Voltage-controlled electrochemical wet etching preparation of porous monocrystalline silicon carbide thin films and multilayered wafer production

The voltage-controlled electrochemical wet etching method addresses the high cost of silicon carbide substrates by producing efficient, morphologically tailored porous films, enhancing material reuse and reducing energy consumption in silicon carbide semiconductor production.

WO2024240961A1PCT designated stage expired Publication Date: 2024-11-28UMICORE(BE)

Patent Information

Application Number
PCT/EP2024/064539
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-05-27
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The high cost of monocrystalline silicon carbide substrates for compound semiconductors is a barrier to their widespread adoption due to expensive crystal growth processes and substrate polishing, which are energy and material intensive.

Method used

A voltage-controlled electrochemical wet etching method is used to create morphologically tuned, porous monocrystalline silicon carbide thin films from monocrystalline substrates, allowing for efficient detachment and reuse of substrates, reducing material and energy consumption.

Benefits of technology

This method enables the production of high-quality, porous silicon carbide thin films with tailored morphology, facilitating further processing and reducing the need for costly substrate materials, thereby lowering production costs and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024064539_28112024_PF_FP_ABST
    Figure EP2024064539_28112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides electrochemical wet etching methods and processes useful for manufacturing compound semiconductors, whereby a monocrystalline silicon carbide substrate having a porous surface layer is electrochemically wet etched and whereby the applied voltage is varied during said electrochemical wet etching process step.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] VOLTAGE-CONTROLLED ELECTROCHEMICAL WET ETCHING PREPARATION OF POROUS MONOCRYSTALLINE SILICON CARBIDE THIN FILMS AND MULTILAYERED WAFER PRODUCTION

[0002] TECHNICAL FIELD

[0003] The present invention relates to the field of compound semiconductors, specifically to novel methods for processing compound semiconductors such as silicon carbide.

[0004] INTRODUCTION

[0005] Compound semiconductors are materials made of two or more elements which have been chemically combined to create a new material with unique electronic properties. These materials are used in a variety of electronic devices such as transistors, solar cells, and LEDs. Often, they have a bandgap that is wider than that of singleelement semiconductors, which allows them to operate at higher temperatures and higher switching efficiencies in power electronic devices. Some examples of compound semiconductor materials include gallium arsenide, indium phosphide, and cadmium selenide.

[0006] Given their wide electronic bandgap silicon carbide (SiC) semiconductors operate at higher temperatures and higher voltages than traditional silicon-based semiconductors. In general, they also have a high breakdown electric field, which makes them suitable for high-power and high-frequency applications. Silicon carbide semiconductors are industrially important because they have unique electronic properties that make them suitable for a wide range of applications. For example, they are used in power electronics devices such as high-voltage, high-frequency transistors, diodes, and thyristors. These devices are used in a wide range of applications such as electric vehicles, renewable energy systems, and industrial motor drives. Silicon carbide semiconductors also have potential applications in high-temperature and high-radiation environments, such as in aerospace and nuclear power systems.

[0007] In spite of progress over the last decades in both material quality and device manufacturing, widespread adoption of silicon carbide semiconductors is obstructed by the high cost of monocrystalline silicon carbide substrates. The main factors con- tributing to that high cost are the crystal growth process, the subsequent ingot or boule slicing and the polishing of the substrates.

[0008] To this aim, the current inventors have previously developed new methods for preparing silicon carbide semiconductor multilayers. Leitgeb, M. et al. J. Electrochem. Soc. 2017, 164 (12), E337, described novel methods for preparing porous 4H-SiC layers from monocrystalline samples applying photo-electrochemical etching in hydrofluoric acid. It was found that the resulting degree of porosity, the homogeneity in porosity as well as the pore morphology mainly depend on the applied voltage. Importantly, the approach allowed to detach the porous 4H-SiC layers from the 4H- SiC substrate. WO 2022 / 184630 Al teaches structures prepared by electrochemical porosification followed by fusion bonding of the porous film on a polycrystalline silicon carbide layer. WO 2022 / 243501 Al describes methods for releasing a porous silicon carbide thin film from a substrate via a stressor layer.

[0009] SUMMARY

[0010] The current invention provides in a solution for at least one of the above-mentioned problems by providing electrochemical wet etching methods and processes useful for manufacturing compound semiconductors, whereby a monocrystalline silicon carbide substrate having an exposed surface layer is electrochemically wet etched and whereby the applied voltage is varied during said electrochemical wet etching process step, as described in claim 1.

[0011] Preferably, the compound semiconductors are monocrystalline silicon carbide substrates, specifically 4H-silicon carbide (4H-SiC).

[0012] The method according to the first aspect of the present invention allows for the formation of a monocrystalline silicon carbide substrate with a morphologically tuned, porous thin film at an electrochemically wet etched surface. The inventors have now found that the parameters defining the electrochemical wet etching method, specifically the applied voltage profile, allow to tailor the structure of the obtained porous, monocrystalline silicon carbide thin film, to provide a structure which is suitably configured for further processing. As such, the inventive methods and processes as described herein allow for material and energy efficient use of compound semiconductor materials which otherwise require material and energy intensive processing methods.

[0013] DESCRIPTION OF THE FIGURES

[0014] By means of further guidance, figures are included to better appreciate the teaching of the present invention. Said figures are intended to assist the description of the invention and are nowhere intended as a limitation of the presently disclosed invention. The figures and symbols contained therein have the meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.

[0015] - Figure 1 shows the applied voltage profile during the PECE (photoelectrochemical etching) method according to Example 1, whereby time (minutes) is shown on the X-axis, and voltage (V) is shown on the Y-axis.

[0016] - Figure 2 shows the porosity of a porous silicon carbide thin film obtained from the PECE method of Example 1, as a function of the etching depth, expressed in pm, whereby porosity is expressed as the fraction void volume relative to total volume.

[0017] - Figure 3 shows a SEM analysis of a cross section of the porous silicon carbide thin film obtained from the PECE method of Example 1.

[0018] - Figure 4 shows the applied voltage profile during the PECE method according to Example 2, whereby time (minutes) is shown on the X-axis, and voltage (V) is shown on the Y-axis.

[0019] DETAILED DESCRIPTION OF THE INVENTION

[0020] Unless otherwise defined, all terms used in disclosing the invention, including technical and scientific terms, have the meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. By means of further guidance, term definitions are included to better appreciate the teaching of the present invention.

[0021] As used herein, the following terms have the following meanings: "A", "an", and "the" as used herein refers to both singular and plural referents unless the context clearly dictates otherwise. By way of example, "a compartment" refers to one or more than one compartment.

[0022] "About" as used herein referring to a measurable value such as a parameter, an amount, a temporal duration, and the like, is meant to encompass variations of + / - 20% or less, preferably + / -10% or less, more preferably + / -5% or less, even more preferably + / -1% or less, and still more preferably + / -0.1% or less of and from the specified value, in so far such variations are appropriate to perform in the disclosed invention. However, it is to be understood that the value to which the modifier "about" refers is itself also specifically disclosed.

