Modified aluminum alloy conductor and production process therefor, and modified aluminum alloy conductor cable
By adjusting the composition and process of aluminum alloy, the creep resistance and mechanical properties of aluminum alloy conductors are improved, and the problem of poor creep resistance of aluminum alloy conductors is solved, ensuring the reliability and safety of cable connections.
Patent Information
- Application Number
- PCT/CN2024/091789
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-28
AI Technical Summary
The poor creep resistance of existing aluminum alloy conductors leads to slipping and dislocation at the conductor connections, which poses safety hazards, especially during the cable laying process, which may lead to unsafe and reliable operation of the cable.
By adjusting the composition of the aluminum alloy, the mass ratio of Fe to Si is controlled to be 12-15:1, and the mass ratio of Al to Cu is 350-490:1. Electromagnetic purification filtration and annealing process are adopted to improve the tensile strength and fracture of the conductor. Elongation and repeated bending times ensure that the conductor has good creep resistance and mechanical properties.
It significantly improves the creep resistance and mechanical properties of aluminum alloy conductors, avoids slippage at the conductor connection, ensures the safe and reliable operation of the cable, and extends the service life of the cable.
Smart Images

Figure PCTCN2024091789-FTAPPB-I100001 
Figure PCTCN2024091789-FTAPPB-I100002 
Figure PCTCN2024091789-FTAPPB-I100003
Abstract
Description
Modified aluminum alloy conductor and its production process, modified aluminum alloy conductor cable
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 24, 2023, with application number 202310593286.8 and application name “Modified aluminum alloy conductor and its production process, modified aluminum alloy conductor cable”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present invention relates to the technical field of aluminum alloy processing, and in particular to a modified aluminum alloy conductor and a production process thereof, and a modified aluminum alloy conductor cable. Background Art
[0003] Traditional aluminum cables have drawbacks such as low strength, susceptibility to creep, poor corrosion resistance, and the tendency to form a strong oxide film on the surface, which increases contact resistance. Therefore, their application is greatly limited. Aluminum alloy cables significantly enhance the mechanical properties of aluminum alloy conductors by adding alloying elements to electrical aluminum and adjusting the process. This avoids the low elongation, poor creep resistance, and poor flexibility associated with pure aluminum conductors, thereby improving cable connection reliability.
[0004] In recent years, aluminum alloy cables have been widely used in photovoltaic and offshore wind power projects. During cable installation and operation, some cables become submerged in water, sometimes even completely submerged. To ensure safe and reliable operation, the demand for waterproof aluminum alloy cables is growing. However, existing aluminum conductor cables on the market suffer from poor creep resistance. As the cables age, conductor connections are prone to slippage, posing safety risks to both production and domestic electricity use.
[0005] Summary of the Invention
[0006] The main purpose of the present invention is to provide a modified aluminum alloy conductor and its production process, and a modified aluminum alloy conductor cable, so as to solve the problem of poor creep resistance of aluminum alloy conductors in the prior art leading to potential safety hazards.
[0007] To achieve the above object, according to one aspect of the present invention, a modified aluminum alloy conductor is provided. The modified aluminum alloy conductor comprises, by mass percentage, 0.03-0.06 wt% Si, 0.50-0.80 wt% Fe, 0.20-0.30 wt% Cu, Mg≤0.01 wt%, Zn≤0.02 wt%, B≤0.04 wt%, a total content of unavoidable impurities≤0.08 wt%, and the balance being Al.
[0008] Furthermore, the mass ratio of Fe to Si in the modified aluminum alloy conductor is 12 to 15:1.
[0009] Furthermore, the mass ratio of Al to Cu in the modified aluminum alloy conductor is 350-490:1.
[0010] Furthermore, the tensile strength of the single wire of the modified aluminum alloy conductor is ≥105N / mm 2 , the elongation at break of single yarn is ≥15%, and the number of repeated bending of single yarn is ≥23 times.
