Narrow-groove gas-shielded arc welding method
The narrow-gap gas shielded arc welding method with multi-electrode and controlled parameters achieves high tensile strength and efficiency, addressing the challenge of thick steel plate welding with reduced costs and defects.
Patent Information
- Application Number
- PCT/JP2024/010618
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-03-18
- Publication Date
- 2024-11-28
AI Technical Summary
Current narrow-gap gas shielded arc welding methods struggle to achieve high tensile strength of 550 MPa or more in weld metal while maintaining high welding efficiency, particularly for thick steel plates, leading to increased construction costs and potential welding defects.
A narrow-gap gas shielded arc welding method using multi-electrode welding with specific parameters: a groove angle of 25° or less, a bottom groove gap of 7 mm to 18 mm, and employing three or more electrodes with controlled heat input and carbon equivalent, along with a mixed shielding gas containing 20% CO2, and rare earth element in the welding wires to ensure sufficient tensile strength and efficiency.
The method achieves a tensile strength of 550 MPa or more in weld metal with reduced construction costs and minimizes welding defects, making it suitable for large-scale applications like architecture and shipbuilding.
Smart Images

Figure JP2024010618_28112024_PF_FP_ABST
Abstract
Description
Narrow gap gas shielded arc welding method
[0001] The present invention relates to a gas-shielded arc welding method, and in particular to a narrow-groove gas-shielded arc welding method applicable to steel plates having a thickness of 22 mm or more, which can ensure a tensile strength of 550 MPa or more in the weld metal. Here, "narrow groove" means a groove angle of 25° or less, and a minimum groove gap width between steel plates to be welded (base metal) that is 50% or less of the plate thickness of the steel plates.
[0002] Gas shielded arc welding, which is used for welding steel plates, is a 2 Single gas or Ar and CO 2 The most common type is the consumable electrode type, which uses a mixed gas of argon and argon to shield the molten area, and is widely used in the manufacturing fields of automobiles, construction, bridges, electrical equipment, etc.
[0003] In recent years, as steel structures have become larger and thicker, the amount of welding during the manufacturing process, particularly in butt welding of steel plates, has increased, and the welding work has become much more time-consuming, resulting in increased construction costs.
[0004] One possible way to improve this is to apply narrow-gap gas-shielded arc welding, which uses arc welding to multi-layer weld a groove with a gap that is small relative to the plate thickness. Narrow-gap gas-shielded arc welding reduces the amount of deposition compared to conventional gas-shielded arc welding, achieving high welding efficiency and energy savings, and is expected to ultimately reduce construction costs.
[0005] Recently, a technology has been proposed for performing this narrow-gap gas-shielded arc welding method using multiple electrodes. Multi-electrode welding can increase the amount of weld metal deposited to fill the groove in one weld, making it possible to achieve higher welding efficiency than single-electrode welding, and is an effective means for increasing welding efficiency.
[0006] For example, Patent Document 1 discloses a narrow-gap gas-shielded arc welding method for joining steel plates by narrow-gap multi-layer welding. In this patent document, the first layer welding is performed using multi-electrode welding with two or more electrodes. The first and second electrodes are positioned along a predetermined parallel weld line, and the distance between the tips of the welding wires of the first and second electrodes is controlled to a range of 5 mm to 16 mm. The angle of the line connecting the tips of the welding wires of the first and second electrodes relative to the perpendicular direction of the weld line is controlled to a range of 45° or less. It is described that these methods result in no welding defects and improved welding efficiency, even when groove preparation such as gas cutting or plasma cutting is performed.
[0007] Patent No. 6137053
[0008] However, the technology described in Patent Document 1 was unable to ensure sufficient tensile strength when high-strength steel was used as the base material, particularly when a high tensile strength of 550 MPa or more was required in the weld.
[0009] In view of the above-described conventional techniques, an object of the present invention is to provide a narrow-gap gas-shielded arc welding method that can ensure sufficiently high strength of the weld metal with high welding efficiency.
