Inkjet recording method

The inkjet recording method addresses the challenges of high-speed inkjet recording by using specific ink formulations with controlled mass ratios and viscosity to maintain ejection performance and image quality, enhancing the stability and quality of inkjet printing.

WO2024241860A1PCT designated stage expired Publication Date: 2024-11-28FUJIFILM CORP
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016890
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-02
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

High-speed inkjet recording technologies face challenges in maintaining ink ejection performance and image quality due to nozzle drying and reduced droplet interval, leading to deteriorated ejection properties and image quality.

Method used

The method involves using a first ink with a specific pigment and organic solvent mass ratio, combined with resin particles and wax, to control viscosity and surface tension, while a second ink with a different organic solvent mass ratio is used to enhance image quality, ensuring continuous ink ejection and improved ejection performance by adjusting the mass ratios and viscosity.

Benefits of technology

This approach effectively suppresses ink ejection deterioration and maintains high image quality by optimizing the mass ratios of organic solvents and resin particles in both inks, ensuring stable ejection performance and improved image quality during high-speed inkjet recording.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016890_28112024_PF_FP_ABST
    Figure JP2024016890_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an inkjet recording method comprising: a step for discharging a first ink from a first inkjet head positioned on the upstream side in a conveyance direction with respect to a base material conveyed at a conveyance speed of 80 m / min or more; and a step for discharging a second ink from a second inkjet head positioned on the downstream side in the conveyance direction with respect to the base material, wherein the distance between the first inkjet head and the second inkjet head is 100-500 mm, the first ink and the second ink both contain a pigment and an organic solvent, the mass ratio S1 of the content of the organic solvent having an SP value of 28 MPa1 / 2 or less to the content of the pigment in the first ink is 0.5-1.6, and the mass ratio S2 of the content of the organic solvent having an SP value of 28 MPa1 / 2 or less to the content of the pigment in the second ink is more than 1.6 and 5.0 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Inkjet recording method

[0001] The present disclosure relates to an inkjet recording method.

[0002] Various studies have been conducted on inkjet recording methods. For example, Japanese Patent Application Laid-Open No. 2022-107611 describes an ink set for inkjet recording of three or more colors, which includes three or more aqueous inks containing a pigment (A), a water-insoluble polymer (B), an organic solvent (C), a surfactant (D), and water. Japanese Patent Application Laid-Open No. 2022-047492 describes an ink containing a water-soluble organic solvent, a pigment, and resin particles, in which the SP value of the water-soluble organic solvent is 10 (cal / cm 3 ) 1/2 Above 14 (cal / cm 3 ) 1/2 The ink is characterized in that the Tg of the resin particles is 80° C. or higher, and the difference between the median diameter (D50) of the pigment and the median diameter (D50) of the resin particles is 10 nm or less.

[0003] However, when performing high-speed inkjet recording (specifically, inkjet recording in which the substrate is transported at a high speed), it may be difficult to simultaneously suppress a decrease in ejection performance from the inkjet head and obtain good image quality.

[0004] An object of one aspect of the present disclosure is to provide an inkjet recording method that can suppress deterioration in ink ejection properties and record images with good image quality.

[0005] The present disclosure includes the following aspects: <1> A method for printing a printing medium comprising the steps of: ejecting a first ink from a first inkjet head located upstream in the conveyance direction onto a substrate being conveyed at a conveyance speed of 80 m / min or more; and ejecting a second ink from a second inkjet head located downstream in the conveyance direction onto the substrate, wherein the distance between the first inkjet head and the second inkjet head is 100 mm to 500 mm, each of the first ink and the second ink contains a pigment and an organic solvent, and the SP value of the first ink relative to the pigment content is 28 MPa. 1/2The mass ratio S1 of the content of the organic solvent is 0.5 to 1.6, and the SP value of the second ink relative to the content of the pigment is 28 MPa. 1/2<2> The inkjet recording method according to <1>, wherein the mass ratio S1 is 1.0 to 1.4, and the mass ratio S2 is 3.5 to 4.5. <3> The inkjet recording method according to <1> or <2>, wherein the difference between the mass ratios S1 and S2 is 1.5 to 4.0. <4> The inkjet recording method according to any one of <1> to <3>, wherein the first ink and the second ink both contain resin particles, the content of the resin particles in the first ink is 0.1% to 1.8% by mass relative to the total amount of the first ink, and the content of the resin particles in the second ink is 0.1% to 4.0% by mass relative to the total amount of the second ink. <5> The inkjet recording method according to any one of <1> to <4>, wherein the first ink and the second ink both contain wax, the mass ratio T1 of the resin particle content to the wax content in the first ink is 0.1 to 2.0, and the mass ratio T2 of the resin particle content to the wax content in the second ink is 0.1 to 6.0. <6> The inkjet recording method according to <5>, wherein the mass ratio T1 is 0.5 to 1.6, and the mass ratio T2 is 0.5 to 4.5. <7> The inkjet recording method according to any one of <1> to <6>, wherein the viscosity D of the first ink and the second ink when the volatile components are evaporated to reduce the mass by 45% is 10 mPa·s to 100 mPa·s. <8> The inkjet recording method according to <7>, wherein the viscosity D of the first ink and the second ink is 20 mPa·s to 50 MPa·s. <9> The inkjet recording method according to any one of <1> to <8>, wherein both the first ink and the second ink contain a surfactant, and the surfactant contains at least one selected from the group consisting of a polyoxyalkylene alkyl ether compound, an acetylene compound, and a silicone compound. <10> The inkjet recording method according to any one of <1> to <9>, wherein both the pigments contained in the first ink and the second ink are at least partially coated with a resin having a crosslinked structure.<11> The inkjet recording method according to any one of <1> to <10>, wherein the first ink is a black ink, and the second ink is a cyan ink.

[0006] According to one aspect of the present disclosure, there is provided an inkjet recording method that can suppress deterioration in ink ejection properties and record images with good image quality.

[0007] FIG. 1 is a diagram conceptually illustrating an example of an inkjet recording apparatus used in an inkjet recording method of the present disclosure.

[0008] In this specification, a numerical range indicated using "to" means a range that includes the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in the numerical ranges described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.

[0009] As used herein, the amount of each component in a composition refers to the total amount of the components in the composition unless otherwise specified, when the composition contains multiple substances corresponding to each component. In this specification, a combination of two or more preferred aspects is a more preferred aspect. As used herein, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.

[0010] In this specification, the term "image" refers to a film in general, and the term "image recording" refers to the formation of an image (i.e., a film). The concept of "image" in this specification also includes a solid image.

[0011] In this specification, the term "(meth)acrylate" encompasses both acrylate and methacrylate, and the term "(meth)acrylic acid" encompasses both acrylic acid and methacrylic acid.

[0012] [Inkjet Recording Method] The inkjet recording method of the present disclosure includes a step of ejecting a first ink from a first inkjet head located upstream in a transport direction onto a substrate transported at a transport speed of 80 m / min or more, and a step of ejecting a second ink from a second inkjet head located downstream in the transport direction onto the substrate, wherein the distance between the first inkjet head and the second inkjet head is 100 mm to 500 mm, the first ink and the second ink both contain a pigment and an organic solvent, and the SP value of the first ink relative to the pigment content is 28 MPa. 1/2 The mass ratio S1 of the content of the organic solvent is 0.5 to 1.6, and the SP value of the second ink relative to the content of the pigment is 28 MPa. 1/2 The mass ratio S2 of the organic solvent content is greater than 1.6 and not more than 5.0.

[0013] In the inkjet recording method of the present disclosure, the first ink and the second ink are ejected onto a substrate being transported at a transport speed of 80 m / min or more. That is, the inkjet recording method of the present disclosure is a method of performing inkjet recording at high speed. Generally, when inkjet recording is performed at high speed, the nozzle surface of the inkjet head is blown with air during transport, which makes the nozzle surface prone to drying, and when ink is continuously ejected, the ejection properties tend to deteriorate. Furthermore, when inkjet recording is performed at high speed, the interval between ink landings becomes short, which tends to deteriorate image quality. In contrast, in the inkjet recording method of the present disclosure, the SP value of the ink relative to the pigment content is 28 MPa. 1/2By focusing on the mass ratio of the organic solvent content, which is equal to or less than 1.6, and controlling this mass ratio, ejection performance and image quality are improved. In particular, because the first ink, which is ejected first, dries more easily than the second ink, which is ejected later, it is believed that by setting the mass ratio S1 in the first ink to 0.5 to 1.6 and the mass ratio S2 in the second ink to more than 1.6 and not more than 5.0, landing interference is suppressed and image quality is improved. Furthermore, by setting the mass ratio S1 in the first ink to 0.5 to 1.6 and the mass ratio S2 in the second ink to more than 1.6 and not more than 5.0, the increase in viscosity that accompanies drying of the ink is appropriately adjusted, thereby improving ejection performance.

[0014] On the other hand, in JP-A-2022-107611 and JP-A-2022-047492, the SP value for the pigment content in the ink is 28 MPa. 1/2 There is no description that focuses on the mass ratio of the organic solvent content, which is as follows:

[0015] The inkjet recording method of the present disclosure will be described in detail below.

