Carbon material graphite crystallization and growth method and application thereof

By using molten salt medium under the protection of inert gas, carbon materials come into contact with activated materials for graphite crystallization and growth, the problems of high temperature, high energy consumption and size limitation of existing graphite preparation methods are solved, and efficient and low-cost graphite material preparation is achieved , suitable for a variety of application fields.

WO2024240228A1PCT designated stage expired Publication Date: 2024-11-28WUHAN UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/094983
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-23
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The existing graphite preparation methods have high temperature and high energy consumption, large product size, and are not suitable for catalytic and energy storage applications. It is difficult to reuse the catalyst and make sheet graphite difficult to prepare.

Method used

Under the protection of inert gas, molten salts are used as a medium to crystallize and grow graphite of carbon materials through contact or electronic paths between carbon materials and activated materials, and control temperature and time to regulate the crystallinity and size of the product.

Benefits of technology

It has achieved low energy consumption, low cost and high product crystallinity preparation, suitable for catalysis, energy storage and other fields, and supports the continuous preparation and structural diversity of graphite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024094983_28112024_PF_FP_ABST
    Figure CN2024094983_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of graphite preparation. Disclosed are a carbon material graphite crystallization and growth method and an application thereof. Under the protection of an inert gas, in the copresence of a carbon material, an activation material M1-Y, and a molten salt M-X, a non-graphite carbon material is converted into graphite-structured carbon, or the size of the graphite-structured carbon is increased. The method involves a simple process, requires a simple device, has a low reaction temperature, short reaction time, low costs and high yield, and facilitates mass operation. Products may be nanometer- and micrometer-scale graphite sheets, nanometer- and micrometer-scale fibers and the like, and have wide prospects for application in the fields such as structural materials, energy storage, catalysis, adsorption and separation.
Need to check novelty before this filing date? Find Prior Art

Description

A method for crystallizing and growing graphite of carbon material and its application Technical Field

[0001] The present invention relates to the technical field of graphite preparation, and in particular to a graphite crystallization and growth method of a carbon material and applications thereof. Background Art

[0002] Graphite materials are widely used due to their excellent physical and chemical properties. However, due to the resource limitations and insufficient performance of natural graphite, people are increasingly demanding artificial graphite. Currently, artificial graphite is prepared by converting amorphous carbon into graphite at high temperatures, but this method requires temperatures as high as 3000°C, has a long cycle, and consumes a lot of energy. Moreover, this method is only applicable to soft carbon raw materials, but most amorphous carbon, including renewable amorphous carbon, is a hard carbon material and is difficult to convert into graphite even if the heat treatment temperature is further increased. In addition, the graphite carbon material prepared by this method is relatively large in size, which limits its application in fields such as catalysis and energy storage. In addition to high-temperature and high-pressure methods, amorphous carbon can also be catalytically converted into graphite at lower temperatures (about 1100°C) in the presence of a catalyst, such as patents US2005 / 0008562A1, CN102745677A, CN102807212A, etc. The catalytic conversion temperature is significantly lower than that of traditional methods, but in the above method, graphite often grows around the catalyst, and the product is spiral graphite rather than flake graphite, which is more widely used. Moreover, the catalyst is confined in the spiral graphite, which makes it difficult to reuse the catalyst and requires cumbersome subsequent processing steps to remove it. Patent CN103510103A reports on the electrochemical conversion of amorphous carbon into flake graphite. It has attracted widespread attention because it does not require the use of a catalyst and can operate at a lower temperature. However, this method consumes a large amount of electrolysis energy, and the electrolysis potential and electrolysis time need to be strictly controlled to take into account both graphite crystallinity and yield.

[0003] Summary of the Invention

[0004] In view of the above-mentioned defects of the prior art, in the first aspect of the present invention, a method for graphite crystallization and growth of carbon materials is provided, which has a simple process, low cost and high product crystallinity, comprising the following steps: under the protection of an inert gas, using molten salt as a medium, contacting the carbon material with an activation material or forming an electron path, and completing the graphite crystallization and growth of the carbon material after treatment.

[0005] Preferably, the elemental composition of the salt is denoted by MX, where M represents at least one of Li, Na, K, Rb, Cs, Be, Mg, Ca, Sr, and Ba, and X represents at least one of the halogens.

[0006] More preferably, the salt includes a halogen salt whose elemental composition is MX, or a mixture formed by the halogen salt.

