Co 2-photothermal dual-responsive nano-emulsion separation membrane, and preparation method therefor and use thereof
Through the three-layer structure design of CO2-photothermal double-responsive nanoemulsion separation membrane, the free radical polymerization reaction of carbon-based nanomaterials and polymers is solved in the prior art with low deprotonation efficiency and difficulty in wettability switching. Problem, fast response and efficient separation efficiency are achieved, suitable for oil-water separation applications.
Patent Information
- Application Number
- PCT/CN2023/141755
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2023-12-26
- Publication Date
- 2024-11-28
AI Technical Summary
The existing CO2 responsive separation membrane is inefficient during deprotonation and is difficult to achieve rapid switching between hydrophobic/oleophilic and hydrophilic/underwater oleophobic wetting, limiting its oil-water separation process application.
The CO2-photothermal double-responsive nanoemulsion separation membrane is woven through three-layer fiber structures. The inner core is fiber, the intermediate layer is a photothermal conversion functional coating, and the outer layer is a CO2-responsive functional coating, using carbon-based nanomaterials and The preparation of free radical polymerization of polyvinyl alcohol and CO2-responsive monomers and hard monomers can achieve rapid deprotonation and wettability switching of the membrane.
The reversible switching between the superhydrophobic and superhydrophilic states of the membrane under CO2 or photothermal stimulation is achieved, the response time is shortened by more than 20 times, the separation efficiency is more than 99.5%, and it is easy to prepare on a large scale.
Smart Images

Figure CN2023141755_28112024_PF_FP_ABST
Abstract
Description
A CO2-photothermal dual-responsive nanoemulsion separation membrane, its preparation method, and its application Technical Field
[0001] The present invention belongs to the field of chemical separation technology, relates to an oil-water separation membrane, and in particular to a CO2-photothermal dual-responsive nanoemulsion separation membrane and a preparation method and a use method thereof. Background Art
[0002] Frequent oil spills and the massive discharge of industrial and domestic wastewater cause severe environmental pollution and endanger human health. Therefore, the development of efficient oil-water separation membrane materials has become a current research hotspot. Stimuli-responsive membranes are a class of intelligent separation membranes that can spontaneously regulate their physicochemical properties by "sensing" changes in the surrounding environment, thereby achieving reversible regulation of membrane flux and selectivity. This property provides flexibility and controllability in practical oil-water separation processes. Compared with traditional stimuli (such as pH, light, heat, redox, etc.), the use of CO2 as a stimulus to construct responsive membranes offers unparalleled advantages, such as no membrane fouling, no damage to the membrane structure, no chemical accumulation, a deep response, and high cyclic stability. Therefore, it is a current research hotspot in the field of responsive membranes. However, existing CO2-responsive membranes can only be used to separate immiscible oil-water mixtures and have difficulty achieving efficient separation of various stable emulsion systems. Furthermore, there are problems such as cumbersome membrane preparation processes, low efficiency, and difficulty in large-scale fabrication. More importantly, CO2-stimulated responsive polymers are usually protonated in the presence of CO2 and then deprotonated when an inert gas is introduced. However, the deprotonation process by introducing an inert gas is time-consuming. This is because the solubility of inert gases in aqueous solutions is low, resulting in a slow deprotonation process on the membrane surface, which causes the membrane to respond to inert gases for a long time (usually more than 20 minutes), which greatly limits the industrial application of such separation membranes.
[0003] Summary of the Invention
[0004] The technical problem to be solved by the present invention is to provide a nanoemulsion separation membrane that can be rapidly deprotonated and can quickly switch back and forth between hydrophobic / oleophilic and hydrophilic / underwater oleophobic wettability.
[0005] The first purpose of the present invention is to provide a CO2-photothermal dual-responsive nanoemulsion separation membrane, which is woven from fibers with a three-layer structure, with the inner core being fibers, the middle layer being a photothermal conversion functional coating, and the outer layer being a CO2 responsive functional coating; the photothermal conversion functional coating is prepared from carbon-based nanomaterials and polyvinyl alcohol; the CO2 responsive functional coating is obtained by free radical polymerization of CO2 responsive monomers and hard monomers; the pore size distribution of the separation membrane is below 0.1um.
[0006] The photothermal conversion layer is made of a hydrophilic material and is easily fallen off when exposed to the outside in a water environment. Therefore, an outer CO2 response layer is required to cover it to prevent it from falling off.
[0007] In one embodiment, the fiber material comprises PET, polyester, acrylic, nylon, spandex, carbon fiber or glass;
[0008] The carbon-based nanomaterial includes one or more of carbon black, carbon nanotubes, graphene, graphene oxide and reduced graphene oxide;
[0009] The CO2-responsive monomer includes N,N-dimethylphenylene (DMSt), dimethylaminoethyl methacrylate (DMAEMA) or diethylaminoethyl methacrylate (DEAEMA);
[0010] The hard monomers include styrene (ST), hydroxyethyl methacrylate (HEMA), acrylamide (AM), methyl methacrylate (MMA), polyethylene glycol methacrylate (PEGMA), and 2-ethoxyethyl methacrylate (EEMA).
[0011] In one embodiment, the mass ratio of the carbon-based nanomaterial to polyvinyl alcohol is 3:1000-10:1000.
[0012] In one embodiment, the mass ratio of the carbon-based nanomaterial to polyvinyl alcohol is 3:1000.
[0013] In one embodiment, the molar ratio of the CO2 responsive monomer to the hard monomer is 1:1-1:2.
[0014] In one embodiment, the molar ratio of the CO2 responsive monomer to the hard monomer is 1:1.
