Conductive material, conductive substrate and composite current collector, and use thereof
By adding nano Ag2S precursor, Ag2Se nanowires and Ag2Te nanowires to the conductive material, a three-dimensional network conductive structure is formed, which solves the problems of large square resistance of the composite fluid collector and low energy volume density of the battery, and realizes the conductivity of the conductive substrate and Improved heat resistance.
Patent Information
- Application Number
- PCT/CN2023/131417
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2023-11-14
- Publication Date
- 2024-11-28
AI Technical Summary
The existing composite fluid collector has a large square resistance and low battery energy and bulk density.
By adding nanoconductive material additives, including nano Ag2S precursors, Ag2Se nanowires and Ag2Te nanowires, an interconnected three-dimensional network conductive structure is formed, which enhances the conductivity and bonding strength of the conductive substrate, reduces square resistance and Improve battery energy bulk density.
It effectively reduces the square resistance of the composite fluid collection, improves the energy volume density of the battery, and improves the heat resistance and thermoelectric properties of the conductive substrate.
Smart Images

Figure PCTCN2023131417-FTAPPB-I100001
Abstract
Description
Conductive materials, conductive substrates, composite current collectors and their applications Technical Field
[0001] The present application belongs to the technical field of conductive materials, and specifically relates to a conductive material, a conductive substrate, a composite current collector and applications thereof, and especially relates to a conductive material, a conductive substrate, a composite current collector, an electrode sheet, a battery and an electrical device. Background Art
[0002] A current collector is a component of a battery, collecting the current generated by the battery's active materials to generate a larger current for external output. Currently, composite current collectors based on polymer membranes are gaining widespread attention and application in the new energy industry.
[0003] The conventional composite current collector preparation process typically involves the following steps: First, a layer of copper or aluminum is deposited on a polymer film using physical vapor deposition methods, such as magnetron sputtering or evaporation, to produce a semi-finished composite current collector with a certain degree of conductivity. This semi-finished composite current collector is then further treated using electroplating to thicken the conductive copper or aluminum layer, thus producing a final composite current collector.
[0004] Compared to traditional copper foil current collectors, polymer film-based composite current collectors offer advantages such as low cost, light weight, and excellent internal insulation. These advantages enable composite current collectors to reduce battery costs and improve battery energy density and safety when used in batteries.
[0005] Composite current collectors based on polymer films have a multilayer structure with copper or aluminum metal layers laminated on both sides of a resin layer. As the battery temperature rises, the temperature of the composite current collector also rises. When the melting point of the resin material is reached, the resin layer melts, breaking the electrode, thereby cutting off the current flow and improving battery safety. However, this approach also increases the current collector's square resistance. The technology related to composite current collectors needs further improvement.
[0006] Summary of the Invention
[0007] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0008] The present application aims to at least partially address one of the technical problems of the prior art. To this end, the present application aims to provide a conductive material, a conductive substrate, a composite current collector, an electrode sheet, a battery, and an electrical device thereof, to address the technical problems of the prior art, such as the large sheet resistance of the composite current collector and the low energy volume density of the battery.
[0009] To solve the above technical problems, the technical solutions of this application are as follows:
[0010] In the first aspect of the present application, a conductive material is provided, comprising a polymer and a nano-conductive material additive, wherein the nano-conductive material additive comprises a nano-Ag2S precursor, Ag2Se nanowires and Ag2Te nanowires. By adding the nano-conductive material additive, the surface roughness of the conductive substrate can be increased, the surface energy difference between the substrate surface and the metal layer surface can be reduced, and ultimately the bonding strength between the metal layer and the substrate can be enhanced. Moreover, none of the three can be missing. The nano-Ag2S particles synthesized from the nano-Ag2S precursor can be mixed with the linear Ag2Se nanowires and Ag2Te nanowires to form a three-dimensional network conductive structure that is interconnected, effectively improving the conductivity of the conductive substrate and reducing the square resistance, so that the square resistance of the obtained composite current collector is reduced and the battery energy volume density is increased. When the content of one of the nano-conductive material additives is significantly increased and the other is missing, the corresponding effect cannot be achieved.
[0011] The conductive material described in this application may further include the following technical features:
[0012] In one embodiment, based on weight parts, the polymer is 83-99 parts, and the nano-conductive material additive is 1-17 parts.
