Semiconductor device
The semiconductor device employs a recessed transistor structure with a vertical channel and stacked metal oxide layers to enhance on-state current and reliability, addressing limitations in oxide semiconductor devices related to leakage current and channel length, achieving efficient and reliable performance.
Patent Information
- Application Number
- PCT/IB2024/054865
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-05-20
- Publication Date
- 2024-11-28
AI Technical Summary
Current semiconductor devices face challenges in achieving high on-state current, low power consumption, miniaturization, high integration, and reliable electrical characteristics, particularly in transistors using oxide semiconductors, where leakage current and channel length limitations hinder performance.
A semiconductor device configuration featuring a transistor with a recessed structure, where the oxide semiconductor is in contact with both the source and drain electrodes, and a metal oxide gate electrode, allowing for a vertical channel configuration and improved electrical properties, including a stacked metal oxide structure with varying crystallinity to enhance conductivity and reduce defect levels.
This configuration enables a semiconductor device with increased on-state current, reduced power consumption, and improved reliability by minimizing leakage current and optimizing channel length, facilitating high integration and miniaturization while maintaining stable electrical characteristics.
Smart Images

Figure IB2024054865_28112024_PF_FP_ABST
Abstract
Description
Semiconductor Devices
[0001] 1. Field of the Invention One embodiment of the present invention relates to a semiconductor device, a memory device, and an electronic device. Another embodiment of the present invention relates to a manufacturing method of the semiconductor device.
[0002] One embodiment of the present invention is not limited to the above technical field, and examples of the technical field of one embodiment of the present invention include semiconductor devices, display devices, light-emitting devices, power storage devices, memory devices, electronic devices, lighting devices, input devices (e.g., touch sensors), input / output devices (e.g., touch panels), driving methods thereof, and manufacturing methods thereof.
[0003] In this specification and the like, a semiconductor device refers to any device that can function by utilizing semiconductor characteristics. Semiconductor elements such as transistors, as well as semiconductor circuits, arithmetic devices, and memory devices are all embodiments of semiconductor devices. Display devices (such as liquid crystal display devices and light-emitting display devices), projection devices, lighting devices, electro-optical devices, power storage devices, memory devices, semiconductor circuits, imaging devices, electronic devices, and the like may be considered to include semiconductor devices.
[0004] In recent years, the development of semiconductor devices has progressed, and semiconductor devices mainly use LSIs (Large Scale Integration), CPUs (Central Processing Units), memories, etc. A CPU is an aggregate of semiconductor elements that have semiconductor integrated circuits (at least transistors and memories) formed into chips by processing a semiconductor wafer and on which electrodes serving as connection terminals are formed.
[0005] 2. Description of the Related Art Semiconductor circuits (IC chips) such as LSIs, CPUs, and memories are mounted on circuit boards, such as printed wiring boards, and are used as components of various electronic devices.
[0006] Furthermore, a technology for constructing a transistor using a semiconductor thin film formed on a substrate having an insulating surface has attracted attention. Such transistors are widely applied to electronic devices such as integrated circuits (ICs) and image display devices (also simply referred to as display devices). While silicon-based semiconductor materials are widely known as semiconductor thin films applicable to transistors, oxide semiconductors have also attracted attention as other materials.
[0007] Furthermore, it is known that a transistor using an oxide semiconductor has an extremely small leakage current in a non-conducting state. For example, Patent Document 1 discloses a CPU with low power consumption that utilizes the property of a transistor using an oxide semiconductor having a small leakage current. Furthermore, Patent Document 2 discloses a memory device that can retain stored data for a long period of time by utilizing the property of a transistor using an oxide semiconductor having a small leakage current.
[0008] In recent years, with the trend toward smaller and lighter electronic devices, there has been an increasing demand for higher density integrated circuits. There is also a demand for improved productivity of semiconductor devices including integrated circuits. For example, Patent Document 3 and Non-Patent Document 1 disclose a technique for increasing the density of integrated circuits by stacking a first transistor using an oxide semiconductor film and a second transistor using an oxide semiconductor film to provide multiple memory cells in an overlapping manner. Furthermore, Patent Document 4, for example, discloses a technique for increasing the density of integrated circuits by vertically arranging the channel of a transistor using an oxide semiconductor film.
[0009] JP 2012-257187 A JP 2011-151383 A WO 2021 / 053473 JP 2013-211537 A
[0010] M. Oota et al. , “3D-Stacked CAAC-In-Ga-Zn Oxide FETs with Gate Length of 72nm”, IEDM Tech. Dig. , 2019, pp. 50-53
[0011] An object of one embodiment of the present invention is to provide a semiconductor device having favorable electrical characteristics.An object of one embodiment of the present invention is to provide a semiconductor device having a large on-state current.An object of one embodiment of the present invention is to provide a semiconductor device having a high operating speed.An object of one embodiment of the present invention is to provide a semiconductor device which can be miniaturized or highly integrated.An object of one embodiment of the present invention is to provide a highly reliable semiconductor device.An object of one embodiment of the present invention is to provide a semiconductor device in which variation in electrical characteristics of transistors is small.An object of one embodiment of the present invention is to provide a semiconductor device with low power consumption.An object of one embodiment of the present invention is to provide a novel semiconductor device.An object of one embodiment of the present invention is to provide a method for manufacturing a semiconductor device with high productivity.An object of one embodiment of the present invention is to provide a method for manufacturing a novel semiconductor device.
[0012] Another object of one embodiment of the present invention is to provide a memory device that can be miniaturized or highly integrated.An object of one embodiment of the present invention is to provide a memory device with a large storage capacity.An object of one embodiment of the present invention is to provide a memory device with high operation speed.An object of one embodiment of the present invention is to provide a memory device with low power consumption.An object of one embodiment of the present invention is to provide a novel memory device.
[0013] Note that the description of these problems does not preclude the existence of other problems. One embodiment of the present invention does not necessarily have to solve all of these problems. Problems other than these can be extracted from the description in the specification, drawings, and claims.
[0014] One embodiment of the present invention is a semiconductor device including a transistor and a first insulator. The transistor includes a first conductor, a second conductor over the first conductor and the first insulator, an oxide semiconductor, the second insulator, and a third conductor. The first insulator and the second conductor have openings that reach the first conductor. The first conductor has a recess that overlaps with the openings. Part of the oxide semiconductor, part of the second insulator, and part of the third conductor are provided in the recesses. The oxide semiconductor is in contact with the first conductor and the second conductor. The second insulator is disposed on the oxide semiconductor and in contact with at least a part of a top surface of the first conductor. The third conductor is disposed on the second insulator.
[0015] In the above, it is preferable that at least a part of the bottom surface of the oxide semiconductor be removed in the recess.
[0016] In the above, it is preferable that the lower surface of the third conductor is lower than the upper surface of the first conductor in the region that does not overlap with the opening.
[0017] In the above, it is preferable that the second conductor has a first layer and a second layer on the first layer, the first layer having a metal oxide, and the second layer having a higher conductivity than the first layer.
[0018] In the above, the first layer preferably contains indium. Furthermore, in the above, the first layer preferably contains tin and silicon.
[0019] In the above, the second layer preferably comprises tungsten.
[0020] In the above, it is preferable that the side surface of the first layer on the opening side is located closer to the opening side than the side surface of the second layer on the opening side.
[0021] In the above, the oxide semiconductor is preferably in contact with a side surface of the first layer on the opening side and a part of an upper surface of the first layer.
[0022] In the above, it is preferable that a third insulator is disposed between the second layer and the third conductor.
[0023] In the above, it is preferable that the first conductor has a third layer and a fourth layer on the third layer, the third layer being more conductive than the fourth layer, and the fourth layer having a metal oxide.
[0024] In the above, the third layer preferably comprises tungsten.
[0025] In the above, the fourth layer preferably contains indium. Furthermore, in the above, the fourth layer preferably contains tin and silicon.
[0026] In the above, the opening can be configured to reach the third layer.
[0027] Another embodiment of the present invention is a semiconductor device including a transistor and a first insulator. The transistor includes a first conductor provided over an underlayer insulator, a second conductor over the first conductor and the first insulator, an oxide semiconductor, the second insulator, and a third conductor. Openings reaching the underlayer insulator are provided in the first conductor, the first insulator, and the second conductor, and parts of the oxide semiconductor, the second insulator, and the third conductor are provided in the openings. The oxide semiconductor is in contact with the first conductor and the second conductor. The second insulator is disposed over the oxide semiconductor and in contact with at least a part of a top surface of the underlayer insulator. The third conductor is disposed over the second insulator.
[0028] According to one embodiment of the present invention, a semiconductor device having favorable electrical characteristics can be provided. According to one embodiment of the present invention, a semiconductor device having a large on-state current can be provided. According to one embodiment of the present invention, a semiconductor device having a high operating speed can be provided. According to one embodiment of the present invention, a semiconductor device which can be miniaturized or highly integrated can be provided. According to one embodiment of the present invention, a highly reliable semiconductor device can be provided. According to one embodiment of the present invention, a semiconductor device with little variation in electrical characteristics of transistors can be provided. According to one embodiment of the present invention, a semiconductor device with low power consumption can be provided. According to one embodiment of the present invention, a novel semiconductor device can be provided. According to one embodiment of the present invention, a method for manufacturing a semiconductor device with high productivity can be provided. According to one embodiment of the present invention, a method for manufacturing a novel semiconductor device can be provided.
[0029] According to one embodiment of the present invention, a memory device that can be miniaturized or highly integrated can be provided. According to one embodiment of the present invention, a memory device with a large storage capacity can be provided. According to one embodiment of the present invention, a memory device with a high operating speed can be provided. According to one embodiment of the present invention, a memory device with low power consumption can be provided. According to one embodiment of the present invention, a novel memory device can be provided.
[0030] Note that the description of these effects does not preclude the existence of other effects. One embodiment of the present invention does not necessarily have all of these effects. Effects other than these can be extracted from the description in the specification, drawings, and claims.
[0031] FIG. 1A is a plan view showing an example of a semiconductor device. FIGS. 1B to 1D are cross-sectional views showing an example of a semiconductor device. FIGS. 2A and 2B are cross-sectional views showing an example of a semiconductor device. FIGS. 3A to 3C are cross-sectional views showing an example of a semiconductor device. FIGS. 4A to 4F are cross-sectional views showing an example of a manufacturing method of a semiconductor device. FIGS. 5A to 5F are cross-sectional views showing an example of a manufacturing method of a semiconductor device. FIG. 6A is a plan view showing an example of a semiconductor device. FIGS. 6B to 6D are cross-sectional views showing an example of a semiconductor device. FIG. 7A is a plan view showing an example of a semiconductor device. FIGS. 7B to 7D are cross-sectional views showing an example of a semiconductor device. FIG. 8A is a plan view showing an example of a semiconductor device. FIGS. 8B to 8D are cross-sectional views showing an example of a semiconductor device. FIG. 9A is a plan view showing an example of a semiconductor device. FIGS. 9B to 9D are cross-sectional views showing an example of a semiconductor device. FIG. 10A is a plan view showing an example of a semiconductor device. FIGS. 10B to 10D are cross-sectional views showing an example of a semiconductor device. FIG. 11A is a plan view showing an example of a semiconductor device. FIG. 11B is a cross-sectional view showing an example of a semiconductor device. 12A and 12B are plan views illustrating an example of a semiconductor device. FIG. 12C is a cross-sectional view illustrating an example of a semiconductor device. FIG. 13A is a plan view illustrating an example of a semiconductor device. FIGS. 13B and 13C are cross-sectional views illustrating an example of a semiconductor device. FIGS. 14A and 14B are plan views illustrating an example of a semiconductor device. FIG. 14C is a cross-sectional view illustrating an example of a semiconductor device. FIGS. 15A to 15D are conceptual diagrams illustrating cross sections of an oxide semiconductor layer. FIG. 16 is a block diagram illustrating a configuration example of a semiconductor device. FIGS. 17A to 17H are diagrams illustrating a circuit configuration example of a memory cell. FIG. 18A is a plan view illustrating an example of a semiconductor device. FIGS. 18B and 18C are cross-sectional views illustrating an example of a semiconductor device. FIG. 19A is a plan view illustrating an example of a semiconductor device. FIG. 19B is a cross-sectional view illustrating an example of a semiconductor device. FIGS. 20A and 20B are perspective views illustrating a configuration example of a semiconductor device. FIG. 21 is a cross-sectional view illustrating an example of a semiconductor device. FIG. 22 is a block diagram illustrating a CPU. FIGS. 23A and 23B are perspective views of a semiconductor device. 24A and 24B are perspective views of a semiconductor device.FIGS. 25A and 25B are diagrams showing various types of storage devices by hierarchical level. FIGS. 26A and 26B are diagrams showing an example of electronic equipment, and FIGS. 26C to 26E are diagrams showing an example of a mainframe computer. FIG. 27 is a diagram showing an example of space equipment. FIG. 28 is a diagram showing an example of a storage system applicable to a data center. FIGS. 29A and 29B are configuration examples of a display device. FIG. 30 is a configuration example of a display device. FIG. 31 is a configuration example of a display device. FIGS. 32A to 32C are configuration examples of a display device. FIGS. 33A and 33B are configuration examples of a display device. FIGS. 34A to 34D are configuration examples of electronic equipment. FIGS. 35A to 35F are configuration examples of electronic equipment. FIGS. 36A to 36G are configuration examples of electronic equipment. FIG. 37 is a cross-sectional view of a transistor according to this example. FIG. 38 is a graph showing electrical characteristics of the transistor according to this example.
[0032] The embodiments will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various changes can be made in form and detail without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.
[0033] In the configuration of the invention described below, the same parts or parts having similar functions are denoted by the same reference numerals in different drawings, and repeated explanations thereof will be omitted. Furthermore, when referring to similar functions, the same hatching pattern may be used and no particular reference numeral may be assigned.
[0034] Furthermore, for ease of understanding, the position, size, range, etc. of each component shown in the drawings may not represent the actual position, size, range, etc. Therefore, the disclosed invention is not necessarily limited to the position, size, range, etc. disclosed in the drawings.
[0035] In order to facilitate understanding of the invention, particularly in plan views or perspective views, some components may be omitted from the drawings, and some hidden lines may be omitted.
[0036] In this specification, the ordinal numbers "first" and "second" are used for convenience and do not limit the number of components or the order of the components (for example, the order of processes or the order of stacking). Furthermore, the ordinal numbers assigned to components in one part of this specification may not match the ordinal numbers assigned to the same components in other parts of this specification or in the claims.
[0037] Note that the terms "film" and "layer" can be interchanged in some cases or depending on the situation. For example, the term "conductive layer" can be interchanged with the term "conductive film." Or, for example, the term "insulating film" can be interchanged with the term "insulating layer." Furthermore, the term "conductor" can be interchanged with the term "conductive layer" or the term "conductive film" in some cases or depending on the situation. Furthermore, the term "insulator" can be interchanged with the term "insulating layer" or the term "insulating film" in some cases or depending on the situation. Furthermore, the term "oxide semiconductor" can be interchanged with the term "oxide semiconductor layer" or the term "oxide semiconductor film" in some cases or depending on the situation.
[0038] Furthermore, in this specification, "parallel" refers to a state in which two straight lines are arranged at an angle of -10 degrees or more and 10 degrees or less. Therefore, it also includes cases in which the angle is -5 degrees or more and 5 degrees or less. Furthermore, "substantially parallel" refers to a state in which two straight lines are arranged at an angle of -30 degrees or more and 30 degrees or less. Furthermore, "perpendicular" refers to a state in which two straight lines are arranged at an angle of 80 degrees or more and 100 degrees or less. Therefore, it also includes cases in which the angle is 85 degrees or more and 95 degrees or less. Furthermore, "substantially perpendicular" refers to a state in which two straight lines are arranged at an angle of 60 degrees or more and 120 degrees or less.
[0039] The openings include, for example, grooves, slits, recesses, etc. Furthermore, the area in which the openings are formed may be referred to as an opening portion.
[0040] Furthermore, in the drawings used in this specification, the sidewalls of the insulator at the openings in the insulator are shown as being perpendicular or approximately perpendicular to the substrate surface or the surface on which the film is formed, but they may also be tapered.
[0041] In this specification, a tapered shape refers to a shape in which at least a portion of the side of a structure is inclined relative to the substrate surface or the surface on which the structure is to be formed. For example, the angle between the inclined side and the substrate surface or the surface on which the structure is to be formed (hereinafter, sometimes referred to as the taper angle) is less than 90°. The side of the structure and the substrate surface do not necessarily need to be completely flat, but may be substantially planar with a slight curvature or a substantially planar with minute irregularities. In this specification, a reverse tapered shape refers to a shape having a side or top that protrudes in a direction parallel to the substrate from the bottom.
[0042] In this specification, the term "equal heights" refers to a configuration in which the heights from a reference surface (e.g., a flat surface such as a substrate surface) are equal in cross-sectional view. For example, in a manufacturing process for a memory device, a planarization process (typically a chemical mechanical polishing (CMP) process) may be performed to expose the surface of a single layer or multiple layers. In this case, the surfaces treated by the CMP process are configured to have the same height from the reference surface. However, the heights of multiple layers may differ depending on the processing device, processing method, or material of the treated surface during the CMP process. In this specification, this case is also considered to be "equal heights." For example, when there are two layers (here, a first layer and a second layer) with different heights relative to the reference surface, and the difference in height between the top surface of the first layer and the top surface of the second layer is 20 nm or less, this is also considered to be "equal heights."
[0043] In this specification, "side edges coincide" means that, in a plan view, at least a portion of the contours of stacked layers overlap. For example, this includes cases where the upper and lower layers are processed using the same mask pattern or a portion of the same mask pattern. However, strictly speaking, the contours may not overlap, and the contour of the upper layer may be located inside the contour of the lower layer, or the contour of the upper layer may be located outside the contour of the lower layer. In these cases, the term "side edges coincide" is also used.
[0044] Generally, it is difficult to clearly distinguish between an "exact match" and an "approximate match." For this reason, in this specification, "match" includes both an exact match and an approximate match.
[0045] In this specification, the expression "the first film thickness and the second film thickness are the same" means that the absolute value of the difference between the first film thickness and the second film thickness divided by the first film thickness is 0.1 or less, or the absolute value of the difference between the first film thickness and the second film thickness divided by the second film thickness is 0.1 or less.
[0046] In this specification, the expression "distance A and distance B are the same" means that the value obtained by dividing the absolute value of the difference between distance A and distance B by distance A is 0.1 or less. Alternatively, the value obtained by dividing the absolute value of the difference between distance A and distance B by distance B is 0.1 or less.
[0047] Embodiment 1 In this embodiment, an example of a semiconductor device which is one embodiment of the present invention will be described with reference to FIGS. 1A to 14C.
[0048] <Structural Example of Semiconductor Device> An example of the structure of a semiconductor device according to one embodiment of the present invention will be described with reference to FIGS. 1A to 3C. FIGS. 1A to 1D are plan views and cross-sectional views of a semiconductor device including a transistor 200. FIG. 1A is a plan view of the semiconductor device. FIGS. 1B to 1D are cross-sectional views of the semiconductor device. FIG. 1B is a cross-sectional view of a portion indicated by a dashed dotted line A1-A2 in FIG. 1A. FIG. 1C is a cross-sectional view of a portion indicated by a dashed dotted line A3-A4 in FIG. 1A. Note that some elements are omitted from the plan view of FIG. 1A for clarity. FIGS. 2A and 2B are enlarged views corresponding to FIG. 1B. FIGS. 3A to 3C show other structural examples of the semiconductor device corresponding to FIG. 1B.
[0049] In the drawings and the like relating to this specification, arrows indicating the X direction, Y direction, and Z direction may be used. In this specification, the "X direction" refers to the direction along the X axis, and the forward direction and the reverse direction may not be distinguished unless explicitly stated. The same applies to the "Y direction" and the "Z direction." The X direction, Y direction, and Z direction are directions that intersect with each other. For example, the X direction, Y direction, and Z direction are directions that are perpendicular to each other. In this specification, one of the X direction, Y direction, and Z direction may be referred to as the "first direction" or "first direction." The other may be referred to as the "second direction" or "second direction." The remaining one may be referred to as the "third direction" or "third direction."
[0050] 1A to 1D includes an insulator 210 on a substrate (not shown), an insulator 222 on the insulator 210, a transistor 200 on the insulator 222, an insulator 280 on the insulator 222, an insulator 270 on the insulator 280, and an insulator 283 on the transistor 200. The insulators 210, 280, and 270 function as interlayer insulating films. The insulators 210 and 222 also function as base insulators.
[0051] The transistor 200 includes a conductor 220 over the insulator 222, a conductor 240 over the insulator 280, an oxide semiconductor 230 in contact with the conductor 220 and the conductor 240, an insulator 250 over the oxide semiconductor 230 and the insulator 270, and a conductor 260 over the insulator 250. The conductor 240 includes a conductor 240a and a conductor 240b over the conductor 240a. The conductor 220 includes a conductor 220a and a conductor 220b over the conductor 220a.
[0052] In the transistor 200, the oxide semiconductor 230 functions as a semiconductor layer, the conductor 260 functions as a gate electrode, the insulator 250 functions as a gate insulator, the conductor 220 functions as one of a source electrode and a drain electrode, and the conductor 240 functions as the other of the source electrode and the drain electrode.
[0053] In the transistor 200, a metal oxide (also referred to as an oxide semiconductor) functioning as a semiconductor is preferably used for the oxide semiconductor 230 including the channel formation region. Hereinafter, a transistor using an oxide semiconductor for a channel formation region, such as the transistor 200, may be referred to as an OS transistor.
[0054] As shown in FIGS. 1B and 1C , the insulator 280 and the conductor 240a have openings 290 that reach the conductor 220. A recess is formed in the upper surface of the conductor 220, and the recess overlaps the opening 290. The bottom of the opening 290 is the bottom surface of the recess in the conductor 220. The sidewalls of the opening 290 are the side surfaces of the insulator 280, the side surfaces of the conductor 240a, and the side surfaces of the recess in the conductor 220. The opening 290 includes an opening in the insulator 280 and an opening in the conductor 240a. In other words, the opening in the region where the insulator 280 overlaps with the conductor 220 is part of the opening 290, and the opening in the region where the conductor 240a overlaps with the conductor 220 is another part of the opening 290.
[0055] At least some of the components of the transistor 200 are disposed in the opening 290. Specifically, at least some of the oxide semiconductor 230, the insulator 250, and the conductor 260 are disposed in the opening 290.
[0056] Furthermore, the portions of the oxide semiconductor 230 and the insulator 250 that are disposed in the opening 290 are provided to reflect at least a part of the shape of the opening 290. That is, the oxide semiconductor 230 is provided so as to cover the sidewall of the opening 290, the insulator 250 is provided so as to cover the oxide semiconductor 230, and the conductor 260 is provided so as to fill the recess of the insulator 250 that reflects the shape of the opening 290.
[0057] However, at least a portion of the bottom surface of the oxide semiconductor 230 is removed in the opening 290. In other words, an opening is formed in part of the bottom surface of the oxide semiconductor 230. Therefore, in the region at the bottom of the opening 290 where the oxide semiconductor 230 has been removed, the insulator 250 is in contact with the conductor 220. That is, the insulator 250 is in contact with at least a portion of the top surface of the conductor 220. Here, when part of the bottom surface of the oxide semiconductor 230 is removed using lithography, the lower portion of the oxide semiconductor 230 has a shape that protrudes toward the center of the opening 290, as shown in FIGS. 1A to 1C . The protruding shape of the lower portion of the oxide semiconductor 230 is reflected in the shape of the insulator 250.
[0058] Here, the oxide semiconductor 230 is provided inside an opening formed in the insulator 280. The transistor 200 has a structure in which one of the source electrode and the drain electrode (the conductor 220 here) is located below and the other of the source electrode and the drain electrode (the conductor 240 here) is located above, and thus current flows vertically. That is, in the transistor 200, a channel is formed along the side surface of the opening 290 formed in the insulator 280. Therefore, the transistor of one embodiment of the present invention can be referred to as a vertical channel transistor or a vertical field effect transistor (VFET). Note that although the insulator 280 has a single-layer structure in FIGS. 1B and 1C , the insulator 280 is not limited thereto and can have a stacked-layer structure. For example, the insulator 280 can have a two-layer structure, in which the height of the top surface of the first insulator is the same as the height of the top surface of the conductor 220, and the second insulator is provided above the first insulator.
[0059] In the oxide semiconductor 230, a source region and a drain region are formed to sandwich a channel formation region. One of the source region and the drain region includes at least a part of a region of the oxide semiconductor 230 that is in contact with the conductor 240. The other of the source region and the drain region includes at least a part of a region of the oxide semiconductor 230 that is in contact with the conductor 220. That is, the channel formation region of the transistor 200 is located in a region of the oxide semiconductor 230 between the conductor 220 and the conductor 240. It can also be said that the channel formation region of the transistor 200 is located in a region of the oxide semiconductor 230 that is in contact with the insulator 280 or in a region in the vicinity of the insulator 280.
[0060] The channel length of the transistor 200 is the distance between the source region and the drain region. In other words, it can be said that the channel length of the transistor 200 is determined by the thickness of the insulator 280 on the conductor 220. In FIG. 1B , the channel length L of the transistor 200 is indicated by a dashed double-headed arrow. The channel length L is the distance between the edge of the region where the oxide semiconductor 230 and the conductor 220 contact each other and the edge of the region where the oxide semiconductor 230 and the conductor 240 contact each other in a cross-sectional view. It can also be said that the channel length L corresponds to the distance between the top surface of the conductor 220b and the bottom surface of the conductor 240a in a cross-sectional view.
[0061] 1D shows a cross-sectional view of the XY plane in the region between the conductor 220 and the conductor 240. As shown in FIG. 1D , the oxide semiconductor 230, the insulator 250, and the conductor 260 are concentrically arranged inside the opening 290 of the insulator 280. Therefore, the side surface of the conductor 260 provided in the center faces the side surface of the oxide semiconductor 230 with the insulator 250 interposed therebetween. That is, in the region between the conductor 220 and the conductor 240, the entire periphery of the oxide semiconductor 230 becomes a channel formation region.
[0062] In this case, if no recess is formed on the top surface of the conductor 220 and the top surface of the conductor 220 is flat, the insulator 250 is formed on the conductor 220, and the bottom surface of the conductor 260 becomes higher than the top surface of the conductor 220. In this case, the contact between the oxide semiconductor 230 and the conductor 220 becomes bottom contact, which is mainly performed on the bottom surface of the oxide semiconductor 230. In the vicinity of the conductor 220, the concentric structure of the oxide semiconductor 230, the insulator 250, and the conductor 260 shown in FIG. 1D is no longer formed. As a result, an offset region is formed in the oxide semiconductor 230 near the conductor 220, which may cause degradation in electrical characteristics of the transistor, such as on-state current, subthreshold swing (hereinafter sometimes referred to as S value), field-effect mobility, and frequency characteristics.
[0063] In contrast, it is preferable to form a recess in the conductor 220 that overlaps with the opening 290 as described above, and provide the conductor 260 so as to be embedded in the recess. With this configuration, as shown in FIG. 2A , the height H1 of the lower surface of the conductor 260 is lower than the height H2 of the upper surface of the conductor 220 in a region that does not overlap with the opening 290. Here, the heights H1 and H2 are based on the lower surface of the conductor 220. In this case, contact between the oxide semiconductor 230 and the conductor 220 is side contact that occurs mainly on the side surface of the oxide semiconductor 230. Furthermore, as described above, by forming a region in which at least a portion of the bottom surface of the oxide semiconductor 230 is removed and configuring a structure in which the insulator 250 is in contact with the conductor 220 in the region, the height H1 of the lower surface of the conductor 260 in the region can be further reduced.
[0064] With the above structure, the oxide semiconductor 230, the insulator 250, and the conductor 260 can be provided concentrically even in the region near the conductor 220. That is, in the region near the conductor 220, the conductor 260 and the oxide semiconductor 230 can be provided with their side surfaces facing each other with the insulator 250 interposed therebetween. Therefore, the electric field of the conductor 260 functioning as a gate electrode can be sufficiently applied to the oxide semiconductor 230 even in the vicinity of the conductor 220. This can prevent an offset region from being formed in the oxide semiconductor 230 near the conductor 220. In this way, the electrical characteristics of the transistor 200, such as the on-state current, the S value, the field-effect mobility, and the frequency characteristics, can be improved.
[0065] Furthermore, in planar transistors, the channel length is limited by the exposure limit of lithography, making further miniaturization difficult. In the present invention, the channel length can be set by the film thickness of the insulator 280 on the conductor 220. Therefore, the channel length L of the transistor 200 can be, for example, 1 μm or less, 500 nm or less, 100 nm or less, 60 nm or less, 50 nm or less, 40 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less, and 0.1 nm or more, 1 nm or more, or 5 nm or more. For example, by making the channel length L a very fine structure that is equal to or less than the exposure limit of lithography, the on-state current, frequency characteristics, and the like of the transistor 200 can be improved. Furthermore, for example, by increasing the channel length L, drain-induced barrier lowering (DIBL) can be suppressed in the transistor 200, thereby improving the electrical characteristics.
[0066] Furthermore, as described above, a channel formation region, a source region, and a drain region can be formed in the opening 290. This allows the area occupied by the transistor 200 to be reduced compared to a planar transistor in which the channel formation region, the source region, and the drain region are separately provided on the XY plane. For example, while the area occupied by the transistor 200 is reduced, the channel length L can be made larger than the width in the X direction and the width in the Y direction of the transistor 200. This allows for higher integration of the semiconductor device. Furthermore, when the semiconductor device of one embodiment of the present invention is used in a memory device, the memory capacity per unit area can be increased.
[0067] As shown in FIG. 1D , in the region between the conductor 220 and the conductor 240, the entire periphery of the oxide semiconductor 230 becomes a channel formation region. In this case, for example, the channel width of the transistor 200 is determined by the periphery length of the oxide semiconductor 230. In other words, the channel width of the transistor 200 can be determined by the maximum width of the opening 290 (the maximum diameter when the opening 290 is circular in plan view). In FIGS. 1B and 1D , the maximum width D of the opening 290 is indicated by a double-headed, dashed arrow. In FIG. 1D , the channel width W of the transistor 200 is indicated by a double-headed, dashed arrow. By increasing the maximum width D of the opening 290, the channel width per unit area can be increased, and the on-current can be increased.