[0023] "Comprise," "comprising," and "comprises" and "comprised of" as used herein are synonymous with "include", "including", "includes" or "contain", "containing", "contains" and are inclusive or open-ended terms that specifies the presence of what follows e.g. component and do not exclude or preclude the presence of additional, non-recited components, features, element, members, steps, known in the art or disclosed therein.

[0024] The recitation of numerical ranges by endpoints includes all numbers and fractions subsumed within that range, as well as the recited endpoints. All percentages are to be understood as percentage by weight, abbreviated as "wt.%" or as volume percent, abbreviated as "vol.%", unless otherwise defined or unless a different meaning is obvious to the person skilled in the art from its use and in the context wherein it is used.

[0025] A semiconductor is a solid-state material that exhibits electrical conductivity intermediate between that of an insulator and that of a conductor. Silicon is a commonly used semiconductor material. The semiconductor layer can take various forms, such as a single bulk wafer or multiple sublayers. In particular, a semiconductor layer and more preferably a silicon carbide semiconductor layer may include multiple non-continuous porous portions. The multiple non-continuous porous portions may have different densities and may be horizontally distributed or vertically layered. Examples of semiconductor materials include, without limitation, silicon carbide, gallium-arsenide and indium-phosphide. In the context of the present invention, a compound semiconductor is a material composed of at least two different chemical species, such as Group III and V elements or Group II and VI elements. These materials typically belong to periodic table groups 13-15, for example elements from the Boron group (e.g. boron, aluminium, gallium, indium) and group 15 (e.g. nitrogen, phosphorus, arsenic, antimony, bismuth). The range of possible chemical compositions is quite broad, as these elements can form binary compounds (e.g. gallium arsenide, GaAs), ternary compounds (e.g. indium gallium arsenide, InGaAs) and quaternary compounds (e.g. aluminum gallium indium phosphide, AlInGaP). GaAs, GaN, InP and InGaAlP are commonly used in high-frequency devices and optoelectronic devices, while SiC and GaN compounds are often employed in power semiconductors. Typical compound semiconductors are:

[0026] Group II-VI : ZnSe

[0027] Group III-V: GaAs, GaN, InP, InGaAlP, InGaN

[0028] Group IV-IV: SiC, SiGe

[0029] In the context of the present invention, the term "substrate" or "semiconductor substrate" or "compound semiconductor substrate" refers to a material composed of a semiconductor, specifically a compound semiconductor, specifically silicon carbide, on which layers of material may be deposited or applied. Ideally, the substrate is a single-crystalline substrate. This semiconductor substrate may also be referred to as a slice, a wafer, a puck or substrate and is known within the field. These semiconductor substrates are commonly used as a base for building microelectronic devices. These substrates may undergo various processes such as doping, ion implantation, etching, thin-film deposition, or lithographic patterning. Examples of substrates include, but are not limited to: bulk germanium wafers, bulk silicon wafers (comprising a homogeneous thickness of single-crystal silicon or germanium); composite semiconductor wafers (comprising a homogeneous thickness of mono- or polycrystalline compound semiconductor material); composite wafers such as silicon-on-insulator wafers (comprising a layer of silicon disposed on a layer of silicon dioxide on a bulk silicon handle wafer); porous germanium, germanium over oxide and silicon, germanium over silicon, patterned germanium, germanium tin over germanium, and the like; or any other material that serves as a base layer for device formation. Preferably, the semiconductor substrate comprises silicon car- bide. More preferably, the semiconductor substrate consists essentially of silicon carbide. A substrate may have a single bulk wafer or multiple sublayers, specifically, a substrate may include multiple non-continuous porous portions with varying densities and can be horizontally distributed or vertically layered. In the context of this invention, the term "substrate" generally refers to a material with a thickness of at least 1 pm. Semiconductor substrates generally have a substantially cylindrical form with the diameter referred to as the wafer size and the height referred to as the wafer thickness. Semiconductor substrates as used in the context of the present invention may have a wafer size of 1-inch (25 mm) and having a thickness of typically around 275 pm; a wafer size of 2-inch (51 mm) and having a thickness of typically around 275 pm; a wafer size of 3-inch (76 mm) and having a thickness of typically around 375 pm; a wafer size of 4-inch (100 mm) and having a thickness of typically around 525 pm; a wafer size of 5-inch (125 mm) and having a thickness of typically around 625 pm; a wafer size of 6-inch (150 mm) and having a thickness of typically around 675 pm; a wafer size of 8-inch (200 mm) and having a thickness of typically around 725 pm; a wafer size of 12-inch (300 mm) and having a thickness of typically around 775 pm.

[0030] In the context of the present invention, the term "puck" is characterized as a cylindrical piece of monocrystalline material, composed of a compound semiconductor like silicon carbide or gallium arsenide. The typical dimensions for semiconductor pucks, such as those made of silicon carbide, can vary based on the application and manufacturing specifications. Generally, these pucks can range in diameter from about 100 mm to 300 mm (4 to 12 inches), with thicknesses in the order of a few millimeters to a few centimeters. The puck acts as a foundational platform, analogous to the substrate, facilitating the deposition or growth of thin material layers essential for semiconductor device fabrication, or is sliced into multiple wafers, the individual wafers being often less than a millimeter thick. In the context of the present invention, the term "wafer" is a synonym for substrate but typically refers to thinner slices of semiconductor materials, typically having a thickness of less than 1 mm. While a "puck" may serve as a foundational element in certain manufacturing processes, a "wafer" is more commonly associated with the later stages of semiconductor device fabrication. In the context of the present invention, the term "surface" is defined as the two- dimensional outer face or exterior boundary of a body or part of a body, such as a layer. Correspondingly, the term "surface area" is defined as the quantitative measure of said surface. Furthermore, the term "surface layer" is defined as the three-dimensional outer layer or exterior boundary of a body or part of a body, such as a layer. It is important to note that the aforementioned terms are distinct and should not be used interchangeably; the term "surface" is distinct from the term "surface area" and the term "surface layer."

[0031] In the context of the present invention, the term "film," "thin film" or "semiconductor film" denotes a semiconductor material with a substantially uniform thickness that is deposited on a surface. The film can exhibit either a porous or nonporous structure. In this context, the term "film" is used to describe a material that has a thickness ranging from 0.01 pm to 50 pm.

[0032] In the context of the present invention, the term "layer" or "semiconductor layer" refers to a semiconductor material having a substantially uniform thickness of a material covering a surface. A layer can be either continuous or discontinuous (i.e., having gaps between regions of the material). For example, a layer can completely or partially cover a surface, or be segmented into discrete regions, which collectively define the layer (i.e., regions formed using selective-area epitaxy). Furthermore, a layer can have a porous or a non-porous structure. In the context of the present invention, the term "layer" refers to a material having a thickness of at least 0.1 pm and at most 800 pm. Also, in the context of the present invention, the term "core" is to be understood as synonymous to the term "core layer."

