containing leaching solution obtained in step (3) is subjected to deep purification steps such as extraction and stripping to obtain battery-grade nickel / cobalt / manganese sulfate, which can be used for the preparation of ternary precursors.
[0094] According to calculation, the leaching rate of lithium in this embodiment reaches 94.80%, and the leaching rates of nickel, cobalt and manganese in the acidic leaching solution reach 99.59%, 98.00% and 98.63% respectively.
[0095] Comparative Example 1: Calcination time is too long
[0096] (1) 5 g of retired lithium-ion battery powder waste (lithium content 3%) and 2.0 g of high-sulfur nickel matte (sulfur content 26%) were mixed in a molar ratio of n(Li):n(S) = 2:1.5, stirred thoroughly and spread evenly in an alumina crucible with a material layer thickness of 5 mm. The alumina crucible was placed in a high-temperature furnace and co-calcined in an air atmosphere with an air flow rate of 500 mL / min in the furnace, a reaction temperature of 600°C, and a reaction time of 480 min to obtain a solid product.
[0097] (2) The solid product obtained in step (1) is subjected to water leaching at a leaching temperature of 60° C., a leaching time of 1 h, and a solid-liquid ratio of 1:10 (g / mL) to obtain a lithium-containing aqueous leaching solution and leaching residue containing impurity ions such as Ni and Mn.
[0098] (3) The lithium-containing aqueous solution obtained in step (2) is evaporated and concentrated, and the pH value of the aqueous solution is adjusted to 11 with a 2 mol / L NaOH solution, and impurities are removed by precipitation to obtain impurity-removed residue and impurity-removed liquid.
[0099] (4) directly leaching the leached residue obtained in step (2) and the impurity-removed residue obtained in step (3) with a sulfuric acid solution, dissolving the filter residue to obtain an acidic leachate.
[0100] (5) The impurity-removed liquid obtained in step (3) is added to a saturated Na2CO3 solution (the molar amount of Na2CO3 is approximately twice the molar amount of lithium element in the raw material) to precipitate Li2CO3, which is filtered to obtain solid Li2CO3. The solid Li2CO3 is washed with hot water to remove residual sodium ions to obtain lithium carbonate with a purity greater than 99.5%.
[0101] (6) The nickel, cobalt and manganese-containing leaching solution obtained in step (3) is subjected to deep purification steps such as extraction and stripping to obtain battery-grade nickel / cobalt / manganese sulfate, which can be used for the preparation of ternary precursors.
[0102] According to calculation, the leaching rates of lithium, nickel and manganese in the aqueous leaching solution in this comparative example are 92.03%, 5.12% and 10.25%, respectively; the leaching rates of nickel, cobalt and manganese in the acidic leaching solution are 93.89%, 99.66% and 88.54%, respectively.
[0103] During the coordinated roasting process in this comparative example, the roasting time was too long, and some of the Ni and Mn in the raw materials were converted into sulfates during the roasting process and entered the aqueous solution, affecting the lithium separation effect. Therefore, the longer the reaction time, the less well-coupled the entire process flow is, and the selective separation of Li, Ni, Co, and Mn cannot be achieved. At the same time, the ionic composition of the aqueous solution is more complicated, increasing the difficulty of removing impurities from the aqueous solution and reducing the recovery rate of each element.
[0104] Comparative Example 2: Excessive addition of high-grade nickel matte
[0105] (1) 5 g of retired lithium-ion battery powder waste (lithium content 3%) and 5.3 g of high-sulfur nickel matte (sulfur content 26%) were mixed in a molar ratio of n(Li):n(S) = 1:2, stirred thoroughly and spread evenly in an alumina crucible with a material layer thickness of 15 mm. The alumina crucible was placed in a high-temperature furnace and co-calcined in an air atmosphere with an air flow rate of 500 mL / min in the furnace, a reaction temperature of 600 ° C, and a reaction time of 120 min to obtain a solid product.
[0106] (2) The solid product obtained in step (1) is subjected to water leaching at a leaching temperature of 60° C., a leaching time of 1 h, and a solid-liquid ratio of 1:10 (g / mL) to obtain a lithium-containing aqueous leaching solution and leaching residue containing impurity ions such as Ni, Co, and Mn.
[0107] (3) The lithium-containing aqueous solution obtained in step (2) is evaporated and concentrated, and the pH value of the aqueous solution is adjusted to 11 with a 2 mol / L NaOH solution, and impurities are removed by precipitation to obtain impurity-removed residue and impurity-removed liquid.
[0108] (4) directly leaching the leached residue obtained in step (2) and the impurity-removed residue obtained in step (3) with a sulfuric acid solution, dissolving the filter residue to obtain an acidic leachate.