[0016] <Substrate> The substrate used in the inkjet recording method of the present disclosure is not particularly limited, and examples thereof include so-called coated paper used in general offset printing, etc. Coated paper is a type of paper that is made primarily of cellulose and that is generally not surface-treated, such as wood-free paper or neutral paper, on the surface of which a coating material is applied to form a coating layer.

[0017] The coated paper may be any commercially available coated paper, for example, a general coated paper for printing, specifically, coated papers (A2, B2) such as "OK Top Coat +" manufactured by Oji Paper Co., Ltd., "Aurora Coat" and "Yurite" manufactured by Nippon Paper Industries Co., Ltd., and art papers (A1) such as "Tokubishi Art" manufactured by Mitsubishi Paper Mills, Ltd.

[0018] The substrate may be a low water-absorbent substrate or a non-water-absorbent substrate. In the present disclosure, a low water-absorbent recording medium is a recording medium having a water absorption coefficient Ka of 0.05 mL / m 2 ・ms 1/2 ~0.5 mL / m 2 ・ms 1/2 0.1 mL / m2 ・ms 1/2 ~0.4 mL / m 2 ・ms 1/2 It is preferable that the concentration is 0.2 mL / m 2 ・ms 1/2 ~0.3 mL / m 2 ・ms 1/2 Furthermore, a non-water-absorbent substrate is a substrate having a water absorption coefficient Ka of 0.05 mL / m 2 ・ms 1/2 The water absorption coefficient Ka is the same as that described in JAPAN TAPPI Paper and Pulp Testing Method No. 51:2000 (published by the Paper and Pulp Technology Association), and specifically, the absorption coefficient Ka is calculated from the difference in the amount of water transferred between a contact time of 100 ms and a contact time of 900 ms using an automatic scanning absorption meter KM500Win (manufactured by Kumagai Riki Co., Ltd.).

[0019] The non-absorbent substrate is preferably a resin substrate. Examples of the resin substrate include substrates obtained by molding a thermoplastic resin into a sheet. The resin substrate preferably contains polypropylene, polyethylene terephthalate, nylon, polyethylene, or polyimide. The resin substrate may be a transparent resin substrate, a colored resin substrate, or a resin substrate at least partially subjected to a metal vapor deposition treatment or the like. The shape of the resin substrate is not particularly limited, but a sheet-like resin substrate is preferable, and from the viewpoint of productivity of printed matter, a resin substrate that can be formed into a roll by winding the sheet-like resin substrate is more preferable.

[0020] <Substrate Conveying Speed> In the inkjet recording method of the present disclosure, the substrate conveying speed is 80 m / min or more. This allows high-speed inkjet recording to be achieved. In general, high-speed inkjet recording that satisfies the above conveying speed is likely to result in a decrease in ink ejection properties. In high-speed inkjet recording that satisfies the above conveying speed, the effect of improving ejection properties in the inkjet recording method of the present disclosure is significantly exhibited.

[0021] The substrate conveying speed may be 80 m / min or more, and may be constant or not. For example, when the substrate conveying speed is 150 m / min or more, the effect of improving the ejection properties in the inkjet recording method of the present disclosure is significantly exhibited. The upper limit of the substrate conveying speed is, for example, 300 m / min.

[0022] <Ejection Step> The inkjet recording method of the present disclosure is a method for recording an image using an inkjet recording system. The inkjet recording method of the present disclosure includes a step of ejecting a first ink from a first inkjet head located upstream in the transport direction, and a step of ejecting a second ink from a second inkjet head located downstream in the transport direction. That is, after the first ink is ejected, the second ink is ejected.

[0023] The ink is preferably ejected using an inkjet head having a resolution of 300 dpi or more (more preferably 600 dpi or more, and even more preferably 800 dpi or more), where dpi stands for dots per inch, and 1 inch is 2.54 cm.

[0024] From the viewpoint of obtaining a high-definition image, the droplet volume of each of the first ink and the second ink is preferably 1 pL (picoliter) to 10 pL, and more preferably 1.5 pL to 6 pL.

[0025] In the inkjet recording method of the present disclosure, the distance between the first inkjet head and the second inkjet head (hereinafter also referred to as the "head-to-head distance") is 100 mm to 500 mm, and preferably 110 mm to 300 mm. When the head-to-head distance is in this range, the viscosity of the first ink and the second ink increases appropriately due to drying, and both the ejection performance and the image quality can be achieved.

[0026] Specifically, the inter-head distance is the shortest distance between the center of the first inkjet and the center of the second inkjet, and is the distance parallel to the transport direction.

[0027] Between the first inkjet head and the second inkjet head, other inkjet heads that eject inks other than the first ink and the second ink may be provided, but from the viewpoint of suppressing interference between ink droplets, it is preferable that no other inkjet heads are provided. In other words, it is preferable that the first ink and the second ink are ejected continuously.

[0028] Note that other inkjet heads that eject inks other than the first ink and the second ink may be provided further downstream in the transport direction than the position where the second inkjet head is installed. For example, using an ink set consisting of black ink, cyan ink, magenta ink, and yellow ink, the black ink may be ejected from the first inkjet head, the cyan ink may be ejected from the second inkjet head, the magenta ink may be ejected from the third inkjet head, and the yellow ink may be ejected from the fourth inkjet head.

[0029] The inkjet recording method of the present disclosure may include other steps in addition to the step of ejecting the first ink and the step of ejecting the second ink, such as a step of preheating the substrate and a step of drying the substrate to which the inks have been applied.

[0030] <First ink, second ink> The inkjet recording method of the present disclosure uses a first ink ejected from a first inkjet head located upstream in the transport direction, and a second ink ejected from a second inkjet head located downstream in the transport direction.

[0031] Both the first ink and the second ink contain a pigment and an organic solvent. The first ink and the second ink may contain other components as needed. Hereinafter, the content common to both the first ink and the second ink will be simply referred to as "ink."

[0032] (Water) The ink of the present disclosure preferably contains water. The water content is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, relative to the total amount of the ink. The upper limit of the water content depends on the amounts of other components. The upper limit of the water content relative to the total amount of the ink is, for example, 90% by mass or 80% by mass.

[0033] (Pigment) The ink contains at least one type of pigment. The type of pigment contained in the first ink and the type of pigment contained in the second ink may be the same or different. The pigment may be an organic pigment or an inorganic pigment.

[0034] Examples of organic pigments include azo pigments, polycyclic pigments, dye chelates, nitro pigments, nitroso pigments, and aniline black. Among these, azo pigments or polycyclic pigments are preferred. Examples of azo pigments include azo lakes, insoluble azo pigments, condensed azo pigments, and chelate azo pigments. Examples of polycyclic pigments include phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, indigo pigments, thioindigo pigments, isoindolinone pigments, and quinophthalone pigments. Examples of dye chelates include basic dye chelates and acid dye chelates.

[0035] Examples of inorganic pigments include titanium oxide, iron oxide, calcium carbonate, barium sulfate, aluminum hydroxide, barium yellow, cadmium red, chrome yellow, and carbon black.

[0036] Examples of the pigment include those described in "Encyclopedia of Pigments" edited by Seijiro Ito (published in 2000), "Industrial Organic Pigments" by W. Herbst and K. Hunger, and JP-A Nos. 2002-12607, 2002-188025, 2003-26978, and 2003-342503.

[0037] The volume average particle diameter of the pigment is preferably 10 nm to 200 nm, more preferably 10 nm to 180 nm, and even more preferably 10 nm to 150 nm. When the volume average particle diameter is 200 nm or less, color reproducibility is improved and ejection properties are improved when recording images using an inkjet recording method. Furthermore, when the volume average particle diameter is 10 nm or more, light resistance is improved.

[0038] The particle size distribution of the pigment is not particularly limited, and may be either a broad particle size distribution or a monodisperse particle size distribution. Two or more pigments having a monodisperse particle size distribution may be mixed and used.

[0039] The volume average particle size and particle size distribution of the pigment are values ​​measured using a particle size distribution measuring device (for example, Microtrac UPA (registered trademark) EX150 manufactured by Nikkiso Co., Ltd.).

[0040] Although the types of pigments contained in the first ink and the second ink are not particularly limited, it is preferable that the pigment contained in the first ink is a black pigment and the pigment contained in the second ink is a cyan pigment, i.e., it is preferable that the first ink is a black ink and the second ink is a cyan ink.

[0041] In general, the first ink located upstream in the transport direction dries more easily than the second ink located downstream in the transport direction, and image quality is likely to deteriorate due to the difference in dryness. In particular, when the first ink is black ink and the second ink is cyan ink, image quality is likely to deteriorate due to the difference in dryness. Therefore, when the first ink is black ink and the second ink is cyan ink, the inkjet recording method of the present disclosure is particularly effective in improving image quality.

[0042] The content of the pigment in the first ink is preferably 1% by mass to 20% by mass, and more preferably 3% by mass to 10% by mass, relative to the total amount of the first ink. The content of the pigment in the second ink is preferably 1% by mass to 20% by mass, and more preferably 1% by mass to 5% by mass, relative to the total amount of the second ink.