[0068] When the opening 290 is formed using lithography, the maximum width D of the opening 290 is limited by the exposure limit of lithography. The maximum width D of the opening 290 is set depending on the film thickness of each of the oxide semiconductor 230, the insulator 250, and the conductor 260 provided in the opening 290. The maximum width D of the opening 290 is, for example, 5 nm or more, 10 nm or more, or 20 nm or more, and is preferably 100 nm or less, 60 nm or less, 50 nm or less, 40 nm or less, or 30 nm or less. Note that when the opening 290 has a circular shape in a plan view, the maximum width D of the opening 290 corresponds to the diameter of the opening 290, and the channel width W can be calculated as "D × π".
[0069] Furthermore, by forming the opening 290 so as to have a circular shape in a plan view, the oxide semiconductor 230, the insulator 250, and the conductor 260 are arranged concentrically. This makes the distance between the conductor 260 and the oxide semiconductor 230 approximately uniform, allowing a gate electric field to be applied to the oxide semiconductor 230 approximately uniformly.
[0070] In this embodiment, an example has been shown in which the opening 290 is circular in plan view, but the present invention is not limited to this. For example, the opening 290 may be approximately circular in plan view, such as an ellipse, polygonal in plan view, or polygonal in plan view with rounded corners. In this case, the maximum width of the opening 290 can be calculated appropriately according to the shape of the top of the opening 290. For example, if the opening is rectangular in plan view, the maximum width of the opening 290 can be considered to be the length of the diagonal line at the top of the opening 290.
[0071] Furthermore, it is preferable that the sidewalls of the opening 290 are perpendicular to the upper surface of the insulator 210. With this configuration, miniaturization or high integration of the semiconductor device can be achieved.
[0072] 1B and 1C, the opening 290 is provided so that the sidewall of the opening 290 is perpendicular to the upper surface of the conductor 220, but the present invention is not limited to this. For example, the sidewall of the opening 290 may not be strictly perpendicular but may have a tapered shape. The taper angle formed between the side surface of the insulator 280, which is part of the sidewall of the opening 290, and the upper surface of the conductor 220 (which may be the upper surface of the insulator 222 or the upper surface of the insulator 210) is preferably 90 degrees or an angle close to 90 degrees. For example, the taper angle is preferably between 75 degrees and 90 degrees.
[0073] The taper angle may be less than 75 degrees, less than 70 degrees, less than 65 degrees, or less than 60 degrees. The tapered sidewall of the opening 290 allows the oxide semiconductor 230 and the insulator 250 to be deposited with good coverage.
[0074] The oxide semiconductor 230 is in contact with the side surface of the conductor 240a facing the opening 290, part of the top surface of the conductor 240a, the side surface of the conductor 240b facing the opening 290, and the top surface of the conductor 240b. As shown in FIG. 1C , the side surface of the oxide semiconductor 230 is preferably flush with the side surface of the conductor 240a opposite the opening 290 and the side surface of the conductor 240b opposite the opening 290. This configuration allows the oxide semiconductor 230, the conductor 240a, and the conductor 240b to be processed in the same process, thereby simplifying the manufacturing process of the semiconductor device.
[0075] 1B shows a configuration in which the oxide semiconductor 230 is arranged to extend in the X direction, but the present invention is not limited to this. For example, the oxide semiconductor 230 may have an island shape.
[0076] 1C shows a configuration in which the side surface of the oxide semiconductor 230 is flush with the side surfaces of the conductor 240a and the conductor 240b, but the present invention is not limited to this. For example, a structure in which the side surface of the oxide semiconductor 230 is located more inward than the side surfaces of the conductor 240a and the conductor 240b in the Y direction may be used. Alternatively, a structure in which the side surface of the oxide semiconductor 230 is located more outward than the side surfaces of the conductor 240a and the conductor 240b may be used. In this case, a structure in which the conductor 240a and the conductor 240b are covered with the oxide semiconductor 230 may be used.
[0077] As the oxide semiconductor 230, a metal oxide described in the section [Metal Oxide] below can be used as a single layer or a stacked layer.
[0078] Specifically, the oxide semiconductor 230 may be a metal oxide having an atomic ratio of In:M:Zn = 1:3:2 or a composition thereof, an atomic ratio of In:M:Zn = 1:3:4 or a composition thereof, an atomic ratio of In:M:Zn = 1:1:0.5 or a composition thereof, an atomic ratio of In:M:Zn = 1:1:1 or a composition thereof, an atomic ratio of In:M:Zn = 1:1:1.2 or a composition thereof, an atomic ratio of In:M:Zn = 1:1:2 or a composition thereof, or an atomic ratio of In:M:Zn = 4:2:3 or a composition thereof. Note that a composition having an atomic ratio in the vicinity thereof includes a range of ±30% of the desired atomic ratio. Furthermore, it is preferable to use one or more of gallium, aluminum, and tin as the element M.
[0079] The oxide semiconductor 230 may not contain the element M. For example, the metal oxide used as the oxide semiconductor 230 may be an In—Zn oxide. Specifically, the oxide semiconductor 230 may have a composition of In:Zn=1:1 (atomic ratio) or a composition thereabout, or an In:Zn=4:1 (atomic ratio) or a composition thereabout. Alternatively, indium oxide may be used as the oxide semiconductor 230. Furthermore, the oxide semiconductor 230 may contain a trace amount of the element M. For example, the oxide semiconductor 230 may have a composition of In:Sn:Zn=4:0.1:1 (atomic ratio) or a composition thereabout.
[0080] For example, energy dispersive X-ray spectroscopy (EDX), X-ray photoelectron spectroscopy (XPS), inductively coupled plasma mass spectrometry (ICP-MS), or inductively coupled plasma atomic emission spectrometry (ICP-AES) can be used to analyze the composition of the metal oxide used in the oxide semiconductor 230. Alternatively, a combination of these techniques may be used for the analysis. For elements with low content, the actual content may differ from the content obtained by analysis due to the influence of analytical accuracy. For example, when the content of element M is low, the content of element M obtained by analysis may be lower than the actual content.
[0081] The metal oxide can be preferably formed by sputtering or atomic layer deposition (ALD). When the metal oxide is formed by sputtering, the composition of the formed metal oxide may differ from the composition of the sputtering target. In particular, the zinc content in the formed metal oxide may be reduced to about 50% of that of the sputtering target.
[0082] Examples of the ALD method include a thermal ALD method in which a precursor and a reactant are reacted using only thermal energy, and a plasma enhanced ALD (PEALD) method in which a plasma-excited reactant is used.
[0083] The ALD method allows atoms to be deposited layer by layer, and therefore has the advantages of enabling ultrathin film formation, film formation on high-aspect-ratio structures or surfaces with large steps, film formation with fewer defects such as pinholes, film formation with excellent coverage, and film formation at low temperatures. Furthermore, the PEALD method may be preferable because it utilizes plasma, enabling film formation at lower temperatures. Note that some precursors used in the ALD method contain elements such as carbon or chlorine. Therefore, films formed by the ALD method may contain higher amounts of elements such as carbon or chlorine than films formed by other film formation methods. The amounts of these elements can be quantified using XPS or SIMS. The metal oxide film formation method of one embodiment of the present invention uses the ALD method, but employs one or both of a high substrate temperature during film formation and an impurity removal treatment. Therefore, the amount of carbon and chlorine contained in the film may be lower than when the ALD method is used without these.
[0084] Unlike film formation methods in which particles emitted from a target or the like are deposited, the ALD method is a film formation method in which a film is formed by a reaction on the surface of a workpiece. Therefore, it is a film formation method that is less affected by the shape of the workpiece and has good step coverage. In particular, the ALD method has excellent step coverage and excellent thickness uniformity, making it suitable for coating the surface of an opening with a high aspect ratio. However, because the ALD method has a relatively slow film formation rate, it may be preferable to use it in combination with other film formation methods, such as a sputtering method or a CVD method, which have a faster film formation rate. For example, when a metal oxide has a layered structure of a first metal oxide and a second metal oxide, a method can be used in which the first metal oxide is formed by a sputtering method and the second metal oxide is formed on the first metal oxide by an ALD method. For example, when the first metal oxide has crystalline portions, the second metal oxide may grow as crystals using the crystalline portions as nuclei.
[0085] The ALD method can control the composition of the resulting film by adjusting the amount of source gas introduced. For example, the ALD method can form a film of any composition by adjusting the amount of source gas introduced, the number of introductions (also referred to as the number of pulses), the time required for one pulse (also referred to as the pulse time), etc. Furthermore, for example, the ALD method can form a film whose composition changes continuously by changing the source gas while forming the film. When forming a film while changing the source gas, the time required for film formation can be shortened compared to when forming a film using multiple film formation chambers because no time is required for transportation and pressure adjustment. Therefore, the productivity of semiconductor devices can be improved in some cases.
[0086] Note that there is no particular limitation on the method for forming the oxide semiconductor film that becomes the oxide semiconductor 230. For example, the oxide semiconductor film may be formed by a CVD method, an MBE method, a PLD method, or the like.
[0087] The crystallinity of the semiconductor material used for the oxide semiconductor 230 is not particularly limited, and any of an amorphous semiconductor (a semiconductor having an amorphous structure), a single crystal semiconductor (a semiconductor having a single crystal structure), and a semiconductor having crystallinity other than single crystal (a microcrystalline semiconductor, a polycrystalline semiconductor, or a semiconductor having a crystalline region in part) may be used. Use of a single crystal semiconductor or a crystalline semiconductor is preferable because it can suppress deterioration of transistor characteristics.
[0088] The oxide semiconductor 230 preferably includes a crystalline metal oxide layer. Examples of the crystalline metal oxide structure include a c-axis aligned crystal (CAAC) structure, a polycrystalline (poly-crystal) structure, and a nanocrystalline (nc) structure. By using a crystalline metal oxide layer for the oxide semiconductor 230, the density of defect states in the oxide semiconductor 230 can be reduced, thereby realizing a highly reliable semiconductor device. The CAAC structure is a crystal structure in which multiple microcrystals (typically, multiple IGZO microcrystals) have c-axis orientation and are connected without being oriented in the a-b plane. Furthermore, when a cross section of an OS film having a CAAC structure is observed using a high-resolution TEM image, it can be confirmed that metal atoms are arranged in a layered manner in the crystalline portion. Therefore, an OS film having a CAAC structure can also be said to have a layered crystalline portion.
[0089] A polycrystalline structure has crystal grain boundaries. Furthermore, when a heat treatment is performed after forming an oxide semiconductor layer with a polycrystalline structure, tiny gaps (also referred to as nanocracks or microcracks) or tiny spaces (also referred to as nanospaces or microspaces) can be formed between crystal portions. When tiny gaps or tiny spaces are formed in the oxide semiconductor layer, the electrical resistance of the oxide semiconductor layer increases. This is because the electrical resistance of the tiny gaps or tiny spaces is very high, for example, infinite. When an oxide semiconductor layer having tiny gaps or tiny spaces is used in a channel formation region of a transistor, the contact resistance between the oxide semiconductor layer and one or both of a source electrode and a drain electrode increases. This adversely affects the initial characteristics or reliability of the transistor. The CAAC structure has fewer crystal grain boundaries in the a-b plane than a polycrystalline structure, and therefore can realize a highly reliable semiconductor device.
[0090] The higher the crystallinity of the metal oxide layer used for the oxide semiconductor 230, the more the density of defect states in the oxide semiconductor 230 can be reduced. On the other hand, by using a metal oxide layer with low crystallinity, a transistor capable of passing a large current can be realized.
[0091] The higher the substrate temperature (stage temperature) during the formation of the metal oxide layer, the higher the crystallinity of the formed metal oxide layer.Furthermore, the higher the ratio of the flow rate of oxygen gas to the total film formation gas used during the formation (hereinafter also referred to as oxygen flow rate ratio), the higher the crystallinity of the formed metal oxide layer.
[0092] The crystallinity of the oxide semiconductor 230 can be analyzed by, for example, X-ray diffraction (XRD), a transmission electron microscope (TEM), or electron diffraction (ED). Alternatively, the analysis may be performed by combining a plurality of these techniques.
[0093] 1B and 1C, the oxide semiconductor 230 is shown as a single layer, but the present invention is not limited to this. The oxide semiconductor 230 may have a stacked structure of multiple oxide layers with different chemical compositions. For example, the oxide semiconductor 230 may have a structure in which multiple types of metal oxides selected from those described in the section "Metal Oxide" below are appropriately stacked.
[0094] The oxide semiconductor 230 can have a stacked structure of two or more metal oxide layers with different crystallinity. In this case, the two or more metal oxide layers may have different compositions or the same or approximately the same composition. For example, as shown in FIG. 2A , the oxide semiconductor 230 may have a stacked structure of an oxide semiconductor 230a and an oxide semiconductor 230b over the oxide semiconductor 230a. Here, the oxide semiconductor 230b can have a region with higher crystallinity than the oxide semiconductor 230a. Alternatively, the oxide semiconductor 230b can have a region with lower crystallinity than the oxide semiconductor 230a. Note that when the oxide semiconductor 230b has a region with lower crystallinity than the oxide semiconductor 230a, the crystallinity of the oxide semiconductor 230b can be increased by performing heat treatment (also referred to as crystallization treatment) after the oxide semiconductor 230b is formed.
[0095] For example, it is preferable to use a metal oxide having an In:M:Zn=1:3:2 (atomic ratio) or a metal oxide having an In:M:Zn=1:3:4 ... Alternatively, for example, a stacked structure of any one selected from indium oxide, indium gallium oxide, and IGZO and any one selected from IAZO, IAGZO, and ITZO (registered trademark) may be used.
[0096] The conductivity of the material used for the oxide semiconductor 230a is preferably different from the conductivity of the material used for the oxide semiconductor 230b.
[0097] For example, the oxide semiconductor 230a can be made of a material having higher conductivity than the oxide semiconductor 230b. By using a material having high conductivity for the oxide semiconductor 230a which is in contact with the conductor 220 and the conductor 240 which function as a source electrode or a drain electrode, the contact resistance between the oxide semiconductor 230 and the conductor 220 and the contact resistance between the oxide semiconductor 230 and the conductor 240 can be reduced, and a transistor with high on-state current can be obtained.
[0098] Here, if a material with high conductivity is used for the oxide semiconductor 230b provided on the conductor 260 side functioning as the gate electrode, the threshold voltage of the transistor may shift, and the drain current that flows when the gate voltage is 0 V (hereinafter also referred to as cutoff current) may become large. Specifically, if the transistor 200 is an n-channel transistor, the threshold voltage may be reduced. Therefore, it is preferable to use a material with lower conductivity than the oxide semiconductor 230a for the oxide semiconductor 230b. As a result, if the transistor 200 is an n-channel transistor, the threshold voltage can be increased, and the transistor can have a small cutoff current. Note that a small cutoff current is sometimes referred to as a normally-off transistor.
[0099] As described above, by using a material having higher conductivity than the oxide semiconductor 230b for the oxide semiconductor 230a, a normally-off transistor with a large on-state current can be obtained, thereby providing a semiconductor device that achieves both low power consumption and high performance.
[0100] Note that the carrier concentration of the oxide semiconductor 230a is preferably higher than that of the oxide semiconductor 230b. Increasing the carrier concentration of the oxide semiconductor 230a increases the conductivity, and the contact resistance between the oxide semiconductor 230 and the conductor 220 and the contact resistance between the oxide semiconductor 230 and the conductor 240 can be reduced, resulting in a transistor with a large on-state current. Decreasing the carrier concentration of the oxide semiconductor 230b decreases the conductivity, resulting in a normally-off transistor.
[0101] Here, an example is shown in which the oxide semiconductor 230a is made of a material having a higher conductivity than the oxide semiconductor 230b, but the present invention is not limited to this. The oxide semiconductor 230a may be made of a material having a lower conductivity than the oxide semiconductor 230b. A configuration in which the carrier concentration of the oxide semiconductor 230a is lower than the carrier concentration of the oxide semiconductor 230b may be used.
[0102] The band gap of the first metal oxide used in the oxide semiconductor 230 a is preferably different from the band gap of the second metal oxide used in the oxide semiconductor 230 b. For example, the difference between the band gaps of the first metal oxide and the second metal oxide is preferably 0.1 eV or more, more preferably 0.2 eV or more, and even more preferably 0.3 eV or more.
[0103] The band gap of the first metal oxide used for the oxide semiconductor 230a can be smaller than the band gap of the second metal oxide used for the oxide semiconductor 230b. As a result, the contact resistance between the oxide semiconductor 230 and the conductor 220 and the contact resistance between the oxide semiconductor 230 and the conductor 240 can be reduced, and the transistor can have a large on-state current. Furthermore, when the transistor 200 is an n-channel transistor, the threshold voltage can be increased, and the transistor can be a normally-off transistor.
[0104] Although an example in which the band gap of the first metal oxide is smaller than that of the second metal oxide has been shown here, the present invention is not limited to this example and may have a configuration in which the band gap of the first metal oxide is larger than that of the second metal oxide.
[0105] As described above, the band gap of the first metal oxide used in the oxide semiconductor 230a can be smaller than the band gap of the second metal oxide used in the oxide semiconductor 230b. The composition of the first metal oxide is preferably different from that of the second metal oxide. The band gap can be controlled by differentiating the compositions of the first metal oxide and the second metal oxide. For example, the content of element M in the first metal oxide is preferably lower than the content of element M in the second metal oxide. Specifically, when the first metal oxide and the second metal oxide are In-M-Zn oxides, the first metal oxide can have a composition of In:M:Zn = 1:1:1 [atomic ratio] or a composition therearound, and the second metal oxide can have a composition of In:M:Zn = 1:3:2 [atomic ratio] or a composition therearound. It is particularly preferable to use one or more of gallium, aluminum, and tin as the element M.
[0106] The first metal oxide may not contain the element M. For example, the first metal oxide used for the oxide semiconductor 230a may be In—Zn oxide, and the second metal oxide used for the oxide semiconductor 230b may be In-M-Zn oxide. Specifically, the first metal oxide may be In—Zn oxide, and the second metal oxide may be In—Ga—Zn oxide. More specifically, the first metal oxide may have a composition of In:Zn=1:1 (atomic ratio) or a composition thereof in the vicinity thereof, or a composition of In:Zn=4:1 (atomic ratio) or a composition thereof in the vicinity thereof, and the second metal oxide may have a composition of In:Ga:Zn=1:1:1 (atomic ratio) or a composition thereof in the vicinity thereof. Alternatively, the first metal oxide may contain a trace amount of the element M. For example, the first metal oxide may have a composition of In:Sn:Zn=4:0.1:1 (atomic ratio) or a composition thereof in the vicinity thereof.
[0107] Here, an example is shown in which the content of element M in the first metal oxide is lower than the content of element M in the second metal oxide, but one embodiment of the present invention is not limited to this. The content of element M in the first metal oxide may be higher than the content of element M in the second metal oxide. Note that the first metal oxide and the second metal oxide may have different compositions, and the contents of elements other than element M may also be different. Furthermore, the first metal oxide and the second metal oxide may have the same or substantially similar compositions. In this case, it is preferable to use different film formation methods for the first metal oxide and the second metal oxide.
[0108] When the oxide semiconductors 230a and 230b are formed by different methods, it is preferable to use an ALD method and a sputtering method. For example, a first metal oxide film used for the oxide semiconductor 230a can be formed by sputtering, and a second metal oxide film used for the oxide semiconductor 230b can be formed by ALD. Alternatively, for example, a first metal oxide film used for the oxide semiconductor 230a can be formed by ALD, and a second metal oxide film used for the oxide semiconductor 230b can be formed by sputtering.
[0109] The thickness of the oxide semiconductor 230 is preferably 3 nm to 200 nm, more preferably 3 nm to 100 nm, further preferably 5 nm to 100 nm, further preferably 10 nm to 100 nm, further preferably 10 nm to 70 nm, further preferably 15 nm to 70 nm, further preferably 15 nm to 50 nm, and further preferably 20 nm to 50 nm. In a transistor used in a smaller semiconductor device, the thickness of the oxide semiconductor 230 is preferably 1 nm to 3 nm, or 5 nm, and is preferably 20 nm to 15 nm, 12 nm to 10 nm.
[0110] The thickness of each layer (here, the oxide semiconductor 230a and the oxide semiconductor 230b) constituting the oxide semiconductor 230 may be determined so that the thickness of the oxide semiconductor 230 falls within the above-described range. The thickness of the oxide semiconductor 230a can be determined so that the contact resistance between the oxide semiconductor 230a and the conductor 220 and the contact resistance between the oxide semiconductor 230a and the conductor 240 fall within the desired range. The thickness of the oxide semiconductor 230b can be determined so that the threshold voltage of the transistor falls within the desired range. Note that the thickness of the oxide semiconductor 230a may be the same as or different from the thickness of the oxide semiconductor 230b.
[0111] Furthermore, the oxide semiconductor 230a and the oxide semiconductor 230b may have different ratios of the film thickness at the portion where the top surface of the conductor 240 is the formation surface to the film thickness at the portion where the side surface of the conductor 240 and the side surface of the insulator 280 are the formation surfaces.
[0112] 2A shows the oxide semiconductor 230 having a two-layer structure of an oxide semiconductor 230a and an oxide semiconductor 230b, but the present invention is not limited to this. The oxide semiconductor 230 may have a three-layer or more layer structure.
[0113] 2B, the oxide semiconductor 230 may have a stacked structure of an oxide semiconductor 230a, an oxide semiconductor 230b on the oxide semiconductor 230a, and an oxide semiconductor 230c on the oxide semiconductor 230b. In other words, in the configuration shown in FIG. 2A, the oxide semiconductor 230c may be provided between the insulator 250 and the oxide semiconductor 230b.
[0114] In the metal oxide used for the oxide semiconductor 230a, the atomic ratio of the element M to In is preferably larger than the atomic ratio of the element M to In in the metal oxide used for the oxide semiconductor 230b. This configuration can suppress the diffusion of impurities and oxygen from structures formed outside the oxide semiconductor 230a to the oxide semiconductor 230b. Furthermore, it can suppress the diffusion of elements contained in the insulator 280, the conductor 220, or the conductor 240 into the oxide semiconductor 230b.
[0115] When a material with high conductivity is used for the oxide semiconductor 230c provided on the conductor 260 side functioning as a gate electrode, the threshold voltage of the transistor 200 might shift and the cutoff current might increase. Specifically, when the transistor 200 is an n-channel transistor, the threshold voltage might decrease. Therefore, it is preferable to use a material with lower conductivity than the oxide semiconductor 230b for the oxide semiconductor 230c. As a result, when the transistor 200 is an n-channel transistor, the threshold voltage can be increased and the cutoff current can be reduced.
[0116] As described above, by using a material having higher conductivity than that of the oxide semiconductor 230c for the oxide semiconductor 230b, a normally-off transistor with large on-state current can be obtained, thereby providing a semiconductor device with both low power consumption and high performance.
[0117] The carrier concentration of the oxide semiconductor 230b is preferably higher than that of the oxide semiconductor 230c. Increasing the carrier concentration of the oxide semiconductor 230b increases the conductivity, resulting in a transistor with a large on-state current. Increasing the carrier concentration of the oxide semiconductor 230c decreases the conductivity, resulting in a normally-off transistor.
[0118] Here, an example is shown in which the oxide semiconductor 230b is made of a material having higher conductivity than the oxide semiconductor 230c, but one embodiment of the present invention is not limited to this. The oxide semiconductor 230b may be made of a material having lower conductivity than the oxide semiconductor 230c. The carrier concentration of the oxide semiconductor 230b may be lower than the carrier concentration of the oxide semiconductor 230c.
[0119] The oxide semiconductors 230a and 230c preferably have a larger band gap than the oxide semiconductor 230b. Thus, the oxide semiconductor 230b is sandwiched between the pair of oxide semiconductors with a larger band gap, and the oxide semiconductor 230b mainly functions as a current path (channel). The sandwiching of the oxide semiconductor 230b between the pair of oxide semiconductors can reduce trap states at the interface of the oxide semiconductor 230b and in its vicinity. This allows a buried-channel transistor in which the channel is spaced away from the insulating layer interface to be realized, thereby increasing the field-effect mobility. Furthermore, the influence of interface states that may form on the back channel side can be reduced, suppressing photodegradation (e.g., photodegradation due to negative bias current) of the transistor and improving the reliability of the transistor.
[0120] The first metal oxide used in the oxide semiconductor 230a and the third metal oxide used in the oxide semiconductor 230c may have the same composition or different compositions.
[0121] For example, the oxide semiconductors 230a and 230c may be made of a metal oxide having an atomic ratio of In:Ga:Zn=1:1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Ga:Zn=1:3:2 or a composition thereof, or a metal oxide having an atomic ratio of In:Ga:Zn=1:3:4 or a composition thereof. Furthermore, the oxide semiconductor 230b may be made of a metal oxide having an atomic ratio of In:Zn=1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Zn=2:1 or a composition thereof, a metal oxide having an atomic ratio of In:Sn:Zn=2:0.1:1 or a composition thereof, a metal oxide having an atomic ratio of In:Zn=4:1 or a composition thereof, a metal oxide having an atomic ratio of In:Sn:Zn=4:0.1:1 or a composition thereof, or an indium oxide. With this structure, the on-state current of the transistor 200 can be increased, and the transistor structure can have high reliability with little variation.
[0122] Note that the oxide semiconductors 230a, 230b, and 230c may be formed by different methods. In this case, it is preferable to use an ALD method and a sputtering method. For example, a first metal oxide film for the oxide semiconductor 230a may be formed by sputtering, a second metal oxide film for the oxide semiconductor 230b may be formed by ALD, and a third metal oxide film for the oxide semiconductor 230c may be formed by sputtering. Alternatively, for example, a first metal oxide film for the oxide semiconductor 230a may be formed by ALD, a second metal oxide film for the oxide semiconductor 230b may be formed by sputtering, and a third metal oxide film for the oxide semiconductor 230c may be formed by ALD.
[0123] Furthermore, when forming the oxide semiconductor layer having the above-described two-layer structure, it is preferable to use two types of film formation methods, namely, a sputtering method and an ALD method. For example, if a first oxide semiconductor layer having a CAAC structure is formed by a sputtering method and then a second oxide semiconductor layer having lower crystallinity than the CAAC structure is formed by an ALD method, it is expected that the atomic layer of the second oxide semiconductor layer fills or repairs gaps in the atomic-level crystalline portions of the CAAC structure of the first oxide semiconductor layer. Furthermore, it is preferable to perform heat treatment (for example, at 100° C. or higher and 500° C. or lower, preferably 200° C. or higher and 450° C. or lower, more preferably 300° C. or higher and 400° C. or lower) after forming the second oxide semiconductor layer by the ALD method. It is expected that the heat treatment will repair gaps in the atomic-level crystalline portions of the CAAC structure of the first oxide semiconductor layer with the second oxide semiconductor layer (in other words, each crystalline molecule formed by the ALD method). An oxide semiconductor layer formed using the above two types of film formation methods may be referred to as a hybrid OS.
[0124] Here, the concept of heat treatment for improving the crystallinity of an oxide semiconductor layer will be described with reference to Figures 15A, 15B, 15C, and 15D. Figures 15A, 15B, 15C, and 15D are conceptual diagrams illustrating cross sections of an oxide semiconductor layer having a CAAC structure. In each of the figures, the c-axis is indicated by an arrow.
[0125] The oxide semiconductor layer 370a shown in FIG. 15A includes a region 372a and a region 372b located between the regions 372a. The region 372a corresponds to a region of a CAAC structure (i.e., a structure having layered crystalline portions), and the region 372b corresponds to a region between the CAAC structures. The CAAC structure has fewer grain boundaries in the a-b plane than a polycrystalline structure. Thus, even in the oxide semiconductor layer 370a having the CAAC structure, minute gaps or spaces (regions 372b in FIG. 15A ) may exist between the crystalline portions.
[0126] Therefore, in order to improve the crystallinity of the oxide semiconductor layer, in other words, to reduce the region 372b shown in FIG. 15A , an oxide semiconductor layer having a CAAC structure is formed as a first oxide semiconductor layer by a sputtering method, and then an oxide semiconductor layer having a microcrystalline structure or an amorphous structure, which has lower crystallinity than the CAAC structure, is formed as a second oxide semiconductor layer by an ALD method.
[0127] 15B , an oxide semiconductor layer having a region 372 a is formed by sputtering as a first oxide semiconductor layer, and then an oxide semiconductor layer having a region 372 c with lower crystallinity than a CAAC structure is formed by ALD as a second oxide semiconductor layer. In FIG. 15B , the oxide semiconductor layer 370 b has the region 372 a and the region 372 c. Since the ALD method can deposit atoms layer by layer, the second oxide semiconductor layer can be formed to fill the region 372 b.
[0128] Then, heat treatment is performed to enhance the crystallinity of the region 372c of the second oxide semiconductor layer using the region 372a of the first oxide semiconductor layer as a seed. In other words, the region 372c of the second oxide semiconductor layer can be crystal-grown using the region 372a of the first oxide semiconductor layer as a seed. Alternatively, the region 372a of the first oxide semiconductor layer having a CAAC structure can be used as a nucleus to crystal-grow the region 372c of the second oxide semiconductor layer having an amorphous structure. This crystal growth model can be considered as a concept equivalent to heteroepitaxy. Note that in FIG. 15C , the oxide semiconductor layer 370c includes the region 372a and the region 372c. The region 372a shown in FIG. 15C has higher crystallinity or a higher density of crystalline portions than the region 372a shown in FIG. 15B. By performing heat treatment, the crystallinity of one or both of the regions 372a and 372c can be improved. Furthermore, the region 372c has, for example, a crystalline portion having the same crystal structure as the crystalline portion of the region 372a. Alternatively, the region 372c has, for example, a crystalline portion connected to the crystalline portion of the region 372a.
[0129] 15D , the oxide semiconductor layer 370d includes a region 372a. The region 372a has improved crystallinity compared to the region 372a shown in FIGS. 15B and 15C , and the boundary between the region 372a and the region 372c disappears, or the boundary between the region 372a and the region 372c is no longer visible. Therefore, the entire oxide semiconductor layer 370d has a CAAC structure. When the entire oxide semiconductor layer 370d has a CAAC structure as shown in FIG. 15D , a highly reliable semiconductor device can be realized. The presence or absence of the boundary between the region 372a and the region 372c can be confirmed using, for example, cross-sectional TEM, cross-sectional STEM, or the like.