[0010] In order to achieve the above object, the present inventors have conducted extensive research into welding methods for improving the strength of the weld metal, and as a result have found that it is important to set the average carbon equivalent of the welding wire divided by the number of wires to 0.400 mass% or more, to set the ratio of the maximum to the minimum heat input of each electrode to 1.40 or less, and to set the total heat input to 10 kJ / cm to 60 kJ / cm.
[0011] The present invention was made based on this finding and further studies, and is summarized as follows: [1] A narrow-groove gas-shielded arc welding method for joining steel plates with a thickness t of 22 mm or more by multi-layer welding with a narrow groove having a groove angle θ of 25° or less and a bottom groove gap G of 7 mm to 18 mm, wherein the multi-layer welding is performed by multi-electrode welding with three or more electrodes, the average value obtained by dividing the sum of the carbon equivalents (Ceq) of the welding wires, as defined by the following formula (1), by the number of electrodes is 0.400 mass% or more, the ratio of the maximum heat input to the minimum heat input of the electrodes is 1.40 or less, and the sum of the heat inputs of the electrodes is 10 kJ / cm to 60 kJ / cm. Ceq = [C] + [Si] / 24 + [Mn] / 6 + [Ni] / 40 + [Cr] / 5 + [Mo] / 4 + [V] / 14 (1) Here, [element] indicates the content (mass%) of the element in the welding wire, and if no element is added, substitute 0. [2] The narrow gap gas-shielded arc welding method in [1], wherein one of the first electrode and the second electrode is a negative wire (positive polarity) and the other is a positive wire (reverse polarity), the distance a between tips of the welding wires supplied from power feed tips at the tips of the welding torches of the first electrode and the second electrode is 5 mm to 16 mm, the angle α of a line connecting the tips of the welding wires of the first electrode and the second electrode with respect to the groove width direction is 60° or less, the diameter of the welding wire used for each electrode is 1.0 mm to 1.6 mm, and the distance between adjacent electrodes after the second electrode is 10 mm to 100 mm. [3] The narrow gap gas-shielded arc welding method according to [2], wherein a third electrode and subsequent electrodes are disposed at the center of the groove behind the first electrode and the second electrode. [4] In any one of [1] to [3], the shielding gas contains 20% or more by volume of CO 2 [5] The narrow-gap gas-shielded arc welding method according to any one of [1] to [4], wherein at least one welding wire used in the positive electrode contains 0.005% to 0.060% by mass of REM (rare earth element).
[0012] According to the present invention, narrow-gap gas-shielded arc welding, which has high welding efficiency, can be performed even when a tensile strength of more than 550 MPa is required for the weld metal of the joint. Furthermore, the narrow-gap gas-shielded arc-welded joint obtained by this method has a significantly reduced manufacturing cost compared to conventional welded joints, making it extremely useful for application to general structures such as buildings, bridges, and ships.
[0013] Fig. 1 is an explanatory diagram showing a groove shape used in the present invention, and Fig. 2 is an explanatory diagram showing an example of a welding procedure when welding with four electrodes in the present invention, (a) is a front view, and (b) is a top view.
[0014] The present invention will be specifically described below.
[0015] The present invention relates to a narrow-gap gas-shielded arc welding method for joining steel plates with a thickness t of 22 mm or more by narrow-gap multi-layer welding with a groove angle θ of 25° or less and a bottom groove gap G of 7 mm to 18 mm. Note that the term "steel plate" as used herein includes thick steel materials, thick plate steel materials, etc.
[0016] [Thickness t of steel plate: 22 mm or more] The thickness t of the steel plate 1 (see FIG. 1) is 22 mm or more. If the thickness t is less than 22 mm, in a conventional square groove, increasing the groove angle and reducing the groove gap may result in a smaller groove cross-sectional area than the groove targeted by the present invention, and the square groove results in highly efficient welding with a smaller deposition amount. Preferably, the thickness t is 30 mm or more.
[0017] Furthermore, since the thickness of steel structures, including special structures, is often 200 mm or less, in the present invention, it is preferable that the upper limit of the thickness t of the steel plate is set to 200 mm.
[0018] The present invention can be applied to various types of thick steel plates, from mild steel plates to high-tensile steel plates of 780 MPa class. 590 MPa class high-tensile steel plates can also be welded without preheating.
