Negative electrode material and battery employing same
The use of lithium vanadium oxide in a negative electrode material with a sulfide solid electrolyte and conductive aid, optimized for volume ratios, addresses the conductivity limitations of lithium vanadium oxide, enhancing battery capacity and performance.
Patent Information
- Application Number
- PCT/JP2024/011306
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-03-22
- Publication Date
- 2024-11-28
AI Technical Summary
Lithium vanadium oxide, despite its high capacity and low reaction potential, faces challenges due to poor electronic conductivity, which limits battery capacity when used as a negative electrode active material, as increasing conductive additives reduces electrolyte and active material amounts, compromising ionic and electronic conductivity.
A negative electrode material composition comprising lithium vanadium oxide, a sulfide solid electrolyte, and a conductive aid, with specific volume ratios that balance electronic and ionic conductivity, enhancing battery capacity and charge/discharge characteristics.
The proposed configuration effectively increases battery capacity by maintaining a balance between electronic and ionic conductivity, improving energy density and input/output characteristics, while optimizing the volume ratios of active material, sulfide solid electrolyte, and conductive additive.
Smart Images

Figure JP2024011306_28112024_PF_FP_ABST
Abstract
Description
Negative electrode material and battery using the same
[0001] The present disclosure relates to a negative electrode material and a battery using the same.
[0002] Lithium vanadium oxide (LiVO) has attracted attention as a next-generation negative electrode active material due to its low reaction potential and high capacity. Patent Document 1 discloses a nonaqueous secondary battery using lithium vanadium oxide as the negative electrode active material.
[0003] JP 2008-77847 A
[0004] However, lithium vanadium oxide has poor electronic conductivity, so it is difficult to obtain a battery with sufficient capacity when using lithium vanadium oxide as a negative electrode active material.
[0005] Increasing the amount of conductive additive can improve the electronic conductivity of a lithium vanadium oxide-based negative electrode. However, increasing the amount of conductive additive means reducing the amount of electrolyte and / or the amount of lithium vanadium oxide as the active material. Reducing the amount of electrolyte reduces the ionic conductivity of the negative electrode. Reducing the amount of lithium vanadium oxide as the active material reduces the battery capacity.
[0006] An object of the present disclosure is to provide a technique for increasing the capacity of a battery using lithium vanadium oxide.
[0007] The present disclosure provides an anode material comprising: an anode active material; a sulfide solid electrolyte; and a conductive additive, wherein the anode active material contains lithium vanadium oxide; a ratio of the volume of the anode active material to a total volume of the anode active material and the sulfide solid electrolyte is 40% or more and 80% or less; and a ratio of the volume of the conductive additive to a total volume of the anode active material, the sulfide solid electrolyte, and the conductive additive is more than 4.4% and 15% or less.
[0008] According to the present disclosure, the capacity of a battery using lithium vanadium oxide can be increased.
[0009] Fig. 1 shows a cross-sectional view of an anode material 1000 according to a first embodiment. Fig. 2 shows a cross-sectional view of a battery 2000 according to a second embodiment. Fig. 3 shows a cross-sectional view of a battery 3000 according to a modified example.
[0010] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. The present disclosure is not limited to the following embodiments.
[0011] First Embodiment FIG. 1 shows a cross-sectional view of a negative electrode material 1000 according to a first embodiment. The negative electrode material 1000 includes a negative electrode active material 111, a sulfide solid electrolyte 100, and a conductive additive 110. The negative electrode active material 111, the sulfide solid electrolyte 100, and the conductive additive 110 each have a particle shape. The negative electrode active material 111 includes lithium vanadium oxide. The lithium vanadium oxide is an oxide containing lithium and vanadium. In this specification, the oxide containing lithium and vanadium will be simply referred to as "vanadium oxide."
[0012] In the negative electrode material 1000, the ratio of the volume of the negative electrode active material 111 to the total volume of the negative electrode active material 111 and the sulfide solid electrolyte 100 is 40% or more and 80% or less. The ratio of the volume of the conductive additive 110 to the total volume of the negative electrode active material 111, the sulfide solid electrolyte 100, and the conductive additive 110 is more than 4.4% and 15% or less. With this configuration, a balance between electronic conductivity and ionic conductivity can be achieved in the negative electrode of a battery using the negative electrode material 1000. As a result, a battery using the negative electrode material 1000 exhibits high capacity.
[0013] The negative electrode material 1000 according to the first embodiment can be used, for example, to obtain a battery having excellent charge / discharge characteristics. The negative electrode material 1000 according to the first embodiment is suitable, for example, for improving battery capacity. An example of the battery is a solid-state battery. The solid-state battery may be a primary battery or a secondary battery.
[0014] The vanadium oxide contained in the negative electrode active material 111 may be a material represented by the following composition formula (1). In composition formula (1), 0≦x<1.0 and 0≦α≦1.0 are satisfied. M is at least one element selected from the group consisting of tetravalent metal elements and tetravalent metalloid elements. Li can be inserted into and removed from the vanadium oxide represented by composition formula (1).
[0015] Li (3+α+x) V (1-x) M x O (4+α / 2) ...(1)
[0016] In composition formula (1), 0 < α < 1.0 may be satisfied. In other words, the vanadium oxide represented by composition formula (1) may contain Li and O in amounts exceeding those derived from the stoichiometric composition. With this configuration, the negative electrode material 1000 according to the first embodiment can improve battery capacity. This is because the excess Li and O improve the electronic conductivity of the vanadium oxide, facilitating the insertion and desorption of Li into the vanadium oxide. A stoichiometric composition refers to a composition in which the molar ratio of the elements constituting the vanadium oxide is an integer multiple. For example, Li3VO4 has a stoichiometric composition.
