Metal recovery method
The method of heat treatment, crushing, and eddy current sorting addresses the inefficiency in cobalt and nickel recovery from lithium-ion battery waste by separating impurities, thereby improving the recovery rate of these valuable metals.
Patent Information
- Application Number
- PCT/JP2024/000199
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-01-09
- Publication Date
- 2024-11-28
AI Technical Summary
Current methods for recovering cobalt and nickel from lithium-ion battery waste are inefficient due to the entanglement of magnetic cobalt and nickel with non-magnetic aluminum and copper, leading to insufficient separation and reduced recovery rates.
A method involving heat treatment, crushing, sieving, and eddy current sorting to separate impurity metals from medium-diameter sieved materials, allowing for the effective extraction of cobalt and nickel by distinguishing between magnetic and non-magnetic conductive materials.
This method improves the recovery rate of cobalt and nickel by effectively separating impurities like aluminum and copper, enhancing the overall efficiency of metal recovery from lithium-ion battery waste.
Smart Images

Figure JP2024000199_28112024_PF_FP_ABST
Abstract
Description
Metal recovery method
[0001] This specification relates to a method for recovering metals, including at least one of cobalt and nickel, from lithium ion battery waste.
[0002] Vehicles such as hybrid vehicles, fuel cell vehicles, and electric vehicles are equipped with an in-vehicle battery pack that supplies power to an electric motor as a drive source (see, for example, Patent Documents 1 to 6). In an in-vehicle battery pack, battery cells may be housed inside a frame that forms the skeleton of the exterior. Note that many in-vehicle battery packs are configured by bundling multiple battery cells into a battery module, and then connecting multiple battery modules together. In addition, an in-vehicle battery pack may further include a battery management system (BMS) that monitors each battery cell, a cooling device that cools the battery, wires that connect them, etc.
[0003] The battery cells of the above-mentioned automotive battery packs generally use secondary batteries, particularly nickel-metal hydride batteries, which can store electricity by charging and be used repeatedly. However, in recent years, lithium-ion batteries using lithium-transition metal composite oxides for the positive electrode have been increasingly used. Furthermore, such automotive lithium-ion batteries contain valuable metals such as cobalt. Therefore, when automotive lithium-ion batteries are discarded after use, it is desirable to easily recover the valuable metals that may be contained in the lithium-ion battery waste at a relatively low cost for reuse, from the perspective of effective resource utilization.
[0004] When recovering valuable metals from lithium-ion battery waste, not just from in-vehicle batteries, the lithium-ion battery waste may be pretreated to obtain battery powder containing as much of the metals of the positive electrode active material as possible while removing metals that are not subject to recovery as impurities. This is followed by a wet treatment in which the metals in the battery powder are leached with an acid or the like, and various metals are recovered from the resulting leaching solution.
[0005] JP 2006-179190 A JP 2007-172938 A U.S. Patent Application Publication No. 2007 / 0141454 JP 2007-172939 A U.S. Patent Application Publication No. 2007 / 0141455 JP 2011-198713 A
[0006] In the pretreatment for obtaining battery powder from lithium-ion battery waste, a sieving process is performed after a heat treatment process, a crushing process, etc. Small-diameter sieved matter having a relatively small particle size obtained in the sieving process can be effectively used to recover metals as battery powder by wet processing. In addition, large-diameter sieved matter having a relatively large particle size obtained in the sieving process can be subsequently subjected to a predetermined process and then included in the battery powder and subjected to wet processing.
[0007] On the other hand, the medium-sized sieved matter, which is selected in the sieving process as having a particle size intermediate between the small-sized and large-sized sieved matter, contains valuable metals such as nickel and cobalt, and it is desirable to recover these metals. However, since the medium-sized sieved matter contains relatively large amounts of impurity metals such as aluminum and copper, it is necessary to perform some appropriate treatment before it can be included in the battery powder.
[0008] This specification provides a metal recovery method that can effectively separate impurity metals from the medium-sized sieve fraction obtained by sieving and improve the recovery rate of cobalt and / or nickel.
[0009] The metal recovery method described in this specification is a method for recovering metals containing at least one of cobalt and nickel from lithium ion battery waste, and includes a heat treatment step in which the lithium ion battery waste is subjected to heat treatment, a crushing step in which the lithium ion battery waste after the heat treatment step is crushed to obtain crushed material, a sieving step in which the crushed material is separated by sieving into at least small-diameter screened material having a relatively small particle size, large-diameter screened material having a relatively large particle size, and medium-diameter screened material having a particle size intermediate between the small-diameter screened material and the large-diameter screened material, and an eddy current separation step in which non-magnetic conductive material is separated from the medium-diameter screened material by eddy current separation, and magnetic material containing at least one of cobalt and nickel is extracted as magnetic material, and the metal is recovered from battery powder containing the small-diameter screened material and the magnetic material.