[0033] A first layer or film, as described and / or depicted in the context of the present invention as "configured on," "deposited on," "on top of," "on," or "over" a second layer or film, may be immediately adjacent to the second layer or may be separated by one or more intervening layers. In a preferred embodiment, the first layer or film is in direct contact or bonded to the second layer or film. In the context of this invention, the term "disposed on" refers to the presence of a material on an underlying layer or substrate. This layer may include intermediate layers, such as transitional layers, to ensure an appropriate surface. For example, when a material is stated to be "disposed on a substrate," it may indicate that the material is in direct contact with the substrate, or it may be in contact with one or more transitional layers that are positioned on the substrate.

[0034] In the context of the present invention, the term "in direct contact with" refers to a state of physical adhesion between two distinct layers, characterized by the absence of an intervening bonding agent, such as such an organic or inorganic gluing agent. These layers may have similar compositions, crystallinities, and porosities, but can be distinguished by layer boundaries as observed through cross-sectional scanning electron microscopy analysis. The term is synonymous with "adhered directly to," "bonded directly to," and "in direct contact with."

[0035] In the context of the present invention, the term "porosity" refers to the presence of small voids or empty spaces within a material. These voids can be caused by a variety of factors, such as incomplete filling of the mold during the material's fabrication process, or by the evaporation of solvent during the material's synthesis. Porosity can have a significant impact on the material's electronic properties, such as its conductivity, as well as its mechanical properties, such as its strength and density. Porosity can also affect the material's ability to function as a substrate for the growth of epitaxial layers, which are important for many electronic and optoelectronic devices. Porosity can be measured using a variety of techniques, such as mercury intrusion porosimetry, nitrogen sorption, and helium pycnometry. Specifically, in the context of the present invention, the porosity of a material is expressed as volume percent, abbreviated as "vol.%" or as "%." In the context of the present invention, the porosity of a layer or a film can be determined by SEM analysis of said layer or film during multiple stages of an electrochemical etching process. SEM image analysis of a layer or film is obtained by etching with an electrolyte solution comprising 150 ml of 48 wt.% HF, 150 ml ethanol and 1200 ml deionized water in an etching chamber from AMMT GmbH for porous silicon etching and using a 250 Watt mercury arc lamp for front side illumination. The electrochemical etching process parameters used are (i) for C-face: 1 min 11.5V applied, 6 min 8.5 V applied, 1 min 11.5 V applied, 0.05 min 60 V applied for foil release from the substrate; and (ii) Si-face: 1 min 11.5V applied, 9 min 8.5 V applied, 1 min 11.5 V applied, 0.05 min 60 V applied for foil release from the substrate. The degree of porosity is analysed with an OpenCV image analysis library, using denoising and adaptive Gaussian image thresholding to determine the degree of porosity. In the context of the present invention, the term "porous" refers to a layer or film comprising pores, whereby the void volume of said layer or film is at least 1 vol.% of the total volume of said layer or film. Typically, the void volume of a porous layer is up to 30%, 40%, 50%, 60%, or even up to 70%. In the context of the present invention, the term "non-porous" refers to a layer or film preferably devoid of pores or a layer or film having a porosity of at most 1%, preferably at most 0.8%, more preferably at most 0.5% and most preferably 0%.

[0036] Any of the structures depicted and described herein can be part of larger structures with additional layers above and / or below those depicted. For clarity, the figures herein can omit these additional layers, although these additional layers can be part of the structures disclosed. In addition, the structures depicted can be repeated in units, even if this repetition is not depicted in the figures.

[0037] In the context of the present invention, the term photo-electrochemical wet etching (PECE) refers to an electrochemical porosification technique according to the experimental procedure which is, amongst others, described in Leitgeb, M. et al. Stacked Layers of Different Porosity in 4H SiC Substrates Applying a Photoelectrochemical Approach. J. Electrochem. Soc. 2017, 164 (12), E337, https: / / doi.Org / 10.1149 / 2.1081712jes; Leitgeb, M. et al. Metal Assisted Photochemical Etching of 4H Silicon Carbide. J. Phys. Appl. Phys. 2017, 50 (43), 435301, https: / / doi.org / 10.1088 / 1361-6463 / aa8942. The skilled person will appreciate that the porosity of the compound semiconductor surface film can easily be modified by variation of the electrochemical process parameters. The inventors have previously discovered that such an electrochemical porosification procedure maintains the crystallinity of the original semiconductor material.

[0038] In general, in a first aspect, the present invention provides a method for electrochemical wet etching of a monocrystalline silicon carbide substrate, comprising a step of propagation, whereby a monocrystalline silicon carbide substrate having a porous surface layer is electrochemically wet etched on an exposed surface comprising said porous surface layer, whereby the applied voltage, or in short the voltage, is varied during said electrochemical wet etching process step. The inventors have found that specific variation of the voltage during the electrochemical wet etching of a monocrystalline silicon carbide substrate allows to obtained a desired morphology of the porous layer.

[0039] The term "propagation" is to be understood as the process step whereby porosifica- tion through electrochemical wet etching, preferably photo-electrochemical wet etching (PECE), is propagated on a substrate having a porous surface layer on top of a monolithic substrate core.

[0040] More specifically, in a first aspect, the present invention provides a method for electrochemical wet etching of a monocrystalline silicon carbide substrate, comprising the steps of: i. initiation, whereby a surface layer of a monocrystalline silicon carbide substrate is electrochemically wet etched to produce a porous surface layer on the substrate; and ii. propagation, whereby the monocrystalline silicon carbide substrate obtained from step i. is further electrochemically wet etched at a progressively varying voltage, thereby obtaining a monocrystalline silicon carbide substrate having a porous, monocrystalline silicon carbide surface layer or top layer.

[0041] The term "initiation" is to be understood as the process step whereby porosification through electrochemical wet etching, preferably photo-electrochemical wet etching (PECE), is initiated on a substrate, whereby said substrate may be a partially po- rosified substrate having a porous surface layer on top of a monocrystalline substrate core, or whereby said substrate is monocrystalline.

[0042] Preferably, the voltage during the initiation phase is held constant or at least substantially constant. This means that the voltage does not or not significantly change and remains at a fixed level during a particular stage of the process. Ensuring a constant voltage in said initiation step ensures that a uniform frontline of porosity is formed.

