Low-cost and high-strength bi-series superconductive wire and tape and manufacturing method therefor

Through electrochemical silver reduction and additive technology, the Ag alloy layer on the surface of Bi-type superconducting wire strips is removed and the Cu layer is plated, which solves the problems of high cost and insufficient strength of Bi-type superconducting wire strips, and achieves low cost and high strength Prepared for large super magnets and high magnetic field applications.

WO2024239671A1PCT designated stage expired Publication Date: 2024-11-28NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH

Patent Information

Application Number
PCT/CN2024/071771
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-01-11
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Bi-type superconducting wire strips are made of high cost and insufficient strength because they use precious metal Ag or Ag alloy as the cover material, which makes them difficult to meet the requirements of large-scale applications and strong magnetic field applications.

Method used

Electrochemical silver reduction technology is used to remove the Ag alloy layer on the surface of Bi-type superconducting wire strip, and a high-strength Cu layer is coated on the surface, so as to improve the strength of wire strip by electrochemical additive method.

Benefits of technology

It reduces the cost of Bi-type superconducting wire strips, improves its strength, meets the requirements of large super-strong magnets and high magnetic field applications, and avoids damage to superconducting core wires by mechanical silver reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024071771_28112024_PF_FP_ABST
    Figure CN2024071771_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a low-cost and high-strength Bi-series superconductive wire and tape and a manufacturing method therefor. The method comprises: 1, electrochemically decreasing silver of a Bi-series superconductive wire and tape, so as to remove an Ag alloy layer; and 2, carrying out surface reinforcement treatment on the Bi-series superconductive wire and tape of which the silver has been electrochemically decreased so as to form a Cu layer, thus obtaining the low-cost and high-strength Bi-series superconductive wire and tape. The present invention combines an electrochemical silver decreasing technique with an electrochemical additive method to remove the Ag alloy layer from the surface of the Bi-series superconductive wire and tape and to form a high-strength Cu layer by plating, thereby manufacturing the low-cost and high-strength Bi-series superconductive wire and tape, reducing manufacturing costs, and improving the strength of the Bi-series superconductive wire and tape to satisfy use requirements of large-sized ultra-strong magnets. In addition, the present invention adjusts the thickness of the Cu layer to manufacture wires and tapes of different critical curvature radii suitable for small-caliber magnets, involves a simple process, and is suitable for mass production.
Need to check novelty before this filing date? Find Prior Art

Description

A low-cost, high-strength Bi-based superconducting wire strip and its preparation method

[0001] This application claims priority to Chinese patent application No. 2023105658469, filed on May 19, 2023. This application incorporates the entirety of the aforementioned Chinese patent application. Technical Field

[0002] The present invention belongs to the technical field of high-temperature superconducting wire strip preparation, and in particular relates to a low-cost, high-strength Bi-based superconducting wire strip and a preparation method thereof. Background Art

[0003] Bi-based high-temperature superconducting wires and strips have excellent current-carrying performance, an ultra-high upper critical field of ~100T, and a superconducting transition temperature above 77K. They have good application prospects in liquid nitrogen temperature range power transmission and liquid helium strong magnetic field fields. They have been used in ultra-strong NMR magnetic field magnets, superconducting cables, superconducting current limiters, superconducting energy storage magnets, fusion superconducting magnets, and accelerator magnets.

[0004] Bi-based wire strips are prepared by the powder tube method, that is, the precursor ceramic oxide powder is loaded into a silver tube to form a single-core composite, and then single-core wire drawing, multi-core wire bundle drawing or rolling, and then heat treatment to make high-performance Bi-based wire strips. During the entire heat treatment process, the oxygen partial pressure around the superconducting core wire must always remain consistent, otherwise segregation problems will occur, resulting in a significant decrease in the current-carrying performance of the sample. During the heating process, the oxide core wire will absorb oxygen, and during the heat preservation, the superconducting core wire will release oxygen, which will cause real-time changes in the oxygen partial pressure around the core wire. Therefore, the sheath material for preparing Bi-based superconducting wire strips must be an oxygen-permeable material. In addition, the sheath material cannot react with the Bi-based precursor powder. At present, the only sheath materials that can meet these two conditions are silver and silver alloys. Therefore, for the preparation of Bi-based superconducting wire strips, only Ag and Ag alloys can be used as sheath materials. However, Ag and Ag alloys have the following disadvantages as sheath materials:

[0005] (1) The content of pure Ag and Ag alloy (the Ag alloy used in Bi-based superconducting wire strips is a silver alloy with an Ag content exceeding 99%) is too high, resulting in excessively high costs for Bi-based superconducting wire strips. The content of Ag and Ag alloys in Bi-based superconducting wire strips is close to 70%, and the content of Ag and Ag alloys in Bi-based superconducting wire strips is even greater than 80%. Ag and Ag alloys are precious metals, and their prices are much higher than other metals, resulting in high costs for Bi-based superconducting wire strips, which restricts their large-scale application. Therefore, to achieve large-scale application of Bi-based superconducting wire strips, it is necessary to reduce the Ag content and reduce costs.