[0017] The amount of Li and O represented by α in composition formula (1) may be incorporated into the vanadium oxide particles, or may exist outside the particles as a second phase different from the first phase constituting the particles.
[0018] In the composition formula (1), 0<α<0.85 may be satisfied, or 0.2≦α≦0.6 may be satisfied. According to this configuration, the negative electrode material 1000 according to the first embodiment can improve the battery capacity.
[0019] As described above, M is at least one element selected from tetravalent metal elements and tetravalent metalloid elements. Examples of tetravalent metal elements and tetravalent metalloid elements include Ti, Zr, Si, Ge, and Sn. When the pentavalent V element is substituted with a tetravalent metal element and / or a tetravalent metalloid element, holes and / or Li ions become charge carriers. This makes it easier to insert and extract Li into the vanadium oxide.
[0020] In the composition formula (1), M may contain Ti. According to this configuration, the negative electrode material 1000 according to the first embodiment can improve the battery capacity. M may be Ti.
[0021] In the composition formula (1), 0<x<1.0 may be satisfied. With this configuration, the negative electrode material 1000 according to the first embodiment can improve the battery capacity. This is thought to be because the electronic conductivity of the vanadium oxide is improved by replacing some of the vanadium ions with ions of the metal M.
[0022] In the composition formula (1), 0<x≦0.1 may be satisfied. According to this configuration, the negative electrode material 1000 according to the first embodiment can improve the battery capacity. x may be in the range of 0.04 or more and 0.06 or less.
[0023] In the composition formula (1), when x satisfies the above range, insertion and desorption of Li into and from the vanadium oxide becomes easier. Therefore, as described above, the negative electrode material 1000 according to the first embodiment can improve the battery capacity.
[0024] From the viewpoint of the energy density and input / output characteristics of the battery, the ratio of the volume of the negative electrode active material 111 to the total volume of the negative electrode active material 111 and the sulfide solid electrolyte 100 may be 50% or more. With this configuration, a further improvement in battery capacity can be expected.
[0025] From the viewpoint of the energy density and input / output characteristics of the battery, the ratio of the volume of the negative electrode active material 111 to the total volume of the negative electrode active material 111 and the sulfide solid electrolyte 100 may be 70% or less. With this configuration, a further improvement in battery capacity can be expected.
[0026] From the viewpoint of the energy density and input / output characteristics of the battery, the ratio of the volume of the conductive additive 110 to the total volume of the negative electrode active material 111, the sulfide solid electrolyte 100, and the conductive additive 110 may be 5.8% or more. With this configuration, a further improvement in battery capacity can be expected.
[0027] From the viewpoint of the energy density and input / output characteristics of the battery, the ratio of the volume of the conductive additive 110 to the total volume of the negative electrode active material 111, the sulfide solid electrolyte 100, and the conductive additive 110 may be 13.8% or less. With this configuration, a further improvement in battery capacity can be expected.
[0028] In a battery including the negative electrode material 1000, the volumes of the negative electrode active material 111, the sulfide solid electrolyte 100, and the conductive additive 110 can be directly determined by obtaining a three-dimensional SEM image of the negative electrode of the battery using a three-dimensional SEM observation method. The three-dimensional SEM observation method is a method of obtaining a three-dimensional image of an object to be observed by repeating focused ion beam processing and SEM observation.
[0029] The particles of the negative electrode active material 111 are particles containing vanadium oxide. The particles of the negative electrode active material 111 may be particles containing vanadium oxide of composition formula (1) as a main component. Particles containing vanadium oxide of composition formula (1) as a main component refer to particles in which the component contained most abundantly by mass is vanadium oxide of composition formula (1). The particles of the negative electrode active material 111 may be particles made of vanadium oxide of composition formula (1).
[0030] The particles of the negative electrode active material 111 may have a median diameter of 0.1 μm or more and 100 μm or less. When the particles of the negative electrode active material 111 have a median diameter of 0.1 μm or more, the particles of the negative electrode active material 111 and the particles of the sulfide solid electrolyte 100 can be well dispersed in the negative electrode of the battery. This improves the charge / discharge characteristics of the battery. When the particles of the negative electrode active material 111 have a median diameter of 100 μm or less, the lithium diffusion rate within the particles of the negative electrode active material 111 improves. This allows the battery to operate at high power. The particles of the negative electrode active material 111 may have a median diameter of 0.5 μm or more and 10 μm or less.
[0031] The particles of the sulfide solid electrolyte 100 may have a median diameter of 1 nm or more and 10 μm or less, or may have a median diameter of 1 nm or more and 1 μm or less. With the above configuration, the negative electrode active material 111 and the sulfide solid electrolyte 100 can be well dispersed in the negative electrode. The particles of the conductive additive 110 may have a median diameter of 1 nm or more and 100 μm or less.
[0032] The particles of the negative electrode active material 111 may have a larger median diameter than the particles of the sulfide solid electrolyte 100. This allows the particles of the negative electrode active material 111 and the particles of the sulfide solid electrolyte 100 to be dispersed well.
[0033] The median particle size refers to the particle size (d50) corresponding to 50% cumulative volume in the volume-based particle size distribution. The volume-based particle size distribution can be measured using a laser diffraction measurement device or an image analysis device.
[0034] The sulfide solid electrolyte 100 is a solid electrolyte containing sulfur. Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, and Li 3.25 Ge 0.25 P 0.75 S4, Li 10 GeP2S 12 And so on.