[0043] (Organic Solvent) The ink contains at least one organic solvent. The type of organic solvent contained in the first ink and the type of organic solvent contained in the second ink may be the same or different. As described above, the ink preferably contains water, and the organic solvent is preferably a water-soluble organic solvent.

[0044] In the present disclosure, the term "water-soluble" in "water-soluble organic solvent" means that 1 g or more of the solvent dissolves in 100 g of water at 25°C.

[0045] The organic solvent contained in the ink has an SP value of 28 MPa. 1/2 The organic solvent includes the following organic solvent (hereinafter also referred to as "organic solvent A").

[0046] In this disclosure, "SP value" means solubility parameter, and its unit is MPa 1/2 The SP value is calculated by the Okitsu method (Okitsu Toshinao, Journal of the Adhesion Society of Japan, 29 (5) (1993)). Specifically, the SP value is calculated using the following formula. ΔF is a value given in the literature. SP value (δ) = ΣΔF (Molar Attraction Constants) / V (Molar Volume)

[0047] Examples of organic solvent A include diethylene glycol monobutyl ether, diethylene glycol monoethyl ether, dipropylene glycol monomethyl ether, ethylene glycol monobutyl ether, propylene glycol monobutyl ether, ethylene glycol monopropyl ether, propylene glycol monopropyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether, tripropylene glycol monomethyl ether, ethylene glycol isopropyl ether, diethylene glycol isopropyl ether, diethylene glycol isobutyl ether, 2-ethyl-1-hexanol, 2-ethyl-1,3-hexanediol, 2-ethyl-1,3-butanediol, 1,2-hexanediol, 2-pyrrolidone, 3-methoxy-1-butanol, diethylene glycol monoisopropyl ether, 3-ethyl-3-hydroxymethyloxetane, and ethylene glycol monohexyl ether.

[0048] In particular, the SP value of organic solvent A is preferably 24 or less. When the SP value of organic solvent A is 24 or less, the graininess of the image is improved. From the above-mentioned viewpoints, organic solvent A is preferably a glycol ether having 5 to 8 carbon atoms. Examples of glycol ethers having 5 to 8 carbon atoms include ethylene glycol monobutyl ether, propylene glycol monoethyl ether, ethylene glycol isopropyl ether, diethylene glycol monoethyl ether, propylene glycol monopropyl ether, diethylene glycol monobutyl ether, and diethylene glycol isopropyl ether.

[0049] The organic solvent contained in the ink may be only organic solvent A, or may contain, in addition to organic solvent A, an organic solvent having an SP value of 28 MPa or more. 1/2 The solvent may contain an organic solvent exceeding 1000 ppm.

[0050] SP value is 28 MPa 1/2Examples of organic solvents that are greater than 1,2,5-trimethyl- ...

[0051] Among them, the SP value is 28 MPa 1/2 The organic solvent having a carbon number of 2 to 6 or more is preferably a diol having 2 to 6 carbon atoms or a triol having 2 to 6 carbon atoms. Examples of the diol having 2 to 6 carbon atoms or the triol having 2 to 6 carbon atoms include ethylene glycol, diethylene glycol, 1,2-propanediol, glycerin, and triethylene glycol.

[0052] The content of the organic solvent in the first ink is preferably 1% by mass to 20% by mass, and more preferably 3% by mass to 15% by mass, relative to the total amount of the first ink. The content of the organic solvent in the second ink is preferably 1% by mass to 20% by mass, and more preferably 5% by mass to 20% by mass, relative to the total amount of the second ink.

[0053] The content of organic solvent A in the first ink is preferably 1% by mass to 20% by mass, and more preferably 3% by mass to 15% by mass, relative to the total amount of the first ink. The content of organic solvent A in the second ink is preferably 1% by mass to 20% by mass, and more preferably 5% by mass to 20% by mass, relative to the total amount of the second ink.

[0054] In the present disclosure, the mass ratio S1 of the content of organic solvent A to the content of pigment in the first ink is 0.5 to 1.6, and preferably 1.0 to 1.4.

[0055] When the mass ratio S1 is 0.5 or more, the granularity is excellent and bleeding is suppressed, whereas when the mass ratio S1 is 1.6 or less, the ejection property is excellent.

[0056] In the present disclosure, the mass ratio S2 of the content of organic solvent A to the content of pigment in the second ink is greater than 1.6 and not more than 5.0, and is preferably 3.5 to 4.5.

[0057] When the mass ratio S2 is more than 1.6, the granularity is excellent and bleeding is suppressed, whereas when the mass ratio S2 is 5.0 or less, the ejection property is excellent.

[0058] By setting the mass ratio S2 and the mass ratio S1 within the above ranges, it is possible to achieve both good ejection performance and good image quality.

[0059] From the viewpoint of further improving the ejection properties and image quality, the difference between the mass ratio S1 and the mass ratio S2 (i.e., "mass ratio S2 - mass ratio S1") is preferably 1.5 to 4.0, and more preferably 2.5 to 3.0.

[0060] (Resin) The ink preferably contains at least one type of resin. The type of resin contained in the first ink and the type of resin contained in the second ink may be the same or different.

[0061] Examples of the resin include pigment dispersion resin, resin particles, and water-soluble resin.

[0062] Pigment Dispersion Resin The resin may contain at least one pigment dispersing resin. In the present disclosure, a pigment dispersing resin is a resin that has the function of dispersing a pigment.

[0063] The form of the pigment dispersing resin is not particularly limited, and may be any of a random resin, a block resin, and a graft resin. The pigment dispersing resin is preferably a resin having a crosslinked structure.

[0064] The pigment contained in the ink is preferably at least partially coated with a resin having a crosslinked structure. When the pigment dispersing resin is a resin having a crosslinked structure and at least a portion of the pigment is coated with the pigment dispersing resin, it is thought that the pigment dispersing resin is less likely to be detached from the surface of the pigment, and the dispersion stability of the pigment is high.

[0065] For example, the pigment can be mixed with an uncrosslinked resin and then crosslinked with a crosslinking agent, thereby coating at least a portion of the pigment with a resin having a crosslinked structure.

[0066] In this disclosure, a resin refers to a compound having a weight average molecular weight (Mw) of 1,000 or more.

[0067] In this disclosure, the weight average molecular weight (Mw) refers to a value measured by gel permeation chromatography (GPC). Measurements by gel permeation chromatography (GPC) are performed using an HLC (registered trademark)-8020GPC (manufactured by Tosoh Corporation) as a measuring device, three TSKgel (registered trademark) Super Multipore HZ-H columns (4.6 mm ID x 15 cm, manufactured by Tosoh Corporation), and THF (tetrahydrofuran) as an eluent. Measurements are performed using an RI detector at a sample concentration of 0.45% by mass, a flow rate of 0.35 mL / min, a sample injection volume of 10 μL, and a measurement temperature of 40°C. The calibration curve is prepared from eight samples of "Standard Sample TSK Standard, Polystyrene" manufactured by Tosoh Corporation: "F-40", "F-20", "F-4", "F-1", "A-5000", "A-2500", "A-1000", and "n-propylbenzene".

[0068] The resin having a crosslinked structure is not particularly limited as long as it has at least one crosslinked structure in the molecule.

[0069] Whether or not the resin contained in the ink has a crosslinked structure can be determined, for example, by the following method: First, the resin is separated from the ink using a separation method such as solvent extraction. The separated resin is analyzed using various analytical methods such as nuclear magnetic resonance (NMR), infrared spectroscopy (IR), and thermal analysis, allowing a comprehensive determination of whether or not the resin has a crosslinked structure.

[0070] A resin having a crosslinked structure (hereinafter also referred to as a "crosslinked resin") is formed, for example, by crosslinking an uncrosslinked resin (hereinafter also referred to as an "uncrosslinked resin") with a crosslinking agent. The uncrosslinked resin is preferably a water-soluble resin.

[0071] In the present disclosure, "water-soluble" in "water-soluble resin" means the property of dissolving 1 g or more in 100 g of water at 25° C. Preferably, "water-soluble" means the property of dissolving 3 g or more (more preferably 10 g or more) in 100 g of water at 25° C.

[0072] Even if the uncrosslinked resin is water-soluble, the crosslinked resin is not necessarily water-soluble.

[0073] Examples of the uncrosslinked resin include vinyl resin, acrylic resin, urethane resin, and polyester resin, and the uncrosslinked resin is preferably an acrylic resin.

[0074] The uncrosslinked resin is preferably a resin having a functional group that can be crosslinked by a crosslinking agent. Examples of the crosslinkable functional group include a carboxy group or a salt thereof, an isocyanate group, and an epoxy group. Among these, from the viewpoint of improving the dispersibility of the pigment, the crosslinkable functional group is preferably a carboxy group or a salt thereof, and a carboxy group is particularly preferred. That is, the uncrosslinked resin is preferably a resin containing a carboxy group.

[0075] The uncrosslinked resin is preferably a copolymer containing a structural unit derived from a monomer containing a carboxy group (hereinafter referred to as a "carboxy group-containing monomer"). The structural unit derived from the carboxy group-containing monomer contained in the copolymer may be of only one type, or may be of two or more types. The copolymer may be a random copolymer or a block copolymer, but is preferably a random copolymer.