[0015] The second object of the present invention is to provide a method for preparing a CO2-photothermal dual-responsive nanoemulsion separation membrane, comprising the following steps:
[0016] S1. Preparation of a photothermal conversion functional coating: 7.5-12.5 wt % polyvinyl alcohol and deionized water were added to a flask, followed by 0.2-0.5 mg / ml of a carbon-based nanomaterial, and the mixture was heated and stirred in an oil bath at 90-110° C. for 30-90 min to prepare a photothermal conversion functional coating;
[0017] S2. Preparation of CO2 responsive functional coating: preparing a CO2 responsive polymer by free radical polymerization of a CO2 responsive monomer and a hard monomer in tetrahydrofuran, and dissolving the prepared CO2 responsive polymer in ethanol to prepare a CO2 responsive functional coating with a mass fraction of 5 to 20 wt%;
[0018] S3. Preparation of CO2-photothermal dual-responsive fiber: Use a sizing machine to evenly coat the photothermal conversion functional coating prepared in S1 on the surface of the PET fiber and heat-treat it in an oven at 70-90°C for 2-10 min to obtain the photothermal conversion functional fiber. Then use a sizing machine to evenly coat the CO2-responsive functional coating prepared in S2 on the surface of the photothermal conversion functional fiber and heat-treat it in an oven at 70-90°C for 2-10 min to obtain the CO2-photothermal dual-responsive fiber.
[0019] S4. Preparation of CO2-photothermal dual-responsive nanoemulsion separation membrane: Use a loom to weave the CO2-photothermal dual-responsive fibers prepared in S3 into a membrane to obtain a CO2-photothermal dual-responsive nanoemulsion separation membrane.
[0020] In one embodiment, the CO2 responsive functional coating in step S2 is a transparent material, and the light transmittance of the coating after film formation is 85-92%.
[0021] The third object of the present invention is to provide an application of a CO2-photothermal dual-responsive nanoemulsion separation membrane, which can achieve reversible switching between superhydrophobic and superhydrophilic states under CO2 or photothermal stimulation.
[0022] In one embodiment, the CO2 stimulation is to place the nanoemulsion separation membrane in a water environment and pass CO2 for 5 minutes; the photothermal stimulation is to raise the temperature of the nanoemulsion separation membrane to 120-180°C within 10-20 seconds under the irradiation of a near-infrared light source.
[0023] In one embodiment, when the nanoemulsion separation membrane separates an oil-water mixture, when the mixture type is an oil-in-water nanoemulsion, the hydrophobic / oleophilic membrane in the initial state is used for separation; when the mixture type is an oil-in-water nanoemulsion, the hydrophobic / oleophilic separation membrane is placed in a water environment and CO2 is introduced for 5 minutes to convert it into a hydrophilic / underwater oleophobic separation membrane before separation; when the oil-in-water nanoemulsion needs to be separated again, the hydrophilic / underwater oleophobic separation membrane is placed in a water environment and irradiated with a 1.2V 808nm near-infrared light source for 1 minute to convert it into a hydrophobic / oleophilic separation membrane again before separation.
[0024] In one embodiment, the separation membrane can achieve reversible switching between superhydrophobic and superhydrophilic states under alternating CO2-light stimulation. In the initial state, the water contact angle (WCA) of the membrane is above 150° (superhydrophobic). After the membrane is placed in a water environment and CO2 is passed through for 5 minutes, the WCA drops to 0° (superhydrophilic). Subsequently, after the membrane is irradiated with a near-infrared light source for 1 minute, the WCA is again increased to above 150° (superhydrophobic). Beneficial effects:
[0025] After the separation membrane provided by the present invention is stimulated by CO2, the membrane is converted into a hydrophilic state, allowing water to pass through. Since the membrane surface is occupied by water, oil droplets cannot contact and pass through the membrane, thereby achieving the retention of oil droplets; conversely, after being stimulated by near-infrared light, photothermal energy is provided to enable the hydrophilic CO2 polymer to quickly restore to a hydrophobic state, allowing oil to pass through. Since the membrane surface is occupied by oil, water droplets cannot contact and pass through the membrane, thereby achieving the retention of water droplets.
[0026] The separation membrane of the present invention exhibits excellent photothermal properties. Under near-infrared light irradiation, the membrane surface temperature can be significantly increased within 15 seconds, resulting in a transition from a protonated to a deprotonated state within 1 minute. Compared to inert gas stimulation, the membrane's response time is shortened by more than 20 times. The separation efficiency of the membrane exceeds 99.5% for 20nm oil-in-water emulsions in the superhydrophobic state and exceeds 99.5% for 20nm oil-in-water emulsions in the hydrophilic state.
[0027] The separation membrane of the present invention has narrowly distributed submicron pores and can realize the separation of nanoemulsions.
[0028] The separation membrane of the present invention is easy to prepare on a large scale, and can easily prepare a separation membrane with an area of 4800 cm 2 separation membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is a schematic diagram of the membrane preparation process, which transitions from a blank membrane to a photothermal functional coating membrane and then to a CO2-photothermal dual response membrane.
[0030] Figure 2 is an SEM image of a fiber cross-section with a photothermal functional coating and a CO2 responsive functional coating. The inner layer is the photothermal functional coating, through which graphene oxide powder within 2 μm can be seen. The outer layer is the CO2 responsive functional coating, which is smoother and more uniform than the inner layer.
[0031] Figure 3 shows SEM images and optical photographs, where A is a blank film, B is a photothermal functional coating film, and C is a CO2-photothermal dual response film. DETAILED DESCRIPTION
[0032] The preparation process of CO2-photothermal dual-responsive nanoemulsion separation membrane is shown in Figure 1.
[0033] Example 1 Preparation of CO2-photothermal dual-responsive nanoemulsion separation membrane-1
[0034] The carbon-based nanomaterial used in this embodiment is graphene oxide, and the polymer is formed by free radical polymerization of two monomers, CO2-responsive DMAEMA and hard monomer HEMA, in a solvent. The amount of initiator used is 1% of the total mass of the DMAEMA and HEMA monomers.
[0035] The method for preparing the CO2-photothermal dual-responsive nanoemulsion separation membrane-1 is characterized by comprising the following specific steps:
[0036] S1. Preparation of photothermal conversion functional coating: 7.5 wt% polyvinyl alcohol (PVA) and deionized water were added to a flask, followed by 0.2 mg / ml of graphene oxide, and the mixture was heated and stirred in a 90°C oil bath for 30 min to prepare a photothermal conversion functional coating;
[0037] S2. Preparation of CO2-responsive functional coating: DMAEMA monomer and HEMA monomer were dissolved in tetrahydrofuran at a mass ratio of 1:0.5, and an initiator azobisisobutyronitrile was added. The mixture was heated and stirred in a nitrogen atmosphere for 24 hours at a heating temperature of 65°C. An excess of n-hexane was added to precipitate the polymer. The precipitated polymer was taken out and dried in an oven. The prepared CO2-responsive polymer was dissolved in a solvent to prepare a CO2-responsive functional coating with a mass fraction of 5 wt%. The light transmittance of the coating after film formation was 92%.