[0035] The conductive additive 110 improves the electronic conductivity of the negative electrode material 1000. Examples of the conductive additive 110 include graphites such as natural graphite and artificial graphite; carbon blacks such as acetylene black and ketjen black; conductive fibers such as carbon fiber and metal fiber; carbon fluoride; metal powders such as aluminum; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymer compounds such as polyaniline, polypyrrole, and polythiophene. The conductive additive may be a carbon material such as carbon black or carbon fiber.
[0036] The shapes of the particles of the negative electrode active material 111, the particles of the sulfide solid electrolyte 100, and the conductive additive 110 are not limited. Examples of these shapes include needles, spheres, ellipsoids, etc. The negative electrode active material 111 may be formed into a pellet or plate shape.
[0037] <Method for Producing Vanadium Oxide> Vanadium oxide as the negative electrode active material 111 can be produced by the following method.
[0038] Raw material powders are prepared to have a desired composition, and examples of raw material powders include oxides, hydroxides, carbonates, nitrates, and organic salts.
[0039] As an example, the composition formula (1): Li (3+α+x) V (1-x) M x O (4+α / 2) In the vanadium oxide represented by the formula (1), it is assumed that M is Ti, x is 0.05 when the raw materials are mixed, and α is 0. At this time, Li2CO3, VO, and TiO2 are mixed in a molar ratio of Li2CO3:VO:TiO2 = (3.05 / 2):(0.95 / 2):0.05.
[0040] When α≠0, a Li source material, for example, Li2CO3, may be further added and mixed with the raw material powder, taking into consideration the value of α in the target composition. The amount of the excess Li source to be mixed in excess can be determined appropriately depending on, for example, the value of α in the target composition and the material used as the Li source. For example, to produce a vanadium oxide that satisfies 0<x<1.0 and 0<α<1.0, the Li source may be used in excess in the range of, for example, 0.5% by mass to 40% by mass, or 1% by mass to 30% by mass, relative to the amount of the Li source whose molar ratio is determined assuming that α is 0.
[0041] Lithium hydroxide or its hydrate may be used instead of Li2CO3.
[0042] The mixture of raw material powders is fired to obtain a reaction product. The firing atmosphere may be air or an inert gas atmosphere. The inert atmosphere is, for example, an argon atmosphere or a nitrogen atmosphere.
[0043] Alternatively, a mixture of raw material powders may be reacted with each other mechanochemically (by mechanochemical milling) in a mixing device such as a planetary ball mill to obtain a reactant.
[0044] By these methods, the vanadium oxide according to the first embodiment can be obtained.
[0045] Here, the molar ratio of the raw materials when mixed does not necessarily match the molar ratio of the reactants, because the raw materials may not be incorporated into the reactants due to evaporation during the reaction.
[0046] The composition of vanadium oxide is determined by quantitative analysis. Li is quantified by atomic absorption spectrometry. V and M are quantified by high-frequency inductively coupled plasma (ICP) atomic emission spectrometry. The value of x in composition formula (1) can be determined from the amount of element M in the vanadium oxide. The value of α in composition formula (1) can be determined from the amount of Li and the amount of element M in the vanadium oxide.
[0047] Second Embodiment A second embodiment will be described below, and the matters described in the first embodiment will be omitted as appropriate.
[0048] The battery according to the second embodiment comprises a positive electrode, an electrolyte layer, and a negative electrode, the electrolyte layer being disposed between the positive electrode and the negative electrode, and the negative electrode including the negative electrode material according to the first embodiment.
[0049] The battery according to the second embodiment has excellent charge / discharge characteristics.
[0050] FIG. 2 shows a cross-sectional view of a battery 2000 according to a second embodiment.
[0051] The battery 2000 includes a positive electrode 201, an electrolyte layer 202, and a negative electrode 203. The electrolyte layer 202 is disposed between the positive electrode 201 and the negative electrode 203.
[0052] The positive electrode 201 contains a positive electrode active material and a solid electrolyte.
[0053] The electrolyte layer 202 contains an electrolyte material, such as a solid electrolyte material.
[0054] The negative electrode 203 contains the negative electrode material 1000 according to the first embodiment.
[0055] To improve the energy density and output of the battery 2000, the negative electrode 203 may have a thickness of 10 μm or more and 500 μm or less.
[0056] The positive electrode 201 contains a material capable of absorbing and releasing metal ions such as lithium ions, and also contains, for example, a positive electrode active material (for example, particles of a positive electrode active material).
[0057] Examples of the positive electrode active material include lithium-containing transition metal oxides, transition metal fluorides, polyanion materials, fluorinated polyanion materials, transition metal sulfides, transition metal oxysulfides, transition metal oxynitrides, etc. Examples of lithium-containing transition metal oxides include Li(Ni,Co,Al)O, Li(Ni,Co,Mn)O, LiCoO, etc.
[0058] In the present disclosure, "(A, B, C)" means "at least one selected from the group consisting of A, B, and C."
[0059] From the viewpoint of cost and safety of the battery 2000, lithium phosphate or lithium-containing transition metal phosphate may be used as the positive electrode active material.
[0060] The particles of the positive electrode active material may have a median diameter of 0.1 μm or more and 100 μm or less. When the particles of the positive electrode active material have a median diameter of 0.1 μm or more, the particles of the positive electrode active material and the particles of the solid electrolyte can be well dispersed in the positive electrode 201. This improves the charge / discharge characteristics of the battery. When the particles of the positive electrode active material have a median diameter of 100 μm or less, the lithium diffusion rate within the particles of the positive electrode active material improves. This allows the battery 2000 to operate at high power.