[0013] The content of the nano-conductive material additive should not be too high or too low. If the content of the nano-conductive material additive is too high, it will affect the quality of the film formed when the conductive material forms the conductive substrate. If the content of the nano-conductive material additive is too low, it will not significantly solve the problems of large square resistance and low energy volume density of existing composite current collectors.
[0014] In one embodiment, the weight ratio of the nano Ag2S precursor, the Ag2Se nanowire, and the Ag2Te nanowire is (1-7): (1-7): (1-4), and can be optionally (1.5-5): (1.5-4): (1.5-4). According to an embodiment of the present application, the nano Ag2S precursor, the Ag2Se nanowire, and the Ag2Te nanowire are mixed to form a three-dimensional network conductive structure that is interconnected, which effectively improves the conductivity of the substrate. Under the appropriate weight ratio conditions, the nano conductive material formed by the three increases the surface roughness of the substrate, reduces the surface energy difference between the substrate surface and the metal layer surface, and ultimately enhances the bonding strength between the metal layer and the substrate. It can also enable the substrate to have both good plasticity and thermoelectric properties, which can not only ensure the tensile properties of the substrate while effectively reducing the thermal shrinkage of the substrate, but also effectively improve the heat resistance of the substrate, which is more beneficial to production.
[0015] In one embodiment, the nano-Ag2S precursor is silver N,N-dibutyldithiocarbamate.
[0016] In one embodiment, the Ag2Se nanowires have a diameter of 100-300 nm and a length of 5 μm-30 μm.
[0017] In one embodiment, the Ag2Te nanowires have a diameter of 100-300 nm and a length of 5 μm-30 μm.
[0018] In one embodiment, the polymer is one or a combination of at least two of polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyimide, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene oxide, polystyrene and polyamide.
[0019] The second aspect of the present application provides a conductive substrate obtained by melt-molding the conductive material described in the first aspect of the present application.
[0020] In one embodiment, the nano-Ag2S precursor is used to in-situ synthesize nano-Ag2S particles during the melt molding process. The diameter of the nano-Ag2S particles is 8-30 nm, and the particle size is 40-150 nm.
[0021] A third aspect of the present application provides a composite current collector comprising the conductive substrate described in the second aspect and a metal layer located on at least one side of the conductive substrate.
[0022] In one embodiment, the conductive substrate has a thickness of 1 μm to 8 μm.
[0023] In one embodiment, the metal layer is one or a combination of at least two of titanium, silver, aluminum, nickel, copper, and alloys thereof.
[0024] In one embodiment, the thickness of the metal layer is 500 nm-2000 nm.
[0025] The present application also provides a method for preparing a composite current collector, comprising the following steps:
[0026] At 1400-1800° C., the metal raw material of the metal layer is melted and evaporated, and the atoms of the evaporated metal raw material are cooled and deposited on at least one side surface of the conductive substrate to form the metal layer, thereby obtaining a composite current collector.
[0027] The fourth aspect of the present application further provides an electrode sheet, comprising the composite current collector described in the third aspect, and an active material layer attached to at least one surface of the composite current collector.
[0028] The fifth aspect of the present application further provides a battery, comprising the electrode sheet described in the fourth aspect.
[0029] The sixth aspect of the present application further provides an electrical device comprising the battery described in the fifth aspect.
[0030] The above solution of the present application includes at least the following beneficial effects:
[0031] (1) The conductive material provided in the present application contains a nano-conductive material additive, which includes a nano-Ag2S precursor, Ag2Se nanowires, and Ag2Te nanowires. The nano-Ag2S particles synthesized from the nano-Ag2S precursor can be mixed with the linear Ag2Se nanowires and Ag2Te nanowires to form a three-dimensional network conductive structure that is interconnected, effectively improving the conductivity of the conductive substrate, reducing the square resistance, and reducing the square resistance of the obtained composite current collector and increasing the battery energy volume density. Moreover, when the conductive substrate formed by the provided conductive material is applied as a high molecular polymer film to the composite current collector, the nano-conductive material increases the surface roughness of the conductive substrate, reduces the surface energy difference between the substrate surface and the metal layer surface, and ultimately enhances the bonding strength between the metal layer and the substrate. In addition, the addition of nano-Ag2S particles, Ag2Se nanowires, and Ag2Te nanowires synthesized from nano-Ag2S precursors enables the conductive substrate to have both good plasticity and thermoelectric properties. It can not only effectively reduce the thermal shrinkage of the substrate while ensuring the tensile properties of the substrate, but also effectively improve the heat resistance of the substrate, which is more beneficial to production.