[0007] Preferably, the elemental composition of the activation material is represented by M1-Y, where M1 represents at least one of Li, Na, K, Rb, Cs, Be, Mg, Ca, Sr, and Ba, and Y represents at least one of Zn, Cd, B, Al, Ga, In, Tl, C, Si, Ge, Sn, Pb, N, P, As, Sb, and Bi.

[0008] Further preferably, the activation material includes a compound with an elemental composition of M1-Y, a mixture formed by the compound, and a metal alloy with an elemental composition of M1-Y.

[0009] Preferably, the carbon material includes non-graphite structural carbon material, graphite structural carbon material, non-graphite structural carbon composite material, and graphite structural carbon composite material; the non-graphite structural carbon composite material and graphite structural carbon composite material are respectively composited by non-graphite structural carbon material, graphite structural carbon material and the substance to be dispersed or the precursor of the substance to be dispersed.

[0010] The substance to be dispersed or its precursor can induce graphite growth, thereby obtaining one-dimensional graphite structured carbon materials, such as graphite fibers, or porous materials constructed from graphite structured carbon, providing richer structural options based on the preparation of flake graphite.

[0011] Further preferably, the non-graphite structural carbon material includes at least one of biomass carbon, organic carbon, amorphous carbon, fullerene, and diamond.

[0012] The raw materials of the non-graphite structure carbon material of the present invention are widely available, among which amorphous carbon can be activated carbon, carbon black, charcoal, coke, bone char, carbon fiber, carbon tubes, and amorphous carbon materials obtained by carbonization of organic matter and other preparation methods. The organic matter used for carbonization includes various agricultural and forestry crops, sediments such as petroleum and coal, artificially synthesized organic matter, and various organic solid and liquid wastes. In the present invention, the carbon material is not limited to pure substances composed of carbon elements. Carbon materials containing heteroatoms can also be converted into graphite structure carbon materials containing heteroatoms using the method provided in the first aspect of the present invention.

[0013] Further preferably, when the carbon material adopts a non-graphite structure carbon composite material or a graphite structure carbon composite material, the substance to be dispersed is at least one of a metal element, a metal alloy, and a metal carbide; and the precursor of the substance to be dispersed is at least one of a metal sulfide, a metal oxide, and a metal salt.

[0014] Furthermore, when the carbon material adopts a non-graphite structure carbon composite material or a graphite structure carbon composite material, the impurities formed by the substance to be dispersed or the precursor of the substance to be dispersed are removed after the crystallization and growth of graphite to obtain a graphite-based material; or the impurities formed by the substance to be dispersed or the precursor of the substance to be dispersed are retained after the crystallization and growth of graphite to obtain a graphite-based composite material.

[0015] Furthermore, the metal element is at least one of Mn, Fe, Co, Ni, Cu, and Zn.

[0016] Preferably, the contacting manner of the carbon material with the activation material includes at least one of contacting the carbon material with the activation material dispersed in a molten salt and immersing the carbon material and the activation material in a molten salt after mixing; the dispersion form of the activation material in the molten salt includes dissolution.

[0017] Preferably, the contacting method of the carbon material and the activation material comprises immersing the carbon material in a molten salt in which the activation material is dissolved.

[0018] The carbon material and the activation material form an electron path in the following ways: connecting the carbon material and the activation material through a conductor and immersing them in molten salt, or directly contacting the carbon material immersed in the molten salt with the undissolved activation material or connecting them through a conductor.

[0019] Preferably, the treatment temperature is 400-1400° C., and the treatment time is 0.5-50 h.

[0020] The product with a graphite structure obtained by the present invention has a size between 10 nm and 100 μm. The graphite crystallinity, graphite sheet thickness and lateral size of the product can be regulated by controlling the treatment temperature and time, so that non-graphite structured carbon materials can be converted into graphite structured carbon, or the size of graphite structured carbon can be grown. The dimensional size is adjustable and has broad application prospects in the fields of structural materials, energy storage, catalysis, adsorption, separation and the like.

[0021] In a second aspect of the present invention, there is provided an application of a graphite crystallization and growth method of a carbon material in the continuous preparation of a graphite material.

[0022] The specific application method includes the following steps:

[0023] After the graphite crystallization and growth of the carbon material are completed, a product with a graphite structure is recovered from the molten salt, and then a new round of carbon material is prepared and graphite crystallization and growth are carried out using the same method.