[0043] During a significant part of the propagation step, i.e. at least 30% or even at least 50% of the period of said propagation step, the propagation proceeds through electrochemical wet etching at a progressively varying voltage. This means that the voltage is controlled to be constant during an uninterrupted period of time for less than 50% of the total time of the propagation phase, preferably less than 25% of the time, and more preferably less than 10% of the time. This ensures that the voltage variation is controlled and optimized for the specific etching requirements of the monocrystalline silicon carbide substrate. In the context of the present invention, the term "progressively varying the voltage" refers to any change in voltage over time during the propagation step of the electrochemical wet etching process. Although the term "progressively varying the voltage" refers to the process of increasing the voltage from a lower voltage to a higher voltage, or decreasing the voltage from a higher voltage to a lower voltage, temporary changes in direction of the progress are not excluded. E.g., a propagation phase whereby the voltage is progressively decreased from a higher to a lower voltage may experience one or more temporary increases in voltage to achieve a specific porosity profile. This includes, but is not limited to, continuous or discrete changes in voltage. The voltage may be adjusted in a variety of ways to achieve the desired etching characteristics of the monocrystalline silicon carbide substrate. Specifically, the voltage variation may encompass the following scenarios:

[0044] - The voltage may continuously increase from an initial lower voltage to a final higher voltage. This gradual increase can be linear or follow a more complex function such as exponential or logarithmic function. The voltage may continuously decrease from an initial higher voltage to a final lower voltage. This gradual decrease can be linear or follow a more complex function such as exponential or logarithmic function.

[0045] - The voltage may be increased in discrete steps or increments over time. Each increment can be uniform or vary in magnitude, allowing for a controlled etching process. The voltage may be decreased in discrete steps or increments, again with each decrement being uniform or variable.

[0046] - The voltage may fluctuate, involving cycles of increasing and decreasing voltages. This fluctuation can be periodic or aperiodic, depending on the specific requirements of the etching process. For instance, the voltage can be increased for a certain period, then decreased, and this pattern can repeat multiple times.

[0047] - The voltage may follow a combination of the above variations. For example, it may initially increase continuously, then decrease in steps, and then flue- tuate cyclically. The specific combination can be tailored to optimize the etching characteristics for different applications.

[0048] - The rate at which the voltage changes can also vary. This includes scenarios where the voltage change accelerates or decelerates over time. For example, the voltage might increase rapidly initially and then slow down as it approaches the final value.

[0049] Preferably, the monocrystalline silicon carbide substrate subjected to said electrochemically wet etching process comprises 4H-silicon carbide (4H-SiC). More preferably, said silicon carbide consists essentially of 4H-silicon carbide (4H-SiC). Preferably, the monocrystalline silicon carbide substrate subjected to said electrochemically wet etching process is electrochemically wet etched in step i. and ii. on a C- face surface layer.

[0050] The method according to the first aspect of the present invention allows for the formation, and the subsequent detachment, of a morphologically tuned, porous silicon carbide thin film from the photo-electrochemically wet etched monocrystalline silicon carbide substrate. The monocrystalline, porous silicon carbide thin film has characteristics which are directly the result of the electrochemical wet etching process parameters. I.e., the parameters defining the electrochemical wet etching process, specifically the applied voltage profile, allow to tailor the pores morphology of the obtained porous, monocrystalline silicon carbide thin film.

[0051] With the method according to the first aspect of the present invention, the obtained monocrystalline silicon carbide thin film can easily be structured to have a surface layer of medium porosity, a core of relatively low porosity, and a highly porous bottom layer.

[0052] A sufficiently high porosity of the surface layer can be achieved by applying a sufficiently high, yet substantially constant voltage during the initiation phase, as further detailed below. The sufficiently high, constant voltage ensures that the etching frontline advances uniformly across the substrate surface and provides a uniform etching frontline. In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, whereby the monocrystalline silicon carbide substrate which is used in step i. comprises a monocrystalline silicon carbide puck.

[0053] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, whereby said voltage is varied stepwise during said propagation step ii. in increments or decrements of at least 10 mV, preferably at least 25 mV. Preferably, said voltage is varied stepwise during said propagation step in increments or decrements of at least 10 mV, at least 15 mV, at least 20 mV, at least 25 mV, or even at least 50 mV. Preferably, said voltage is varied stepwise during said propagation step in increments or decrements of less than 1000 mV, less than 800 mV, less than 600 mV, less than 500 mV, less than 400 mV, or even less than 300 mV. Most preferably, said voltage is varied stepwise during said propagation step in increments or decrements of about 50 mV, 100 mV, 150 mV, 200 mV, 250 mV, or any value there in between. The inventors found that the size of the increment or decrement determines the morphology of the porous structure, especially of the porous bottom layer. Thus, selection of the optimized voltage increments or decrements as indicated above ensures that a high-quality, porous structure is achieved. This is important since this porous structure forms the basis of forming the line of controlled breakage downstream in the process, as further disclosed below.

[0054] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, whereby said voltage is decreased during said propagation step ii. The inventors found that starting the propagation phase at a higher voltage and lowering the voltage subsequently in a stepwise or steady manner in combination with etching at a higher voltage during the termination phase afforded a better morphological structure which allows for the subsequent formation of a more well-defined porous zone which acts as a line of controlled breakage.

[0055] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, whereby said voltage is varied during said propagation step ii. with a gradient of 50 mV / min to 1.000 mV / min, or with a gradient of -50 mV / min to -1.000 mV / min. In this context, the term "gradient" is to be under- stood as the "average slope" or the "average voltage slope" of the voltage profile. The average voltage slope can be calculated as the total voltage increase or decrease during the propagation phase divided by the time of the propagation phase. Preferably, the voltage is increased or decreased, preferably stepwise, during said propagation step whereby the absolute value of the gradient is 75 mV / min to 750 mV / min, and more preferably 100 mV / min to 500 mV / min. Most preferably, said absolute value of said gradient is 100 mV / min, 200 mV / min, 300 mV / min, 400 mV / min, 500 mV / min, or any value there in between.

[0056] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, whereby the voltage is progressively varied during the propagation step (ii) within a specified voltage window and over a certain time period. Preferably, the first voltage is between 7 V and 10 V, and the second voltage is between 10 V and 13 V. The voltage variation occurs over a voltage window of 4 V to 20 V, preferably of 5 V to 15 V. The voltage variation occurs over a processing window of 1 minute to 30 minutes, preferably for a period of 2 minutes to 20 minutes, and more preferably for a period between 3 minutes and 15 minutes. Most preferably, the voltage is varied over a period of 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, or any period therein between.

[0057] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, whereby said voltage is progressively varied during said propagation step ii. from a first voltage to a second voltage, whereby the difference between said first voltage and said second voltage is between 0.5 V and 7.5 V, preferably between 1.0 V and 5.0 V, and more preferably said difference is 1.0 V, 2.0 V, 3.0 V, 4.0 V, 5.0 V, or any value there in between. In one embodiment, the present invention provides a method according to the first aspect of the invention, whereby said first voltage is between 5 V and 10 V, and whereby said second voltage is between 8 V and 15 V. Preferably, said first voltage is between 7 V and 10 V, and said second voltage is between 10 V and 13 V. In this embodiment, said voltage is increased during said propagation phase over a period of 1 minute to 30 minutes, preferably for a period of 2 minutes to 20 minutes, and more preferably for a period between 3 minutes and 15 minutes. Most preferably, said voltage is varied stepwise over a period of 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, or any period there in between. Said voltage may be increased, stepwise or progressively, during said propagation step from a first voltage to a second voltage. Yet, in a more preferred embodiment, the present invention provides a process according to the first aspect of the invention, whereby said voltage is decreased stepwise during said propagation step from a first voltage to a second voltage, whereby said second voltage has a lower value than said first voltage, and whereby the difference between said first voltage and said second voltage is between 0.5 V and 7.5 V, preferably between 1.0 V and 5.0 V, and more preferably said difference is 1.0 V, 2.0 V, 3.0 V, 4.0 V, 5.0 V, or any value there in between. In a preferred embodiment, the present invention provides a process according to the first aspect of the invention, whereby said second voltage is between 5 V and 10 V, and whereby said first voltage is between 8 V and 15 V. Preferably, said second voltage is between 7 V and 10 V, and said first voltage is between 10 V and 13 V. Preferably, said voltage is decreased during said propagation phase over a period of 1 minute to 30 minutes, preferably for a period of 2 minutes to 20 minutes, and more preferably for a period between 3 minutes and 15 minutes. Most preferably, said voltage is decreased over a period of 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, or any period there in between.