[0038] S3. Preparation of CO2-photothermal dual-responsive fiber: Use a sizing machine to evenly coat the photothermal conversion functional coating prepared in S1 on the surface of the PET fiber and heat-treat it in an oven at 70°C for 2 minutes to obtain the photothermal conversion functional fiber. Then use a sizing machine to evenly coat the CO2-responsive functional coating prepared in S2 on the surface of the photothermal conversion functional fiber and heat-treat it in an oven at 70°C for 2 minutes to obtain the CO2-photothermal dual-responsive fiber.
[0039] S4. Preparation of CO2-photothermal dual-responsive nanoemulsion separation membrane: Use a loom to weave the CO2-photothermal dual-responsive fiber prepared in S3 into a membrane with a sum of warp density and weft density of 300T to obtain CO2-photothermal dual-responsive nanoemulsion separation membrane-1.
[0040] The PPGOM in Figure 1 is a schematic diagram of the membrane prepared in this embodiment, whose core is PET fiber, the middle layer is graphene oxide coating, and the outer layer is copolymer coating; Figure 2 corresponds to the SEM image of the fiber cross-section with photothermal functional coating and CO2 response functional coating in this embodiment, the inner layer is the photothermal functional coating, and graphene oxide microflakes within 2 μm can be seen, and the outer layer is the CO2 response functional coating, which is smoother and more uniform than the inner layer; Figure 3C corresponds to the SEM image of the membrane prepared in this embodiment. Compared with the membrane without CO2 response coating in Figure 3B, its color is darker and the surface is smoother.
[0041] Example 2 Wettability switching process of CO2-photothermal dual-responsive nanoemulsion separation membrane-1
[0042] When needed, the hydrophobic / oleophilic CO2-photothermal dual-responsive nanoemulsion separation membrane-1 was placed in a water environment and CO2 was introduced for 5 minutes to obtain a hydrophilic / underwater oleophobic CO2-photothermal dual-responsive nanoemulsion separation membrane-1. The water contact angle of the membrane in the air at this time was measured using a contact angle meter, and the contact angle was measured to be 0°.
[0043] When needed, the hydrophilic / underwater oleophobic CO2-photothermal dual-responsive nanoemulsion separation membrane-1 was irradiated with a 1.2V 808nm near-infrared light source for 1 min to obtain the hydrophobic / oleophilic CO2-photothermal dual-responsive nanoemulsion separation membrane-1 again. The water contact angle of the membrane in the air at this time was measured using a contact angle meter, and the contact angle was measured to be 151.2°.
[0044] Example 3 Performance Testing of CO2-Photothermal Dual-Response Nanoemulsion Separation Membrane-1
[0045] When the oil-water mixture is separated using the CO2-photothermal dual-responsive nanoemulsion separation membrane-1, when the mixture type is oil-water nanoemulsion, a hydrophobic / lipophilic separation membrane is used for separation. The separation performance test data are shown in Table 1.
[0046] When the mixture type is oil-in-water nanoemulsion, the hydrophobic / oleophilic separation membrane is placed in a water environment and CO2 is introduced for 5 minutes to convert it into a hydrophilic / underwater oleophobic separation membrane, and then separation is performed. The separation performance test data are shown in Table 1;
[0047] When the water-in-oil nanoemulsion needs to be separated again, the hydrophilic / underwater oleophobic separation membrane is irradiated with a 1.2V 808nm near-infrared light source for 1 minute to be converted back into a hydrophobic / oleophilic separation membrane before separation.
[0048] After 50 cycles of separation, the separation efficiency of the prepared separation membrane for isooctane oil-in-water nanoemulsion (20 nm) and oil-in-water nanoemulsion (20 nm) can be maintained above 99%.
[0049] Example 4 Preparation of CO2-photothermal dual-responsive nanoemulsion separation membrane-2
[0050] The carbon-based nanomaterial used in this embodiment is graphene, and the polymer is formed by free radical polymerization of two monomers, DMSt (a CO2-responsive monomer) and HEMA (a hard monomer), in a solvent. The amount of initiator used is 1% of the total mass of the DMSt and HEMA monomers.
[0051] The method for preparing the CO2-photothermal dual-responsive nanoemulsion separation membrane-2 is characterized by comprising the following specific steps:
[0052] S1. Preparation of photothermal conversion functional coating: 10 wt% polyvinyl alcohol (PVA) and deionized water were added to a flask, followed by 0.3 mg / ml of graphene, and the mixture was heated and stirred in an oil bath at 100°C for 1 h to prepare the photothermal conversion functional coating;
[0053] S2. Preparation of CO2-responsive functional coating: DMSt monomer and HEMA monomer were dissolved in tetrahydrofuran at a mass ratio of 1:0.5, and the initiator azobisisobutyronitrile was added. The mixture was heated and stirred in a nitrogen atmosphere for 36 hours at a heating temperature of 75°C. An excess of n-hexane was added to precipitate the polymer. The precipitated polymer was taken out and dried in an oven. The prepared CO2-responsive polymer was dissolved in a solvent to prepare a CO2-responsive functional coating with a mass fraction of 10 wt%. The light transmittance of the coating after film formation was 90%.
[0054] S3. Preparation of CO2-photothermal dual-responsive fiber: Use a sizing machine to evenly coat the photothermal conversion functional coating prepared in S1 on the surface of acrylic fiber and heat-treat it in an oven at 80°C for 5 minutes to obtain photothermal conversion functional fiber. Then use a sizing machine to evenly coat the CO2-responsive functional coating prepared in S2 on the surface of photothermal conversion functional fiber and heat-treat it in an oven at 80°C for 5 minutes to obtain CO2-photothermal dual-responsive fiber.