[0130] Note that even when the first oxide semiconductor layer has minute gaps or spaces, the minute gaps or spaces in the first oxide semiconductor layer can be filled by forming a second oxide semiconductor layer over the first oxide semiconductor layer or by forming the second oxide semiconductor layer and then performing heat treatment. In this manner, by using an oxide semiconductor layer with a CAAC structure for the first oxide semiconductor layer and an oxide semiconductor layer with a microcrystalline structure or an amorphous structure for the second oxide semiconductor layer, a dense oxide semiconductor layer with increased crystallinity can be obtained. When the dense oxide semiconductor layer with increased crystallinity is used for a channel formation region of a transistor, it is expected that an increase in the electrical resistance of the oxide semiconductor layer can be suppressed or initial characteristics (particularly, on-state current) of the transistor can be improved, thereby making the transistor suitable for high-speed operation.
[0131] When an oxide semiconductor layer is formed by both a sputtering method and an ALD method, if the thickness of the oxide semiconductor layer formed by the ALD method is small, the oxide semiconductor layer can be regarded as a single-layer structure, not a stacked structure of the oxide semiconductor layer formed by the sputtering method and the oxide semiconductor layer formed by the ALD method. For example, when the thickness of the oxide semiconductor layer formed by the ALD method is more than 0 nm and less than or equal to 3 nm, preferably more than 0 nm and less than or equal to 2 nm, and more preferably more than 0 nm and less than or equal to 1 nm, the oxide semiconductor layer formed by the two film formation methods, that is, the sputtering method and the ALD method, can be regarded as a single-layer structure. On the other hand, when the thickness of the oxide semiconductor layer formed by the ALD method exceeds 3 nm, the oxide semiconductor layer can be regarded as a stacked structure, a multilayer structure, or a multiple structure of the oxide semiconductor layer formed by the sputtering method and the oxide semiconductor layer formed by the ALD method.
[0132] Furthermore, when an oxide semiconductor layer is formed by both a sputtering method and an ALD method, it is preferable that the compositions of the metal oxide layers be different from each other. Typically, a metal oxide having an atomic ratio of In:Ga:Zn=1:1:1 or a composition thereabout can be formed by a sputtering method, and then a metal oxide having an atomic ratio of In:Ga:Zn=4:0.1:1 or a composition thereabout can be formed by an ALD method. By using an oxide semiconductor layer having the above composition, a structure can be obtained in which the metal oxide layer having an atomic ratio of In:Ga:Zn=1:1:1 has high reliability, and the metal oxide having an atomic ratio of In:Ga:Zn=4:0.1:1 or a composition thereabout can have high on-state current or high field-effect mobility. Instead of a metal oxide having a composition of In:Ga:Zn=4:0.1:1 (atomic ratio) or a composition close to that, a metal oxide having an atomic ratio of In:Ga:Zn=1:0:0 (atomic ratio), i.e., indium oxide or a metal oxide having a high proportion of In, can be used.
[0133] The oxide semiconductor layer formed by the above two types of film formation methods can be regarded as a structure in which gaps in the crystal parts of a CAAC structure are filled with atomic layers formed by an ALD method. Note that the structure can be analyzed by analytical techniques such as cross-sectional SEM, cross-sectional STEM, cross-sectional TEM, SIMS, and EDX.
[0134] In addition, an oxide semiconductor layer having a CAAC structure formed by the above-described two kinds of film formation methods may have higher relative dielectric constant, film density, and film hardness than an oxide semiconductor layer having a CAAC structure formed by one kind of film formation method. Thus, by using an oxide semiconductor layer having a CAAC structure formed by two kinds of film formation methods in a channel formation region of a transistor, a transistor with excellent characteristics (e.g., a transistor with high on-state current, a transistor with high field-effect mobility, a transistor with a small S value, a transistor with high frequency characteristics (also referred to as f characteristics), a highly reliable transistor, etc.) can be realized.
[0135] To improve the electrical characteristics and reliability of an OS transistor, it is important to sufficiently reduce the hydrogen concentration in a channel formation region of an oxide semiconductor. For example, the hydrogen concentration in the channel formation region of an oxide semiconductor measured by secondary ion mass spectrometry (SIMS) is 1×10 20 atoms / cm 3 Preferably less than 5 x 10 19 atoms / cm 3 More preferably, less than 1 x 10 19 atoms / cm 3 Less than 5×10 is more preferable. 18 atoms / cm 3 More preferably, less than 1 x 10 18 atoms / cm 3 More preferably, less than 1 x 10 17 atoms / cm 3 Less than is even more preferred.
[0136] Therefore, it is preferable that a barrier insulator against hydrogen be used for the insulator 210 and the insulator 283. The insulator 210 and the insulator 283 are provided to sandwich the transistor 200 including the oxide semiconductor 230. When the insulator 210 and the insulator 283 provided on the outer side of the oxide semiconductor 230 have a barrier property against hydrogen, diffusion of hydrogen into the oxide semiconductor 230 can be suppressed.
[0137] In this specification and the like, a barrier insulator refers to an insulator having barrier properties. The barrier properties are defined as a property that makes it difficult for a corresponding substance to diffuse (also referred to as a property that makes it difficult for a corresponding substance to permeate, a property that makes the corresponding substance less permeable, or a function that suppresses the diffusion of a corresponding substance). Note that hydrogen when described as a corresponding substance includes, for example, a hydrogen atom, a hydrogen molecule, a water molecule, and OH. − Furthermore, unless otherwise specified, impurities when described as corresponding substances refer to impurities in the channel formation region or semiconductor layer, and include, for example, hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, and nitrogen oxide molecules (N 2 O, NO, NO 2 The term "oxygen" refers to at least one of an oxygen atom, an oxygen molecule, etc., when described as a corresponding substance.
[0138] Examples of barrier insulators against hydrogen include aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, indium gallium zinc oxide, silicon nitride, and silicon nitride oxide.
[0139] It is preferable to use, for example, silicon nitride as the insulator 210 and the insulator 283. In this case, the insulator 210 and the insulator 283 contain silicon and nitrogen.
[0140] Silicon nitride applicable to the insulator 210 and the insulator 283 has barrier properties against hydrogen if the film thickness is, for example, 2 nm or more. To enhance the barrier properties against hydrogen, the silicon nitride film thickness is preferably 3 nm or more, and more preferably 5 nm or more. Silicon nitride has barrier properties against oxygen if the film thickness is, for example, 1 nm or more. To enhance the barrier properties against oxygen, the silicon nitride film thickness is preferably 2 nm or more. In other words, silicon nitride formed to a film thickness that has barrier properties against hydrogen also has barrier properties against oxygen.
[0141] The insulator 222 is preferably an insulator having a function of capturing or fixing hydrogen. When the insulator 222 has a function of capturing or fixing hydrogen, the hydrogen concentration in the oxide semiconductor 230 located between the insulators 210 and 283 can be reduced. At this time, hydrogen in the oxide semiconductor 230 is captured or fixed by the insulator 222, so the hydrogen concentration in the insulator 222 is increased. For example, the hydrogen concentration in at least a part of the insulator 222 obtained by SIMS is 1×10 19 atoms / cm 3 or more, or 1 x 10 20 atoms / cm 3 In this case, the hydrogen concentration in at least a part of the insulator 222 is higher than the hydrogen concentration in the oxide semiconductor 230. In other words, the oxide semiconductor 230 has a region where the hydrogen concentration is lower than the hydrogen concentration in the insulator 222.
[0142] The ability to capture or fix a corresponding substance can also be said to have the property of making it difficult for the corresponding substance to diffuse. Therefore, the ability to capture or fix a corresponding substance can be rephrased as barrier properties.
[0143] As an insulator having the function of capturing or fixing hydrogen, a metal oxide containing hafnium or the like (e.g., hafnium oxide, etc.) is preferable. Furthermore, the above metal oxide preferably has oxygen atoms with dangling bonds. Such metal oxides may have the property of capturing or fixing hydrogen through dangling bonds. For example, the above metal oxide preferably has an amorphous structure. This is because in metal oxides with an amorphous structure, some oxygen atoms have dangling bonds. Note that the above metal oxide preferably has an amorphous structure, but crystalline regions may be formed in some parts. Furthermore, the above metal oxide may have crystal grain boundaries in some parts.
[0144] Here, adding silicon to hafnium oxide can suppress crystallization of hafnium oxide. In other words, an oxide containing hafnium and silicon (hereinafter, sometimes referred to as hafnium silicate) tends to have an amorphous structure. Therefore, hafnium silicate has the property of capturing or fixing hydrogen, making it suitable as the insulator 222. In this case, the insulator 222 contains hafnium, silicon, and oxygen.
[0145] In the above, oxides containing hafnium are cited as examples of insulators having the function of capturing or fixing hydrogen, but the present invention is not limited to this. Examples include oxides containing magnesium, oxides containing aluminum, and oxides containing aluminum and hafnium (hafnium aluminate). Furthermore, the above metal oxides may be further converted into oxides containing zirconium. For example, oxides containing hafnium and zirconium are included. Furthermore, it is preferable that these metal oxides have silicon added thereto and have an amorphous structure.
[0146] The insulator 280 covers the conductor 220 and is in contact with the side surface of the oxide semiconductor 230 and the bottom surface of the conductor 240. The insulator 280 is preferably formed using a material with a low dielectric constant. This allows the insulator 280 to function as an interlayer insulating film, thereby reducing the parasitic capacitance between the conductor 240 and the conductor 220. This enables the frequency characteristics of the transistor 200 to be improved.
[0147] The insulator 280 can be a single layer or a stack of insulators containing a material with a low dielectric constant, as described in the section [Insulator] below. Specifically, silicon oxide or silicon oxynitride can be used as the insulator 280. The concentrations of impurities such as water and hydrogen in the insulator 280 are preferably reduced. This can prevent impurities such as water and hydrogen from entering the channel formation region of the oxide semiconductor 230.
[0148] An insulator containing oxygen is preferably used for the insulator 280. When the insulator 280 contains a large amount of oxygen, oxygen can be supplied to the oxide semiconductor 230 in contact with the insulator 280, which makes it easier to reduce oxygen vacancies.
[0149] It is more preferable to use a film that releases oxygen by heating as the insulator 280. The insulator 280 releases oxygen due to heat applied during the manufacturing process of the transistor 200, and thus oxygen can be supplied to the oxide semiconductor 230. By supplying oxygen from the insulator 280 to the oxide semiconductor 230, particularly to the channel formation region of the oxide semiconductor 230, oxygen vacancies in the channel formation region of the oxide semiconductor 230 and V O H can be reduced, and a highly reliable transistor can be obtained that exhibits favorable electrical characteristics.
[0150] As an example, the amount of oxygen molecules released from the insulator 280b is 1.0×10 14 molecules / cm 2 That's it, 1.0 x 10 15 molecules / cm 2 The amount of released oxygen molecules can be measured by thermal desorption spectroscopy.
[0151] In particular, when the channel length of the transistor 200 is small, oxygen vacancies in the channel formation region and V O The influence of H on the electrical characteristics and reliability is particularly large. Therefore, by sufficiently reducing the hydrogen concentration in the oxide semiconductor 230 and then optimizing the amount of oxygen supplied to the oxide semiconductor 230, a transistor with a short channel length, favorable electrical characteristics, and high reliability can be realized.
[0152] The insulator 280 is preferably formed by a deposition method such as a sputtering method or a plasma-enhanced chemical vapor deposition (PECVD) method. In particular, the sputtering method does not require the use of hydrogen gas as a deposition gas, and therefore a film with an extremely low hydrogen content can be obtained. Therefore, supply of hydrogen to the oxide semiconductor 230 can be suppressed, and the electrical characteristics of the transistor 200 can be stabilized.
[0153] To increase the amount of oxygen supplied to the oxide semiconductor 230, for example, heat treatment in an oxygen-containing atmosphere or plasma treatment in an oxygen-containing atmosphere may be performed after the insulator 280 is formed. Alternatively, oxygen may be supplied by forming an oxide film on the top surface of the insulator 280 by a sputtering method in an oxygen atmosphere. The oxide film may then be removed. By performing such treatment, oxygen can be supplied to the insulator 280, and the amount of oxygen supplied to the oxide semiconductor 230 can be increased.
[0154] The insulator 280 can also have a structure using the above-described barrier insulator against hydrogen. For example, silicon nitride can be used for the insulator 280. Such a structure can suppress diffusion of hydrogen into the oxide semiconductor 230. Furthermore, the concentrations of impurities such as water and hydrogen in the insulator 280 are preferably reduced. This can suppress entry of impurities such as water and hydrogen into the channel formation region of the oxide semiconductor 230.
[0155] As shown in FIG. 2A, the insulator 280 may have a layered structure of an insulator 280a, an insulator 280b on the insulator 280a, and an insulator 280c on the insulator 280b.
[0156] The insulator 280a has a region in contact with the upper surface of the insulator 222, a region in contact with the side surface of the conductor 220, and a region in contact with the upper surface of the conductor 220. The insulator 280c has a region in contact with the lower surface of the conductor 240.
[0157] The insulator 280b may be any of the insulating materials applicable to the insulator 280. Specifically, silicon oxide or silicon oxynitride may be used for the insulator 280b. The concentrations of impurities such as water and hydrogen in the insulator 280b are preferably reduced.
[0158] When an insulator containing oxygen is used as the insulator 280b, it is preferable to use an oxygen barrier insulator, as described in the section [Insulator] below, for each of the insulators 280a and 280c. By providing the insulator 280a between the insulator 280b and the conductor 220, it is possible to prevent the conductor 220 from being oxidized and the resistance of the conductor 220 from increasing. Furthermore, by providing the insulator 280c between the insulator 280b and the conductor 240, it is possible to prevent the conductor 240 from being oxidized and the resistance of the conductor 240 from increasing.
[0159] The insulator 280a and the insulator 280c may each be a barrier insulator against hydrogen. This allows the insulator 280b to be sandwiched between the barrier insulators against hydrogen. This prevents hydrogen from diffusing from below the insulator 280a or from above the insulator 280c to the insulator 280b. A silicon nitride film and a silicon nitride oxide film each have the characteristics of releasing little impurities (e.g., water and hydrogen) from themselves and being less permeable to oxygen and hydrogen, and therefore can be suitably used for the insulator 280a and the insulator 280c. Note that the insulator 280a and the insulator 280c may be made of the same material or different materials.
[0160] Alternatively, one or both of the insulators 280a and 280c may be an insulator capable of capturing or fixing hydrogen. Such a structure can suppress diffusion of hydrogen from below the insulator 280a or from above the insulator 280c to the insulator 280b, and can further trap or fix hydrogen contained in the insulator 280b. Therefore, the hydrogen concentration in the oxide semiconductor 230 and its vicinity can be reduced. The insulator 280a can be made of magnesium oxide, aluminum oxide, hafnium oxide, or an oxide containing hafnium and silicon. For example, the insulator 280a may be a stacked film of aluminum oxide and silicon nitride on the aluminum oxide. For example, the insulator 280c may be a stacked film of silicon nitride and aluminum oxide on the silicon nitride.
[0161] For example, silicon nitride can be used for the insulators 280a and 280c, and silicon oxide can be used for the insulator 280b. In this case, the insulators 280a and 280c each contain at least silicon and nitrogen. The insulator 280b contains at least silicon and oxygen.
[0162] 2A shows a structure in which the insulator 280c is provided on the planarized insulator 280b, but the present invention is not limited to this. For example, the insulator 280c may be formed without performing planarization treatment on the insulator 280b. Eliminating the planarization treatment can reduce manufacturing costs and increase production yields. Furthermore, the insulators 280a, 280b, and 280c can be successively formed without exposure to the air environment. By forming the insulators 280a to 280c without exposure to the air, impurities or moisture from the air environment can be prevented from adhering to the insulators 280a to 280c, and the vicinity of the interface between the insulators 280a and 280b and the vicinity of the interface between the insulators 280b and 280c can be kept clean.
[0163] Furthermore, the amount of oxygen supplied to the region of the oxide semiconductor 230 in contact with the insulator 280a and the region of the oxide semiconductor 230 in contact with the insulator 280c is smaller than that to the region of the oxide semiconductor 230 in contact with the insulator 280b. Therefore, the resistance of the region of the oxide semiconductor 230 in contact with the insulator 280a and the region of the oxide semiconductor 230 in contact with the insulator 280c may be low. That is, by adjusting the thickness of the insulator 280a, the range of the region that functions as one of the source region and the drain region can be controlled. Similarly, by adjusting the thickness of the insulator 280c, the range of the region that functions as the other of the source region and the drain region can be controlled. Therefore, the thicknesses of the insulators 280a and 280c can be set appropriately according to the characteristics desired for the transistor 200.
[0164] 2A shows the insulator 280 having a three-layer laminated structure, the present invention is not limited to this. The insulator 280 may have a two-layer or four or more layer laminated structure.
[0165] The insulator 270 is provided to cover the conductor 240 and the oxide semiconductor 230. The insulator 270 is preferably formed using a material with a low dielectric constant. Since the insulator 270 functions as an interlayer insulating film, the parasitic capacitance between the conductor 260 and the conductor 240 can be reduced. This can improve the frequency characteristics of the transistor 200. The insulator 270 may be formed using any of the insulating materials that can be used for the insulator 280. Specifically, the insulator 270 can be made of silicon oxide or silicon oxynitride. The concentrations of impurities such as water and hydrogen in the insulator 270 are preferably reduced.
[0166] 1C , the insulator 270 preferably covers the side surface edge of the oxide semiconductor 230, the side surface edge of the conductor 240a, and the side surface edge of the conductor 240b, thereby preventing the conductor 260 from shorting out with the oxide semiconductor 230, the conductor 240a, and the conductor 240b.
[0167] The conductor 240 preferably has a conductor 240a and a conductor 240b on the conductor 240a. The conductor 240a has an opening 290 in the region where it overlaps with the conductor 220. As shown in Figures 1B and 1C, the side of the conductor 240b on the opening 290 side is set back from the side of the conductor 240a on the opening 290 side. In other words, the side of the conductor 240a on the opening 290 side is positioned closer to the opening 290 than the side of the conductor 240b on the opening 290 side.
[0168] It is preferable that the conductor 240a is not provided inside the opening of the insulator 280. In other words, it is preferable that the conductor 240a does not have a region in contact with the side surface of the insulator 280 in the opening 290. With this configuration, the opening of the conductor 240a and the opening of the insulator 280 can be formed at the same time. Furthermore, by configuring the side surface of the conductor 240a in the opening 290 to be flush with the side surface of the insulator 280 in the opening 290, the film thickness distribution of the oxide semiconductor 230 provided inside the opening 290 can be made uniform. Furthermore, it is possible to prevent the oxide semiconductor 230 from being divided by a step between the conductor 240a and the insulator 280.
[0169] 1B and 1C show a configuration in which the side surface of the conductor 240a in the opening 290 and the side surface of the insulator 280 in the opening 290 are flush with each other, but the present invention is not limited to this. For example, the side surface of the conductor 240a in the opening 290 and the side surface of the insulator 280 in the opening 290 may be discontinuous. Furthermore, the inclination of the side surface of the conductor 240a in the opening 290 may be different from the inclination of the side surface of the insulator 280 in the opening 290. In this case, for example, the angle formed between the side surface of the conductor 240a in the opening 290 and the top surface of the insulator 210 is preferably smaller than the angle formed between the side surface of the insulator 280 in the opening 290 and the top surface of the insulator 210. With this configuration, coverage of the oxide semiconductor 230 on the side surface of the conductor 240a in the opening 290 is improved, and defects such as voids can be reduced.
[0170] The conductor 240 preferably has a layered structure. For example, the conductor 240 preferably has a layered structure of a conductor 240a and a conductor 240b that is in contact with the upper surface of the conductor 240a.
[0171] The bottom surface of the conductor 240 a is in contact with the insulator 280 , one side surface and part of the top surface are in contact with the oxide semiconductor 230 , and the other side surface is in contact with the insulator 270 .
[0172] The conductor 240a preferably has ohmic contact with the oxide semiconductor 230 and low contact resistance with the oxide semiconductor 230. For example, the contact resistance between the conductor 240a and the oxide semiconductor 230 is preferably lower than the contact resistance between the metal layer used for the conductor 240b and the oxide semiconductor 230. For this reason, the conductor 240a is preferably made of a metal oxide having conductivity (sometimes referred to as a conductive oxide). Furthermore, as described above, by recessing the side surface of the conductor 240b and providing a structure in which one of the side surfaces and part of the top surface of the conductor 240a are in contact with the oxide semiconductor 230, the contact area between the conductor 240a and the oxide semiconductor 230 can be increased. This can further reduce the contact resistance between the conductor 240a and the oxide semiconductor 230. The above-described structure of the conductor 240a can improve the on-state current, field-effect mobility, S value, and frequency characteristics of the transistor 200.
[0173] The conductive oxide (OC: Oxide Conductor, also referred to as a conductive material containing oxygen) used for the conductor 240a is preferably a conductive oxide containing indium. Examples of conductive oxides containing indium include indium oxide, indium tin oxide (sometimes referred to as ITO), indium zinc oxide, and silicon-added indium tin oxide (also referred to as ITSO). Indium oxide may contain tungsten or titanium, for example, In-W oxide, In-W-Zn oxide, In-Ti oxide, and In-Ti-Sn oxide. A conductive oxide containing zinc may also be used, for example, zinc oxide, zinc oxide doped with gallium, and In-Ga-Zn oxide. Examples of conductive oxides that can be used include ruthenium oxide, oxides containing strontium and ruthenium, and oxides containing lanthanum and nickel. In particular, conductive oxides containing indium are preferred due to their high conductivity.
[0174] For example, indium tin oxide with silicon added may be used for the conductor 240a. In this case, the conductor 240a contains indium, tin, silicon, and oxygen. Here, adding silicon to indium tin oxide can suppress polycrystallization of indium tin oxide. In other words, indium tin oxide with silicon added is likely to have an NC structure (nanocrystal structure) or an amorphous structure. However, the present invention is not limited to the above. Polycrystallized indium tin oxide may also be used for the conductor 240a. In this case, the conductor 240a contains indium, tin, and oxygen.
[0175] One of the side surfaces and the top surface of the conductor 240b are in contact with the oxide semiconductor 230. The bottom surface of the conductor 240b is in contact with the conductor 240a. The other side surface of the conductor 240b is in contact with the insulator 270.
[0176] The conductor 240b is preferably made of a metal having higher conductivity than the conductor 240a. Also, the conductor 240b is preferably made of a metal having lower sheet resistance than the conductor 240a. With this structure, the conductor 240 including the conductor 240b can function as a wiring electrically connected to one of the source electrode and the drain electrode.
[0177] The conductor 240b may be made of one or more of ruthenium, tantalum, nickel, titanium, molybdenum, tungsten, hafnium, vanadium, niobium, aluminum, chromium, copper, silver, gold, platinum, zinc, manganese, iron, cobalt, magnesium, zirconium, beryllium, indium, iridium, strontium, and lanthanum, or an alloy containing one or more of the aforementioned metals as a component, etc. For example, it is preferable to use tungsten as the conductor 240b.
[0178] In some cases, a part of the conductor 240b contains a metal oxide of the above metal. In this case, a layer of the metal oxide may be formed near the interface of the conductor 240b with the conductor 240a and near the interface with the oxide semiconductor 230. Here, ruthenium and ruthenium alloys are preferable because they are materials that maintain relatively low electrical resistance even when oxidized.
[0179] In the above, an example has been described in which the conductor 240 has a two-layer laminated structure of the conductor 240a and the conductor 240b, but the present invention is not limited to this. The conductor 240 may have a laminated structure of three or more layers. Also, in the above, a configuration in which the conductor 240b is laminated on the conductor 240a has been shown, but the present invention is not limited to this. A configuration in which the conductor 240a is laminated on the conductor 240b may also be used.
[0180] The conductor 220 is provided on the insulator 222, and can be formed in an island shape as shown in Figures 1B and 1C. When the conductor 220 is formed in an island shape, a conductor that functions as a via can be formed below the conductor 220 and can be connected to a wiring layer provided below the insulator 210. The conductor 220 can also be extended in the X direction or Y direction to function as wiring.
[0181] The conductor 220 may be a single layer or a multilayer of the conductors described in the section below under "Conductor." It is preferable to use a conductive material that is resistant to oxidation or a conductive material that has the function of suppressing oxygen diffusion as the conductor 220. For example, titanium nitride or tantalum nitride may be used.
[0182] 1B and 1C, the conductor 220 preferably has a layered structure of a conductor 220a and a conductor 220b on the conductor 220a. Here, the conductor 220a is preferably made of a metal with high conductivity. Therefore, the conductor 220a may be made of, for example, a metal that can be used for the conductor 240b. For example, tungsten may be used for the conductor 220a. With this structure, the conductor 220 including the conductor 220a can function as a wiring electrically connected to the other of the source electrode and the drain electrode.
[0183] Furthermore, as shown in FIG. 2A , a configuration may be adopted in which a conductor 220c is provided below the conductor 220a. The conductor 220c is preferably made of the aforementioned conductive material that is resistant to oxidation or a conductive material that has the function of suppressing oxygen diffusion. For example, titanium nitride or tantalum nitride may be used. By providing such a conductor 220c, oxidation of the conductor 220b can be prevented, and a decrease in the conductivity of the conductor 220b can be prevented.
[0184] The conductor 220b in contact with the oxide semiconductor 230 is preferably made of a conductive oxide. Therefore, for example, a conductive oxide that can be used for the conductor 240a may be used for the conductor 220b. For example, indium tin oxide to which silicon is added may be used for the conductor 220b. In this case, the conductor 220b contains indium, tin, silicon, and oxygen. This allows the conductor 220b to form ohmic contact with the oxide semiconductor 230, thereby reducing the contact resistance between the conductor 220b and the oxide semiconductor 230. Therefore, the on-state current, field-effect mobility, and frequency characteristics of the transistor 200 can be improved.
[0185] 1B, 1C, 2A, and 2B, a recess connected to the opening 290 is preferably formed on the upper surface of the conductor 220b. By configuring the oxide semiconductor 230 to be in contact with the side surface of the recess, the area of ohmic contact between the conductor 220b and the oxide semiconductor 230 can be increased, and the contact resistance between the conductor 220b and the oxide semiconductor 230 can be further reduced. Furthermore, by forming the recess in the conductor 220b, the conductor 220a can be prevented from contacting the oxide semiconductor 230 and being excessively oxidized.
[0186] Although FIG. 1B and other figures show a configuration in which the recess connected to the opening 290 reaches the conductor 220b, the present invention is not limited to this. For example, as shown in FIG. 3A , a configuration in which the opening 290 reaches the conductor 220a is also possible. With such a configuration, the position of the bottom surface of the conductor 260 can be lowered, making it easier to apply the electric field of the conductor 260 to the oxide semiconductor 230 near the conductor 220. Here, since at least a portion of the bottom surface of the oxide semiconductor 230 is removed, the area in contact between the oxide semiconductor 230 and the top surface of the conductor 220a can be reduced. This can prevent the conductor 220a from being excessively oxidized.
[0187] 3B , a configuration may be adopted in which the conductor 220b is provided inside the conductor 220a. For example, an opening may be formed in the conductor 220a, the conductor 220b may be formed in the opening, and an opening 290 may be formed to overlap the conductor 220b. Here, as shown in FIG. 3B , the opening 290 reaches the insulator 222, and the oxide semiconductor 230 and the insulator 250 are in contact with the insulator 222. With this configuration, the inner side surface of the conductor 220b is in contact with the side surface of the oxide semiconductor 230, and therefore, the conductor 220 and the oxide semiconductor 230 can be in ohmic contact. Furthermore, contact between the oxide semiconductor 230 and the conductor 220a can be prevented, thereby suppressing oxidation of the conductor 220a.
[0188] 3C , the conductor 220a may be embedded in the insulator 285, and the conductor 220b may be provided in contact with the upper surface of the conductor 220a. The insulator 285 may be made of an insulating material that can be used for the insulator 270. An opening 290 is formed to overlap the conductor 220b. The opening 290 is preferably positioned so as not to overlap the conductor 220a. In this case, as shown in FIG. 3C , the opening 290 reaches the insulator 285, and the oxide semiconductor 230 and the insulator 250 are in contact with the insulator 285. With this structure, the inner side surface of the conductor 220b contacts the side surface of the oxide semiconductor 230, allowing the conductor 220 and the oxide semiconductor 230 to form ohmic contact. Furthermore, contact between the oxide semiconductor 230 and the conductor 220a can be prevented, thereby suppressing oxidation of the conductor 220a.
[0189] 2A and other drawings, the insulator 250 is provided in contact with the upper surfaces of the insulator 270, the oxide semiconductor 230, and the conductor 220. Alternatively, as shown in FIG. 2B , the heights of the upper end of the insulator 250 and the upper surface of the insulator 270 may be the same or approximately the same, and the insulator 250 may not be provided on the insulator 270.
[0190] 2A , the insulator 250 may have a stacked structure of an insulator 250a, an insulator 250b over the insulator 250a, and an insulator 250c over the insulator 250b. The insulator 250a is in contact with the conductor 220, the oxide semiconductor 230, and the insulator 270. The insulator 250c is in contact with the conductor 260 and the insulator 283. The insulator 250b is provided between the insulator 250a and the insulator 250c.
[0191] The insulators 250a and 250c are preferably made of an insulator having a barrier property against oxygen. Furthermore, the insulators 250a and 250c are preferably made of an insulator having a function of capturing or fixing hydrogen. An insulating material that can be used for the insulator 222 may be used for the insulators 250a and 250c. By providing such insulators 250a and 250c, oxidation of the conductor 220 in contact with the insulator 250a and the conductor 260 in contact with the insulator 250c can be suppressed. Furthermore, the insulators 250a and 250c can more effectively capture or fix hydrogen contained in the oxide semiconductor 230 and its vicinity. Therefore, the hydrogen concentration in the oxide semiconductor 230 can be reduced. For example, aluminum oxide can be used as the insulator 250a, and hafnium oxide can be used as the insulator 250c. As the insulator 250a and the insulator 250c, the insulators described in the section [Insulator] below may be used in a single layer or a stacked layer.
[0192] Furthermore, aluminum oxide and hafnium oxide are high-dielectric-constant (high-k) materials. Therefore, when the insulators 250a and 250c are used as gate insulators, it is possible to reduce the gate potential applied during transistor operation while maintaining the physical thickness of the gate insulator. Furthermore, it is possible to reduce the equivalent oxide thickness (EOT) of the insulator functioning as the gate insulator.
[0193] The thickness of the insulator 250a and the insulator 250c is preferably 0.5 nm to 15 nm, more preferably 0.5 nm to 12 nm, and even more preferably 0.5 nm to 10 nm. At least a portion of the insulator 250a and the insulator 250c may have a region with the above thickness.