[0006] (2) The high content of Ag and Ag alloys results in the Bi-based superconducting wire strip having too low strength. The most important application of Bi-based superconducting wire strips is strong magnetic fields above 30T. The strong magnetic field interacts strongly with the superconducting current in the superconducting wire strips, causing the superconducting wire strips to be subjected to large tensile stress. Moreover, as the diameter of the superconducting magnet increases, the tensile stress on the superconducting wire strips gradually increases. However, the strength of Ag and Ag alloys is relatively low, which makes it difficult for Bi-based superconducting wire strips with Ag and Ag alloys as sheathing materials to meet the requirements of high-magnetic-field magnets. Therefore, in order to realize the application of Bi-based superconducting wire strips in ultra-strong magnetic fields, the strength of conventional Bi-based superconducting wire strips must be improved.

[0007] (3) The critical engineering current density of the enhanced Bi-based superconducting wire is greatly reduced. At present, the enhanced Bi-based superconducting wire is a high-strength metal strip directly welded on the surface of the Bi-based superconducting wire strip. Compared with the original superconducting wire strip, the thickness or diameter of this enhanced superconducting wire strip is significantly increased, which will cause the critical engineering current density of the sample to be greatly reduced, resulting in a significant increase in the size of the superconducting device prepared by the enhanced superconducting wire strip, which greatly increases the cooling cost of the superconducting device and the cost of superconducting materials. Therefore, in order to achieve large-scale application of enhanced Bi-based superconducting wire strips, it is necessary to reduce the size of the enhanced Bi-based superconducting wire strips and increase the engineering critical current density of the wire strips.

[0008] Summary of the Invention

[0009] The present invention addresses the shortcomings of the prior art by providing a low-cost, high-strength Bi-based superconducting wire strip and a method for its preparation. This method combines electrochemical silver reduction with electrochemical additive processes to remove the Ag alloy layer on the surface of the Bi-based superconducting wire strip and plate it with a high-strength Cu layer. This enables the production of low-cost, high-strength Bi-based superconducting wire strip, reducing its cost and increasing its strength. This addresses the issue of high cost and low strength associated with using Ag or Ag alloy sheathing in Bi-based superconducting wire strip.

[0010] To solve the above technical problems, the present invention provides, in one aspect, a method for preparing a low-cost, high-strength Bi-based superconducting wire strip, comprising:

[0011] Step 1: Electrochemical silver reduction: connect the Bi-based superconducting wire strip to the positive electrode of a voltage-stabilized power supply, connect a graphite electrode to the negative electrode of the voltage-stabilized power supply, then install the Bi-based superconducting wire strip and the graphite electrode in parallel on a bracket, place them in an electrolyte for electrochemical silver reduction, and remove the Ag alloy layer on the surface of the Bi-based superconducting wire strip;

[0012] Step 2, surface enhancement: The Bi-based superconducting wire strip after electrochemical silver reduction in step 1 is connected to the negative electrode of a voltage-stabilized power supply, and the copper sheet is connected to the positive electrode of the voltage-stabilized power supply. Then, the Bi-based superconducting wire strip after electrochemical silver reduction and the copper sheet are installed parallel to each other on a bracket, placed in an electrochemical additive solution for surface enhancement treatment, and a Cu layer is formed on the surface of the Bi-based superconducting wire strip to obtain the low-cost and high-strength Bi-based superconducting wire strip.

[0013] The Bi-based superconducting wire strips initially used in the present invention all use Ag or / and Ag alloy as the sheath material.

[0014] In the above-mentioned method for preparing a low-cost, high-strength Bi-based superconducting wire strip, the width of the graphite electrode in step 1 is greater than or equal to 3 times the width or diameter of the Bi-based superconducting wire strip, preferably 3 to 5 times, and more preferably 3 times;

[0015] And / or, the electrolyte is a 2 g / L to 10 g / L soluble silver salt deionized water solution, and the pH of the soluble silver salt deionized water solution is adjusted to 3 to 5 using metal hydroxide;

[0016] Preferably, the concentration of the soluble silver salt deionized water solution is 6 g / L. The present invention controls the pH of the electrolyte to achieve electrochemical silver reduction while avoiding damage to the superconducting core filament in the Bi-based superconducting wire strip.

[0017] In the above-mentioned method for preparing a low-cost, high-strength Bi-based superconducting wire strip, the soluble silver salt is selected from one of silver nitrate, silver fluoride, silver chlorate, and silver perchlorate;

[0018] And / or, the metal hydroxide is selected from one of sodium hydroxide, potassium hydroxide, barium hydroxide and lithium hydroxide.

[0019] In the above-mentioned method for preparing a low-cost, high-strength Bi-based superconducting wire strip, in step 1, the distance between the Bi-based superconducting wire strip and the graphite electrode is 1 cm to 5 cm, preferably 3.5 cm;

[0020] And / or, the current density on the surface of the Bi-based superconducting wire strip is 0.1A / dm 2 ~10A / dm 2 , preferably 5A / dm 2 ;

[0021] And / or, the power-on time is 0.1 min to 30 min, preferably 3 min.

[0022] In the above-mentioned method for preparing a low-cost, high-strength Bi-based superconducting wire strip, the electrochemical additive solution in step 2 is a deionized water solution containing 0.1 g / L to 20 g / L of a soluble copper salt and 10 g / L to 50 g / L of an acidic substance;

[0023] The concentration of the soluble copper salt is preferably 10 g / L;

[0024] The concentration of the acidic substance is preferably 30 g / L.

[0025] In the above-mentioned method for preparing a low-cost, high-strength Bi-based superconducting wire strip, the soluble copper salt is selected from one of copper sulfate, copper chloride, and copper nitrate;

[0026] And / or, the acidic substance is selected from one of citric acid, sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid.