[0011] Furthermore, the creep resistance of the modified aluminum alloy conductor is ≥70%.
[0012] According to another aspect of the present invention, a production process for a modified aluminum alloy conductor is provided, comprising, in sequence, a batching step, a smelting and casting step, a refining step, a purification step, a slab casting step, a rod rolling step, and a finished product annealing step. The smelting and casting step comprises, in sequence, primary filtration and fine filtration of the aluminum alloy liquid to obtain filtered aluminum alloy liquid, wherein the fine filtration process is performed using electromagnetic purification.
[0013] Furthermore, the above-mentioned fine filtration process includes: passing the filtrate obtained from the primary filtration through the first-level magnetic field and the second-level magnetic field in sequence, the magnetic field strength of the first-level magnetic field is smaller than the magnetic field strength of the second-level magnetic field, preferably the magnetic field strength of the first-level magnetic field is 0.3T~0.5T, and preferably the magnetic field strength of the second-level magnetic field is 0.6T~0.8T.
[0014] Furthermore, a 30 / 50PPI double-stage ceramic filter plate is used for primary filtration. Preferably, the removal rate of non-metallic impurity particles ≥1μm in the aluminum alloy liquid after filtration is ≥90%, and the impurity content of non-metallic impurity particles in the aluminum alloy liquid after filtration is preferably 0.010~0.022mm 2 / kg.
[0015] Furthermore, the temperature in the finished product annealing step is controlled between 310° C. and 340° C., and the finished product annealing time is preferably controlled between 8 hours and 12 hours.
[0016] According to another aspect of the present invention, a modified aluminum alloy conductor cable is provided, comprising a conductor, which is the aforementioned modified aluminum alloy conductor.
[0017] By applying the technical solution of the present invention, the composition of the aluminum alloy is adjusted, and the content of components such as copper and iron is reasonably controlled, the synergistic effect between the components is maximized, ensuring that the aluminum alloy conductor has good creep resistance, mechanical properties, flexibility and electrical properties, thereby improving the connection reliability of the cable, avoiding slippage at the conductor connection, and ensuring safe and reliable operation of the cable. DETAILED DESCRIPTION
[0018] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the embodiments.
[0019] As analyzed in the background technology of this application, the poor creep resistance of aluminum alloy conductors in the prior art leads to safety hazards. To solve this problem, this application provides a modified aluminum alloy conductor and its production process, and a modified aluminum alloy cable.
[0020] In a typical embodiment of the present application, a modified aluminum alloy conductor is provided. The modified aluminum alloy conductor includes, by mass percentage, 0.03-0.06 wt% Si, 0.50-0.80 wt% Fe, 0.20-0.30 wt% Cu, Mg≤0.01 wt%, Zn≤0.02 wt%, B≤0.04 wt%, a total content of unavoidable impurities≤0.08 wt%, and the balance is Al.
[0021] This application adjusts the aluminum alloy composition and reasonably controls the content of components such as copper and iron, thereby maximizing the synergistic effect between the components and ensuring that the aluminum alloy conductor has good creep resistance, mechanical properties, flexibility and electrical properties, thereby improving the connection reliability of the cable, avoiding slippage at the conductor connection, and ensuring safe and reliable operation of the cable.
[0022] In one embodiment of the present application, the mass ratio of Fe to Si in the modified aluminum alloy conductor is 12-15:1.
[0023] Fe usually exists as an impurity element in aluminum alloys. In the presence of Si, FeAl3 phase, α(Al 12 Fe3Si2) phase, β(Al9Fe2Si2) phase, etc. These iron-rich phases have high hardness, which is beneficial to improve the strength and creep resistance of the alloy, but at the same time it will also reduce the plasticity of the alloy. 12 The Fe3Si2) phase is in regular, blocky form and has little effect on the alloy's plasticity. By adjusting the Fe / Si ratio within the above range, the iron-rich phase is primarily precipitated as the α(Al9Fe2Si2) phase, effectively improving the strength of the aluminum alloy while minimizing the adverse effects of Fe on its plasticity.