[0194] The insulator 250b is preferably made of silicon oxide or silicon oxynitride, which have a high withstand voltage. To improve the withstand voltage, the insulator 250b may be thicker than the insulators 250a and 250c. By providing such an insulator 250b, the withstand voltage of the insulator 250 can be improved and leakage current can be reduced.
[0195] Furthermore, an insulator having a barrier property against hydrogen may be provided between the insulator 250c and the conductor 260. This can suppress diffusion of impurities such as hydrogen contained in the conductor 260 into the oxide semiconductor 230. As the insulator having a barrier property against hydrogen, an insulator that can be used for the insulator 210 and the insulator 283 can be used. For example, silicon nitride is preferable because it has a high barrier property against hydrogen. When the insulator has a barrier property against hydrogen, the insulator also has a barrier property against oxygen.
[0196] The conductor 260 is provided in contact with the upper surface of the insulator 250. Also, as shown in Figures 1A to 1C, the portion of the conductor 260 above the insulator 270 can be extended in the Y direction to function as a wiring.
[0197] A single layer or a stack of conductors described in the section [Conductor] below can be used as the conductor 260. For example, a conductive material with high conductivity, such as tungsten, can be used as the conductor 260.
[0198] Furthermore, it is preferable to use a conductive material that is resistant to oxidation or a conductive material that has the function of suppressing oxygen diffusion as the conductor 260. Examples of such conductive materials include conductive materials containing nitrogen (e.g., titanium nitride or tantalum nitride) and conductive materials containing oxygen (e.g., ruthenium oxide). This can suppress a decrease in the conductivity of the conductor 260.
[0199] Although the conductor 260 is shown as a single layer in FIGS. 1B and 1C, the present invention is not limited to this. The conductor 260 may have a laminated structure. For example, as shown in FIG. 2A, the conductor 260 may have a laminated structure of a conductor 260a and a conductor 260b on the conductor 260a. In this case, for example, titanium nitride may be used as the conductor 260a, and tungsten may be used as the conductor 260b. By providing a layer containing tungsten in this manner, the conductivity of the conductor 260 can be improved, allowing it to function sufficiently as wiring.
[0200] 2A shows a configuration in which the conductor 260 has a two-layer structure of the conductor 260a and the conductor 260b, but the present invention is not limited to this. The conductor 260 may have a three or more layer structure.
[0201] For example, as shown in FIG. 2B , the conductors 260a and 260b may be provided only below the upper surface of the insulator 270, and a conductor 260c functioning as wiring may be provided on top of the conductors 260a and 260b. Here, the height of the upper end of the conductor 260a and the upper surface of the conductor 260b coincides with or approximately coincides with the height of the upper surface of the insulator 270. Since the conductor 260c functions as wiring, it may be formed by extending in, for example, the Y direction. The conductor 260c may be made of a conductive material that can be used as the conductor 260a or the conductor 260b. For example, the conductor 260c may have a layered structure of titanium nitride and tungsten.
[0202] A barrier insulator against hydrogen is preferably used for the insulator 283. This can prevent hydrogen from diffusing from above the insulator 283 to the oxide semiconductor 230. A silicon nitride film and a silicon nitride oxide film are suitable for use as the insulator 283 because they each release little impurities (for example, water and hydrogen) and are impermeable to oxygen and hydrogen.
[0203] It is particularly preferable to use silicon nitride deposited by a sputtering method as the insulator 283. In this case, the insulator 283 contains silicon and nitrogen. The sputtering method does not require the use of molecules containing hydrogen in the deposition gas, and therefore the hydrogen concentration in the insulator 283 can be reduced. Furthermore, by depositing the insulator 283 by a sputtering method, silicon nitride with high density can be formed.
[0204] Alternatively, a silicon nitride film formed by a PEALD method may be used as the insulator 283. By forming the insulator 283 by a PEALD method, the conductor 260 can be covered with good coverage.
[0205] Such a structure can suppress diffusion of hydrogen from above the insulator 283 to the oxide semiconductor 230. Thus, the hydrogen concentration in the oxide semiconductor 230 can be reduced.
[0206] <Example of Manufacturing Method of Semiconductor Device> Next, a manufacturing method of the transistor 200 shown in FIGS. 1A to 1D will be described with reference to FIGS. 4A to 5F. Note that FIGS. 4A to 4C and 4E to 5F correspond to FIG. 1B. Also, FIG. 4D corresponds to FIG. 1C.
[0207] In the following, an insulating material for forming an insulator, a conductive material for forming a conductor, or a semiconductor material for forming a semiconductor can be formed as a film by appropriately using a sputtering method, a chemical vapor deposition (CVD) method, a molecular beam epitaxy (MBE) method, a pulsed laser deposition (PLD) method, an ALD method, or the like.
[0208] Sputtering methods include RF sputtering, which uses a high-frequency power supply as the sputtering power source, DC sputtering, which uses a direct current power supply, and pulsed DC sputtering, which changes the voltage applied to the electrode in a pulsed manner. RF sputtering is mainly used to deposit insulating films, while DC sputtering is mainly used to deposit metal conductive films. Pulsed DC sputtering is mainly used to deposit films of compounds such as oxides, nitrides, and carbides using reactive sputtering.
[0209] CVD methods can be classified into plasma-enhanced CVD (PECVD) methods that utilize plasma, thermal CVD (TCVD) methods that utilize heat, and photo-CVD (photo-CVD) methods that utilize light. CVD methods can also be further classified into metal CVD (MCVD) methods and metal organic CVD (MOCVD) methods depending on the source gas used.
[0210] The plasma CVD method can produce high-quality films at relatively low temperatures. Furthermore, the thermal CVD method is a film formation method that can minimize plasma damage to the workpiece because it does not use plasma. For example, wiring, electrodes, elements (transistors, capacitors, etc.) included in a semiconductor device may become charged up by receiving electric charge from the plasma. In this case, the accumulated electric charge may destroy the wiring, electrodes, elements, etc. included in the semiconductor device. On the other hand, the thermal CVD method, which does not use plasma, does not cause such plasma damage, and therefore can increase the yield of semiconductor devices. Furthermore, the thermal CVD method does not cause plasma damage during film formation, so films with fewer defects can be obtained.
[0211] As the ALD method, a thermal ALD method in which a precursor and a reactant are reacted using only thermal energy, a PEALD method in which a plasma-excited reactant is used, or the like can be used.
[0212] The CVD and ALD methods differ from sputtering, in which particles emitted from a target or the like are deposited. Therefore, they are film formation methods that are less affected by the shape of the workpiece and have good step coverage. In particular, the ALD method has excellent step coverage and excellent thickness uniformity, making it suitable for coating the surfaces of openings with high aspect ratios. However, because the ALD method has a relatively slow film formation rate, it may be preferable to use it in combination with other film formation methods, such as the CVD method, which has a faster film formation rate.
[0213] Furthermore, the CVD method allows deposition of a film with any composition by adjusting the flow rate ratio of the source gases. For example, the CVD method allows deposition of a film with a continuously changing composition by changing the flow rate ratio of the source gases during deposition. When deposition is performed while changing the flow rate ratio of the source gases, the time required for deposition can be shortened compared to deposition using multiple deposition chambers because no time is required for transport or pressure adjustment. Therefore, the productivity of semiconductor devices can be improved in some cases.
[0214] Furthermore, in the ALD method, a film of any composition can be formed by introducing multiple different precursors. For example, when multiple different precursors are introduced, a film of any composition can be formed by controlling the number of cycles of each precursor.
[0215] In addition, when introducing a plurality of different precursors in the ALD method, the type of oxidizing agent may be changed depending on each precursor. For example, when introducing at least a first precursor and a second precursor, ozone (O 3 ) is used as the second precursor, and oxygen (O 2 ) may also be used.
[0216] Before forming the film, a heat treatment may be performed. The heat treatment may be performed under reduced pressure, and the film may be formed continuously without exposure to the atmosphere. By performing such a treatment, moisture and hydrogen adsorbed on the surface on which the film is to be formed can be removed, and the moisture concentration and hydrogen concentration in the structure on which the film is to be formed can be further reduced. The temperature of the heat treatment is preferably 100° C. or higher and 600° C. or lower.
[0217] First, a substrate (not shown) is prepared, and an insulator 210 is formed on the substrate (see FIG. 4A ). The insulator 210 can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like, as appropriate. For example, a silicon nitride film can be formed as the insulator 210 by a sputtering method.
[0218] Next, the insulator 222 is deposited on the insulator 210 (see FIG. 4A ). The insulator 222 can be deposited by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like, as appropriate. For example, hafnium silicate can be deposited as the insulator 222 by a sputtering method. In this case, a deposition target containing hafnium and silicon can be used. For example, a co-sputtering method using a silicon oxide target and a hafnium oxide target can be used.
[0219] Next, the conductor 220a and the conductor 220b are formed on the insulator 222 (see FIG. 4A ). The conductor 220a and the conductor 220b can be formed by depositing a conductive film on the insulator 222 and patterning the conductive film by lithography. The conductive film can be deposited by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like, as appropriate. For example, a tungsten film can be deposited by sputtering as the conductive film to be the conductor 220a, and an ITSO film can be deposited by sputtering as the conductive film to be the conductor 220b.
[0220] Next, the insulator 280 is formed over the insulator 222 and the conductor 220 (see FIG. 4A ). The insulator 280 may be formed using any of the insulating materials described above as appropriate. The insulator 280 may be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like as appropriate. For example, the insulator 280 may have a structure including insulators 280a, 280b, and 280c as shown in FIG. 2A . In this case, silicon nitride may be formed as the insulator 280a by a PEALD method, silicon oxide may be formed as the insulator 280b by a sputtering method, and silicon nitride may be formed as the insulator 280c by a sputtering method. Note that the insulator 280 is preferably subjected to CMP treatment after deposition to planarize its top surface. By performing planarization treatment on the insulator 280, the conductor 240 that functions as a wiring can be suitably formed.
[0221] In some cases, the CMP process may not be necessary. In this case, the upper surface of the insulator 280 has an upwardly convex curved shape. By not performing the planarization process, the manufacturing cost can be reduced and the production yield can be increased.
[0222] Note that planarization treatment is not necessarily performed after the insulators 280a to 280c are formed. For example, after the insulators 280a and 280b are formed, planarization treatment may be performed and then the insulator 280c may be formed.
[0223] Furthermore, when the insulator 280 is formed by a sputtering method that does not require the use of hydrogen-containing molecules in a deposition gas, the hydrogen concentration in the insulator 280 can be reduced. By forming the insulator 280 in this manner, hydrogen diffusing from the insulator 280 to the oxide semiconductor 230 can be reduced, and oxygen vacancies and VoH in the channel formation region can be reduced.
[0224] Next, a conductive film 240A is formed over the insulator 280, and a conductive film 240B is formed over the conductive film 240A (see FIG. 4A ). The conductive film 240A becomes the conductor 240a in a later step, and the conductive film 240B becomes the conductor 240b in a later step. The conductive films 240A and 240B may be formed using any of the above-described conductive materials as appropriate. The conductive films 240A and 240B may be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like as appropriate. For example, ITSO can be formed as the conductive film 240A by sputtering. Tungsten can be formed as the conductive film 240B by sputtering.
[0225] Next, part of the conductive film 240A, part of the conductive film 240B, and part of the insulator 280 are processed to form an opening 290 that reaches the conductor 220 (see FIG. 4B). The opening 290 may be formed by lithography.
[0226] In lithography, a resist is first exposed through a mask. The exposed area is then removed or left behind using a developer to form a resist mask. Next, an etching process is performed through the resist mask, allowing a conductor, semiconductor, or insulator to be processed into a desired shape. For example, a resist mask can be formed by exposing the resist using KrF excimer laser light, ArF excimer laser light, or EUV (Extreme Ultraviolet) light. An immersion technique may also be used, in which a liquid (e.g., water) is filled between the substrate and the projection lens for exposure. Alternatively, an electron beam or an ion beam may be used instead of the light described above. When an electron beam or an ion beam is used, a mask may not be required.
[0227] The resist mask that is no longer needed after processing can be removed by performing a dry etching treatment such as ashing using oxygen plasma (hereinafter, sometimes referred to as oxygen plasma treatment), a wet etching treatment, a dry etching treatment followed by a wet etching treatment, or a wet etching treatment followed by a dry etching treatment.
[0228] Alternatively, a configuration may be adopted in which an SOC (spin on carbon) film and an SOG (spin on glass) film are formed between the workpiece and the resist mask. Using the SOC film and the SOG film as masks can improve the durability of the mask pattern. For example, a lithography method can be performed by forming an SOC film, an SOG film, and a resist mask in this order on the workpiece. Alternatively, a configuration may be adopted in which a hard mask made of an insulator or a conductor is provided between the workpiece and the SOC film.
[0229] For example, an SOC film, an SOG film, and a resist mask may be formed in this order on the conductive film 240B, and the resist mask may be patterned into the shape of the opening 290.
[0230] The opening 290 can be formed by dry etching or wet etching. Dry etching is suitable for forming the opening 290 with a high aspect ratio because it allows anisotropic etching. However, the opening 290 can also be formed by appropriately using dry etching and wet etching.
[0231] Here, as the etching gas for the dry etching process, an etching gas containing halogen can be used, and specifically, an etching gas containing one or more of fluorine, chlorine, and bromine can be used. For example, as the etching gas, C 4 F 6 Gas, C 5 F 6 Gas, C 4 F 8 Gas, CF 4 Gas, SF 6 Gas, CHF 3 Gas, CH 2 F 2 Gas, CH 3 F gas, Cl 2 Gas, BCl 3 Gas, SiCl 4 Gas, CCl 4 gas, HBr gas, or BBr 3Gases such as fluorine-containing gases can be used alone or in combination of two or more gases. Oxygen gas, carbon dioxide gas, nitrogen gas, helium gas, argon gas, hydrogen gas, or hydrocarbon gas can be added to the above-mentioned etching gas as appropriate. Depending on the object to be dry-etched, gases containing hydrocarbon gas or hydrogen gas but not containing halogen gas can be used as the etching gas. Examples of hydrocarbons used in the etching gas include methane (CH 4 ), ethane (C 2 H 6 ), propane (C 3 H 8 ), butane (C 4 H 10 ), ethylene (C 2 H 4 ), propylene (C 3 H 6 ), acetylene (C 2 H 2 ), and propyne (C 3 H 4 The etching conditions can be appropriately set depending on the target to be etched.
[0232] Furthermore, a capacitively coupled plasma (CCP) etching apparatus having parallel-plate electrodes can be used as the dry etching apparatus. A capacitively coupled plasma etching apparatus having parallel-plate electrodes can be configured to apply a high-frequency voltage to one of the parallel-plate electrodes. Alternatively, a high-frequency voltage of the same frequency can be applied to each of the parallel-plate electrodes. Alternatively, a plurality of different high-frequency voltages can be applied to the parallel-plate electrodes. Such a CCP etching apparatus is called a dual-frequency capacitively coupled plasma (DF-CCP) etching apparatus. In a DF-CCP etching apparatus, a high-frequency voltage of a different frequency can be applied to each of the parallel-plate electrodes. Alternatively, a plurality of different high-frequency voltages can be applied to one of the parallel-plate electrodes. Alternatively, a dry etching apparatus having a high-density plasma source can be used. The dry etching apparatus having a high-density plasma source can be, for example, an inductively coupled plasma (ICP) etching apparatus. The etching apparatus can be appropriately configured according to the object to be etched. In the above-mentioned dry etching apparatus, reactive ion etching can be performed by applying a high-frequency voltage to the electrode on the substrate side to generate a self-bias potential. In reactive ion etching, etching is performed by accelerating ion species in the plasma and causing them to collide with the workpiece, thereby enabling highly anisotropic etching.
[0233] It is preferable that the following process of forming the opening 290 be performed continuously without exposure to the outside air. For example, a multi-chamber etching apparatus may be used to perform the process without exposure to the outside air.
[0234] The above etching gas and etching apparatus can be appropriately selected according to the configuration of the SOG film, the SOC film, the conductive film 240B, the conductive film 240A, and the insulator 280. For example, when a tungsten film is used for the conductive film 240B, Cl 2and CF 4 For example, when an ITSO film is used as the conductive film 240A, CH 4 For example, when a stacked film of silicon oxide and silicon nitride is used for the insulator 280, C 4 F 8 and C 4 F 6 The treatment can be carried out in a DF-CCP etching apparatus using oxygen gas and argon gas as etching gases.
[0235] It is preferable that the SOC film remains on the conductive film 240B at the stage where the opening 290 is formed. By performing wet etching in this state, the conductive film 240B can be side-etched. As an etchant for the wet etching, it is preferable to use, for example, an ammonia hydrogen peroxide mixture (a mixture of ammonia, water, and hydrogen peroxide solution). This allows the side surface of the conductive film 240B to be recessed from the side surface of the conductive film 240A.
[0236] Furthermore, it is preferable to perform a cleaning process to remove impurities and the like that have adhered to the opening 290 during the etching process. As a cleaning method, wet cleaning (which can also be called a wet etching process) using a cleaning solution or the like can be performed. Furthermore, the wet cleaning etches the upper surface of the conductor 220, and a recess that connects to the opening 290 is formed on the upper surface of the conductor 220.
[0237] Wet cleaning may be performed using an aqueous solution in which one or more of oxalic acid, phosphoric acid, and hydrofluoric acid are diluted with carbonated water or pure water. Wet cleaning may also be performed using an aqueous solution in which ammonia water is diluted with carbonated water or pure water. Wet cleaning may also be performed using pure water or carbonated water. Ultrasonic cleaning may also be performed using these aqueous solutions, pure water, or carbonated water. These cleaning methods may also be combined appropriately. The above cleaning process may also be performed multiple times, and the cleaning solution may be changed for each cleaning process. For example, wet cleaning may be performed using diluted hydrofluoric acid, which is obtained by diluting hydrofluoric acid with pure water.
[0238] Furthermore, the recesses on the upper surface of the conductor 220 do not necessarily have to be formed by the above-described wet cleaning. For example, the recesses on the upper surface of the conductor 220 may be formed using a dry etching method following the dry etching process of the insulator 280.
[0239] After the opening 290 is formed, a microwave treatment may be performed in an oxygen-containing atmosphere to reduce the impurity concentration in the insulator 280. Here, the microwave treatment refers to a treatment using, for example, an apparatus having a power source that generates high-density plasma using microwaves. In this specification and the like, microwaves refer to electromagnetic waves having a frequency of 300 MHz or more and 300 GHz or less. Impurities include, in particular, hydrogen and carbon. By performing the microwave treatment in an oxygen-containing atmosphere, the hydrogen contained in the insulator 280 is converted to H 2 The hydrogen can be released to the outside as O. By releasing hydrogen from the insulator 280 located in the vicinity of the oxide semiconductor 230, a highly reliable semiconductor device can be provided.
[0240] Subsequently, heat treatment may be performed. Note that the heat treatment may be performed consecutively after the microwave treatment without exposure to the air. The heat treatment may be performed at a temperature of 250° C. to 650° C., preferably 300° C. to 500° C., more preferably 320° C. to 450° C. The heat treatment may be performed in a nitrogen gas or inert gas atmosphere, or an atmosphere containing an oxidizing gas at 10 ppm or more, 1% or more, or 10% or more. For example, when the heat treatment is performed in a mixed atmosphere of nitrogen gas and oxygen gas, the oxygen gas concentration can be approximately 20%. The heat treatment may be performed under reduced pressure. Alternatively, the heat treatment may be performed in an atmosphere containing an oxidizing gas at 10 ppm or more, 1% or more, or 10% or more after the heat treatment in the nitrogen gas or inert gas atmosphere. By performing the above heat treatment, impurities such as water contained in the insulator 280 can be reduced before the formation of an oxide semiconductor film that becomes the oxide semiconductor 230 described later. Note that the heat treatment is preferably performed under conditions that do not cause the conductors 220 and 240 to be excessively oxidized.
[0241] Furthermore, it is preferable that the gas used in the heat treatment be highly purified. For example, the amount of moisture contained in the gas used in the heat treatment can be 1 ppb or less, preferably 0.1 ppb or less, and more preferably 0.05 ppb or less. By performing the heat treatment using a highly purified gas, it is possible to prevent moisture and the like from being absorbed into the insulator 280, etc., as much as possible.
[0242] Although the above description has been given of a configuration in which the heat treatment is performed after the microwave treatment, the present invention is not limited to this. It is also possible to perform the microwave treatment after the heat treatment.
[0243] Next, an oxide semiconductor film to be the oxide semiconductor 230 is formed in contact with the top surface of the conductor 220, the side surface of the insulator 280, the side surface of the conductive film 240A, part of the top surface of the conductive film 240A, and the top surface and side surface of the conductive film 240B. The oxide semiconductor film may be formed using any of the above-described metal oxides applicable to the oxide semiconductor 230 as appropriate. The oxide semiconductor film can be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like as appropriate.
[0244] For example, similar to FIG. 2A , a stacked film of oxide semiconductors can be formed to have a stacked structure of oxide semiconductors 230a and 230b. In this case, the oxide semiconductor film that becomes the oxide semiconductor 230a can be formed by sputtering, and the oxide semiconductor film that becomes the oxide semiconductor 230b can be formed thereon by ALD. The oxide semiconductor film that becomes the oxide semiconductor 230a can be formed using a target having an atomic ratio of In:Ga:Zn=1:1:1.2 or a composition similar thereto. The oxide semiconductor film that becomes the oxide semiconductor 230b can be formed to have an atomic ratio of In:Ga:Zn=1:1:1 or a composition similar thereto.
[0245] Note that the microwave treatment and the heat treatment may be performed after the oxide semiconductor film is formed.
[0246] Next, the oxide semiconductor film to be the oxide semiconductor 230, the conductive film 240A, and the conductive film 240B are processed by lithography to form the oxide semiconductor 230, the conductor 240a, and the conductor 240b (see FIGS. 4C and 4D ). The oxide semiconductor film to be the oxide semiconductor 230, the conductive film 240A, and the conductive film 240B can be processed by dry etching or wet etching. Dry etching is suitable for microfabrication.
[0247] As a result, the conductors 240a and 240b are formed to extend in the X direction and can function as wiring. The oxide semiconductor 230 is also formed to extend in the X direction, similar to the conductors 240a and 240b. However, a portion of the oxide semiconductor 230 is formed within the opening 290. Here, as shown in FIG. 4D , the side surfaces of the oxide semiconductor 230, the conductor 240a, and the conductor 240b are preferably formed to be flush with each other.
[0248] Although the oxide semiconductor 230, the conductor 240a, and the conductor 240b are formed simultaneously in the above description, the present invention is not limited to this. For example, the conductive films 240A and 240B may be processed after the oxide semiconductor 230 is formed. In this case, the side surface of the oxide semiconductor 230 is located inside the side surfaces of the conductor 240a and the conductor 240b.
[0249] Next, the oxide semiconductor 230 is processed by lithography to remove a portion of the oxide semiconductor 230 at the bottom of the opening 290 (see FIG. 4E ). As a result, a portion of the upper surface of the conductor 220b is exposed from the oxide semiconductor 230. In addition, in a cross-sectional view, the lower portion of the oxide semiconductor 230 protrudes into the opening 290. Note that the oxide semiconductor 230 can be processed by dry etching or wet etching. Dry etching is suitable for microfabrication.
[0250] Here, the oxide semiconductor 230 is preferably formed in contact with the recess of the conductor 220 at the opening 290, the side surface of the insulator 280 at the opening 290, the side surface of the conductor 240a, part of the top surface of the conductor 240a, and the top surface and side surface of the conductor 240b. When the oxide semiconductor 230 is formed in contact with the side surface of the recess of the conductor 220, the conductor 220 functions as one of the source electrode and drain electrode of the transistor 200. When the oxide semiconductor 230 is formed in contact with the conductor 240a, the conductor 240a and the conductor 240b function as the other of the source electrode and drain electrode of the transistor 200.
[0251] Next, a coating film 287A is formed so as to fill the opening 290 (see FIG. 4F). The coating film 287A can be formed by first coating an SOC film and then coating an SOG film on top of that. The coating film 287A functions as a sacrificial layer when forming the insulator 270.
[0252] Next, the coating film 287A is processed using lithography to form a sacrificial layer 287 that protrudes above the opening 290 (see FIG. 5A ). The sacrificial layer 287 can be patterned to match the shape of the opening in the insulator 270 to be formed later. The coating film 287A can be processed using dry etching or wet etching. Dry etching is suitable for microfabrication. By forming the sacrificial layer 287 in a structure in which an SOG film is stacked on an SOC film, the shape of the sacrificial layer 287 can be prevented from being distorted during the above processing.
[0253] Next, the insulating film 270A serving as the insulator 270 is formed to cover the sacrificial layer 287 and the oxide semiconductor 230 (see FIG. 5B ). The insulating film 270A may be formed using any of the above-described insulating materials as appropriate. The insulating film 270A may be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like as appropriate. For example, the insulating film 270A may be formed using silicon oxide by a sputtering method. The hydrogen concentration in the insulating film 270A can be reduced by using a sputtering method that does not require the use of hydrogen-containing molecules in the deposition gas. By forming the insulating film 270A in this manner, hydrogen diffusing from the insulating film 270A to the oxide semiconductor 230 can be reduced, thereby reducing oxygen vacancies and VoH in the channel formation region.
[0254] Alternatively, the insulating film 270A may be a laminated film of an aluminum oxide film formed by ALD and a silicon oxide film on the aluminum oxide film. In this case, the upper part of the sacrificial layer 287 is covered with the aluminum oxide film. By forming a silicon oxide film by sputtering while the sacrificial layer 287 is covered with the aluminum oxide film in this manner, it is possible to prevent the shape of the sacrificial layer 287 from being distorted during the formation of the silicon oxide film.
[0255] Next, the insulating film 270A is subjected to CMP processing until the sacrificial layer 287 is exposed, thereby forming the insulator 270 (see FIG. 5C). At this time, the SOG film on the sacrificial layer 287 is also removed, so that the SOC film of the sacrificial layer 287 is exposed.
[0256] Next, the sacrificial layer 287 is removed to form an opening in the insulator 270 that overlaps with the opening 290 (see FIG. 5D ). The sacrificial layer 287 can be removed by performing a dry etching process such as ashing, a wet etching process, a dry etching process followed by a wet etching process, or a wet etching process followed by a dry etching process.
[0257] Next, the insulator 250 is formed over the insulator 270, the oxide semiconductor 230, and the conductor 220 (see FIG. 5E ). The insulator 250 may be formed using any of the above-described insulating materials as appropriate. The insulator 250 may be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like as appropriate. The insulator 250 is preferably formed in contact with the oxide semiconductor 230 in the opening 290. Therefore, the insulator 250 is preferably formed by a film formation method with good coverage, more preferably a CVD method, an ALD method, or the like. For example, as shown in FIG. 2A , the insulator 250 can have a stacked structure of insulators 250a, 250b, and 250c. For example, aluminum oxide can be deposited as insulator 250a using a thermal ALD method, silicon oxide can be deposited as insulator 250b using a PEALD method, and hafnium oxide can be deposited as insulator 250c using a thermal ALD method.
[0258] The microwave treatment and heat treatment described above may be performed after the formation of the insulator 250. Furthermore, when the insulator 250 has a layered structure, the microwave treatment does not necessarily need to be performed after the formation of all of the insulators contained in the insulator 250. For example, in the structure shown in FIG. 2A , the microwave treatment may be performed after the formation of the insulator 250b, and then the insulator 250c may be formed. Furthermore, for example, the microwave treatment may be performed after the formation of the insulator 250b, and then the microwave treatment may be performed after the formation of the insulator 250c. In this way, the microwave treatment in an oxygen-containing atmosphere may be performed multiple times.
[0259] Next, a conductive film 260A to be the conductor 260 is formed so as to fill the recessed portion of the insulator 250. The conductive film 260A may be formed using any of the above-described conductive materials as appropriate. The conductive film 260A may be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like as appropriate. Here, the conductive film 260A is preferably formed in contact with the insulator 250 provided in the opening 290. Therefore, the conductive film is preferably formed by a film formation method with good coverage or filling properties, and more preferably by a CVD method, an ALD method, or the like. For example, the conductive film 260A may be formed by depositing titanium nitride by a CVD method or an ALD method, and then depositing tungsten on the titanium nitride by a CVD method.
[0260] In the above description, the conductive film 260A is provided so as to fill the opening 290, but the present invention is not limited to this. For example, a recess that reflects the shape of the opening 290 may be formed in the center of the conductive film. Alternatively, the recess may be filled with an inorganic insulating material or the like.
[0261] Next, the conductive film that will become the conductive film 260A is processed to form the conductor 260 (see FIG. 5F). The conductor 260 may be formed by lithography. The above processing can be performed by dry etching or wet etching. Processing by dry etching is suitable for fine processing.
[0262] Alternatively, CMP treatment can be performed on the conductive film 260A and the insulator 250 to remove the portions of the conductive film 260A and the insulator 250 above the insulator 270. In this case, the remaining portions of the conductive film 260A correspond to the conductors 260a and 260b shown in FIG. 2B , and the remaining portion of the insulator 250 corresponds to the insulator 250 shown in FIG. 2B . Then, a conductor 260c that functions as a wiring can be formed on the conductors 260a and 260b.
[0263] Next, the insulator 283 is formed to cover the conductor 260 and the insulator 250. The insulator 283 may be formed using any of the insulating materials described above as appropriate. The insulator 283 may be formed by a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like as appropriate. For example, a silicon nitride film may be formed as the insulator 283 by a PEALD method.
[0264] The microwave treatment and heat treatment may be performed after the insulator 283 is formed. When the insulators 210 and 283 are made of insulators having a function of suppressing hydrogen diffusion and the insulators 222 and 250 are made of insulators having a function of capturing or fixing hydrogen, heat treatment can be performed in a state where the insulators 222 and 250 are provided in the region sandwiched between the insulators 210 and 283. This allows hydrogen in the region sandwiched between the insulators 210 and 283 to be captured or fixed to the insulators 222 and 250. This reduces the hydrogen concentration in the channel formation region of the oxide semiconductor 230. Therefore, the electrical characteristics of the transistor can be improved, and the reliability of the transistor can be enhanced. Furthermore, a semiconductor device with reduced variation in the electrical characteristics of the transistor can be provided.
[0265] Through the above steps, the transistor 200 shown in FIGS. 1A to 1D can be manufactured.
[0266] 1A to 1D, the insulator 250 is formed after the insulator 270 is formed, but the present invention is not limited to this. For example, the insulator 270 may be formed after the insulator 250 is formed.