[0109] (5) The impurity-removed liquid obtained in step (3) is added to a saturated Na2CO3 solution (the molar amount of Na2CO3 is approximately twice the molar amount of lithium element in the raw material) to precipitate Li2CO3, which is filtered to obtain solid Li2CO3. The solid Li2CO3 is washed with hot water to remove residual sodium ions to obtain lithium carbonate with a purity greater than 99.5%.
[0110] (6) The nickel, cobalt and manganese-containing leaching solution obtained in step (3) is subjected to deep purification steps such as extraction and stripping to obtain battery-grade nickel / cobalt / manganese sulfate, which can be used for the preparation of ternary precursors.
[0111] Calculations show that the leaching rates of lithium, nickel, cobalt, and manganese in the aqueous leaching solution are 95.90%, 13.93%, 15.29%, and 21.43%, respectively, while the leaching rates of nickel, cobalt, and manganese in the acidic leaching solution are 85.53%, 84.61%, and 77.86%, respectively.
[0112] During the co-roasting process of this comparative example, due to the excessive addition of high-grade nickel matte, some of the Ni, Co, Mn, Al, and Cu in the raw materials were converted into sulfates during the roasting process and entered the water leachate, affecting the separation of lithium. Therefore, the excessive use of high-grade nickel matte prevents the entire process from being well coupled, making it impossible to achieve the selective separation of Li, Ni, Co, and Mn. At the same time, the ionic composition of the water leachate is complicated, increasing the difficulty of removing impurities from the water leachate and reducing the recovery rate of each element.
[0113] Comparative Example 3: Calcination temperature is too low
[0114] (1) 5 g of retired lithium-ion battery powder waste (lithium content 3%) and 2.6 g of high-sulfur nickel matte (sulfur content 26%) were mixed in a molar ratio of n(Li):n(S)=1:1, stirred thoroughly and spread evenly in an alumina crucible with a material layer thickness of 10 mm. The alumina crucible was placed in a high-temperature furnace and co-calcined in an air atmosphere with an air flow rate of 500 mL / min in the furnace, a reaction temperature of 400°C, and a reaction time of 180 min to obtain a solid product.
[0115] (2) The solid product obtained in step (1) was subjected to water leaching at a leaching temperature of 60° C., a leaching time of 1 h, and a solid-liquid ratio of 1:10 (g / mL) to obtain a lithium-containing water leaching solution and leaching residue.
[0116] (3) The lithium-containing aqueous solution obtained in step (2) is evaporated and concentrated, and the pH value of the aqueous solution is adjusted to 11 with a 2 mol / L NaOH solution, and impurities are removed by precipitation to obtain impurity-removed residue and impurity-removed liquid.
[0117] (4) directly leaching the leached residue obtained in step (2) and the impurity-removed residue obtained in step (3) with a sulfuric acid solution, dissolving the filter residue to obtain an acidic leachate.
[0118] (5) The impurity-removed liquid obtained in step (3) is added to a saturated Na2CO3 solution (the molar amount of Na2CO3 is approximately twice the molar amount of lithium element in the raw material) to precipitate Li2CO3, which is filtered to obtain solid Li2CO3. The solid Li2CO3 is washed with hot water to remove residual sodium ions to obtain lithium carbonate with a purity greater than 99.5%.
[0119] (6) The nickel, cobalt and manganese-containing leaching solution obtained in step (3) is subjected to deep purification steps such as extraction and stripping to obtain battery-grade nickel / cobalt / manganese sulfate, which can be used for the preparation of ternary precursors.
[0120] According to calculation, the leaching rate of lithium in this comparative example is 63.82%, and the leaching rates of nickel, cobalt and manganese in the nickel-containing, cobalt-containing and manganese-containing leaching solutions are 99.19%, 98.93% and 99.67% respectively.
[0121] During the co-roasting process in this comparative example, the roasting temperature was low, and the co-roasting effect was weakened, resulting in insufficient reaction between the retired lithium-ion battery powder waste and the high-grade nickel matte. This resulted in a significant reduction in the leaching rate of Li during the water leaching process. The Li that was not leached by water would enter the sulfate solution containing Ni, Co, and Mn during the acid leaching process, reducing the recovery rate of Li. Therefore, the roasting temperature was low, the entire process flow could not achieve good coupling, and it was difficult for the nickel element in the high-grade nickel matte to enter the solution through acid leaching under normal pressure conditions, reducing the recovery rate of each element.
[0122] Comparative Example 4: Material layer thickness is too large
[0123] (1) 30 g of retired lithium-ion battery powder waste (lithium content 3%) and 15.8 g of high-sulfur nickel matte (sulfur content 26%) were mixed in a molar ratio of n(Li):n(S) = 1:1, stirred thoroughly and spread evenly in an alumina crucible with a material layer thickness of 40 mm. The alumina crucible was placed in a high-temperature furnace and co-calcined in an air atmosphere with an air flow rate of 500 mL / min in the furnace, a reaction temperature of 600 ° C, and a reaction time of 180 min to obtain a solid product.