[0027] In the above-mentioned method for preparing a low-cost, high-strength Bi-based superconducting wire strip, in step 2, the distance between the Bi-based superconducting wire strip and the copper sheet is 2 cm to 5 cm, preferably 3.5 cm;

[0028] And / or, the current density on the surface of the Bi-based superconducting wire strip is 0.1A / dm 2 ~10A / dm 2 , preferably 5A / dm 2 ;

[0029] and / or, the treatment time is 0.1 min to 20 min, preferably 10 min;

[0030] And / or, the thickness of the Cu layer is 10 μm to 40 μm, preferably 25 μm.

[0031] The above-mentioned method for preparing a low-cost, high-strength Bi-based superconducting wire strip further comprises, before step 1:

[0032] Surface scrubbing: ethanol is used to clean the surface of the Bi-based superconducting wire strip to remove the dirt remaining on the surface of the Bi-based superconducting wire strip.

[0033] The above-mentioned method for preparing a low-cost, high-strength Bi-based superconducting wire strip further comprises, before step 2:

[0034] Residual liquid cleaning: immerse the Bi-based superconducting wire strip after the electrochemical silver reduction in step 1 in high-purity water to clean and remove the electrolyte remaining on the surface.

[0035] In another aspect, the present invention provides a low-cost, high-strength Bi-based superconducting wire strip, which is produced by the above-mentioned method for producing a low-cost, high-strength Bi-based superconducting wire strip.

[0036] Compared with the prior art, the present invention has the following advantages:

[0037] 1. To address the problem that Bi-based superconducting wire strips must use precious metal Ag or Ag alloy as the sheathing material, resulting in an Ag content of 66% to 82% and high cost, the present invention first uses electrochemical silver reduction technology to remove the Ag alloy layer on the surface of the Bi-based superconducting wire strip, thereby reducing the effective Ag content in the Bi-based superconducting wire strip by about 50%, reducing the cost of the Bi-based superconducting wire strip by nearly 45%. Then, after the Ag alloy layer is removed, a high-strength Cu layer is plated on the surface of the Bi-based superconducting wire strip for surface enhancement treatment, thereby achieving the preparation of low-cost, high-strength Bi-based superconducting wire strip. Compared with Bi-based superconducting wire strips, the Ag mass content of the Bi-based superconducting wire strips can be reduced by less than 1 times, and the superconducting critical strength can be increased by more than 2 times. At the same time, the electrochemical silver reduction process is an ultra-low stress or even stress-free controllable Ag reduction process, which can avoid the excessive stress of conventional mechanical silver reduction that causes damage to the ceramic superconducting core, thereby avoiding the loss of superconducting performance of the Bi-based superconducting wire strip.

[0038] 2. The present invention adopts an electrochemical additive method to plate a high-strength Cu layer on the surface of Bi-based superconducting wire strip instead of Ag alloy, thereby improving the strength of Bi-based superconducting wire strip, especially the yield strength, to adapt to the strong tensile stress generated by the strong interaction between the Bi-based superconducting wire strip and the electric current after being formed into a strong magnetic field. This solves the problem of the weak mechanical support of Bi-based superconducting wire strip caused by the low strength of Ag and Ag alloy sheath materials, thereby enabling Bi-based superconducting wire strip to meet the application requirements of large-scale superstrong magnets, promoting the development of large-scale Bi-based superconducting magnets, and promoting the development of fusion, accelerators and large-caliber NMR.

[0039] 3. The present invention uses electrochemical silver reduction technology to remove the Ag alloy layer on the surface of the Bi-based superconducting wire strip, while forming electroplated Ag on the surface of the graphite electrode. The mass purity of the electroplated Ag reaches more than 99.9%, which can be directly made into Ag tubes and used to prepare Bi-based superconducting wire strips, realizing the reuse of Ag, reducing waste, and further reducing the cost of Bi-based superconducting wire strips.

[0040] 4. The present invention adopts an electrochemical additive method to plate a high-strength Cu layer on the surface of the Bi-based superconducting wire strip to replace the lower-strength Ag or Ag alloy, which greatly improves the strength of the Bi-based superconducting wire strip and reduces the damage to the Bi-based superconducting wire strip during the winding process of cables and magnets, making it suitable for the preparation of cables and magnets.

[0041] 5. The present invention adjusts the thickness of the Cu layer by controlling the surface enhancement treatment process, thereby controlling the diameter or thickness of the Bi-based superconducting wire strip, thereby realizing the preparation of wire strips with different critical bending radii. This not only greatly reduces the cost of the Bi-based superconducting wire strip, but also can prepare Bi-based superconducting wire strips with smaller diameter or thickness, reducing the critical bending radius of the Bi-based superconducting wire strip, making it suitable for the preparation of small-diameter magnets.

[0042] 6. The preparation process of the present invention is simple and the process design is reasonable, which can realize the batch preparation of low-cost and high-strength Bi-based wire strips, and is of great significance to promoting the industrialization and application of Bi-based superconducting wire strips.

[0043] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] FIG1 is a schematic structural diagram of the Bi-based superconducting tape used in Example 1 of the present invention.

[0045] FIG2 is a schematic structural diagram of the low-cost, high-strength Bi-based superconducting tape prepared in Example 1 of the present invention.

[0046] FIG3 is a schematic structural diagram of the Bi-based superconducting wire used in Example 2 of the present invention.

[0047] FIG4 is a schematic structural diagram of the low-cost, high-strength Bi-based superconducting wire prepared in Example 2 of the present invention.