[0267] 6A to 6D show another example of a semiconductor device according to one embodiment of the present invention. FIG. 6A is a plan view of the semiconductor device. FIGS. 6B to 6D are cross-sectional views of the semiconductor device. FIG. 6B is a cross-sectional view of a portion indicated by a dashed line A1-A2 in FIG. 6A. FIG. 6C is a cross-sectional view of a portion indicated by a dashed line A3-A4 in FIG. 6A. FIG. 6D is a cross-sectional view in the XY plane including an insulator 280. Note that some elements are omitted from the plan view of FIG. 6A for clarity.
[0268] 6A to 6D differ from the semiconductor device shown in Fig. 1 in that an insulator 270 is provided on an insulator 250. Hereinafter, differences from the content described using Fig. 1A to 1D will be mainly described, and overlapping parts will be referred to and may not be described again.
[0269] 6B , in a region not overlapping with the opening 290, the insulator 250 is provided in contact with the top surface of the oxide semiconductor 230, and the insulator 270 is provided in contact with the top surface of the insulator 250. The top surface of the insulator 270 is in contact with the conductor 260 and the insulator 283. As shown in FIG. 6C , the insulator 250 is provided to cover the side surfaces of the oxide semiconductor 230, the conductor 240b, and the conductor 240a. The insulator 250 is in contact with the top surface of the insulator 280 on the outside of the conductor 240.
[0270] 6A to 6D, the insulator 250 can be formed after part of the bottom surface of the oxide semiconductor 230 is removed in the step shown in Fig. 4E. After that, a semiconductor device can be manufactured according to the steps shown in Fig. 4F to 5F.
[0271] 1A to 1D, the semiconductor device includes the insulator 270, but the present invention is not limited to this. For example, the semiconductor device may include no insulator 270.
[0272] 7A to 7D show another example of a semiconductor device according to one embodiment of the present invention. FIG. 7A is a plan view of the semiconductor device. FIGS. 7B to 7D are cross-sectional views of the semiconductor device. FIG. 7B is a cross-sectional view of the portion indicated by the dashed dotted line A1-A2 in FIG. 7A. FIG. 7C is a cross-sectional view of the portion indicated by the dashed dotted line A3-A4 in FIG. 7A. FIG. 7D is a cross-sectional view in the XY plane including the insulator 280. Note that some elements are omitted from the plan view of FIG. 7A for clarity.
[0273] 7A to 7D differ from the semiconductor device shown in Fig. 1 mainly in that the semiconductor device shown in Fig. 1 does not include an insulator 270. Hereinafter, differences from the content described using Fig. 1A to 1D will be mainly described, and overlapping portions will be referred to and may not be described again.
[0274] 7B, the insulator 250 is provided in contact with the top surface of the oxide semiconductor 230. As shown in Fig. 7C, the insulator 250 is provided to cover the side surfaces of the oxide semiconductor 230, the conductor 240b, and the conductor 240a. The insulator 250 is in contact with the top surface of the insulator 280 on the outside of the conductor 240.
[0275] 7A to 7D, the steps shown in FIGS. 4F to 5D can be omitted. That is, part of the bottom surface of the oxide semiconductor 230 is removed in the step shown in FIG. 4E, and then a semiconductor device can be manufactured according to the steps shown in FIGS. 5E and 5F. By omitting the manufacturing steps in this way, productivity of the semiconductor device can be improved.
[0276] 7B and 7C, a structure can be formed in which the side surface of the conductor 240a facing the opening 290 is flush with the side surface of the conductor 240b facing the opening 290. In this case, the side etching process for recessing the side surface of the conductive film 240B in the step shown in FIG. 4B can be omitted. By omitting the manufacturing step in this way, the productivity of the semiconductor device can be improved.
[0277] 1A to 1D, the semiconductor device has been described as being configured to remove a portion of the bottom surface of the oxide semiconductor 230 using lithography, but the present invention is not limited to this. For example, the semiconductor device may be configured to remove a portion of the bottom surface of the oxide semiconductor 230 using anisotropic etching.
[0278] 8A to 8D show another example of a semiconductor device according to one embodiment of the present invention. FIG. 8A is a plan view of the semiconductor device. FIGS. 8B to 8D are cross-sectional views of the semiconductor device. FIG. 8B is a cross-sectional view of a portion indicated by a dashed line A1-A2 in FIG. 8A. FIG. 8C is a cross-sectional view of a portion indicated by a dashed line A3-A4 in FIG. 8A. FIG. 8D is a cross-sectional view in the XY plane including an insulator 280. Note that some elements are omitted from the plan view of FIG. 8A for clarity.
[0279] 8A to 8D differ from the semiconductor device shown in Fig. 1 in that the oxide semiconductor 230 does not cover the conductors 240a and 240b. Hereinafter, differences from the description using Fig. 1A to 1D will be mainly described, and overlapping parts will be referred to and may not be described again.
[0280] 8B and 8C , the oxide semiconductor 230 is formed along the sidewall of the opening 290 and is in contact with the side surface of the conductor 240a, the side surface of the insulator 280, and the side surface of the recess of the conductor 220. In other words, the oxide semiconductor 230 is formed in a sidewall shape with respect to the opening 290. It is preferable that the oxide semiconductor 230 is not formed to cover the conductors 240a and 240b and is not in contact with the top surfaces of the conductors 240a and 240b. Here, the top end of the oxide semiconductor 230 may coincide or approximately coincide with the top surface of the conductor 240a. Furthermore, the lower part of the oxide semiconductor 230 may not protrude.
[0281] 8A to 8D , the oxide semiconductor 230 can be processed by anisotropic etching without using lithography in the step shown in FIG. 4E . Dry etching is preferably used for the anisotropic etching. For example, reactive ion etching is preferably performed. By performing anisotropic etching, the oxide semiconductor 230 can be processed into a sidewall shape even in the opening 290 with a high aspect ratio. Note that part of the oxide semiconductor 230 may remain in contact with the side surface of the conductor 240b on the opening 290 side and the side surfaces of the conductors 240a and 240b opposite to the opening 290. By using such a method, part of the bottom surface of the oxide semiconductor can be removed without using a mask.
[0282] 9A to 9D , when the oxide semiconductor 230 is processed by anisotropic etching, the insulator 270 may be formed after the insulator 250 is formed. Also, when the oxide semiconductor 230 is processed by anisotropic etching, the insulator 270 may not be formed. Furthermore, when the oxide semiconductor 230 is processed by anisotropic etching, the insulator 270 may not be formed. Furthermore, the side surface of the conductor 240a on the opening 290 side and the side surface of the conductor 240b on the opening 290 side may be flush with each other.
[0283] 1A to 1D, a configuration in which one transistor 200 is provided inside the opening 290 is shown, but the present invention is not limited to this. For example, a configuration in which multiple transistors 200 are provided inside the opening 290 is also possible.
[0284] 11A, 11B, and 12A to 12C show another example of a semiconductor device according to one embodiment of the present invention. FIGS. 11A, 12A, and 12B are plan views of the semiconductor device. FIG. 11B is a cross-sectional view of a portion indicated by a dashed dotted line A1-A2 in FIG. 11A. FIG. 12C is a cross-sectional view in the XY plane including an insulator 280. Note that some elements are omitted from the plan views of FIGS. 11A, 12A, and 12B for clarity.
[0285] 11A to 12C differs from the semiconductor device illustrated in FIGS. 1A to 1D in that a transistor 200_1 and a transistor 200_2 are provided inside an opening 290. Hereinafter, differences from the description using FIGS. 1A to 1D will be mainly described, and overlapping portions will be referred to and may not be described again.
[0286] The transistor 200_1 and the transistor 200_2 are arranged side by side in the X direction. The transistor 200_1 includes an oxide semiconductor 230_1, a conductor 240_1, and a conductor 220_1, and the transistor 200_2 includes an oxide semiconductor 230_2, a conductor 240_2, and a conductor 220_2. The conductor 240_1 has a stacked structure of a conductor 240a_1 and a conductor 240b_1, and the conductor 240_2 has a stacked structure of a conductor 240a_2 and a conductor 240b_2. The conductor 220_1 has a stacked structure of a conductor 220a_1 and a conductor 220b_1, and the conductor 220_2 has a stacked structure of a conductor 220a_2 and a conductor 220b_2.
[0287] 11A, 11B, and 12C, the oxide semiconductors 230_1 and 230_2 are arranged side by side in the X direction. In other words, the oxide semiconductors 230_1 and 230_2 are obtained by dividing the oxide semiconductor 230 shown in FIG. 1 and arranging them side by side in the X direction.
[0288] 12A, the conductor 240_1 and the conductor 240_2 are arranged side by side in the X direction. In other words, the conductor 240_1 and the conductor 240_2 are obtained by dividing the conductor 240 shown in FIG. 1 and arranging them side by side in the X direction.
[0289] 12B, the conductor 220_1 and the conductor 220_2 are arranged side by side in the X direction. In other words, the conductor 220_1 and the conductor 220_2 are obtained by dividing the conductor 220 shown in FIG. 1 and arranging them side by side in the X direction.
[0290] 12C , the oxide semiconductors 230_1 and 230_2 have approximately half the shape of the oxide semiconductor 230 shown in FIG 1. Therefore, the channel width W_1 of the transistor 200_1 and the channel width W_2 of the transistor 200_2 are approximately half or less of the channel width W of the transistor 200.
[0291] As described above, by forming two transistors in the opening 290, a semiconductor device with a higher integration density can be provided.
[0292] 13A to 14C , the transistor may be further divided, and four transistors may be provided inside the opening 290. That is, the transistors 200_1 and 200_2 shown in FIGS. 11A to 12C may be divided in the Y direction to form the transistors 200_1, 200_2, 200_3, and 200_4.
[0293] 11A to 12C can be cut in the Y direction to form the oxide semiconductors 230_1, 230_2, 230_3, and 230_4. Note that the oxide semiconductors 230_1 to 230_4 have roughly half the shapes of the oxide semiconductors 230_1 and 230_2 shown in FIGS. 11A to 12C. Therefore, the channel width W_1 of the transistor 200_1, the channel width W_2 of the transistor 200_2, the channel width W_3 of the transistor 200_3, and the channel width W_4 of the transistor 200_4 shown in FIGS. 13 and 14 are roughly half or less of the channel width W_1 of the transistor 200_1.
[0294] 11A to 12C can be divided in the Y direction to form conductors 2401, 2402, 2403, and 2404. Here, the conductors 2401 to 2404 have stacked structures of conductors 240a1 to 240a4 and conductors 240b1 to 240b4, respectively.
[0295] 11A to 12C can be divided in the Y direction to form conductors 220_1, 220_2, 220_3, and 220_4. Here, the conductors 220_1 to 220_4 have stacked structures of conductors 220a_1 to 220a_4 and conductors 220b_1 to 220b_4, respectively.
[0296] As described above, by forming four transistors in the opening 290, a semiconductor device with a higher integration density can be provided.
[0297] <Constituent Materials of Semiconductor Device> Constituent materials that can be used in the semiconductor device will be described below.
[0298] [Substrate] The substrate on which a transistor is formed may be, for example, an insulating substrate, a semiconductor substrate, or a conductive substrate. Examples of insulating substrates include glass substrates, quartz substrates, sapphire substrates, stabilized zirconia substrates (e.g., yttria-stabilized zirconia substrates), and resin substrates. Examples of semiconductor substrates include semiconductor substrates made of silicon or germanium, or compound semiconductor substrates made of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, and gallium oxide. Examples of semiconductor substrates include those having an insulating region within the semiconductor substrate, such as an SOI (Silicon-On-Insulator) substrate. Examples of conductive substrates include graphite substrates, metal substrates, alloy substrates, and conductive resin substrates. Other examples include substrates having a metal nitride or a metal oxide. Examples of other substrates include a substrate having a conductor or semiconductor provided on an insulating substrate, a substrate having a conductor or insulator provided on a semiconductor substrate, and a substrate having a semiconductor or insulator provided on a conductive substrate. Alternatively, a substrate provided with elements may be used, such as a capacitor element, a resistor element, a switch element, a light-emitting element, a memory element, and the like.
[0299] [Insulator] Examples of the insulator include oxides, nitrides, oxynitrides, nitride oxides, metal oxides, metal oxynitrides, and metal nitride oxides, all of which have insulating properties.
[0300] For example, as transistors become more miniaturized and highly integrated, problems such as leakage current may occur due to thinner gate insulators. Using a high-k material for the insulator that functions as the gate insulator allows for lower voltage operation of the transistor while maintaining the physical film thickness. It also allows for thinner equivalent oxide thickness (EOT) of the insulator that functions as the gate insulator. On the other hand, using a material with a low dielectric constant for the insulator that functions as the interlayer insulating film can reduce the parasitic capacitance that occurs between wiring. Therefore, it is preferable to select materials according to the insulator's function. Note that materials with a low dielectric constant also have high dielectric strength.
[0301] Examples of high-dielectric-constant (high-k) materials include aluminum oxide, gallium oxide, hafnium oxide, tantalum oxide, zirconium oxide, hafnium zirconium oxide, oxides containing aluminum and hafnium, oxynitrides containing aluminum and hafnium, oxides containing silicon and hafnium, oxynitrides containing silicon and hafnium, and nitrides containing silicon and hafnium.
[0302] Examples of materials with a low dielectric constant include inorganic insulating materials such as silicon oxide, silicon oxynitride, and silicon nitride oxide, and resins such as polyester, polyolefin, polyamide (nylon, aramid, etc.), polyimide, polycarbonate, and acrylic. Other examples of inorganic insulating materials with a low dielectric constant include silicon oxide doped with fluorine, silicon oxide doped with carbon, and silicon oxide doped with carbon and nitrogen. Another example is silicon oxide having vacancies. These silicon oxides may contain nitrogen.
[0303] Furthermore, a material that can have ferroelectricity may be used as the insulator. Examples of the material that can have ferroelectricity include hafnium oxide, zirconium oxide, and HfZrO. X(X is a real number greater than 0). Ferroelectric materials include materials obtained by adding element J1 (here, element J1 is one or more selected from zirconium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) to hafnium oxide. The ratio of the number of hafnium atoms to the number of element J1 can be set appropriately. For example, the ratio of the number of hafnium atoms to the number of element J1 can be set to 1:1 or close to 1:1. Ferroelectric materials include materials obtained by adding element J2 (here, element J2 is one or more selected from hafnium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) to zirconium oxide. The ratio of the number of zirconium atoms to the number of element J2 can be set appropriately. For example, the ratio of the number of zirconium atoms to the number of element J2 can be set to 1:1 or close to 1:1. Furthermore, lead titanate (PbTiO X Piezoelectric ceramics having a perovskite structure, such as barium strontium titanate (BST), strontium titanate, lead zirconate titanate (PZT), strontium bismuth tantalate (SBT), bismuth ferrite (BFO), and barium titanate, may also be used.
[0304] Furthermore, a transistor using a metal oxide can have stable electrical characteristics by being surrounded by an insulator that has a function of suppressing the permeation of impurities and oxygen. Examples of insulators that have a function of suppressing the permeation of impurities and oxygen include insulators containing boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium, and tantalum, and can be used in a single layer or a stacked layer. Specifically, examples of insulators that have a function of suppressing the permeation of impurities and oxygen include metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, and tantalum oxide, and metal nitrides such as aluminum nitride, silicon nitride oxide, and silicon nitride.
[0305] Furthermore, an insulator such as a gate insulator that is in contact with a semiconductor or that is provided near a semiconductor layer is preferably an insulator that has a region containing oxygen that is desorbed by heating (hereinafter, sometimes referred to as excess oxygen). For example, by providing an insulator that has a region containing excess oxygen in contact with a semiconductor layer or near the semiconductor layer, oxygen vacancies in the semiconductor layer can be reduced. Examples of insulators that are likely to form a region containing excess oxygen include silicon oxide, silicon oxynitride, and silicon oxide with vacancies.
[0306] Examples of the barrier insulator against oxygen include oxides containing either or both of aluminum and hafnium, oxides containing hafnium and silicon (hafnium silicate), magnesium oxide, gallium oxide, gallium zinc oxide, silicon nitride, and silicon nitride oxide. Examples of oxides containing either or both of aluminum and hafnium include aluminum oxide, hafnium oxide, and oxides containing aluminum and hafnium (hafnium aluminate).
[0307] For the barrier insulator against hydrogen, the contents described in this embodiment can be referred to.
[0308] The barrier insulator against oxygen and the barrier insulator against hydrogen can be said to be a barrier insulator against one or both of oxygen and hydrogen.
[0309] Further, the contents described in this embodiment can be referred to for an insulator having a function of capturing or fixing hydrogen.
[0310] [Conductor] The conductor is preferably a metal element selected from aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, cobalt, titanium, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium, lanthanum, etc., or an alloy containing the aforementioned metal element or an alloy combining the aforementioned metal elements. As an alloy containing the aforementioned metal element, a nitride of the alloy or an oxide of the alloy may be used. For example, tantalum nitride, titanium nitride, tungsten, nitride containing titanium and aluminum, nitride containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, oxide containing strontium and ruthenium, oxide containing lanthanum and nickel, etc. may be used. Furthermore, semiconductors with high electrical conductivity, such as polycrystalline silicon containing impurity elements such as phosphorus, or silicides such as nickel silicide may also be used.
[0311] Nitrogen-containing conductive materials, such as nitrides containing tantalum, nitrides containing titanium, nitrides containing molybdenum, nitrides containing tungsten, nitrides containing ruthenium, nitrides containing tantalum and aluminum, or nitrides containing titanium and aluminum; oxygen-containing conductive materials, such as ruthenium oxide, oxides containing strontium and ruthenium, or oxides containing lanthanum and nickel; and materials containing metal elements, such as titanium, tantalum, or ruthenium, are preferred because they are conductive materials that are resistant to oxidation, have a function of suppressing oxygen diffusion, or maintain conductivity even after absorbing oxygen. Examples of oxygen-containing conductive materials include indium oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide, indium tin oxide containing titanium oxide, indium tin oxide with added silicon, indium zinc oxide, and indium zinc oxide containing tungsten oxide. In this specification and the like, a conductive film formed using a conductive material containing oxygen may be referred to as an oxide conductive film.
[0312] Furthermore, conductive materials containing tungsten, copper, or aluminum as a main component are preferred because they have high conductivity.
[0313] Furthermore, a plurality of conductive layers formed from the above materials may be stacked. For example, a stacked structure may be formed by combining the above-described material containing a metal element and a conductive material containing oxygen. A stacked structure may be formed by combining the above-described material containing a metal element and a conductive material containing nitrogen. A stacked structure may be formed by combining the above-described material containing a metal element, a conductive material containing oxygen, and a conductive material containing nitrogen.
[0314] When a metal oxide is used for the channel formation region of a transistor, a conductor functioning as a gate electrode preferably has a stacked structure in which a material containing the metal element and a conductive material containing oxygen are combined. In this case, the conductive material containing oxygen is preferably provided on the channel formation region side. By providing the conductive material containing oxygen on the channel formation region side, oxygen desorbed from the conductive material is easily supplied to the channel formation region.
[0315] In particular, as a conductor functioning as a gate electrode, it is preferable to use a conductive material containing oxygen and a metal element contained in the metal oxide in which the channel is formed. Alternatively, the conductive materials containing the metal element and nitrogen described above may be used. For example, conductive materials containing nitrogen, such as titanium nitride and tantalum nitride, may be used. Alternatively, one or more of indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide doped with silicon may be used. Furthermore, indium gallium zinc oxide containing nitrogen may be used. Using such a material may allow hydrogen contained in the metal oxide in which the channel is formed to be captured. Alternatively, hydrogen introduced from an external insulator or the like may be captured.
[0316] [Metal Oxide] Metal oxides may have lattice defects. Lattice defects include point defects such as atomic vacancies and heteroatoms, line defects such as dislocations, planar defects such as grain boundaries, and volume defects such as voids. Factors that cause lattice defects include a discrepancy in the ratio of the number of atoms of constituent elements (excess or deficiency of constituent atoms) and impurities.
[0317] When a metal oxide is used for the semiconductor layer of a transistor, lattice defects in the metal oxide can cause carrier generation or capture. Therefore, if a metal oxide with many lattice defects is used for the semiconductor layer of a transistor, the electrical characteristics of the transistor may become unstable. Therefore, it is preferable that the metal oxide used for the semiconductor layer of a transistor has few lattice defects.
[0318] The type of lattice defects likely to exist in a metal oxide and the amount of lattice defects present vary depending on the structure of the metal oxide or the method for forming the metal oxide film.
[0319] Metal oxide structures are divided into single-crystal structures and other structures (non-single-crystal structures). Non-single-crystal structures include, for example, CAAC structures, polycrystalline structures, nc structures, pseudo-amorphous (a-like) structures, and amorphous structures. The a-like structure has a structure between the nc structure and the amorphous structure.
[0320] Furthermore, metal oxides having an a-like structure and metal oxides having an amorphous structure have voids or low-density regions. That is, metal oxides having an a-like structure and metal oxides having an amorphous structure have lower crystallinity than metal oxides having an nc structure and metal oxides having a CAAC structure. Furthermore, metal oxides having an a-like structure have a higher hydrogen concentration than metal oxides having an nc structure and metal oxides having a CAAC structure. Therefore, lattice defects are likely to be generated in metal oxides having an a-like structure and metal oxides having an amorphous structure.
[0321] Therefore, it is preferable to use a metal oxide with high crystallinity for the semiconductor layer of a transistor. For example, it is preferable to use a metal oxide having a CAAC structure or a metal oxide with a single crystal structure. By using such a metal oxide for a transistor, a transistor with good electrical characteristics can be realized. In addition, a highly reliable transistor can be realized.
[0322] Furthermore, a metal oxide that increases the on-state current of the transistor is preferably used for the channel formation region of the transistor. To increase the on-state current of the transistor, it is preferable to increase the carrier mobility of the metal oxide used in the transistor. To increase the carrier mobility of the metal oxide, it is necessary to improve the transport of carriers (electrons in the case of an n-channel transistor) or reduce scattering factors that contribute to the transport of carriers. Carriers flow from the source to the drain through the channel formation region. Therefore, by providing a channel formation region in which carriers can easily flow in the channel length direction, the on-state current of the transistor can be increased.
[0323] Here, it is preferable to use a metal oxide with high crystallinity for the metal oxide including the channel formation region. Furthermore, the crystal preferably has a crystal structure in which multiple layers (e.g., a first layer, a second layer, and a third layer) are stacked. That is, the crystal has a layered crystal structure (also referred to as a layered crystal or layered structure). In this case, the c-axis of the crystal is oriented in the direction in which the multiple layers are stacked. Examples of metal oxides having such crystals include single-crystal oxide semiconductors and CAAC-OS.
[0324] It is also preferable that the c-axis of the crystal is oriented in the normal direction to the surface on which the metal oxide is to be formed or the film surface, so that the layers are arranged parallel or approximately parallel to the surface on which the metal oxide is to be formed or the film surface, i.e., the layers extend in the channel length direction.
[0325] For example, the above-described three-layered crystal structure may have the following structure: The first layer has an octahedral oxygen atomic coordination structure with the metal contained in the first layer at the center; The second layer has a trigonal bipyramidal or tetrahedral oxygen atomic coordination structure with the metal contained in the second layer at the center; and The third layer has a trigonal bipyramidal or tetrahedral oxygen atomic coordination structure with the metal contained in the third layer at the center.
[0326] The crystal structure of the above crystal is, for example, YbFe 2 O 4 Type structure, Yb 2 Fe 3 O 7 There are various types of structures, including modified structures.
[0327] Furthermore, each of the first to third layers is preferably composed of one metal element or multiple metal elements having the same valence and oxygen. The valence of the one or more metal elements constituting the first layer is preferably the same as the valence of the one or more metal elements constituting the second layer. The first layer and the second layer may contain the same metal element. The valence of the one or more metal elements constituting the first layer is preferably different from the valence of the one or more metal elements constituting the third layer.
[0328] The above structure can improve the crystallinity of the metal oxide and increase the carrier mobility of the metal oxide. Therefore, by using the metal oxide in a channel formation region of a transistor, the on-state current of the transistor can be increased, and the electrical characteristics of the transistor can be improved.
[0329] Examples of metal oxides according to one embodiment of the present invention include indium oxide, gallium oxide, and zinc oxide. The metal oxide according to one embodiment of the present invention preferably contains at least indium (In) or zinc (Zn). The metal oxide preferably contains two or three elements selected from indium, element M, and zinc. The element M is a metal element or a metalloid element having a high bond energy with oxygen, e.g., a metal element or a metalloid element having a bond energy with oxygen higher than that of indium. Specific examples of the element M include aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium, and antimony. The element M contained in the metal oxide is preferably one or more of the above elements, more preferably one or more selected from aluminum, gallium, tin, and yttrium, and even more preferably gallium. When the element M contained in the metal oxide is gallium, the metal oxide of one embodiment of the present invention preferably contains one or more selected from indium, gallium, and zinc. Note that in this specification and the like, metal elements and metalloid elements may be collectively referred to as "metal elements," and the "metal elements" described in this specification and the like may also include metalloid elements.
[0330] Examples of metal oxides of one embodiment of the present invention include indium zinc oxide (In-Zn oxide), indium tin oxide (In-Sn oxide), indium titanium oxide (In-Ti oxide), indium gallium oxide (In-Ga oxide), indium gallium aluminum oxide (In-Ga-Al oxide), indium gallium tin oxide (In-Ga-Sn oxide, also referred to as IGTO), gallium zinc oxide (Ga-Zn oxide, also referred to as GZO), aluminum zinc oxide (Al-Zn oxide, also referred to as AZO), and indium gallium tin oxide (In-Ga-Sn oxide, also referred to as IGTO). Examples of the usable oxide include indium aluminum zinc oxide (In-Al-Zn oxide, also referred to as IAZO), indium tin zinc oxide (In-Sn-Zn oxide), indium titanium zinc oxide (In-Ti-Zn oxide), indium gallium zinc oxide (In-Ga-Zn oxide, also referred to as IGZO), indium gallium tin zinc oxide (In-Ga-Sn-Zn oxide, also referred to as IGZTO), and indium gallium aluminum zinc oxide (In-Ga-Al-Zn oxide, also referred to as IGAZO or IAGZO). Alternatively, examples include silicon-containing indium tin oxide, gallium tin oxide (Ga-Sn oxide), and aluminum tin oxide (Al-Sn oxide).
[0331] By increasing the ratio of the number of indium atoms to the total number of atoms of all metal elements contained in the metal oxide, the field-effect mobility of the transistor can be increased.
[0332] Note that the metal oxide may contain one or more metal elements with a higher periodic number instead of indium. Alternatively, the metal oxide may contain one or more metal elements with a higher periodic number in addition to indium. The greater the overlap of the orbitals of metal elements, the greater the carrier conduction in the metal oxide tends to be. Therefore, including a metal element with a higher periodic number may improve the field-effect mobility of a transistor. Examples of metal elements with a higher periodic number include metal elements belonging to the fifth period and the sixth period. Specific examples of such metal elements include yttrium, zirconium, silver, cadmium, tin, antimony, barium, lead, bismuth, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium. Note that lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium are called light rare earth elements.
[0333] The metal oxide may also contain one or more nonmetallic elements, which may increase the field-effect mobility of the transistor. Examples of nonmetallic elements include carbon, nitrogen, phosphorus, sulfur, selenium, fluorine, chlorine, bromine, and hydrogen.
[0334] Furthermore, by increasing the ratio of the number of zinc atoms to the sum of the numbers of atoms of all metal elements contained in the metal oxide, the metal oxide can be made highly crystalline, and the diffusion of impurities in the metal oxide can be suppressed, thereby suppressing fluctuations in the electrical characteristics of the transistor and improving its reliability.
[0335] Furthermore, by increasing the ratio of the number of atoms of element M to the sum of the numbers of atoms of all metal elements contained in the metal oxide, the formation of oxygen vacancies in the metal oxide can be suppressed. Therefore, carrier generation due to oxygen vacancies can be suppressed, and a transistor with a small off-state current can be obtained. Furthermore, fluctuations in the electrical characteristics of the transistor can be suppressed, thereby improving reliability.
[0336] Furthermore, by increasing the ratio of the number of In atoms to the total number of atoms of all metal elements contained in the metal oxide, the transistor can have a large on-state current and high frequency characteristics.
[0337] In the present embodiment, an In—Ga—Zn oxide may be used as an example of the metal oxide.
[0338] In order to form a metal oxide having the above-described layered crystal structure, it is preferable to deposit atoms layer by layer. In the method for forming a metal oxide film according to one embodiment of the present invention, an ALD method is used, and therefore, it is easy to form a metal oxide having the above-described layered crystal structure.
[0339] [Transistor Having Metal Oxide] Next, a case where a metal oxide (oxide semiconductor) is used as a transistor will be described. Hereinafter, a transistor using silicon for a semiconductor layer will sometimes be referred to as a Si transistor.
[0340] By using the metal oxide (oxide semiconductor) of one embodiment of the present invention for a transistor, a transistor with high field-effect mobility can be realized. Furthermore, a highly reliable transistor can be realized. Furthermore, a miniaturized or highly integrated transistor can be realized. For example, a transistor with a channel length of 2 nm to 30 nm can be manufactured.
[0341] For the channel formation region of the transistor, an oxide semiconductor with a low carrier concentration is preferably used. For example, the carrier concentration of the channel formation region of the oxide semiconductor is 1×10 18 cm −3 Below 1 × 10, preferably 17 cm −3 or less, more preferably 1 × 10 15 cm −3 or less, more preferably 1 × 10 13 cm −3 or less, more preferably 1 × 10 11 cm −3 More preferably, 1×10 10 cm −3 is less than 1×10 −9 cm −3That is all. Note that when the carrier concentration of an oxide semiconductor film is reduced, the impurity concentration in the oxide semiconductor film can be reduced, thereby reducing the density of defect states. In this specification and the like, a semiconductor having a low impurity concentration and a low density of defect states is referred to as a highly purified intrinsic or substantially highly purified intrinsic oxide semiconductor. Note that an oxide semiconductor having a low carrier concentration may be referred to as a highly purified intrinsic or substantially highly purified intrinsic oxide semiconductor.
[0342] Furthermore, a highly purified intrinsic or substantially highly purified intrinsic oxide semiconductor film has a low density of defect states, and therefore the density of trap states may also be low.