[0061] The particles of the positive electrode active material may have a larger median diameter than the particles of the solid electrolyte, which allows the particles of the positive electrode active material and the particles of the solid electrolyte to be dispersed well.
[0062] In order to improve the energy density and output of the battery 2000, the ratio of the volume of the positive electrode active material to the sum of the volume of the positive electrode active material and the volume of the solid electrolyte in the positive electrode 201 may be 0.30 or more and 0.95 or less.
[0063] A coating layer may be formed on the surface of the positive electrode active material particles to prevent the positive electrode active material from reacting with the solid electrolyte. This can suppress an increase in the reaction overvoltage of the battery. Examples of coating materials included in the coating layer include solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, polymer solid electrolytes, and halide solid electrolytes.
[0064] The coating material may be a halide solid electrolyte or an oxide solid electrolyte. The halide solid electrolyte may contain F. This improves the stability of the coating material at high potentials. As a result, the battery 2000 has high charge / discharge efficiency. The oxide solid electrolyte may be lithium niobate or a polyanion material, which has excellent stability even at high potentials. As a result, the battery 2000 has high charge / discharge efficiency.
[0065] To improve the energy density and output of the battery 2000, the positive electrode 201 may have a thickness of 10 μm or more and 500 μm or less.
[0066] The solid electrolyte contained in the positive electrode 201 may be a solid electrolyte such as a sulfide solid electrolyte, a halide solid electrolyte, an oxide solid electrolyte, a polymer solid electrolyte, or an organic polymer solid electrolyte.
[0067] In the present disclosure, a "sulfide solid electrolyte" refers to a solid electrolyte containing sulfur. An "oxide solid electrolyte" refers to a solid electrolyte containing oxygen. The oxide solid electrolyte may contain anions other than oxygen (excluding sulfur anions and halogen anions). A "halide solid electrolyte" refers to a solid electrolyte that contains a halogen element but does not contain sulfur. The halide solid electrolyte may contain not only a halogen element but also oxygen.
[0068] Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, and Li 3.25 Ge 0.25 P 0.75 S4, Li 10 GeP2S 12 And so on.
[0069] Examples of halide solid electrolytes include Li a Me b Y c X6, where the formula: a + mb + 3c = 6, and c > 0 is satisfied. Me is at least one element selected from the group consisting of metal elements other than Li and Y and metalloid elements. X is at least one element selected from the group consisting of F, Cl, Br, and I. The value of m represents the valence of Me.
[0070] "Metalloid elements" are B, Si, Ge, As, Sb, and Te. "Metal elements" are all elements in groups 1 to 12 of the periodic table (except H) and all elements in groups 13 to 16 of the periodic table (except B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se).
[0071] In order to increase the ionic conductivity of the halide solid electrolyte, Me may be at least one selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta, and Nb.
[0072] Another example of a halide solid electrolyte is Li α’ Me' β O γ X δ where α', β, γ, and δ are all greater than 0, Me' is at least one element selected from the group consisting of metal elements and metalloid elements other than Li, X is at least one element selected from the group consisting of Cl, Br, and I, and the following mathematical formulas are satisfied: 0.9≦α'≦1.2, β=1.0, 1.0≦γ≦1.3, and 3.6≦δ≦4.0.
[0073] Examples of oxide solid electrolytes include: (i) NASICON-type solid electrolytes such as LiTi2(PO4)3 and elemental substitution products thereof; (ii) perovskite-type solid electrolytes such as (LaLi)TiO3; (iii) Li 14 ZnGeO 16 LISICON-type solid electrolytes such as LiSiO, LiGeO, and elemental substitution products thereof; (iv) LiLaZrO 12 (v) Li3PO4 or an N-substituted LiPO4, etc.
[0074] An example of a polymer solid electrolyte is a compound of a polymer compound and a lithium salt. The polymer compound may have an ethylene oxide structure. A polymer compound having an ethylene oxide structure can contain a large amount of lithium salt, and therefore has higher ionic conductivity. The polymer solid electrolyte may be, for example, a composite compound of polyethylene oxide and a lithium salt. An example of such a polymer solid electrolyte is lithium bis(trifluoromethanesulfonyl)imide.
[0075] Examples of lithium salts include LiPF, LiBF, LiSbF, LiAsF, LiSOCF, LiN(SOCF), LiN(SOCF), LiN(SOCF)(SOCF), LiC(SOCF), etc. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used.
[0076] The positive electrode 201 may contain the conductive additive described above for the purpose of increasing electronic conductivity.
[0077] The electrolyte layer 202 contains an electrolyte material. The electrolyte material is, for example, a solid electrolyte material. The electrolyte layer 202 may be a solid electrolyte layer. The solid electrolyte material contained in the electrolyte layer 202 may be a sulfide solid electrolyte, a halide solid electrolyte, or a polymer solid electrolyte.
[0078] The electrolyte layer 202 may have a thickness of 1 μm or more and 100 μm or less. When the electrolyte layer 202 has a thickness of 1 μm or more, the cathode 201 and the anode 203 are less likely to short-circuit. When the electrolyte layer 202 has a thickness of 100 μm or less, the battery 2000 can operate at high power.
[0079] At least one selected from the group consisting of the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a non-aqueous electrolyte, a gel electrolyte, or an ionic liquid for the purpose of facilitating the exchange of lithium ions and improving the output characteristics of the battery.