[0048] Explanation of Reference Numerals 1—superconducting core wire; 2—Ag layer; 3—Ag alloy layer; 4—Cu layer. DETAILED DESCRIPTION

[0049] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Experimental methods in the following examples where specific conditions are not specified were performed according to conventional methods and conditions or selected according to the product specifications.

[0050]

Performance test

[0051] The products prepared in the examples and comparative examples were tested for their application performance. The test standards or methods are as follows:

[0052] 1. Test of Ag content:

[0053] The Ag content was determined according to GB / T 11067.1-2006 “Chemical analysis method of silver - Determination of silver content - Silver chloride precipitation-flame atomic absorption spectrometry”.

[0054] 2. Breaking strength test:

[0055] The fracture strength test was carried out in accordance with GB / T 36611-2018 "Measurement of Mechanical Properties of Ag and / or Ag Alloy Encapsulated Bi-2223 and Bi-2212 Composite Superconductors - Room Temperature Tensile Test Method".

[0056] 3. Cost accounting:

[0057] In conventional Bi-based superconducting wire strips, the cost of Ag raw materials accounts for ~96%, the cost of other materials accounts for 2%, and the processing cost accounts for 2%. In this application, we replace the outer layer Ag of the Bi-based superconducting wire strip with Cu. The replaced Ag accounts for half of the silver content of the superconducting wire strip. The price of Cu raw material is only 1 / 100 of the price of Ag raw material. The processing cost of replacing Ag with copper (including electrochemical Ag reduction and electrochemical additive processing costs) is about 20% of the price of copper raw material. According to the standard that the cost of conventional Bi-based superconducting wire strip is 100%, the cost calculation method of the superconducting wire strip in this application is as follows:

[0058] Cost reduction rate = 100% - cost of replacement raw material Cu - replacement processing cost - remaining Ag raw material in the superconducting tape - other materials and processing costs.

[0059] 4. Superconducting critical current:

[0060] Superconducting critical current testing is carried out in accordance with GB / T 18502-2018 / IEC 61788-3:2006 "Critical current measurement of the DC critical current of silver and / or silver alloy-encapsulated Bi-2212 and Bi-2223 oxide superconductors".

[0061] 5. Superconducting critical tensile strength test:

[0062] Tension is applied to both ends of the strip along its length, and the superconducting critical current of the sample is measured in situ. When the critical current of the sample drops to 95% of the stress-free state, the tension is the superconducting critical tensile strength of the sample [Fischer K, Fahr T, Schlafer U, et al. Effect of processing parameters and tensile stress on the properties of Bi-2223 strip (with Ag and AgMn sheaths) [J]. IEEE transactions on applied superconductivity, 1999, 9(2): 2625-2628] and [Mao ZH, Jin H, Qin JG, et al. Axial tensile stress-strain characteristics of Bi-2212 round wire under different heat treatment conditions [J]. IEEE Transactions on Applied Superconductivity, 2017, 27(6): 6400405].

[0063] 6. Critical bending radius:

[0064] The tape was uniformly bent along its length, and the superconducting critical current of the sample was measured in situ. When the critical current of the sample dropped to 95% of that of the straight sample, the bending radius was the superconducting critical bending radius of the sample [Shin HS, Katagiri K. Critical current degradation behavior of Bi-2223 superconducting tape under bending and torsional strain [J]. Superconductor Science and Technology, 2003, 16(9): 1012–1018].

[0065] Example 1

[0066] This embodiment includes the following steps:

[0067] Step 1: Surface scrubbing: Use a cotton cloth moistened with ethanol to scrub the surface of the Bi-based superconducting tape (as shown in FIG1 ) to remove dirt remaining on the surface of the Bi-based superconducting tape during the heat treatment process;

[0068] Step 2: Electrochemical silver reduction: Connect the Bi-based superconducting tape that has been scrubbed in Step 1 to the positive electrode of a regulated power supply, and connect the graphite electrode to the negative electrode of the regulated power supply. The width of the graphite electrode is 12 mm, and the width of the Bi-based superconducting tape is 4 mm. The width of the graphite electrode is three times the width of the Bi-based superconducting tape. Then, the scrubbed Bi-based superconducting tape and the graphite electrode are mounted parallel to each other on a bracket and placed in an electrolyte for electrochemical silver reduction. The distance between the Bi-based superconducting tape and the graphite electrode is 1 cm. The electrolyte is a 2 g / L AgNO3 solution, and the pH of the AgNO3 solution is adjusted to 3 using sodium hydroxide. During the electrochemical silver reduction process, the current density on the surface of the Bi-based superconducting tape is adjusted to 0.1 A / dm 2 The power-on time is 30 minutes, which removes the Ag alloy layer on the surface of the Bi-based superconducting tape, reveals the silver layer on the surface of the superconducting core wire of the outer layer of the Bi-based superconducting tape, and forms electroplated Ag with a purity of 99.99% on the surface of the graphite electrode.