[0343] Furthermore, charges trapped in the trap states of an oxide semiconductor take a long time to disappear and may behave like fixed charges. Therefore, a transistor in which a channel formation region is formed in an oxide semiconductor with a high density of trap states may have unstable electrical characteristics.
[0344] Therefore, reducing the impurity concentration in the oxide semiconductor is effective for stabilizing the electrical characteristics of a transistor. Furthermore, in order to reduce the impurity concentration in the oxide semiconductor, it is preferable to also reduce the impurity concentration in adjacent films. Examples of impurities include hydrogen, carbon, and nitrogen. Note that the impurity in the oxide semiconductor refers to, for example, any element other than the main component constituting the oxide semiconductor. For example, an element with a concentration of less than 0.1 atomic % can be considered an impurity.
[0345] The band gap of the oxide semiconductor is preferably larger than that of silicon (typically 1.1 eV), preferably 2 eV or more, more preferably 2.5 eV or more, and further preferably 3.0 eV or more. By using an oxide semiconductor having a band gap larger than that of silicon, the off-state current (also referred to as Ioff) of the transistor can be reduced.
[0346] Furthermore, in Si transistors, a short channel effect (also referred to as SCE) occurs as the transistors are miniaturized. This makes miniaturization of Si transistors difficult. One of the reasons for the short channel effect is the small band gap of silicon. On the other hand, an OS transistor uses an oxide semiconductor, which is a semiconductor material with a wide band gap, and therefore the short channel effect can be suppressed. In other words, an OS transistor is a transistor that does not have the short channel effect or has an extremely small short channel effect.
[0347] The short-channel effect is a degradation of electrical characteristics that becomes apparent as transistors are miniaturized (channel lengths are reduced). Specific examples of the short-channel effect include a decrease in threshold voltage, an increase in subthreshold swing (sometimes referred to as S value), and an increase in leakage current. Here, the S value refers to the amount of change in gate voltage in the subthreshold region that changes the drain current by one order of magnitude at a constant drain voltage.
[0348] Furthermore, the characteristic length is widely used as an index of resistance to the short channel effect. The characteristic length is an index of how easily the potential in the channel formation region bends. The smaller the characteristic length, the steeper the potential rises, and therefore the more resistant it is to the short channel effect.
[0349] An OS transistor is an accumulation-mode transistor, while a Si transistor is an inversion-mode transistor. Therefore, compared with a Si transistor, an OS transistor has a smaller characteristic length between a source region and a channel formation region and a smaller characteristic length between a drain region and a channel formation region. Therefore, an OS transistor is more resistant to the short-channel effect than a Si transistor. That is, when a transistor with a short channel length is to be manufactured, an OS transistor is more suitable than a Si transistor.
[0350] Even when the carrier concentration of the oxide semiconductor is reduced to the point where the channel formation region becomes i-type or substantially i-type, the conduction band minimum of the channel formation region in a short-channel transistor is lowered due to the conduction-band-lowering (CBL) effect, and therefore the energy difference between the conduction band minimums of the source or drain region and the channel formation region can be reduced to 0.1 eV or more and 0.2 eV or less. − The source and drain regions are n-type regions. + The region of type n + / n − / n + an accumulation-type junction-less transistor structure, or + / n − / n + This can also be regarded as an accumulation type non-junction transistor structure.
[0351] By using an OS transistor with the above structure, good electrical characteristics can be obtained even when a semiconductor device is miniaturized or highly integrated. For example, good electrical characteristics can be obtained even when the channel length or gate length of an OS transistor is 20 nm or less, 15 nm or less, 10 nm or less, 7 nm or less, or 6 nm or less, or 1 nm or more, 3 nm or more, or 5 nm or more. On the other hand, a Si transistor may have difficulty achieving a gate length of 20 nm or less or 15 nm or less due to the short-channel effect. Therefore, an OS transistor can be suitably used as a transistor having a shorter channel length than a Si transistor. Note that the gate length refers to the length of a gate electrode in a direction in which carriers move inside a channel formation region during transistor operation.
[0352] Furthermore, miniaturization of an OS transistor can improve the high-frequency characteristics of the transistor. Specifically, the cutoff frequency of the transistor can be improved. When the gate length of an OS transistor is within the above range, the cutoff frequency of the transistor can be set to, for example, 50 GHz or higher, preferably 100 GHz or higher, and further preferably 150 GHz or higher at room temperature.
[0353] As described above, compared to Si transistors, OS transistors have excellent advantages such as a smaller off-state current and the ability to be manufactured as transistors with a short channel length.
[0354] [Impurities in Metal Oxides] Here, the influence of each impurity in a metal oxide (oxide semiconductor) will be described.
[0355] When an oxide semiconductor contains silicon or carbon, which is one of the Group 14 elements, defect levels are formed in the oxide semiconductor. Therefore, the carbon concentration in the channel formation region of the oxide semiconductor measured by SIMS is 1×10 20 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 Less than or equal to 3×10 19 atoms / cm 3 or less, more preferably 1 × 10 19 atoms / cm 3 Less than or equal to 3×10 18 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 The silicon concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 Less than or equal to 3×10 19 atoms / cm 3 or less, more preferably 1 × 10 19 atoms / cm3 Less than or equal to 3×10, more preferably 18 atoms / cm 3 More preferably, 1×10 18 atoms / cm 3 The following applies.
[0356] Furthermore, when nitrogen is contained in an oxide semiconductor, electrons serving as carriers are generated, the carrier concentration increases, and the semiconductor is likely to become n-type. As a result, a transistor using an oxide semiconductor containing nitrogen as a semiconductor tends to have normally-on characteristics. Alternatively, when nitrogen is contained in an oxide semiconductor, trap states may be formed. As a result, the electrical characteristics of the transistor may become unstable. Therefore, the nitrogen concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Below 5 × 10, preferably 19 atoms / cm 3 or less, more preferably 1 × 10 19 atoms / cm 3 Less than or equal to 5 × 10, more preferably 18 atoms / cm 3 or less, more preferably 1 × 10 18 atoms / cm 3 or less, more preferably 5 × 10 17 atoms / cm 3 The following applies.
[0357] Furthermore, hydrogen contained in an oxide semiconductor may react with oxygen bonded to a metal atom to form water, which may form an oxygen vacancy. Hydrogen entering the oxygen vacancy may generate electrons as carriers. Furthermore, some of the hydrogen may bond with oxygen bonded to a metal atom to generate electrons as carriers. Therefore, a transistor using an oxide semiconductor containing hydrogen is likely to have normally-on characteristics. Therefore, it is preferable to reduce hydrogen as much as possible in the channel formation region of the oxide semiconductor. Specifically, the hydrogen concentration in the channel formation region of the oxide semiconductor obtained by SIMS is 1×10 20 atoms / cm 3 Less than 5×1019 atoms / cm 3 less than 1×10 19 atoms / cm 3 less than 5×10 18 atoms / cm 3 less than 1×10 18 atoms / cm 3 less than 1×10 17 atoms / cm 3 Less than.
[0358] Furthermore, when an oxide semiconductor contains an alkali metal or an alkaline earth metal, defect levels may be formed and carriers may be generated. Therefore, a transistor using an oxide semiconductor containing an alkali metal or an alkaline earth metal is likely to have normally-on characteristics. Therefore, when the concentration of the alkali metal or the alkaline earth metal in the channel formation region of the oxide semiconductor obtained by SIMS is set to 1×10 18 atoms / cm 3 Below 2 × 10, preferably 16 atoms / cm 3 Do the following:
[0359] When an oxide semiconductor with sufficiently reduced impurities is used for a channel formation region of a transistor, stable electrical characteristics can be obtained.
[0360] [Other Semiconductor Materials] The oxide semiconductor 230 can be rephrased as a semiconductor layer including a channel formation region of a transistor. The semiconductor material that can be used for the semiconductor layer is not limited to the above-mentioned metal oxides. A semiconductor material having a band gap (a semiconductor material that is not a zero-gap semiconductor) may also be used for the semiconductor layer. For example, a semiconductor of a single element, a compound semiconductor, or a layered material (also referred to as an atomic layer material, a two-dimensional material, or the like) is preferably used as the semiconductor material.
[0361] In this specification and the like, a layered material is a general term for a group of materials having a layered crystal structure. A layered crystal structure is a structure in which layers formed by covalent or ionic bonds are stacked via bonds weaker than covalent or ionic bonds, such as van der Waals bonds. A layered material has high electrical conductivity within a unit layer, that is, high two-dimensional electrical conductivity. By using a material that functions as a semiconductor and has high two-dimensional electrical conductivity in the channel formation region, a transistor with a large on-current can be provided.
[0362] Examples of semiconductors that can be used as semiconductor materials include silicon and germanium. Examples of silicon that can be used as semiconductor layers include single-crystal silicon, polycrystalline silicon, microcrystalline silicon, and amorphous silicon. Examples of polycrystalline silicon include low-temperature polysilicon (LTPS).
[0363] Compound semiconductors that can be used for the semiconductor material include silicon carbide, silicon germanium, gallium arsenide, indium phosphide, boron nitride, and boron arsenide. Boron nitride that can be used for the semiconductor layer preferably has an amorphous structure. Boron arsenide that can be used for the semiconductor layer preferably has a cubic crystal structure.
[0364] Examples of layered materials include graphene, silicene, boron carbonitride, and chalcogenides. Boron carbonitride, a layered material, has carbon atoms, nitrogen atoms, and boron atoms arranged in a hexagonal lattice structure on a plane. Chalcogenides are compounds containing chalcogen. Chalcogen is a general term for elements belonging to Group 16, including oxygen, sulfur, selenium, tellurium, polonium, and livermorium. Examples of chalcogenides include transition metal chalcogenides and Group 13 chalcogenides.
[0365] For example, it is preferable to use a transition metal chalcogenide that functions as a semiconductor for the semiconductor layer. Specific examples of transition metal chalcogenides that can be used for the semiconductor layer include molybdenum sulfide (typically, MoS2 ), molybdenum selenide (typically MoSe 2 ), molybdenum telluride (typically MoTe 2 ), tungsten sulfide (typically WS 2 ), tungsten selenide (typically WSe 2 ), tungsten tellurium (typically WTe 2 ), hafnium sulfide (typically HfS 2 ), hafnium selenide (typically HfSe 2 ), zirconium sulfide (typically ZrS 2 ), zirconium selenide (typically ZrSe 2 By applying the above-mentioned transition metal chalcogenide to a semiconductor layer, a semiconductor device with a large on-current can be provided.
[0366] This embodiment mode can be combined with other embodiment modes and examples as appropriate. In addition, in this specification, when a plurality of configuration examples are shown in one embodiment mode, the configuration examples can be combined as appropriate.
[0367] Embodiment 2 In this embodiment, a semiconductor device 900 according to one embodiment of the present invention will be described. The semiconductor device 900 can function as a memory device.
[0368] Fig. 16 is a block diagram showing a configuration example of a semiconductor device 900. The semiconductor device 900 shown in Fig. 16 has a driver circuit 910 and a memory array 920. The memory array 920 has one or more memory cells 950. Fig. 16 shows an example in which the memory array 920 has a plurality of memory cells 950 arranged in a matrix.
[0369] The transistors described in the above embodiments can be applied to the memory cell 950. By using the transistors, miniaturization and high integration of a memory device can be achieved. In addition, the capacitance per area of the memory device can be increased.
[0370] The drive circuit 910 includes a PSW 931 (power switch), a PSW 932, and a peripheral circuit 915. The peripheral circuit 915 includes a peripheral circuit 911, a control circuit 912, and a voltage generation circuit 928.
[0371] In the semiconductor device 900, each circuit, signal, and voltage can be appropriately selected or omitted as needed. Alternatively, other circuits or signals may be added. The signals BW, CE, GW, CLK, WAKE, ADDR, WDA, PON1, and PON2 are input signals from the outside, and the signal RDA is an output signal to the outside. The signal CLK is a clock signal.
[0372] Furthermore, signals BW, CE, and GW are control signals. Signal CE is a chip enable signal, signal GW is a global write enable signal, and signal BW is a byte write enable signal. Signal ADDR is an address signal. Signal WDA is write data, and signal RDA is read data. Signals PON1 and PON2 are power gating control signals. Note that signals PON1 and PON2 may be generated by the control circuit 912.
[0373] The control circuit 912 is a logic circuit having a function of controlling the overall operation of the semiconductor device 900. For example, the control circuit 912 performs a logical operation on the signals CE, GW, and BW to determine the operation mode (e.g., write operation, read operation) of the semiconductor device 900. Alternatively, the control circuit 912 generates a control signal for the peripheral circuit 911 so that this operation mode is executed.
[0374] The voltage generating circuit 928 has a function of generating a negative voltage. The signal WAKE has a function of controlling the input of the signal CLK to the voltage generating circuit 928. For example, when an H-level signal is given as the signal WAKE, the signal CLK is input to the voltage generating circuit 928, and the voltage generating circuit 928 generates a negative voltage.
[0375] The peripheral circuit 911 is a circuit for writing and reading data to and from the memory cells 950. The peripheral circuit 911 includes a row decoder 941, a column decoder 942, a row driver 923, a column driver 924, an input circuit 925, an output circuit 926, and a sense amplifier 927.
[0376] The row decoder 941 and the column decoder 942 have the function of decoding the signal ADDR. The row decoder 941 is a circuit for specifying a row to be accessed, and the column decoder 942 is a circuit for specifying a column to be accessed. The row driver 923 has the function of selecting the row specified by the row decoder 941. The column driver 924 has the function of writing data to the memory cells 950, reading data from the memory cells 950, and retaining the read data.
[0377] The input circuit 925 has a function of holding a signal WDA. The data held by the input circuit 925 is output to the column driver 924. The output data of the input circuit 925 is data (Din) to be written to the memory cell 950. The data (Dout) read from the memory cell 950 by the column driver 924 is output to the output circuit 926. The output circuit 926 has a function of holding Dout. In addition, the output circuit 926 has a function of outputting Dout to the outside of the semiconductor device 900. The data output from the output circuit 926 is a signal RDA.
[0378] The PSW 931 is a V DD The PSW 932 has the function of controlling the supply of V to the row driver 923. HM Here, the high power supply voltage of the semiconductor device 900 is V DD and the low power supply voltage is GND (ground potential). HM is the high power supply voltage used to drive the word line high, and V DDThe signal PON1 controls the on / off of the PSW 931, and the signal PON2 controls the on / off of the PSW 932. In FIG. 16, in the peripheral circuit 915, V DD Although the number of power domains to which power is supplied is set to one, it is also possible to set it to a plurality of power domains. In this case, a power switch may be provided for each power domain.
[0379] 17A to 17H, other examples of memory cell configurations that can be applied to the memory cell 950 will be described.
[0380] 17A shows an example of a circuit configuration of a DRAM memory cell. In this specification and the like, a DRAM using an OS transistor is referred to as a DOSRAM (Dynamic Oxide Semiconductor Random Access Memory). The memory cell 951 includes a transistor M1 and a capacitor CA.
[0381] The transistor M1 may have a front gate (sometimes simply referred to as a gate) and a back gate. In this case, the back gate may be connected to a wiring that supplies a constant potential or a signal, or the front gate and the back gate may be connected to each other.
[0382] A first terminal of the transistor M1 is connected to a first terminal of the capacitance element CA, a second terminal of the transistor M1 is connected to the wiring BIL, and a gate of the transistor M1 is connected to the wiring WOL. The second terminal of the capacitance element CA is connected to the wiring CAL.
[0383] The wiring BIL functions as a bit line, and the wiring WOL functions as a word line. The wiring CAL functions as a wiring for applying a predetermined potential to the second terminal of the capacitance element CA. When writing and reading data, it is preferable to apply a low-level potential (sometimes referred to as a reference potential) to the wiring CAL.
[0384] Data is written and read by applying a high-level potential to the wiring WOL, turning on the transistor M1, and connecting the wiring BIL and the first terminal of the capacitor CA.
[0385] Furthermore, the memory cell that can be used as the memory cell 950 is not limited to the memory cell 951, and the circuit configuration can be changed. For example, the memory cell 950 can have the configuration of a memory cell 952 as shown in FIG. 17B. The memory cell 952 is an example in which the memory cell 952 does not include a capacitor CA and a wiring CAL. The first terminal of the transistor M1 is in an electrically floating state.
[0386] In the memory cell 952, the potential written through the transistor M1 is held in a capacitance (also referred to as a parasitic capacitance) between the first terminal and the gate, which is indicated by a dashed line. With this configuration, the configuration of the memory cell can be significantly simplified.
[0387] Note that the OS transistor described in the above embodiment is preferably used as the transistor M1. By using the OS transistor described in the above embodiment, the area occupied by the memory cell can be reduced. Furthermore, the OS transistor has a characteristic of extremely low off-state current. By using an OS transistor as the transistor M1, the leakage current of the transistor M1 can be significantly reduced. That is, written data can be held by the transistor M1 for a long time, which reduces the frequency of refreshing the memory cell. Alternatively, the refresh operation of the memory cell can be eliminated. Furthermore, because the leakage current is extremely low, multilevel data or analog data can be held in the memory cell 951 and the memory cell 952.
[0388] An example of the structure of a DOSRAM will now be described with reference to FIG. 18. FIGS. 18A to 18C are plan and cross-sectional views of a memory device including a transistor 200 and a capacitor 400. FIG. 18A is a plan view of the memory device. FIGS. 18B and 18C are cross-sectional views of the memory device. Here, FIG. 18B is a cross-sectional view of the portion indicated by the dashed dotted line A1-A2 in FIG. 18A. FIG. 18C is a cross-sectional view of the portion indicated by the dashed dotted line A3-A4 in FIG. 18A. Note that some elements have been omitted from the plan view of FIG. 18A for clarity.
[0389] 18A to 18C includes an insulator 440 on a substrate (not shown), a conductor 410 on the insulator 440, a memory cell 450 on the conductor 410, an insulator 480 on the conductor 410, an insulator 280, and an insulator 283 on the memory cell 450. The insulator 440, the insulator 480, and the insulator 280 function as interlayer films. The conductor 410 functions as a wiring.
[0390] The memory cell 450 includes a capacitor 400 over a conductor 410 and a transistor 200 over the capacitor 400. Here, the transistor 200 may be the transistor described in Embodiment 1. For details of the transistor 200, the description in Embodiment 1 can be referred to.
[0391] The capacitor 400 includes a conductor 415 on a conductor 410, an insulator 430 on the conductor 415, and a conductor 220a on the insulator 430. The conductor 220a functions as one of a pair of electrodes (sometimes referred to as an upper electrode), the conductor 415 functions as the other of the pair of electrodes (sometimes referred to as a lower electrode), and the insulator 430 functions as a dielectric. That is, the capacitor 400 constitutes a metal-insulator-metal (MIM) capacitor.
[0392] As shown in Figures 18B and 18C, an opening 490 is provided in the insulator 480, reaching the conductor 410. At least a portion of the conductor 415 is disposed in the opening 490. The conductor 415 has a region in contact with the upper surface of the conductor 410 in the opening 490, a region in contact with the side surface of the insulator 480 in the opening 490, and a region in contact with at least a portion of the upper surface of the insulator 480. The insulator 430 is disposed so that at least a portion of it is located in the opening 490. The conductor 220a is disposed so that at least a portion of it is located in the opening 490. As shown in Figures 18B and 18C, the conductor 220a is preferably disposed so as to fill the opening 490.
[0393] The capacitor 400 has a configuration in which the upper electrode and the lower electrode face each other across a dielectric not only on the bottom surface but also on the side surface of the opening 490, allowing for a larger capacitance per unit area. Therefore, the deeper the opening 490, the larger the capacitance of the capacitor 400 can be. Increasing the capacitance per unit area of the capacitor 400 in this way can stabilize the read operation of the memory device. Furthermore, this can promote miniaturization or high integration of memory devices.
[0394] The sidewall of the opening 490 is preferably perpendicular to the top surface of the conductor 410. In this case, the opening 490 has a cylindrical shape. With such a structure, miniaturization or high integration of the memory device can be achieved.
[0395] A conductor 415 and an insulator 430 are stacked along the sidewall of the opening 490 and the top surface of the conductor 410. In addition, a conductor 220a is provided on the insulator 430 so as to fill the opening 490. The capacitor 400 having such a structure may be called a trench capacitor or a trench capacitor.
[0396] As shown in FIGS. 18A to 18C , the transistor 200 is provided so as to overlap with the capacitor 400. The opening 290 where part of the structure of the transistor 200 is provided overlaps with the opening 490 where part of the structure of the capacitor 400 is provided. In particular, the conductor 220a functions as one of the source electrode and drain electrode of the transistor 200 and as the upper electrode of the capacitor 400. Therefore, the transistor 200 and the capacitor 400 share part of their structures. With this structure, the transistor 200 and the capacitor 400 can be provided without significantly increasing the occupied area in a plan view. This reduces the occupied area of the memory cell 450, thereby enabling the memory cells 450 to be arranged at a high density and increasing the storage capacity of the memory device. In other words, the memory device can be highly integrated.
[0397] 18A to 18C functions as, for example, the memory cell 951 of the DOSRAM shown in FIG.
[0398] Here, the wiring BIL corresponds to the conductor 240 (conductor 240a and conductor 240b), the wiring WOL corresponds to the conductor 260, and the wiring CAL corresponds to the conductor 410. As shown in FIGS. 18A to 18C , it is preferable that the conductor 260 is provided extending in the Y direction, and the conductor 240 is provided extending in the X direction. With this configuration, the wiring BIL and the wiring WOL are provided so as to intersect with each other. Also, in FIG. 18A , the wiring CAL (conductor 410) is provided extending in the X direction, but the present invention is not limited to this. For example, the wiring CAL may be provided extending in the Y direction or in a planar form.
[0399] The conductor 410 is provided over the insulator 440. The conductors described in the section [Conductor] of Embodiment 1 can be used as the conductor 410 in a single layer or a stacked layer. For example, a conductive material with high conductivity, such as tungsten, can be used as the conductor 410. By using such a conductive material with high conductivity, the conductivity of the conductor 410 can be improved, and the conductor 410 can function sufficiently as a wiring CAL.
[0400] The conductor 410 is preferably made of a conductive material that is resistant to oxidation or a conductive material that has a function of suppressing oxygen diffusion, and is used in a single layer or a stacked layer. For example, titanium nitride or indium tin oxide with added silicon may be used. Alternatively, for example, a structure in which titanium nitride is stacked on tungsten may be used. Alternatively, for example, a structure in which tungsten is stacked on a first titanium nitride and a second titanium nitride is stacked on the tungsten may be used. With such a structure, when an oxide insulator is used for the insulator 480, oxidation of the conductor 410 by the insulator 480 can be suppressed.
[0401] The conductor 415 can be a single layer or a stacked layer of the conductors described in the [Conductor] section of Embodiment 1. It is preferable to use a conductive material that is resistant to oxidation or a conductive material that has a function of suppressing oxygen diffusion as the conductor 415. For example, titanium nitride or tantalum nitride can be used. Alternatively, for example, a structure in which tantalum nitride is stacked on titanium nitride may be used. With such a structure, when an oxide insulator is used for the insulator 430, the insulator 430 can suppress oxidation of the conductor 415. Furthermore, when an oxide insulator is used for the insulator 480, the insulator 480 can suppress oxidation of the conductor 415.
[0402] The insulator 430 is provided on the conductor 415. The insulator 430 is provided so as to be in contact with the top surface and side surfaces of the conductor 415. In other words, the insulator 430 preferably has a structure that covers the side end portions of the conductor 415. This can prevent the conductor 415 and the conductor 220a from shorting out.
[0403] Alternatively, a structure may be used in which the side edge of the insulator 430 coincides with the side edge of the conductor 415. With such a structure, the insulator 430 and the conductor 415 can be formed using the same mask, thereby simplifying the manufacturing process of the memory device.
[0404] It is preferable to use a material with a high relative dielectric constant, a so-called high-k material, as described in the [Insulator] section of Embodiment 1, as the insulator 430. By using a high-k material as the insulator 430, the insulator 430 can be made thick enough to suppress leakage current and the capacitance of the capacitor 400 can be sufficiently ensured.
[0405] The insulator 430 is preferably formed by stacking insulating layers made of a high-k material, and preferably by using a layered structure of a high-k material with a high relative dielectric constant and a material with a higher dielectric strength than the high-k material. For example, the insulator 430 can be formed by stacking zirconium oxide, aluminum oxide, and zirconium oxide in this order. Alternatively, the insulator 430 can be formed by stacking zirconium oxide, aluminum oxide, zirconium oxide, and aluminum oxide in this order. Alternatively, the insulator 430 can be formed by stacking hafnium zirconium oxide, aluminum oxide, hafnium zirconium oxide, and aluminum oxide in this order. By stacking insulators with a relatively high dielectric strength, such as aluminum oxide, the dielectric strength is improved, and electrostatic breakdown of the capacitor element 400 can be suppressed.
[0406] Furthermore, a material that can have ferroelectricity may be used as the insulator 430. Examples of the material that can have ferroelectricity include hafnium oxide, zirconium oxide, and HfZrO. X (X is a real number greater than 0). Ferroelectric materials include materials obtained by adding element J1 (here, element J1 is one or more selected from zirconium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) to hafnium oxide. The ratio of the number of hafnium atoms to the number of element J1 can be set appropriately. For example, the ratio of the number of hafnium atoms to the number of element J1 can be set to 1:1 or close to 1:1. Ferroelectric materials include materials obtained by adding element J2 (here, element J2 is one or more selected from hafnium, silicon, aluminum, gadolinium, yttrium, lanthanum, strontium, etc.) to zirconium oxide. The ratio of the number of zirconium atoms to the number of element J2 can be set appropriately. For example, the ratio of the number of zirconium atoms to the number of element J2 can be set to 1:1 or close to 1:1. Furthermore, lead titanate (PbTiO XPiezoelectric ceramics having a perovskite structure, such as barium strontium titanate (BST), strontium titanate, lead zirconate titanate (PZT), strontium bismuth tantalate (SBT), bismuth ferrite (BFO), and barium titanate, may also be used.
[0407] Furthermore, examples of materials that can exhibit ferroelectricity include metal nitrides containing elements M1, M2, and nitrogen. Here, element M1 is one or more elements selected from aluminum, gallium, indium, etc. Furthermore, element M2 is one or more elements selected from boron, scandium, yttrium, lanthanum, cerium, neodymium, europium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, etc. The ratio of the number of atoms of element M1 to the number of atoms of element M2 can be set as appropriate. Furthermore, metal oxides containing element M1 and nitrogen may exhibit ferroelectricity even without containing element M2. Furthermore, examples of materials that can exhibit ferroelectricity include materials in which element M3 is added to the above metal nitrides. Furthermore, element M3 is one or more elements selected from magnesium, calcium, strontium, zinc, cadmium, etc. Here, the ratio of the number of atoms of element M1 to the number of atoms of element M2 to the number of atoms of element M3 can be set as appropriate.
[0408] Furthermore, materials that can have ferroelectricity include SrTaO 2 N, BaTaO 2 Perovskite-type oxynitrides such as N, GaFeO with κ-alumina structure 3 Examples include:
[0409] Although the above description has been given with reference to metal oxides and metal nitrides, the present invention is not limited to these. For example, metal oxynitrides in which nitrogen is added to the above metal oxides, or metal oxynitrides in which oxygen is added to the above metal nitrides, may also be used.
[0410] Furthermore, the material capable of exhibiting ferroelectricity may be, for example, a mixture or compound of multiple materials selected from the materials listed above. Alternatively, the insulator 430 may have a layered structure of multiple materials selected from the materials listed above. However, since the crystal structure (characteristics) of the materials listed above may change depending not only on the film formation conditions but also on various processes, in this specification and the like, not only materials that exhibit ferroelectricity are referred to as ferroelectrics, but also as materials capable of exhibiting ferroelectricity.
[0411] Metal oxides containing one or both of hafnium and zirconium are preferred because they can exhibit ferroelectricity even in thin films of only a few nanometers. Here, the film thickness of the insulator 430 can be 100 nm or less, preferably 50 nm or less, more preferably 20 nm or less, and even more preferably 10 nm or less (typically, 2 nm to 9 nm). For example, a film thickness of 8 nm to 12 nm is preferred. By using a ferroelectric layer that can be thinned, the capacitor element 400 can be combined with semiconductor elements such as miniaturized transistors to form a semiconductor device. Note that, in this specification, a layer of a material that can exhibit ferroelectricity may be referred to as a ferroelectric layer, a metal oxide film, or a metal nitride film. Furthermore, a device having such a ferroelectric layer, a metal oxide film, or a metal nitride film may be referred to as a ferroelectric device in this specification.
[0412] Furthermore, a metal oxide containing one or both of hafnium and zirconium is preferable because it can have ferroelectricity even in a very small area. 2 Below, 10μm 2 Below, 1μm 2 or less than 0.1 μm 2 Even if the thickness is less than 10,000 nm, the film can still have ferroelectricity. 2 or less than 1000 nm 2 Even if the thickness is less than 100 nm, the ferroelectric layer may have ferroelectricity. By using a ferroelectric layer with a small area, the area occupied by the capacitor element 400 can be reduced.
[0413] A ferroelectric material is an insulator that generates polarization internally when an external electric field is applied, and the polarization remains even when the electric field is removed. Therefore, a nonvolatile memory element can be formed using a capacitance element (hereinafter sometimes referred to as a ferroelectric capacitor) that uses this material as a dielectric. A nonvolatile memory element using a ferroelectric capacitor is sometimes called a Ferroelectric Random Access Memory (FeRAM), a ferroelectric memory, or the like. For example, a ferroelectric memory has a transistor and a ferroelectric capacitor, and one of the source and drain of the transistor is electrically connected to one terminal of the ferroelectric capacitor. Therefore, when a ferroelectric capacitor is used as the capacitance element 400, the memory device described in this embodiment functions as a ferroelectric memory.
[0414] Ferroelectricity is believed to be exhibited by the displacement of oxygen or nitrogen in crystals contained in the ferroelectric layer due to an external electric field. Furthermore, it is believed that the exhibiting of ferroelectricity depends on the crystal structure of the crystals contained in the ferroelectric layer. Therefore, for the insulator 430 to exhibit ferroelectricity, the insulator 430 must contain crystals. In particular, the insulator 430 preferably contains crystals having an orthorhombic crystal structure, since this exhibits ferroelectricity. The crystal structure of the crystals contained in the insulator 430 may be one or more selected from the group consisting of cubic, tetragonal, orthorhombic, monoclinic, and hexagonal. The insulator 430 may also have an amorphous structure. In this case, the insulator 430 may have a composite structure having an amorphous structure and a crystalline structure.
