Member for producing lithium-containing composite oxide, method for producing same, and firing furnace for producing lithium-containing composite oxide
The use of a metal or alloy base material with a specific coating film on containers and furnaces addresses temperature and corrosion issues in lithium-containing composite oxide production, enhancing battery performance and production efficiency.
Patent Information
- Application Number
- PCT/JP2024/000809
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-01-15
- Publication Date
- 2024-11-28
AI Technical Summary
Current methods for producing lithium-containing composite oxides, such as those used in lithium ion secondary batteries, face challenges with temperature uniformity and corrosion resistance during the synthesis process, leading to variations in solid phase reactions and potential battery performance issues due to inadequate thermal conductivity and low thermal shock resistance of ceramic containers.
A metal or alloy base material with a coating film containing aluminum, nickel, rhenium, and cobalt is used, with an aluminum concentration of 60-81 atomic % to provide excellent corrosion resistance and temperature uniformity, applied to the surface of containers and furnaces in contact with lithium-containing composite oxide powders, ensuring uniform heating and cooling.
This approach enhances the production of lithium-containing composite oxides by achieving better temperature followability and corrosion resistance, resulting in improved battery performance and reduced risk of container damage, while maintaining mechanical strength at high temperatures.
Smart Images

Figure JP2024000809_28112024_PF_FP_ABST
Abstract
Description
Lithium-containing composite oxide manufacturing component, manufacturing method thereof, and calcination furnace for manufacturing lithium-containing composite oxide
[0001] The present invention relates to a member for producing a lithium-containing composite oxide, a method for producing the same, and a firing furnace for producing a lithium-containing composite oxide, which is suitable for use in producing a positive electrode active material for a lithium ion secondary battery, for example.
[0002] The positive electrode active material of a lithium-ion secondary battery is a lithium-containing composite oxide (e.g., a lithium transition metal composite oxide such as lithium cobalt composite oxide, lithium nickel composite oxide, lithium manganese composite oxide, lithium manganese cobalt composite oxide, lithium nickel cobalt composite oxide, or lithium nickel cobalt manganese composite oxide). This positive electrode active material is produced by placing raw material powder in a container and firing it.
[0003] Ceramic saggers are widely used as containers for firing positive electrode active materials (see, for example, Patent Documents 1 to 3). Raw material powder is placed in the ceramic sagger, which is then placed in a firing furnace and heated to perform firing.
[0004] The atmosphere inside the firing furnace varies depending on the type of powder, but resistance heaters are widely used as a heating means. Resistance heaters are installed on the ceiling of the furnace and radiate heat to the saggers and raw powder. Since the atmosphere inside the furnace is also heated, convection heating also occurs inside the furnace.
[0005] The thickness of the powder layer in the ceramic sagger is usually about 50 to 100 mm, and heating occurs primarily from the surface layer. The thermal conductivity of ceramic saggers is low, and the powder itself also has a relatively low thermal conductivity. Therefore, the powder on the surface of the ceramic sagger heats up easily, but the powder inside heats up more slowly, resulting in unavoidable temperature differences during the heating process. While the powder on the surface is maintained at the highest temperature for a relatively long period of time, the powder inside is maintained at the highest temperature for a shorter period of time, resulting in variations in the progress of the solid-state reaction.
[0006] When attempting to sinter a positive electrode active material, if a ceramic container such as a crucible or sagger is used, there is a problem that the crucible or sagger will deteriorate and break with repeated use because the crucible or sagger has low thermal shock resistance.
[0007] Furthermore, for example, in the synthesis of a lithium-nickel composite oxide using lithium hydroxide and nickel composite oxide as raw materials, the reaction between lithium hydroxide and nickel composite oxide starts at around 450°C. If oxygen is not sufficiently diffused to the bottom of the ceramic sagger, unreacted molten lithium hydroxide may remain. The remaining lithium hydroxide may react with, for example, carbon dioxide gas to form lithium carbonate (Li 2 CO 3 If lithium carbonate is produced, gas caused by this lithium carbonate will be generated at high temperatures during battery use, which can lead to the problem of battery expansion.
[0008] In addition, in the synthesis reaction of lithium nickel composite oxide, when the temperature is further increased to 650°C, if unreacted lithium hydroxide and nickel composite oxide are present and oxygen is insufficient, for example, Li 2 Ni 8 O 10 These heterogeneous phases, which hinder the movement of lithium ions during the battery reaction, occur in the resulting lithium nickel composite oxide crystals, which can lead to deterioration of battery performance.
[0009] With the aim of obtaining a positive electrode active material having excellent battery characteristics, many proposals have been made so far regarding the conditions for synthesizing a lithium metal composite oxide by calcination.
[0010] In the synthesis reaction of a lithium-containing composite oxide, a metal or alloy sagger and related components that have excellent temperature tracking ability and temperature uniformity when the temperature is increased and decreased inside the sagger are desirable, but they are not currently in practical use due to their poor corrosion resistance.
[0011] Against this background, a sagger has recently been proposed in which at least the surface that comes into contact with the lithium positive electrode material powder is formed from a nickel-based alloy with an aluminum content of 1% by weight to 10% by weight (see Patent Document 4).
[0012] Japanese Patent No. 3552210 Japanese Patent Application Laid-Open No. 2003-165767 Japanese Patent Application Laid-Open No. 2015-218098 Japanese Patent No. 7090784
[0013] However, according to the investigations of the present inventors, the sagger proposed in Patent Document 4 has the drawback that the aluminum content of the nickel-based alloy is low, at 1% by weight or more and 10% by weight or less, and therefore protective alumina is not formed during use, resulting in poor corrosion resistance and the Cr contained in the nickel-based alloy being oxidized, which in turn has an adverse effect on the charge-discharge characteristics of the lithium-ion secondary battery.
[0014] Therefore, the problem to be solved by the present invention is to provide a lithium-containing composite oxide production member including various containers such as saggers and related members, which can obtain excellent corrosion resistance against a synthesis reaction of a lithium-containing composite oxide and have excellent temperature followability and temperature uniformity in heating and cooling, a method for producing the same, and a calcination furnace for producing a lithium-containing composite oxide which has such a lithium-containing composite oxide production member inside the furnace.
[0015] Another problem to be solved by the present invention is to provide a firing furnace for producing a lithium-containing composite oxide, which can obtain excellent corrosion resistance when firing a powder of a raw material for the lithium-containing composite oxide, and which is excellent in temperature followability and temperature uniformity in heating and cooling.
[0016] In order to solve the above problems, the present invention provides a member for producing a lithium-containing composite oxide, comprising: a substrate made of a metal or an alloy; and a coating film provided on a surface of the substrate that comes into contact with at least a powder of a raw material for a lithium (Li)-containing composite oxide, the coating film containing at least one metal selected from aluminum (Al), nickel (Ni), rhenium (Re) and cobalt (Co), in which the maximum aluminum concentration is 60 atomic % or more and 81 atomic % or less, and in which at least a portion of the at least one metal exists as an alloy in which part of the nickel in a nickel-aluminum alloy is substituted with the metal, or an alloy in which part of the cobalt in a cobalt-aluminum alloy is substituted with at least the nickel of nickel and rhenium.
[0017] The metal or alloy constituting the substrate is not particularly limited as long as it does not lose mechanical strength when heated to the firing temperature of the raw material powder of the Li-containing composite oxide, and can be selected as needed. Examples include Ni, Ni-based alloys, iron (Fe)-based alloys, etc. Among these, Ni-based alloys include, for example, MA47P (Ni-2Cr-4Al-1.5Si-0.5Mn), Inconel, Hastelloy, Alloy-X, etc. Furthermore, Fe-based alloys include, for example, stainless steel (SUS304, SUS310, etc.). The substrate may be made of a porous body of the above metal or alloy, or a sintered body obtained by sintering powder of the above metal or alloy. Furthermore, the above porous body or sintered body may be provided on at least the surface of the substrate that comes into contact with the raw material powder of the Li-containing composite oxide, and used as a substrate. The shape of the substrate is selected depending on the application of the Li-containing composite oxide production member. When the member for producing a lithium-containing composite oxide is a container such as a sagger, it has, for example, a bowl-like shape, and a coating film is provided on the inner surface of the container.When the member for producing a lithium-containing composite oxide is a tube, it is a circular tube, a square tube, etc., and a coating film is provided on the outer and inner surfaces of the tube.When the member for producing a lithium-containing composite oxide is a rod, it is a square rod, a round rod, etc., and a coating film is provided on the outer surface of the rod.
[0018] Since the maximum value of the Al concentration of the coating film is 60 atomic % or more and 81 atomic % or less, a protective alumina (Al 2 O 3 ) can be maintained, thereby obtaining corrosion resistance. The maximum Al concentration of the coating film is preferably 70 atomic % or more. The coating film may further contain at least one metal selected from the group consisting of tungsten (W), molybdenum (Mo), and niobium (Nb) as needed. The coating film may also contain other metals that are inevitably mixed in.
[0019] The coating film may consist of a single layer or multiple layers. In the coating film, Al, Ni, Re, and Co exist as various alloys, such as a Ni(Re,Co)-Al alloy in which part of the Ni in a Ni-Al alloy is substituted with Re and Co, a Ni(Re)-Al alloy in which part of the Ni in a Ni-Al alloy is substituted with Re, a Co(Ni,Re)-Al alloy in which part of the Co in a Co-Al alloy is substituted with Ni and Re, a Co(Ni)-Al alloy in which part of the Co in a Co-Al alloy is substituted with Ni, a Ni-Al alloy, a Re-Al alloy, and a Co-Al alloy. The coating film may also contain metals other than Al, Ni, Re, and Co, and in this case, these alloys may contain one or more of these metals. When the coating film consists of multiple layers, typically, each layer contains one of these alloys.
[0020] The present invention also provides a method for producing a member for producing a lithium-containing composite oxide, the method comprising the steps of: forming a raw material film containing at least nickel (Ni) and at least one metal selected from rhenium (Re) and cobalt (Co) on a substrate made of a metal or alloy; and performing an aluminum (Al) diffusion treatment on the substrate on which the raw material film has been formed, thereby forming a coating film on a surface of the substrate that comes into contact with at least a powder of raw material for the lithium (Li)-containing composite oxide, the coating film containing at least aluminum and at least one metal selected from nickel and rhenium and cobalt, wherein the maximum aluminum concentration is 60 atomic % or more and 81 atomic % or less, and at least a portion of the at least one metal being present as an alloy in which part of the nickel in a nickel-aluminum alloy has been substituted with said metal, or an alloy in which part of the cobalt in a cobalt-aluminum alloy has been substituted with at least the nickel of nickel and rhenium.