[0069] Step 3: Residual liquid cleaning: Immerse the Bi-based superconducting tape after electrochemical silver reduction in step 2 in high-purity water to clean and remove residual electrolyte on the surface;

[0070] Step 4: Surface enhancement: Connect the cleaned Bi-based superconducting tape in step 3 to the negative electrode of the stabilized power supply, connect the copper sheet to the positive electrode of the stabilized power supply, and then install the cleaned Bi-based superconducting tape and the copper sheet in parallel on a bracket and place them in an electrochemical additive solution for surface enhancement treatment. The distance between the cleaned Bi-based superconducting tape and the copper sheet is 2 cm. The electrochemical additive solution contains 0.1 g / L copper sulfate and 10 g / L citric acid. During the surface enhancement treatment, the current density on the surface of the Bi-based superconducting tape is adjusted to 0.1 A / dm 2 The processing time is 20 minutes, and a Cu layer with a thickness of 20 μm is formed on the surface of the Bi-based superconducting tape, thereby obtaining a low-cost and high-strength Bi-based superconducting tape (as shown in FIG2 ).

[0071] Testing revealed that the Ag content of the low-cost, high-strength Bi-based superconducting tape prepared in this example was reduced from 66% to 33% of the original Bi-based superconducting tape. The fracture strength increased from 90 MPa to 94 MPa in the original Bi-based superconducting tape to 102 MPa to 104 MPa, and the superconducting critical tensile strength at 77 K increased from 5 kg to 14 kg, demonstrating enhanced mechanical properties. The original Bi-based superconducting tape and the low-cost, high-strength Bi-based superconducting tape prepared in this example exhibited identical superconducting critical current-carrying performance, with both exhibiting a superconducting critical current of 53 A at 77 K. This further confirms that the electrochemical Ag reduction and copper deposition processes have no impact on the performance of the superconducting core.

[0072] In this embodiment, copper is used to replace nearly half of the precious metal Ag in the Bi-based superconducting tape, thereby reducing the cost of the Bi-based superconducting tape by 47.424% without reducing the current-carrying performance. The enhanced mechanical properties enable the Bi-based superconducting tape to be used in conditions with more stringent magnetic fields or pressures, thus broadening the application areas of the Bi-based superconducting tape.

[0073] Figure 1 is a schematic structural diagram of the Bi-based superconducting tape used in this embodiment 1, including a superconducting core wire 1, an Ag layer coated on the outside of the superconducting core wire 1, and an Ag alloy layer 3 coated on the outermost layer; Figure 2 is a schematic structural diagram of the low-cost, high-strength Bi-based superconducting tape prepared in this embodiment, including a superconducting core wire 1, an Ag layer coated on the outside of the superconducting core wire 1, and a Cu layer 4 coated on the outermost layer; By comparing Figures 1 and 2, it can be seen that the present invention adopts electrochemical silver reduction technology and electrochemical additive method to remove the Ag alloy layer on the surface of the Bi-based superconducting wire strip and plate a high-strength Cu layer instead.

[0074] Example 2

[0075] This embodiment includes the following steps:

[0076] Step 1: Surface scrubbing: Use a cotton cloth moistened with ethanol to scrub the surface of the Bi-based superconducting wire (as shown in FIG3 ) to remove dirt remaining on the surface of the Bi-based superconducting wire during the heat treatment process;

[0077] Step 2: Electrochemical silver reduction: Connect the Bi-based superconducting wire after scrubbing in step 1 to the positive electrode of a regulated power supply, and connect the graphite electrode to the negative electrode of the regulated power supply. The width of the graphite electrode is 16 mm, the diameter of the Bi-based superconducting tape is 4 mm, and the width of the graphite electrode is 4 times the diameter of the Bi-based superconducting tape. Then, the scrubbed Bi-based superconducting wire and the graphite electrode are mounted in parallel on a bracket and placed in an electrolyte for electrochemical silver reduction. The distance between the Bi-based superconducting wire and the graphite electrode is 1 cm. The electrolyte is a 2 g / L AgNO3 solution, and the pH of the AgNO3 solution is adjusted to 3 using sodium hydroxide. The current density on the surface of the Bi-based superconducting wire during the electrochemical silver reduction process is adjusted to 10 A / dm 2 The power-on time is 15 minutes, which removes the Ag alloy layer on the surface of the Bi-based superconducting wire, revealing the silver layer on the surface of the outer superconducting core of the Bi-based superconducting wire. At the same time, electroplated Ag with a purity of 99.99% is formed on the surface of the graphite electrode.

[0078] Step 3: Same as Example 1;

[0079] Step 4: The difference from Example 1 is that the electrochemical additive solution contains 2g / L copper sulfate and 10g / L citric acid, and the current density on the surface of the Bi-based superconducting wire is adjusted to 3A / dm during the surface enhancement treatment. 2 The processing time is 15 minutes, and a Cu layer with a thickness of 40 μm is formed on the surface of the Bi-based superconducting wire to obtain a low-cost and high-strength Bi-based superconducting wire (as shown in Figure 4).

[0080] Testing revealed that the Ag content of the low-cost, high-strength Bi-based superconducting wire prepared in this example was reduced from 80% to 40% of the original Bi-based superconducting wire. The breaking strength increased from 100 MPa in the original Bi-based superconducting wire to 135 MPa, and the superconducting critical tensile strength at 77 K increased from 7 kg to 17 kg, demonstrating enhanced mechanical properties. The original Bi-based superconducting wire and the low-cost, high-strength Bi-based superconducting wire prepared in this example exhibited identical superconducting critical current-carrying performance, with both exhibiting a superconducting critical current of 17 A at 77 K. This further confirms that the electrochemical Ag reduction and copper deposition processes have no impact on the performance of the superconducting core wire.