[0055] S4, preparation of CO2-photothermal dual-responsive nanoemulsion separation membrane: Use a loom to weave the CO2-photothermal dual-responsive fiber prepared in S3 into a membrane with a sum of warp density and weft density of 330T to obtain CO2-photothermal dual-responsive nanoemulsion separation membrane-2.
[0056] Example 5 Wettability switching process of CO2-photothermal dual-responsive nanoemulsion separation membrane-2
[0057] When needed, the hydrophobic / oleophilic CO2-photothermal dual-responsive nanoemulsion separation membrane-2 was placed in a water environment and CO2 was introduced for 8 minutes to obtain a hydrophilic / underwater oleophobic CO2-photothermal dual-responsive nanoemulsion separation membrane-2. The water contact angle of the membrane in the air at this time was measured using a contact angle meter, and the contact angle was measured to be 0°.
[0058] When needed, the hydrophilic / underwater oleophobic CO2-photothermal dual-responsive nanoemulsion separation membrane-2 was irradiated with a 1.5V 780nm near-infrared light source for 1.5 minutes to obtain the hydrophobic / oleophilic CO2-photothermal dual-responsive nanoemulsion separation membrane-2 again. The water contact angle of the membrane in the air at this time was measured using a contact angle meter, and the contact angle was measured to be 150.6°.
[0059] Example 6 Performance Testing of CO2-Photothermal Dual-Response Nanoemulsion Separation Membrane-2
[0060] When the oil-water mixture is separated using the CO2-photothermal dual-responsive nanoemulsion separation membrane-2, when the mixture type is oil-water nanoemulsion, a hydrophobic / lipophilic separation membrane is used for separation. The separation performance test data are shown in Table 1.
[0061] When the mixture type is oil-in-water nanoemulsion, the hydrophobic / oleophilic separation membrane is placed in a water environment and CO2 is introduced for 8 minutes to convert it into a hydrophilic / underwater oleophobic separation membrane, and then separation is performed. The separation performance test data are shown in Table 1;
[0062] When the water-in-oil nanoemulsion needs to be separated again, the hydrophilic / underwater oleophobic separation membrane is irradiated with a 1.5V 780nm near-infrared light source for 1.5 minutes and then converted into a hydrophobic / oleophilic separation membrane before separation.
[0063] After 50 cycles of separation, the separation efficiency of the prepared separation membrane for isooctane oil-in-water nanoemulsion (20 nm) and oil-in-water nanoemulsion (20 nm) can be maintained above 99%.
[0064] Example 7 Preparation of CO2-Photothermal Dual-Response Nanoemulsion Separation Membrane-3
[0065] The carbon-based nanomaterial used in this embodiment is carbon nanotubes, and the polymer is formed by free radical polymerization of two monomers, CO2-responsive monomer DMSt and hard monomer AEMA, in a solvent. The amount of initiator used is 1% of the total mass of the DMSt monomer and AEMA monomer.
[0066] The method for preparing the CO2-photothermal dual-responsive nanoemulsion separation membrane-3 is characterized by comprising the following specific steps:
[0067] S1. Preparation of a photothermal conversion functional coating: 12.5 wt% polyvinyl alcohol (PVA) and deionized water were added to a flask, followed by 0.4 mg / ml of carbon nanotubes. The mixture was heated and stirred in an oil bath at 95°C for 90 min to prepare a photothermal conversion functional coating.
[0068] S2. Preparation of CO2-responsive functional coating: DMSt monomer and AEMA monomer were dissolved in tetrahydrofuran at a mass ratio of 1:1.5, and dibenzoyl peroxide as an initiator was added. The mixture was heated and stirred in a nitrogen atmosphere for 36 hours at a heating temperature of 85°C. An excess of n-hexane was added to precipitate the polymer. The precipitated polymer was taken out and dried in an oven. The prepared CO2-responsive polymer was dissolved in a solvent to prepare a CO2-responsive functional coating with a mass fraction of 20 wt%. The light transmittance of the coating after film formation was 85%.
[0069] S3. Preparation of CO2-photothermal dual-responsive fiber: Use a sizing machine to evenly coat the photothermal conversion functional coating prepared in S1 on the surface of the nylon fiber and heat-treat it in an oven at 90°C for 10 minutes to obtain the photothermal conversion functional fiber. Then use a sizing machine to evenly coat the CO2-responsive functional coating prepared in S2 on the surface of the photothermal conversion functional fiber and heat-treat it in an oven at 90°C for 10 minutes to obtain the CO2-photothermal dual-responsive fiber.
[0070] S4, preparation of CO2-photothermal dual-responsive nanoemulsion separation membrane: Use a loom to weave the CO2-photothermal dual-responsive fiber prepared in S3 into a membrane with a sum of warp density and weft density of 350T to obtain CO2-photothermal dual-responsive nanoemulsion separation membrane-3.
[0071] Example 8 Wettability switching process of CO2-photothermal dual-responsive nanoemulsion separation membrane-3
[0072] When needed, the hydrophobic / oleophilic CO2-photothermal dual-responsive nanoemulsion separation membrane-3 was placed in a water environment and CO2 was introduced for 10 minutes to obtain a hydrophilic / underwater oleophobic CO2-photothermal dual-responsive nanoemulsion separation membrane-3. The water contact angle of the membrane in the air at this time was measured using a contact angle meter, and the contact angle was measured to be 0°.
[0073] When needed, the hydrophilic / underwater oleophobic CO2-photothermal dual-responsive nanoemulsion separation membrane-3 was irradiated with a 2V 900nm near-infrared light source for 2 minutes to obtain the hydrophobic / oleophilic CO2-photothermal dual-responsive nanoemulsion separation membrane-3 again. The water contact angle of the membrane in the air at this time was measured using a contact angle meter, and the contact angle was measured to be 152.3°.
[0074] Example 9 Performance Testing of CO2-Photothermal Dual-Response Nanoemulsion Separation Membrane-3
[0075] When the oil-water mixture is separated using the CO2-photothermal dual-responsive nanoemulsion separation membrane-3, when the mixture type is oil-water nanoemulsion, a hydrophobic / lipophilic separation membrane is used for separation. The separation performance test data are shown in Table 1.