[0415] The conductor 220a is provided in contact with part of the top surface of the insulator 430. The conductor 220a is similar to that used in the transistor 200. Alternatively, a structure in which a conductor 220c is stacked below the conductor 220a may be used.
[0416] The insulator 480 preferably has a low dielectric constant because it functions as an interlayer film. Using a material with a low dielectric constant as the interlayer film can reduce parasitic capacitance between wirings. As the insulator 480, a single layer or a stacked layer of insulators containing a material with a low dielectric constant, as described in the [Insulator] section of Embodiment 1, can be used. Silicon oxide and silicon oxynitride are preferable because they are thermally stable. In this case, the insulator 480 contains at least silicon and oxygen.
[0417] 18B and 18C show the insulator 480 as a single layer, but the present invention is not limited to this. The insulator 480 may have a stacked structure. In the case of a stacked structure, it is preferable to use an insulator having a barrier property against hydrogen, as described in the [Insulator] section of Embodiment 1, for one or more layers of the insulator 480. This can prevent hydrogen from diffusing from below to the insulator 430 through the insulator 480 and the conductor 415. Silicon nitride and silicon nitride oxide are suitable for use as the insulator 480 because they each release little impurities (e.g., water and hydrogen) and are less permeable to oxygen and hydrogen.
[0418] 19A and 19B will be used to describe an example of a memory device in which two memory cells 450 (hereinafter referred to as memory cell 450a and memory cell 450b) are connected to a common wiring. FIG. 19A is a plan view of the memory device. FIG. 19B is a cross-sectional view of the portion indicated by the dashed dotted line A1-A2 in FIG. 19A. Note that some elements are omitted from the plan view of FIG. 19A for clarity.
[0419] 19A and 19B have the same configuration as the memory cell 450. The memory cell 450a has a capacitor 400a and a transistor 200a, and the memory cell 450b has a capacitor 400b and a transistor 200b. Therefore, in the memory device shown in FIGS. 19A and 19B, structures having the same functions as the structures constituting the memory device shown in FIG. 18 are denoted by the same reference numerals.
[0420] 19A and 19B , the conductor 260 functioning as the wiring WOL is provided in each of the memory cell 450a and the memory cell 450b. The conductor 240 functioning as part of the wiring BIL is provided in common to the memory cell 450a and the memory cell 450b. That is, the conductor 240 is in contact with the oxide semiconductor 230 of the memory cell 450a and the oxide semiconductor 230 of the memory cell 450b.
[0421] 19A and 19B includes a conductor 445 and a conductor 446 that are electrically connected to the memory cell 450a and the memory cell 450b and function as plugs (which can also be referred to as connection electrodes). The conductor 445 is disposed in openings formed in the insulators 480, 430, and 280 and is in contact with the bottom surface of the conductor 240a and the top surface of a conductor 447 that is formed in the same layer as the conductor 410. The conductor 446 is disposed in openings formed in the insulators 288, 283, 250, 270, and the oxide semiconductor 230 and is in contact with the top surface of the conductor 240b. A conductor similar to the conductor 446 may be provided under the conductor 447. Note that the conductors 445 and 446 can be formed using a conductive material that can be used for the conductor 240, or the like.
[0422] The insulator 288 is provided over the insulator 283. Since the insulator 288 functions as an interlayer film, it is preferable that the insulator 288 has a low dielectric constant. By using a material with a low dielectric constant as the interlayer film, parasitic capacitance occurring between wirings can be reduced. As the insulator 288, an insulator containing a material with a low dielectric constant, as described in the [Insulator] section of Embodiment 1, can be used in a single layer or a stacked layer.
[0423] The conductors 445 and 446 function as plugs or wirings for electrically connecting circuit elements such as switches, transistors, capacitors, inductors, resistors, and diodes, wirings, electrodes, or terminals to the memory cells 450a and 450b. For example, the memory cells 450a and 450b can be electrically connected to a sense amplifier provided below the memory device or another memory device provided above the memory device. In this case, the conductors 445 and 446 function as part of the wiring BIL. In this way, by providing a memory device above or below the memory device shown in FIG. 19, the memory capacity per unit area can be increased.
[0424] The memory cell 450a and the memory cell 450b are configured in line symmetry with respect to the perpendicular bisector of the dashed-dotted line A1-A2. Therefore, the transistors 200a and 200b are also arranged symmetrically with respect to the conductors 445 and 446. The conductor 240 functions as the other of the source and drain electrodes of the transistor 200a and the other of the source and drain electrodes of the transistor 200b. The transistors 200a and 200b share the conductors 445 and 446, which function as plugs. By configuring the connections between the two transistors and the plugs as described above, a memory device that can be miniaturized or highly integrated can be provided.
[0425] Note that the conductor 410 functioning as the wiring CAL may be provided in each of the memory cells 450 a and 450 b, or may be provided in common to the memory cells 450 a and 450 b. However, as shown in FIG. 19B , the conductor 410 is provided apart from the conductor 447 to prevent the conductor 410 and the conductor 447 from shorting out.
[0426] 17C shows an example circuit configuration of a gain cell type memory cell having two transistors and one capacitor. The memory cell 953 includes a transistor M2, a transistor M3, and a capacitor CB. In this specification and the like, a memory device having a gain cell type memory cell in which the transistor M2 is an OS transistor is referred to as a nonvolatile oxide semiconductor RAM (NOSRAM).
[0427] The first terminal of transistor M2 is connected to the first terminal of capacitance element CB, the second terminal of transistor M2 is connected to wiring WBL, and the gate of transistor M2 is connected to wiring WOL. The second terminal of capacitance element CB is connected to wiring CAL. The first terminal of transistor M3 is connected to wiring RBL, the second terminal of transistor M3 is connected to wiring SL, and the gate of transistor M3 is connected to the first terminal of capacitance element CB.
[0428] The wiring WBL functions as a write bit line, the wiring RBL functions as a read bit line, and the wiring WOL functions as a word line. The wiring CAL functions as a wiring for applying a predetermined potential to the second terminal of the capacitance element CB. When writing data, while retaining data, and when reading data, it is preferable to apply a low-level potential (sometimes referred to as a reference potential) to the wiring CAL.
[0429] Data is written by applying a high-level potential to the wiring WOL, turning on the transistor M2, and connecting the wiring WBL to the first terminal of the capacitance element CB. Specifically, when the transistor M2 is on, a potential corresponding to the information to be recorded is applied to the wiring WBL, and the potential is written to the first terminal of the capacitance element CB and the gate of the transistor M3. Then, a low-level potential is applied to the wiring WOL, turning off the transistor M2, thereby maintaining the potential of the first terminal of the capacitance element CB and the potential of the gate of the transistor M3.
[0430] Data is read by applying a predetermined potential to the wiring SL. The current flowing between the source and drain of the transistor M3 and the potential of the first terminal of the transistor M3 are determined by the potential of the gate of the transistor M3 and the potential of the second terminal of the transistor M3. Therefore, the potential held in the first terminal of the capacitor CB (or the gate of the transistor M3) can be read by reading the potential of the wiring RBL connected to the first terminal of the transistor M3. In other words, information written in this memory cell can be read from the potential held in the first terminal of the capacitor CB (or the gate of the transistor M3).
[0431] Alternatively, for example, the wiring WBL and the wiring RBL may be combined into a single wiring BIL. An example circuit configuration of such a memory cell is shown in FIG. 17D. The memory cell 954 is configured such that the wiring WBL and the wiring RBL of the memory cell 953 are combined into a single wiring BIL, and the second terminal of the transistor M2 and the first terminal of the transistor M3 are connected to the wiring BIL. In other words, the memory cell 954 is configured to operate as a write bit line and a read bit line using a single wiring BIL.
[0432] 17E is an example in which the capacitor element CB and the wiring CAL in the memory cell 953 are omitted. Also, a memory cell 956 in Fig. 17F is an example in which the capacitor element CB and the wiring CAL in the memory cell 954 are omitted. With such a configuration, the integration degree of the memory cells can be increased.
[0433] Note that it is preferable to use the OS transistor described in the above embodiment for at least the transistor M2. In particular, it is preferable to use the OS transistor described in the above embodiment for the transistor M2 and the transistor M3. By using the OS transistor described in the above embodiment, the area occupied by the memory cell can be reduced.
[0434] Since the OS transistor has an extremely low off-state current, written data can be held by the transistor M2 for a long time, which reduces the frequency of refreshing the memory cell. Alternatively, the refresh operation of the memory cell can be eliminated. Furthermore, since the leakage current is extremely low, multilevel data or analog data can be held in the memory cell 953, the memory cell 954, the memory cell 955, and the memory cell 956.
[0435] The memory cell 953, the memory cell 954, the memory cell 955, and the memory cell 956, in which an OS transistor is used as the transistor M2, are one embodiment of an NOSRAM.
[0436] Note that a Si transistor may be used as the transistor M3. The Si transistor can increase the field effect mobility and can also be used as a p-channel transistor, thereby increasing the degree of freedom in circuit design.
[0437] When an OS transistor is used as the transistor M3, the memory cell can be configured as a unipolar circuit.
[0438] 17G shows a three-transistor, one-capacitor gain cell type memory cell 957. The memory cell 957 includes transistors M4 to M6 and a capacitor CC.
[0439] The first terminal of the transistor M4 is connected to the first terminal of the capacitor CC, the second terminal of the transistor M4 is connected to the wiring BIL, and the gate of the transistor M4 is connected to the wiring WOL. The second terminal of the capacitor CC is electrically connected to the first terminal of the transistor M5 and the wiring GNDL. The second terminal of the transistor M5 is connected to the first terminal of the transistor M6, and the gate of the transistor M5 is connected to the first terminal of the capacitor CC. The second terminal of the transistor M6 is connected to the wiring BIL, and the gate of the transistor M6 is connected to the wiring RWL.
[0440] The wiring BIL functions as a bit line, the wiring WOL functions as a write word line, and the wiring RWL functions as a read word line. The wiring GNDL is a wiring that applies a low-level potential.
[0441] Data is written by applying a high-level potential to the wiring WOL, turning on the transistor M4, and connecting the wiring BIL to the first terminal of the capacitor CC. Specifically, when the transistor M4 is turned on, a potential corresponding to the information to be recorded is applied to the wiring BIL, and the potential is written to the first terminal of the capacitor CC and the gate of the transistor M5. Then, a low-level potential is applied to the wiring WOL, turning off the transistor M4, thereby maintaining the potential of the first terminal of the capacitor CC and the potential of the gate of the transistor M5.
[0442] Data is read by precharging the wiring BIL to a predetermined potential, then electrically floating the wiring BIL, and applying a high-level potential to the wiring RWL. Because the wiring RWL is at a high-level potential, the transistor M6 is turned on, and the wiring BIL and the second terminal of the transistor M5 are electrically connected. At this time, the potential of the wiring BIL is applied to the second terminal of the transistor M5. The potential of the second terminal of the transistor M5 and the potential of the wiring BIL change depending on the potential held in the first terminal of the capacitor CC (or the gate of the transistor M5). By reading the potential of the wiring BIL, the potential held in the first terminal of the capacitor CC (or the gate of the transistor M5) can be read. In other words, information written in this memory cell can be read from the potential held in the first terminal of the capacitor CC (or the gate of the transistor M5).
[0443] Note that it is preferable to use the OS transistor described in any of the above embodiments as at least the transistor M4, since the area occupied by the memory cell can be reduced by using the OS transistor described in any of the above embodiments.
[0444] Note that Si transistors may be used as the transistors M5 and M6. As described above, Si transistors may have higher field-effect mobility than OS transistors depending on the crystalline state of silicon used in the semiconductor layer.
[0445] When OS transistors are used as the transistors M5 and M6, the memory cell can be configured as a unipolar circuit.
[0446] 17H shows an example of an SRAM (Static Random Access Memory) using an OS transistor. In this specification and the like, an SRAM using an OS transistor is referred to as an OS-SRAM (Oxide Semiconductor-SRAM). Note that a memory cell 958 shown in FIG. 17H is a memory cell of an SRAM capable of backing up data.
[0447] The memory cell 958 includes transistors M7 to M10, transistors MS1 to MS4, and capacitors CD1 and CD2. Note that the transistors MS1 and MS2 are p-channel transistors, and the transistors MS3 and MS4 are n-channel transistors.
[0448] A first terminal of transistor M7 is connected to wiring BIL, and a second terminal of transistor M7 is connected to a first terminal of transistor MS1, a first terminal of transistor MS3, the gate of transistor MS2, the gate of transistor MS4, and a first terminal of transistor M10. The gate of transistor M7 is connected to wiring WOL. A first terminal of transistor M8 is connected to wiring BILB, and a second terminal of transistor M8 is connected to a first terminal of transistor MS2, the first terminal of transistor MS4, the gate of transistor MS1, the gate of transistor MS3, and a first terminal of transistor M9. The gate of transistor M8 is connected to wiring WOL.
[0449] A second terminal of the transistor MS1 is electrically connected to the wiring VDL. A second terminal of the transistor MS2 is electrically connected to the wiring VDL. A second terminal of the transistor MS3 is electrically connected to the wiring GNDL. A second terminal of the transistor MS4 is electrically connected to the wiring GNDL.
[0450] A second terminal of the transistor M9 is connected to a first terminal of the capacitor CD1, and a gate of the transistor M9 is connected to the wiring BRL. A second terminal of the transistor M10 is connected to a first terminal of the capacitor CD2, and a gate of the transistor M10 is connected to the wiring BRL.
[0451] A second terminal of the capacitance element CD1 is connected to the wiring GNDL, and a second terminal of the capacitance element CD2 is connected to the wiring GNDL.
[0452] The wirings BIL and BILB function as bit lines, the wiring WOL functions as a word line, and the wiring BRL is a wiring that controls the conductive state and non-conductive state of the transistors M9 and M10.
[0453] The wiring VDL is a wiring that applies a high-level potential, and the wiring GNDL is a wiring that applies a low-level potential.
[0454] Data is written by applying a high-level potential to the wiring WOL and a high-level potential to the wiring BRL. Specifically, when the transistor M10 is in a conductive state, a potential corresponding to information to be recorded is applied to the wiring BIL, and the potential is written to the second terminal of the transistor M10.
[0455] Since the memory cell 958 includes an inverter loop formed by the transistors MS1 and MS2, an inverted signal of the data signal corresponding to the potential is input to the second terminal of the transistor M8. Because the transistor M8 is conductive, the potential applied to the wiring BIL, i.e., the inverted signal of the signal input to the wiring BIL, is output to the wiring BILB. Furthermore, because the transistors M9 and M10 are conductive, the potentials of the second terminals of the transistors M7 and M8 are held in the first terminals of the capacitors CD2 and CD1, respectively. Subsequently, a low-level potential is applied to the wiring WOL and a low-level potential is applied to the wiring BRL to turn off the transistors M7 to M10, thereby holding the potentials of the first terminals of the capacitors CD1 and CD2.
[0456] Data is read by precharging the wirings BIL and BILB to a predetermined potential in advance, and then applying a high-level potential to the wiring WOL and a high-level potential to the wiring BRL, so that the potential of the first terminal of the capacitor CD1 is refreshed by the inverter loop of the memory cell 958 and output to the wiring BILB. Also, the potential of the first terminal of the capacitor CD2 is refreshed by the inverter loop of the memory cell 958 and output to the wiring BIL. In the wirings BIL and BILB, the potentials of the first terminal of the capacitor CD2 and the first terminal of the capacitor CD1 change from the precharged potentials, respectively, so that the potential held in the memory cell can be read from the potential of the wiring BIL or the wiring BILB.
[0457] Note that it is preferable to use OS transistors as the transistors M7 to M10. This allows written data to be held by the transistors M7 to M10 for a long time, thereby reducing the frequency of refreshing the memory cells. Alternatively, refreshing the memory cells can be eliminated. Furthermore, by using the OS transistors described in the above embodiment as the transistors M7 to M10, the area occupied by the memory cells can be reduced.
[0458] Note that Si transistors may be used as the transistors MS1 to MS4.
[0459] The driver circuit 910 and memory array 920 of the semiconductor device 900 may be provided on the same plane. Alternatively, as shown in FIG. 20A, the driver circuit 910 and memory array 920 may be provided overlapping each other. By providing the driver circuit 910 and memory array 920 overlapping each other, the signal propagation distance can be shortened. Alternatively, as shown in FIG. 20B, the memory array 920 may be provided in multiple layers on the driver circuit 910.
[0460] Here, an example of a structure in which multiple memory arrays are stacked over a driver circuit 910 will be described with reference to FIG. 21 . The memory device illustrated in FIG. 21 has a structure in which m (m is an integer greater than or equal to 2) memory arrays 920 each including memory cells 450 are stacked. Here, the layer provided in the first layer (bottom) is referred to as memory array 920[1], the layer provided in the second layer is referred to as memory array 920[2], and the layer provided in the mth layer (top) is referred to as memory array 920[m]. That is, the memory device of one embodiment of the present invention may have a structure in which multiple layers are stacked, including multiple layers each including memory cells 450. Furthermore, in each memory array 920, a conductor 446, a conductor 445, and a conductor 447 are provided, as in FIG. 19 .
[0461] 21 , the conductors 446, 445, and 447 function as wirings that connect the memory arrays 920 provided in the upper or lower layers to each other. For example, the conductor 240 of the memory array 920[2] is electrically connected to the conductor 240 of the memory array 920[1] via the conductors 445, 447, and 446. As shown in FIG. 21 , the conductors 446, 445, and 447 can be provided outside the memory array 920. Alternatively, the conductors 446, 445, and 447 may be provided inside the memory array 920.
[0462] Furthermore, a drive circuit 910 is provided below the memory array 920. By providing the drive circuit below the memory device in this manner, the area of the memory device can be increased, and the memory capacity of the memory device can be increased.
[0463] 21 illustrates a transistor 310 included in a driver circuit 910. The transistor 310 is provided over a substrate 311 and includes a conductor 316 functioning as a gate, an insulator 315 functioning as a gate insulator, a semiconductor region 313 including part of the substrate 311, and low-resistance regions 314a and 314b functioning as source and drain regions. An element isolation layer 318 is preferably provided between adjacent transistors 310. The transistor 310 may be either a p-channel transistor or an n-channel transistor. The substrate 311 may be, for example, a single-crystal silicon substrate.
[0464] Here, in the transistor 310 shown in FIG. 21 , a semiconductor region 313 (a part of a substrate 311) where a channel is formed has a convex shape. A conductor 316 is provided to cover the side and top surfaces of the semiconductor region 313 with an insulator 315 interposed therebetween. Note that the conductor 316 may be made of a material that adjusts the work function. Such a transistor 310 is also called a FIN-type transistor because it utilizes the convex portion of the semiconductor substrate. Note that an insulator may be provided in contact with the top of the convex portion and function as a mask for forming the convex portion. Here, the case where the convex portion is formed by processing a part of the semiconductor substrate is shown, but a semiconductor film having a convex shape may also be formed by processing an SOI (silicon-on-insulator) substrate.
[0465] Note that the transistor 310 illustrated in FIG. 21 is just an example, and the structure is not limited thereto. An appropriate transistor can be used depending on the circuit configuration or the driving method.
[0466] A wiring layer including an interlayer film, wiring, plugs, and the like may be provided between the memory array 920 and the drive circuit 910. Furthermore, multiple wiring layers may be provided depending on the design. Furthermore, in this specification and the like, wiring and a plug electrically connected to the wiring may be integrated. That is, there are cases where a part of a conductor functions as wiring, and cases where a part of a conductor functions as a plug.
[0467] For example, an insulator 320, an insulator 322, an insulator 324, and an insulator 326 are stacked in this order as an interlayer film over the transistor 310. A conductor 328 or the like is embedded in the insulators 320 and 322. A conductor 330 or the like is embedded in the insulators 324 and 326. The conductors 328 and 330 function as contact plugs or wirings.
[0468] The insulator functioning as an interlayer film may also function as a planarizing film that covers the underlying unevenness. For example, the top surface of the insulator 322 may be planarized by CMP processing to improve flatness.
[0469] Next, an example of a processing unit that can include a semiconductor device such as the memory device will be described.
[0470] 22 shows a block diagram of the arithmetic device 960. The arithmetic device 960 shown in FIG. 22 can be applied to, for example, a CPU. The arithmetic device 960 can also be applied to processors such as a GPU (Graphics Processing Unit), a TPU (Tensor Processing Unit), and an NPU (Neural Processing Unit) that have a larger number (several tens to several hundreds) of processor cores capable of parallel processing than a CPU.
[0471] The arithmetic device 960 shown in FIG. 22 has an ALU 991 (ALU: Arithmetic logic unit, arithmetic circuit), an ALU controller 992, an instruction decoder 993, an interrupt controller 994, a timing controller 995, a register 996, a register controller 997, a bus interface 998, a cache 999, and a cache interface 989 on a substrate 990. The substrate 990 may be a semiconductor substrate, an SOI substrate, a glass substrate, or the like. It may also have a rewritable ROM and a ROM interface. The cache 999 and the cache interface 989 may also be provided on separate chips.
[0472] The cache 999 is connected to a main memory provided on a separate chip via a cache interface 989. The cache interface 989 has a function of supplying part of the data held in the main memory to the cache 999. The cache interface 989 also has a function of outputting part of the data held in the cache 999 to the ALU 991, register 996, etc. via the bus interface 998.
[0473] As will be described later, a memory array 920 can be provided by stacking it on the arithmetic unit 960. The memory array 920 can be used as a cache. In this case, the cache interface 989 may have a function of supplying data held in the memory array 920 to the cache 999. In this case, it is preferable that a drive circuit 910 be included as part of the cache interface 989.
[0474] It is also possible to use only the memory array 920 as a cache without providing the cache 999 .
[0475] The arithmetic device 960 shown in FIG. 22 is merely an example of a simplified configuration, and actual arithmetic devices 960 have a wide variety of configurations depending on their applications. For example, it is preferable to use a configuration including the arithmetic device 960 shown in FIG. 22 as one core, and to include multiple such cores, each of which operates in parallel, in a so-called multi-core configuration. The greater the number of cores, the higher the computational performance. The greater the number of cores, for example, two, preferably four, more preferably eight, even more preferably twelve, and even more preferably sixteen or more. Furthermore, when extremely high computational performance is required, such as for server applications, a multi-core configuration with 16 or more, preferably 32 or more, and even more preferably 64 or more cores is preferable. Furthermore, the number of bits that the arithmetic device 960 can handle via its internal computation circuit, data bus, etc. can be, for example, 8 bits, 16 bits, 32 bits, or 64 bits.
[0476] An instruction input to the arithmetic unit 960 via the bus interface 998 is input to the instruction decoder 993, decoded, and then input to the ALU controller 992, interrupt controller 994, register controller 997, and timing controller 995.
[0477] The ALU controller 992, interrupt controller 994, register controller 997, and timing controller 995 perform various controls based on the decoded instructions. Specifically, the ALU controller 992 generates signals for controlling the operation of the ALU 991. Furthermore, the interrupt controller 994 determines and processes interrupt requests from external input / output devices, peripheral circuits, etc. based on their priority, mask status, etc. while the arithmetic unit 960 is executing a program. The register controller 997 generates an address for a register 996 and reads or writes data from or to the register 996 depending on the state of the arithmetic unit 960.
[0478] Furthermore, the timing controller 995 generates signals that control the timing of the operations of the ALU 991, the ALU controller 992, the instruction decoder 993, the interrupt controller 994, and the register controller 997. For example, the timing controller 995 includes an internal clock generation unit that generates an internal clock signal based on a reference clock signal, and supplies the internal clock signal to the various circuits described above.
[0479] 22, the register controller 997 selects the holding operation of the register 996 in accordance with an instruction from the ALU 991. That is, it selects whether the memory cells of the register 996 will hold data using flip-flops or using capacitive elements. If holding data using flip-flops is selected, a power supply voltage is supplied to the memory cells in the register 996. If holding data using capacitive elements is selected, the data is rewritten to the capacitive elements, and the supply of power supply voltage to the memory cells in the register 996 can be stopped.
[0480] The memory array 920 and the arithmetic unit 960 can be provided overlapping each other. Perspective views of a semiconductor device 970A are shown in Figures 23A and 23B. The semiconductor device 970A has a layer 930 on which memory arrays are provided above the arithmetic unit 960. The layer 930 is provided with memory arrays 920L1, 920L2, and 920L3. The arithmetic unit 960 and each memory array have overlapping regions. To make the configuration of the semiconductor device 970A easier to understand, the arithmetic unit 960 and the layer 930 are shown separately in Figure 23B.
[0481] By stacking the layer 930 having the memory array and the arithmetic unit 960, the connection distance between them can be shortened, thereby increasing the communication speed between them. In addition, the short connection distance reduces power consumption.
[0482] As a method for stacking the layer 930 having a memory array and the arithmetic device 960, a method (also called monolithic stacking) in which the layer 930 having a memory array is stacked directly on the arithmetic device 960 may be used, or a method in which the arithmetic device 960 and the layer 930 are formed on different substrates, the two substrates are bonded together, and the two substrates are electrically connected using a through-via or a conductive film bonding technique (such as Cu-Cu bonding) may be used. The former method does not require consideration of misalignment during bonding, and therefore can not only reduce the chip size but also reduce the manufacturing cost.
[0483] Here, the arithmetic unit 960 does not have a cache 999, and the memory arrays 920L1, 920L2, and 920L3 provided in the layer 930 can each be used as a cache. In this case, for example, the memory array 920L1 can be used as an L1 cache (also referred to as a level 1 cache), the memory array 920L2 can be used as an L2 cache (also referred to as a level 2 cache), and the memory array 920L3 can be used as an L3 cache (also referred to as a level 3 cache). Of the three memory arrays, the memory array 920L3 has the largest capacity and the lowest access frequency. Furthermore, the memory array 920L1 has the smallest capacity and the highest access frequency.
[0484] When the cache 999 provided in the arithmetic unit 960 is used as an L1 cache, each memory array provided in the layer 930 can be used as a lower-level cache or a main memory. The main memory has a larger capacity than the cache and is accessed less frequently.
[0485] 23B, a driving circuit 910L1, a driving circuit 910L2, and a driving circuit 910L3 are provided. The driving circuit 910L1 is connected to the memory array 920L1 via a connection electrode 940L1. Similarly, the driving circuit 910L2 is connected to the memory array 920L2 via a connection electrode 940L2, and the driving circuit 910L3 is connected to the memory array 920L3 via a connection electrode 940L3.
[0486] Although the number of memory arrays functioning as caches is three in this example, it may be one or two, or four or more.
[0487] When the memory array 920L1 is used as a cache, the driver circuit 910L1 may function as part of the cache interface 989, or may be configured to be connected to the cache interface 989. Similarly, the driver circuits 910L2 and 910L3 may also function as part of the cache interface 989, or may be configured to be connected thereto.
[0488] Whether the memory array 920 is made to function as a cache or as a main memory is determined by a control circuit 912 included in each drive circuit 910. The control circuit 912 can cause some of the memory cells 950 included in the semiconductor device 900 to function as RAM based on a signal supplied from the arithmetic device 960.
[0489] The semiconductor device 900 can cause some of the memory cells 950 to function as a cache and the other memory cells to function as a main memory. That is, the semiconductor device 900 can function as both a cache and a main memory. The semiconductor device 900 according to one embodiment of the present invention can function as, for example, a universal memory.
[0490] Furthermore, a layer 930 having one memory array 920 may be provided over the arithmetic device 960. Figure 24A shows a perspective view of a semiconductor device 970B.
[0491] In the semiconductor device 970B, one memory array 920 can be divided into multiple areas, each of which can be used for a different function. Figure 24A shows an example in which area L1 is used as an L1 cache, area L2 is used as an L2 cache, and area L3 is used as an L3 cache.
[0492] Furthermore, in the semiconductor device 970B, the capacity of each of the areas L1 to L3 can be changed depending on the situation. For example, if it is desired to increase the capacity of the L1 cache, this can be achieved by increasing the area of the area L1. This configuration can improve the efficiency of calculation processing and increase the processing speed.
[0493] Also, multiple memory arrays may be stacked. Figure 24B shows a perspective view of a semiconductor device 970C.
[0494] The semiconductor device 970C includes a layer 930L1 having a memory array 920L1, a layer 930L2 having a memory array 920L2 on top of that, and a layer 930L3 having a memory array 920L3 on top of that. The memory array 920L1, which is physically closest to the arithmetic unit 960, can be used as a higher-level cache, and the memory array 920L3, which is farthest, can be used as a lower-level cache or main memory. This configuration allows the capacity of each memory array to be increased, thereby further improving processing power.
[0495] Note that this embodiment mode can be appropriately combined with other embodiment modes and examples described in this specification.
[0496] Embodiment 3 In this embodiment, an application example of a memory device according to one embodiment of the present invention will be described.
[0497] Generally, various memory devices are used in semiconductor devices such as computers depending on the application. FIG. 25A shows various memory devices used in semiconductor devices by layer. The higher the layer, the faster the operating speed of the memory device is required, while the lower the layer, the larger the memory capacity and recording density are required. In FIG. 25A , from the top layer, there are memories embedded as registers in a processing unit such as a CPU, an L1 cache, an L2 cache, an L3 cache, a main memory, and storage. Note that while an example having up to an L3 cache is shown here, lower-level caches may also be included.
[0498] The memory embedded as a register in a processing unit such as a CPU is used for temporary storage of calculation results, and is therefore frequently accessed by the processing unit. Therefore, a higher operating speed is required than a larger memory capacity. Registers also have the function of storing setting information for the processing unit.
[0499] A cache has the function of duplicating and storing a portion of the data stored in main memory. By duplicating frequently used data and storing it in the cache, the access speed to the data can be increased. The storage capacity required for a cache is smaller than that of main memory, but it is required to operate faster than main memory. In addition, data rewritten in the cache is duplicated and supplied to main memory.
[0500] The main memory has a function of holding programs, data, etc. read from the storage.
[0501] Storage has the function of storing data that requires long-term storage and various programs used by processing units. Therefore, storage requires a large memory capacity and high recording density rather than an operating speed. For example, high-capacity, non-volatile storage devices such as 3D NAND can be used.
[0502] A storage device (OS memory) using an oxide semiconductor according to one embodiment of the present invention has high operating speed and can retain data for a long period of time. Therefore, as shown in FIG. 25A , the storage device according to one embodiment of the present invention can be suitably used in both a tier where a cache is located and a tier where a main memory is located. The storage device according to one embodiment of the present invention can also be applied to a tier where a storage is located.