[0081] In this embodiment, by using copper to replace the precious metal Ag in the Bi-based superconducting wire, the cost of the Bi-based superconducting wire is reduced by 47.924% without reducing the current-carrying performance. The enhanced mechanical properties enable the Bi-based superconducting wire to be used in conditions where the magnetic field or pressure is increased by more than 30%, thereby broadening the application field of the Bi-based superconducting wire.

[0082] Figure 3 is a schematic structural diagram of the Bi-based superconducting tape used in this embodiment 1, including a superconducting core wire 1, an Ag layer coated on the outside of the superconducting core wire 1, and an Ag alloy layer 3 coated on the outermost layer; Figure 4 is a schematic structural diagram of the low-cost, high-strength Bi-based superconducting tape prepared in this embodiment, including a superconducting core wire 1, an Ag layer coated on the outside of the superconducting core wire 1, and a Cu layer 4 coated on the outermost layer; By comparing Figures 3 and 4, it can be seen that the present invention adopts electrochemical Ag reduction technology and electrochemical material addition method to remove the Ag alloy layer on the surface of the Bi-based superconducting wire strip and plate a high-strength Cu layer instead.

[0083] Example 3

[0084] This embodiment includes the following steps:

[0085] Step 1: Surface scrubbing: Use a cotton cloth moistened with ethanol to scrub the surface of the Bi-based superconducting tape to remove dirt remaining on the surface of the Bi-based superconducting tape during the heat treatment process;

[0086] Step 2: Electrochemical silver reduction: Connect the Bi-based superconducting tape after scrubbing in step 1 to the positive electrode of a regulated power supply, and connect the graphite electrode to the negative electrode of the regulated power supply. The width of the graphite electrode is 20 mm, the width of the Bi-based superconducting tape is 4 mm, and the width of the graphite electrode is 5 times the width of the Bi-based superconducting tape. Then, the scrubbed Bi-based superconducting tape and the graphite electrode are mounted on a bracket in parallel, and placed in an electrolyte for electrochemical silver reduction. The distance between the Bi-based superconducting tape and the graphite electrode is 5 cm. The electrolyte is a 10 g / L AgNO3 solution, and the pH of the AgNO3 solution is adjusted to 5 using sodium hydroxide. During the electrochemical silver reduction process, the current density on the surface of the Bi-based superconducting tape is adjusted to 10 A / dm 2 The power-on time is 0.1 min, which removes the Ag alloy layer on the surface of the Bi-based superconducting tape, revealing the silver layer on the surface of the superconducting core wire of the outer layer of the Bi-based superconducting tape, and at the same time forms electroplated Ag with a mass purity of 99.99% on the surface of the graphite electrode;

[0087] Step 3: Same as Example 1;

[0088] Step 4: The difference from Example 1 is that the distance between the cleaned Bi-based superconducting wire strip and the copper sheet is 5 cm, the electrochemical additive solution contains 20 g / L copper chloride and 50 g / L sulfuric acid, and the current density on the surface of the Bi-based superconducting tape is adjusted to 10 A / dm during the surface enhancement treatment. 2 The processing time is 0.1 min, and a Cu layer with a thickness of 10 μm is formed on the surface of the Bi-based superconducting tape, thereby obtaining a low-cost and high-strength Bi-based superconducting tape.

[0089] Testing revealed that the Ag content of the low-cost, high-strength Bi-based superconducting tape prepared in this example was reduced from 66% to 45% of the original Bi-based superconducting tape, achieving a cost reduction of 30.179%. The fracture strength increased from 90 MPa to 94 MPa in the original Bi-based superconducting tape to 98 MPa, and the critical superconducting tensile strength at 77 K increased from 5 g to 5.5 kg. The original Bi-based superconducting tape and the low-cost, high-strength Bi-based superconducting tape prepared in this example exhibited identical superconducting critical current-carrying performance, with both exhibiting a superconducting critical current of 56 A at 77 K. This further confirms that the electrochemical Ag reduction and electrochemical copper deposition processes have no impact on the performance of the superconducting core. While its mechanical properties did not significantly improve, the critical bending radius of the low-cost, high-strength Bi-based superconducting tape was reduced from 3 cm to 2.5 cm, enabling its application in applications with even smaller bending radii.

[0090] Example 4

[0091] This embodiment includes the following steps:

[0092] Step 1: Same as Example 1;

[0093] Step 2: Electrochemical silver reduction: Connect the Bi-based superconducting tape after scrubbing in step 1 to the positive electrode of a regulated power supply, and connect the graphite electrode to the negative electrode of the regulated power supply. The width of the graphite electrode is 12 mm, the width of the Bi-based superconducting tape is 4 mm, and the width of the graphite electrode is 3 times the width of the Bi-based superconducting tape. Then, install the scrubbed Bi-based superconducting tape and the graphite electrode in parallel on a bracket and place them in an electrolyte for electrochemical silver reduction. The distance between the Bi-based superconducting tape and the graphite electrode is 3.5 cm. The electrolyte is a 6 g / L AgNO3 solution, and the pH of the AgNO3 solution is adjusted to 4 using sodium hydroxide. The current density on the surface of the Bi-based superconducting tape during the electrochemical silver reduction process is adjusted to 5 A / dm 2 The power-on time is 3 minutes, which removes the Ag alloy layer on the surface of the Bi-based superconducting tape, revealing the silver layer on the surface of the superconducting core wire of the outer layer of the Bi-based superconducting tape, and at the same time forms electroplated Ag with a purity of 99.99% on the surface of the graphite electrode;

[0094] Step 3: Same as Example 1;

[0095] Step 4: The difference from Example 1 is that the distance between the cleaned Bi-based superconducting wire strip and the copper sheet is 3.5 cm, the electrochemical additive solution contains 10 g / L copper sulfate and 30 g / L citric acid, and the current density on the surface of the Bi-based superconducting tape is adjusted to 5 A / dm during the surface enhancement treatment. 2 The processing time is 10 minutes, and a Cu layer with a thickness of 40 μm is formed on the surface of the Bi-based superconducting tape, thereby obtaining a low-cost and high-strength Bi-based superconducting tape.