[0076] When the mixture type is oil-in-water nanoemulsion, the hydrophobic / oleophilic separation membrane is placed in a water environment and CO2 is introduced for 10 minutes to convert it into a hydrophilic / underwater oleophobic separation membrane, and then separation is performed. The separation performance test data are shown in Table 1;
[0077] When the water-in-oil nanoemulsion needs to be separated again, the hydrophilic / underwater oleophobic separation membrane is irradiated with a 2V 900nm near-infrared light source for 2 minutes to be converted back into a hydrophobic / oleophilic separation membrane before separation.
[0078] After 50 cycles of separation, the separation efficiency of the prepared separation membrane for isooctane oil-in-water nanoemulsion (20 nm) and oil-in-water nanoemulsion (20 nm) can be maintained above 99%.
[0079] Example 10 Preparation of CO2-photothermal dual-responsive nanoemulsion separation membrane-4
[0080] The carbon-based nanomaterial used in this embodiment is redox graphene, and the polymer is formed by free radical polymerization of two monomers, CO2-responsive DMAEMA and hard monomer AEMA, in a solvent. The initiator used is 1% of the total weight of the DMAEMA and AEMA monomers.
[0081] The method for preparing the CO2-photothermal dual-responsive nanoemulsion separation membrane-4 is characterized by comprising the following specific steps:
[0082] S1. Preparation of photothermal conversion functional coating: 10 wt% polyvinyl alcohol (PVA) and deionized water were added to a flask, followed by 0.4 mg / ml of graphene, and the mixture was heated and stirred in an oil bath at 95°C for 1 h to prepare the photothermal conversion functional coating;
[0083] S2. Preparation of CO2-responsive functional coating: DMAEMA monomer and AEMA monomer were dissolved in tetrahydrofuran at a mass ratio of 1:2, and dibenzoyl peroxide as an initiator was added. The mixture was heated and stirred in a nitrogen atmosphere for 48 hours at a heating temperature of 85°C. An excess of n-hexane was added to precipitate the polymer. The precipitated polymer was taken out and dried in an oven. The prepared CO2-responsive polymer was dissolved in a solvent to prepare a CO2-responsive functional coating with a mass fraction of 10 wt%. The light transmittance of the coating after film formation was 88%.
[0084] S3. Preparation of CO2-photothermal dual-responsive fiber: Use a sizing machine to evenly coat the photothermal conversion functional coating prepared in S1 on the surface of the polyester fiber and heat-treat it in an oven at 75°C for 4 minutes to obtain the photothermal conversion functional fiber. Then use a sizing machine to evenly coat the CO2-responsive functional coating prepared in S2 on the surface of the photothermal conversion functional fiber and heat-treat it in an oven at 75°C for 4 minutes to obtain the CO2-photothermal dual-responsive fiber.
[0085] S4, preparation of CO2-photothermal dual-responsive nanoemulsion separation membrane: The CO2-photothermal dual-responsive fiber prepared in S3 was woven into a membrane using a loom with a sum of warp density and weft density of 300T to obtain CO2-photothermal dual-responsive nanoemulsion separation membrane-4.
[0086] Example 11 Wettability switching process of CO2-photothermal dual-responsive nanoemulsion separation membrane-4
[0087] When needed, the hydrophobic / oleophilic CO2-photothermal dual-responsive nanoemulsion separation membrane-4 was placed in a water environment and CO2 was introduced for 5 minutes to obtain the hydrophilic / underwater oleophobic CO2-photothermal dual-responsive nanoemulsion separation membrane-4. The water contact angle of the membrane in the air at this time was measured using a contact angle meter, and the contact angle was measured to be 0°.
[0088] When needed, the hydrophilic / underwater oleophobic CO2-photothermal dual-responsive nanoemulsion separation membrane-4 was irradiated with a 1.2V 808nm near-infrared light source for 1 min to obtain the hydrophobic / oleophilic CO2-photothermal dual-responsive nanoemulsion separation membrane-4 again. The water contact angle of the membrane in the air at this time was measured using a contact angle meter, and the contact angle was measured to be 151.0°.
[0089] Example 12 Performance Testing of CO2-Photothermal Dual-Response Nanoemulsion Separation Membrane-4
[0090] When the oil-water mixture is separated using the CO2-photothermal dual-responsive nanoemulsion separation membrane-4, when the mixture type is oil-water nanoemulsion, a hydrophobic / lipophilic separation membrane is used for separation. The separation performance test data are shown in Table 1.
[0091] When the mixture type is oil-in-water nanoemulsion, the hydrophobic / oleophilic separation membrane is placed in a water environment and CO2 is introduced for 5 minutes to convert it into a hydrophilic / underwater oleophobic separation membrane, and then separation is performed. The separation performance test data are shown in Table 1;
[0092] When the water-in-oil nanoemulsion needs to be separated again, the hydrophilic / underwater oleophobic separation membrane is irradiated with a 1.2V 808nm near-infrared light source for 1 minute to be converted back into a hydrophobic / oleophilic separation membrane before separation.
[0093] After 50 cycles of separation, the separation efficiency of the prepared separation membrane for isooctane oil-in-water nanoemulsion (20 nm) and oil-in-water nanoemulsion (20 nm) can be maintained above 99%.
[0094] Comparative Example 1 Effect of not adding carbon-based nanomaterials on the deprotonation process
[0095] The polymer used in this embodiment is prepared by free radical polymerization of two monomers, DMAEMA (a CO2-responsive monomer) and HEMA (a hard monomer), in a solvent. The amount of initiator used is 1% of the total mass of the DMAEMA and HEMA monomers.
[0096] The method for preparing the above-mentioned CO2-responsive nanoemulsion separation membrane is characterized by comprising the following specific steps:
[0097] S1. Preparation of PVA coating: 7.5 wt% polyvinyl alcohol (PVA) and deionized water were added to a flask, and heated and stirred in a 95°C oil bath for 30 min to prepare the PVA coating;
[0098] S2. Preparation of CO2 responsive functional coating: DMAEMA monomer and HEMA monomer were dissolved in tetrahydrofuran at a mass ratio of 1:0.5, and an initiator, azobisisobutyronitrile, was added, and the mixture was heated and stirred in a nitrogen atmosphere for 24 hours at a heating temperature of 65°C. An excess of n-hexane was added to precipitate the polymer, and the precipitated polymer was taken out and dried in an oven. The prepared CO2 responsive polymer was dissolved in a solvent to prepare a CO2 responsive functional coating with a mass fraction of 5 wt%;
[0099] S3. Preparation of CO2 responsive fiber: Use a sizing machine to evenly coat the PVA coating prepared in S1 on the surface of the PET fiber and heat treat it in an oven at 80°C for 5 minutes to obtain PVA coated fiber. Then use a sizing machine to evenly coat the CO2 responsive functional coating prepared in S2 on the surface of the PVA coated fiber and heat treat it in an oven at 80°C for 4 minutes to obtain CO2 responsive fiber.