[0503] FIG. 25B also shows an example in which an SRAM is used as part of a cache and an OS memory of one embodiment of the present invention is used as the other part of the cache.
[0504] The lowest level cache can be called a Last Level Cache (LLC). An LLC does not require faster operation speed than higher level caches, but it is desirable for it to have a large storage capacity. The OS memory of one embodiment of the present invention is suitable for use as an LLC because it operates quickly and can retain data for a long period of time. Note that the OS memory of one embodiment of the present invention can also be used as a Final Level Cache (FLC).
[0505] For example, as shown in Fig. 25B, a configuration can be adopted in which SRAM is used for the higher-level caches (L1 cache, L2 cache, etc.) and the OS memory according to one aspect of the present invention is used for the LLC. Also, as shown in Fig. 25B, not only the OS memory but also DRAM can be applied to the main memory.
[0506] Note that this embodiment mode can be appropriately combined with other embodiment modes and examples described in this specification.
[0507] In this embodiment, electronic components, electronic devices, mainframes, space equipment, and data centers (also referred to as data centers (DCs)) that can use the semiconductor device described in the above embodiment will be described. The electronic devices, mainframes, space equipment, and data centers that use the semiconductor device of one embodiment of the present invention are effective in achieving high performance, such as low power consumption.
[0508] [Electronic Device] Next, a perspective view of an electronic device 6500 is shown in FIG. 26A . The electronic device 6500 shown in FIG. 26A is a portable information terminal that can be used as a smartphone. The electronic device 6500 includes a housing 6501, a display portion 6502, a power button 6503, a button 6504, a speaker 6505, a microphone 6506, a camera 6507, a light source 6508, a control device 6509, and the like. Note that the control device 6509 includes, for example, one or more selected from a CPU, a GPU, and a memory device. The semiconductor device of one embodiment of the present invention can be applied to the display portion 6502, the control device 6509, and the like.
[0509] 26B is an information terminal that can be used as a laptop personal computer. The electronic device 6600 includes a housing 6611, a keyboard 6612, a pointing device 6613, an external connection port 6614, a display portion 6615, a control device 6616, and the like. Note that the control device 6616 includes, for example, one or more selected from a CPU, a GPU, and a memory device. The semiconductor device of one embodiment of the present invention can be applied to the display portion 6615, the control device 6616, and the like. Note that the use of the semiconductor device of one embodiment of the present invention in the control device 6509 and the control device 6616 is preferable because power consumption can be reduced.
[0510] [Mainframe] Next, Fig. 26C shows a perspective view of a mainframe 5600. The mainframe 5600 shown in Fig. 26C has a rack 5610 housing a plurality of rack-mounted computers 5620. The mainframe 5600 may also be called a supercomputer.
[0511] The computer 5620 can have the configuration shown in the perspective view in Fig. 26D, for example. In Fig. 26D, the computer 5620 has a motherboard 5630, which has a plurality of slots 5631 and a plurality of connection terminals. A PC card 5621 is inserted into the slot 5631. In addition, the PC card 5621 has connection terminals 5623, 5624, and 5625, which are each connected to the motherboard 5630.
[0512] PC card 5621 shown in Figure 26E is an example of a processing board equipped with a CPU, GPU, storage device, etc. PC card 5621 has board 5622. Board 5622 also has connection terminals 5623, 5624, 5625, semiconductor devices 5626, 5627, 5628, and 5629. Note that Figure 26E illustrates semiconductor devices other than semiconductor devices 5626, 5627, and 5628, but for these semiconductor devices, the following descriptions of semiconductor devices 5626, 5627, and 5628 can be referenced.
[0513] The connection terminal 5629 has a shape that allows it to be inserted into a slot 5631 of the motherboard 5630, and the connection terminal 5629 functions as an interface for connecting the PC card 5621 and the motherboard 5630. An example of the standard for the connection terminal 5629 is PCIe.
[0514] The connection terminals 5623, 5624, and 5625 can be, for example, interfaces for supplying power to the PC card 5621, inputting signals, etc. Furthermore, they can be, for example, interfaces for outputting signals calculated by the PC card 5621. Examples of the standards for the connection terminals 5623, 5624, and 5625 include USB, SATA (Serial ATA), and SCSI (Small Computer System Interface). Furthermore, when a video signal is output from the connection terminals 5623, 5624, and 5625, examples of the standards for each include HDMI (registered trademark).
[0515] The semiconductor device 5626 has a terminal (not shown) for inputting and outputting signals, and the semiconductor device 5626 and the board 5622 can be electrically connected by inserting the terminal into a socket (not shown) provided on the board 5622.
[0516] The semiconductor device 5627 has a plurality of terminals, and the semiconductor device 5627 can be electrically connected to the board 5622 by, for example, reflow soldering the terminals to wiring provided on the board 5622. Examples of the semiconductor device 5627 include an FPGA, a GPU, and a CPU.
[0517] The semiconductor device 5628 has a plurality of terminals, and the semiconductor device 5628 can be electrically connected to the board 5622 by, for example, reflow soldering the terminals to wiring provided on the board 5622. The semiconductor device 5628 is, for example, a memory device.
[0518] The mainframe computer 5600 can also function as a parallel computer. By using the mainframe computer 5600 as a parallel computer, it is possible to perform large-scale calculations required for, for example, learning and inference in artificial intelligence.
[0519] [Space Equipment] The semiconductor device of one embodiment of the present invention can be suitably used in space equipment such as equipment for processing and storing information.
[0520] The semiconductor device of one embodiment of the present invention can include an OS transistor. The OS transistor exhibits small changes in electrical characteristics due to radiation exposure. That is, the OS transistor has high radiation resistance and can be suitably used in an environment where radiation may be incident. For example, the OS transistor can be suitably used in outer space.
[0521] Fig. 27 shows an artificial satellite 6800 as an example of space equipment. The artificial satellite 6800 has a body 6801, a solar panel 6802, an antenna 6803, a secondary battery 6805, and a control device 6807. In Fig. 27, a planet 6804 is shown in outer space. Note that outer space refers to an altitude of 100 km or higher, for example, but the outer space described in this specification may also include the thermosphere, mesosphere, and stratosphere.
[0522] 27 , a battery management system (also referred to as a BMS) or a battery control circuit may be provided for the secondary battery 6805. The use of an OS transistor in the battery management system or the battery control circuit is preferable because it consumes low power and has high reliability even in space.
[0523] Furthermore, outer space is an environment with radiation levels 100 times higher than on Earth. Examples of radiation include electromagnetic waves (electromagnetic radiation) such as X-rays and gamma rays, and particle radiation such as alpha rays, beta rays, neutron rays, proton rays, heavy ion rays, and meson rays.
[0524] When sunlight is irradiated onto the solar panel 6802, the power required for the operation of the satellite 6800 is generated. However, for example, in a situation where sunlight is not irradiated onto the solar panel or where the amount of sunlight irradiating the solar panel is small, the generated power is small. Therefore, there is a possibility that the power required for the operation of the satellite 6800 will not be generated. In order to operate the satellite 6800 even in a situation where the generated power is small, it is preferable to provide a secondary battery 6805 on the satellite 6800. Note that the solar panel may be called a solar cell module.
[0525] The satellite 6800 can generate a signal. The signal is transmitted via an antenna 6803, and can be received by, for example, a receiver installed on the ground or another satellite. By receiving the signal transmitted by the satellite 6800, the position of the receiver that received the signal can be determined. As described above, the satellite 6800 can constitute a satellite positioning system.
[0526] The control device 6807 has a function of controlling the artificial satellite 6800. The control device 6807 is configured using, for example, one or more selected from a CPU, a GPU, and a storage device. Note that the semiconductor device of one embodiment of the present invention is preferably used for the control device 6807. An OS transistor has smaller fluctuations in electrical characteristics due to radiation exposure than a Si transistor. That is, an OS transistor has high reliability even in an environment where radiation may be incident, and can be preferably used.
[0527] The artificial satellite 6800 can also be configured to include a sensor. For example, by including a visible light sensor, the artificial satellite 6800 can have the function of detecting sunlight reflected from an object on the ground. Alternatively, by including a thermal infrared sensor, the artificial satellite 6800 can have the function of detecting thermal infrared rays emitted from the earth's surface. As described above, the artificial satellite 6800 can function as, for example, an earth observation satellite.
[0528] Although an artificial satellite is described as an example of space equipment in this embodiment, the present invention is not limited thereto. For example, the semiconductor device of one embodiment of the present invention can be suitably used in space equipment such as a spaceship, a space capsule, or a space probe.
[0529] As described above, OS transistors have excellent advantages over Si transistors, such as the ability to achieve a wide memory bandwidth and high radiation resistance.
[0530] [Data Center] The semiconductor device of one embodiment of the present invention can be suitably used in a storage system applied to, for example, a data center. The data center is required to perform long-term management of data, such as ensuring data immutability. To manage long-term data, the building must be large enough to install storage and servers for storing a huge amount of data, to ensure a stable power supply for maintaining the data, or to ensure cooling equipment required for maintaining the data.
[0531] By using the semiconductor device of one embodiment of the present invention in a storage system applied to a data center, it is possible to reduce the power required to store data and the size of the semiconductor device that stores data. Therefore, it is possible to reduce the size of the storage system, the size of the power supply for storing data, the scale of the cooling equipment, and the like. Therefore, it is possible to reduce the space required for the data center.
[0532] Furthermore, the semiconductor device of one embodiment of the present invention consumes less power, which allows heat generation from the circuit to be reduced. Therefore, adverse effects of the heat generation on the circuit itself, peripheral circuits, and modules can be reduced. Furthermore, by using the semiconductor device of one embodiment of the present invention, a data center that operates stably even in a high-temperature environment can be realized. Therefore, the reliability of the data center can be improved.
[0533] Fig. 28 shows a storage system applicable to a data center. The storage system 6900 shown in Fig. 28 has a plurality of servers 6901sb as hosts 6901 (illustrated as Host Computers). It also has a plurality of storage devices 6903md as storage 6903 (illustrated as Storage). The host 6901 and storage 6903 are shown connected via a storage area network 6904 (illustrated as SAN: Storage Area Network) and a storage control circuit 6902 (illustrated as Storage Controller).
[0534] The host 6901 corresponds to a computer that accesses data stored in the storage 6903. The hosts 6901 may be connected to each other via a network.
[0535] The storage 6903 uses flash memory to reduce the data access speed, i.e., the time required to store and output data, but this time is significantly longer than the time required for DRAM, which can be used as cache memory within the storage. In order to solve the problem of the long access speed of the storage 6903, a storage system typically provides cache memory within the storage to reduce the time required to store and output data.
[0536] The above-mentioned cache memory is used in the storage control circuit 6902 and the storage 6903. Data exchanged between the host 6901 and the storage 6903 is stored in the cache memory in the storage control circuit 6902 and the storage 6903, and then output to the host 6901 or the storage 6903.
[0537] By using OS transistors as transistors for storing data in the cache memory and holding a potential corresponding to the data, the frequency of refresh operations can be reduced, and power consumption can be reduced.
[0538] Note that the application of the semiconductor device of one embodiment of the present invention to any one or more selected from electronic components, electronic devices, mainframe computers, space equipment, and data centers is expected to have an effect of reducing power consumption. Therefore, while energy demand is expected to increase with the improvement in performance or high integration of semiconductor devices, the use of the semiconductor device of one embodiment of the present invention can contribute to the reduction of carbon dioxide (CO 2 Furthermore, the semiconductor device of one embodiment of the present invention is effective as a countermeasure against global warming because it consumes low power.
[0539] The structures, configurations, methods, and the like described in this embodiment can be used in appropriate combination with structures, configurations, methods, and the like described in other embodiment modes and examples.
[0540] Embodiment 5 In this embodiment, a structural example of a display device to which a transistor of one embodiment of the present invention can be applied will be described.
[0541] Since the transistor of one embodiment of the present invention can be made extremely small, a display device using the transistor of one embodiment of the present invention can have extremely high resolution. For example, the display device of one embodiment of the present invention can be used in a display portion of a wristwatch-type or bracelet-type information terminal (wearable device), a VR device such as a head-mounted display, and a head-mounted display (HMD), such as a glasses-type AR device.
[0542] 29A shows a perspective view of a display module 580. The display module 580 includes a display device 500A and an FPC 590. Note that the display panel included in the display module 580 is not limited to the display device 500A, and may be a display device 500C described later.
[0543] The display module 580 has a substrate 591 and a substrate 592. The display module 580 has a display unit 581. The display unit 581 is an area for displaying an image.
[0544] 29B is a perspective view schematically illustrating the configuration on the substrate 591 side. A circuit portion 582, a pixel circuit portion 583 on the circuit portion 582, and a pixel portion 584 on the pixel circuit portion 583 are stacked on the substrate 591. A terminal portion 585 for connecting to the FPC 590 is provided in a portion of the substrate 591 that does not overlap with the pixel portion 584. The terminal portion 585 and the circuit portion 582 are electrically connected by a wiring portion 586 composed of a plurality of wirings.
[0545] The pixel section 584 has a plurality of periodically arranged pixels 584a. An enlarged view of one pixel 584a is shown on the right side of Fig. 29B. The pixel 584a has a light-emitting element 110R that emits red light, a light-emitting element 110G that emits green light, and a light-emitting element 110B that emits blue light.
[0546] The pixel circuit portion 583 has a plurality of pixel circuits 583a arranged periodically. Each pixel circuit 583a is a circuit that controls the light emission of three light-emitting devices included in one pixel 584a. One pixel circuit 583a may be configured to have three circuits that control the light emission of one light-emitting device. For example, the pixel circuit 583a may be configured to have at least one selection transistor, one current control transistor (drive transistor), and a capacitor for each light-emitting device. In this case, a gate signal is input to the gate of the selection transistor, and a source signal is input to the source. This realizes an active matrix display panel.
[0547] The circuit portion 582 includes a circuit for driving each pixel circuit 583a of the pixel circuit portion 583. For example, it preferably includes one or both of a gate line driver circuit and a source line driver circuit. In addition, the circuit portion 582 may include at least one of an arithmetic circuit, a memory circuit, a power supply circuit, and the like. Furthermore, a transistor provided in the circuit portion 582 may constitute a part of the pixel circuit 583a. That is, the pixel circuit 583a may be composed of a transistor included in the pixel circuit portion 583 and a transistor included in the circuit portion 582.
[0548] The FPC 590 functions as wiring for supplying a video signal, a power supply potential, and the like from the outside to the circuit portion 582. An IC may be mounted on the FPC 590.
[0549] The display module 580 can be configured such that one or both of the pixel circuit portion 583 and the circuit portion 582 are provided overlapping below the pixel portion 584, thereby enabling the aperture ratio (effective display area ratio) of the display portion 581 to be extremely high. For example, the aperture ratio of the display portion 581 can be set to 40% or more and less than 100%, preferably 50% or more and 95% or less, and more preferably 60% or more and 95% or less. Furthermore, the pixels 584a can be arranged at extremely high density, enabling the resolution of the display portion 581 to be extremely high. For example, the pixels 584a are preferably arranged in the display portion 581 at a resolution of 2000 ppi or more, preferably 3000 ppi or more, more preferably 5000 ppi or more, and even more preferably 6000 ppi or more, and 20,000 ppi or less, or 30,000 ppi or less.
[0550] Because such a display module 580 has extremely high resolution, it can be suitably used in VR devices such as head-mounted displays, or eyeglass-type AR devices. For example, even in a configuration in which the display unit of the display module 580 is viewed through lenses, the display module 580 has an extremely high-resolution display unit 581, so even when the display unit is enlarged with lenses, the pixels are not visible, allowing for a highly immersive display. Furthermore, the display module 580 is not limited to this, and can be suitably used in electronic devices with relatively small display units. For example, it can be suitably used in the display unit of a wearable electronic device such as a wristwatch.
[0551] Display Device 500A A display device 500A shown in FIG. 30 includes a substrate 201, a light-emitting element 110R, a light-emitting element 110G, a light-emitting element 110B, a capacitor 140, and a transistor 520.
[0552] Substrate 201 corresponds to substrate 591 in FIG. 29A.
[0553] The transistor 520 is a vertical channel transistor in which an oxide semiconductor is used for a semiconductor layer in which a channel is formed, and includes an oxide semiconductor 230, an insulator 250, a conductor 260, a conductor 240, a conductor 220, and the like.
[0554] The transistor 520 can be any of the various transistors described as examples in Embodiment 1. For example, as shown in FIG.
[0555] An insulator 210 is provided over the substrate 201. The insulator 210 functions as a barrier layer that prevents impurities such as water or hydrogen from diffusing from the substrate 201 to the transistor 520 and prevents oxygen from being released from the oxide semiconductor 230 toward the insulator 210. As the insulator 210, for example, a film through which hydrogen or oxygen is less likely to diffuse than a silicon oxide film, such as an aluminum oxide film, a hafnium oxide film, or a silicon nitride film, can be used.
[0556] Further, an insulator 222 is provided over the insulator 210. The insulator 222 functions as an insulating film that captures or fixes hydrogen contained in the insulator 280, the oxide semiconductor 230, and the like. As the insulator 222, for example, a hafnium silicate film can be used.
[0557] The conductor 220 and the insulator 280 are provided over the insulator 222, and the conductor 240 is provided over the insulator 280. An opening is provided in the insulator 280, and the oxide semiconductor 230, the insulator 250, and the conductor 260 are provided in the opening. An insulator 270 is provided to cover the conductor 240 and the oxide semiconductor 230. An insulating layer 164 is provided to cover the conductor 260.
[0558] The insulating layer 164 functions as an interlayer insulating layer. A barrier layer that prevents impurities such as water or hydrogen from diffusing from the insulating layer 164 or the like to the transistor 520 may be provided between the insulating layer 164 and the insulating layer 154. As the barrier layer, an insulating film similar to that of the insulator 210 can be used.
[0559] A plug 174 electrically connected to one side of the conductor 240 is provided so as to be embedded in the insulating layer 164. Here, the plug 174 preferably has a conductive layer 174a that covers the side surface of the opening in the insulating layer 164 and part of the upper surface of the conductor 240, and a conductive layer 174b that contacts the upper surface of the conductive layer 174a. In this case, it is preferable to use a conductive material that is difficult for hydrogen and oxygen to diffuse into as the conductive layer 174a.
[0560] Furthermore, a capacitor 140 is provided on the insulating layer 164. The capacitor 140 has a conductive layer 141, a conductive layer 145, and an insulating layer 143 located therebetween. The conductive layer 141 functions as one electrode of the capacitor 140, the conductive layer 145 functions as the other electrode of the capacitor 140, and the insulating layer 143 functions as a dielectric of the capacitor 140.
[0561] The conductive layer 141 is provided over the insulating layer 164 and is buried in the insulating layer 154. The conductive layer 141 is electrically connected to a conductor 240 of the transistor 520 by a plug 174. The insulating layer 143 is provided to cover the conductive layer 141. The conductive layer 145 is provided in a region overlapping with the conductive layer 141 with the insulating layer 143 interposed therebetween.
[0562] An insulating layer 155a is provided to cover the capacitor 140, an insulating layer 155b is provided over the insulating layer 155a, and an insulating layer 155c is provided over the insulating layer 155b.
[0563] An inorganic insulating film can be preferably used for each of the insulating layers 155a, 155b, and 155c. For example, it is preferable to use a silicon oxide film for the insulating layer 155a and the insulating layer 155c, and a silicon nitride film for the insulating layer 155b. This allows the insulating layer 155b to function as an etching protection film. In this embodiment, an example is shown in which part of the insulating layer 155c is etched to form a recess, but the insulating layer 155c does not necessarily have to have a recess.
[0564] The light emitting elements 110R, 110G, and 110B are provided on the insulating layer 155c.
[0565] The light-emitting element 110R has a pixel electrode 111R, an organic layer 112R, a common layer 114, and a common electrode 113. The light-emitting element 110G has a pixel electrode 111G, an organic layer 112G, a common layer 114, and a common electrode 113. The light-emitting element 110B has a pixel electrode 111B, an organic layer 112B, a common layer 114, and a common electrode 113. The common layer 114 and the common electrode 113 are provided in common to the light-emitting element 110R, the light-emitting element 110G, and the light-emitting element 110B.
[0566] The organic layer 112R of the light-emitting element 110R contains a light-emitting organic compound that emits at least red light. The organic layer 112G of the light-emitting element 110G contains a light-emitting organic compound that emits at least green light. The organic layer 112B of the light-emitting element 110B contains a light-emitting organic compound that emits at least blue light. The organic layer 112R, the organic layer 112G, and the organic layer 112B can also be called EL layers, and each contains at least a layer (light-emitting layer) that contains a light-emitting organic compound.
[0567] The display device 500A has a separate light-emitting device for each emitted color, so there is little change in chromaticity between light emitted at low and high luminance. Furthermore, because the organic layers 112R, 112G, and 112B are spaced apart from one another, crosstalk between adjacent subpixels can be suppressed even in a high-resolution display panel. This makes it possible to realize a high-resolution, high-quality display panel.
[0568] In the region between adjacent light emitting elements, an insulating layer 125, a resin layer 126, and a layer 128 are provided.
[0569] The pixel electrodes 111R, 111G, and 111B of the light-emitting element are electrically connected to the conductor 240 of the transistor 520 via a plug 156 embedded in the insulating layers 155a, 155b, and 155c, a conductive layer 141 embedded in the insulating layer 154, and a plug 174. The height of the top surface of the insulating layer 155c and the height of the top surface of the plug 156 are the same or approximately the same. Various conductive materials can be used for the plug.
[0570] A protective layer 121 is provided on the light emitting elements 110R, 110G, and 110B. A substrate 170 is attached to the protective layer 121 with an adhesive layer 171.
[0571] There is no insulating layer covering the upper end of each pixel electrode 111 between two adjacent pixel electrodes 111. This allows the distance between adjacent light-emitting elements to be extremely narrow, resulting in a high-definition or high-resolution display device.
[0572] [Display Device 500C] A display device 500C shown in FIG. 31 has a stacked structure of a transistor 310 having a channel formed in a semiconductor substrate and a vertical channel transistor 520.
[0573] Similar to the transistor 310 shown in FIG. 21 , the transistor 310 has a channel formation region in a substrate 311. The substrate 311 can be, for example, a semiconductor substrate such as a single crystal silicon substrate. The transistor 310 includes a part of the substrate 311, a conductor 316, a low-resistance region 314 a, a low-resistance region 314 b, an insulator 315, and an insulator 317. The conductor 316 functions as a gate electrode. The insulator 315 is located between the substrate 311 and the conductor 316 and functions as a gate insulating layer. The low-resistance region 314 a and the low-resistance region 314 b are regions in the substrate 311 doped with impurities. The low-resistance region 314 a functions as one of a source and a drain, and the low-resistance region 314 b functions as the other of the source and the drain. The insulator 317 is provided to cover a side surface of the conductor 316.
[0574] Furthermore, an element isolation layer 318 is provided between two adjacent transistors 310 so as to be embedded in the substrate 311 .
[0575] This embodiment mode can be implemented by appropriately combining at least a part thereof with other embodiment modes and examples described in this specification.
[0576] In this embodiment, a structural example of a display device that can be applied to a display device manufactured using a transistor of one embodiment of the present invention will be described. The display device exemplified below can be applied to the pixel portion 584 in Embodiment 5, for example.
[0577] One embodiment of the present invention is a display device having a light-emitting element (also referred to as a light-emitting device). The display device has two or more pixels that emit light of different colors. Each pixel has a light-emitting element. Each light-emitting element has a pair of electrodes and an EL layer therebetween. The light-emitting element is preferably an organic EL element (organic electroluminescent element). Two or more light-emitting elements that emit light of different colors each have an EL layer containing a different light-emitting material. For example, a full-color display device can be realized by having three types of light-emitting elements that emit red (R), green (G), or blue (B) light, respectively.
[0578] When fabricating a display device having multiple light-emitting elements that emit different colors of light, it is necessary to form at least one layer containing a light-emitting material (light-emitting layer) in an island shape. When fabricating a partial or entire EL layer, a method of forming island-shaped organic films by vapor deposition using a shadow mask such as a metal mask is known. However, this method can cause deviations in the shape and position of the island-shaped organic films from the design due to various factors such as the accuracy of the metal mask, misalignment between the metal mask and the substrate, deflection of the metal mask, and spreading of the contours of the deposited film due to vapor scattering, making it difficult to achieve high-definition and high-aperture display devices. Furthermore, during vapor deposition, the contours of the layer can become blurred, resulting in thinning of the edges. In other words, the thickness of the island-shaped light-emitting layer can vary depending on the location. Furthermore, when fabricating large, high-resolution, or high-definition display devices, there is a concern that low dimensional accuracy of the metal mask and deformation due to heat, etc., can reduce manufacturing yield. Therefore, measures have been taken to artificially increase the resolution (also known as pixel density) by adopting special pixel arrangements such as a pentile array.
[0579] In this specification, the term "island-like" refers to a state in which two or more layers formed using the same material in the same process are physically separated. For example, an island-like light-emitting layer refers to a state in which the light-emitting layer is physically separated from an adjacent light-emitting layer.
[0580] In one embodiment of the present invention, an EL layer is processed into a fine pattern by photolithography without using a shadow mask such as a fine metal mask (FMM). This makes it possible to realize a display device with high definition and a large aperture ratio, which have been difficult to achieve until now. Furthermore, because the EL layer can be individually fabricated, a display device with extremely vivid images, high contrast, and high display quality can be realized. Note that, for example, the EL layer may be processed into a fine pattern using both a metal mask and photolithography.
[0581] Furthermore, the EL layer can be partially or entirely separated physically. This can suppress leakage current between adjacent light-emitting elements through a layer shared between the light-emitting elements (also referred to as a common layer). This can prevent unintended light emission due to crosstalk, thereby realizing a display device with extremely high contrast. In particular, a display device with high current efficiency at low luminance can be realized.
[0582] One embodiment of the present invention can also be a display device that combines a white-emitting light-emitting element and a color filter. In this case, light-emitting elements provided in pixels (subpixels) that emit light of different colors can have the same configuration, and all layers can be common layers. Furthermore, part or all of each EL layer can be separated by photolithography. This suppresses leakage current through the common layer, thereby achieving a display device with high contrast. In particular, in an element having a tandem structure in which multiple light-emitting layers are stacked via a highly conductive intermediate layer, leakage current through the intermediate layer can be effectively prevented, thereby achieving a display device that combines high brightness, high definition, and high contrast.
[0583] When the EL layer is processed by photolithography, a portion of the light-emitting layer may be exposed, which may cause deterioration. Therefore, it is preferable to provide an insulating layer that covers at least the side surfaces of the island-shaped light-emitting layer. The insulating layer may also be configured to cover a portion of the top surface of the island-shaped EL layer. The insulating layer is preferably made of a material that has barrier properties against water and oxygen. For example, an inorganic insulating film that is less likely to diffuse water or oxygen can be used. This suppresses deterioration of the EL layer, thereby achieving a highly reliable display device.
[0584] Furthermore, there is a region (recess) between two adjacent light-emitting elements where the EL layer of either light-emitting element is not provided. When a common electrode, or a common electrode and a common layer, is formed to cover the recess, a phenomenon in which the common electrode is separated by a step at the edge of the EL layer (also called a step discontinuity) may occur, resulting in insulation of the common electrode on the EL layer. Therefore, it is preferable to use a configuration in which the local step located between two adjacent light-emitting elements is filled with a resin layer functioning as a planarization film (also called LFP: Local Filling Planarization). The resin layer functions as a planarization film. This suppresses step discontinuity of the common layer or common electrode, thereby achieving a highly reliable display device.
[0585] A more specific example of the structure of the display device of one embodiment of the present invention will be described below with reference to the drawings.
[0586] 32A shows a schematic top view of a di...
Claims
a transistor and a first insulator; the transistor includes a first conductor, a second conductor on the first conductor and the first insulator, an oxide semiconductor, a second insulator, and a third conductor; the first insulator and the second conductor are provided with an opening reaching the first conductor; the first conductor is provided with a recess overlapping the opening, a portion of the oxide semiconductor, a portion of the second insulator, and a portion of the third conductor are provided in the recess; the oxide semiconductor is in contact with the first conductor and the second conductor; the second insulator is disposed on the oxide semiconductor and in contact with at least a portion of an upper surface of the first conductor; the third conductor is disposed on the second insulator. Semiconductor device. In claim 1, At least a part of a bottom surface of the oxide semiconductor is removed in the recess. Semiconductor device. In claim 2, a lower surface of the third conductor is lower than an upper surface of a region of the first conductor that does not overlap with the opening; Semiconductor device. In claim 1, the second conductor has a first layer and a second layer on the first layer; the first layer comprises a metal oxide; the second layer being more conductive than the first layer; Semiconductor device. In claim 4, the first layer comprises indium; Semiconductor device. In claim 5, The first layer comprises tin and silicon. Semiconductor device. In claim 4, the second layer comprises tungsten; Semiconductor device. In claim 4, a side surface of the first layer on the opening side is located closer to the opening side than a side surface of the second layer on the opening side; Semiconductor device. In claim 8, the oxide semiconductor is in contact with a side surface of the first layer on the opening side and a part of an upper surface of the first layer; Semiconductor device. In claim 9, a third insulator disposed between the second layer and the third conductor; Semiconductor device. In any one of claims 1 to 10, the first conductor has a third layer and a fourth layer on the third layer; the third layer being more conductive than the fourth layer; the fourth layer comprises a metal oxide; Semiconductor device. In claim 11, the third layer comprises tungsten; Semiconductor device. In claim 12, the fourth layer comprises indium; Semiconductor device. In claim 13, the fourth layer comprises tin and silicon; Semiconductor device. In claim 11, the opening reaches the third layer; Semiconductor device. a transistor and a first insulator; the transistor includes a first conductor provided over a base insulator, a second conductor over the first conductor and the first insulator, an oxide semiconductor, a second insulator, and a third conductor; the first conductor, the first insulator, and the second conductor are provided with openings reaching the underlying insulator; a portion of the oxide semiconductor, a portion of the second insulator, and a portion of the third conductor are provided in the opening; the oxide semiconductor is in contact with the first conductor and the second conductor; the second insulator is disposed on the oxide semiconductor and in contact with at least a portion of an upper surface of the underlying insulator; the third conductor is disposed on the second insulator. Semiconductor device.
Citation Information
Patent Citations
Thin-film semiconductor device
JP1991291973A
Semiconductor device, and manufacturing method for the same
JP2016149552A
Semiconductor device and manufacturing method thereof