[0021] The raw coating may contain at least one metal selected from the group consisting of W, Mo, and Nb, in addition to Ni and at least one metal selected from Re and Co, and may also contain Al in some cases. If necessary, the raw coating may be formed in multiple steps. In this case, it is sufficient that the final raw coating as a whole contains at least one metal selected from Ni, Re, and Co, and each raw coating does not necessarily contain all of these elements. The method for forming the raw coating is not particularly limited and may be selected as needed. Examples of suitable methods include plating (electroplating), thermal spraying, and electron beam vacuum deposition.
[0022] The Al diffusion treatment is carried out by, for example, diffusing the base material on which the raw material coating is formed by diffusing powder containing Al (for example, Al powder) and NH 4 Cl powder and Al 2 O 3 The mixture is then immersed in a mixed powder containing the powder and an inert gas atmosphere, preferably argon (Ar) + 3 vol % hydrogen (H 2 ) atmosphere at a temperature of 950° C. or higher and 1150° C. or lower for 1 hour or higher and 10 hours or lower.
[0023] If necessary, after the formation of the raw material coating, the substrate on which the raw material coating is formed is heat-treated before the Al diffusion treatment. This heat treatment diffuses and homogenizes the metals that make up the raw material coating. The temperature and time of this heat treatment are selected as needed, but the temperature is, for example, 950°C or higher and 1150°C or lower, and the time is, for example, 30 minutes to 20 hours, typically 1 hour to 10 hours. This heat treatment is preferably carried out in an inert gas atmosphere similar to that described above. This heat treatment is typically carried out by diffusing the substrate on which the raw material coating is formed with, for example, Cr powder or Al powder and Al. 2 O 3 The base material is embedded in a mixed powder of Ni and Cr powder, and heated in an inert gas atmosphere similar to that described above. When the base material coating is formed in multiple steps, for example, a heat treatment may be performed after the first base material coating is formed, and then a second base material coating is formed to form the desired base material coating. Also, if necessary, a Cr diffusion treatment may be performed after the first base material coating is formed, and then a second base material coating is formed to form the desired base material coating. The Cr diffusion treatment may be performed, for example, by diffusing a base material on which a base material coating has been formed with a powder containing Ni and Cr and NH 4 Cl powder and Al 2 O 3 The mixture is then heated in an inert gas atmosphere similar to that described above at a temperature of 950° C. to 1150° C. for 1 hour to 10 hours.
[0024] In this invention, with respect to matters other than those mentioned above, what has been explained in relation to the invention of the member for producing a Li-containing composite oxide is valid, unless it is contrary to the nature of the invention.
[0025] The present invention also provides a sintering furnace for producing a lithium-containing composite oxide, comprising: a substrate made of a metal or an alloy; and a coating film provided on a surface of the substrate on the side that comes into contact with a substance generated during sintering of at least a powder of raw materials for a lithium (Li)-containing composite oxide, the coating film containing at least one metal selected from aluminum (Al), nickel (Ni), rhenium (Re) and cobalt (Co), wherein the maximum aluminum concentration is 60 atomic % or more and 81 atomic % or less, and at least a portion of the at least one metal exists as an alloy in which part of the nickel in a nickel-aluminum alloy is substituted with the metal, or an alloy in which part of the cobalt in a cobalt-aluminum alloy is substituted with at least the nickel of nickel and rhenium.
[0026] The substrate includes all substrates used in various structural members in a firing furnace, such as furnace walls including the ceiling, supports, structural materials, etc. In this invention, for matters other than those mentioned above, what has been explained in relation to the invention of the member for producing a Li-containing composite oxide described above is valid, unless it is contrary to the nature of the matter.
[0027] The present invention also relates to a sintering furnace for producing a lithium-containing composite oxide, the furnace containing therein a member for producing a lithium-containing composite oxide, the member comprising: a substrate made of a metal or an alloy; and a coating film provided on a surface of the substrate with which at least a powder of a raw material for a lithium-containing composite oxide comes into contact, the coating film containing at least one metal selected from aluminum (Al), nickel (Ni), rhenium (Re) and cobalt (Co), the maximum aluminum concentration being 60 atomic % or more and 81 atomic % or less, and at least a portion of the at least one metal being present as an alloy in which part of the nickel in a nickel-aluminum alloy is substituted with the metal, or an alloy in which part of the cobalt in a cobalt-aluminum alloy is substituted with at least the nickel of nickel and rhenium.
[0028] In the invention of this calcination furnace for producing lithium-containing composite oxide, what has been explained in relation to the invention of the member for producing Li-containing composite oxide is valid, unless it is contrary to the nature of the invention.
[0029] According to the present invention, a coating film is provided on at least the surface of a substrate made of a metal or alloy, with which at least the powder of the raw material of the lithium-containing composite oxide comes into contact, the coating film containing at least Al and at least one metal selected from Ni, Re, and Co, wherein the maximum value of the Al concentration is 60 atomic % or more and 81 atomic % or less, and at least a part of the at least one metal is present as an alloy in which part of the nickel in a nickel-aluminum alloy has been substituted with said metal, or an alloy in which part of the cobalt in a cobalt-aluminum alloy has been substituted with at least nickel of nickel and rhenium. This makes it possible to obtain excellent corrosion resistance when firing the powder of the raw material of the lithium-containing composite oxide, and since the substrate is made of a metal or alloy with excellent thermal conductivity and the coating film is also made of an alloy with similarly excellent thermal conductivity, it is possible to realize various members for producing lithium-containing composite oxides that are excellent in temperature followability and temperature uniformity when heating and cooling the powder during firing, and by having this member for producing a lithium-containing composite oxide in the furnace, it is possible to realize an excellent firing furnace for producing a lithium-containing composite oxide. Furthermore, a coating film containing at least Al and at least one metal selected from Ni, Re, and Co, in which the maximum Al concentration is 60 atomic % or more and 81 atomic % or less, and in which at least a part of the at least one metal exists as an alloy in which part of the nickel in a nickel-aluminum alloy is substituted with the metal, or an alloy in which part of the cobalt in a cobalt-aluminum alloy is substituted with at least the nickel of nickel and rhenium, is provided on at least the surface of a substrate made of a metal or alloy that comes into contact with a substance generated during firing of the raw material powder of the lithium-containing composite oxide. This makes it possible to obtain excellent corrosion resistance when firing the raw material powder of the lithium-containing composite oxide, and also makes it possible to realize a firing furnace for producing a lithium-containing composite oxide that is excellent in temperature followability and temperature uniformity during heating and cooling during firing.
[0030] 7A is a plan view showing a Li-containing composite oxide manufacturing vessel according to a first embodiment of the present invention. FIG. 7B is a cross-sectional view showing a Li-containing composite oxide manufacturing vessel according to the first embodiment of the present invention. FIG. 7C is a cross-sectional view showing a method of using the Li-containing composite oxide manufacturing vessel according to the first embodiment of the present invention. FIG. 7D is a cross-sectional view showing a method of using the Li-containing composite oxide manufacturing vessel according to the first embodiment of the present invention. FIG. 7E is a plan view showing a Li-containing composite oxide manufacturing tube according to a second embodiment of the present invention. FIG. 7F is a cross-sectional view showing a Li-containing composite oxide manufacturing tube according to the second embodiment of the present invention. FIG. 7G is a cross-sectional view showing a Li-containing composite oxide manufacturing rod according to a third embodiment of the present invention. FIG. 7H is a cross-sectional view showing a Li-containing composite oxide manufacturing rod according to the third embodiment of the present invention. FIG. 7I is a cross-sectional view showing a method of using the Li-containing composite oxide manufacturing rod according to the third embodiment of the present invention. FIG. 7I is a photograph, as a substitute for a drawing, showing the cross-sectional structure of the Ni base material of Example 1 after Al diffusion treatment. FIG. 7I is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. The Ni substrate of Example 1 was heated to 950°C in air using molten Li. 2 CO 3 8A is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 8A. FIG. 9A is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 9A. The Ni base material of Example 1 was immersed in molten Li at 950° C. in air. 2 CO 3 10A is a schematic diagram showing the results of measuring the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 10A. FIG. 11A is a schematic diagram showing the results of measuring the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 11A. The Ni base material of Example 1 was immersed in molten Li at 950° C. in air. 2 CO 3 12A is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 12A. The Ni base material of Example 1 was immersed in molten Li at 950° C. in air. 2 CO 3 13A is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 13A. 2 CO 3 1 is a diagram showing the relationship between the concentration of each element in the coating film of the Ni substrate and the immersion time in molten Li 2 CO 3 16A is a schematic diagram showing the relationship between the immersion time in molten Li in air at 950°C. 16B is a schematic diagram showing the relationship between the immersion time in molten Li in air at 950°C. 16C is a schematic diagram showing the relationship between the immersion time in molten Li in air at 950°C. 16D is a schematic diagram showing the relationship between the immersion time in molten Li in air at 950°C. 2 CO 3 17A is a diagrammatic line drawing showing the results of measuring the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 17A. FIG. 18A is a diagrammatic line drawing showing the results of measuring the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 18A. The Ni base material of Example 2 was immersed in molten Li at 950° C. in air. 2 CO 3 19A is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 19A. The Ni base material of Example 2 was immersed in molten Li at 950° C. in air. 2 CO 3 20A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 20B. The Ni base material of Example 2 was immersed in molten Li at 950° C. in air. 2 CO 3 21A is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 21A. 2 CO 3 1 is a diagram showing the relationship between the concentration of each element in the coating film of the Ni substrate and the immersion time in molten Li 2 CO 3 24A is a schematic diagram showing the relationship between the immersion time in molten Li in air at 950°C. 24B is a schematic diagram showing the relationship between the immersion time in molten Li in air at 950°C. 24C is a schematic diagram showing the relationship between the immersion time in molten Li in air at 950°C. 2 CO 3 26A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 26A. FIG. 27A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 27A. The Ni base material of Example 4 is immersed in molten Li at 950° C. in air. 2 CO 3 28A is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the Ni base material shown in FIG. 28A. FIG. 29A is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS304 base material shown in FIG. 29A. The SUS304 base material of Example 5 was immersed in molten Li at 950° C. in air. 2 CO 3 31A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS304 substrate shown in FIG. 31A. FIG. 32A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS304 substrate shown in FIG. 32A. The SUS304 substrate of Example 6 was immersed in molten Li at 950°C in air. 2 CO 3 34A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS304 substrate shown in FIG. 34A. FIG. 35A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 35A. FIG. 35B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 35A. FIG. 35C is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 35A. 2 CO 3 36A is a schematic diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 36A. FIG. 37A is a schematic diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 37A. FIG. 38A is a schematic diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 38A. The SUS310 substrate of Example 8 was immersed in molten Li at 950°C in air. 2 CO 3 39A is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 39B. 39B is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 40A. 40C is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 40B. 40D is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 40C. 40E is a diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 40F ... 2 CO 3 41B is a diagrammatic line drawing showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 41A. FIG. 41C is a diagrammatic line drawing showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 41A. FIG. 41D is a diagrammatic line drawing showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 43A. FIG. 43E is a diagrammatic line drawing showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 43A. 2 CO 3 44B is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 44A. FIG. 44C is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 44A. FIG. 46A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 46A. The SUS310 substrate of Example 11 was immersed in molten Li at 950°C in air. 2 CO 3 47A is a schematic diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 47A. FIG. 48A is a schematic diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 48A. FIG. 49A is a schematic diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 49A. The SUS310 substrate of Example 12 was immersed in molten Li at 950°C in air. 2 CO3 51A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 51A. FIG. 52A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 52A. The SUS310 substrate of Example 13 was immersed in molten Li at 950°C in air. 2 CO 3 54A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 54A. FIG. 55A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 55A. The SUS310 substrate of Example 14 was immersed in molten Li at 950°C in air. 2 CO 3 56A is a schematic diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 57A. FIG. 57A is a schematic diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 58A. FIG. 58A is a schematic diagram showing the results of measuring the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 58A. The SUS310 substrate of Example 15 was immersed in molten Li at 950°C in air. 2 CO 3 59A is a schematic diagram showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 substrate shown in FIG. 59B. The SUS310 substrate of Example 15 was immersed in molten Li at 950° C. in air for 20 hours.2 CO 3 60A is a diagrammatic line drawing showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in Fig. 60A. 61A is a diagrammatic line drawing showing the measurement results of the concentration distribution of each element in the cross section of the SUS310 base material shown in Fig. 61A.