[0032] (2) The conductive substrate provided in the present application, the nano-Ag2S precursor is a precursor for in-situ synthesis of nano-Ag2S particles, and can directly grow on the surface of the Ag2Se nanowires or Ag2Te nanowires during the process of mixing and melting with the Ag2Se nanowires or Ag2Te nanowires. During the growth process, the Ag2S particles can make up for the surface defects of the Ag2Se nanowires or Ag2Te nanowires. In addition, during the heating process, Se and Te can be used to improve the gap defects of Ag, thereby more effectively improving the conductive and heat dissipation performance of the substrate.
[0033] (3) The present invention discloses a method for preparing a conductive substrate, comprising the steps of: uniformly mixing a polymer, polyamide-imide, and a nano-conductive material additive, and melt-molding the mixture to obtain a conductive substrate. The nano-Ag2S precursor in the nano-conductive material can be synthesized in situ during the melt-molding process to form nano-Ag2S particles, eliminating the need for additional synthesis operations and simplifying the process.
[0034] Still other aspects will become apparent upon reading and understanding the detailed description. DETAILED DESCRIPTION
[0035] The embodiments of the present application are described in detail below. The described embodiments are exemplary and intended to be used to explain the present application, but should not be understood as limiting the present application.
[0036] The “many” mentioned in this article includes two, three, four, or more.
[0037] The present application provides a conductive material, including a polymer and a nano-conductive material additive, wherein the nano-conductive material additive includes a nano-Ag2S precursor, Ag2Se nanowires, and Ag2Te nanowires.
[0038] In one embodiment, based on weight parts, the polymer is 83-99 parts and the nano-conductive material additive is 1-17 parts.
[0039] In one embodiment, the weight ratio of the nano-Ag2S precursor, the Ag2Se nanowire, and the Ag2Te nanowire is (1-7):(1-7):(1-4), and can be optionally (1.5-5):(1.5-4):(1.5-4).
[0040] In one embodiment, the weight ratio of the nano-Ag2S precursor, the Ag2Se nanowires, and the Ag2Te nanowires is 2:3:3.
[0041] In one embodiment, the nano-Ag2S precursor is silver N,N-dibutyldithiocarbamate.
[0042] In one embodiment, the Ag2Se nanowires have a diameter of 100-300 nm and a length of 5 μm-30 μm.
[0043] In one embodiment, the Ag2Se nanowires have a diameter of 150-250 nm and a length of 10 μm-20 μm.
[0044] In one embodiment, the Ag2Se nanowires have a diameter of 180-220 nm and a length of 15 μm-18 μm.
[0045] In one embodiment, the Ag2Te nanowires have a diameter of 100-300 nm and a length of 5 μm-30 μm.
[0046] In one embodiment, the Ag2Te nanowires have a diameter of 150-250 nm and a length of 10 μm-20 μm.
[0047] In one embodiment, the Ag2Te nanowires have a diameter of 180-220 nm and a length of 15 μm-18 μm.
[0048] In one embodiment, the polymer is one or more of polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyimide, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene oxide, polystyrene and polyamide.
[0049] In one embodiment, the polymer is polyethylene terephthalate.
[0050] The present application also provides a conductive substrate, which is obtained by melt-molding the above conductive material.
[0051] In one embodiment, the nano-Ag2S precursor is used to in-situ synthesize nano-Ag2S particles during the melt molding process. The diameter of the nano-Ag2S particles is 8-30 nm, and the particle size is 40-150 nm.
[0052] In one embodiment, the diameter of the nano-Ag2S particles is 12-20 nm, and the particle size is 80-120 nm.
[0053] In one embodiment, the diameter of the nano-Ag2S particles is 15-20 nm, and the particle size is 80-100 nm. The diameter refers to the diameter of the equivalent circle of the particle cross section; the particle size refers to the length of the particle.
[0054] The present application also provides a method for preparing the conductive substrate, comprising the following steps: melting and molding the conductive material to obtain a conductive substrate.
[0055] In one embodiment, the method for preparing the conductive substrate comprises the following steps: the conductive material is sequentially subjected to crystallization and drying, melt extrusion, sheet casting, stretching, and heat setting treatment to obtain the conductive substrate.