[0076] Examples of carboxy group-containing monomers include (meth)acrylic acid, β-carboxyethyl acrylate, fumaric acid, itaconic acid, maleic acid, and crotonic acid.

[0077] From the viewpoint of crosslinkability and dispersibility, the carboxy group-containing monomer is preferably (meth)acrylic acid or β-carboxyethyl acrylate, and more preferably (meth)acrylic acid.

[0078] The content of the structural unit derived from the carboxy group-containing monomer is preferably 5% by mass to 40% by mass, more preferably 10% by mass to 35% by mass, and even more preferably 10% by mass to 30% by mass, relative to the total amount of the uncrosslinked resin.

[0079] The uncrosslinked resin preferably contains a structural unit derived from a hydrophobic monomer in addition to the structural unit derived from the carboxyl group-containing monomer. The structural unit derived from the hydrophobic monomer contained in the copolymer may be of one type or two or more types.

[0080] Examples of hydrophobic monomers include (meth)acrylates having an alkyl group having 1 to 20 carbon atoms, (meth)acrylates having an aromatic ring (for example, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, etc.), styrene, and styrene derivatives.

[0081] The content of the structural unit derived from the hydrophobic monomer is preferably 60% by mass to 95% by mass, more preferably 65% ​​by mass to 90% by mass, and even more preferably 70% by mass to 90% by mass, based on the total amount of the uncrosslinked resin.

[0082] The uncrosslinked resin is preferably a random copolymer containing a structural unit derived from a carboxy group-containing monomer and at least one of a structural unit derived from a (meth)acrylate having an alkyl group with 1 to 20 carbon atoms and a structural unit derived from a (meth)acrylate having an aromatic ring, more preferably a random copolymer containing a structural unit derived from (meth)acrylic acid and a structural unit derived from a (meth)acrylate having an aromatic ring, and even more preferably a copolymer containing a structural unit derived from (meth)acrylic acid and a structural unit derived from benzyl (meth)acrylate.

[0083] The weight average molecular weight (Mw) of the uncrosslinked resin is not particularly limited, but from the viewpoint of pigment dispersibility, it is preferably 3,000 to 300,000, more preferably 5,000 to 200,000, and even more preferably 7,000 to 100,000.

[0084] The preferred range of the weight average molecular weight of the crosslinked resin is the same as the preferred range of the weight average molecular weight of the uncrosslinked resin.

[0085] The crosslinking agent used to crosslink the uncrosslinked resin is preferably a compound having two or more reactive sites with the uncrosslinked resin (e.g., a resin having a carboxy group). Only one type of crosslinking agent may be used, or two or more types may be used.

[0086] A preferred combination of a crosslinking agent and an uncrosslinked resin is a combination of a compound having two or more epoxy groups (i.e., a bifunctional or higher epoxy compound) and a resin having a carboxy group. In this combination, a crosslinked structure is formed by the reaction between the epoxy group and the carboxy group. The formation of the crosslinked structure by the crosslinking agent is preferably carried out after the pigment has been dispersed with the uncrosslinked resin.

[0087] Examples of difunctional or higher functional epoxy compounds include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, dipropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and trimethylolpropane triglycidyl ether.

[0088] Among these, the difunctional or higher epoxy compound is preferably polyethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, or trimethylolpropane triglycidyl ether.

[0089] The crosslinking agent may be a commercially available product, such as Denacol EX-321, EX-821, EX-830, EX-850, and EX-851 (manufactured by Nagase ChemteX Corporation).

[0090] The molar ratio of the reactive site (e.g., epoxy group) in the crosslinking agent to the reactive site (e.g., carboxy group) in the uncrosslinked resin is preferably 1:1.1 to 1:10, more preferably 1:1.1 to 1:5, and even more preferably 1:1.1 to 1:3, from the viewpoints of the crosslinking reaction rate and the dispersion stability after crosslinking.

[0091] The mixing ratio of the pigment to the pigment dispersing resin is preferably 1:0.02 to 1:2, more preferably 1:0.03 to 1:1.5, and even more preferably 1:0.04 to 1:1, on a mass basis.

[0092] Resin Particles: From the viewpoint of improving blocking resistance, the resin preferably contains at least one type of resin particle. The resin particles contain a resin and may also contain a core material other than a resin, but are preferably resin particles consisting only of a resin.

[0093] The resin particles are preferably particles made of an acrylic resin, particles made of a polyester resin, particles made of a polyurethane resin, or particles made of a polyolefin resin, and more preferably particles made of an acrylic resin.

[0094] In the present disclosure, an acrylic resin refers to a resin containing at least one of a structural unit derived from (meth)acrylic acid and a structural unit derived from a (meth)acrylic acid ester.

[0095] For the resin particles, reference may be made to, for example, paragraphs 0038 to 0114 of International Publication No. 2021 / 192720 and paragraphs 0109 to 0120 of JP-A-2015-25076.

[0096] From the viewpoint of further improving the abrasion resistance of the image, the glass transition temperature (Tg) of the resin particles is preferably 90°C to 250°C, and more preferably 100°C to 230°C. Here, the glass transition temperature (Tg) of the resin particles is a measured Tg obtained by actual measurement. For the method of measuring the measured Tg, see paragraph 0111 of JP2015-25076A.

[0097] The content of the resin particles in the first ink is preferably 0.1% to 1.8% by mass, and more preferably 0.5% to 1.8% by mass, relative to the total amount of the first ink, and the content of the resin particles in the second ink is preferably 0.1% to 4.0% by mass, and more preferably 0.7% to 4.0% by mass, relative to the total amount of the second ink.

[0098] The greater the resin particle content, the more likely the ink will thicken due to drying after landing on the substrate. Because the first ink is ejected before the second ink and is therefore more likely to dry, it is preferable that the resin particle content of the first ink be less than the resin particle content of the second ink.

[0099] The ink containing resin particles may be prepared using a commercially available resin emulsion (i.e., an aqueous dispersion of resin particles). Examples of commercially available resin emulsions include A-810 (Sansui Co., Ltd.), A-995 (Sansui Co., Ltd.), Hiros-X NE-2186 (Seiko PMC Corporation), Hiros-X TE-1048 (Seiko PMC Corporation), Saibinol SK-202 (Saiden Chemical Industry Co., Ltd.), TOCRYL W-1048 (Toyochem), WC-M-1217 (Arakawa Chemical Industries, Ltd.), WC-M-1219 (Arakawa Chemical Industries, Ltd.), N985(A)-1 (E-TEC Co., Ltd.), and Neocryl A-1105 (DSM coating resin), Acrylic SE-810A, Acrylic SE-953A-2, Acrylic SE-1658F, Acrylic SE-2974F, Acrylic SE-2978F (Taisei Fine Chemical), Luckstar 7132-C (DIC), ST200 (Nippon Shokubai), Movinyl 972 (Japan Coating Resin Co., Ltd.), and the like.

[0100] -Water-soluble resin- The resin may contain at least one water-soluble resin. The definition of "water-soluble" in the water-soluble resin is as described above. Examples of the water-soluble resin include the same resins as the uncrosslinked resin described above.

[0101] (Wax) The ink preferably contains at least one type of wax. The inclusion of wax improves the scratch resistance of the image. The type of wax contained in the first ink and the type of wax contained in the second ink may be the same or different.

[0102] In the present disclosure, wax refers to a polymer having a melting point of 170° C. or lower. The melting point refers to the temperature at the top of an endothermic peak in measurement using a differential scanning calorimetry (DSC), for example, a differential scanning calorimetry (product name "EXSTAR6220" manufactured by Hitachi High-Tech Science Corporation).

[0103] Waxes include natural waxes and synthetic waxes.

[0104] Examples of natural waxes include petroleum wax, vegetable wax, and animal and vegetable wax. Examples of petroleum waxes include paraffin wax, microcrystalline wax, and petrolatum. Examples of vegetable waxes include carnauba wax, candelilla wax, rice wax, and Japan wax. Examples of animal and vegetable waxes include lanolin and beeswax.

[0105] Examples of synthetic waxes include synthetic hydrocarbon waxes, modified waxes, and resin waxes. Examples of synthetic hydrocarbon waxes include polyethylene (PE) wax, polypropylene (PP) wax, and Fischer-Tropsch wax. Examples of modified waxes include paraffin wax derivatives, montan wax derivatives, microcrystalline wax derivatives, and fatty acid amide wax derivatives. Examples of resin waxes include acrylic wax and urethane wax.

[0106] The melting point of the wax is preferably 170° C. or lower, more preferably 100° C. to 170° C., even more preferably 100° C. to 160° C., and still more preferably 110° C. to 150° C. In the present disclosure, the melting point refers to the temperature at the top of the endothermic peak in measurement using a differential scanning calorimetry (DSC), for example, a differential scanning calorimetry (product name "EXSTAR6220" manufactured by Hitachi High-Tech Science Corporation).

[0107] The ink of the present disclosure may be prepared using a commercially available aqueous dispersion of wax, such as Hitec E-6314 and Hitec E-9015 manufactured by Toho Chemical Industry Co., Ltd., Nopcoat PEM17 manufactured by San Nopco Ltd., Chemipearl (registered trademark) W4005 manufactured by Mitsui Chemicals, Inc., AQUACER 515, AQUACER 531, AQUACER 552, and AQUACER 593 manufactured by BYK Japan, and Cellosol 524 manufactured by Chukyo Yushi Co., Ltd.