[0058] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, whereby said voltage at the end of said propagation step ii. is initially held constant at a value between 5 V and 15 V, more preferably at a value between 10 V and 15 V, and even more preferably at a value of 10 V, 11 V, 12 V or 13 V, or any value there in between. Preferably, said voltage is held constant during said termination step for a period of 6 seconds to 300 seconds, preferably for a period of 15 seconds to 150 seconds, and more preferably for a period between 30 seconds and 90 seconds. Most preferably, said voltage is held constant during said termination step for a period of 30 seconds, 40 seconds, 50 seconds, 60 seconds, 70 seconds, 80 seconds, 90 seconds, or any value there in between.

[0059] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, whereby said voltage during said initiation step is constant. In a preferred embodiment, the present invention provides a process ac- cording to the first aspect of the invention, whereby said voltage during said initiation step is between 5 V and 15 V, preferably between 7 V and 15 V. Preferably, said voltage is held constant during said initiation step for a period of 6 seconds to 300 seconds, preferably for a period of 15 seconds to 150 seconds, and more preferably for a period between 30 seconds and 90 seconds. Most preferably, said voltage is held constant during said initiation step for a period of 30 seconds, 40 seconds, 50 seconds, 60 seconds, 70 seconds, 80 seconds, 90 seconds, or any value there in between.

[0060] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, whereby said monocrystalline silicon carbide substrate is electrochemically wet etched in step i. and ii. on a C-face surface layer.

[0061] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, whereby the step of electrochemical wet etching in step i. and / or step ii. comprises photo-electrochemical wet etching. The inventors found that porosification of the silicon carbide surface layer is achieved in absence of light as well, although photo-electrochemical wet etching is preferred.

[0062] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, whereby said voltage at the end of said propagation step is initially held constant at a value between 5 V and 15 V, more preferably at a value between 10 V and 15 V. This results in the formation of a highly porous bottom layer, which is suitably configured to form a line of controlled breakage upon applying a stress to the structure. Preferably, said voltage is held constant during the end of said propagation step for a period of 6 seconds to 300 seconds, preferably for a period of 15 seconds to 150 seconds, and more preferably for a period between 30 seconds and 90 seconds. Most preferably, said voltage is held constant during said the end of said propagation step for a period of 30 seconds, 40 seconds, 50 seconds, 60 seconds, 70 seconds, 80 seconds, 90 seconds, or any value there in between.

[0063] In a preferred embodiment, the present invention provides a method according to the first aspect of the invention, further comprising the step of: Hi. termination, whereby the monocrystalline silicon carbide substrate obtained from step ii. is electrochemically wet etched, preferably photo- electrochemically wet etched, whereby the applied voltage is sufficient to achieve a scission between said porous, monocrystalline silicon carbide surface layer and said monocrystalline silicon carbide substrate.

[0064] Preferably, the monocrystalline silicon carbide substrate obtained from step ii. is electrochemically wet etched, preferably photo-electrochemically wet etched, in the termination step at a constant voltage, whereby said voltage is between 30 V and 100 V. Preferably, the monocrystalline silicon carbide substrate which is released in step Hi. is subjected to an electrochemical wet etching method according to the first aspect of the invention.

[0065] In the termination phase, the applied voltage is raised to ensure that its effect on the porous surface layer is sufficient to achieve a scission between the porous surface layer and the underlying non-porous, monocrystalline silicon carbide substrate. In this context, the term "scission" is synonymous for the terms "cutting," "dividing," "splitting," "division" or "separation." Said scission refers to a complete cleavage or disconnect between a porous, monocrystalline silicon carbide thin film and the underlying non-porous, monocrystalline silicon carbide substrate. Preferably, the monocrystalline silicon carbide substrate obtained from step ii. is electrochemically wet etched in the termination step, step iii ., at a voltage of at least 30 V, preferably at least 40 V and more preferably at least 50 V. Preferably, said voltage during said termination step, step iii., is increased to a voltage not higher than 200 V, preferably not higher than 100 V, more preferably not higher than 90 V and even more preferably not higher than 80 V.

[0066] In a preferred embodiment, the present invention provides a process according to the first aspect of the invention, whereby the monocrystalline silicon carbide substrate which is released or regenerated in step iii. is subjected to a electrochemical wet etching process according to the first aspect of the invention. The inventors have contemplated that the electrochemical lift-off of a monocrystalline silicon carbide thin film allows for the re-use of the underlying substrate for subsequent liftoff of a second, third, fourth, etc. monocrystalline silicon carbide thin film according to the inventive processes of the present invention. More specifically, the present invention provides a method according to the first aspect of the invention, comprising the steps of: i. initiation, whereby a surface layer of a monocrystalline silicon carbide substrate is electrochemically wet etched at a constant voltage to produce a porous surface layer on the substrate; ii. propagation, whereby the monocrystalline silicon carbide substrate obtained from step i. is further electrochemically wet etched to produce a monocrystalline silicon carbide substrate having a porous, monocrystalline silicon carbide surface layer or top layer or substrate; and iii. termination, whereby the monocrystalline silicon carbide substrate obtained from step ii. is electrochemically wet etched, whereby the applied voltage is sufficient to achieve a scission between said porous, monocrystalline silicon carbide surface layer and said monocrystalline silicon carbide substrate, thereby obtaining a porous, monocrystalline silicon carbide thin film and regenerating a monocrystalline silicon carbide substrate.

[0067] Preferably, the method is characterized in that the applied voltage of the electrochemically wet etching process in said propagation step, step ii., is decreased, preferably stepwise decreased, from a higher voltage to a lower voltage. Alternatively, the method is characterized in that the applied voltage of the electrochemically wet etching process in said propagation step, step ii., is increased, preferably stepwise increased from a lower voltage to a higher voltage.

[0068] In a preferred embodiment, said steps i., ii. and iii. are executed sequentially.

[0069] Figures 1 and 4 schematically show the progress of the applied voltage during a process according to the first aspect of the invention.