[0024] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0025] The method adopted by the present invention has low energy consumption cost, simple and flexible operation, and is suitable for preparing graphite materials with high crystallinity.

[0026] The present invention provides an application method for continuously preparing graphite materials, which has high yield and good application prospect of large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] FIG1 is an X-ray diffraction (XRD) test pattern of amorphous carbon XC-72 and the product obtained in Example 3;

[0028] FIG2 is a scanning electron microscope (SEM) test pattern of amorphous carbon XC-72;

[0029] FIG3 is a scanning electron microscope (SEM) test spectrum of the product obtained in Example 3;

[0030] FIG4 is a scanning electron microscope (SEM) test spectrum of the product obtained in Example 4;

[0031] FIG5 is a scanning electron microscope (SEM) test spectrum of the product obtained in Example 9. DETAILED DESCRIPTION

[0032] The present invention is further illustrated by way of examples below, but the present invention is not limited to the scope of the examples. Experimental methods in the following examples where specific conditions are not specified were performed according to conventional methods and conditions, or selected according to the product specifications.

[0033] The carbon material used in the examples is amorphous carbon XC-72 (Carbot Corp.); the molar concentration of hydrochloric acid is 1 mol / L.

[0034] Example 1

[0035] Graphite crystallization and growth methods of carbon materials:

[0036] At 950°C and under argon protection, 0.5g of calcium boride and 1.5g of amorphous carbon XC-72 were mixed evenly and pressed into tablets, which were then wrapped with a porous metal mesh and then immersed in molten calcium chloride and kept at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere. The finished product was obtained after washing and drying. The finished product was characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product were similar to the product spectrum in Figure 1, confirming that a product with a graphite structure was obtained.

[0037] Example 2

[0038] Graphite crystallization and growth methods of carbon materials:

[0039] At 950°C and under argon protection, 0.5g of calcium carbide and 1.5g of amorphous carbon XC-72 were mixed evenly and pressed into tablets, which were then wrapped with a porous metal mesh and then immersed in molten calcium chloride and kept at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere. The finished product was obtained after washing and drying. The finished product was characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product were similar to the product spectrum in Figure 1, confirming that a product with a graphite structure was obtained.

[0040] Example 3

[0041] Graphite crystallization and growth methods of carbon materials:

[0042] At 950 ° C and under argon protection, 1.5g of calcium carbide was uniformly dispersed in 10.0g of molten calcium chloride, and then 1.0g of amorphous carbon XC-72 was pressed into a pellet and wrapped with a porous metal mesh and immersed in the molten calcium chloride containing calcium carbide. The pellet was kept at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere. After washing and drying, the finished product was obtained. The finished product and the amorphous carbon XC were analyzed by X-ray diffraction. The XC-72 raw material was characterized. The XRD patterns of the finished product and amorphous carbon XC-72 are shown in Figure 1. The characteristic peaks of the finished product in Figure 1 are consistent with those of graphite. The XRD pattern of the amorphous carbon only shows a broad, low peak near 2θ of 25° and 44°, while the XRD pattern of highly crystalline graphitized carbon exhibits a very sharp peak near 2θ of 26.4°. Figure 1 confirms that the amorphous carbon XC-72 undergoes transformation from an amorphous structure to highly crystalline graphite after treatment. Scanning electron microscopy (SEM) observations of the finished product and the amorphous carbon XC-72 raw material, as shown in Figures 2 and 3, show that the amorphous carbon XC-72 particles with a particle size of approximately 50 nm transform into flake graphite after treatment.

[0043] Example 4

[0044] Graphite crystallization and growth methods of carbon materials:

[0045] At 1100°C under argon protection, 1.0g of barium carbide was uniformly dispersed in 10.0g of molten barium chloride. 1.0g of amorphous carbon XC-72 was then pressed into a pellet, wrapped with a porous metal mesh, and immersed in the molten barium chloride containing the barium carbide. The pellet was then incubated at this temperature for 2 hours to complete graphite crystallization and growth of the carbon material. The product was removed and cooled to room temperature in an argon atmosphere, washed, and dried to obtain a finished product. The finished product was characterized by X-ray diffraction. The resulting XRD pattern showed characteristic peaks similar to those of the product in Figure 1, confirming that a product with a graphite structure was obtained. The microscopic morphology of the finished product was observed by scanning electron microscopy (SEM). As shown in Figure 4, micron-sized graphite blocks were obtained in this embodiment.