[0124] (2) The solid product obtained in step (1) was subjected to water leaching at a leaching temperature of 60° C., a leaching time of 1 h, and a solid-liquid ratio of 1:10 (g / mL) to obtain a lithium-containing water leaching solution and leaching residue.
[0125] (3) The lithium-containing aqueous solution obtained in step (2) is evaporated and concentrated, and the pH value of the aqueous solution is adjusted to 11 with a 2 mol / L NaOH solution, and impurities are removed by precipitation to obtain impurity-removed residue and impurity-removed liquid.
[0126] (4) directly leaching the leached residue obtained in step (2) and the impurity-removed residue obtained in step (3) with a sulfuric acid solution, dissolving the filter residue to obtain an acidic leachate.
[0127] (5) The impurity-removed liquid obtained in step (3) is added to a saturated Na2CO3 solution (the molar amount of Na2CO3 is approximately twice the molar amount of lithium element in the raw material) to precipitate Li2CO3, which is filtered to obtain solid Li2CO3. The solid Li2CO3 is washed with hot water to remove residual sodium ions to obtain lithium carbonate with a purity greater than 99.5%.
[0128] (6) The nickel, cobalt and manganese-containing leaching solution obtained in step (3) is subjected to deep purification steps such as extraction and stripping to obtain battery-grade nickel / cobalt / manganese sulfate, which can be used for the preparation of ternary precursors.
[0129] According to calculation, the leaching rate of lithium in this comparative example is 61.00%, and the leaching rates of nickel, cobalt and manganese in the nickel-containing, cobalt-containing and manganese-containing leaching solutions are 99.99%, 98.81% and 98.23% respectively.
[0130] During the co-roasting process in this comparative example, the material layer thickness was large, and the co-roasting effect was weakened, resulting in insufficient reaction between the retired lithium-ion battery powder waste and the high-grade nickel matte, which led to a significant reduction in the leaching rate of Li during the water leaching process. The Li that was not leached by water would enter the sulfate solution containing Ni, Co, and Mn during the acid leaching process, reducing the recovery rate of Li. Therefore, the material layer thickness was large, the entire process flow could not achieve good coupling, and it was difficult for the nickel element in the high-grade nickel matte to enter the solution through acid leaching under normal pressure conditions, reducing the recovery rate of each element.
[0131] Comparative Example 5: No coordinated roasting process
[0132] (1) 5 g of retired lithium-ion battery powder waste (lithium content 3%) and 2.6 g of high-sulfur nickel matte (sulfur content 26%) were mixed in a molar ratio of n(Li):n(S) = 1:1, and stirred thoroughly to obtain a solid mixture;
[0133] (2) The solid mixture obtained in step (1) was subjected to water leaching at a leaching temperature of 50° C., a leaching time of 0.5 h, and a solid-liquid ratio of 1:5 (g / mL) to obtain a lithium-containing water leaching solution and leaching residue.
[0134] (3) The lithium-containing aqueous solution obtained in step (2) is evaporated and concentrated, and the pH value of the aqueous solution is adjusted to 11 with a 2 mol / L NaOH solution, and impurities are removed by precipitation to obtain impurity-removed residue and impurity-removed liquid.
[0135] (4) directly leaching the leached residue obtained in step (2) and the impurity-removed residue obtained in step (3) with a sulfuric acid solution, dissolving the filter residue to obtain an acidic leachate.
[0136] (5) The impurity-removed liquid obtained in step (3) is added to a saturated Na2CO3 solution (the molar amount of Na2CO3 is approximately twice the molar amount of lithium element in the raw material) to precipitate Li2CO3, which is filtered to obtain solid Li2CO3. The solid Li2CO3 is washed with hot water to remove residual sodium ions to obtain lithium carbonate with a purity greater than 99.5%.
[0137] (6) The leachate obtained in step (3) is subjected to deep purification steps such as extraction and stripping to obtain battery-grade nickel / cobalt / manganese sulfate, which can be used to prepare ternary precursors. However, due to the presence of a large amount of lithium ions in the acid leachate, an additional step is required to recover the lithium element, which reduces production efficiency and the lithium recovery rate.
[0138] According to calculation, the lithium leaching rate in this embodiment is 0.05%, and the leaching rates of nickel, cobalt and manganese in the acidic leaching solution are 21.24%, 23.11% and 33.44% respectively.