[0056] In one embodiment, the conductive material is crystallized at 120-220° C. and dried at 150-180° C. for 40-60 minutes and 140-160 minutes, respectively. The crystallization process includes, but is not limited to, being performed in a crystallizer, and the drying process includes, but is not limited to, being performed in a drying tower.
[0057] In one embodiment, the dried product is melt-extruded at 200-350° C. The melting includes but is not limited to being carried out in a twin-screw extruder, and the formed molten material is extruded through a die.
[0058] In one embodiment, the extruded molten material is cast onto a casting roll, and is shaped by the casting roll and water cooling to form a cast sheet.
[0059] In one embodiment, the stretching is biaxial stretching, including longitudinal stretching and transverse stretching.
[0060] In one embodiment, the cast sheet is preheated at 70-150°C (e.g., 90-120°C), and then subjected to longitudinal stretching treatment, the longitudinal stretching temperature is 90-170°C (e.g., 110-150°C), the longitudinal stretching ratio is (3-5):1, and the film is cooled and formed at 20-40°C; then the film is preheated at 70-150°C (e.g., 90-120°C), and then subjected to transverse stretching treatment, the transverse stretching temperature is 90-170°C (e.g., 110-150°C), the transverse stretching ratio is (3-5):1, and the film obtained by transverse stretching is heat-set at 120-250°C (e.g., 140-200°C) and cooled and formed at 20-40°C.
[0061] The nano-Ag2S precursor is any precursor that can be synthesized in situ to have a diameter of 8-30 nm and a particle size of 40-150 nm.
[0062] In one embodiment, the nano-Ag2S precursor, N,N-dibutyldithiocarbamate, can be obtained by conventional techniques in the art, or can be directly purchased commercially.
[0063] In one embodiment, the silver N,N-dibutyldithiocarbamate is obtained by the following method:
[0064] Dissolve (C4H9)2NH and KOH in a 90% to 95% ethanol solution, stir evenly, and then add CS2 in an ice-water bath to obtain a mixed solution;
[0065] The mixed solution was stirred at 15-35° C. for 10-14 h, ethanol and an aqueous solution of AgNO 3 were added thereto, and then stirred at 15-35° C. for 3-5 h to obtain a reaction solution;
[0066] The reaction solution is filtered and separated, and washed alternately with ethanol or deionized water until the filtrate is colorless. The washed product is finally dried to obtain silver N,N-dibutyldithiocarbamate.
[0067] The Ag2Se nanowires can be obtained by methods commonly used in the art, or can be purchased commercially, for example, by thermal evaporation.
[0068] In one embodiment, the Ag2Se nanowires are obtained by the following method: weighing Ag and Se, and suspending and smelting Ag and Se under Ar gas protection to obtain a smelting product; then, placing the smelting product and a quartz substrate coated with Au glue nanoparticles into a quartz tube, and evacuating the tube to seal the tube; adjusting the distance between the smelting product and the quartz substrate in the quartz tube to 40-80 mm, placing the quartz tube in a tube furnace, and heating the tube furnace to 840-880°C at a heating rate of 4-8°C / min, and then heating for 300-460 minutes to obtain the Ag2Se nanowires.
[0069] The Ag2Te nanowires can be obtained by methods commonly used in the art, or purchased commercially.
[0070] In one embodiment, the Ag2Te nanowires in the nano-conductive material additive are obtained by the following method: dissolving AgNO3 and Na2TeO3 in water, adding hydrazine hydrate and ammonia water thereto to obtain a mixed solution; heating the mixed solution to 160-200°C, and then quickly transferring it to a reactor and placing it at 160-200°C for 20-28 hours to obtain Ag2Te nanowires.
[0071] The present application also provides a composite current collector, comprising the conductive substrate and a metal layer located on at least one side of the conductive substrate.
[0072] In one embodiment, the conductive substrate has a thickness of 1 μm to 8 μm.
[0073] In one embodiment, the metal layer is one or a combination of two or more of titanium, silver, aluminum, nickel, copper, and alloys thereof.
[0074] In one embodiment, the thickness of the metal layer is 500 nm-2000 nm.
[0075] The present application also provides a method for preparing a composite current collector, comprising the following steps:
[0076] The metal raw material of the metal layer is melted and evaporated at 1400-1800°C. The evaporated metal raw material atoms are cooled and deposited on at least one surface of the conductive substrate to form the metal layer, thereby obtaining a composite current collector. For example, this can be carried out at 1500-1600°C.