[0019] [Groove angle θ: 25° or less] The groove shape used in the present invention is a narrow groove shape of a V-shaped groove or an I-shaped groove (including θ = 0°) with a gap at the bottom. An example of a V-shaped groove with a gap at the bottom is shown in FIG. 1. Here, 1 is a steel plate (base material), and 2 is a groove surface. The smaller the groove cross-sectional area of the groove portion of the steel plate 1, the more efficient welding becomes, but defects such as poor fusion are more likely to occur. Furthermore, when the groove angle θ of the groove portion exceeds 25°, it can be performed using conventional construction methods. For this reason, the present invention targets cases where the groove angle θ is 25° or less, which is difficult to perform using conventional construction methods and where even higher efficiency is expected. In addition, when the groove angle θ in a V-shaped groove is 0°, it is called an I-shaped groove, and in terms of the amount of welding, this 0° case is the most efficient. However, since the groove may close during welding due to welding thermal distortion, it is preferable to set the groove angle θ according to the plate thickness t in anticipation of this. When the plate thickness t exceeds 100 mm, the upper limit of the preferable range is preferably 10°. A more preferable range of the included angle θ is 5° to 10°.
[0020] [Bottom Groove Gap G: 7 mm to 18 mm] The smaller the groove of the steel plate, the faster and more efficient the welding, but the more likely defects such as incomplete fusion are to occur. Furthermore, welding with a bottom groove gap G (Figure 1), which is the gap between the bottoms of the grooves (groove width) before welding begins, exceeding 18 mm can be performed using conventional construction methods. For this reason, the present invention targets bottom groove gaps G of 18 mm or less, which are expected to be even more efficient than conventional construction methods. On the other hand, if the bottom groove gap G is less than 7 mm, welding with three or more electrodes may be difficult. Therefore, the bottom groove gap G should be in the range of 7 mm to 18 mm. Preferably, it is in the range of 8 mm to 12 mm. It is preferable to use a backing material 7 during welding (see Figure 2(a)).
[0021] [Multi-layer welding with three or more electrodes] In the present invention, the first layer and each layer after the second layer are joined by multi-layer welding with three or more electrodes using the narrow groove described above. Here, although it is permissible to form each layer by multiple welding passes, from the viewpoint of welding efficiency, it is preferable to form each layer by one welding pass per layer.
[0022] The reason for using three or more electrodes is that it is difficult to improve the welding efficiency with two or fewer electrodes. Preferably, the number of electrodes is three to five. More than five electrodes are undesirable because they tend to cause non-uniformity in the components of the weld metal.
[0023] An example of a welding procedure using four electrodes according to the present invention is shown in Figure 2. In Figure 2, 3, 4, 5, and 6 represent the first, second, third, and fourth electrodes, 3a, 4a, 5a, and 6a represent the current feed tips of the electrodes 3, 4, 5, and 6, respectively, 3b, 4b, 5b, and 6b represent the welding wires supplied to the electrodes 3, 4, 5, and 6, respectively, and 7 represents a backing material. Also, 8 represents the weld line (the line along which the tip of the welding wire is placed), 9 represents the weld bead of the first layer, 10 represents the molten pool (second layer), and 11 represents the weld bead (second layer) during welding. In the example shown in Figure 2, the welding wires 3b and 4b extend from the current feed tips 3a and 4a in a curved shape. However, the present invention is not limited to this example, and the protruding portions may also be linear.
[0024] [Average value obtained by dividing the sum of the carbon equivalents (Ceq) of the welding wires by the number of electrodes: 0.400 mass % or more] The carbon equivalent (Ceq) is defined by the following formula (1), and is an index that greatly affects the tensile strength of the weld metal: Ceq = [C] + [Si] / 24 + [Mn] / 6 + [Ni] / 40 + [Cr] / 5 + [Mo] / 4 + [V] / 14 (1) Here, [element] indicates the element content (mass %) in the welding wire, and 0 is substituted if no element is added.