[0108] The wax content in the first ink is preferably 0.1% to 3.0% by mass, and more preferably 0.5% to 2.5% by mass, relative to the total amount of the first ink. The wax content in the second ink is preferably 0.1% to 3.0% by mass, and more preferably 0.5% to 2.5% by mass, relative to the total amount of the second ink.

[0109] In the present disclosure, the mass ratio T1 of the resin particle content to the wax content in the first ink is preferably 0.1 to 2.0, and more preferably 0.5 to 1.6, and the mass ratio T2 of the resin particle content to the wax content in the second ink is preferably 0.1 to 6.0, and more preferably 0.5 to 4.5.

[0110] When the mass ratio T1 is 0.1 or more, the image quality is improved. On the other hand, when the mass ratio T1 is 2.0 or less, the ejection properties are improved. When the mass ratio T2 is 0.1 or more, the image quality is improved. On the other hand, when the mass ratio T1 is 6.0 or less, the ejection properties are improved.

[0111] Among the pigment resins, resin particles, and waxes that can be contained in ink, wax has the highest hydrophobicity. Therefore, when wax is contained in ink, it is thought that the wax is unevenly distributed on the nozzle surface of the inkjet head. When the water contained in the ink evaporates in this state, the organic solvent content increases, the charge repulsion between the pigment dispersion resins decreases, and the ink tends to thicken, resulting in a decrease in ejection performance. However, when the mass ratio T1 is 2.0 or less, the ink viscosity is suppressed, improving ejection performance. Furthermore, when the mass ratio T2 is 6.0 or less, the ink viscosity is suppressed, improving ejection performance.

[0112] (Surfactant) The ink preferably contains at least one surfactant. The type of surfactant contained in the first ink and the type of surfactant contained in the second ink may be the same or different.

[0113] The surfactant contained in the ink preferably includes at least one selected from the group consisting of polyoxyalkylene alkyl ether compounds, acetylene compounds, and silicone compounds.

[0114] The polyoxyalkylene alkyl ether compound is preferably an ethylene oxide adduct of alcohol or an ethylene oxide and propylene oxide adduct of alcohol, and more preferably an ethylene oxide adduct of alcohol (i.e., a polyoxyethylene alkyl ether compound).

[0115] As the polyoxyalkylene alkyl ether compound, a compound represented by the following formula (1) is more preferred: 5 O-[(EO) m / (PO) n ]-H... Formula (1)

[0116] In formula (1), R 5represents a hydrocarbon group having 6 to 30 carbon atoms, EO represents an ethyleneoxy group, and PO represents a propyleneoxy group. In formula (1), m and n represent the average number of moles added, m is 2 to 100, n is 0 to 50, and the sum of m and n is 2 to 120. In formula (1), "(EO) m / (PO) n " indicates that the arrangement of EO and PO may be that of a random copolymer or that of a block copolymer. m / (PO) n In the portion indicated as "," the order of addition of EO and PO does not matter.

[0117] In formula (1), when n is 2 or more, the compound represented by formula (1) may be a block copolymer or a random copolymer. When the compound represented by formula (1) is a block copolymer, it is preferably a compound in which an oxyethylene group is located on the hydroxy group side, i.e., RO-(PO)(EO)-H. Furthermore, when the compound represented by formula (1) is a block copolymer, it may be a triblock copolymer of RO-(EO)(PO)(EO)-H.

[0118] Commercially available polyoxyalkylene alkyl ether compounds include ethylene oxide adducts of lauryl alcohol, such as Emulgen 102 (HLB: 6.3, average number of moles of EO added: 2), Emulgen 103 (HLB: 8.1, average number of moles of EO added: 3), Emulgen 103 (HLB: 9.7, average number of moles of EO added: 4), Emulgen 108 (HLB: 12.1, average number of moles of EO added: 6), Emulgen 109P (HLB: 13.6, average number of moles of EO added: 8), Emulgen 120 (HLB: 15.3, average number of moles of EO added: 13), Emulgen 147 (HLB: 16.3, average number of moles of EO added: 17), and Emulgen 150 (HLB: 18.4, average number of moles of EO added: 44), all manufactured by Kao Corporation; Examples of ethylene oxide adducts of secondary alcohols having 12 carbon atoms include Tergitol TMN-3 (HLB: 8.1, average number of moles of EO added: 3), Triton HW-1000 (HLB: 10, average number of moles of EO added: 6), Tergitol TMN-6 (HLB: 13.1, average number of moles of EO added: 8), Tergitol TMN-100X (HLB: 14.0, average number of moles of EO added: 9), and Tergitol TMN-10 (HLB: 14.4, average number of moles of EO added: 10), all of which are manufactured by The Dow Chemical Company. Commercially available polyoxyalkylene alkyl ether compounds include Emulgen 707 (ethylene oxide adduct of secondary alcohol having 11 to 15 carbon atoms, HLB: 12.1, average number of moles of EO added: 6) and Emulgen 220 (ethylene oxide adduct of linear primary alcohol having 16 to 18 carbon atoms, HLB: 14.2, average number of moles of EO added: 13), manufactured by Kao Corporation.

[0119] As the silicone compound, a polyether-modified silicone compound is preferred, and a compound represented by the following formula (D1) is more preferred.

[0120]

[0121] In formula (D1), R 1 each independently represents an alkyl group having 1 to 3 carbon atoms or a hydroxy group, R 2 represents an alkanediyl group having 2 to 5 carbon atoms, and R 3represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a hydroxy group, PO represents a propyleneoxy group, and EO represents an ethyleneoxy group. a, b, m, and n represent the average number of moles of each unit added, with a being 0 to 10, b being 1 to 50, m being 1 to 500, and n being 1 to 50.

[0122] In formula (D1), the arrangement of PO and EO may be a block copolymerization arrangement or a random copolymerization arrangement, and in formula (D1), the arrangement of the structural unit with subscript m and the structural unit with subscript n may be a block copolymerization arrangement or a random copolymerization arrangement.

[0123] R 1 is preferably an alkyl group having 1 to 3 carbon atoms, and more preferably a methyl group. 2 is preferably an alkanediyl group having 3 or 4 carbon atoms, and more preferably a trimethylene group. 3 is preferably an alkyl group having 1 to 3 carbon atoms, and more preferably a methyl group.

[0124] It is more preferable that a is 0, b is 1 to 15, m is 1 to 10, and n is 1 to 5. It is further more preferable that a is 0, b is 3 to 10, m is 1 to 3, and n is 1 to 3.

[0125] The silicone compound may be a commercially available product. Examples of commercially available silicone compounds include BYK-302, BYK-307, BYK-331, BYK-333, BYK-345, BYK-347, BYK-348, BYK-349, BYK-378, BYK-3400, BYK-3450, BYK-3451, BYK-3455, and BYK-3760 (all manufactured by BYK Japan), KF-351A, KF-352A, KF-353, KF-354L, KF-355A, KF-615A, KF-945, KF-640, KF-642, and KF-64 3, KF-644, KF-6011, KF-6012, KF-6015, KF-6017, KF-6020 (all manufactured by Shin-Etsu Chemical Co., Ltd.), Silface SAG002, Silface SAG005, Silface SAG008, Silface SAG503A (all manufactured by Nissin Chemical Industry Co., Ltd.), TEGOWet KL245, TEGOWet 240, TEGOWet 250, TEGOWet 260, TEGOWet 270, TEGOWet 280 (all manufactured by Evonik). All of these commercially available products are compounds represented by formula (D1).

[0126] As the acetylene compound, for example, a compound represented by the following formula (A1) is preferable.

[0127]

[0128] In formula (A1), R 1 and R 4 each independently represents an alkyl group having 3 to 10 carbon atoms; R 2 and R 3 each independently represents a methyl group or an ethyl group, and a, b, c, and d represent the average number of moles of each unit added, each of which is 0 to 50.

[0129] Examples of acetylene compounds include acetylene glycols selected from the group consisting of 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 3,6-dimethyl-4-octyne-3,6-diol, 2,5,6,11-tetramethyl-6-dodecyne-5,8-diol, 2,5-dimethyl-3-hexyne-2,5-diol, and 2,5,8,11-tetramethyl-6-dodecyne-5,8-diol; and ethylene oxide adducts of the above acetylene glycols. The acetylene compound can be synthesized, for example, by reacting acetylene with a ketone or aldehyde corresponding to the desired acetylene glycol. The acetylene compound can be obtained, for example, by the method described in Takehiko Fujimoto, revised edition, "New Introduction to Surfactants" (published by Sanyo Chemical Industries, Ltd., 1992), pp. 94-107. The acetylene compound may be a commercially available product. Examples of commercially available acetylene compounds include Surfynol 104E (HLB value 4), Surfynol 104H (HLB value 4), Surfynol 104A (HLB value 4), Surfynol 104PA (HLB value 4), Surfynol 104PG-50 (HLB value 4), Surfynol 104S (HLB value 4), Surfynol 420 (HLB value 4), Surfynol 440 (HLB value 8), Surfynol 465 (HLB value 13), Surfynol 485 (HLB value 17), Surfynol SE (HLB value 6), Surfynol SE-F (HLB value 6), Surfynol 61 (HLB value 6), Surfynol 82 (HLB value 8), and Surfynol 83 (HLB value 8). Examples of the surfactant include acetylcellulose (HLB value: 4), Surfynol DF110D (HLB value: 3), Dynol 604 (HLB value: 8), Dynol 607 (HLB value: 8), Surfynol 2502 (HLB value: 8), Surfynol TG (HLB value: 9), Olfine E1004 (HLB value: 7 to 9), Olfine E1010 (HLB value: 13 to 14) (all manufactured by Evonik Industries), Acetylenol E00, Acetylenol E13T, Acetylenol E40, Acetylenol E60, Acetylenol E100, Acetylenol E200 (all manufactured by Kawaken Fine Chemicals Co., Ltd.), and the like.