[0024] In one embodiment of the present application, the mass ratio of Al to Cu in the modified aluminum alloy conductor is 350-490:1.
[0025] A small amount of Cu added to an aluminum alloy forms a CuAl2 compound with aluminum, dissolving into a solid solution and precipitating as a metallic compound during heat treatment, thereby improving the electrical conductivity of the aluminum alloy. Furthermore, the present application preferably controls the mass ratio of Al to Cu within the aforementioned range, which further contributes to improving the electrical conductivity and other properties of the modified aluminum alloy conductor.
[0026] In some embodiments of the present application, the single-filament tensile strength of the modified aluminum alloy conductor is preferably ≥105N / mm 2 , the elongation at break of single yarn is ≥15%, and the number of repeated bending of single yarn is ≥23 times.
[0027] The above properties of the modified aluminum alloy conductor monofilament make the corresponding modified aluminum alloy conductor have excellent mechanical properties and flexibility.
[0028] In some embodiments of the present application, the creep resistance of the modified aluminum alloy conductor is preferably ≥70%, which is more helpful in avoiding phenomena such as slippage at the conductor connection and ensuring safe and reliable operation of the cable.
[0029] In another typical embodiment of the present application, a production process for a modified aluminum alloy conductor is provided, which sequentially comprises: a batching step, a smelting and casting step, a refining step, a purification step, a slab casting step, a rod rolling step, and a finished product annealing step. The smelting and casting step includes: performing primary filtration and fine filtration on the aluminum alloy liquid in sequence to obtain filtered aluminum alloy liquid, wherein the fine filtration process is performed using electromagnetic purification.
[0030] In the production process of modified aluminum alloy conductors, the aluminum alloy liquid is subjected to primary filtration and fine filtration in sequence, which helps to fully filter and remove impurities in the aluminum alloy metal melt, thereby improving the electrical conductivity and fatigue resistance of the aluminum alloy.
[0031] In one embodiment of the present application, the above-mentioned fine filtration process includes: passing the filtrate obtained by primary filtration through the first-level magnetic field and the second-level magnetic field in sequence, the magnetic field strength of the first-level magnetic field is smaller than the magnetic field strength of the second-level magnetic field, preferably the magnetic field strength of the first-level magnetic field is 0.3~0.5T, and preferably the magnetic field strength of the second-level magnetic field is 0.6~0.8T.
[0032] Through the sequential action of the first-level magnetic field in the weak zone and the second-level magnetic field in the strong zone, the separation effect of non-metallic impurity particles and metal particles is effectively improved. Overall, the removal efficiency of particles larger than 10μm reaches more than 98%, thereby greatly eliminating non-metallic slag inclusions inside the aluminum alloy, promoting the purification of the melt, and improving its conductive properties.
[0033] In one embodiment of the present application, a 30 / 50PPI double-stage ceramic filter plate is used for the primary filtration. Preferably, the removal rate of non-metallic impurity particles ≥1μm in the aluminum alloy liquid after filtration is ≥90%, and the impurity content of non-metallic impurity particles in the aluminum alloy liquid after filtration is preferably 0.010~0.022mm 2 / kg.
[0034] The above primary filtration helps remove non-metallic impurity particles with a particle size of 10 μm or larger. The removal rate of non-metallic impurity particles and the inclusion content in the aluminum alloy liquid after the above filtration preferably help significantly improve the fatigue resistance of the aluminum alloy material. The components in the aluminum alloy liquid other than Al, Si, Fe, Cu, Mg, Zn, and B are all impurities.