[0010] According to the above-described metal recovery method, impurity metals can be effectively separated from the medium-sized sieved matter obtained by sieving, and the recovery rate of cobalt and / or nickel can be improved.
[0011] Fig. 1 is a flow chart showing a metal recovery method of one embodiment; Fig. 2 is a flow chart showing a metal recovery method of another embodiment; Fig. 3 is a photograph showing an example of lithium ion battery waste before and after a heat treatment process; Fig. 4 is a schematic diagram showing an example of an eddy current separator that can be used in an eddy current separation process; Fig. 5 is a schematic diagram showing retained matter above the pulley of the eddy current separator and a modified belt for preventing this;
[0012] An embodiment of the metal recovery method described above will be described in detail below. The metal recovery method of one embodiment is a method for recovering metals containing at least one of cobalt and nickel from lithium ion battery waste.
[0013] 1 and 2, this metal recovery method includes a heat treatment step of heat treating lithium ion battery waste, a crushing step of crushing the lithium ion battery waste after the heat treatment step to obtain crushed material, and a sieving step of separating the crushed material into at least three types of sieved material having different particle sizes by sieving. The three types of sieved material separated in the sieving step are small-diameter sieved material having a relatively small particle size, large-diameter sieved material having a relatively large particle size, and medium-diameter sieved material having a particle size intermediate between the small-diameter sieved material and the large-diameter sieved material. Regarding the classification of small-diameter sieved materials, medium-diameter sieved materials, and large-diameter sieved materials by particle size, when sieving using a sieve having lattice-shaped sieve holes with a specified side length, the sieved materials that pass through the sieve have a particle size that is equal to or greater than the specified side length of the sieve holes, and the sieved materials that pass through the sieve have a particle size that is less than the side length of the sieve holes.
[0014] Among these, if the medium-sized sieved material is included in the battery powder as is, the purity of aluminum and copper, which are impurity metals in the battery powder, will increase. On the other hand, if the medium-sized sieved material is not included in the battery powder at all, the cobalt and / or nickel contained in the medium-sized sieved material will be lost. Therefore, it is necessary to separate the aluminum and copper from the medium-sized sieved material and recover the cobalt and / or nickel. However, high-intensity magnetic separators have not been able to sufficiently separate the aluminum and copper. This is presumably because the particle size of the medium-sized sieved material is relatively small, and the magnetic cobalt and nickel entrap the non-magnetic aluminum and copper, resulting in insufficient separation.
[0015] Therefore, in this embodiment, an eddy current separation process is performed on the medium-sized sieved material, and non-magnetic conductive materials are separated from the medium-sized sieved material by eddy current separation, and magnetic materials containing at least one of cobalt and nickel are extracted as magnetic materials. This allows aluminum and copper to be effectively separated from cobalt and / or nickel. By including the magnetic materials extracted in the eddy current separation process in the battery powder, the recovery rate of cobalt and nickel is improved. In some cases, the recovery rate of lithium can also be further improved.
[0016] (Lithium-ion battery waste) Lithium-ion battery waste can be various automotive lithium-ion batteries that can be installed in vehicles such as hybrid cars, fuel cell cars, and electric cars, discarded due to vehicle scrapping, battery replacement, manufacturing defects, or other reasons. However, it is not limited to automotive lithium-ion battery waste, and can also include various lithium-ion battery waste for other uses. Lithium-ion battery waste refers to lithium-ion batteries that are eligible for recycling, regardless of whether the lithium-ion batteries are traded for a value, free of charge, or treated as industrial waste.
[0017] The lithium-ion batteries contained in such lithium-ion battery waste include cathode materials, anode materials, and electrolytes, as well as the surrounding aluminum casings. The cathode materials and anode materials may be formed by adhering a cathode active material or an anode active material to a cathode current collector such as aluminum foil or an anode current collector such as copper foil, respectively, using, for example, polyvinylidene fluoride (PVDF) or other organic binders. The cathode active material may be, for example, a single metal oxide of lithium, nickel, cobalt, or manganese, or a composite metal oxide of two or more of these metals. Examples of such cathode active materials include LiCoO2, LiNiO2, Li-Co-Ni-O2, and Li-Co-Ni-Mn-O. It is desirable to recover the metals contained in the cathode active material as valuable metals in order to effectively utilize resources. In this embodiment, the metals contained in the positive electrode active material may change form from the oxides described above during a heat treatment process or the like, as described below. Regardless of their form, the metals derived from the positive electrode active material (hereinafter also referred to as "positive electrode-derived metals"), at least cobalt and / or nickel, are targeted for recovery. Lithium may also be targeted for recovery. Carbon-based materials are often used as negative electrode active materials, and electrolytic solutions such as ethylene carbonate or diethyl carbonate are often used as electrolytes. Furthermore, automotive lithium-ion battery waste may include terminals containing copper and / or iron, iron housings, stainless steel housings, etc.