[0100] S4. Preparation of CO2-responsive nanoemulsion separation membrane: The CO2-responsive fiber prepared in S3 was woven into a membrane using a loom with a sum of warp density and weft density of 300T to obtain a CO2-responsive nanoemulsion separation membrane.
[0101] When the above-mentioned CO2-responsive nanoemulsion separation membrane is used to separate the oil-water mixture, when the mixture type is isooctane water-in-oil nanoemulsion (20nm), the hydrophobic / oleophilic separation membrane is placed in a water environment and CO2 is introduced for 5 minutes to convert it into a hydrophilic / underwater oleophobic separation membrane, and then separation is performed. The separation performance test data are shown in Table 1; when isooctane oil-in-water nanoemulsion (20nm) needs to be separated, the hydrophilic / underwater oleophobic separation membrane is irradiated with a 1.2V 808nm near-infrared light source for 1 minute, and then separation is performed. The results are shown in Table 1.
[0102] Comparison with Comparative Example 1 reveals that omitting the addition of carbon-based nanomaterials results in a loss of the membrane's photothermal deprotonation capacity, significantly reducing both the flux and performance for water-in-oil emulsion separations. The heat generated by the carbon-based nanomaterials directly replenishes the energy required for deprotonation of the CO2-responsive polymer, rapidly restoring its deprotonated state and restoring its hydrophobicity. Therefore, omitting the addition of carbon-based nanomaterials slows the membrane's ability to recover its hydrophobicity, reducing its performance for water-in-oil emulsion separations.
[0103] Comparative Example 2 Effect of N2 deprotonation on the deprotonation process rate
[0104] The polymer used in this embodiment is prepared by free radical polymerization of two monomers, DMAEMA (a CO2-responsive monomer) and HEMA (a hard monomer), in a solvent. The amount of initiator used is 1% of the total mass of the DMAEMA and HEMA monomers.
[0105] The method for preparing the above-mentioned CO2-responsive nanoemulsion separation membrane is characterized by comprising the following specific steps:
[0106] S1. Preparation of PVA coating: 10 wt% polyvinyl alcohol (PVA) and deionized water were added to a flask, and heated and stirred in an oil bath at 95°C for 1 h to prepare the PVA coating;
[0107] S2. Preparation of CO2 responsive functional coating: DMAEMA monomer and HEMA monomer were dissolved in tetrahydrofuran at a mass ratio of 1:0.5, and an initiator, azobisisobutyronitrile, was added, and the mixture was heated and stirred in a nitrogen atmosphere for 24 hours at a heating temperature of 65°C. An excess of n-hexane was added to precipitate the polymer, and the precipitated polymer was taken out and dried in an oven. The prepared CO2 responsive polymer was dissolved in a solvent to prepare a CO2 responsive functional coating with a mass fraction of 5 wt%;
[0108] S3. Preparation of CO2 responsive fiber: Use a sizing machine to evenly coat the PVA coating prepared in S1 on the surface of the PET fiber and heat treat it in an oven at 70°C for 2 minutes to obtain PVA coated fiber. Then use a sizing machine to evenly coat the CO2 responsive functional coating prepared in S2 on the surface of the PVA coated fiber and heat treat it in an oven at 70°C for 2 minutes to obtain CO2 responsive fiber.
[0109] S4. Preparation of CO2-responsive nanoemulsion separation membrane: The CO2-responsive fiber prepared in S3 was woven into a membrane using a loom with a sum of warp density and weft density of 300T to obtain a CO2-responsive nanoemulsion separation membrane.
[0110] When the above-mentioned CO2-responsive nanoemulsion separation membrane is used to separate an oil-water mixture, when the mixture type is isooctane water-in-oil nanoemulsion (20nm), the hydrophobic / oleophilic separation membrane is placed in a water environment and CO2 is introduced for 5 minutes to convert it into a hydrophilic / underwater oleophobic separation membrane, and then separation is performed. The separation performance test data are shown in Table 1; when isooctane oil-in-water nanoemulsion (20nm) needs to be separated, the hydrophilic / underwater oleophobic separation membrane is placed in a water environment and N2 is introduced for 1 minute, and then separation is performed. The results are shown in Table 1. The water contact angle of the membrane in air at this time was measured using a contact angle meter, and the measured contact angle was 46.3°
[0111] By comparing with Comparative Example 2, it was found that the contact angle could not be fully restored to above 150° within 1 minute using N2 deprotonation, and deprotonation could not be fully achieved. However, the contact angle could be restored to above 150° within 1 minute using photothermal deprotonation, indicating that photothermal conversion deprotonation is faster and more efficient.
[0112] Comparative Example 3 Effect of Reversing the Coating Order of the Photothermal Conversion Layer and the CO2 Response Layer on Separation Efficiency
[0113] The carbon-based nanomaterial used in this embodiment is graphene oxide, and the polymer is formed by free radical polymerization of two monomers, DMSt, a CO2-responsive monomer, and AEMA, a hard monomer, in a solvent. The amount of initiator used is 1% of the total mass of the DMSt and AEMA monomers.
[0114] The method for preparing the above-mentioned emulsion separation membrane is characterized by comprising the following specific steps:
[0115] S1. Preparation of a photothermal conversion functional coating: 12.5 wt% polyvinyl alcohol (PVA) and deionized water were added to a flask, followed by 0.5 mg / ml of graphene. The mixture was heated and stirred in an oil bath at 95°C for 90 min to prepare a photothermal conversion functional coating.