[0046] Example 5

[0047] Graphite crystallization and growth methods of carbon materials:

[0048] Under the set temperature and argon protection of the experimental group of this embodiment, 0.5 g of lithium carbide was dispersed in 10.0 g of a molten salt formed by 35% by mass of calcium chloride and 65% by mass of lithium chloride, and then 1.0 g of amorphous carbon XC-72 was pressed into a tablet and wrapped with a porous metal mesh and immersed in the molten salt containing lithium carbide. The heat treatment was carried out at the set temperature for a predetermined time to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere. The finished product was washed and dried to obtain the finished product, and the finished product was characterized by X-ray diffraction. In the obtained XRD pattern, the characteristic peaks of the finished product were similar to the product spectrum in Figure 1, confirming that a product with a graphite structure was obtained.

[0049] Table 1: Treatment temperature and corresponding treatment time of Example 5

[0050] The microstructure of the finished product was observed by scanning electron microscopy (SEM). The SEM images showed that as the treatment temperature increased, the product grew from few-layer graphene sheets to nanographene sheets, confirming that the thickness of the graphite layer increased with the increase of treatment temperature.

[0051] Example 6

[0052] Graphite crystallization and growth methods of carbon materials:

[0053] At 850°C and under argon protection, 1.5g of lithium nitride was uniformly dispersed in 10.0g of a molten salt formed by 35% by mass of calcium chloride and 65% by mass of lithium chloride. Then, 1.0g of amorphous carbon XC-72 was pressed into a tablet and wrapped with a porous metal mesh and immersed in molten calcium chloride containing lithium nitride. The tablet was kept at this temperature for 2h to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere. The finished product was obtained by washing and drying. The finished product was characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product were similar to the product spectrum in Figure 1, confirming that a product with a graphite structure was obtained.

[0054] Example 7

[0055] Graphite crystallization and growth methods of carbon materials:

[0056] At 850°C and under argon protection, 1.0g of calcium carbide was uniformly dispersed in 10.0g of a molten salt formed by 35% by mass of calcium chloride and 65% by mass of lithium chloride. Then, 1.0g of sycamore charcoal, phenolic resin charcoal, and petroleum coke were respectively pressed into tablets and wrapped with a porous metal mesh and immersed in the molten salt containing calcium carbide. The tablets were heat-treated at this temperature for 2h to complete the graphite crystallization and growth of the corresponding carbon materials. The products were taken out and cooled to room temperature in an argon atmosphere. The finished products were washed and dried to obtain the finished products. The finished products were characterized by X-ray diffraction. The characteristic peaks of the different finished products in the obtained XRD patterns were similar to the product patterns in Figure 1, confirming that products with graphite structures were obtained in all of the embodiments.

[0057] Example 8

[0058] Graphite crystallization and growth methods of carbon materials:

[0059] At 850°C and under argon protection, 1.0g of calcium carbide was uniformly dispersed in 10.0g of molten salt of a set ratio. Then, 1.0g of amorphous carbon XC-72 was pressed into a tablet, wrapped with a porous metal mesh, and immersed in various molten salts containing calcium carbide. The tablets were kept at this temperature for 2h to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere. The finished product was obtained after washing and drying.

[0060] Table 2: Types of molten salts used in Example 8 and their mass percentages of corresponding substances

[0061] The finished products were characterized by X-ray diffraction, and the characteristic peaks of different finished products in the obtained XRD patterns were similar to the product patterns in FIG1 , confirming that products with graphite structures were obtained in this embodiment.

[0062] Example 9

[0063] Graphite crystallization and growth methods of carbon materials:

[0064] At 850°C under argon, 1.0g of calcium carbide was uniformly dispersed in 10.0g of molten calcium chloride. 1.0g of amorphous carbon XC-72 was then mixed with ferrous sulfide, iron, and nickel oxide to produce a mixture in which the ferrous sulfide accounted for 5% of the mixture, the iron accounted for 7%, and the nickel oxide accounted for 3%. The mixtures were pressed into tablets, wrapped with porous metal mesh, and then immersed in molten calcium chloride containing calcium carbide. The tablets were then incubated at this temperature for 2 hours to complete the crystallization and growth of graphite in the carbon material. The product was removed and cooled to room temperature under argon, washed with water and hydrochloric acid, and dried to obtain the final product. The final product was characterized by X-ray diffraction. The resulting XRD pattern showed characteristic peaks similar to those in Figure 1, confirming that the product had a graphite structure. Scanning electron microscopy (SEM) was used to observe the micromorphology of the final product with 5% ferrous sulfide added. Figure 5 shows that the graphite product was fibrous. In this embodiment, the product is not washed with hydrochloric acid to obtain a fibrous graphite-based composite material containing iron or nickel.