[0031] Hereinafter, a mode for carrying out the invention (hereinafter simply referred to as "embodiment") will be described.
[0032] 1A and 1B show a container 10 for producing a lithium-containing composite oxide according to a first embodiment (hereinafter referred to as "container 10" as necessary), with FIG. 1A being a plan view and FIG. 1B being a cross-sectional view (longitudinal cross-sectional view). This container 10 is used to sinter raw material powder of a lithium-containing composite oxide used as a positive electrode active material for a lithium-ion secondary battery. As shown in FIGS. 1A and 1B, this container 10 is made of a metal or alloy and has a coating film 12 formed on the entire inner surface of a bowl-shaped substrate 11 with a flat bottom. The boundary between the flat bottom and the inner side of the substrate 11 is rounded, and reflecting this, the coating film 12 is also rounded at the same position. This allows the raw material powder of the lithium-containing composite oxide placed in the container 10 to be uniformly heated and sintered regardless of location. The coating film 12 contains at least Al and Ni and at least one metal selected from Re and Co, with the maximum Al concentration being 60 atomic % or more, preferably 70 atomic % or more, and typically 81 atomic % or less. As described above, the coating film 12 contains various alloys such as Ni(Re, Co)-Al alloys (typically collectively referred to as (Co, Ni, Re, Fe, Cr)-Al alloys). If necessary, the coating film 12 may be provided on not only the inner surface but also the outer surface of the container 10. Alternatively, the coating film 12 may be provided only on the inner surface of the container 10, and a coating film made of an Al-containing alloy with an Al concentration of, for example, 20 atomic % or more may be provided on the outer surface.
[0033] The substrate 10 is selected as needed, for example, from those already listed, and specifically, it is made of, for example, Ni, a Ni-based alloy, an Fe-based alloy, etc. The Ni-based alloy is, for example, Alloy-X, etc. The Fe-based alloy is various stainless steels, for example, SUS304, SUS310, etc.
[0034] 2A and 2B , a container 10 is filled with powder 20 of raw materials for the Li-containing composite oxide, and then placed in a firing furnace (not shown) and fired by heating to a high temperature using a heating means (not shown). In this way, the target Li-containing composite oxide is produced.
[0035] [Method for manufacturing the vessel for manufacturing the Li-containing composite oxide] A method for manufacturing the vessel 10 will be described.
[0036] (1) Manufacturing Method 1 First, a raw material coating containing at least Ni and at least one metal selected from Re and Co is formed on the inner surface of the substrate 11 by plating, thermal spraying, electron beam vacuum deposition, or the like. The raw material coating may be formed multiple times, for example, in two separate steps, as necessary. In this case, it is sufficient that the entire raw material coating containing at least Ni and at least one metal selected from Re and Co is formed.
[0037] Next, the substrate 11 on which the base film has been formed is subjected to an Al diffusion treatment (Al pack), thereby forming a coating film 12 on the inner surface of the substrate 11, as shown in Figures 1A and 1B. In this way, the container 10 is manufactured. The Al diffusion treatment is performed by the method described above.
[0038] (2) Manufacturing Method 2 First, as in Manufacturing Method 1, a raw material coating containing at least Ni and at least one metal selected from Re and Co is formed on the inner surface of the substrate 11. The raw material coating may be formed multiple times, for example, twice, as necessary. In this case, it is sufficient that the entire raw material coating containing multiple layers contains at least Ni and at least one metal selected from Re and Co.
[0039] Next, the base material 11 on which the raw material coating has been formed is subjected to a heat treatment to homogenize the raw material coating. The heat treatment is performed by the method described above.
[0040] Next, the base material 11 that has been subjected to the heat treatment is subjected to an Al diffusion treatment, thereby forming a coating film 12 on the inner surface of the base material 11. In this way, the container 10 is manufactured.
[0041] (3) Manufacturing Method 3 First, similarly to Manufacturing Method 1, a first layer of a raw material coating containing at least Ni and at least one metal selected from Re and Co is formed on the inner surface of the substrate 11 .
[0042] Next, the substrate 11 on which the first layer of the raw material coating has been formed is subjected to a heat treatment to homogenize the raw material coating. The heat treatment is carried out by the method described above.
[0043] Next, a second layer of raw film is formed on the first layer of raw film that has been heat treated in this way.
[0044] Thereafter, the substrate 11 on which the second layer of raw material film has been formed is subjected to an Al diffusion treatment, thereby forming a coating film 12 on the inner surface of the substrate 11. In this manner, the container 10 is manufactured.
[0045] (4) Manufacturing Method 4 First, similarly to Manufacturing Method 1, a first layer of a raw material coating containing at least Ni and at least one metal selected from Re and Co is formed on the inner surface of the substrate 11 .
[0046] Next, the substrate 11 on which the first layer of the base coating has been formed is subjected to a Cr diffusion treatment (Cr pack) by the method described above.
[0047] Next, a second layer of raw film is formed on the first layer of raw film that has been subjected to the Cr diffusion treatment.
[0048] Thereafter, the substrate 11 on which the second layer of raw material film has been formed is subjected to an Al diffusion treatment, thereby forming a coating film 12 on the inner surface of the substrate 11. In this manner, the container 10 is manufactured.
[0049] As described above, according to the first embodiment, the lithium-containing composite oxide producing container 10 is configured by providing the coating film 12, which contains at least Al and at least one metal selected from Ni and Re and Co, and has a maximum Al concentration of 60 atomic % or more and 81 atomic % or less, on the entire inner surface of the base material 11 made of a metal or alloy such as Ni, a Ni-based alloy, or an Fe-based alloy. Therefore, excellent corrosion resistance can be obtained when firing the powder of raw materials for the lithium-containing composite oxide, and since the base material 11 is made of a metal or alloy with excellent thermal conductivity and the coating film 12 is also made of an alloy with similarly excellent thermal conductivity, the lithium-containing composite oxide producing container 12 can be realized with excellent temperature tracking ability and temperature uniformity when heating and cooling the powder during firing.
[0050] Second Embodiment [Tube for Producing Li-Containing Composite Oxide] Figures 3A and 3B show a tube 30 for producing a Li-containing composite oxide according to a second embodiment (hereinafter referred to as "tube 30" as necessary), with Figure 3A being a plan view and Figure 3B being a cross-sectional view (longitudinal cross-sectional view). This tube 30 is an associated member used together with the container 10 according to the first embodiment. As shown in Figures 3A and 3B, this tube 10 has a coating film 32 provided on the entire outer and inner surfaces as well as the lower end surface of a cylindrical substrate 31 made of a metal or alloy. The coating film 32 is the same as the coating film 12. The substrate 31 is also the same as the substrate 10 except for its shape.
[0051] [Method of using the tube for producing a Li-containing composite oxide] As shown in Fig. 4, powder 20, which is a raw material for the Li-containing composite oxide, is charged into a container 10, and calcination is carried out with the tube 30 inserted inside the powder 20, thereby producing the target Li-containing composite oxide. In this case, carbon dioxide (CO 2 ) is efficiently discharged to the outside of the container 10 through the pipe 30.
[0052] [Method for Manufacturing Tube for Producing Li-Containing Composite Oxide] The method for manufacturing the tube 30 is basically the same as the method for manufacturing the container 10 .
[0053] According to the second embodiment, it is possible to obtain excellent corrosion resistance when calcining the powder of raw materials for the lithium-containing composite oxide, and further to realize a tube 30 for producing a lithium-containing composite oxide that is excellent in temperature followability and temperature uniformity in heating and cooling the powder when calcining.
[0054] Third Embodiment [Rod for Producing Li-Containing Composite Oxide] Figures 5A and 5B show a rod 40 for producing a Li-containing composite oxide according to a third embodiment (hereinafter referred to as "rod 40" as necessary), with Figure 5A being a plan view and Figure 5B being a cross-sectional view (longitudinal cross-sectional view). This rod 40 is an associated member used together with the container 10 according to the first embodiment. As shown in Figures 5A and 5B, this rod 40 has a coating film 42 provided on the entire outer surface of a round bar-shaped substrate 41 made of a metal or alloy. The coating film 42 is the same as the coating film 12. The substrate 41 is also the same as the substrate 11 except for its shape.
[0055] 6, powder 20, which is a raw material for the Li-containing composite oxide, is placed in a container 10, and firing is carried out with a rod 40 inserted inside the powder 20, thereby producing the desired Li-containing composite oxide. Generally, in use, a tube 30 is inserted into the powder 20 in addition to the rod 40.