[0077] The present application also provides an electrode sheet, comprising the composite current collector described above, and an active material layer attached to at least one surface of the composite current collector.
[0078] The present application also provides a battery, comprising the electrode sheet described above.
[0079] The present application also provides an electrical device comprising the battery described above.
[0080] In the examples of this application, if no specific conditions are specified, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. Reagents or instruments used without specifying the manufacturer are all commercially available conventional products. The following only provides some of the reagents used in the examples of this application. Raw materials of different manufacturers and models do not affect the implementation of the technical solutions of this application and the achievement of the technical effects.
[0081] It should be noted that, for achieving the purpose of the present application, the polymer is not limited to one of polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyimide, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene oxide, polystyrene, and polyamide, or a combination of two or more thereof. Those skilled in the art can select an appropriate polymer according to actual needs.
[0082] Example 1
[0083] Example 1 provides a conductive material, a conductive substrate, and a composite current collector.
[0084] 1. Nano conductive material additives
[0085] The Ag2S precursor is any precursor that can be synthesized in situ to produce particles with a diameter of 8-30 nm and a particle size of 40-150 nm. Its preparation method includes: first, dissolving 6.46 g of (C4H9)2NH and 2.80 g of potassium hydroxide in 45 mL of anhydrous ethanol and 5 mL of deionized water, stirring vigorously, and then adding 4.56 g of CS2 dropwise to the solution in an ice-water bath. After the dropwise addition is complete, the mixed solution is stirred at room temperature for 12 hours, followed by the addition of 100 mL of ethanol to obtain a preliminary solution. Then, 25 mL of a 2.0 mol / L aqueous AgNO3 solution is slowly added to the preliminary solution, followed by vigorous stirring for 3 hours. During the addition of the AgNO3 solution, the color of the solution first changes from colorless and transparent to light yellow, then gradually deepens, and finally turns orange-yellow. The reaction solution is filtered and separated, and the filtered product is washed alternately with ethanol and deionized water until the filtrate is colorless. Finally, the washed product was dried at 60°C to obtain N,N-dibutyldithiocarbamate silver [(C4H9)2NCS2Ag] powder. The prepared Ag2S precursor had a diameter of approximately 15-20 nm and a particle size of approximately 80-100 nm.
[0086] Ag2Se nanowires were obtained by thermal evaporation, comprising the following steps: a. Analytically pure Ag filaments and Se were smelted to form Ag2Se. The materials were weighed and proportioned according to their composition, followed by suspension melting under Ar gas protection and water cooling in a copper crucible. Because Se has a low melting point and is easily volatile, the Se cake was pressed into a Se cake before melting. The order of melting was to first melt the Ag filament in the crucible, then add the Se cake. After completion, the resulting ingot was flipped and remelted to avoid compositional segregation. b. A quartz substrate coated with Au colloidal nanoparticles and Ag2Se particles were then placed in a quartz tube and sealed with vacuum. After the tube was sealed, the distance between the source and the substrate was adjusted to 60 mm. The source was placed in the higher temperature zone and the substrate in the lower temperature zone. The quartz tube was then placed in a tube furnace and heated to 860°C for 360 minutes at a controlled heating rate of 6°C / min. The resulting Ag2Se nanowires had a diameter of approximately 200 nm and a length of approximately 15 μm.
[0087] The preparation method of Ag2Te nanowires can be any one to prepare nanowires with a diameter of 100-300nm and a length of 5μm-30μm. It includes the following steps: (1) Prepare 2mmol of AgNO3 and 1mmol of Na2TeO3, dissolve them in 30mL of aqueous solution, and then stir for 5 minutes to mix evenly. (2) Use a dropper to take 0.8mL of hydrazine hydrate (80%) and 0.8mL of ammonia water (25%), and quickly drop them into the mixed solution in (1). (3) Heat the vacuum drying oven to 180℃, then quickly transfer the mixed solution in (2) to a high-pressure reactor with a capacity of 30mL, and then place it in the heated vacuum drying oven and keep it for 24 hours. (4) After the reaction is completed, take out the reactor and cool it naturally to room temperature. The diameter of the prepared Ag2Te nanowires is about 200nm and the length is about 15μm.
[0088] 2. Conductive materials
[0089] 2.0 mass% of N,N-dibutyldithiocarbamate silver [(C4H9)2NCS2Ag] powder was blended with 92.0 mass% of polyethylene terephthalate, 3.0 mass% of Ag2Te nanowires, and 3.0 mass% of Ag2Se nanowires to obtain a mixture.