[0116] S2. Preparation of CO2-responsive functional coating: DMSt monomer and AEMA monomer were dissolved in tetrahydrofuran at a mass ratio of 1:1.5, and dibenzoyl peroxide as an initiator was added. The mixture was heated and stirred in a nitrogen atmosphere for 36 hours at a heating temperature of 85°C. An excess of n-hexane was added to precipitate the polymer. The precipitated polymer was taken out and dried in an oven. The prepared CO2-responsive polymer was dissolved in a solvent to prepare a CO2-responsive functional coating with a mass fraction of 20 wt%;
[0117] S3. Preparation of CO2-photothermal dual-responsive fiber: Use a sizing machine to evenly coat the CO2-responsive functional coating prepared in S2 on the surface of the PET fiber and heat-treat it in an oven at 90°C for 5 minutes to obtain the CO2-responsive functional fiber. Then use a sizing machine to evenly coat the photothermal conversion functional coating prepared in S1 on the surface of the photothermal conversion functional fiber and heat-treat it in an oven at 90°C for 5 minutes to obtain the photothermal / CO2 dual-responsive fiber.
[0118] S4. Preparation of photothermal / CO2 dual-responsive nanoemulsion separation membrane: Use a loom to weave the photothermal / CO2 dual-responsive fiber prepared in S3 into a membrane with a sum of warp density and weft density of 350T to obtain a photothermal / CO2 dual-responsive nanoemulsion separation membrane.
[0119] Wettability switching: When needed, the hydrophobic / oleophilic photothermal / CO2 dual-responsive nanoemulsion separation membrane is placed in a water environment and CO2 is introduced for 5 minutes to obtain a hydrophilic / underwater oleophobic photothermal / CO2 dual-responsive nanoemulsion separation membrane; when needed, the hydrophilic / underwater oleophobic photothermal / CO2 dual-responsive nanoemulsion separation membrane is irradiated with a 1.2V 808nm near-infrared light source for 1 minute to obtain a hydrophobic / oleophilic photothermal / CO2 dual-responsive nanoemulsion separation membrane again.
[0120] When the above-mentioned photothermal / CO2 dual-responsive nanoemulsion separation membrane is used to separate the oil-water mixture, when the mixture type is oil-in-water nanoemulsion, a hydrophobic / oleophilic separation membrane is used for separation, and the separation performance test data are shown in Table 1; when the mixture type is water-in-oil nanoemulsion, the hydrophobic / oleophilic separation membrane is placed in a water environment and CO2 is introduced for 5 minutes to convert it into a hydrophilic / underwater oleophobic separation membrane, and then separation is performed, and the separation performance test data are shown in Table 1; when the oil-in-water nanoemulsion needs to be separated again, the hydrophilic / underwater oleophobic separation membrane is irradiated with a 1.2V 808nm near-infrared light source for 1 minute and then converted into a hydrophobic / oleophilic separation membrane, and then separation is performed. After two cycles of separation, the separation efficiency of the prepared separation membrane for isooctane water-in-oil nanoemulsion (20nm) and oil-in-water nanoemulsion (20nm) dropped to below 90%.
[0121] By comparing with Comparative Example 3, it was found that after exchanging the coating order of the photothermal conversion layer and the CO2 response layer, the cycle performance of the membrane dropped significantly. This is because the PVA material in the photothermal conversion layer is hydrophilic. Therefore, when the photothermal conversion layer is placed outside in a water environment, the coating is easily dissolved and fallen off by water, resulting in an increase in the pore size of the membrane and a significant decrease in the separation performance.
[0122] Comparative Example 4 Effect of not adding CO2 response layer coating on separation efficiency
[0123] The carbon-based nanomaterial used in this embodiment is graphene oxide.
[0124] The method for preparing the above-mentioned photothermal responsive nanoemulsion separation membrane is characterized by comprising the following specific steps:
[0125] S1. Preparation of photothermal conversion functional coating: 10 wt% polyvinyl alcohol (PVA) and deionized water were added to a flask, followed by 0.3 mg / ml of graphene, and the mixture was heated and stirred in an oil bath at 95°C for 1 h to prepare the photothermal conversion functional coating;
[0126] S2. Preparation of photothermal responsive fiber: The photothermal conversion functional coating prepared in S1 was evenly coated on the surface of the PET fiber using a sizing machine, and then heat-treated in an oven at 70°C for 5 minutes to obtain the photothermal responsive fiber.
[0127] S4. Preparation of photothermal responsive nanoemulsion separation membrane: The photothermal responsive fibers prepared in S2 were woven into a membrane using a loom at a sum of warp and weft densities of 350T to obtain a photothermal responsive nanoemulsion separation membrane.
[0128] Wettability switching: When needed, the hydrophobic / oleophilic photothermal responsive nanoemulsion separation membrane was placed in a water environment and CO2 was introduced for 5 minutes; when needed, the hydrophilic / underwater oleophobic photothermal responsive nanoemulsion separation membrane was irradiated with a 1.2V 808nm near-infrared light source for 1 minute.
[0129] When necessary, the photothermal responsive nanoemulsion separation membrane was placed in a water environment and CO2 was introduced for 5 minutes. The water contact angle of the membrane in air was measured using a contact angle meter, and the contact angle was measured to be 0°.
[0130] When necessary, the photothermal responsive nanoemulsion separation membrane was irradiated with a 1.2V 808nm near-infrared light source for 1 min, and the water contact angle of the membrane in air was measured using a contact angle meter, and the contact angle was measured to be 0°.
[0131] When the above-mentioned photothermal responsive nanoemulsion separation membrane is used to separate an oil-water mixture, when the mixture type is an oil-in-water nanoemulsion, the separation performance test data are shown in Table 1; when the mixture type is an oil-in-water nanoemulsion, the hydrophobic / lipophilic separation membrane is placed in a water environment and CO2 is introduced for 5 minutes before separation, and the separation performance test data are shown in Table 1; when the oil-in-water nanoemulsion needs to be separated again, it will be irradiated with a 1.2V 808nm near-infrared light source for 1 minute before separation. After two cycles of separation, the separation efficiency of the prepared separation membrane for isooctane water-in-oil nanoemulsion (20nm) and oil-in-water nanoemulsion (20nm) dropped to below 90%.