[0025] The average value obtained by dividing the sum of the carbon equivalents (Ceq) of the welding wires by the number of electrodes is hereinafter also referred to as the "average Ceq." The average Ceq is defined by the following formula (2): Average Ceq = ([Ceq #1 ]+〔Ceq #2 ]+〔Ceq#3 ]+...+〔Ceq #n ]) / n (2) where, [Ceq #i ] (i: 1 to n) indicates the Ceq of the welding wire of the i-th electrode, and n indicates the total number of electrodes.
[0026] The present inventors have found through experiments that in order to ensure a tensile strength of 550 MPa or more in the weld metal, the Ceq of the weld metal needs to be 0.320 mass% or more, and that to achieve this, the average Ceq of the welding wire used needs to be 0.400 mass% or more. Therefore, the average Ceq is set to 0.400 mass% or more, and preferably 0.420 mass% or more. Note that, because an excessively high average Ceq may adversely affect the toughness of the weld metal, it is preferable to set the upper limit to 0.520 mass%.
[0027] [Ratio of Maximum to Minimum Heat Input of Each Electrode: 1.40 or Less] The amount of metal deposited from each welding wire is affected by the heat input of each electrode. Even if the average Ceq is 0.400 mass% or more, if there is a deviation in the heat input between the electrodes, a sufficient Ceq may not be imparted to the weld metal. In other words, if the ratio of the maximum to minimum heat input of each electrode (hereinafter also referred to as the "maximum / minimum heat input ratio") exceeds 1.40, the Ceq of the weld metal may not reach 0.320 mass% or more. Therefore, the maximum / minimum heat input ratio is set to 1.40 or less.
[0028] Here, the heat input is defined by the following formula (3): Heat input (kJ / cm) = {welding current (A) × welding voltage (V) / 1000} × 60 / {welding speed (cm / min)} (3)
[0029] The heat inputs of each electrode calculated using this definition formula are compared to select the maximum and minimum heat inputs, and the ratio of the selected maximum and minimum heat inputs is defined as the maximum / minimum heat input ratio. If the heat inputs of each electrode are equal, the maximum / minimum heat input ratio is 1.00.
[0030] By setting the welding current, welding voltage, and welding speed so that the maximum / minimum heat input ratio is 1.40 or less, it is possible to stably maintain a Ceq of 0.320 mass% or more over the entire length of the weld metal and ensure a tensile strength of 550 MPa or more. The maximum / minimum heat input ratio is preferably 1.20 or less.
[0031] [Total Heat Input of Each Electrode: 10 kJ / cm to 60 kJ / cm] If the total heat input of each electrode is less than 10 kJ / cm, the strength of the weld metal will be excessively high, raising concerns about reduced toughness and cold cracking. On the other hand, if the total heat input of each electrode exceeds 60 kJ / cm, the strength of the weld metal will decrease, and it may become impossible to ensure a tensile strength of 550 MPa or more for the weld metal. Therefore, the total heat input of each electrode is set to 10 kJ / cm to 60 kJ / cm. Preferably, it is 15 kJ / cm to 45 kJ / cm.
[0032] In the present invention, the above-mentioned welding conditions relating to the average Ceq of the welding wire, the maximum / minimum ratio of the heat input, and the sum of the heat inputs of the electrodes are essential. In addition, the following conditions can be mentioned as other preferable welding conditions.
[0033] [Electrode Polarity] If the first and second electrodes have the same polarity (e.g., both the first and second electrodes are wire-positive), the mutual electromagnetic force causes the arcs to be directed inward, concentrating heat at the center of the groove. This may result in insufficient melting at the groove surface. On the other hand, if one of the first and second electrodes is wire-negative (positive polarity) and the other is wire-positive (reverse polarity), and the arrangement of the first and second electrodes is appropriately controlled, the magnetic fields generated by the welding currents generate a strong outward electromagnetic force, causing the arcs to repel each other. As a result, sufficient melting depth can be achieved at the groove surface. For these reasons, in the present invention, it is preferable to use wire-negative (positive polarity) and wire-positive (reverse polarity) for one of the first and second electrodes. Note that the polarity of the third electrode 5 and subsequent electrodes is not particularly limited and may be either wire-negative (positive polarity) or wire-positive (reverse polarity).