[0139] This comparative example does not have a coordinated roasting process, resulting in no reaction between the retired lithium-ion battery powder waste and the high-grade nickel matte, so that Li is not leached during the water leaching process, but enters the sulfate solution containing Ni, Co, and Mn during the acid leaching process, reducing the recovery rate of Li. At the same time, the lack of a coordinated roasting process also prevents the nickel sulfide in the high-grade nickel matte from reacting, making it difficult to leach in normal pressure acid leaching, resulting in nickel loss. Therefore, the lack of a coordinated roasting process makes the entire process flow unable to be effectively coupled, and affects the acid leaching recovery rate of each element under normal pressure conditions.
Claims
1. A method for the coordinated recovery of waste lithium-ion battery materials and high-grade nickel matte, characterized in that: The steps include: (1) mixing waste lithium-ion battery materials with high nickel matte to obtain a mixture; (2) roasting the mixture obtained in step (1) to obtain a co-roasted solid product; (3) leaching the solid product obtained in step (2) with deionized water to obtain a lithium-containing aqueous solution and aqueous leaching residue; (4) acid dissolving the water-leached residue obtained in step (3) to obtain an acidic leaching solution; and the leaching solution is subjected to precipitation, impurity removal, extraction and separation to obtain metal sulfate; (5) Purifying the lithium-containing aqueous solution obtained in step (3) to obtain lithium carbonate.
2. The method for synergistically recovering waste lithium-ion battery materials and high-grade nickel matte according to claim 1, characterized in that: The waste lithium-ion battery material in step (1) has a lithium content of 1 to 7 wt%.
3. The method for synergistically recovering waste lithium-ion battery materials and high-grade nickel matte according to claim 1, characterized in that: The waste lithium-ion battery material is a retired lithium-ion battery positive electrode material or a mixed powder of positive / negative electrode materials, and the retired lithium-ion battery positive electrode material or the positive / negative electrode material contains lithium and one or more of graphite, manganese, nickel, cobalt, copper, aluminum, phosphorus or fluorine.
4. The method for synergistically recovering waste lithium-ion battery materials and high-grade nickel matte according to claim 1, characterized in that: The nickel matte in step (1) is an intermediate product produced in the nickel metallurgical production process, and the nickel matte contains the main elements Ni, S and one or more of other metal elements such as Cu, Fe or Co.
5. The method for synergistically recovering waste lithium-ion battery materials and high-grade nickel matte according to claim 1, characterized in that: The high-matte nickel in step (1) includes nickel sulfide as a main component and one or more of copper, cobalt or iron valuable metals, with a nickel content of 40 to 70 wt% and a sulfur content of 20 to 35 wt%.
6. The method for synergistically recovering waste lithium-ion battery materials and high-grade nickel matte according to claim 1, characterized in that: The molar ratio of Li in the waste lithium-ion battery material and S in the high nickel matte in step (1) is 2:1 to 2:
3.
7. The method for synergistically recovering waste lithium-ion battery materials and high-grade nickel matte according to claim 1, characterized in that: The calcination temperature in step (2) is 550-750° C. and the calcination time is 0.5-3 h.
8. The method for synergistically recovering waste lithium-ion battery materials and high-grade nickel matte according to claim 1, characterized in that: The mixed material is laid with a thickness of 3 mm to 30 mm during the roasting process.
9. The method for synergistically recovering waste lithium-ion battery materials and high-grade nickel matte according to claim 1, characterized in that: The deionized water in step (3) is mixed with the solid product obtained by roasting at a solid-liquid ratio of 1:3 to 1:10 g / mL, the water immersion temperature is 20 to 90° C., and the leaching time is 0.5 to 3 h.
10. The method for synergistically recovering waste lithium-ion battery materials and high-grade nickel matte according to claim 1, characterized in that: The solution used for the acid leaching in step (4) is one or more of sulfuric acid, hydrochloric acid or nitric acid, and the acid solution [H + ] concentration is greater than 0.1 mol / L, the water leaching residue and the acid leaching solution are mixed at a solid-liquid ratio of 1:5 to 1:20 g / mL, the acid leaching temperature is 20 to 90°C, and the leaching time is 0.5 to 3h.
Citation Information
Patent Citations
Novel technique for comprehensively recovering nickel-cobalt-iron from nickel laterite ore through low-temperature acidification and acidolysis
CN105907949A
Method for recovering valuable metal from waste lithium ion battery material
CN109935922A
Method for preparing ternary positive electrode material through recovering waste ternary lithium battery
CN111206148A
Collaborative recovery method for waste lithium ion battery material and high nickel matte
CN116676493A
Silicon nozzle detachable cornerhera
KR102065923B1
Cited By
Synergistic resource recycling method for zinc hydrometallurgy slag and waste lithium battery positive electrode material
CN121204388A