[0035] A reasonable finished product annealing process helps improve the microstructure of the aluminum alloy, reduce internal stress, and enhance its mechanical properties and electrical conductivity. Furthermore, the temperature in the finished product annealing step is preferably controlled between 310° C. and 340° C., and the finished product annealing time is preferably controlled between 8 and 12 hours, thereby optimizing the overall performance of the modified aluminum alloy conductor. Compared with before finished product annealing, the tensile strength of the conductor single wire after finished product annealing is reduced by 15 to 20%, the elongation at break is increased by 400 to 600%, and the resistivity is reduced by 10 to 15%.
[0036] In another typical embodiment of the present application, a modified aluminum alloy conductor cable is provided, comprising a conductor, which is the aforementioned modified aluminum alloy conductor.
[0037] The aforementioned modified aluminum alloy conductor has good creep resistance, mechanical properties, flexibility and electrical properties, so that the cable including the modified aluminum alloy conductor has high connection reliability, avoids phenomena such as slippage at the conductor connection, and ensures safe and reliable operation of the cable.
[0038] Furthermore, the cable of this application utilizes a longitudinally wrapped aluminum-plastic composite tape + extruded waterproof PE sheath as the radial waterproof layer of the cable. After soaking the cable sample in water for 120 hours and removing the composite layer outside the insulation, the outer surface of the insulation layer was observed to be dry by naked eye. This prevents water treeing in cables laid directly in water during power engineering applications, ultimately preventing cable breakdown, extending the cable's service life, and improving economic efficiency.
[0039] The beneficial effects of the present application will be further illustrated below with reference to examples.
[0040] Example 1
[0041] Table 1
[0042] After weighing and mixing the ingredients according to the composition table in Table 1, the modified aluminum alloy conductor is obtained by sequentially performing a mixing step, a smelting and purification step, a continuous casting and rolling step, a finished product annealing step, a finished product slitting step, a finished product testing step, and a finished product packaging step, wherein the mass ratio of Fe to Si is 12:1, and the mass ratio of Al to Cu is 395.8:1.
[0043] In the smelting purification step, a 30 / 50PPI two-stage ceramic filter plate is used to perform primary filtration on the aluminum alloy liquid to obtain a filtrate; the filtrate is sequentially passed through an alternating electromagnetic field electromagnetic purification device for fine filtration. Specifically, the fine filtration process includes: sequentially passing the filtrate through a first-stage magnetic field with a magnetic field strength of 0.4T and a second-stage magnetic field with a magnetic field strength of 0.7T to obtain a filtered aluminum alloy liquid.
[0044] Continuous casting and rolling process, melting temperature is 780℃, casting temperature is 720℃, crystallization wheel speed during casting is 0.2~0.4m / s, cooling water pressure is 0.03MPa; inlet temperature of the billet into the rolling mill is 500~520℃, cooling emulsion temperature is 50℃, and cooling emulsion dosage is 1m 3 / min, the final temperature of the rolled wire billet is above 480℃, the online quenching temperature is 460℃, and the rolling speed is 5.0-6.0m / s.
[0045] The temperature of the finished product annealing step is between 320° C. and the time is 10 hours. Finally, after finished product slitting, finished product testing, and finished product packaging, the modified aluminum alloy conductor is obtained.
[0046] Example 2
[0047] The difference from Example 1 is that
[0048] Table 2
[0049] According to Table 2, the modified aluminum alloy conductor is obtained by sequentially performing the batching step, the melting and casting step, the refining step, the purification step, the billet casting step, the rod rolling step, the finished product annealing step, the finished product slitting, the finished product testing, and the finished product packaging. The modified aluminum alloy conductor has a mass ratio of Fe to Si of 15:1 and a mass ratio of Al to Cu of 395.84:1.
[0050] Example 3
[0051] The difference from Example 1 is that
[0052] Table 3
[0053] According to Table 3, the modified aluminum alloy conductor is obtained by sequentially performing the batching step, the melting and casting step, the refining step, the purification step, the billet casting step, the rod rolling step, the finished product annealing step, the finished product slitting, the finished product testing, and the finished product packaging. The modified aluminum alloy conductor has a mass ratio of Fe to Si of 8.3:1 and a mass ratio of Al to Cu of 396.16:1.