[0070] In a second aspect, the present invention provides a porous, monocrystalline silicon carbide thin film obtained by a process according to the first aspect of the invention

[0071] In a third aspect, the present invention provides a porous, monocrystalline silicon carbide thin film comprising a top layer, a core layer and a bottom layer, whereby said top layer and said bottom layer are on opposite sides of said core layer, and whereby: i. said top layer has a thickness of 2 to 10 pm and an average porosity of less than 25 vol.%, or between 5 vol.% to 20 vol.%, ii. said core layer has a thickness of 2 pm to 15 pm having an average porosity between 5 vol.% and 20 vol.%, and iii. said bottom layer has a thickness of 1 pm to 10 pm and an average porosity of less than 10 vol.%, or even less than 5 vol.%, wherein said top layer is comprised of a surface layer of said porous, monocrystalline silicon carbide thin film which has an exposed Si-face surface; and wherein said bottom layer is comprised of a surface layer of said porous, monocrystalline silicon carbide thin film which has an exposed C-face surface. The porous, monocrystalline silicon carbide thin film is further characterized by a porosity of said core layer decreasing with increasing depth. In this context, it is to be understood that the porosity of said core layer decreases "gradually" or "stepwise" or "progressively" without excluding the possibility of local increases in porosity.

[0072] Alternatively to said third aspect, the present invention further provides a porous, monocrystalline silicon carbide thin film comprising a top layer, a core layer and a bottom layer, whereby said top layer and said bottom layer are on opposite sides of said core layer, and whereby: i. said top layer has a thickness of 2 to 10 pm and an average porosity of 5 vol.% to 20 vol.%, ii. said core layer has a thickness of 2 pm to 15 pm having an average porosity of less than 5 vol.%, and iii. said bottom layer has a thickness of 1 pm to 10 pm and an average porosity between 5 vol.% and 20 vol.%, whereby the porosity of said core layer increases with increasing depth. In this context, it is to be understood that the porosity of said core layer increases "gradually" or "stepwise" or "progressively" without excluding the possibility of local decreases in porosity. This is well illustrated in Figure 2. Figure 2 displays the porosity of a porous, monocrystalline silicon carbide thin film as described above and as obtained by the process according to the first aspect of the invention, whereby the porosity of the core layer, i.e., the layer at a depth of 5 pm to 20 pm, increases gradually as the depth increases. With reference to the term "porous, monocrystalline silicon carbide thin film," the term "top layer" is to be understood as a surface layer of said porous, monocrystalline silicon carbide thin film which has an exposed surface which is characterized as a Si-face surface; and the term "bottom layer" is to be understood as a surface layer of said porous, monocrystalline silicon carbide thin film which has an exposed surface which is characterized as a C-face surface.

[0073] In a fourth aspect, the present invention provides a method for producing an intermediate silicon carbide multilayer product, comprising the steps of: i. providing a monocrystalline, porous silicon carbide thin film according to the second or third aspect of the invention; and ii. binding a support layer onto an exposed surface, preferably on the exposed C-face surface, of said monocrystalline, porous silicon carbide thin film, thereby forming an intermediate silicon carbide multilayer product comprising a monocrystalline, porous silicon carbide thin film adhered to a support layer. Preferably, said support layer comprises a polycrystalline silicon carbide material.

[0074] In a preferred embodiment, the present invention provides a method according to the fourth aspect of the invention, wherein said monocrystalline, porous silicon carbide thin film is bonded onto said support layer, whereby a C-face surface of said monocrystalline, porous silicon carbide thin film is contacted with said support layer

[0075] In a preferred embodiment, the present invention provides a method according to the fourth aspect of the invention, wherein said support layer is bonded onto an exposed surface of said monocrystalline, porous silicon carbide thin film using a ceramic-forming polymer precursor. Preferably, said ceramic-forming polymer precursor comprises a polycarbosilane. The ceramic-forming polymer precursor preferably comprises essentially carbon, silicon, and hydrogen. When the hydrogen diffuses during the bonding process, only polycarbosilane-evolved silicon carbide may remain. For example, the ceramic-forming polymer precursor may be an allyl- hydrido-polycarbosilane or another polycarbosilane. The bonding process comprises the step of a) applying a ceramic-forming polymer precursor onto a surface of a support layer, b) applying the thin film onto the layer comprising the ceramicforming polymer precursor, c) pre-polymerizing said ceramic-forming polymer precursor at a temperature between 40°C and 400°C, d) subjecting the pre-treated structure to a thermal treatment at a temperature of 1400°C to 1700°C, preferably a temperature of 1400°C to 1650°C, preferably at a temperature above 1400°C, above 1450°C, or even above 1500°C and below 3000°C, below 2500°C, below 2000°C, below 1800°C, below 1700°C or even below 1600°C. More preferably, the thermal treatment is at a temperature of 1500°C to 1600°C, preferably at a temperature above 1550°C, such as 1560°C, 1570°C, 1580°C, 1590°C or 1600°C, or any temperature there in between. In one embodiment, step c) comprises prepolymerization of said ceramic-forming polymer precursor in presence of radical initiator at a temperature between 40°C and 400°C. Preferably, said radical initiator is a radical photoinitiator, more preferably a N-containing radical photoinitiator. N- containing radical photoinitiator provide the advantage that they introduce nitrogen in the silicon carbide crystal and accordingly improve conductivity. Preferably, said radical initiator is comprised in said ceramic-forming polymer precursor in an amount of 0.5 to 5.0 wt.%, relative to the total weight of said ceramic-forming polymer precursor, more preferably in an amount of 1, 2 or 3 wt.% or any amount there in between. Suitable radical initiators are, e.g., azobisisobutyronitrile (abbreviated AIBN). In another embodiment, step c) comprises pre-polymerization of said ceramic-forming polymer precursor in absence of a radical initiator at a temperature between 140°C and 400°C, more preferably between 200°C and 300°C, and most preferably at a temperature of about 250°C. Preferably, said thermal treatments are performed under an inert atmosphere, such as helium, argon or hydrogen gas. Preferably, the thermal treatments are performed under an atmosphere comprising silicon, e.g., in the form of Sil- . This is advantageous to suppress the outgassing of silicon from the silicon carbide material. In the context of the present invention, N2 gas is not considered to be an inert gas. Yet, said thermal treatments may proceed in presence of N2 gas. Preferably, said atmosphere is free of O2 gas. Preferably, said thermal treatments are performed for a period of 10 minutes to 8 hours, or for a period of at least at least 15 minutes, at least 20 minutes or at least 30 minutes. Preferably, said heat treatments are performed for a period of at most 4 hours, at most 2 hours or even at most 1 hour. Most preferably, said heat treatments are performed for a period of about 30 to 45 minutes.