[0018] As shown in FIG. 3 , automotive lithium-ion battery waste has an iron-containing metal frame as the exterior skeleton, with lithium-ion battery cells housed within the frame. The metal constituting the frame may be primarily iron. This type of lithium-ion battery waste often includes multiple battery cells, bundled together to form a battery module, which is then connected to each other. The lithium-ion battery waste may also include a battery management system (BMS) that monitors each battery cell, a cooling device that cools the battery, and wires connecting them. The wires may be made of a copper-containing metal, such as copper (Cu wire), and are connected to each battery cell and the BMS to transmit information about the temperature, voltage, etc. of each battery cell to the BMS. Furthermore, resin materials containing glass fibers may be provided between or around the battery cells. The glass fibers may contain calcium and / or magnesium.
[0019] In the heat treatment process, the lithium-ion battery waste described above is heated in a heat treatment furnace without being dismantled. Because the lithium-ion battery waste for vehicles has a rigid structure, it is not easy to dismantle it before the heat treatment. Furthermore, dismantling it before the heat treatment poses a risk of electric shock due to residual voltage.
[0020] The heat treatment can convert metals such as lithium and cobalt contained in the lithium-ion battery waste into a form that is easily dissolved by leaching with water or acid in wet processing. In addition, the heat treatment removes the electrolyte from the lithium-ion battery waste, and also pulverizes resin materials that may be contained inside the frames of the lithium-ion battery waste, turning them into resin powder.
[0021] During the heat treatment, the lithium-ion battery waste is preferably heated at a temperature of 350°C to 650°C for 1 hour to 8 hours. This may convert the positive electrode active material in the lithium-ion battery waste to at least one of metallic cobalt (Co) and cobalt oxide (CoO). The positive electrode active material may also be converted to at least one of metallic nickel (Ni) and nickel oxide (NiO, etc.). While the positive electrode active material is not magnetic, metallic cobalt and metallic nickel are magnetic. Therefore, by adjusting the heating temperature, the magnetic material can contain the metallic cobalt and / or metallic nickel in the subsequent magnetic separation and eddy current separation processes, thereby improving the recovery rate of cobalt and nickel. If the heating temperature is too low, there are concerns that the decomposition of lithium metal oxide and the reduction of the nickel oxide and cobalt oxide obtained after the decomposition may be insufficient, and that organic matter such as the electrolyte may not be sufficiently removed. On the other hand, if the heating temperature is too high, the aluminum of the aluminum foil may melt, resulting in a large amount of impurities being mixed in during the wet treatment. From this viewpoint, it is more preferable that the heating temperature be 400°C to 600°C.
[0022] Furthermore, if the heating temperature is maintained for a short period of time, the heat treatment may not be sufficient, especially for waste automotive lithium-ion batteries with a sturdy structure surrounded by a metal frame, and a large amount of organic matter may remain. However, if the holding time is too long, depending on the atmosphere, various components may oxidize and become brittle, potentially contaminating the battery powder as impurities. Therefore, a holding time of 2 to 9 hours is more preferable. The holding time may be 6 to 9 hours or 2 to 4 hours.
[0023] The heating during roasting can be performed in, for example, air or an inert atmosphere, but various atmospheres are also possible. In particular, heating in an inert atmosphere prevents the combustion of the flammable electrolyte, thereby suppressing melting of the battery cell casing and the generation of lithium aluminate (LiAlO). If lithium aluminate is generated, the aluminum foil becomes brittle and is more likely to be mixed into the battery powder. On the other hand, aluminum foil that has not reacted to form lithium aluminate can be easily separated in a subsequent sieving process. Thus, heating in an inert atmosphere is advantageous in that it can prevent aluminum from being mixed into the battery powder. Heating in an air atmosphere can reach relatively high temperatures under certain conditions, which can lead to melting of the casing and pulverization of the aluminum foil. Furthermore, oxygen in the air can react with the aluminum foil and the lithium metal from the positive electrode to produce lithium aluminate, which can then be mixed into the battery powder. An increase in the aluminum content in the battery powder can increase the loss of cobalt and nickel during subsequent wet processing to remove the aluminum. Furthermore, if the battery cell housing is prevented from melting by heating in an inert atmosphere, it becomes easier to remove the resin powder containing magnesium and calcium derived from the resin member in the component removal process described below. Therefore, it is desirable to heat in an inert atmosphere.