[0056] According to the third embodiment, it is possible to obtain excellent corrosion resistance when firing the powder of raw materials for the lithium-containing composite oxide, and further to realize a rod 40 for producing a lithium-containing composite oxide that is excellent in temperature followability and temperature uniformity in heating and cooling the powder when firing.
[0057] An example will be described.
[0058] The following three types of substrates were used in the following Examples 1 to 15. The nominal composition (mass %) of each substrate is shown below.
[0059] (1) Ni base material (2) SUS304 base material (3) SUS310 base material
[0060] The nominal composition (mass %) of each substrate is as follows:
[0061] (1) Ni base material C Si Mn Cr Ni Fe Cu Al 0.02 or less 0.35 or less 0.35 or less none 99 or more 0.40 or less 0.25 or less none (2) SUS304 base material C Si Mn Cr Ni Fe Cu Al 0.08 or less 1.5 or less 2.0 or less 24.00-26.00 19.00-22.00 Remaining none none (3) SUS310 base material C Si Mn Cr Ni Fe Cu Al 0.08 or less 1.0 or less 2.0 or less 18.00-20.00 8.00-10.50 Remaining none none
[0062] Example 1 A coating film was formed by manufacturing method 2 on a Ni substrate.
[0063] First, the surface of the Ni substrate was polished to a smooth finish and degreased, and then a Ni strike film, a Re(Ni) film, and a Co-containing Re(Ni) film containing 20 mass% Co were formed on the surface by plating in this order. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating solution was composed of 0.1 atomic % Co and 99.9 atomic % Ni. The plating of the Re(Ni) film was performed at a current density of 60 mA / cm. 2 The plating was carried out for 60 minutes at a current density of 60 mA / cm. The composition of the plating solution was 0.2 atomic % Co, 59.2 atomic % Ni, and 40.3 atomic % Re. 2 The plating was carried out for 90 minutes at a temperature of 10.5 atomic % Co, 60.7 atomic % Ni, and 28.5 atomic % Re.
[0064] Next, the Ni base material on which the plating film was formed was subjected to a heat treatment. The heat treatment was carried out by mixing the Ni base material on which the plating film was formed with 10 g of Cr powder and 100 g of Al. 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1100° C. for 2 hours.
[0065] Next, the heat-treated Ni base material was subjected to an Al diffusion treatment. The Al diffusion treatment was carried out by diffusing the heat-treated Ni base material with 8 g of Al powder and 2 g of NH 4 Cl powder and 100g of Al 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1100° C. for 2 hours.
[0066] A portion of the Ni substrate / coating surface after the Al diffusion treatment was cut, and its cross-sectional structure was observed and the concentration distribution of each element was measured using a scanning electron microscope-energy dispersive spectroscopy (SEM-EDX) device. Figures 7A and 7B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG4 in the photograph shown in Figure 7A) measured using EDX, respectively. Figures 7A and 7B reveal that a coating film made of a Ni(Re, Co)-Al alloy is formed on the Ni substrate. The maximum Al concentration of this coating film is approximately 77 atomic %, and the Al concentration is 60 atomic % or higher throughout the majority of the thickness direction, excluding the portion on the Ni substrate side. This high Al concentration is due to the coating film's inclusion of Re and Co. Re is concentrated in the portion of this coating film facing the Ni substrate, and this portion serves as a diffusion barrier layer.
[0067] After the Al diffusion treatment, the Ni substrate was heated to 950°C in air with molten Li. 2 CO 3 The immersion time was set to four levels: 20 hours, 40 hours, 80 hours, and 100 hours.
[0068] After the 20-hour immersion test, a portion of the Ni substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 8A and 8B show cross-sectional SEM photographs and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG4 in the photograph shown in Figure 8A), respectively. Figures 8A and 8B show that the coating film composed of a Ni(Re, Co)-Al alloy is maintained, with the maximum Al concentration being 50 atomic % or more, and the Al concentration being 40 atomic % or more in most of the thickness direction, except for the Ni substrate side portion. It can be seen that the Re in the diffusion barrier layer is further aggregated, resulting in a high Re concentration. The Al concentration in the diffusion barrier layer is reduced. The Ni concentration is higher than the Co concentration throughout the coating film. Figures 9A and 9B show cross-sectional SEM photographs of an enlarged portion (surface side) of the cross-sectional structure shown in Figure 8A and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG4 in the photograph shown in Figure 9A), respectively. 9A and 9B, Al is present on the surface of the Ni(Re, Co)-Al layer. 2 O 3 It can be seen that an oxide consisting of (Ni, CoAl) is formed in close contact with the surface of the oxide.
[0069] After the 40-hour immersion test, a portion of the Ni substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 10A and 10B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG1 in the photograph shown in Figure 10A), respectively. Figures 10A and 10B show no significant changes in the coating film compared to the Ni substrate subjected to the 20-hour immersion test. The maximum Al concentration of the coating film is 40 atomic % or more, and the Al concentration is 40 atomic % or more throughout the majority of the thickness direction, except for the portion on the Ni substrate side. Figures 11A and 11B show a cross-sectional SEM photograph of an enlarged portion (surface side portion) of the cross-sectional structure shown in Figure 10A and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG2 in the photograph shown in Figure 11A), respectively. Figures 11A and 11B show that Al is present on the surface of the Ni(Re, Co)-Al layer. 2 O 3 It can be seen that oxides consisting of (Al, Ni, Co) are formed in close contact with each other. (Al, Ni, Co) oxides are observed on the outermost surface of the oxide.
[0070] After the 80-hour immersion test, a portion of the Ni substrate / coated surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 12A and 12B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG2 in the photograph shown in Figure 12A), respectively. Figures 12A and 12B show that the maximum value of the Al concentration is 40 atomic % or more. 2 O 3 The oxides consisting of Al, Ni, Co are formed in close contact with each other. (Al, Ni, Co) oxides are observed on the outermost surface of the oxide.
[0071] After the 100-hour immersion test, a portion of the Ni substrate / coated surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 13A and 13B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG4 in the photograph shown in Figure 13A), respectively. Figures 13A and 13B show that Al was deposited on the surface of the Ni(Re, Co)-Al layer. 2 O 3 It can be seen that an oxide consisting of these elements is formed in close contact. The maximum Al concentration in the coating film is 40 atomic % or more. (Al, Ni, Co) oxides are observed on the outermost surface of the oxide. The diffusion barrier layer of the coating film is maintained.
[0072] From the results of the above immersion test, it was found that by forming a coating film made of Ni(Re, Co)-Al alloy on a Ni substrate and with a maximum Al concentration of 60 atomic % or more, it is possible to prevent the formation of molten Li. 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0073] FIG. 14 shows the melted Li 2 CO 3 The graph shows the change in the Al concentration (maximum value) in the coating film and the thickness of the coating film with respect to the immersion time in molten Li. As shown in Fig. 14, both the Al concentration in the coating film and the thickness of the coating film rapidly decrease from the start of immersion until 20 hours have passed, but the decrease thereafter becomes gradual, and even after 100 hours, the Al concentration (maximum value) is approximately 40 atomic % or more. 2 CO 3 15 shows the changes in the Al concentration (maximum value) and the concentrations of Co, Ni, and Re in the coating film versus the immersion time in immersion. As shown in Figure 15, Ni concentration increases rapidly from the start of immersion until 20 hours have elapsed, but the increase thereafter becomes gradual.
[0074] Example 2 A coating film was formed by Manufacturing Method 1 using a Ni substrate.
[0075] First, the surface of the Ni base material was smooth-polished and degreased, and then a Ni strike film and a Co-containing Re(Ni) film containing 20% by mass of Co were sequentially formed on the surface by a plating method. The plating conditions for the Ni strike film and the composition of the plating solution were the same as in Example 1. The plating conditions for the Co-containing Re(Ni) film and the composition of the plating solution were the same as in Example 1. Subsequently, a Ni strike film and a Co-containing Re(Ni) film containing 20% by mass of Co were sequentially formed by a plating method. The plating of the Ni strike film was performed in the same manner as above. The plating conditions for the Co-containing Re(Ni) film and the composition of the plating solution were the same as in Example 1.
[0076] Next, the Ni base material on which the plating film was formed was subjected to a heat treatment under the same conditions as in Example 1.
[0077] Next, the Ni base material thus heat-treated was subjected to an Al diffusion treatment under the same conditions as in Example 1.
[0078] A portion of the Ni substrate / coating surface after the Al diffusion treatment was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 16A and 16B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG5 in the photograph shown in Figure 16A), respectively. Figures 16A and 16B show that a coating film made of a Ni(Re, Co)-Al alloy was formed on the Ni substrate. The maximum Al concentration of this coating film was approximately 77 atomic %, and the Al concentration was 60 atomic % or higher throughout the majority of the thickness direction, except for the portion on the Ni substrate side.
[0079] After the Al diffusion treatment, the Ni substrate was heated to 950°C in air with molten Li. 2 CO 3 The immersion time was set to four levels: 20 hours, 40 hours, 80 hours, and 100 hours.
[0080] After the 20-hour immersion test, a portion of the Ni substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 17A and 17B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG2 in the photograph shown in Figure 17A), respectively. Figures 17A and 17B show that the maximum Al concentration of the coating film was 40 atomic % or more. Figures 18A and 18B show a cross-sectional SEM photograph of an enlarged portion of the cross-sectional structure shown in Figure 17A and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG5 in the photograph shown in Figure 18A), respectively. Figures 18A and 18B show that Al was present on the surface of the Ni(Re, Co)-Al layer. 2 O 3 It can be seen that oxides consisting of (Al, Ni, Co) are formed in close contact with each other. (Al, Ni, Co) oxides are observed on the outermost surface of the oxide.
[0081] After the 40-hour immersion test, a portion of the Ni substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 19A and 19B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG3 in the photograph shown in Figure 19A), respectively. Figures 19A and 19B show that the maximum Al concentration of the coating film was 40 atomic % or more.
[0082] After the 80-hour immersion test, a portion of the Ni substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 20A and 20B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG3 in the photograph shown in Figure 20A), respectively. Figures 20A and 20B show that the maximum Al concentration of the coating film is still 40 atomic % or more. 2 O 3 The oxides consisting of Al, Ni, Co are formed in close contact with each other. (Al, Ni, Co) oxides are observed on the outermost surface of the oxide.
[0083] After the 100-hour immersion test, a portion of the Ni substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 21A and 21B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG6 in the photograph shown in Figure 21A), respectively. Figures 21A and 21B show that the maximum Al concentration of the coating film is still 40 atomic % or more. 2 O 3 The oxides consisting of Al, Ni, Co are formed in close contact with each other. (Al, Ni, Co) oxides are observed on the outermost surface of the oxide.