[0090] 3. Preparation of Conductive Substrate
[0091] The film is prepared using a melt-biaxial stretching method, which includes the following steps: crystallization and drying, melt extrusion, sheet casting, longitudinal stretching, transverse stretching, and heat setting. The resulting film has a thickness of 5 microns. During this process, N,N-dibutyldithiocarbamate silver ((C4H9)2NCS2Ag) undergoes thermal decomposition to form nano-Ag2S particles.
[0092] The specific steps include:
[0093] The mixture is sequentially conveyed into a crystallizer and a drying tower for treatment, treated at 180° C. in the crystallizer for 50 min, and dried at 150° C. in the drying tower for 160 min; the dried product is heated to 280° C. in a twin-screw extruder for melting, and the formed molten material is extruded through a die head; the extruded molten material is cast onto a casting roll, and is formed by cooling the casting roll and water cooling to form a casting sheet; the casting sheet is preheated at 90° C., and then subjected to a longitudinal stretching treatment at a longitudinal stretching temperature of 110° C. and a longitudinal stretching ratio of 4:1, and is cooled and formed at 30° C.; the film is preheated at 90° C., and then subjected to a transverse stretching treatment at a transverse stretching temperature of 120° C. and a transverse stretching ratio of 4:1, and the film obtained by transverse stretching is sequentially heat-set at 140° C. and cooled and formed at 30° C. to obtain the corresponding film.
[0094] 4. Preparation of composite current collector
[0095] The prepared film is placed in a vacuum evaporation chamber, and the high-purity copper wire (purity greater than 99.99%) in the metal evaporation chamber is melted and evaporated at a high temperature of 1500°C. The evaporated metal atoms pass through the cooling system in the vacuum coating chamber and are deposited on the two opposite surfaces of the film, forming a copper metal conductive layer with a thickness of 1μm. The thickness of the conductive substrate is 5μm.
[0096] Example 2
[0097] Example 2 provides a conductive material, a conductive substrate, and a composite current collector.
[0098] Example 2 is basically the same as Example 1, with the main difference being that 5.0 mass% N,N-dibutyldithiocarbamate silver [(C4H9)2NCS2Ag] powder is blended with 87.0 mass% polypropylene, 4.0 mass% Ag2Te nanowires, and 4.0 mass% Ag2Se nanowires.
[0099] Example 3
[0100] Example 3 provides a conductive material, a conductive substrate, and a composite current collector.
[0101] Example 3 is basically the same as Example 1, with the main difference being that 1.5 mass% N,N-dibutyldithiocarbamate silver [(C4H9)2NCS2Ag] powder is blended with 95.5 mass% polypropylene, 1.5 mass% Ag2Te nanowires, and 1.5 mass% Ag2Se nanowires.
[0102] Comparative Example 1
[0103] The conductive substrate provided in Comparative Example 1 has the same raw materials and the same preparation method as Example 1, with the only difference being that the nano-conductive material additive is not included.
[0104] Comparative Example 2
[0105] The conductive substrate provided in Comparative Example 2 has the same raw materials and the same preparation method as Example 1, with the only difference being that the nano-conductive material additive does not include Ag2Se nanowires and Ag2Te nanowires.
[0106] Comparative Example 3
[0107] The conductive substrate provided in Comparative Example 3 has the same raw materials and the same preparation method as Example 1, with the only difference being that the nano-conductive material additive does not include Ag2Se nanowires.
[0108] Comparative Example 4
[0109] The conductive substrate provided in Comparative Example 4 has the same raw materials and the same preparation method as Example 1, with the only difference being that the nano-conductive material additive does not include Ag2Te nanowires.
[0110] Effect comparison ratio
[0111] To verify the technical effect of the conductive substrate described in this application, the following tests were conducted:
[0112] The conductive substrates prepared in Examples 1-3 and Comparative Examples 1-4 were tested for thermal shrinkage by heating at 150° C. for 10 minutes according to the method specified in GB / T 10003-2008.
[0113] The conductive substrates prepared in Examples 1-3 and Comparative Examples 1-4 were used to prepare composite current collectors according to the method in Example 1, and the sheet resistance was measured using a four-probe sheet resistance meter.