[0024] Specifically, the heat treatment in an inert atmosphere can be performed in an atmosphere containing at least one selected from the group consisting of nitrogen, carbon dioxide, and water vapor. Among these, an atmosphere containing primarily nitrogen is preferred. The heat treatment can be performed while flowing such an inert gas. A trace amount of oxygen may be present. Furthermore, by sufficiently reducing the oxygen concentration, embrittlement of aluminum in battery waste can be suppressed. Embrittlement of aluminum during heat treatment may lead to concerns about poor separability of the aluminum during the sieving process described below. When an inert gas is introduced into the heat treatment furnace, the oxygen concentration in the heat treatment furnace is set to, for example, 0.05% to 4.00% by volume, preferably less than 1% by volume, and more preferably less than 0.1% by volume.
[0025] After heating in an inert atmosphere, it is preferable to switch the atmosphere and further heat in an air atmosphere. Heating in an air atmosphere can suppress foaming that occurs when the battery powder is leached with acid in the subsequent wet treatment leaching step. Heating in an air atmosphere can also remove tar resulting from resin decomposition in the heat treatment furnace or duct. However, it is important to oxidize the aluminum to a degree that does not embrittle it.
[0026] The heat treatment furnace used to heat the lithium-ion battery waste is not particularly limited, but for example, an atmospheric electric furnace or atmospheric muffle furnace can be used for a batch type, or a roller hearth kiln or mesh belt kiln can be used for a continuous type. Among these, roller hearth kilns and pusher kilns are preferred because they are suitable for large-scale treatment.
[0027] (Component Removal Step) After the heat treatment step, a component removal step can be carried out to remove predetermined components from the lithium ion battery waste.
[0028] In the component removal process, iron-containing metal (typically SUS) frames can be removed from the lithium-ion battery waste. This allows most of the iron contained in the lithium-ion battery waste to be removed, significantly reducing the amount of iron mixed into the battery powder. As a result, the load required for iron removal in wet processing can be reduced.
[0029] In addition, in the component removal process, resin powder obtained by powdering the resin components in the heat treatment process can be removed from the lithium-ion battery waste. Such resin powder may contain calcium and / or magnesium derived from glass fibers and other components in the resin components. If calcium is mixed into the battery powder, it can cause problems such as blockages during the solvent extraction process in the subsequent wet processing. Furthermore, magnesium becomes an impurity in the cobalt sulfate and nickel sulfate finally obtained after the wet processing, degrading their quality. Therefore, it is preferable to remove the resin powder in the component removal process.
[0030] In addition, in the component removal process, it is preferable to remove metal wires containing copper from the lithium-ion battery waste, because copper is also an impurity, and if it is mixed into the battery powder, it increases the load of the wet treatment.
[0031] In the part removal process, it is also possible to remove parts other than the frame, without removing the frame. In this case, the part removal process can be automated using a vibrating feeder, a trommel-type sieve, an air blower, or the like, rather than manually. Automation can sometimes remove 99.5% by mass or more of the resin powder and copper-containing metal wire. If the frame is left in the part removal process, it will be crushed in the crushing process described below. However, iron from the frame may be mixed into the large-diameter sieved material in the sieving process. To remove such iron, it is desirable to perform a preliminary magnetic separation process, as shown in FIG. 2, before the eddy current separation process or the magnetic separation process, in which iron is separated from the medium-diameter sieved material and the large-diameter sieved material using low-force magnetic separation.
[0032] In the crushing process, the lithium-ion battery waste that has undergone the component removal process is crushed as needed. This crushing process destroys the battery cell casing and separates the positive electrode-derived metals, such as nickel and cobalt, from the aluminum foil, yielding crushed material.
[0033] Various known crushers can be used here, and specific examples include impact crushers that can crush the case and battery by applying impact while cutting them, such as a sample mill, hammer mill, pin mill, wing mill, tornado mill, hammer crusher, etc. A screen can be installed at the outlet of the crusher, and the batteries are discharged from the crusher through the screen once they have been crushed to a size that can pass through the screen.
[0034] In the shredding process, for example, lithium-ion battery waste with dimensions of several tens of millimeters (e.g., 120 mm x 80 mm x 10 mm) can be shredded into smaller pieces of several tens of millimeters. When lithium-ion battery waste is finely shredded in the shredding process, the aluminum foil and copper foil are pulverized, and impurities such as aluminum and copper are easily contained in the small-diameter sieved pieces in the sieving process, and are therefore more likely to be contained in the battery powder. The size of the screen of the shredding machine can be, for example, 10 mm to 30 mm.
[0035] (Sieving Step) The crushed material obtained in the crushing step is subjected to sieving in the sieving step, and is separated into at least three types of material having different particle sizes, namely, small-diameter sieved material, medium-diameter sieved material, and large-diameter sieved material.