[0084] From the results of the above immersion test, it was found that by forming a coating film made of Ni(Re, Co)-Al alloy on a Ni substrate and with a maximum Al concentration of 60 atomic % or more, it is possible to prevent the formation of molten Li. 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0085] FIG. 22 shows the melted Li 2 CO 3 The graph shows the change in the Al concentration (maximum value) in the coating film and the thickness of the coating film with respect to the immersion time in molten Li. As shown in Fig. 22, both the Al concentration in the coating film and the thickness of the coating film rapidly decrease from the start of immersion until 20 hours have passed, but the decrease thereafter becomes gradual, and even after 100 hours, the Al concentration (maximum value) is still high at about 40 atomic %. Fig. 23 shows the change in the Al concentration in the coating film (maximum value) and the thickness of the coating film with respect to the immersion time in molten Li.2 CO 3 23 shows the changes in the Al concentration (maximum value) and the concentrations (maximum values) of Co, Ni, and Re in the coating film versus the immersion time in immersion. As shown in Fig. 23, Ni concentration increases rapidly from the start of immersion until 20 hours have passed, but the increase thereafter becomes gradual.
[0086] Example 3 A coating film was formed by Manufacturing Method 2 using a Ni substrate.
[0087] First, the surface of the Ni base material was polished to a smooth finish and degreased, and then a Ni strike film and a Co-containing Re(Ni) film containing 50 mass% Co were formed on the surface by plating in this order. The plating conditions for the Ni strike film and the composition of the plating solution were the same as in Example 1. The Co-containing Re(Ni) film was plated at a current density of 60 mA / cm. 2 The plating was carried out for 60 minutes at 1000 K, and the composition of the plating solution was 85.5 atomic % Co, 3.2 atomic % Ni, and 11.2 atomic % Re. Subsequently, a Ni strike film and a Co-containing Re(Ni) film containing 20 mass % Co were formed in this order by plating. The Ni strike film was plated in the same manner as above. The Co-containing Re(Ni) film was plated at a current density of 60 mA / cm. 2 The plating was carried out for 90 minutes, and the composition of the plating solution was the same as in Example 1.
[0088] Next, the Ni base material on which the plating film was formed was subjected to a heat treatment under the same conditions as in Example 1.
[0089] Next, the Ni base material thus heat-treated was subjected to an Al diffusion treatment under the same conditions as in Example 1.
[0090] A portion of the Ni substrate / coating surface after the Al diffusion treatment was cut, and its cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 24A and 24B show cross-sectional SEM photographs and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG6 in the photograph shown in Figure 24A), respectively. Figures 24A and 24B show that a coating film made of a Co(Ni, Re)-Al alloy was formed on the Ni substrate. The maximum Al concentration of this coating film was approximately 76 atomic %, and the Al concentration was 60 atomic % or higher throughout the majority of the thickness direction, except for the portion on the Ni substrate side. The Co contained in the Co(Ni, Re)-Al contributes to achieving such a high Al concentration.
[0091] After the Al diffusion treatment, the Ni substrate was heated to 950°C in air with molten Li. 2 CO 3 The immersion test was carried out for 20 hours.
[0092] After the 20-hour immersion test, a portion of the Ni substrate / coated surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 25A and 25B show a cross-sectional SEM photograph and the concentration distribution of each element measured using EDX (concentration distribution along the analysis line in the photograph shown in Figure 25A), respectively. Figures 25A and 25B reveal that a Co(Ni, Re)-Al layer and a Ni(Co, Re)-Al layer are sequentially formed on the Ni substrate to form a coating film. The maximum Al concentration of this coating film is 60 atomic % or more. Figures 26A and 26B show a cross-sectional SEM photograph enlarging a portion (surface side portion) of the cross-sectional structure shown in Figure 25A and the concentration distribution of each element (concentration distribution along the analysis line LG5 in the photograph shown in Figure 26A), respectively. Figures 26A and 26B reveal that Al is present on the surface of the Ni(Re, Co)-Al layer. 2 O 3 It can be seen that oxides consisting of (Al, Ni, Co) are formed in close contact with each other. (Al, Ni, Co) oxides are observed on the outermost surface of the oxide.
[0093] From the results of the above immersion test, it was found that by forming a coating film made of Ni(Re, Co)-Al alloy on a Ni substrate and with a maximum Al concentration of 60 atomic % or more, it is possible to prevent the formation of molten Li. 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0094] Example 4 A coating film was formed by Manufacturing Method 3 using a Ni substrate.
[0095] First, the surface of the Ni substrate was polished to a smooth surface and degreased, and then a Ni strike film and a Co-containing Re(Ni) film containing 20 mass % Co were formed on the surface by a plating method. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was carried out for 3 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Co-containing Re(Ni) film was carried out at a current density of 60 mA / cm 2 The plating was carried out for 120 minutes using the same plating solution composition as in Example 1.
[0096] Next, the Ni base material on which the plating film was formed was subjected to a heat treatment. The heat treatment was carried out by mixing the Ni base material on which the plating film was formed with 2 g of Al powder and 100 g of Al. 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1100° C. for 1.5 hours.
[0097] Next, a Ni strike film and a Co-containing Re(Ni) film containing 20 mass % Co were formed in this order by plating again. The Ni strike film was plated in the same manner as above. The Co-containing Re(Ni) film was plated at a current density of 60 mA / cm. 2 The plating was carried out for 75 minutes, and the composition of the plating solution was the same as in Example 1.
[0098] Next, the Ni base material on which the second-layer plating film was formed was subjected to an Al diffusion treatment. The Al diffusion treatment was carried out by diffusing the Ni base material on which the second-layer plating film was formed in a solution of 7 g of Al powder and 2 g of NH 4 Cl powder and 100g of Al 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1100° C. for 1.5 hours.
[0099] A portion of the Ni substrate / coating surface after the Al diffusion treatment was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 27A and 27B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG3 in the photograph shown in Figure 27A), respectively. Figures 27A and 27B show that a coating film composed primarily of a Co(Ni, Re)-Al alloy was formed on the Ni substrate. The maximum Al concentration of this coating film was approximately 64 atomic %.
[0100] After the Al diffusion treatment, the Ni substrate was heated to 950°C in air with molten Li. 2 CO 3 The immersion test was carried out for 20 hours.
[0101] After the 20-hour immersion test, a portion of the Ni substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 28A and 28B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG3 in the photograph shown in Figure 28A), respectively. Figures 28A and 28B show that the maximum Al concentration of the coating film was approximately 55 atomic %, and that the Al concentration was 40 atomic % or more in most parts in the thickness direction, except for the part on the Ni substrate side. Al was present on the surface of the Co, Ni-Al layer. 2 O 3 The oxide is formed in close contact with the surface.
[0102] From the results of the above immersion tests, it was found that by forming a coating film consisting of a Co, Ni, Re layer, a Re-Al layer, and a Co, Ni-Al layer on a Ni substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to obtain a coating film that can withstand molten Li. 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0103] Example 5 A coating film was formed by Manufacturing Method 1 on a SUS304 substrate.
[0104] First, the surface of a SUS304 substrate was polished to a smooth finish and degreased, and then a Ni strike film, a Co-containing Re(Ni) film containing 20 mass% Co, and a Co film were formed on the surface by plating in this order. The Ni strike film was plated under the same conditions as in Example 1, and the plating solution had the same composition as in Example 1. The Co-containing Re(Ni) film was plated at a current density of 40 mA / cm. 2 The plating was carried out for 60 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Co film was carried out at a current density of 40 mA / cm 2 The plating was carried out for 20 minutes at a temperature of 99.1 atomic % Co and 0.5 atomic % Ni.
[0105] Next, the SUS304 substrate on which the plating film was formed was subjected to an Al diffusion treatment. The Al diffusion treatment was carried out by immersing the SUS304 substrate on which the plating film was formed in a solution of 7 g of Al powder and 2 g of NH 4 Cl powder and 90g of Al 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1000° C. for 6 hours.
[0106] A portion of the SUS304 substrate / coating surface after the Al diffusion treatment was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 29A and 29B show cross-sectional SEM photographs and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG1 in the photograph shown in Figure 29A), respectively. Figures 29A and 29B show that a coating film composed primarily of Co(Ni, Re)-Al alloy and Co-Al alloy was formed on the SUS304 substrate. The maximum Al concentration of this coating film was approximately 76 atomic %, and the Al concentration was 60 atomic % or higher throughout the majority of the thickness direction, except for the portion facing the SUS304 substrate.
[0107] After the Al diffusion treatment, the SUS304 substrate was heated to 950°C in air with molten Li. 2 CO 3 The immersion test was carried out for 40 hours.
[0108] After the 40-hour immersion test, a portion of the SUS304 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 30A and 30B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG2 in the photograph shown in Figure 30A), respectively. Figures 30A and 30B show that even after 40 hours of immersion, the Al concentration of the coating film remains at around 50 atomic %. Protective Al is present inside the outermost Co-Al layer. 2 O 3 is formed. Fe in the SUS304 substrate diffuses up to the vicinity of the outer layer. Figures 31A and 31B respectively show an enlarged cross-sectional SEM photograph of a portion (surface side portion) of the cross-sectional structure shown in Figure 30A and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG3 in the photograph shown in Figure 31A). Figures 31A and 31B show that the Al concentration in the Co-Al layer has decreased to around 30 atomic %. The top layer of the coating film contains Al. 2 O 3 The oxide is formed in close contact with the surface.
[0109] From the results of the above immersion tests, it was found that by forming a coating film consisting of a (Co, Ni, Re)-Al layer and a Co-Al layer on a SUS304 substrate and with a maximum Al concentration of 60 atomic % or more, it is possible to obtain a coating film that can withstand molten Li. 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0110] Example 6 A coating film was formed by Manufacturing Method 1 on a SUS304 substrate.
[0111] First, the surface of a SUS304 substrate was polished to a smooth finish and degreased, and then a Ni strike film, a Ni film formed using a Watts bath, a Co-containing Re(Ni) film containing 20 mass% Co, and a Co film were formed on the surface by plating in this order. The Ni strike film was plated under the same conditions as in Example 1, and the plating solution had the same composition as in Example 1. The Ni film was plated using a Watts bath at a current density of 40 mA / cm. 2 The plating was carried out for 10 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Co-containing Re(Ni) film was carried out at a current density of 40 mA / cm 2 The plating was carried out for 90 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Co film was carried out at a current density of 40 mA / cm 2 The plating was carried out for 60 minutes, and the composition of the plating solution was the same as in Example 5.