[0096] Testing revealed that the Ag content of the low-cost, high-strength Bi-based superconducting tape prepared in this example was reduced from 60% to 40% of the original Bi-based superconducting tape, achieving a cost reduction of 31.451%. The fracture strength increased from 90 MPa to 94 MPa in the original Bi-based superconducting tape to 124 MPa, and the superconducting critical tensile strength at 77 K increased from 5 kg to 16 kg, demonstrating enhanced mechanical properties. The original Bi-based superconducting tape and the low-cost, high-strength Bi-based superconducting tape prepared in this example exhibited identical superconducting critical current-carrying performance, with both exhibiting a superconducting critical current of 52 A at 77 K. This further confirms that the electrochemical Ag reduction and copper deposition processes have no impact on the performance of the superconducting core.

[0097] In this embodiment, by using copper to replace the precious metal Ag in the Bi-based superconducting tape, the raw material cost of the Bi-based superconducting tape is reduced by 49% without reducing the current-carrying performance. The enhanced mechanical properties enable the Bi-based superconducting tape to be used in more stringent conditions where the magnetic field or pressure is increased by more than 30%, thereby broadening the application areas of the Bi-based superconducting tape.

[0098] Example 5

[0099] The differences between this embodiment and embodiment 2 are as follows: the distance between the cleaned Bi-based superconducting wire and the copper sheet in step 4 is 2 cm; the electrochemical additive solution contains 3 g / L copper sulfate and 10 g / L citric acid; the surface enhancement treatment time is 10 minutes, and a Cu layer with a thickness of 25 μm is formed on the surface of the Bi-based superconducting wire.

[0100] After testing, the Ag content in the low-cost, high-strength Bi-based superconducting wire prepared in this embodiment was reduced from 80% of the original Bi-based superconducting wire to 50%, which reduced the raw material cost of the Bi-based superconducting tape by 30% without reducing the current-carrying performance. The original Bi-based superconducting wire and the low-cost, high-strength Bi-based superconducting wire prepared in this embodiment showed completely consistent performance in terms of superconducting critical current-carrying performance, with the superconducting critical current under 77K self-field being 16A. This further confirms that the electrochemical Ag reduction and electrochemical copper deposition processes have no effect on the performance of the superconducting core wire. Although its fracture strength and superconducting critical tensile strength at 77K did not change, the critical bending radius of the low-cost, high-strength Bi-based superconducting wire was reduced from the original 12.5cm to 10cm, making it suitable for applications in areas with smaller bending radii.

[0101] Comparative Example 1

[0102] The method of mechanically reducing Ag and soldering copper strip reinforcement is adopted. The specific steps are as follows:

[0103] First, an electric planer on a CNC machining center mechanically removes Ag with a 5-micron cut depth. After 10 passes, the Ag on the surface of the Bi-based superconducting tape is successfully removed. However, while this method produces a high-purity Ag byproduct, each pass generates stress and even strain, which can damage the ceramic superconducting core. Furthermore, each pass causes the critical current of the superconducting tape to drop by 5-10%.

[0104] Similar to Example 1, this mechanical Ag reduction method reduces the Ag content in the superconducting tape by half, but the current carrying performance of the superconducting tape decreases by nearly 70%. In contrast, the electrochemical Ag reduction method of Example 1 of this patent reduces the Ag content to the same level without affecting the current carrying performance of the superconducting tape.

[0105] Next, the Ag content in the superconducting tape after mechanical Ag reduction was reduced to half, and then the copper strip was reinforced with solder. This method can increase the strength of the tape to 150 MPa. However, if a completely natural soldering process is used, the excessive solder thickness will cause the cross-sectional area of ​​the tape to increase by nearly 100%. This not only affects the dimensional uniformity of the tape, but also reduces the engineering critical current density of the tape by half.

[0106] If pressure-assisted soldering is used, the external pressure allows the solder between the reinforcement tape and the superconducting tape to be expelled as much as possible, maintaining the weld strength between the two tapes and ultimately maintaining the uniformity of the reinforcement tape's dimensions. However, external pressure can also damage the ceramic core of the Bi-based superconducting tape, resulting in a decrease in the tape's current-carrying performance by approximately 20%.

[0107] In contrast, in Example 1 of this patent, electrochemical additive manufacturing was performed on Ag-reduced superconducting tapes with the same Ag content. Since the electrochemical additive manufacturing process introduces almost no stress, the ceramic superconducting core of the superconducting tape is hardly affected before and after the electrochemical additive manufacturing, and thus the current-carrying performance of the final tape is not affected.

[0108] By comparison, it was found that although mechanical Ag reduction and welding copper strip reinforcement can nominally reduce the Ag content and enhance the mechanical strength of the Bi-based superconducting tape, the superconducting performance of the superconducting tape is reduced by nearly 90%; while the electrochemical Ag reduction and electrochemical material addition technology of the present invention can achieve a reduction of the Ag content by nearly 50% without reducing the superconducting performance, and the mechanical properties can be improved by at least 30%.