[0036] As the sieve used at this time, the mesh size of the sieve with the largest opening can be, for example, 9.16 mm. The large-diameter sieved material can be the undersize material of a sieve with an opening of 9.16 mm and the oversize material of a sieve with an intermediate opening described later, and may further include the oversize material of a sieve with an opening of 9.16 mm. The particle size of the large-diameter sieved material is, for example, 1 mm or more, and may be 4.75 mm or more. The large-diameter sieved material may include a state in which cobalt or nickel is not separated from aluminum or copper, such as a sieve in which cobalt or nickel remains attached to aluminum foil. Note that the lower limit of the particle size of the sieved material, such as a sieve having a lattice-shaped sieve hole with a side length equal to the lower limit, means that the sieved material will be the oversize material of the sieve. On the other hand, the upper limit of the particle size of the sieved material means that when sieved through a sieve having lattice-shaped sieve holes with a side length equal to the upper limit, the sieved material will be under the sieve. The same applies to the particle sizes of the magnetized material and the re-crushed material described below.
[0037] Furthermore, it is preferable to use a sieve with the smallest mesh size, such as 0.425 mm or less, for example 0.25 mm. Using a sieve with too large mesh size tends to allow impurities such as aluminum and copper to migrate to the small-diameter sieved material, resulting in a high level of impurities in the battery powder. On the other hand, a sieve with too small mesh size also prevents nickel and cobalt from passing through, resulting in a low recovery rate of valuable metals. Therefore, it is preferable to use a sieve with an opening size of 0.15 mm or more. By using the sieve with the smallest mesh size, the particle size of the small-diameter sieved material is preferably less than 0.25 mm, which sufficiently removes aluminum, copper, and the like, and contains large amounts of lithium, cobalt, nickel, and the like. The small-diameter sieved material is added to the battery powder.
[0038] Furthermore, the mesh size of the sieve with an intermediate mesh size is preferably 1 mm to 4.75 mm, and in one example, 1 mm. The intermediate sieve-rejected material can be the material that falls under the sieve with the medium mesh size and the material that remains on the sieve with the smallest mesh size. The particle size of the intermediate sieve-rejected material is, for example, 0.425 mm or more and less than 4.75 mm, or may be 0.25 mm or more and less than 4.75 mm. In intermediate sieve-rejected material of this size, cobalt and nickel are often essentially separated from aluminum and copper, and these can be effectively separated in the eddy current separation process described below. Material with a particle size of 4.75 mm or more may be difficult to separate by eddy current separation.
[0039] (Eddy Current Separation Step) In the eddy current separation step, non-magnetic conductive materials are separated from the medium-sized sieved materials by eddy current separation, and magnetic materials containing at least one of cobalt and nickel are extracted as magnetic materials.
[0040] As shown in Figure 4, an example of an eddy current separator is one equipped with a belt conveyor, which includes a belt for transporting the target material (here, medium-sized sieved material) and a pulley around which the belt is wound and driven to rotate. The pulley houses a rotor that rotates at high speed to generate a high-frequency alternating magnetic field. The rotor has alternating north and south poles arranged circumferentially, and when it rotates at high speed, it generates an alternating magnetic field. When conductive metals (non-magnetic conductive materials) among the target materials being transported by the belt pass through the alternating magnetic field, eddy currents proportional to the alternating magnetic field are generated in the metal. The magnetic force generated by these currents creates a repulsive effect with the magnetic force of the rotor, resulting in the separation of the metals. Meanwhile, magnetic metals (magnetic materials) among the target materials are essentially attracted to the belt surface by the magnetic force of the rotor, sent below the pulley, and then dropped off the belt surface when the magnetic influence weakens.
[0041] When performing eddy current separation, if the target material contains a large amount of iron, which is easily attracted to a magnet, the iron will remain on the pulley (here, on the belt), causing the belt to burn due to induction heating. In the embodiment shown in FIG. 1, the iron-containing metal frame is removed in the parts removal process, and in the embodiment shown in FIG. 2, the frame fragments are separated in the preliminary magnetic separation process. Therefore, in both embodiments, the medium-sized sieved material contains almost no iron, making eddy current separation possible. Note that, due to the heat treatment process, metallic cobalt and metallic nickel that may be contained in the medium-sized sieved material have a lower magnetic permeability than iron, and CoO and NiO also have a lower magnetic permeability than iron. Furthermore, both are mixed with non-magnetic carbon, so retention on the pulley is unlikely to occur.