[0034] [Arrangement of First and Second Electrodes] In narrow-gap multi-pass welding, when one pass is performed per layer, welding heat tends to concentrate at the center of the groove with one electrode, resulting in insufficient melting at the groove surface of the steel sheet, and defects due to incomplete fusion (cold lap) and spatter and slag inclusion on the groove surface are likely to occur. In particular, in the first layer welding, the temperature of the steel sheet is low and the melting depth is small, making defects due to incomplete fusion more likely to occur. Therefore, in the present invention, it is preferable to arrange the first electrode 3 and the second electrode 4 at positions along a predetermined parallel weld line 8, as shown in Figure 2(b).
[0035] [Distance a between the welding wire tips of the first electrode and the second electrode: 5 mm to 16 mm] The distance a between the tips of the welding wires 3 b, 4 b supplied from the power feed tips 3 a, 4 a at the tip of the welding torch of each of the first electrode 3 and the second electrode 4 (hereinafter also referred to simply as the "distance between the first and second electrodes"; see FIG. 2( b)) is preferably adjusted to a range of 5 mm to 16 mm. Note that the "distance between the welding wire tips" referred to here refers to the distance between the centers of the welding wire tips of the respective electrodes.
[0036] If the distance a between the first and second electrodes is less than 5 mm, the current (electrons) flowing between the electrodes reduces the heat of the arc itself, which may result in insufficient melting of the groove surface 2. On the other hand, if the distance a between the first and second electrodes is greater than 16 mm, the outward electromagnetic force between the electrodes decreases inversely proportional to the distance, and no arc repulsion force is obtained to overcome the inward electromagnetic force generated by the current flowing through the groove surface 2. As a result, the arcs are directed inward, and heat is concentrated at the center of the groove. As a result, sufficient melting of the groove surface 2 may not be achieved.
[0037] Furthermore, in narrow gap welding, suppressing welding defects due to adhesion of spatter to the groove surface is an issue. However, by arranging the first electrode 3 and the second electrode 4 along predetermined parallel welding lines 8, 8, one of which is wire-negative (positive polarity) and the other is wire-positive (reverse polarity), and adjusting the distance a between the first and second electrodes to a range of 5 mm to 16 mm, the spatter is absorbed by the molten metal, suppressing adhesion of spatter to the groove surface, resulting in a sound weld.
[0038] In view of the above, it is preferable to adjust the distance a between the first and second electrodes to within the range of 5 mm to 16 mm.
[0039] [Angle α of the Line Connecting the Tips of the Welding Wires of the First and Second Electrodes: 60° or Less] In the present invention, melting of the groove face is ensured by utilizing the repulsion of the arc. However, if the angle α of the line connecting the tips of the welding wires of the first electrode 3 and the second electrode 4 with respect to the groove width direction (perpendicular to the weld line 8) exceeds 60°, a sufficient repulsive force of the arc cannot be obtained, and sufficient melting of the groove face may not be achieved. Therefore, the angle α of the line connecting the tips of the welding wires of the first electrode and the second electrode (hereinafter simply referred to as the "first-second electrode arrangement angle"; see FIG. 2(b)) is preferably 60° or less. More preferably, it is 50° or less. Note that the first-second electrode arrangement angle α may be 0°.
[0040] [Welding wire diameter: 1.0 mm to 1.6 mm] Welding wire for narrow-gap gas-shielded arc welding is generally manufactured with a diameter in the range of 0.6 mm to 2.0 mm. However, when welding with the same current, the thinner the wire diameter, the higher the deposition rate due to Joule heat. Therefore, to achieve highly efficient welding, it is preferable to select a relatively thin wire diameter. On the other hand, if the wire diameter is too thin, the wire will soften due to Joule heat, making the welding unstable. For this reason, the diameter of the welding wire used in the present invention is preferably in the range of 1.0 mm to 1.6 mm.