[0112] Next, the SUS304 substrate on which the plating film was formed was subjected to an Al diffusion treatment. The Al diffusion treatment was carried out by immersing the SUS304 substrate on which the plating film was formed in a solution of 8 g of Al powder and 2 g of NH 4 Cl powder and 90g of Al 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1000° C. for 4 hours.
[0113] A portion of the SUS304 substrate / coating surface after the Al diffusion treatment was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 32A and 32B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG1 in the photograph shown in Figure 32A), respectively. Figures 32A and 32B show that a coating film composed primarily of Co(Ni, Re)-Al alloy and Co-Al alloy was formed on the SUS304 substrate. The maximum Al concentration of this coating film was approximately 77 atomic %, and the Al concentration was 60 atomic % or higher throughout the majority of the thickness direction, except for the portion facing the SUS304 substrate.
[0114] After the Al diffusion treatment, the SUS304 substrate was heated to 950°C in air with molten Li. 2 CO 3 The immersion test was carried out for 20 hours.
[0115] After the 20-hour immersion test, a portion of the SUS304 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 33A and 33B show cross-sectional SEM photographs and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG4 in the photograph shown in Figure 33A), respectively. Figures 33A and 33B show that even after 20 hours of immersion, the maximum Al concentration of the coating film remained above 60 atomic % and that the Al concentration was above 40 atomic % in most parts of the thickness direction, except for the portion on the SUS304 substrate side. Figures 34A and 34B show cross-sectional SEM photographs enlarged from a portion of the cross-sectional structure (surface side portion) shown in Figure 33A and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG7 in the photograph shown in Figure 34A), respectively. Figures 34A and 34B reveal that dense, protective Al was formed on the surface of the Co-Al layer. 2 O 3 It can be seen that is formed.
[0116] From the results of the above immersion test, it was found that by forming a coating film consisting of Co, Ni, Re-Al layers and Co-Al layers on a SUS304 substrate and with a maximum Al concentration of 60 atomic % or more, it is possible to obtain a coating film that is resistant to molten Li. 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0117] Example 7 A coating film was formed by Manufacturing Method 3 on a SUS310 substrate.
[0118] First, the surface of a SUS310 substrate was polished to a smooth finish and degreased, and then a Ni strike film and a Co-containing Re(Ni) film containing 20 mass% Co were formed on the surface by plating in this order. The Ni strike film was plated under the same conditions as in Example 1, and the plating solution had the same composition as in Example 1. The Co-containing Re(Ni) film was plated at a current density of 40 mA / cm. 2 The plating was carried out for 60 minutes, and the composition of the plating solution was the same as in Example 1.
[0119] Next, the SUS310 substrate on which the plating film was formed was subjected to a heat treatment.2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1100° C. for 2 hours.
[0120] Next, a Ni strike film and a Co-containing Re(Ni) film containing 20 mass % of Co were formed in this order on the heat-treated SUS310 substrate by plating. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was carried out for 3 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Co-containing Re(Ni) film was carried out at a current density of 60 mA / cm 2 The plating was carried out for 60 minutes, and the composition of the plating solution was the same as in Example 1.
[0121] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment. The Al diffusion treatment was carried out by diffusing 10 g of Al powder and 2 g of NH 4 Cl powder and 100g of Al 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1100° C. for 2 hours.
[0122] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 35A and 35B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG2 in the photograph shown in Figure 35A), respectively. Figures 35A and 35B show that a coating film composed primarily of a Co(Ni, Re)-Al alloy was formed on the SUS310 substrate. The maximum Al concentration of this coating film was approximately 67 atomic %.
[0123] After the Al diffusion treatment, the SUS310 substrate was heated in air at 950°C with molten Li. 2 CO 3 The immersion test was carried out for 20 hours.
[0124] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 36A and 36B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG1 in the photograph shown in Figure 36A), respectively. Figures 36A and 36B reveal that even after 20 hours of immersion, the maximum Al concentration of the coating film was approximately 60 atomic %, and the Al concentration was 40 atomic % or higher throughout the majority of the Co(Ni, Re)-Al layer thickness. Figures 37A and 37B show an enlarged cross-sectional SEM photograph of a portion (surface side) of the cross-sectional structure shown in Figure 36A and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG1 in the photograph shown in Figure 37A), respectively. Figures 37A and 37B reveal the presence of dense, protective Al on the surface of the Co(Ni, Re)-Al layer. 2 O 3 It can be seen that is formed.
[0125] From the results of the above immersion tests, it was found that by forming a coating film consisting of Co, Re, Fe, Cr, Ni layers and Co(Ni, Re)-Al layers on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to prevent the molten Li 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0126] Example 8 A coating film was formed by Manufacturing Method 3 on a SUS310 substrate.
[0127] First, the surface of the SUS310 substrate was polished to a smooth surface and degreased, and then a Ni strike film and a Co-containing Re(Ni) film containing 20 mass% Co were formed on the surface by plating. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was carried out for 3 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Co-containing Re(Ni) film was carried out at a current density of 60 mA / cm 2 The plating was carried out for 120 minutes using the same plating solution composition as in Example 1.
[0128] Next, the SUS310 substrate on which the plating film was formed was subjected to a heat treatment. 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1100° C. for 1.5 hours.
[0129] Next, a Ni strike film and a Co-containing Re(Ni) film containing 20 mass % of Co were formed in this order on the heat-treated SUS310 substrate by plating. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was carried out for 3 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Co-containing Re(Ni) film was carried out at a current density of 60 mA / cm 2 The plating was carried out for 75 minutes, and the composition of the plating solution was the same as in Example 1.
[0130] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment. The Al diffusion treatment was carried out by diffusing 7 g of Al powder and 2 g of NH 4 Cl powder and 100g of Al 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1100° C. for 1.5 hours.
[0131] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 38A and 38B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG1 in the photograph shown in Figure 38A), respectively. Figures 38A and 38B show that a coating film composed primarily of a Co(Ni, Re)-Al alloy was formed on the SUS310 substrate. The maximum Al concentration of the coating film was approximately 64 atomic %.
[0132] After the Al diffusion treatment, the SUS310 substrate was heated in air at 950°C with molten Li. 2 CO 3 The immersion test was carried out for 20 hours.
[0133] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 39A and 39B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG1 in the photograph shown in Figure 39A), respectively. Figures 39A and 39B show that even after 20 hours of immersion, the maximum Al concentration of the coating film was approximately 66 atomic %. Only the outermost Co, Ni, and Re-Al layers of the coating film were corroded. Protective Al was deposited on the surface of the outermost Co, Ni, and Re-Al layers. 2 O 3 are tightly adhered to each other.
[0134] From the results of the above immersion tests, it was found that by forming a coating film consisting of a Co, Re, Fe, Cr, Ni layer and a Co, Ni, Re-Al layer on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to prevent the molten Li 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0135] Example 9 A coating film was formed by Production Method 4 on a SUS310 substrate.
[0136] First, the surface of the SUS310 substrate was polished to a smooth surface and degreased, and then a Ni strike film and a Re (Ni) film were formed on the surface by plating. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was carried out for 3 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Re(Ni) film was carried out at a current density of 60 mA / cm 2 The plating was carried out for 90 minutes, and the composition of the plating solution was the same as in Example 1.
[0137] Next, the SUS310 substrate on which the plating film was formed was subjected to a Cr diffusion treatment (Cr pack). The SUS310 substrate on which the plating film was formed was immersed in 5 g of (Ni+Cr) powder and 2 g of NH 4 Cl powder and 100g of Al 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1100° C. for 2 hours.
[0138] Next, a Ni strike film and a Re(Ni) film were formed in this order on the SUS310 substrate that had been subjected to the Cr diffusion treatment by plating again. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was carried out for 1 minute, and the composition of the plating solution was the same as in Example 1. The plating of the Re(Ni) film was carried out at a current density of 60 mA / cm 2 The plating was carried out for 90 minutes, and the composition of the plating solution was the same as in Example 1.
[0139] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment. The Al diffusion treatment was carried out by immersing the SUS310 substrate on which the plating film was formed in a solution of 7 g of Al powder and 2 g of NH 4 Cl powder and 100g of Al 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1100° C. for 2 hours.
[0140] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 40A and 40B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG2 in the photograph shown in Figure 40A), respectively. Figures 40A and 40B show that a coating film composed primarily of a Ni(Re)-Al alloy was formed on the SUS310 substrate. The maximum Al concentration of the coating film was approximately 67 atomic %.
[0141] After the Al diffusion treatment, the SUS310 substrate was heated in air at 950°C with molten Li. 2 CO 3 The immersion test was carried out for 6 hours.
[0142] After the 6-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 41A and 41B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG3 in the photograph shown in Figure 41A), respectively. Figure 42 shows an enlarged cross-sectional SEM photograph of a portion (surface side portion) of the cross-sectional structure shown in Figure 41A. Figures 41A, 41B, and 42 show that even after 6 hours of immersion, the maximum Al concentration of the coating film was approximately 70 atomic %. Only the outermost Ni, Re-Al layer was corroded. Protective Al was deposited on the surface of the outermost Ni, Re-Al layer. 2 O 3 are formed in close contact with each other.
[0143] From the results of the above immersion tests, it was found that by forming a coating film consisting of Ni, Re, Fe, Cr layers and Ni, Re-Al layers on the SUS310 substrate and with a maximum Al concentration of 60 atomic % or more, it is possible to prevent the formation of molten Li. 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0144] Example 10 A coating film was formed by Production Method 4 on a SUS310 substrate.
[0145] First, the surface of the SUS310 substrate was polished to a smooth surface and degreased, and then a Ni strike film and a Co-containing Re(Ni) film containing 20 mass% Co were formed on the surface by plating. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was carried out for 3 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Co-containing Re(Ni) film was carried out at a current density of 60 mA / cm 2 The plating was carried out for 90 minutes, and the composition of the plating solution was the same as in Example 1.
[0146] Next, the SUS310 substrate on which the plating film was formed was subjected to a Cr diffusion treatment (Cr pack). The SUS310 substrate on which the plating film was formed was immersed in 5 g of (Ni+Cr) powder and 2 g of NH 4 Cl powder and 100g of Al 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1100° C. for 2 hours.
[0147] Next, a Ni strike film and a Re(Ni) film were formed in this order on the SUS310 substrate that had been subjected to the Cr diffusion treatment by plating again. The Ni strike film was plated at a current density of 0.5 A / cm. 2 The plating was carried out for 1 minute, and the composition of the plating solution was the same as in Example 1. The plating of the Re(Ni) film was carried out at a current density of 60 mA / cm 2 The plating was carried out for 90 minutes, and the composition of the plating solution was the same as in Example 1.