[0042] The copper and aluminum contained in the medium-sized sieved material are non-magnetic and conductive, and when the magnetic cobalt and nickel are magnetically attracted to the belt surface by the magnetic force of the rotor, the repulsive force caused by eddy currents is greater than the effect of being caught in them, and they are pulled away from the belt surface. On the other hand, the cobalt and nickel contained in the medium-sized sieved material are magnetic, and they are attracted to the belt surface by the magnetic force of the rotor, and do not separate from the belt surface even when the repulsive force caused by eddy currents acts. Therefore, eddy current separation can separate the non-magnetic conductive aluminum and copper from the medium-sized sieved material, and extract the magnetic cobalt and nickel.
[0043] It is assumed that some of the medium-sized sieved materials contain copper and aluminum that are caught in the cobalt and nickel particles and adhere to the belt. The copper and aluminum caught in this way are thought to be weakly magnetically attached to the belt surface by the magnetic force of the rotor due to the cobalt and nickel contained in them.
[0044] The particles contained in the medium-sized sieved material are thought to be separated around the pulley in the following manner. First, due to the inertial force caused by the movement of the belt, particles composed of copper and aluminum are separated above the pulley. Next, although particles containing copper and aluminum and having weak magnetic properties do not leave the belt surface due to inertial force, they are repelled from the belt surface by the repulsive action of eddy currents above the pulley, and the copper and aluminum are separated. Next, the magnetic effect weakens below the pulley where the belt separates from the pulley. Therefore, of the particles that have adhered up to this point, particles composed mainly of copper and aluminum and with relatively weak magnetic attraction fall freely and separate. The particles that remain on the belt surface until the end are particles composed of cobalt and nickel, and particles with little copper or aluminum attached to cobalt or nickel, for which there is almost no repulsive force. These are ultimately recovered as magnetic particles.
[0045] In this way, in order to separate the impurity metals aluminum and copper from the medium-sized sieved material containing relatively fine particles such as cobalt, nickel, aluminum, copper, etc., eddy current sorting, which utilizes not only the inertial force due to the movement of the belt but also the repulsive force due to eddy currents, is effective, and in some cases it is possible to separate more than 90 mass% of the aluminum and copper.
[0046] The rotor inside the pulley of the eddy current separator preferably rotates at a speed of 1500 to 2500 rpm. If the rotor speed is too fast, nickel and cobalt may also be repelled. On the other hand, if the rotor speed is too slow, copper and aluminum may not be repelled.
[0047] As shown in Figure 4, below the pulley of the eddy current separator, a partition plate is provided to guide non-magnetic conductive materials that have been separated from the medium-sized sieved materials transported around the pulley on the belt by the generation of eddy currents and free fall, and magnetic materials that adhere to the belt surface and then fall, to different discharge outlets.
[0048] In an eddy current separator, under certain conditions, such as when the belt speed is slow, cobalt and nickel may accumulate above the pulley and continue to remain in one place, gradually increasing the amount of accumulation. To prevent this, it is preferable to use a belt with an uneven surface, as shown in the schematic diagram of Figure 5.
[0049] When performing eddy current sorting, the surface magnetic flux density on the pulley when the medium-sized sieved material on the belt conveyor of the eddy current sorter passes through the pulley may be set to, for example, 2000 to 3000 gauss, typically 2500 gauss or less.
[0050] The magnetized material extracted by separating the non-magnetic conductive material by the above-mentioned eddy current sorting has copper and aluminum removed and contains high-quality cobalt and / or nickel. If this magnetized material is included in the battery powder and subjected to a wet process, the recovery rate of cobalt and / or nickel can be improved.
[0051] (Preliminary Magnetic Separation Process) If the frame is not removed in the part removal process, as in the embodiment shown in Figure 2, the frame made of a metal such as iron will be crushed in the crushing process, and the crushed pieces may be separated into medium-sized pieces and large-sized pieces in the sieving process. In this case, it is preferable to perform a preliminary magnetic separation process before the eddy current separation process and the magnetic separation process to remove crushed pieces such as iron from the medium-sized pieces and large-sized pieces. Various magnetic separators can be used as long as they can recover iron as magnetic material.
[0052] In the preliminary magnetic separation process, low-force magnetic separation is performed to separate ferromagnetic (high magnetic permeability) iron as magnetic particles. Specifically, it is preferable to use a magnetic force with a surface magnetic flux density of, for example, 900 gauss or less, typically 350 to 550 gauss. Here, the surface magnetic flux density refers to the magnetic flux density at the surface of the magnetic separator where the medium-sized or large-sized particles are subjected to magnetic force. For example, in a pulley-type magnetic separator in which a belt conveyor is wound around a magnet pulley, the surface magnetic flux density is the surface magnetic flux density on the magnet pulley when the large-sized particles on the belt conveyor pass through the magnet pulley. The same applies to the surface magnetic flux density in the magnetic separation process described below.