[0054] Example 4
[0055] The difference from Example 1 is that
[0056] Table 4
[0057] According to Table 4, the modified aluminum alloy conductor is obtained by sequentially performing the batching step, the melting and casting step, the refining step, the purification step, the billet casting step, the rod rolling step, the finished product annealing step, the finished product slitting, the finished product testing, and the finished product packaging. The modified aluminum alloy conductor has a mass ratio of Fe to Si of 26.67:1 and a mass ratio of Al to Cu of 430:1.
[0058] Example 5
[0059] The difference from Example 1 is that
[0060] Table 5
[0061] According to Table 5, the modified aluminum alloy conductor is obtained by sequentially performing the batching step, the melting and casting step, the refining step, the purification step, the billet casting step, the rod rolling step, the finished product annealing step, the finished product slitting, the finished product testing, and the finished product packaging, wherein the mass ratio of Al to Cu is 329.7:1.
[0062] Example 6
[0063] The difference from Example 1 is that
[0064] Table 6
[0065] According to Table 6, the modified aluminum alloy conductor is obtained by sequentially performing the batching step, the melting and casting step, the refining step, the purification step, the billet casting step, the rod rolling step, the finished product annealing step, the finished product slitting, the finished product testing, and the finished product packaging, wherein the mass ratio of Al to Cu is 495:1.
[0066] Example 7
[0067] The difference from Example 1 is that
[0068] Table 7
[0069] According to Table 7, the modified aluminum alloy conductor is obtained by sequentially performing the batching step, the melting and casting step, the refining step, the purification step, the billet casting step, the rod rolling step, the finished product annealing step, the finished product slitting, the finished product testing, and the finished product packaging, wherein the mass ratio of Al to Cu is 396:1.
[0070] Example 8
[0071] The difference from Example 1 is that
[0072] Table 8
[0073] According to Table 8, the modified aluminum alloy conductor is obtained by sequentially performing the batching step, the melting and casting step, the refining step, the purification step, the billet casting step, the rod rolling step, the finished product annealing step, the finished product slitting, the finished product testing, and the finished product packaging, wherein the mass ratio of Al to Cu is 350:1.
[0074] Example 9
[0075] The difference from Example 1 is that
[0076] Table 9
[0077] According to Table 9, the modified aluminum alloy conductor is obtained by sequentially performing the batching step, the melting and casting step, the refining step, the purification step, the ingot casting step, the rod rolling step, the finished product annealing step, the finished product slitting, the finished product testing, and the finished product packaging, wherein the mass ratio of Al to Cu is 490:1.
[0078] Example 10
[0079] The difference from Example 1 is that a 30 / 50PPI two-stage ceramic filter plate is used to perform primary filtration on the aluminum alloy liquid to obtain a filtrate; and an electromagnetic purification device is used to perform a one-step fine filtration under a magnetic field strength of 0.7T to obtain a filtered aluminum alloy liquid.
[0080] Example 11
[0081] The difference from Example 1 is that the magnetic field strength of the first-level magnetic field is 0.3T, and the magnetic field strength of the second-level magnetic field is 0.6T.
[0082] Example 12
[0083] The difference from Example 1 is that the magnetic field strength of the first-level magnetic field is 0.5T, and the magnetic field strength of the second-level magnetic field is 0.8T.
[0084] Example 13
[0085] The difference from Example 1 is that the magnetic field strength of the first-level magnetic field is 0.2T, and the magnetic field strength of the second-level magnetic field is 0.4T.
[0086] Example 14
[0087] The difference from Example 1 is that the temperature in the final annealing step is 310°C.
[0088] Example 15
[0089] The difference from Example 1 is that the temperature in the final annealing step is 340°C.
[0090] Example 16
[0091] The difference from Example 1 is that the temperature in the final annealing step is 300°C.