[0080] The nonaqueous electrolyte contains a nonaqueous solvent and a lithium salt dissolved in the nonaqueous solvent. Examples of the nonaqueous solvent include cyclic carbonate ester solvents, chain carbonate ester solvents, cyclic ether solvents, chain ether solvents, cyclic ester solvents, chain ester solvents, and fluorine solvents. Examples of the cyclic carbonate ester solvents include ethylene carbonate, propylene carbonate, and butylene carbonate. Examples of the chain carbonate ester solvents include dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate. Examples of the cyclic ether solvents include tetrahydrofuran, 1,4-dioxane, and 1,3-dioxolane. Examples of the chain ether solvents include 1,2-dimethoxyethane and 1,2-diethoxyethane. An example of the cyclic ester solvent is γ-butyrolactone. An example of the chain ester solvent is methyl acetate. Examples of fluorine-containing solvents include fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, fluoroethyl methyl carbonate, and fluorodimethylene carbonate. One nonaqueous solvent selected from these may be used alone. Alternatively, a mixture of two or more nonaqueous solvents selected from these may be used.
[0081] Examples of lithium salts include LiPF, LiBF, LiSbF, LiAsF, LiSOCF, LiN(SOCF), LiN(SOCF), LiN(SOCF)(SOCF), and LiC(SOCF). One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used. The concentration of the lithium salt is, for example, in the range of 0.5 mol / L to 2 mol / L.
[0082] The gel electrolyte may be a polymer material impregnated with a non-aqueous electrolyte solution, such as polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polymethyl methacrylate, or a polymer having an ethylene oxide bond.
[0083] Examples of cations contained in the ionic liquid include: (i) aliphatic chain quaternary salts such as tetraalkylammonium and tetraalkylphosphonium; (ii) aliphatic cyclic ammoniums such as pyrrolidiniums, morpholiniums, imidazoliniums, tetrahydropyrimidiniums, piperaziniums, and piperidiniums; and (iii) nitrogen-containing heterocyclic aromatic cations such as pyridiniums and imidazoliums.
[0084] An example of an anion contained in an ionic liquid is PF6 - , BF4 - , SbF6 - , AsF6 - , SO3CF3 - , N(SO2CF3)2 - , N(SO2C2F5)2 - , N(SO2CF3)(SO2C4F9) - , C(SO2CF3)3 - And so on.
[0085] The ionic liquid may contain a lithium salt.
[0086] At least one selected from the group consisting of the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a binder for the purpose of improving adhesion between particles.
[0087] Examples of binders include polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polymethyl ester of acrylic acid, polyethyl ester of acrylic acid, polyhexyl ester of acrylic acid, polymethacrylic acid, polymethyl ester of methacrylic acid, polyethyl ester of methacrylic acid, polyhexyl ester of methacrylic acid, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, hexafluoropolypropylene, styrene-butadiene rubber, and carboxymethyl cellulose. Copolymers may also be used as binders. Examples of such binders include copolymers of two or more materials selected from the group consisting of tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene. Mixtures of two or more materials selected from the above materials may also be used.
[0088] FIG. 3 shows a cross-sectional view of a battery 3000 according to a modified example. As shown in FIG. 3 , another electrolyte layer (i.e., a second electrolyte layer) may be further provided between the electrolyte layer 202 and the negative electrode 203. When the electrolyte layer 202 is composed of a first electrolyte layer 212 and a second electrolyte layer 222, the second electrolyte layer 222 may be composed of a different solid electrolyte material that is electrochemically more stable than the first electrolyte layer 212. Specifically, the reduction potential of the solid electrolyte material constituting the second electrolyte layer 222 may be lower than the reduction potential of the solid electrolyte material constituting the first electrolyte layer 212. This allows the solid electrolyte material contained in the first electrolyte layer 212 to be used without being reduced. As a result, the charge / discharge efficiency of the battery 3000 can be improved.
[0089] Examples of the shape of the battery according to the second embodiment include coin type, cylindrical type, square type, sheet type, button type, flat type, and laminate type.
[0090] The battery according to the second embodiment may be manufactured, for example, by preparing a material for forming a positive electrode, a material for forming an electrolyte layer, and a material for forming a negative electrode, and by a known method, fabricating a laminate in which the positive electrode, the electrolyte layer, and the negative electrode are arranged in this order.
[0091] (Other Embodiments) (Additional Notes) The above description of the embodiments discloses the following techniques.
[0092] (Technology 1) An anode material comprising: a negative electrode active material; a sulfide solid electrolyte; and a conductive additive, wherein the negative electrode active material contains lithium vanadium oxide; a ratio of the volume of the negative electrode active material to a total volume of the negative electrode active material and the sulfide solid electrolyte is 40% or more and 80% or less; and a ratio of the volume of the conductive additive to a total volume of the negative electrode active material, the sulfide solid electrolyte, and the conductive additive is more than 4.4% and 15% or less.
[0093] According to Technique 1, it is possible to achieve a balance between electronic conductivity and ionic conductivity in the negative electrode of a battery using the negative electrode material, and as a result, the battery using the negative electrode material exhibits a high capacity.
[0094] (Technology 2) The lithium vanadium oxide has the composition formula Li (3+α+x) V (1-x) M x O (4+α / 2) In the composition formula, 0≦x<1.0 and 0≦α≦1.0 are satisfied, and in the composition formula, M is at least one element selected from the group consisting of tetravalent metal elements and tetravalent metalloid elements. The negative electrode material according to Technology 1 is capable of inserting and extracting Li into the vanadium oxide represented by composition formula (1).
[0095] (Technology 3) The negative electrode material according to Technology 2, wherein in the composition formula, M contains Ti.
[0096] (Technology 4) The negative electrode material according to Technology 2 or 3, wherein in the composition formula, 0<x<1.0 is satisfied.