[0148] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment in the same manner as in Example 8.
[0149] After the Al diffusion treatment, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 43A and 43B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line of the photograph shown in Figure 43A), respectively. Figures 43A and 43B show that a coating film composed primarily of a Ni(Re)-Al alloy was formed on the SUS310 substrate. The maximum Al concentration of the coating film was approximately 65 atomic %.
[0150] After the Al diffusion treatment, the SUS310 substrate was heated in air at 950°C with molten Li. 2 CO 3 The immersion test was carried out for 6 hours.
[0151] After the 6-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 44A and 44B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG5 in the photograph shown in Figure 44A), respectively. Figure 45 shows an enlarged cross-sectional SEM photograph of a portion (surface side portion) of the cross-sectional structure shown in Figure 44A. Figures 44A, 44B, and 45 show that even after 6 hours of immersion, the maximum Al concentration of the coating film was approximately 66 atomic %. Only the outermost Ni, Re-Al layer was corroded. Protective Al was present on the surface of the outermost Ni, Re-Al layer. 2 O 3 are tightly adhered to each other.
[0152] From the results of the above immersion tests, it was found that by forming a coating film consisting of a Co, Re, Fe, Cr layer and a Ni, Re-Al layer on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to prevent the molten Li 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0153] Example 11 A coating film was formed by Production Method 3 on a SUS310 substrate.
[0154] First, the surface of a SUS310 substrate was polished to a smooth finish and degreased, and then a Ni strike film, a Ni film using a Watts bath, a Co-containing Re(Ni) film containing 20 mass% Co, and a Co film were formed on the surface by plating in this order. The Ni strike film was plated in the same manner as in Example 1. The Ni film using a Watts bath was plated in the same manner as in Example 6. The Co-containing Re(Ni) film was plated at a current density of 40 mA / cm. 2 The plating was carried out for 30 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Co film was carried out at a current density of 40 mA / cm 2 The plating was carried out for 30 minutes, and the composition of the plating solution was the same as in Example 5.
[0155] Next, the SUS310 substrate on which the plating film was formed was subjected to a heat treatment. The heat treatment was carried out by mixing the SUS310 substrate on which the plating film was formed with 10 g of Cr powder and 90 g of Al powder. 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1000° C. for 4 hours.
[0156] Next, on the heat-treated SUS310 substrate, a Ni strike film, a Ni film using a Watts bath, a Co-containing Re(Ni) film containing 20 mass% Co, and a Co film were formed in this order by plating. The Ni strike film was plated in the same manner as in Example 1. The Ni film was plated using a Watts bath at a current density of 40 mA / cm. 2 The plating was carried out for 10 minutes at a current density of 40 mA / cm. The plating solution had a composition of 0.1 atomic % Co and 99.9 atomic % Ni. 2 The plating was carried out for 60 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Co film was carried out at a current density of 40 mA / cm 2 The plating was carried out for 20 minutes, and the composition of the plating solution was the same as in Example 5.
[0157] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment. The Al diffusion treatment was carried out by immersing the SUS310 substrate on which the plating film was formed in a solution of 8 g of Al powder and 2 g of NH 4 Cl powder and 90g of Al 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1000° C. for 4 hours.
[0158] A portion of the SUS310 substrate / coating surface after the Al diffusion treatment was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 46A and 46B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG3 in the photograph shown in Figure 46A), respectively. Figures 46A and 46B show that a coating film composed primarily of a Co(Ni, Re)-Al alloy was formed on the SUS310 substrate. The maximum Al concentration of this coating film was 80 atomic %, and the Al concentration was 60 atomic % or higher throughout the majority of the thickness direction, except for the portion facing the SUS310 substrate.
[0159] After the Al diffusion treatment, the SUS310 substrate was heated in air at 950°C with molten Li.2 CO 3 The immersion test was carried out for 20 hours.
[0160] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 47A and 47B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG2 in the photograph shown in Figure 47A), respectively. From Figures 47A and 47B, it can be seen that even after 20 hours of immersion, the maximum Al concentration of the coating film was approximately 78 atomic %, and the overall Al concentration was 40 atomic % or more. Figures 48A and 48B show an enlarged cross-sectional SEM photograph of a portion (surface side portion) of the cross-sectional structure shown in Figure 47A and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG6 in the photograph shown in Figure 48A), respectively. Figures 48A and 48B show a dense protective Al layer on the surface of the Co(Ni)-Al layer. 2 O 3 It can be seen that they are formed in close contact.
[0161] From the results of the above immersion test, it was found that by forming a coating film consisting of Co, Ni, Re-Al layer and Co-Al layer on the SUS310 substrate and the maximum Al concentration is 60 atomic % or more, it is possible to obtain a high resistance to molten Li. 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0162] Example 12 A coating film was formed by Production Method 3 on a SUS310 substrate.
[0163] First, the surface of a SUS310 substrate was polished to a smooth finish and degreased, and then a Ni strike film, a Ni film using a Watts bath, a Co-containing Re(Ni) film containing 20 mass% Co, and a Co film were formed on the surface by plating in this order. The Ni strike film was plated in the same manner as in Example 1. The Ni film using a Watts bath was plated in the same manner as in Example 11. The Co-containing Re(Ni) film was plated at a current density of 40 mA / cm. 2 The plating was carried out for 30 minutes at a current density of 40 mA / cm. The composition of the plating solution was 10.5 atomic % Co, 60.7 atomic % Ni, and 28.5 atomic % Re.2 The plating was carried out for 30 minutes, and the composition of the plating solution was the same as in Example 5.
[0164] Next, the SUS310 substrate on which the plating film was formed was subjected to a heat treatment in the same manner as in Example 10.
[0165] Next, on the heat-treated SUS310 substrate, a Ni strike film, a Ni film using a Watts bath, a Co-containing Re(Ni) film containing 20 mass% Co, and a Co film were formed in this order by plating. The Ni strike film was plated in the same manner as in Example 1. The Ni film using a Watts bath was plated in the same manner as in Example 11. The Co-containing Re(Ni) film was plated at a current density of 40 mA / cm. 2 The plating was carried out for 60 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Co film was carried out at a current density of 40 mA / cm 2 The plating was carried out for 20 minutes, and the composition of the plating solution was the same as in Example 5.
[0166] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment in the same manner as in Example 10.
[0167] A portion of the SUS310 substrate / coating surface after the Al diffusion treatment was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 49A and 49B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG4 in the photograph shown in Figure 49A), respectively. Figures 49A and 49B show that a coating film composed primarily of a Co(Ni, Re)-Al alloy was formed on the SUS310 substrate. The maximum Al concentration of this coating film was approximately 78 atomic %, and the Al concentration was 60 atomic % or higher throughout the majority of the thickness direction, except for the portion facing the SUS310 substrate.
[0168] After the Al diffusion treatment, the SUS310 substrate was heated in air at 950°C with molten Li. 2 CO 3 The immersion test was carried out for 20 hours.
[0169] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 50A and 50B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG1 in the photograph shown in Figure 50A), respectively. From Figures 50A and 50B, it can be seen that even after 20 hours of immersion, the maximum Al concentration of the coating film was approximately 75 atomic %, and the overall Al concentration was 40 atomic % or more. Figures 51A and 51B show an enlarged cross-sectional SEM photograph of a portion (surface side portion) of the cross-sectional structure shown in Figure 50A and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG5 in the photograph shown in Figure 51A), respectively. From Figures 51A and 51B, it can be seen that a dense protective Al layer was formed on the surface of the Co(Ni)-Al layer. 2 O 3 It can be seen that they are formed in close contact.
[0170] From the results of the above immersion tests, it was found that by forming a coating film consisting of a Co, Re, Ni-Al layer and a Co(Ni)-Al layer on a SUS310 substrate and with a maximum Al concentration of 60 atomic % or more, it is possible to obtain a coating film that can withstand molten Li. 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0171] Example 13 A coating film was formed by Manufacturing Method 1 on a SUS310 substrate.
[0172] First, the surface of the SUS310 substrate was polished to a smooth finish and degreased, and then a Ni strike film, a Ni film, and a Co film were formed on the surface in this order by plating. The Ni strike film was plated in the same manner as in Example 1. The Ni film was plated at a current density of 40 mA / cm. 2 The plating was carried out for 30 minutes, and the composition of the plating solution was the same as in Example 1. The plating of the Co film was carried out at a current density of 40 mA / cm 2 The plating was carried out for 60 minutes, and the composition of the plating solution was the same as in Example 5.
[0173] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment. The Al diffusion treatment was carried out by immersing the SUS310 substrate on which the plating film was formed in a solution of 7 g of Al powder and 2 g of NH 4 Cl powder and 90g of Al 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1000° C. for 6 hours.
[0174] A portion of the SUS310 substrate / coating surface after the Al diffusion treatment was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 52A and 52B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG2 in the photograph shown in Figure 52A), respectively. Figures 52A and 52B show that a coating film composed primarily of Co(Ni)-Al alloy and Co(Ni,Fe)-Al alloy was formed on the SUS310 substrate. The maximum Al concentration of this coating film was approximately 64 atomic %.
[0175] After the Al diffusion treatment, the SUS310 substrate was heated in air at 950°C with molten Li. 2 CO 3 The immersion test was carried out for 20 hours.
[0176] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 53A and 53B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG4 in the photograph shown in Figure 53A), respectively. Figures 53A and 53B show that even after 20 hours of immersion, the maximum Al concentration of the coating film was approximately 60 atomic %, and the overall Al concentration was 40 atomic % or higher, except for the portion on the SUS310 substrate side. Figures 54A and 54B show an enlarged cross-sectional SEM photograph of a portion (surface side portion) of the cross-sectional structure shown in Figure 53A and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG5 in the photograph shown in Figure 54A), respectively. Figures 54A and 54B show that a dense protective Al layer was formed on the surface of the outermost Co-Al layer. 2 O 3 It can be seen that they are formed in close contact.
[0177] From the results of the above immersion test, it was found that by forming a coating film consisting of Fe, Ni, Co-Al layer and Co-Al layer on the SUS310 substrate and the maximum Al concentration is 60 atomic % or more, it is possible to obtain a coating film that can withstand molten Li. 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0178] Example 14 A coating film was formed by Production Method 2 on a SUS310 substrate.