[0130] The content of the surfactant is preferably 0.01% by mass to 5.0% by mass, more preferably 0.02% by mass to 4.0% by mass, and even more preferably 0.1% by mass to 3.0% by mass, relative to the total amount of the ink.

[0131] (Other Components) The ink according to the present disclosure may contain other components in addition to the components described above, as necessary. Examples of other components include colloidal silica, inorganic salts, solid wetting agents (such as urea), anti-fading agents, emulsion stabilizers, penetration enhancers, UV absorbers, preservatives, anti-fungal agents, pH adjusters, antifoaming agents, viscosity adjusters, dispersion stabilizers, anti-rust agents, chelating agents, and water-soluble polymer compounds.

[0132] (Physical Properties of Ink) - Viscosity - The viscosity of the ink is preferably 1.2 mPa·s to 15.0 mPa·s, more preferably 2.0 mPa·s to 13.0 mPa·s, and even more preferably 2.5 mPa·s to 10.0 mPa·s. The viscosity of the ink is measured at a temperature of 30°C using a rotational viscometer, for example, a product name "VISCOMETER TV-22" manufactured by Toki Sangyo Co., Ltd.

[0133] Furthermore, the viscosity D of the ink when the volatile components contained in the ink are evaporated to reduce the mass by 45% is preferably 10 mPa·s to 100 mPa·s, and more preferably 20 mPa·s to 50 mPa·s.

[0134] The volatile components contained in the ink include, for example, water and organic solvents. The viscosity D is measured in the same manner as the ink viscosity described above after heating the ink to 35°C to evaporate the volatile components and reduce the mass by 45%.

[0135] If the viscosity D is 10 mPa·s or more, bleeding is suppressed, whereas if the viscosity D is 100 mPa·s or less, the ink has excellent ejection properties.

[0136] - pH - From the viewpoint of storage stability of the ink, the pH of the ink is preferably 6.0 to 11.0, more preferably 7.0 to 10.0, and even more preferably 7.0 to 9.5. The pH of the ink is measured at 25°C using a pH meter, for example, a product name "WM-50EG" manufactured by Toa DKK Corporation.

[0137] An example of an inkjet recording apparatus used in the inkjet recording method of the present disclosure will be described below with reference to the drawings.

[0138] In the drawings and descriptions thereof in this disclosure, substantially identical elements (for example, parts or portions) are denoted by the same reference numerals, and redundant descriptions may be omitted.

[0139] FIG. 1 is a conceptual diagram showing an inkjet recording apparatus 100, which is an example of an inkjet recording apparatus used in the inkjet recording method of the present disclosure.

[0140] 1, the inkjet recording apparatus 100 includes an ink application unit 101 including a first inkjet head 111A that ejects a first ink, a second inkjet head 111B that ejects a second ink, a second inkjet head 111C that ejects a third ink, and a fourth inkjet head 111D that ejects a fourth ink onto a continuous piece of paper 110 as a substrate. The distance between the first inkjet head 111A and the second inkjet head 111B is 100 mm to 500 mm. The distance between the second inkjet head 111B and the third inkjet head 111C, and the distance between the third inkjet head 111C and the fourth inkjet head 111D are also preferably 100 mm to 500 mm.

[0141] The ink application unit 101 has, for example, full-line inkjet heads 111A, 111B, 111C, and 111D for four colors arranged in this order from the upstream side in the transport direction of the continuous paper 110. The inkjet heads 111A, 111B, 111C, and 111D apply, for example, black (K) ink, cyan (C) ink, magenta (M) ink, and yellow (Y) ink to the continuous paper 110, respectively. However, the types and number of colors are not limited to these.

[0142] The preferred full-line inkjet head used here is a non-circulating head. This type of inkjet head is available from Kyocera. A second preferred full-line inkjet head has an ink circulation channel in the ink supply system. This channel allows fresh ink to be ejected and can be part of the ink supply system or part of a specially developed channel running behind the nozzle plate. The ink supply system preferably runs behind the nozzle plate to allow for more ink to be used without compromising resume / standby behavior. This type of inkjet head is available from Fujifilm Dimatix and Kyocera.

[0143] The inks ejected from the inkjet heads contain a pigment and an organic solvent. The details of the first ink and the second ink are as described above.

[0144] The continuous paper 110 is unwound from the main winding roller 102 and sent out by the transport roller 112 of the transport section 103 onto a transport guide member 113 arranged opposite the ink application section 101, and is transported (moved) while being guided by the transport guide member 113.

[0145] The continuous paper 110 to which ink has been applied by the ink application unit 101 passes through a heating and drying device (not shown), is sent by a discharge roller 118 and is taken up by a take-up roller 105 .

[0146] The inkjet recording apparatus may be provided with a preheating and drying device that heats the substrate in advance, or a substrate reversing device that allows ink to be applied to both sides of the substrate. The inkjet recording apparatus may also be provided with a heating device that applies radiant heating to the substrate to which ink has been applied. "Radiant heating" refers to the propagation of thermal energy through space or a medium, and an example of this is the flow of electromagnetic waves (electromagnetic radiation).

[0147] Hereinafter, the present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to the following examples as long as it does not depart from the gist of the disclosure.

[0148] In preparing each ink, each pigment dispersion and an aqueous dispersion 1 of resin particles were prepared in advance, and each ink was prepared using these.

[0149] <Synthesis of Water-Soluble Resin as Pigment-Dispersion Resin Precursor> Water-soluble resin 1 (resin before crosslinking) was synthesized as a precursor of crosslinked resin 1, a pigment-dispersion resin described below. Details are provided below. A monomer supply composition was prepared by mixing 172 parts by mass of methacrylic acid, 828 parts by mass of benzyl methacrylate, and 375 parts by mass of isopropanol. An initiator supply composition was prepared by mixing 2,2-azobis(2-methylbutyronitrile) (22.05 parts by mass) and 187.5 parts by mass of isopropanol. Next, isopropanol (187.5 parts by mass) was heated to 80°C under a nitrogen atmosphere, and the mixture of the monomer supply composition and the initiator supply composition was added dropwise thereto over 2 hours. After the dropwise addition was completed, the resulting solution was maintained at 80°C for an additional 4 hours and then cooled to 25°C. After cooling, the solvent was removed under reduced pressure to obtain a water-soluble resin 1 (methacrylic acid / benzyl methacrylate copolymer). The obtained water-soluble resin 1 had a weight-average molecular weight of about 30,000 and an acid value of 112 mgKOH / g.

[0150] <Preparation of Black Pigment Dispersion> 0.8 equivalents of methacrylic acid in the obtained water-soluble resin 1 (150 parts by mass) was neutralized with an aqueous potassium hydroxide solution. Ion-exchanged water was then added to adjust the concentration to 25% by mass, yielding an aqueous solution of water-soluble resin Q-1. Water-soluble resin Q-1 is a neutralized product of water-soluble resin 1, in which the carboxy groups (—C(═O)OH groups) in the aforementioned water-soluble resin 1 have been changed to —C(═O)ONa groups. An aqueous solution of water-soluble resin Q-1 (124 parts by mass) was mixed with black pigment (carbon black, product name “MA-100,” manufactured by Mitsubishi Chemical Corporation) (48 parts by mass), water (75 parts by mass), and dipropylene glycol (30 parts by mass), and the mixture was dispersed using a bead mill (bead diameter 0.1 mmφ, zirconia beads) until the desired volume average particle size was obtained, yielding a dispersion (uncrosslinked dispersion) in which the cyan pigment was dispersed in water-soluble resin Q-1. The pigment concentration of the cyan pigment in the uncrosslinked dispersion was 15% by mass. To this uncrosslinked dispersion (136 parts by mass), 1.3 parts by mass of trimethylolpropane polyglycidyl ether (product name "Denacol EX-321", manufactured by Nagase ChemteX Corporation) as a crosslinking agent and 14.3 parts by mass of an aqueous boric acid solution (boric acid concentration: 4% by mass) were added, and the mixture was reacted at 50°C for 6.5 hours. After that, the mixture was cooled to 25°C, whereby the water-soluble resin Q-1 was crosslinked by the crosslinking agent. This resulted in a dispersion (crosslinked dispersion) in which the black pigment was dispersed using the crosslinked resin 1 as a pigment dispersion resin. Here, the crosslinked resin 1 is a pigment dispersion resin obtained by crosslinking the water-soluble resin Q-1 with the above-mentioned crosslinking agent.