[0097] (Technology 5) The negative electrode material according to Technology 2 or 3, wherein in the composition formula, 0<x≦0.1 is satisfied.
[0098] (Technology 6) The negative electrode material according to any one of Technologies 2 to 5, wherein in the composition formula, 0<α<1.0 is satisfied.
[0099] The negative electrode materials of techniques 3 to 6 are more suitable for improving battery capacity.
[0100] (Technology 7) The negative electrode material according to any one of Technologies 1 to 6, wherein the volume ratio of the negative electrode active material is 50% or more.
[0101] (Technology 8) The negative electrode material according to any one of Technologies 1 to 6, wherein the volume ratio of the negative electrode active material is 70% or less.
[0102] (Technology 9) The negative electrode material according to any one of Technologies 1 to 8, wherein the volume ratio of the conductive additive is 5.8% or more.
[0103] (Technology 10) The negative electrode material according to any one of Technologies 1 to 8, wherein the volume ratio of the conductive additive is 13.8% or less.
[0104] The negative electrode materials of Techniques 7 to 10 can improve the energy density and input / output characteristics of the battery.
[0105] (Technology 11) A battery comprising: a positive electrode; a negative electrode containing the negative electrode material according to any one of technologies 1 to 10; and an electrolyte layer disposed between the positive electrode and the negative electrode.
[0106] The battery according to Technique 11 exhibits high capacity.
[0107] Hereinafter, the present disclosure will be described in detail using examples and comparative examples.
[0108] Example 1 Preparation of Vanadium Oxide As raw material powders, Li2CO3 (manufactured by Kojundo Chemical Laboratory Co., Ltd., purity 99.9%), VO (manufactured by Kojundo Chemical Laboratory Co., Ltd., purity 99.9%), and TiO2 (manufactured by Kojundo Chemical Laboratory Co., Ltd., purity 99.9%) were prepared in a molar ratio of Li2CO3:VO5:TiO2 = 1.525:0.475:0.05. These raw material powders were mixed in a mortar to obtain a mixed powder. The obtained mixed powder was calcined in the air at 600°C for 3 hours. The obtained calcined powder was then fired in the air at 920°C for 15 hours. In both the calcination and the calcination, the temperature increase rate was 10°C per minute and the temperature decrease rate was 5°C per minute. In this manner, vanadium oxide was obtained.
[0109] In vanadium oxide, the composition formula (1): Li (3+α+x) V (1-x) M x O (4+α / 2) In this case, x was 0.05 and α was 0.06.
[0110] x was determined by analyzing the amount of Ti using an ICP optical emission spectrometer (PS3520VDDII manufactured by Hitachi High-Tech Science Corporation). α was determined by analyzing the amount of Li using an atomic absorption spectrophotometer (Z-2300 manufactured by Hitachi High-Tech Norges Corporation) and comparing the results with the amount of Ti (i.e., the value of x).
[0111] [Battery Fabrication] Vanadium oxide and Li3PS4 as a solid electrolyte were prepared in an argon atmosphere with a dew point of −60°C or lower at a volume ratio of 40:60 vanadium oxide:Li3PS4. These materials were mixed in an agate mortar. Next, acetylene black as a conductive additive was added in an amount of 8% by mass relative to the vanadium oxide, and the mixture was mixed in the agate mortar. In this way, a negative electrode mixture (negative electrode material) was obtained. The volume ratio of acetylene black to the total volume of the negative electrode mixture was 5.8%.
[0112] Li3PS4 (80 mg) and the negative electrode mixture were stacked in an insulating cylinder with an inner diameter of 9.5 mm to obtain a laminate. The negative electrode mixture was added so that the negative electrode active material amounted to 3.78 mg. A pressure of 360 MPa was applied to this laminate to form a solid electrolyte layer and a negative electrode. The solid electrolyte layer had a thickness of 500 μm.
[0113] Next, Li (thickness: 300 μm) was laminated on the solid electrolyte layer, and a pressure of 80 MPa was applied to this laminate to form a positive electrode.
[0114] Next, current collectors made of stainless steel were attached to the positive and negative electrodes, and current collecting leads were attached to the current collectors.
[0115] Finally, the inside of the insulating tube was isolated from the outside atmosphere using an insulating ferrule, and the inside of the tube was sealed.
[0116] As a result, a battery according to Example 1 was obtained. The battery according to Example 1 is a single-electrode test cell in which the negative electrode serves as a working electrode and the positive electrode serves as a counter electrode, and is used to test the performance of the negative electrode. Specifically, the negative electrode to be tested is used as the working electrode, and an appropriate active material in an amount sufficient to cover the reaction at the working electrode is used as the counter electrode. Since this test cell is intended to test the performance of the negative electrode, metallic Li was used as the counter electrode. The negative electrode whose performance has been tested using such a test cell can be used as a secondary battery, for example, by combining it with a positive electrode containing a positive electrode active material such as that described in the above-described embodiment, such as a transition metal oxide containing Li.
[0117] [Charge-Discharge Test] The battery according to Example 1 was placed in a thermostatic chamber maintained at 25°C.
[0118] The battery according to Example 1 was discharged at a current value corresponding to a 0.1 C rate (10-hour rate) relative to the theoretical capacity of the battery until a voltage of 0.3 V was reached. Next, the battery according to Example 1 was charged at a current value corresponding to a 0.05 C rate until a voltage of 2.5 V was reached. After two cycles of charge and discharge at the above rates, the battery was discharged at a current value corresponding to a 0.5 C rate (2-hour rate) until a voltage of 0.3 V was reached. Further, the battery was charged at a current value corresponding to a 0.05 C rate until a voltage of 2.5 V was reached, and then discharged at a current value corresponding to a 1 C rate (1-hour rate) until a voltage of 0.3 V was reached.