[0076] Alternatively, the present invention provides a method according to the fourth aspect of the invention, wherein said support layer is bonded onto said monocrystalline, porous silicon carbide thin film through direct bonding of the thin film onto a support layer at higher temperature. The direct bonding process comprises the step of pressing the thin film onto a surface of a support layer and subjecting the struc- tures to a thermal treatment at a temperature of 1400°C to 1700°C, preferably a temperature of 1400°C to 1650°C, preferably at a temperature above 1400°C, above 1450°C, or even above 1500°C and below 3000°C, below 2500°C, below 2000°C, below 1800°C, below 1700°C or even below 1600°C. More preferably, the thermal treatment is at a temperature of 1500°C to 1600°C, preferably at a temperature above 1550°C, such as 1560°C, 1570°C, 1580°C, 1590°C or 1600°C, or any temperature there in between. Preferably, during said heat treatment, said monocrystalline, porous silicon carbide thin film is in direct contact with a support layer and is pressed onto said support layer at a hot-press pressure of 5 MPa to 100 MPa. Such processes are easily conducted in a hot-press. Preferably, said heat treatment is performed at a hot-press pressure between 10 MPa and 75 MPa, more preferably between 15 MPa and 60 MPa, and even more preferably between 20 MPa and 50 MPa. Most preferably, said heat treatment is performed at a hot-press pressure of about 20 MPa, 25 MPa, 30 MPa, 35 MPa, 40 MPa, 45 MPa or 50 MPa, or any pressure there in between. It was found that applying a pressure during the fusion bonding process improves the bonding characteristics of the obtained semiconductor layered structure. Preferably, said thermal treatment is performed under an inert atmosphere, such as helium, argon or hydrogen gas. Alternatively, the thermal treatment is performed under an atmosphere comprising Si, e.g., in the form of SiH4. This is advantageous to suppress the outgassing of Si from the silicon carbide material. In the context of the present invention, N2 gas is not considered to be an inert gas. Preferably, said atmosphere is free of O2 gas. Preferably, said thermal treatment is performed for a period of 10 minutes to 8 hours, or for a period of at least at least 15 minutes, at least 20 minutes or at least 30 minutes. Preferably, said heat treatment is performed for a period of at most 4 hours, at most 2 hours or even at most 1 hour. Most preferably, said heat treatment is performed for a period of about 30 to 45 minutes.

[0077] In addition, the present invention provides a method for preparing a multilayered silicon carbide wafer according to the fourth aspect of the invention, said method further comprising the step of: iii. epitaxially growing a monocrystalline silicon carbide overlayer onto an exposed surface of the porous, monocrystalline silicon carbide thin film of the intermediate silicon carbide multilayer product obtained in step ii. In a preferred embodiment, said monocrystalline silicon carbide overlayer is grown onto a Si-face surface of said monocrystalline, porous silicon carbide thin film.

[0078] This allows for a process for preparing a silicon carbide semiconductor overlayer on top of a material- and energy-economic silicon carbide semiconductor thin film. By doing so, dependence on expensive and high carbon footprint bulk substrates is decreased. Waste generation during the production process can be greatly reduced since handling of sensitive silicon carbide thin films is avoided, thereby contributing to an improved carbon dioxide footprint.

[0079] The growth and / or deposition of the monocrystalline silicon carbide overlayer in step iii. may be performed using one or more of chemical vapor deposition (CVD), metalorganic chemical vapor deposition (MOCVD), organometallic vapor phase epitaxy (OMVPE), atomic layer deposition (ALD), molecular beam epitaxy (MBE), hot- wall epitaxy (HWE), halide vapor phase epitaxy (HVPE), pulsed laser deposition (PLD), physical vapor deposition (PVD), and / or hybrid physical vapor deposition (PVD) / chemical vapor deposition (CVD).

[0080] In a preferred embodiment, the present invention provides a method according to the fourth aspect of the invention, further comprising the step of polishing a surface of a silicon carbide semiconductor wafer obtained by the process according to the fourth aspect of the invention, e.g., through mechanical, chemo-mechanical, electrochemical or photoelectrochemical polishing. Preferably, after said polishing step, said polished surface has a surface roughness of at most 50 nm, as determined by Atomic Force Microscopy (AFM). A suitable AFM procedure for determining surface roughness of Si nanostructures is described by Nagase et al. Metrology of Atomic Force Microscopy for Si Nano-Structures. Jpn. J. Appl. Phys. 1995, 34, 3382, https: / / iopscience.iop.org / article / 10.1143 / JJAP.34.3382 / meta. More preferably, said polished surface of said semiconductor substrate has a surface roughness of at most 20 nm, at most 10 nm, at most 5 nm, at most 2 nm, or even at most 1 nm. Most preferably, said polished surface has a surface roughness of about 0.9 nm, 0.8 nm, 0.7 nm, 0.6 nm, 0.5 nm, 0.4 nm, 0.3 nm, 0.2 nm, or 0.1 nm, or any value there in between. In a fifth aspect, the present invention provides a silicon carbide semiconductor product obtained by a method according to the fourth aspect of the invention.

[0081] In a final aspect, the present invention provides an electronic device for power electronics comprising a silicon carbide semiconductor product obtained by a method according to the fourth aspect of the invention. Such power electronic devices are suitable for use in applications of converting DC solar power to AC power for domestic use, and regulating functions with regard to battery power in hybrid electric vehicles. The higher bandgap of the compound semiconductor layered structure according to the present invention allows for the electronics that use it to be smaller and operate much more energy-efficiently. Compound semiconductors according to the present invention function at higher temperatures, higher voltages, and higher frequencies than some prior art semiconductors. Furthermore, the inventive compound semiconductor layered structures can advantageously be used a) as interface layer in SAW devices between piezoelectric layer and silicon substrate, and b) in MEMS, for fabrication of cantilevers or membranes from silicon carbide on Si substrate for harsh environmental applications.

[0082] EXAMPLES

[0083] The following examples are intended to further clarify the present invention, and are nowhere intended to limit the scope of the present invention.

[0084] EXAMPLE 1

[0085] A photo-electrochemical wet etching (PECE) method was employed to process a monocrystalline silicon carbide substrate with a diameter of about 50 mm. Figure 1 shows the applied voltage during the PECE process, whereby time (minutes) is shown on the X-axis, and voltage (V) is shown on the Y-axis, and whereby the Y- axis is cut off at 12 V for clarity. In a first phase (initiation) of the PECE process, a constant voltage of 11.5 V was applied to the substrate for 1 minute. In a second phase (propagation), the voltage was increased in 60 steps of 50 mV, each step lasting 9 seconds, starting from 8.5 V, and subsequently maintaining a constant voltage of 11.5 V for 1 minute. In a third phase (termination), the voltage was raised to 60 V to realize a lift-off of a porous silicon carbide thin film. The porosity, expressed as the fraction void volume relative to total volume, of the porous silicon carbide thin film is depicted in Figure 2 as a function of the etching depth, expressed in pm. Figure 3 depicts a SEM analysis of a cross section of the obtained porous silicon carbide thin film. The PECE process yields a thin film of porous, monocrystalline silicon carbide having a thickness of approximately 22 pm.