[0151] Next, ion-exchanged water was added to the obtained crosslinked dispersion, and ultrafiltration was performed using a stirring type ultra holder (manufactured by ADVANTEC Corporation) and an ultrafiltration filter (manufactured by ADVANTEC Corporation, molecular weight cutoff 50,000, Q0500076E Ultrafilter). The crosslinked dispersion was purified so that the dipropylene glycol concentration in the crosslinked dispersion was 0.1% by mass or less, and then concentrated to a pigment concentration of 15% by mass, thereby obtaining a black pigment dispersion in which the black pigment was dispersed with crosslinked resin 1 (black pigment concentration 15% by mass).

[0152] <Preparation of Cyan Pigment Dispersion> A cyan pigment dispersion (cyan pigment concentration 15% by mass) in which the cyan pigment was dispersed in crosslinked resin 1 was obtained in the same manner as in the preparation of the black pigment dispersion, except that the black pigment was changed to a cyan pigment (Pigment Blue 15:3, product name "Phthalocyanine Blue A220", manufactured by Dainichiseika Color & Chemicals Co., Ltd.).

[0153] <Preparation of Aqueous Dispersion 1 of Resin Particles> A three-necked flask equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube was charged with water (250 g), 12-methacrylamidodecanoic acid (6.7 g), potassium hydrogen carbonate (0.17 g), and isopropanol (20 g), and the temperature was raised to 85° C. under a nitrogen stream. To this was added a mixed solution consisting of 4,4′-azobis(4-cyanovaleric acid) (radical polymerization initiator, product name “V-501”, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) (0.11 g), potassium hydrogen carbonate (0.08 g), and water (9 g), and the mixture was stirred for 10 minutes. Next, a monomer solution consisting of styrene (14 g), benzyl methacrylate (14 g), methyl methacrylate (48 g), butyl methacrylate (3.3 g), and hydroxylethyl methacrylate (14 g) was added dropwise to the three-neck flask at a constant rate so that the addition was completed within 3 hours. Furthermore, a mixed solution consisting of V-501 (0.06 g), potassium bicarbonate (0.04 g), and water (6 g) was added in two portions, one immediately after the start of the addition of the monomer solution and the other 1.5 hours after the start of the addition of the monomer solution. After the addition of the monomer solution was completed, the mixture was stirred for 1 hour. Subsequently, a mixed solution consisting of V-501 (0.06 g), potassium bicarbonate (0.04 g), and water (6 g) was added to the resulting reaction mixture, and the mixture was stirred for an additional 3 hours. The resulting reaction mixture was filtered through a 50 μm mesh to obtain an aqueous dispersion 1 of resin particles.

[0154] Example 1 Preparation of Black Ink The components were mixed according to the following formulation to obtain a mixed solution: Next, coarse particles were removed from the mixed solution using a 1 μm filter to obtain a black ink.

[0155] - Composition - (Pigment) Black pigment dispersion (aqueous dispersion with a pigment concentration of 15% by mass) ... an amount such that the pigment content in the ink was 6 parts by mass and the pigment dispersion resin content was 2.4 parts by mass (Organic solvent) Diethylene glycol monoethyl ether (DEGmEE) (manufactured by Daicel Corporation) ... 8.0 parts by mass (Resin particles) Dispersion 1 of the resin particles prepared above (solid content concentration 25% by mass) ... an amount such that the resin particle content was 1.0 part by mass (Wax) "AQUACER 531" (PE wax emulsion) (solid content 45% by mass) manufactured by BYK Japan ... an amount such that the wax content was 1.0 part by mass (Surfactant) "Dynol 604" (solid content 50% by mass) manufactured by Nissin Chemical Industry Co., Ltd. (acetylene glycol surfactant; 2,5,8,11-tetramethyl-6-dodecyne-5,8-diol ethoxylate) ... 1.0 part by mass "EMULGEN 103" manufactured by Kao Corporation (a polyoxyethylene alkyl ether surfactant having 3 polyoxyethylene repeating units and being a lauryl ether) ... 1.0 part by mass "BYK-345" manufactured by BYK Corporation (a silicone surfactant having a structure represented by formula (D1), in which a is 0, b is 5.9, m is 1.8, and n is 1) ... 0.5 part by mass Water ... an amount that makes the total amount 100 parts by mass

[0156] <Preparation of cyan ink> The components were mixed according to the following formulation to obtain a mixed liquid: Next, coarse particles were removed from the mixed liquid using a 1 μm filter to obtain a cyan ink.

[0157] - Composition - (Pigment) Cyan pigment dispersion (aqueous dispersion with a pigment concentration of 15% by mass) ... an amount such that the pigment content in the ink was 3 parts by mass and the pigment dispersion resin content was 0.9 parts by mass (Organic solvent) Diethylene glycol monoethyl ether (DEGmEE) (manufactured by Daicel Corporation) ... 12.0 parts by mass (Resin particles) Dispersion 1 of the resin particles prepared above (solid content concentration 25% by mass) ... an amount such that the resin particle content was 1.5 parts by mass (Wax) "AQUACER 531" manufactured by BYK Japan KK (solid content 45% by mass) ... an amount such that the wax content was 1.0 part by mass (Surfactants) "Dynol 604" manufactured by Nissin Chemical Industry Co., Ltd. (solid content 50% by mass) ... 1.0 part by mass "Emulgen 103" manufactured by Kao Corporation ... 1.0 part by mass "BYK-345" manufactured by BYK ... 0.5 part by mass Water: Amount that makes the total amount 100 parts by mass

[0158] <Inkjet Recording> An inkjet recording apparatus having the same configuration as the inkjet recording apparatus shown in FIG. 1 was prepared. An inkjet recording line head "KJ4B-1200" (manufactured by Kyocera Corporation) (1200 dpi high-resolution model) was used as each inkjet head in the inkjet recording apparatus. The distance between the first inkjet head and the second inkjet head was 120 mm. The prepared black ink was ejected from the first inkjet head of the inkjet recording apparatus, and the prepared cyan ink was ejected from the second inkjet head of the inkjet recording apparatus. Inkjet recording was performed by drying the ink applied to the substrate while transporting the substrate to which the ink had been applied. After recording an image on one side of the substrate, the substrate was inverted using an inverting device. Then, an image was recorded on the other side of the substrate in the same manner. Detailed conditions for inkjet recording are as follows.

[0159] <Inkjet recording conditions> Substrate: Product name "OK Topcoat", manufactured by Oji Paper Co., Ltd. (water absorption: 4.9 g / m 2) - Substrate transport mechanism: Roll to roll - Inkjet head temperature: 32°C - Inkjet head resolution: 1200 dpi x 1200 dpi - Ink droplet volume: 3.0 pL - Environment around the inkjet head: Temperature 25°C ± 1°C, relative humidity 25°C ± 5% - Substrate transport speed: 80 m / min - Substrate tension during transport: 60 N

[0160] <Drying conditions> A preliminary drying device was used to blow hot air at 80°C onto the substrate before the ink was applied, thereby drying the substrate. After the black ink and cyan ink were applied, radiant heating was performed using an infrared heater within 3.0 seconds, and hot air at 140°C was blown onto the substrate using a drying device to dry the substrate to which the ink had been applied. Using the drying device, the mass of ink per unit area on the ink-applied surface of the substrate was dried to 200 μg / cm. 2 A drying treatment was carried out so that the substrate was dried. Thereafter, the substrate was brought into contact with a cooling roller. The cooling roller had a contact surface that came into contact with the ink-applied surface with a work of adhesion of 68.3 mN / m and a Vickers hardness of 450 Hv. The ink-applied surface of the substrate was then brought into contact with a heating drum and dried. The outer peripheral surface of the heating drum had a maximum static friction coefficient of 0.49 and an arithmetic mean roughness of 2.07 μm.

[0161] The resulting image recording material was used to evaluate the ejection properties and image quality. The evaluation methods were as follows.

[0162] <Ejection Performance> Using the inkjet recording device and the ink described above, a nozzle check pattern, which was a solid image at 100% duty, was continuously recorded in an area of ​​5,000 m in length on the recording medium. The final 10 m of the image-recorded portion was cut, and the number of missing nozzles in the nozzle check pattern was visually observed, and the ink ejection performance was evaluated according to the following evaluation criteria. In the evaluation criteria below, the best rank for ink ejection performance is A. Here, "missing nozzles" means that there are nozzles from which ink is not ejected, resulting in the appearance of white streaks. A: No missing nozzles. B: The number of missing nozzles was 1 to 3. C: The number of missing nozzles was 4 or more.