[0119] As a result of the charge / discharge test, the charge capacity of the battery according to Example 1 was 135.8 mAh / g at 0.5 C. Since the batteries according to the examples and comparative examples are half cells using a Li metal negative electrode, the charge capacities of the batteries according to the examples and comparative examples correspond to the discharge capacities of the batteries described with reference to FIG.
[0120] In the following Examples 2 to 8 and Comparative Examples 1 to 4, the methods for fabricating the batteries and the methods for the charge / discharge tests of the batteries were the same as those in Example 1.
[0121] Example 2 A battery of Example 2 was fabricated in the same manner as Example 1, except that acetylene black as a conductive additive was added in an amount of 10 mass% relative to the vanadium oxide. In Example 2, the ratio of the volume of acetylene black to the total volume of the negative electrode mixture was 7.1%.
[0122] As a result of the charge / discharge test, the charge capacity of the battery of Example 2 at 0.5 C was 207.4 mAh / g.
[0123] Example 3 A battery of Example 3 was fabricated in the same manner as Example 1, except that acetylene black as a conductive additive was added in an amount of 12 mass% relative to the vanadium oxide. In Example 3, the ratio of the volume of acetylene black to the total volume of the negative electrode mixture was 8.4%.
[0124] As a result of the charge / discharge test, the charge capacity of the battery of Example 3 at 0.5 C was 230.6 mAh / g.
[0125] Example 4: Vanadium oxide and Li3PS4 were prepared in a volume ratio of 50:50 vanadium oxide:Li3PS4 in an argon atmosphere having a dew point of −60°C or lower. These materials were mixed in an agate mortar. Next, acetylene black as a conductive additive was added in an amount of 8% by mass relative to the vanadium oxide, and the mixture was mixed in the agate mortar. In this manner, a negative electrode mixture was obtained. The volume ratio of acetylene black to the total volume of the negative electrode mixture was 7.1%.
[0126] Using the negative electrode mixture, a battery of Example 4 was fabricated in the same manner as in Example 1. As a result of a charge-discharge test, the charge capacity of the battery of Example 4 at 0.5 C was 190.7 mAh / g.
[0127] Example 5: Vanadium oxide and Li3PS4 were prepared in a volume ratio of 60:40 vanadium oxide:Li3PS4 in an argon atmosphere having a dew point of −60°C or lower. These materials were mixed in an agate mortar. Next, 10% by mass of acetylene black was added as a conductive additive to the vanadium oxide, and the mixture was mixed in the agate mortar. In this manner, a negative electrode mixture was obtained. The volume ratio of acetylene black to the total volume of the negative electrode mixture was 10.0%.
[0128] Using the negative electrode mixture, a battery of Example 5 was fabricated in the same manner as in Example 1. As a result of a charge-discharge test, the charge capacity of the battery of Example 5 at 0.5 C was 261.5 mAh / g.
[0129] Example 6 A battery of Example 6 was fabricated in the same manner as Example 5, except that acetylene black was added as a conductive additive in an amount of 12 mass% relative to the vanadium oxide. In Example 6, the ratio of the volume of acetylene black to the total volume of the negative electrode mixture was 12.1%.
[0130] As a result of the charge / discharge test, the charge capacity of the battery of Example 6 at 0.5 C was 224.2 mAh / g.
[0131] Example 7 A battery of Example 7 was fabricated in the same manner as Example 5, except that acetylene black as a conductive additive was added in an amount of 14 mass% relative to the vanadium oxide. In Example 7, the ratio of the volume of acetylene black to the total volume of the negative electrode mixture was 13.8%.
[0132] As a result of the charge-discharge test, the charge capacity of the battery of Example 7 at 0.5 C was 223.4 mAh / g.
[0133] Example 8: Vanadium oxide and Li3PS4 were prepared in an argon atmosphere having a dew point of −60°C or lower at a volume ratio of 80:20 vanadium oxide:Li3PS4. These materials were mixed in an agate mortar. Next, acetylene black was added as a conductive additive in an amount of 4% by mass relative to the vanadium oxide, and the mixture was mixed in the agate mortar. In this manner, a negative electrode mixture was obtained. The volume ratio of acetylene black to the total volume of the negative electrode mixture was 5.8%.
[0134] Using the negative electrode mixture, a battery of Example 8 was fabricated in the same manner as in Example 1. As a result of a charge-discharge test, the charge capacity of the battery of Example 8 at 0.5 C was 146.0 mAh / g.
[0135] Comparative Example 1 A battery of Comparative Example 1 was fabricated in the same manner as in Example 8, except that acetylene black as a conductive additive was added in an amount of 3 mass% relative to the vanadium oxide. In Comparative Example 1, the ratio of the volume of acetylene black to the total volume of the negative electrode mixture was 4.4%.
[0136] As a result of the charge / discharge test, the charge capacity of the battery according to Comparative Example 1 at 0.5 C was 0.01 mAh / g.
[0137] Comparative Example 2: Vanadium oxide and Li3PS4 were prepared in an argon atmosphere having a dew point of −60°C or lower at a volume ratio of 90:10 vanadium oxide:Li3PS4. These materials were mixed in an agate mortar. Next, acetylene black was added as a conductive additive in an amount of 4% by mass relative to the vanadium oxide, and the mixture was mixed in the agate mortar. In this manner, a negative electrode mixture was obtained. The volume ratio of acetylene black to the total volume of the negative electrode mixture was 6.4%.