[0041] [Distance Between Adjacent Electrodes After the Second Electrode: 10 mm to 100 mm] The distance between adjacent electrodes after the second electrode 4, in the example of FIG. 2(b), is the distance b between the tips of the welding wires 4b, 5b supplied from the power feed tips 4a, 5a at the tip of the welding torch of the second electrode 4 and the third electrode 5 (hereinafter simply referred to as the "second-third electrode distance"). The distance c between the tips of the welding wires 5b, 6b supplied from the power feed tips 5a, 6a at the tip of the welding torch of the third electrode 5 and the fourth electrode 6 (hereinafter simply referred to as the "third-fourth electrode distance"). The distances b and c between adjacent electrodes after the second electrode 4 are preferably in the range of 10 mm to 100 mm. This range improves hot cracking resistance. More preferably, the distance is 12 mm to 80 mm.
[0042] [Positioning of Electrodes After the Third Electrode] If the weld buildup height exceeds the bottom groove gap G during first-layer welding, the risk of hot cracking increases. To avoid this, it is effective to position the third electrode 5 and subsequent electrodes in the center of the groove behind the first electrode 3 and the second electrode 4. The reason for this is that the final solidification region changes when the third electrode 5 and subsequent electrodes apply heat to the bead center. This also makes it possible to further reduce the number of layers, significantly reducing the risk of stacking defects in multi-layer welding. The reason for this is that it is possible to prevent bias in the weld metal within the groove. Note that the "groove center" here allows a range of ±10% of the bottom groove gap G from the center of the groove.
[0043] [Shielding gas: 20% by volume or more of CO 2 The amount of oxygen in the weld metal is also greatly affected by the shielding gas composition. Therefore, the shielding gas used in the narrow gap gas-shielded arc welding according to the present invention is a mixed gas containing CO 2 It is preferable to use a mixed gas containing 20% by volume or more of CO gas and the remainder being an inert gas such as Ar. 2 Gas: 100% by volume of a single gas. In the present invention, it is preferable to increase the oxygen concentration in the weld metal, which controls the flow of the weld metal, and direct the convection of the weld metal from the center outward, thereby stably increasing the fusion depth at the bottom of the steel sheets in the groove.
[0044] [REM Content of Welding Wire: 0.005% by Mass to 0.060% by Mass] REM (rare earth element) is an element effective in reducing the size of inclusions in the weld metal and improving toughness during welding. Furthermore, when welding is performed using a welding wire containing REM added to at least one electrode with positive polarity, droplet size can be reduced and transfer can be stabilized. This refinement of droplet transfer suppresses the generation of spatter and enables stable gas-shielded arc welding even with positive polarity. For these reasons, in the present invention, it is preferable to supply a steel wire containing REM (rare earth element) to at least one electrode with positive polarity. Note that elements other than REM are generally contained in appropriate amounts depending on the grade (steel type) of the welding wire, as specified in JIS Z 3312.
[0045] Here, if the REM content is less than 0.005% by mass, it is difficult to achieve the above-mentioned droplet refinement and stable transfer. On the other hand, if the REM content exceeds 0.060% by mass, cracks occur during the wire manufacturing process, making it difficult to manufacture the welding wire. Therefore, the REM content is preferably in the range of 0.005% to 0.060% by mass. More preferably, it is in the range of 0.010% to 0.055% by mass.
[0046] [Other Welding Conditions] In the present invention, other welding conditions than those described above do not need to be particularly limited and may be set in accordance with established standards, such as a welding voltage of 32 V to 37 V, a welding speed of 30 cm / min to 90 cm / min, and a welding wire extension length of 15 mm to 30 mm.
[0047] As shown in FIG. 2( a), the feed angle φ (hereinafter simply referred to as the “feed angle φ”) of the welding wires 3b and 4b of the first electrode 3 and the second electrode 4 relative to the bottom groove may be in the range of 0° to 15° with respect to the perpendicular. The feed angle φ is defined as a positive angle in the direction toward the groove face. The “perpendicular” here refers to a perpendicular line to the bottom groove. The distance d (hereinafter simply referred to as the “distance d”) between the side end of the welding wire tip of the first electrode 3 and the second electrode 4 and the bottom of the groove face 2 may be in the range of 0.1 mm to 3.0 mm. The radius of curvature of the welding wire supplied from the power feed tips 3a and 4a at the welding torch tips of the first electrode 3 and the second electrode 4 (hereinafter simply referred to as the “wire curvature radius”) may be in the range of 150 mm to 500 mm.