[0114] The conductive substrates prepared in Examples 1-3 and Comparative Examples 1-4 were formed into 5 μm films. A layer of Permacel P-94 double-sided tape was adhered to a 1 mm thick aluminum foil. The conductive substrate in film form was adhered on top of the double-sided tape. A layer of ethylene acrylic acid copolymer film (DuPont Nurcel 0903, 50 μm thick) was covered on top of the conductive substrate. 5 N / m 2The film was hot-pressed at 120°C for 10 seconds, cooled to room temperature, and cut into 150 mm x 15 mm strips. The ethylene acrylic acid copolymer film strip was secured to the upper fixture of a tensile testing machine, while the remaining strip was secured to the lower fixture. After securing, the two strips were peeled off at an angle of 180° and a speed of 100 mm / min. The peel force was measured to determine the adhesion between the conductive substrate and the polymer base film (ethylene acrylic acid copolymer film).
[0115] After the experiment, the results are shown in Table 1:
[0116] Table 1
[0117] Comparison of Examples 1-3 with Comparative Examples 1-4 reveals that the conductive substrate provided by this application exhibits lower thermal shrinkage and sheet resistance, and significantly improves adhesion to the metal layer. The addition of a nano-Ag2S precursor effectively improves adhesion, while Ag2Se nanowires and Ag2Te nanowires have a certain impact on reducing thermal shrinkage and sheet resistance. When used together, Ag2Se nanowires and Ag2Te nanowires can significantly reduce thermal shrinkage and sheet resistance. Example 1 demonstrates particularly superior performance.
[0118] It is understood from common technical knowledge that the present application may be implemented by other embodiments that do not deviate from its spirit or essential features. Therefore, the embodiments disclosed above are merely illustrative in all respects and are not intended to be exclusive. All modifications that come within the scope of this application or are equivalent to the scope of this application are intended to be included in this application.
Claims
1. A conductive material, comprising: A polymer and a nano-conductive material additive, wherein the nano-conductive material additive comprises a nano-Ag2S precursor, an Ag2Se nanowire and an Ag2Te nanowire; Optionally, based on weight parts, the polymer is 83-99 parts and the nano-conductive material additive is 1-17 parts.
2. The conductive material according to claim 1, wherein The weight ratio of the nano-Ag2S precursor, the Ag2Se nanowire, and the Ag2Te nanowire is (1-7):(1-7):(1-4), and can further be (1.5-5):(1.5-4):(1.5-4); Optionally, the nano-Ag2S precursor is N,N-dibutyldithiocarbamate silver.
3. The conductive material according to claim 2, wherein: The Ag2Se nanowire has a diameter of 100-300 nm and a length of 5 μm-30 μm; Optionally, the Ag2Te nanowire has a diameter of 100-300 nm and a length of 5 μm-30 μm.
4. The conductive material according to claim 1, wherein The polymer is one or a combination of two or more of polypropylene, polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyimide, polypropylene, polyvinyl chloride, polyvinylidene fluoride, polytetrafluoroethylene, polyphenylene sulfide, polyphenylene oxide, polystyrene and polyamide.
5. A conductive substrate obtained by melt-molding the conductive material according to any one of claims 1 to 4, wherein: The nano-Ag2S precursor is used to synthesize nano-Ag2S particles in situ during the melting process. The diameter of the nano-Ag2S particles is 8-30nm and the particle size is 40-150nm.
6. A composite current collector comprising the conductive substrate of claim 5, comprising a metal layer located on at least one side of the conductive substrate.
7. The composite current collector according to claim 6, wherein: The thickness of the conductive substrate is 1 μm-8 μm; Optionally, the metal layer is one or a combination of two or more of titanium, silver, aluminum, nickel, copper and alloys thereof; Optionally, the thickness of the metal layer is 500nm-2000nm.
8. An electrode sheet comprising the composite current collector according to claim 6 or 7, comprising an active material layer attached to at least one surface of the composite current collector.
9. A battery comprising the electrode sheet according to claim 8.
10. An electrical device comprising the battery according to claim 9.
Citation Information
Patent Citations
Preparation method of ultra-small silver sulfide quantum dots
CN112266009A
Flexible composite thermoelectric film and preparation method and application thereof
CN112670398A
Current collector and preparation method thereof, battery pole piece and battery
CN116137330A
Conductive material, conductive base material and composite current collector and application thereof
CN116598044A
Method for preparing of complex electrode of multi layered structure containing metal nanowires having metal nanoparticles thereon
KR1020150077602A