[0053] (Magnetic Separation Step) In the magnetic separation step, magnetic separation is performed on the large-diameter sieved matter to separate the magnetically attached matter from the large-diameter sieved matter. In this step, various known magnetic separators can be used as long as they can separate the desired magnetically attached matter.
[0054] As shown in Fig. 1, when the frames are removed from the lithium-ion battery waste in the aforementioned component removal process, the large-diameter sieved material contains almost no iron. Therefore, in the embodiment shown in Fig. 1, the above-mentioned preliminary magnetic separation process for separating iron can be omitted, and the large-diameter sieved material can be subjected to a magnetic separation process using high magnetic force separation or the like, as described below. On the other hand, in the embodiment shown in Fig. 2, this magnetic separation process is preferably performed after the preliminary magnetic separation process.
[0055] For magnetic separation, it is preferable to use a magnetic force with a surface magnetic flux density of 5000 gauss or more. Metallic cobalt (Co), metallic nickel (Ni), and cobalt-nickel alloys exhibit ferromagnetic properties. Therefore, if only these ferromagnetic metals are to be recovered as magnetically attracted materials, the magnetic force used for magnetic separation may be relatively weak. On the other hand, the cobalt and nickel in the large-diameter sieved material include those that are not separated from the aluminum foil during the crushing process and remain attached to the aluminum foil. Since aluminum is not magnetic, the magnetism of cobalt or nickel attached to aluminum foil is weakened, making it difficult to magnetically attract the cobalt or nickel as a whole. Therefore, with a low surface magnetic flux density, aluminum foil with cobalt or nickel attached cannot be magnetically attracted, and the cobalt or nickel cannot be recovered. In contrast, if a strong magnetic force of 5000 gauss or more is used as described above, cobalt and nickel adhering to the aluminum foil can also be magnetically attracted, and most of the nickel, cobalt, etc. in the large-diameter sieved material can be contained in the magnetically attracted material.
[0056] (Re-crushing process) The magnetized material obtained in the magnetic separation process is crushed in a re-crushing process to produce re-crushed material. Here, the magnetized material is crushed to a certain degree of fineness, and the positive electrode-derived metals that are mainly attached to the aluminum foil are rubbed off, while the aluminum foil to which the positive electrode-derived metals are not attached is not crushed as much as possible. For example, when the magnetized material has a particle size of about 30 mm or less, the re-crushed material may be produced into re-crushed material with a particle size of several mm in the re-crushing process.
[0057] In the re-crushing process, various crushers can be used, as in the shredding process, but it is preferable to use a shear-type crusher. As mentioned above, this is to scrape off the positive electrode-derived metals attached to the aluminum foil. As long as a shear-type crusher is used, equally good results can be obtained whether a vertical or horizontal crusher is used. If a crusher designed solely for pulverization, such as a single-shaft crusher or a biaxial crusher, is used, the aluminum foil will also be crushed, which may increase the amount of aluminum impurities mixed in. The screen size of the crusher used in the re-crushing process may be approximately 5 mm. The smaller the screen size, the better the peelability of cobalt, nickel, and lithium, but if it is too small, fine aluminum fragments from the housing may clog the screen or chip the rotary blade. The aluminum fragments are incorporated into the aluminum foil with the rounded positive electrode-derived metals in the crushing process and migrate to the magnetically attached material side during the high-force magnetic separation process.
[0058] (Re-sieving step) After the re-crushing step, the re-crushed material obtained thereby is sieved in the re-sieving step to separate it into over-sieved material and under-sieved material.
[0059] In the re-sieving step, a sieve with an opening size of 0.25 mm or less is preferably used to sieve out the cobalt, nickel, etc. and oversize the aluminum. This results in an undersize product containing a large amount of valuable metals such as cobalt and nickel. The undersize product is then mixed with the battery powder together with the primary undersize product described above and subjected to wet treatment.
[0060] (Eddy Current Sorting Step) The remaining material may contain valuable metals such as cobalt, nickel, etc. In order to recover these, an eddy current sorting step may be further performed in which the remaining material is subjected to eddy current sorting to separate the re-magnetized material from the remaining material.
[0061] This eddy current separation process can be carried out in a manner similar to the eddy current separation process for the medium-sized sieved material, with the conditions appropriately adjusted so that the cobalt and nickel in the sieved material are transferred to the remagnetized material. The remagnetized material obtained thereby can be included in the battery powder together with the small-sized sieved material and the undersized material. However, since the remagnetized material may contain a certain amount of aluminum, it may be preferable not to include the remagnetized material in the battery powder from the perspective of suppressing the incorporation of impurities. In this case, the eddy current separation process may be omitted.