[0048] [Welding wire feed angle φ relative to the bottom groove: 0° to 15° relative to the perpendicular] The arc has directionality and tends to point in the direction that the tip of the electrode (welding wire) points. To effectively utilize this arc direction in melting the groove surface, it is advantageous to point the electrode tip toward the groove surface, and the direction that the electrode tip points varies greatly depending on the feed angle φ of the welding wire supplied from the power feed tip at the tip of the welding torch. The feed angle φ of the welding wire supplied from the power feed tip at the tip of the welding torch relative to the bottom groove is shown in Figure 2(a).
[0049] When the feed angle φ of the welding wires 3b and 4b supplied from the power feed tips 3a and 4a at the tip of the welding torch relative to the bottom groove is less than 0° relative to the vertical, the current flows through a path with less resistance. As a result, the arc creeps up the wire electrode (arc creep), making it difficult to maintain the desired fusion at the groove surface 2, particularly at the bottom. On the other hand, when the feed angle φ of the welding wire supplied from the power feed tip relative to the bottom groove exceeds 15° relative to the vertical, the arc is directed too far toward the groove surface 2, resulting in a convex weld bead shape. This results in insufficient arc melting in the first and subsequent layers of welding, making welding defects more likely to occur. For this reason, the feed angle φ of the welding wires 3b and 4b of the first and second electrodes 3 and 4 relative to the bottom groove is preferably in the range of 0° to 15° relative to the vertical. More preferably, it is 5° to 12°.
[0050] The feed angle φ of the welding wire of the first electrode 3 and the second electrode 4 relative to each bottom groove is the same as the inclination of the power feed tips 3 a and 4 a, particularly the inclination of the tips of the power feed tips. Therefore, the feed angle φ of the welding wire can be controlled by the inclination of the tips of the power feed tips.
[0051] [Distance d between the side end of the welding wire tip of the first electrode and the second electrode and the groove surface 2 of the steel sheet: 0.1 mm to 3.0 mm] The distance d ( FIG. 2( a) ) between the side end of the welding wire tip of the first electrode 3 and the second electrode 4 and the bottom of the groove surface 2 of the steel sheet is preferably 0.1 mm to 3.0 mm. If the distance d is less than 0.1 mm, an arc may be generated between the upper part of the wire and the groove surface 2, which may prevent efficient melting of the groove surface 2 at the bottom of the steel sheet. On the other hand, if the distance d exceeds 3.0 mm, the arc may be separated from the groove surface 2, which may prevent efficient melting of the groove surface 2. For this reason, the distance d is preferably set to 0.1 mm to 3.0 mm. More preferably, it is set to 0.5 mm to 2.0 mm, and even more preferably, it is set to 0.5 mm to 1.0 mm. Here, the "side end of the welding wire tip" refers to the side end closer to the groove surface 2 of the steel sheet to be melted by each electrode.
[0052] [Curvature Radius of Welding Wire Feed to Power Feed Tip: 150 mm to 500 mm] In the present invention, a power feed tip with a bent tip is used to control the feed angle φ of the welding wires 3b and 4b fed from the power feed tips 3a and 4a at the welding torch tips of the first electrode 3 and the second electrode 4. In this case, the welding wire passes through the bent power feed tip. To ensure smoother passage, it is preferable to pre-bend the welding wire using a so-called three-point roller or the like. If the curvature radius of the welding wire is less than 150 mm, the wire feed resistance increases, making it difficult to feed the welding wire stably and maintaining an arc. On the other hand, if the curvature radius of the welding wire exceeds 500 mm, the bending of the power feed tip is ineffective in reducing the wire feed resistance, making it difficult to feed the welding wire stably and maintaining an arc. In view of the above, the radius of curvature of the welding wires 3b and 4b fed to the power feed tips 3a and 4a of the first electrode 3 and the second electrode 4 is preferably 150 mm to 500 mm, and more preferably 175 mm to 475 mm.
[0053] The present invention will be further described below with reference to examples. However, the following examples are merely intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention.