[0065] Example 10

[0066] Graphite crystallization and growth methods of carbon materials:

[0067] At 850°C under argon, 1.0g of calcium carbide was uniformly dispersed in 10.0g of molten calcium chloride. 1.0g of amorphous carbon XC-72 was then mixed with nano-TiS to produce a mixture in which the TiS accounted for 4% of the total mass of the mixture. After tableting, the mixture was wrapped with a porous metal mesh and immersed in molten calcium chloride containing the calcium carbide. The mixture was then incubated at this temperature for 2.0 hours to complete the graphite crystallization and growth of the amorphous carbon and the conversion of the TiS to TiC. The product was then removed and cooled to room temperature under an argon atmosphere. It was then washed with water and dilute hydrochloric acid and dried to obtain the finished product. XRD analysis of the dried product revealed that it was a composite material of graphite and TiC.

[0068] Example 11

[0069] At 850°C under argon, 1.0g of calcium carbide was uniformly dispersed in 10.0g of molten calcium chloride. 1.0g of amorphous carbon XC-72 was then mixed with Co-Cu alloy nanopowder to obtain a mixture, wherein the Co-Cu alloy accounted for 8% of the total mass of the mixture. After tableting, the mixture was wrapped with a porous metal mesh and immersed in molten calcium chloride containing the calcium carbide. The mixture was kept at this temperature for 2.0h to complete the crystallization and growth of graphite from the amorphous carbon. The product was removed and cooled to room temperature under argon atmosphere, washed with water, and dried to obtain the finished product. XRD analysis of the dried product showed that the finished product was a composite material of graphite and Co-Cu alloy.

[0070] Example 12

[0071] Graphite crystallization and growth methods of carbon materials:

[0072] Ammonium chloroplatinate and glucose were mixed in a platinum-to-carbon atomic ratio of 1:100 and water was added to form a solution. The solution was then dried at 70°C to obtain a colloid. The colloid was then carbonized at 500°C to obtain an amorphous carbon-platinum complex. Under argon protection at 850°C, lithium carbide was uniformly dispersed in a molten salt composed of 35% calcium chloride and 65% lithium chloride by mass, with lithium carbide accounting for 10% of the total mass of the lithium carbide and molten salt. The complex was then pressed into a tablet, wrapped with a porous metal mesh, immersed in the molten salt, and kept at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was removed and cooled to room temperature under an argon atmosphere. It was then washed with water and hydrochloric acid and dried to obtain the finished product. The finished product was characterized by X-ray diffraction. The resulting XRD pattern showed characteristic peaks similar to the product pattern shown in Figure 1, confirming that a product with a graphite structure was obtained. The microscopic morphology of the added product was observed by scanning electron microscopy (SEM), and the SEM image results showed that the product was a porous composite material constructed of platinum and graphite sheets.

[0073] Example 13

[0074] Graphite crystallization and growth methods of carbon materials:

[0075] At 900°C under argon protection, 1.0g of amorphous carbon XC-72 and 1.0g of calcium chloride were mixed with 0.5g of calcium-tin alloy powder, calcium-zinc alloy powder, lithium-tin alloy powder, barium-zinc alloy powder, and sodium-tin alloy powder, respectively, and then pressed into tablets. The mixture was then kept at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was removed and cooled to room temperature in an argon atmosphere, washed, and dried to obtain the finished product. The finished product was characterized by X-ray diffraction. The characteristic peaks of the finished product in the obtained XRD pattern were similar to the product pattern in Figure 1, confirming that products with graphite structures were obtained.