[0086] EXAMPLE 2

[0087] A thin film porous layer of silicon carbide is produced according to Example 1, whereby: in a first phase (initiation) of the PECE process, a constant voltage of 11.5 V was applied to the substrate for 1 minute; in a second phase (propagation), the voltage was decreased in 60 steps of 50 mV, each step lasting 9 seconds, starting from 8.5 V, and subsequently maintaining a constant voltage of 11.5 V for 1 minute; and in a third phase (termination), the voltage was raised to 60 V to realize a lift-off of a porous, monocrystalline silicon carbide thin film. Figure 4 shows the applied voltage during the PECE process, whereby time (minutes) is shown on the X-axis, and voltage (V) is shown on the Y-axis, and whereby the Y-axis is cut off at 12 V for clarity.

[0088] The Examples show that the varying voltage profile during the propagation phase of the has a distinct impact on the morphological characteristics of the porous silicon carbide thin film. The present invention thus allows for fine-tuning of the characteristics of the produced thin film.

[0089] Following the successful lift-off of the porous, monocrystalline silicon carbide thin film, the thin film is bonded onto a polycrystalline SiC. The exposed C-face surface of the thin film was bonded onto a substrate of polycrystalline silicon carbide using allylhydrido-polycarbosilane. The allylhydrido-polycarbosilane precursor is first applied onto the surface of the polycrystalline silicon carbide substrate and the thin film is applied there onto with the bottom facing the polycrystalline substrate. The precursor is then pre-polymerized in presence of azobisisobutyronitrile (AIBN) at a temperature of about 250°C, and the multilayer is then subjected to a thermal treatment at a temperature of about 1550°C for a period of about 45 minutes under an inert Ar atmosphere comprising silicon in the form of SiF to suppress the outgassing of silicon from the silicon carbide material. After bonding, the epitaxial growth of a monocrystalline silicon carbide overlayer was performed on the exposed Si-face surface of the thin film using chemical vapor deposition (CVD). A high-quality monocrystalline structure was obtained. This overlayer growth process demonstrates the capability of the described method to pre- pare a silicon carbide semiconductor overlayer on a material- and energy-economic silicon carbide semiconductor thin film having an contact surface with low porosity. The epitaxially grown overlayer exhibited excellent adhesion and uniformity, confirming the effectiveness of the described electrochemical wet etching process in producing high-quality substrates suitable for further semiconductor applications. This process, therefore, holds significant potential for enhancing the efficiency and sustainability of silicon carbide semiconductor production.

Claims

CLAIMS1. Method for electrochemical wet etching of a monocrystalline silicon carbide substrate, comprising the steps of: i. initiation, whereby a surface layer of a monocrystalline silicon carbide substrate is electrochemically wet etched to produce a porous surface layer on the substrate; ii. propagation, whereby the monocrystalline silicon carbide substrate obtained from step i. is further electrochemically wet etched at a progressively varying voltage, thereby obtaining a monocrystalline silicon carbide substrate having a porous, monocrystalline silicon carbide surface layer, iii. termination, whereby the monocrystalline silicon carbide substrate obtained from step ii. is electrochemically wet etched, whereby the applied voltage is sufficient to achieve a scission between said porous, monocrystalline silicon carbide surface layer and said monocrystalline silicon carbide substrate.

2. Method according to claim 1, whereby said voltage is varied stepwise during said propagation step ii. in increments or decrements of at least 10 mV.

3. Method according to claim 1 or 2, whereby said voltage is varied during said propagation step ii. with a gradient of 50 mV / min to 1.000 mV / min, or with a gradient of -50 mV / min to -1.000 mV / min.

4. Method according to any of claims 1 to 3, whereby said voltage is varied during said propagation step ii. from a first voltage to a second voltage, and whereby the difference between said first voltage and said second voltage is between 1.0 V and 5.0 V.

5. Method according to any of claims 1 to 4, whereby the voltage during the electrochemical wet etching propagation step ii. is decreased from a higher voltage to a lower voltage.

6. Method according to any of claims 1 to 5, whereby said voltage during said initiation step is constant.

7. Method according to any of claims 1 to 6, whereby said voltage during said initiation step is between 7 and 15 V.

8. Method according to any of claims 1 to 7, whereby said monocrystalline silicon carbide substrate is electrochemically wet etched in step i. and ii. on a C-face surface layer.

9. Method according to any of claims 1 to 8, whereby the step of electrochemical wet etching in step i. and / or step ii. comprises photo-electrochemical wet etching.

10. Method according to any of claims 1 to 9, whereby the monocrystalline silicon carbide substrate obtained from step ii. is electrochemically wet etched, preferably photo-electrochemically wet etched, in the termination step at a constant voltage, whereby said voltage is between 30 V and 100 V.

11. Method according to any of claims 1 to 10, whereby the monocrystalline silicon carbide substrate which is released in step iii. is subjected to an electrochemical wet etching method according to any of claims 1 to 10 without initiation step i.

12. Monocrystalline silicon carbide thin film obtained by a process according to any of claims 1 to 11.

13. Monocrystalline silicon carbide thin film comprising a top layer, a core layer and a bottom layer, whereby said top layer and said bottom layer are on opposite sides of said core layer, and whereby: i. said top layer has a thickness of 2 to 10 pm and an average porosity of 5 vol.% to 20 vol.%, ii. said core layer has a thickness of 2 pm to 15 pm having an average porosity between 5 vol.% and 20 vol.%, and iii. said bottom layer has a thickness of 1 pm to 10 pm and an average porosity of less than 10 vol.%, wherein said top layer has an exposed Si-face surface; and wherein said bottom layer has an exposed C-face surface.

14. Method for producing a multilayered silicon carbide wafer, comprising the steps of: i. providing a monocrystalline, porous silicon carbide thin film according to claim 13; ii. binding a support layer onto an exposed surface of said monocrystalline, porous silicon carbide thin film, thereby forming an intermediate silicon carbide multilayer product comprising a monocrystalline, porous silicon carbide thin film adhered to a support layer; and iii. epitaxially growing a monocrystalline silicon carbide overlayer onto an exposed surface of the porous, monocrystalline silicon carbide thin film of the intermediate silicon carbide multilayer product obtained in step ii.

15. Method according to claim 14, wherein said support layer comprises a polycrystalline material, preferably a polycrystalline silicon carbide material.

16. Method according to claim 14 or 15, wherein said support layer is bonded onto said monocrystalline, porous silicon carbide thin film using a ceramic-forming polymer precursor.

17. Method according to any of claims 14 to 16, further comprising the step of polishing a surface of a silicon carbide semiconductor wafer obtained by the process according to any of claims 14 to 16.

Citation Information

Patent Citations

  • Compound semiconductor layered structures and processes for making the same

    WO2022243501A1

  • Compound semiconductor layered structure and process for preparing the same

    WO2022184630A1

Cited By

  • Method for manufacturing a silicon carbide semiconductor component including a monocrystalline silicon carbide substrate and a polycrystalline silicon carbide substrate

    US12757645B2