[0138] Using the negative electrode mixture, a battery of Comparative Example 2 was fabricated in the same manner as in Example 1. As a result of a charge / discharge test, the charge capacity of the battery of Comparative Example 2 at 0.5 C was 0.1 mAh / g.
[0139] Comparative Example 3: Vanadium oxide and Li3PS4 were prepared in an argon atmosphere having a dew point of −60°C or lower at a volume ratio of 30:70 vanadium oxide:Li3PS4. These materials were mixed in an agate mortar. Next, acetylene black as a conductive additive was added in an amount of 10% by mass relative to the vanadium oxide, and the mixture was mixed in the agate mortar. In this manner, a negative electrode mixture was obtained. The volume ratio of acetylene black to the total volume of the negative electrode mixture was 5.4%.
[0140] Using the negative electrode mixture, a battery of Comparative Example 3 was fabricated in the same manner as in Example 1. As a result of a charge-discharge test, the charge capacity of the battery of Comparative Example 3 at 0.5 C was 0.08 mAh / g.
[0141] Comparative Example 4: In an argon atmosphere having a dew point of −60° C. or less, vanadium oxide and Li7La3Zr2O as a solid electrolyte were 12 Vanadium oxide: Li7La3Zr2O 12 The materials were prepared in a volume ratio of 60:40. These materials were mixed in an agate mortar. Next, acetylene black as a conductive additive was added in an amount of 10 mass% relative to the vanadium oxide, and the mixture was mixed in the agate mortar. In this manner, a negative electrode mixture was obtained. At this time, the volume ratio of acetylene black to the total volume of the negative electrode mixture was 10.3%.
[0142] Using the negative electrode mixture, a battery of Comparative Example 4 was fabricated in the same manner as in Example 1. As a result of a charge-discharge test, the charge capacity of the battery of Comparative Example 4 at 0.5 C was 0.08 mAh / g.
[0143]
[0144] <<Discussion>> As can be seen from Table 1, in a battery using vanadium oxide and a sulfide solid electrolyte as the negative electrode active material, when the ratio of the volume of the negative electrode active material to the total volume of the negative electrode active material and the sulfide solid electrolyte was 40% or more and 80% or less, and when the ratio of the volume of the conductive additive to the total volume of the negative electrode mixture was more than 4.4% and 13.8% or less, a high charge capacity was obtained.
[0145] As can be seen from a comparison between Comparative Example 1 and Example 8, when the volume ratio of the negative electrode active material was the same and the amount of the conductive additive was large, a high capacity was obtained.
[0146] As can be seen from a comparison between Comparative Example 2 and Example 8, even if the ratio of the conductive additive was high, only a low capacity was obtained when the volume ratio of the sulfide solid electrolyte was low. In Comparative Example 2, it is thought that the amount of the sulfide solid electrolyte was too small, resulting in insufficient Li ion conductivity.
[0147] In Examples 5 to 7, it was confirmed that the 1 C capacity decreased when the amount of the conductive additive was increased. This is thought to be because the conductive additive inhibited the conduction of Li ions.
[0148] As can be seen from a comparison between Comparative Example 4 and Example 5, a high charge capacity was obtained when a sulfide solid electrolyte was used. It is believed that the materials were mixed in an agate mortar and the powdered negative electrode mixture was compression-molded at room temperature, which resulted in insufficient formation of interfaces between particles in the hard oxide solid electrolyte.
[0149] The negative electrode material of the present disclosure is used, for example, as a material for all-solid-state lithium-ion secondary batteries.
Claims
1. A negative electrode material comprising: a negative electrode active material; a sulfide solid electrolyte; and a conductive assistant, wherein the negative electrode active material contains lithium vanadium oxide, a ratio of the volume of the negative electrode active material to a total volume of the negative electrode active material and the sulfide solid electrolyte is 40% or more and 80% or less, and a ratio of the volume of the conductive assistant to a total volume of the negative electrode active material, the sulfide solid electrolyte, and the conductive assistant is more than 4.4% and 15% or less.
2. The lithium vanadium oxide has the formula Li (3+α+x) V (1-x) M x O (4+α / 2) The negative electrode material according to claim 1, wherein the formula satisfies 0≦x<1.0 and 0≦α≦1.0, and wherein M in the formula is at least one element selected from the group consisting of tetravalent metal elements and tetravalent metalloid elements.
3. The negative electrode material according to claim 2, wherein in the composition formula, M contains Ti.
4. The negative electrode material according to claim 2, wherein in the composition formula, 0<x<1.0 is satisfied.
5. The negative electrode material according to claim 3, wherein in the composition formula, 0<x≦0.1 is satisfied.
6. The negative electrode material according to claim 2, wherein in the composition formula, 0<α<1.0 is satisfied.
7. The negative electrode material according to claim 1, wherein the volume ratio of the negative electrode active material is 50% or more.
8. The negative electrode material according to claim 1, wherein the volume ratio of the negative electrode active material is 70% or less.
9. The negative electrode material according to claim 1, wherein the volume ratio of the conductive additive is 5.8% or more.
10. The negative electrode material according to claim 1, wherein the volume ratio of the conductive additive is 13.8% or less.
11. A battery comprising: a positive electrode; a negative electrode comprising the negative electrode material of claim 1; and an electrolyte layer disposed between said positive electrode and said negative electrode.
Citation Information
Patent Citations
Negative electrode active material and battery
JP2018198171A
Electrode for lithium ion battery, lithium ion battery, and method for manufacturing electrode for lithium ion battery
JP2020095814A
Solid-state battery
WO2021241429A1
Vanadium oxide and battery using same
WO2023238496A1