[0076] Example 14

[0077] Graphite crystallization and growth methods of carbon materials:

[0078] At 900°C and under argon protection, 2.0g of calcium boride and 1.5g of amorphous carbon XC-72 were pressed into tablets, then wrapped with porous metal mesh to obtain calcium boride and amorphous carbon test pieces. The two test pieces were then immersed in molten calcium chloride; the two test pieces were contacted by direct contact and contact through a metal wire, respectively. Then, the temperature was kept at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was removed and cooled to room temperature in an argon atmosphere. After washing and drying, the finished product was obtained. The finished product was characterized by X-ray diffraction. The characteristic peaks of the finished product in the obtained XRD pattern were similar to the product spectrum in Figure 1, confirming that products with graphite structures were obtained under different contact methods.

[0079] By simply replacing calcium boride with an equal amount of calcium carbide and using the same method to carry out graphite crystallization and growth of carbon materials, products with graphite structure can still be obtained under different contact modes.

[0080] Example 15

[0081] Graphite crystallization and growth methods of carbon materials:

[0082] At 1200°C under argon, 1.0g of barium carbide was uniformly dispersed in 10.0g of molten barium chloride. 2.0g of nanoscale graphite was then wrapped in a porous metal mesh and immersed in the molten barium chloride containing the barium carbide. The mixture was then kept at this temperature for 10 hours to complete the crystallization and growth of the carbon material. The product was then removed and cooled to room temperature under an argon atmosphere. After washing and drying, the final product was obtained. Scanning electron microscopy (SEM) was used to observe the micromorphology of the raw nanoscale graphite and the finished product. The SEM images showed that the nanoscale graphite had grown to the micrometer level.

[0083] Example 16

[0084] Application of graphite crystallization and growth methods of carbon materials in the continuous preparation of graphite materials:

[0085] At 850 ° C and under argon protection, 5.0g of calcium carbide was evenly dispersed in 50.0g of molten calcium chloride, 2.0g of amorphous carbon XC-72 was pressed and wrapped with a porous metal mesh, and then placed in the molten calcium chloride containing calcium carbide. It was kept at this temperature for 2h to complete the graphite crystallization and growth of the carbon material. The product was taken out and then another 2.0g amorphous carbon XC-72 pressed tablet was placed and kept at this temperature for 2h. This cycle was repeated for a total of 10 batches. The products were all cooled to room temperature in an argon atmosphere, washed and dried to obtain the finished product. All 20.0g of amorphous carbon XC-72 can be converted into graphite products. The finished product was characterized by X-ray diffraction. The characteristic peaks of the finished product in the obtained XRD pattern were similar to the product pattern in Figure 1, confirming that a product with a graphite structure was obtained. The test showed that there was still a large amount of calcium carbide remaining in the molten salt, indicating that the amorphous carbon can continue to be converted into graphite, realizing the continuous preparation of graphite materials.

[0086] Example 17

[0087] Graphite crystallization and growth methods of carbon materials:

[0088] At 950°C under argon, 1.0g of diamond powder and 1.0g of calcium boride were mixed uniformly, pressed into tablets, and wrapped with porous metal mesh. The tablets were then immersed in a molten salt solution consisting of 15% calcium fluoride and 85% potassium fluoride by weight. The mixture was held at this temperature for 5 hours to complete the crystallization and growth of graphite. The product was then removed and cooled to room temperature under argon, washed, and dried to obtain the final product. The final product was characterized by X-ray diffraction. The resulting XRD pattern showed characteristic peaks similar to those of the product shown in Figure 1, confirming that the diamond powder had been converted to a product with a graphite structure.

[0089] Example 18

[0090] Graphite crystallization and growth methods of carbon materials:

[0091] Under argon at 820°C, 1.0g of activated carbon and nano-cobalt oxide were mixed uniformly, with the atomic ratio of carbon to cobalt in the mixture being 20:1. This mixture was then pressed into a pellet and wrapped with a porous metal mesh to produce a carbon-cobalt test piece. Separately, 2.0g of calcium boride was pressed into a pellet and wrapped with a porous metal mesh to produce a calcium boride test piece. The two test pieces were secured to each other with a molybdenum wire and immersed in molten calcium chloride. The pellets were held at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was then removed and cooled to room temperature under argon, washed with water and hydrochloric acid, and dried to obtain the final product. The final product was characterized by X-ray diffraction. The resulting XRD pattern showed characteristic peaks similar to those in Figure 1, confirming that the product had a graphite structure. Transmission electron microscopy (TEM) was used to observe the micromorphology of the product, which showed nanotubes.