[0062] (Wet Treatment) Wet treatment can be carried out by various known methods to recover valuable metals and other metals from the battery powder. For example, the battery powder can be subjected to the same wet treatment as that used for consumer lithium-ion battery waste such as electronic devices to recover various metals. Specifically, the process can include a leaching step in which the various metals in the battery powder are leached, and a recovery step in which the leached solution is neutralized and / or solvent extracted to separate and recover the metals dissolved therein.
[0063] The metal recovery method described above was experimentally implemented, and its effectiveness was confirmed. The following description is provided for illustrative purposes only and is not intended to be limiting.
[0064] (Test Example 1) Lithium-ion battery waste was heat-treated, crushed, and then sieved to separate the crushed material into small-diameter, medium-diameter, and large-diameter pieces. The medium-diameter pieces had particle sizes of 0.25 mm to 1 mm, and the grades of the main metals (the ratio of the mass of each metal to the mass of the medium-diameter pieces (mass%)) were as shown in Table 1. The medium-diameter pieces were subjected to eddy current sorting using an eddy current sorter as shown in Figure 4. The results are shown in Table 2.
[0065]
[0066]
[0067] Under condition 2, the magnet (rotor) was not rotated to simulate a high-force magnetic separator, and processing was performed without the repulsive force caused by eddy currents. As a result, as shown in Table 2, the separability of Cu and Al was worse than under condition 1. This demonstrates that eddy current separation is effective for separating and removing Cu and Al. Furthermore, as can be seen from Table 2, the recovery rates of Co and Ni were similar under conditions 1 and 2. Therefore, it was found that the recovery of Co and Ni was due to the effect of magnetic force, and that the repulsive force caused by eddy currents assisted in the separation of Cu and Al above the pulley.
[0068] From the above, it was found that the above-mentioned metal recovery method can effectively separate impurity metals from the medium-sized sieved matter obtained by sieving, and can improve the recovery rate of Co and / or Ni.
Claims
1. A method for recovering metals containing at least one of cobalt and nickel from lithium ion battery waste, comprising: a heat treatment step for performing heat treatment on the lithium ion battery waste; a crushing step for crushing the lithium ion battery waste after the heat treatment step to obtain crushed material; a sieving step for separating the crushed material by sieving into at least small diameter screened material having a relatively small particle size, large diameter screened material having a relatively large particle size, and medium diameter screened material having a particle size intermediate between the small diameter screened material and the large diameter screened material; and an eddy current sorting step for separating non-magnetic conductive material from the medium diameter screened material by eddy current sorting, and extracting magnetic material containing at least one of cobalt and nickel as magnetic material, wherein the metal recovery method recovers the metal from battery powder containing the small diameter screened material and the magnetic material.
2. The metal recovery method according to claim 1, wherein the eddy current separation process uses an eddy current separator having a belt conveyor for transporting the medium-sized sieved materials and a belt conveyor pulley around which the belt is wound and driven to rotate, and a rotor built into the pulley that rotates at high speed to generate a high-frequency alternating magnetic field.
3. The metal recovery method according to claim 2, wherein the rotation speed of the rotor inside the pulley is set to 1500 rpm to 2500 rpm in the eddy current sorting process.
4. A metal recovery method as claimed in any one of claims 1 to 3, wherein in the sieving step, a sieve having an opening of 0.425 mm or less and a sieve having an opening of 1 mm to 4.75 mm are used, and the crushed material is separated into at least the small-diameter sieved material, the medium-diameter sieved material, and the large-diameter sieved material.
5. A metal recovery method as described in any one of claims 1 to 3, further comprising: a magnetic separation process in which the large diameter sieved material is subjected to magnetic separation and magnetic materials are extracted from the large diameter sieved material; a re-crushing process in which the magnetic materials are crushed to obtain re-crushed material; and a re-sieving process in which the re-crushed material is separated by sieving into over-sieved material and under-sieved material, and the battery powder further comprises the under-sieved material.
6. The metal recovery method according to claim 5, wherein the magnetic separation step involves magnetic separation using a magnetic force having a surface magnetic flux density of 5,000 gauss or more.
7. A metal recovery method as described in claim 5, wherein in the re-sieving step, a sieve having an opening size of 0.25 mm or less is used to separate the re-crushed material into the oversieve material and the undersieve material.
Citation Information
Patent Citations
Selection of nonferrous metal and device therefor
JP1998202141A
Method of recovering valuable material from used lithium battery
JP1999242967A
Method and apparatus for segregated recovery of communication device and recovery substrate part
JP2001179221A
Method of recovering valuable material from lithium ion secondary battery
JP2020061297A
Method for recovering valuables from used lithium-ion battery
JP2021063304A