[0109] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent variation made to the above embodiment based on the essence of the invention technology shall still fall within the scope of protection of the technical solution of the present invention.

Claims

1. A method for preparing a low-cost high-strength Bi-based superconducting wire strip, characterized in that: The method comprises the following steps: Step 1, electrochemical silver reduction: connect the Bi-based superconducting wire strip to the positive electrode of a voltage-stabilized power supply, connect the graphite electrode to the negative electrode of the voltage-stabilized power supply, and then install the Bi-based superconducting wire strip and the graphite electrode in parallel on a bracket, put them into an electrolyte for electrochemical silver reduction, and remove the Ag alloy layer on the surface of the Bi-based superconducting wire strip; Step 2, surface enhancement: connect the Bi-based superconducting wire strip after electrochemical silver reduction in step 1 to the negative electrode of a voltage-stabilized power supply, connect the copper sheet to the positive electrode of the voltage-stabilized power supply, and then install the Bi-based superconducting wire strip after electrochemical silver reduction and the copper sheet in parallel on a bracket, put them into an electrochemical additive solution for surface enhancement treatment, form a Cu layer on the surface of the Bi-based superconducting wire strip, and obtain the low-cost and high-strength Bi-based superconducting wire strip.

2. The method for preparing a low-cost, high-strength Bi-based superconducting wire strip according to claim 1, characterized in that: The width of the graphite electrode in step 1 is greater than or equal to 3 times the width or diameter of the Bi-based superconducting wire strip, preferably 3 to 5 times, more preferably 3 times; And / or, the electrolyte is a 2 g / L to 10 g / L soluble silver salt deionized water solution, and the pH of the soluble silver salt deionized water solution is adjusted to 3 to 5 using a metal hydroxide; Preferably, the concentration of the soluble silver salt deionized water solution is 6 g / L.

3. The method for preparing a low-cost, high-strength Bi-based superconducting wire strip according to claim 2, characterized in that: The soluble silver salt is selected from one of silver nitrate, silver fluoride, silver chlorate and silver perchlorate; And / or, the metal hydroxide is selected from one of sodium hydroxide, potassium hydroxide, barium hydroxide and lithium hydroxide.

4. The method for preparing a low-cost, high-strength Bi-based superconducting wire strip according to claim 1, characterized in that: In step 1, the distance between the Bi-based superconducting wire strip and the graphite electrode is 1 cm to 5 cm, preferably 3.5 cm; And / or, the current density on the surface of the Bi-based superconducting wire strip is 0.1A / dm 2 ~10A / dm 2 , preferably 5A / dm 2 ; And / or, the power-on time is 0.1 min to 30 min, preferably 3 min.

5. The method for preparing a low-cost and high-strength Bi-based superconducting wire strip according to claim 1, characterized in that: The electrochemical additive solution in step 2 is a deionized water solution containing 0.1 g / L to 20 g / L of soluble copper salt and 10 g / L to 50 g / L of acidic substance; The concentration of the soluble copper salt is preferably 10 g / L; The concentration of the acidic substance is preferably 30 g / L.

6. The method for preparing a low-cost, high-strength Bi-based superconducting wire strip according to claim 5, characterized in that: The soluble copper salt is selected from one of copper sulfate, copper chloride and copper nitrate; And / or, the acidic substance is selected from one of citric acid, sulfuric acid, hydrochloric acid, nitric acid and phosphoric acid.

7. The method for preparing a low-cost and high-strength Bi-based superconducting wire strip according to claim 1, characterized in that: In step 2, the distance between the Bi-based superconducting wire strip and the copper sheet is 2 cm to 5 cm, preferably 3.5 cm; And / or, the current density on the surface of the Bi-based superconducting wire strip is 0.1A / dm 2 ~10A / dm 2 , preferably 5A / dm 2 ; and / or, the treatment time is 0.1 min to 20 min, preferably 10 min; And / or, the thickness of the Cu layer is 10 μm to 40 μm, preferably 25 μm.

8. The method for preparing a low-cost, high-strength Bi-based superconducting wire strip according to claim 1, before step 1, the method further comprises: Surface scrubbing: ethanol is used to clean the surface of the Bi-based superconducting wire strip to remove the dirt remaining on the surface of the Bi-based superconducting wire strip.

9. The method for preparing a low-cost and high-strength Bi-based superconducting wire strip according to claim 1, before step 2, the method further comprises: Residual liquid cleaning: immerse the Bi-based superconducting wire strip after the electrochemical silver reduction in step 1 into high-purity water to clean and remove the electrolyte remaining on the surface.

10. A low-cost, high-strength Bi-based superconducting wire strip, characterized in that: The invention is prepared by the method for preparing a low-cost and high-strength Bi-based superconducting wire strip as claimed in any one of claims 1 to 9.

Citation Information

Patent Citations

  • High-strength Bi-2223 superconducting strip and manufacturing method thereof

    CN110875106A

  • Method for separating superconducting phase in silver-based copper oxide superconducting material

    CN113270235A

  • Preparation method of superconducting tape with small bending diameter, superconducting tape and superconducting cable

    CN114843044A

  • Preparation method of low-cost high-strength Bi-series superconducting wire strip

    CN116580892A

  • Thin film superconducting wire and superconducting cable conductor

    US20110244234A1

Cited By

  • Sampling method of superconducting layer in second-generation high-temperature superconducting tape