[0092] The above describes in detail the preferred embodiments of the present invention. It should be understood that those skilled in the art can make numerous modifications and variations based on the concepts of the present invention without inventive effort. Therefore, any technical solutions that can be derived by those skilled in the art through logical analysis, reasoning, or limited experimentation based on the concepts of the present invention and the prior art should be within the scope of protection defined by the claims.

Claims

1. A method for crystallizing and growing graphite of a carbon material, characterized in that: The method comprises the following steps: under the protection of an inert gas, using molten salt as a medium, contacting the carbon material with the activated material or forming an electron path, and completing the graphite crystallization and growth of the carbon material after treatment.

2. The method according to claim 1, characterized in that: The elemental composition of the salt is MX, where M represents at least one of Li, Na, K, Rb, Cs, Be, Mg, Ca, Sr, and Ba, and X represents at least one of the halogens; the salt includes a halogen salt having an elemental composition of MX and a mixture formed by the halogen salt.

3. The method according to claim 1, characterized in that: The elemental composition of the activation material is denoted by M1-Y, where M1 represents at least one of Li, Na, K, Rb, Cs, Be, Mg, Ca, Sr, and Ba, and Y represents at least one of Zn, Cd, B, Al, Ga, In, Tl, C, Si, Ge, Sn, Pb, N, P, As, Sb, and Bi; the activation material includes a compound with an elemental composition of M1-Y, a mixture formed by the compound, and a metal alloy with an elemental composition of M1-Y.

4. The method according to claim 1, characterized in that: The carbon material includes non-graphite structural carbon material, graphite structural carbon material, non-graphite structural carbon composite material, and graphite structural carbon composite material; the non-graphite structural carbon composite material and graphite structural carbon composite material are respectively composited by non-graphite structural carbon material, graphite structural carbon material and a substance to be dispersed or a precursor of a substance to be dispersed.

5. The method according to claim 4, characterized in that: The non-graphite structure carbon material includes at least one of biomass carbon, organic carbon, amorphous carbon, fullerene, and diamond; when the carbon material adopts a non-graphite structure carbon composite material or a graphite structure carbon composite material, the substance to be dispersed is at least one of a metal element, a metal alloy, and a metal carbide; the precursor of the substance to be dispersed is at least one of a metal sulfide, a metal oxide, and a metal salt.

6. The method according to claim 5, characterized in that: When the carbon material adopts a non-graphite structure carbon composite material or a graphite structure carbon composite material, impurities formed by the substance to be dispersed or the precursor of the substance to be dispersed are removed after graphite crystallization and growth to obtain a graphite-based material; or impurities formed by the substance to be dispersed or the precursor of the substance to be dispersed are retained after graphite crystallization and growth to obtain a graphite-based composite material.

7. The method according to claim 5, characterized in that: The metal element is at least one of Mn, Fe, Co, Ni, Cu and Zn.

8. The method according to claim 1, characterized in that: The method of contacting the carbon material with the activation material comprises at least one of contacting the carbon material with the activation material dispersed in a molten salt and immersing the carbon material and the activation material in a molten salt after mixing; the method of forming an electron path between the carbon material and the activation material comprises connecting the carbon material and the activation material through a conductor and immersing them in a molten salt; the treatment temperature is 400 to 1400°C and the treatment time is 0.5 to 50 hours.

9. The method according to claim 8, characterized in that: The contacting method of the carbon material and the activation material comprises immersing the carbon material in a molten salt in which the activation material is dissolved.

10. The method according to claim 8, characterized in that: The method of forming an electron path between the carbon material and the activation material includes directly contacting the carbon material immersed in the molten salt with the undissolved activation material or connecting them through a conductor.

11. Use of the method according to any one of claims 1 to 10 in the continuous preparation of graphite materials.

12. The use according to claim 11, characterized in that: The specific method comprises the following steps: after the graphite crystallization and growth of the carbon material are completed, a product having a graphite structure is recovered from the molten salt, and then a new round of carbon material is prepared, and graphite crystallization and growth are performed using the same method.

Citation Information

Patent Citations

  • Method for graphitizing amorphous carbon material at low temperature

    CN101723356A

  • Method for preparing porous carbon for super capacitor by waste plastic carbonization

    CN105366658A

  • Method for converting amorphous carbon to graphitized carbon nanofibers

    CN112442761A

  • Method for synthesizing graphite from calcium carbide and amorphous carbon at low temperature

    CN115557492A

  • Low-temperature graphitization method for conversion of bamboo waste-based amorphous carbon

    CN118028831A