[0092] Comparative Example 1
[0093] The difference from Example 1 is that
[0094] Table 10
[0095] According to Table 10, the modified aluminum alloy conductor is obtained by sequentially performing the batching step, the melting and casting step, the refining step, the purification step, the billet casting step, the rod rolling step, the finished product annealing step, the finished product slitting, the finished product testing, and the finished product packaging.
[0096] Comparative Example 2
[0097] The difference from Example 1 is that a 30 / 50PPI double-stage ceramic filter plate is used to filter the aluminum alloy liquid to obtain filtered aluminum alloy liquid.
[0098] The tensile strength, elongation at break, number of repeated bending times of the monofilament, creep resistance and resistivity of the modified aluminum alloy conductor monofilament obtained in the above Examples 1 to 16, Comparative Example 1 and Comparative Example 2 were tested, and the test results are listed in Table 11.
[0099] Among them, the test method for the creep resistance of the modified aluminum alloy conductor is as follows:
[0100] 1. Test equipment: creep testing machine
[0101] 2. Sample preparation: Cut a 130mm cable sample from the straightened cable core of the finished cable test section, retain 40mm at each end, and take the middle 50mm to cut and strip the insulation to expose the cable conductor to obtain the cable conductor sample.
[0102] 3. Test steps
[0103] (1) Installing the sample: A clamp is used to clamp the cable conductor sample in the creep testing machine. The clamp is in the shape of two arc concave surfaces with a clamp width of 10 mm. The inner diameter of the arc is similar to the outer diameter of the conductor. The inner diameter of the clamp corresponding to the conductor cross section is shown in Table 11. The arc angle is 150°. During the test, the arc concave surface contacts the outer surface of the cable conductor sample, and the planes of the upper and lower clamps contact the upper and lower pressure plates of the creep testing machine respectively.
[0104] Table 11
[0105] (2) Set the test conditions: Adjust the temperature in the test chamber to the test temperature of 130℃ and preheat for 30 minutes. Pre-press the sample with a pre-pressing amount of 10% of the conductor's outer diameter. Measure the conductor's outer diameter using the paper tape method and calculate 10% of the conductor's outer diameter as the conductor's indentation. Before pre-pressing, manually adjust the pressure plate close to the upper surface of the fixture and stop when the pressure value is displayed. The reading should not be greater than 20N. Then, set the conductor indentation amount through the automatic control system. Stop pressing when the pressure reaches the specified amount. Record the pressure value displayed on the creep tester, which is the initial pressure value.
[0106] (3) Monitoring and recording: Under the action of high temperature and pressure, the creep of the conductor will cause relaxation between the fixture and the conductor, and between the individual conductor wires, and the pressure value will gradually decrease. As time goes by, the compressive stress value will gradually tend to a stable value. From the start of the test to the stabilization of the pressure value, a pressure change curve can be formed in which the pressure gradually decreases over time and then slowly stabilizes. Monitor and record the pressure value change curve over time within 100 hours of the creep test, as well as the pressure value at the end of the test, that is, the pressure stability value.
[0107] (4) Calculate the ratio of the pressure stability value to the pressure initial value to assess the anti-creep performance of the cable conductor. The higher the ratio, the better the anti-creep performance of the surface conductor.
[0108] 4. Result evaluation
[0109] Under the above test conditions, the indicator for evaluating the creep resistance of aluminum alloy cable conductors is the residual pressure value of the conductor after 100 hours, that is, the ratio of the stable pressure value to the initial pressure value. The assessment standard is no less than 60%. That is, under the specified test conditions, if the residual pressure value is no less than 60%, the sample's creep resistance is qualified; if it is less than 60%, it is unqualified.
[0110] The test method or standard for the tensile strength of monofilament is GB / T 4909.3.
[0111] The test method or standard for single-filament elongation at break is GB / T 4909.3.
[0112] The test method or standard for the number of repeated bending times of a single wire is GB / T 4909.5
[0113] The test method or standard for resistivity is GB / T 3048.2.