[0179] First, the surface of the SUS310 substrate was polished to a smooth finish and degreased, and then a Ni strike film, a Ni film, and a Co film were formed on the surface in this order by plating. The Ni strike film was plated in the same manner as in Example 1. The Ni film was plated in the same manner as in Example 13. The Co film was plated at a current density of 40 mA / cm. 2 The plating was carried out for 60 minutes, and the composition of the plating solution was the same as in Example 5.
[0180] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment in the same manner as in Example 12.
[0181] A portion of the SUS310 substrate / coating surface after the Al diffusion treatment was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 55A and 55B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG3 in the photograph shown in Figure 55A), respectively. Figures 55A and 55B show that a coating film composed primarily of Co(Ni)-Al alloy and Co(Ni, Fe, Cr)-Al alloy was formed on the SUS310 substrate. The maximum Al concentration of this coating film was approximately 75 atomic %.
[0182] After the Al diffusion treatment, the SUS310 substrate was heated in air at 950°C with molten Li. 2 CO 3 The immersion test was carried out for 20 hours.
[0183] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 56A and 56B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG6 in the photograph shown in Figure 56A), respectively. Figures 56A and 56B show that even after 20 hours of immersion, the Al concentration of the coating film was 40 atomic % or more in most parts, except for the part on the SUS310 substrate side. Figures 57A and 57B show an enlarged cross-sectional SEM photograph of a portion of the cross-sectional structure (surface side portion) shown in Figure 56A, and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG7 in the photograph shown in Figure 57A), respectively. Figures 57A and 57B show that a dense protective Al layer was formed on the surface of the Co-Al layer. 2 O 3 It can be seen that they are formed in close contact.
[0184] From the results of the above immersion tests, it was found that by forming a coating film consisting of Ni, Fe, Cr-Al layer, Ni-Al layer and Co-Al layer on the SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to prevent the molten Li 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0185] Example 15 A coating film was formed by Manufacturing Method 1 on a SUS310 substrate.
[0186] First, the surface of a SUS310 substrate was polished to a smooth finish and degreased, and then a Ni strike film, a (Co+W) film, and a Co-containing Re(Ni) film containing 20% by mass of Co were formed on the surface by plating in this order. The Ni strike film was plated in the same manner as in Example 1. The (Co+W) film was plated at a current density of 40 mA / cm. 2 The plating was carried out for 60 minutes, and the composition of the plating solution was 90.3 atomic % Co, 1.7 atomic % Ni, and 7.7 atomic % W. The plating of the Co-containing Re(Ni) film was carried out at a current density of 40 mA / cm. 2 The plating was carried out for 30 minutes, and the composition of the plating solution was the same as in Example 1.
[0187] Next, the SUS310 substrate on which the plating film was formed was subjected to an Al diffusion treatment. The Al diffusion treatment was carried out by immersing the SUS310 substrate on which the plating film was formed in a solution of 7 g of Al powder and 2 g of NH 4 Cl powder and 90g of Al 2 O 3 The mixture was embedded in a mixture of Ar and 3 vol% H 2 The heating was carried out in an atmosphere at 1000° C. for 4 hours.
[0188] A portion of the SUS310 substrate / coating surface after the Al diffusion treatment was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 58A and 58B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line LG in the photograph shown in Figure 58A), respectively. Figures 58A and 58B show that a coating film composed primarily of Co(Re)-Al alloy and Co(Ni, Fe, W)-Al alloy was formed on the SUS310 substrate. The maximum Al concentration of this coating film was approximately 79 atomic %, and the Al concentration was 60 atomic % or higher throughout the majority of the thickness direction.
[0189] After the Al diffusion treatment, the SUS310 substrate was heated in air at 950°C with molten Li. 2 CO 3 The immersion time was set to two levels: 20 hours and 60 hours.
[0190] After the 20-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 59A and 59B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along the analysis line of the photograph shown in Figure 59A), respectively. Figures 59A and 59B show that even after 20 hours of immersion, the maximum Al concentration of the coating film was approximately 77 atomic %, and the overall Al concentration was 40 atomic % or more. A protective Al layer was formed on the surface of the outermost Co-Re-Al layer. 2 O 3 are tightly adhered to each other.
[0191] After the 60-hour immersion test, a portion of the SUS310 substrate / coating surface was cut, and the cross-sectional structure was observed and the concentration distribution of each element was measured. Figures 60A and 60B show a cross-sectional SEM photograph and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG1 in the photograph shown in Figure 60A), respectively. Figures 60A and 60B show that even after 60 hours of immersion, the maximum Al concentration of the coating film was approximately 50 atomic %, and the Al concentration was 40 atomic % or higher in a significant portion, except for the portion on the SUS310 substrate side. Figures 61A and 61B show an enlarged cross-sectional SEM photograph of a portion of the cross-sectional structure (surface side portion) shown in Figure 60A, and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG4 in the photograph shown in Figure 61A), respectively. Figures 61A and 61B show a cross-sectional SEM photograph of an enlarged portion of the cross-sectional structure (surface side portion) shown in Figure 60A, and the measurement results of the concentration distribution of each element (concentration distribution along analysis line LG4 in the photograph shown in Figure 61A). Figures 61A and 61B reveal that a dense protective Al layer was formed on the surface of the Co(Ni)-Al layer. 2 O 3 It can be seen that they are formed in close contact.
[0192] From the results of the above immersion tests, it was found that by forming a coating film consisting of a Co, Ni, Fe-Al layer and a Co, Re-Al layer on a SUS310 substrate, with a maximum Al concentration of 60 atomic % or more, it is possible to obtain a coating film that is resistant to molten Li. 2 CO 3 It can be seen that excellent corrosion resistance can be achieved against
[0193] Although the embodiments and examples of the present invention have been specifically described above, the present invention is not limited to the above-described embodiments and examples, and various modifications based on the technical concept of the present invention are possible.
[0194] REFERENCE SIGNS LIST 10 container 11 substrate 12 coating film 20 powder 30 tube 31 substrate 32 coating film 40 rod 41 substrate 42 coating film
Claims
1. A member for producing a lithium-containing composite oxide comprising: a substrate made of a metal or an alloy; and a coating film provided on a surface of the substrate with which at least a powder of a raw material for a lithium-containing composite oxide comes into contact, the coating film containing at least aluminum, nickel, and at least one metal selected from the group consisting of rhenium and cobalt, the maximum aluminum concentration being between 60 atomic % and 81 atomic %, and at least a portion of the at least one metal being present as an alloy in which part of the nickel in a nickel-aluminum alloy is substituted with said metal, or as an alloy in which part of the cobalt in a cobalt-aluminum alloy is substituted with at least the nickel of the nickel and rhenium.
2. The member for producing lithium-containing composite oxides according to claim 1, wherein said coating film further contains at least one metal selected from the group consisting of tungsten, molybdenum and niobium.
3. The member for producing lithium-containing composite oxides according to claim 1, wherein said at least one metal is present throughout the entire thickness of said coating film.
4. The member for producing lithium-containing composite oxides according to claim 1, wherein the substrate is made of nickel, a nickel-based alloy or an iron-based alloy.
5. The member for producing a lithium-containing composite oxide according to claim 1, wherein the member for producing a lithium-containing composite oxide is a container, and the coating film is provided on the inner surface of the container.
6. The member for producing lithium-containing composite oxides according to claim 1, wherein the member for producing lithium-containing composite oxides is a tube, and the coating film is provided on the outer and inner surfaces of the tube.
7. The member for producing lithium-containing composite oxides according to claim 1, wherein the member for producing lithium-containing composite oxides is a rod, and the coating film is provided on the outer surface of the rod.
8. A method for producing a member for producing a lithium-containing composite oxide, comprising: a step of forming a raw material film containing at least nickel and at least one metal selected from the group consisting of nickel and rhenium and cobalt on a substrate made of a metal or alloy; and a step of performing an aluminum diffusion treatment on the substrate on which the raw material film has been formed, to form a coating film containing at least aluminum, nickel, and at least one metal selected from the group consisting of rhenium and cobalt, with a maximum aluminum concentration of 60 atomic % or more and 81 atomic % or less, and at least a portion of the at least one metal being present as an alloy in which part of the nickel in a nickel-aluminum alloy has been substituted with said metal, or an alloy in which part of the cobalt in a cobalt-aluminum alloy has been substituted with at least one of nickel and rhenium.
9. The method for producing a member for producing lithium-containing composite oxides according to claim 8, wherein the raw film contains nickel, rhenium and cobalt.
10. The method for producing a member for producing lithium-containing composite oxides according to claim 8 or 9, wherein said raw film further contains at least one metal selected from the group consisting of tungsten, molybdenum and niobium.
11. A sintering furnace for producing a lithium-containing composite oxide, comprising: a substrate made of a metal or alloy; and a coating film provided on a surface of the substrate that comes into contact with a substance generated during sintering of at least a powder of a raw material for a lithium-containing composite oxide, the coating film containing at least aluminum, nickel, and at least one metal selected from the group consisting of rhenium and cobalt, the maximum aluminum concentration being between 60 atomic % and 81 atomic %, and at least a portion of the at least one metal being present as an alloy in which part of the nickel in a nickel-aluminum alloy is substituted with said metal, or as an alloy in which part of the cobalt in a cobalt-aluminum alloy is substituted with at least the nickel of the nickel and rhenium.
12. A sintering furnace for producing a lithium-containing composite oxide having within it a member for producing a lithium-containing composite oxide comprising: a substrate made of a metal or alloy; and a coating film provided on a surface of the substrate with which at least the powder of a raw material for a lithium-containing composite oxide comes into contact, the coating film containing at least aluminum, nickel, and at least one metal selected from the group consisting of rhenium and cobalt, the maximum aluminum concentration being between 60 atomic % and 81 atomic %, and at least a portion of the at least one metal being present as an alloy in which part of the nickel in a nickel-aluminum alloy is substituted with said metal, or as an alloy in which part of the cobalt in a cobalt-aluminum alloy is substituted with at least one of nickel and rhenium.
Citation Information
Patent Citations
Holders for burning ceramics
JP1977152409A
JP1982028300U
Heat resistant metal member and method of manufacturing the same, and high-temperature device and method of manufacturing the same
JP2022065441A
HEAT-RESISTANT Ni-ALLOY MATERIAL EXCELLENT IN RESISTANCE TO OXIDATION AT HIGH TEMPERATURE
WO2003074763A1
Nickel-base alloy, heat-resistant and corrosion resistant component, and component for heat-treatment furnace
WO2021132350A1
Cited By
Corrosion-resistant aluminum alloy grounding body material and preparation process thereof