[0054] The base metal (tensile strength 550 MPa or more) was prepared by gas cutting a steel plate with the groove shape shown in Table 1. Multi-layer, narrow-gap gas-shielded arc welding was performed on the base metal under the welding conditions shown in Tables 1 to 3, with one pass per layer, to produce welded joints. In all of the welding conditions shown in Tables 1 to 3, the third and subsequent electrodes were positioned in the center of the groove behind the first and second electrodes. The wire feed angle φ was 8°. The wire curvature radius was 300 mm.
[0055] The welded joints thus produced were inspected for the presence or absence of welding defects (hot cracking, poor fusion) after the cross section of the welded portion was corroded with nital, and no welding defects were found in any of the welded joints.
[0056] The weld metal of the welded joint was chemically analyzed, and the Ceq determined was in the range of 0.320 mass % or more in the inventive examples and less than 0.320 mass % in the comparative examples.
[0057] Round bar tensile test specimens were taken from the weld metal of the welded joint in accordance with the provisions of JIS Z 3111, and the tensile strength of the weld metal was evaluated. The evaluation results are shown in Table 4. As shown in Table 4, in all of the inventive examples, the tensile strength of the weld metal reached 550 MPa or more. In contrast, the tensile strength of the weld metal was below 550 MPa in Comparative Example No. 8, which had an average Ceq of less than 0.400 mass%, Comparative Example No. 9, which had a total heat input of more than 60 kJ / cm, and Comparative Example No. 10, which had a maximum / minimum heat input ratio of more than 1.40.
[0058]
[0059]
[0060]
[0061]
[0062] REFERENCE SIGNS LIST 1 steel plate 2 groove surface 3 first electrode 4 second electrode 5 third electrode 6 fourth electrode 3a, 4a, 5a, 6a power contact tip 3b, 4b, 5b, 6b welding wire 7 backing material 8 welding line 9 first layer weld bead 10 molten pool (second layer) 11 weld bead (second layer) during welding
Claims
1. A narrow-gap gas-shielded arc welding method for joining steel plates having a thickness t of 22 mm or more by multi-layer welding with a narrow gap having a groove angle θ of 25° or less and a bottom groove gap G of 7 mm to 18 mm, wherein the multi-layer welding is performed by multi-electrode welding with three or more electrodes, the average value obtained by dividing the sum of the carbon equivalents (Ceq) of each welding wire defined by the following formula (1) by the number of each electrode is 0.400 mass% or more, the ratio of the maximum heat input to the minimum heat input of each electrode is 1.40 or less, and the sum of the heat inputs of each electrode is 10 kJ / cm to 60 kJ / cm. Ceq=[C]+[Si] / 24+[Mn] / 6+[Ni] / 40+[Cr] / 5+[Mo] / 4+[V] / 14 (1) Here, [element] indicates the element content (mass%) in the welding wire, and 0 is substituted if no element is added.
2. The narrow gap gas-shielded arc welding method according to claim 1, wherein one of the first electrode and the second electrode is wire negative (positive polarity) and the other is wire positive (reverse polarity); the distance a between the tips of the welding wire supplied from the power feed tips at the tip of the welding torch of the first electrode and the second electrode is 5 mm to 16 mm; the angle α of a straight line connecting the welding wire tips of the first electrode and the second electrode with respect to the groove width direction is 60° or less; the diameter of the welding wire used for each electrode is in the range of 1.0 mm to 1.6 mm; and the distance between adjacent electrodes after the second electrode is 10 mm to 100 mm.
3. A narrow gap gas-shielded arc welding method as set forth in claim 2, wherein a third electrode and subsequent electrodes are positioned in the center of the groove behind the first electrode and the second electrode.
4. Shielding gas containing 20% or more CO by volume 2 The narrow gap gas-shielded arc welding method according to any one of claims 1 to 3, wherein a mixed gas containing a gas is used.
5. A narrow gap gas-shielded arc welding method according to any one of claims 1 to 4, wherein at least one of the welding wires used for the positive electrode contains 0.005% by mass to 0.060% by mass of REM (rare earth element).
Citation Information
Patent Citations
Narrow-gap gas shielded arc welding method
JP6137053B2
Narrow groove gas-shield arc-welding method
JP2015223605A
Gas-shielded arc welding method for steel sheets
WO2019182081A1