[0114] Table 12
[0115] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0116] This application adjusts the aluminum alloy composition and reasonably controls the content of components such as copper and iron, thereby maximizing the synergistic effect between the components and ensuring that the aluminum alloy conductor has good creep resistance, mechanical properties, flexibility and electrical properties, thereby improving the connection reliability of the cable, avoiding slippage at the conductor connection, and ensuring safe and reliable operation of the cable.
[0117] The foregoing description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art will readily appreciate that various modifications and variations of the present invention are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention are intended to be within the scope of protection of the present invention.
Claims
1. A modified aluminum alloy conductor, characterized in that: In terms of mass percentage, the modified aluminum alloy conductor includes: 0.03-0.06wt% Si, 0.50-0.80wt% Fe, 0.20-0.30wt% Cu, Mg≤0.01wt%, Zn≤0.02wt%, B≤0.04wt%, the total content of inevitable impurities≤0.08wt%, and the balance is Al.
2. The modified aluminum alloy conductor according to claim 1, characterized in that: The mass ratio of Fe to Si in the modified aluminum alloy conductor is 12 to 15:
1.
3. The modified aluminum alloy conductor according to claim 1 or 2, characterized in that: The mass ratio of Al to Cu in the modified aluminum alloy conductor is 350-490:
1.
4. The modified aluminum alloy conductor according to any one of claims 1 to 3, characterized in that: The single-filament tensile strength of the modified aluminum alloy conductor is ≥105N / mm 2 , the elongation at break of single yarn is ≥15%, and the number of repeated bending of single yarn is ≥23 times.
5. The modified aluminum alloy conductor according to any one of claims 1 to 4, characterized in that: The creep resistance of the modified aluminum alloy conductor is ≥70%.
6. A production process for a modified aluminum alloy conductor, comprising: The process comprises a batching step, a smelting and casting step, a refining step, a purification step, a billet casting step, a rod rolling step, and a finished product annealing step, wherein the smelting and casting step comprises: performing primary filtration and fine filtration on the aluminum alloy liquid in sequence to obtain filtered aluminum alloy liquid, wherein the fine filtration process is performed by electromagnetic purification.
7. The production process according to claim 6, characterized in that: The fine filtration process includes: passing the filtrate obtained from the primary filtration through the first magnetic field and the second magnetic field in sequence, the magnetic field strength of the first magnetic field is smaller than the magnetic field strength of the second magnetic field, preferably the magnetic field strength of the first magnetic field is 0.3-0.5T, and preferably the magnetic field strength of the second magnetic field is 0.6-0.8T.
8. The production process according to claim 6 or 7, characterized in that: The primary filtration is performed using a 30 / 50PPI double-stage ceramic filter plate. Preferably, the removal rate of non-metallic impurity particles ≥1μm in the aluminum alloy liquid after filtration is ≥90%. Preferably, the impurity content of non-metallic impurity particles in the aluminum alloy liquid after filtration is 0.010-0.022mm 2 / kg.
9. The production process according to any one of claims 6 to 8, characterized in that: The temperature in the finished product annealing step is controlled between 310° C. and 340° C., and the finished product annealing time is preferably controlled between 8 h and 12 h.
10. A modified aluminum alloy conductor cable, comprising a conductor, characterized in that: The conductor is the modified aluminum alloy conductor according to any one of claims 1 to 5.
Citation Information
Patent Citations
Modified aluminum alloy conductor, production process thereof and modified aluminum alloy conductor cable
CN116435003A
Interlocking type armored optical fiber composite low-voltage cable of creep-resistant aluminum alloy conductor
CN102222546A
High-conductivity creep-resistant aluminum-alloy conductor and manufacturing method thereof
CN102912193A
Aluminum alloy material, aluminum alloy wire and preparation method of aluminum alloy wire
CN113234966A
Aluminum alloy material and preparation method and application thereof
CN114737089A