[0132] Comparison with Comparative Example 4 reveals that when only the photothermal conversion coating is used, the membrane exhibits no switchable wettability, maintaining a constant contact angle of 0° with water. This is because the wettability switching is achieved by switching between the protonation and deprotonation states of the CO2-responsive functional layer. Furthermore, the membrane's nanoemulsion separation performance decreases significantly over a short period of time. This is because the photothermal conversion coating is hydrophilic and, without the protection of the outer CO2-responsive coating, rapidly dissolves and detaches upon direct contact with water, resulting in an increase in pore size and a decrease in separation performance.
[0133] The GOM in Figure 1 represents a schematic diagram of the membrane of this comparative example, with a core of PET fibers and an outer layer of graphene oxide coating. Figure 3B represents an SEM image of the membrane prepared in this comparative example, showing a rougher surface and lighter color than the membrane with the CO2-responsive coating in Figure 3C.
[0134] Table 1
Claims
1. A CO2-photothermal dual-responsive nanoemulsion separation membrane, characterized in that: The nanoemulsion separation membrane is woven from fibers with a three-layer structure, wherein the inner core is fibers, the middle layer is a photothermal conversion functional coating, and the outer layer is a CO2 response functional coating; the photothermal conversion functional coating is prepared from carbon-based nanomaterials and polyvinyl alcohol; the CO2 response functional coating is obtained by free radical polymerization of CO2 responsive monomers and hard monomers; the pore size distribution of the separation membrane is below 0.1 um.
2. A CO2-photothermal dual-responsive nanoemulsion separation membrane according to claim 1, characterized in that: Fiber materials include PET, polyester, acrylic, nylon, spandex, carbon fiber or glass; The carbon-based nanomaterial includes one or more of carbon black, carbon nanotubes, graphene, graphene oxide and reduced graphene oxide; The CO2 responsive monomer includes N,N-dimethyl paraphenylene, dimethylaminoethyl methacrylate or diethylaminoethyl methacrylate; The hard monomers include styrene, hydroxyethyl methacrylate, acrylamide, methyl methacrylate, polyethylene glycol methacrylate, and 2-ethoxyethyl methacrylate.
3. A CO2-photothermal dual-responsive nanoemulsion separation membrane according to claim 1, characterized in that: The mass ratio of the carbon-based nanomaterial to polyvinyl alcohol is 3:1000-10:1000, preferably 3:1000. The molar ratio of the CO2 responsive monomer to the hard monomer is 1:1-1:2, preferably 1:
1.
4. A method for preparing a CO2-photothermal dual-responsive nanoemulsion separation membrane according to any one of claims 1 to 3, characterized in that: Here are the steps: S1. Preparation of photothermal conversion functional coating: 7.5-12.5 wt% polyvinyl alcohol and deionized water were added to a flask, and then 0.2-0.5 mg / ml of carbon-based nanomaterials were added, and heated and stirred in an oil bath at 90-110° C. for 30-90 min to obtain a photothermal conversion functional coating; S2. Preparation of CO2 responsive functional coating: preparing a CO2 responsive polymer by free radical polymerization of a CO2 responsive monomer and a hard monomer in tetrahydrofuran, and dissolving the prepared CO2 responsive polymer in ethanol to prepare a CO2 responsive functional coating with a mass fraction of 5 to 20 wt%; S3. Preparation of CO2-photothermal dual response fiber: Use a sizing machine to evenly coat the photothermal conversion functional coating prepared in S1 on the surface of the PET fiber and heat treat it in an oven at 70-90°C for 2-10 min to obtain the photothermal conversion functional fiber. Then use a sizing machine to evenly coat the CO2 response functional coating prepared in S2 on the surface of the photothermal conversion functional fiber and heat treat it in an oven at 70-90°C for 2-10 min to obtain the CO2-photothermal dual response fiber. S4. Preparation of CO2-photothermal dual-responsive nanoemulsion separation membrane: Use a loom to weave the CO2-photothermal dual-responsive fibers prepared in S3 into a membrane to obtain a CO2-photothermal dual-responsive nanoemulsion separation membrane.
5. The method for preparing a CO2-photothermal dual-responsive nanoemulsion separation membrane according to claim 3, characterized in that: The CO2 responsive functional coating in step S2 is a transparent material, and the light transmittance of the coating after film formation is 85-92%.
6. Use of a CO2-photothermal dual-responsive nanoemulsion separation membrane according to any one of claims 1 to 3 or a CO2-photothermal dual-responsive nanoemulsion separation membrane prepared by the method according to claim 3 or 4, characterized in that: The nanoemulsion separation membrane can achieve reversible switching between super-hydrophobic and super-hydrophilic states under CO2 stimulation or photothermal stimulation.
7. The use of a CO2-photothermal dual-responsive nanoemulsion separation membrane according to claim 6, characterized in that: The CO2 stimulation is to place the nanoemulsion separation membrane in a water environment and pass CO2 for 5-10 minutes; The photothermal stimulation is to raise the temperature of the nanoemulsion separation membrane to 120-180° C. within 10-20 seconds under the irradiation of a near-infrared light source.
8. The use of a CO2-photothermal dual-responsive nanoemulsion separation membrane according to claim 6, characterized in that: When the nanoemulsion separation membrane separates the oil-water mixture, when the mixture type is oil-in-water nanoemulsion, the hydrophobic / oleophilic membrane in the initial state is used for separation; when the mixture type is water-in-oil nanoemulsion, the hydrophobic / oleophilic separation membrane is placed in a water environment and CO2 is introduced for 5-10 minutes to convert it into a hydrophilic / underwater oleophobic separation membrane before separation; when the oil-in-water nanoemulsion needs to be separated again, the hydrophilic / underwater oleophobic separation membrane is placed in a water environment and irradiated with a 1.2-2V, 780-900nm near-infrared light source for 1-2 minutes to convert it into a hydrophobic / oleophilic separation membrane again before separation.
Citation Information
Patent Citations
Emulsion separation membrane as well as preparation method and use method thereof
CN114259889A
CO2-photo-thermal dual response type nano emulsion separation membrane as well as preparation method and application thereof
CN116407962A
FLUX enhancement in membrane separations
WO2011113117A1