[0163] <Image Quality> -Graininess- The first ink was applied to a substrate in a square pattern with sides of 3 cm, and the second ink was applied over the first ink applied in the square pattern to record a square image with sides of 3 cm as a two-color image. The square image was recorded under conditions of 10% duty to 100% duty increments of 10% (i.e., a total of 10 types). Here, 100% duty refers to an image recorded under conditions in which one droplet of 3.0 pL of ink was applied per pixel (unit area of ​​(1 / 1200) inch x (1 / 1200) inch) at a resolution of 1200 dpi x 1200 dpi. The graininess of the resulting image was visually confirmed and evaluated according to the following evaluation criteria. Ranks based on the following evaluation criteria were determined by majority vote of five evaluators. In the evaluation criteria below, the rank A indicates the best graininess (i.e., the graininess is most suppressed). A: No graininess is observed. B: Slight graininess is observed. C: Graininess is observed. - Bleeding - The first ink was applied to a substrate at 100% duty in a line pattern of 500 μm in width, and the second ink was applied at 100% duty in a solid image form so as to cover the first ink applied in the line pattern and its periphery, thereby obtaining an image recorded material 1 for evaluating intercolor bleeding including a line pattern of a secondary color. Furthermore, the first ink was applied to a substrate at 100% duty in a solid pattern, and the second ink was applied at 100% duty in a line pattern of 500 μm in width on the first ink applied in the solid pattern, thereby obtaining an image recorded material 2 for evaluating intercolor bleeding including a line pattern of a secondary color. The width of the line pattern in image recording 1 and image recording 2 was measured at five locations each (i.e., a total of 10 locations), and the average of the 10 measurement results was calculated as the average width of the line pattern. Based on the calculated average width of the line pattern, inter-color bleeding was evaluated in accordance with the following evaluation criteria. In the evaluation criteria below, the rank in which bleeding and color mixing are most suppressed is A. A: The average width of the line pattern is less than 800 μm. B: The average width of the line pattern is 800 μm or more and less than 1000 μm. C: The average width of the line pattern is 1000 μm or more.

[0164] Examples 2 to 16, Comparative Examples 1 to 4 Image recording materials were obtained in the same manner as in Example 1, except that the types and contents of the components contained in the first ink and the second ink were changed to the types and contents shown in Table 1.

[0165] The evaluation results are shown in Table 1.

[0166] In Table 1, "Viscosity D" refers to the viscosity when the ink is heated to 35°C and the volatile components contained in the ink are evaporated to reduce the mass by 45%. "S1" refers to the viscosity when the SP value of the first ink relative to the pigment content is 28 MPa. 1/2 "S2" means the mass ratio of the organic solvent content in the second ink when the SP value relative to the pigment content is 28 MPa or less. 1/2 "T1" means the mass ratio of the content of the resin particles to the content of the wax in the first ink. "T2" means the mass ratio of the content of the resin particles to the content of the wax in the second ink. The content is expressed in % by mass, and the SP value is expressed in MPa. 1/2 "DEGmBE" means diethylene glycol monobutyl ether. "DEGmiPrE" means diethylene glycol monoisopropyl ether.

[0167]

[0168] As shown in Table 1, Examples 1 to 16 include a step of ejecting a first ink from a first inkjet head located upstream in the transport direction onto a substrate transported at a transport speed of 80 m / min or more, and a step of ejecting a second ink from a second inkjet head located downstream in the transport direction onto the substrate, the distance between the first inkjet head and the second inkjet head being 100 mm to 500 mm, the first ink and the second ink both containing a pigment and an organic solvent, and the SP value of the first ink relative to the pigment content being 28 MPa. 1/2 The mass ratio S1 of the content of the organic solvent is 0.5 to 1.6, and the SP value of the second ink relative to the content of the pigment is 28 MPa. 1/2It was found that the mass ratio S2 of the organic solvent content, which is greater than 1.6 and equal to or less than 5.0, was superior in ejection properties and image quality.

[0169] On the other hand, in Comparative Example 1, the mass ratio S1 was greater than 1.6 and the mass ratio S2 was greater than 5.0, which resulted in poor ejection properties. In Comparative Example 2, the mass ratio S1 was less than 0.5 and the mass ratio S2 was 1.6 or less, which resulted in poor image quality. In Comparative Example 3, the mass ratio S2 was greater than 5.0, which resulted in a blurred image and poor ejection properties. In Comparative Example 4, the mass ratio S1 was greater than 1.6, which resulted in a blurred image and poor ejection properties.

[0170] Example 100 Magenta ink and yellow ink were prepared. A magenta pigment dispersion was prepared in the same manner as for the preparation of the cyan pigment dispersion, except that a magenta pigment (product name "Pro-Jet Magenta APD4000": a pigment dispersion containing Pigment Red 122 (pigment concentration 20.0%, solids concentration 26.0%, manufactured by FUJIFILM Imaging Colorants) was used instead of the cyan pigment. A yellow pigment dispersion was prepared in the same manner as for the preparation of the cyan pigment dispersion, except that a yellow pigment (product name "Pro-Jet Yellow APD1000-TP": a pigment dispersion containing Pigment Yellow 74 (pigment concentration 15.0%, solids concentration 21.0%, manufactured by FUJIFILM Imaging Colorants) was used instead of the cyan pigment.

[0171] <Preparation of Magenta Ink> The components were mixed according to the following formulation to obtain a mixed solution: Next, coarse particles were removed from the mixed solution using a 1 μm filter to obtain a magenta ink.

[0172] - Composition - (Pigment) Magenta pigment dispersion (aqueous dispersion with a pigment concentration of 20% by mass) ... an amount such that the pigment content in the ink was 6.0 parts by mass and the pigment dispersion resin content was 1.8 parts by mass (Organic solvent) Diethylene glycol monoethyl ether (DEGmEE) (manufactured by Daicel Corporation) ... 8.0 parts by mass (Wax) AQUACER 531 (solid content 45% by mass) manufactured by BYK Japan KK ... an amount such that the wax content was 1.0 part by mass (Resin particles) Dispersion 1 of resin particles prepared above (solid content concentration 25% by mass) ... an amount such that the resin particle content was 1.0 part by mass (Surfactants) Dynol 604 (solid content 50% by mass) manufactured by Nissin Chemical Industry Co., Ltd. ... 1.0 part by mass Emulgen 103 manufactured by Kao Corporation ... 1.0 part by mass BYK-345 ... 0.5 parts by mass Water: Amount that makes the total amount 100 parts by mass

[0173] <Preparation of Magenta Ink> The components were mixed according to the following formulation to obtain a mixed solution: Next, coarse particles were removed from the mixed solution using a 1 μm filter to obtain a magenta ink.

[0174] - Composition - (Pigment) Yellow pigment dispersion (aqueous dispersion with a pigment concentration of 15% by mass) ... an amount such that the pigment content in the ink was 4.0 parts by mass and the pigment dispersion resin content was 1.2 parts by mass (Organic solvent) Diethylene glycol monoethyl ether (DEGmEE) (manufactured by Daicel Corporation) ... 8.0 parts by mass (Wax) AQUACER 531 (solid content 45% by mass) manufactured by BYK Japan KK ... an amount such that the wax content was 1.0 part by mass (Resin particles) Dispersion 1 of resin particles prepared above (solid content concentration 25% by mass) ... an amount such that the resin particle content was 1.5 parts by mass (Surfactants) Dynol 604 (solid content 50% by mass) manufactured by Nissin Chemical Industry Co., Ltd. ... 1.0 part by mass Emulgen 103 manufactured by Kao Corporation ... 1.0 part by mass BYK-345 ... 0.5 parts by mass Water: Amount that makes the total amount 100 parts by mass

[0175] <Inkjet recording> An inkjet recording apparatus having the same configuration as the inkjet recording apparatus shown in Fig. 1 was prepared. An image recording was obtained in the same manner as in Example 1, except that the black ink prepared in Example 1 was ejected from the first inkjet head of the inkjet recording apparatus, the cyan ink prepared in Example 1 was ejected from the second inkjet head of the inkjet recording apparatus, the prepared magenta ink was ejected from the third inkjet head of the inkjet recording apparatus, and the prepared yellow ink was ejected from the fourth inkjet head of the inkjet recording apparatus.

[0176] The first inkjet head that ejects black ink is 111A in Fig. 1, the second inkjet head that ejects cyan ink is 111B in Fig. 1, the third inkjet head that ejects magenta ink is 111C in Fig. 1, and the fourth inkjet head that ejects yellow ink is 111D in Fig. 1. In order to obtain the desired performance, the above-mentioned correspondence between the inks and the inkjet heads is most preferable.

[0177] The resulting image recording material was used to evaluate the ejection properties and image quality using the same evaluation methods as in Example 1. As a result, both were rated A.

[0178] Example 101 Aqueous dispersion 2 of resin particles, black ink and cyan ink were prepared.

[0179] <Preparation of Aqueous Dispersion 2 of Resin Particles> A three-neck flask equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen gas inlet tube was charged with water (250 g), 12-methacrylamidodecanoic acid (6.7 g), potassium hydrogen carbonate (2.46 g), and isopropanol (20 g), and the temperature was raised to 85° C. under a nitrogen stream. To this was added a mixed solution consisting of 4,4′-azobis(4-cyanovaleric acid) (radical polymerization initiator, product name “V-501”, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) (0.11 g), potassium hydrogen carbonate (0.08 g), and water (9 g), and the mixture was stirred for 10 minutes. Next, a monomer solution consisting of styrene (14 g), benzyl methacrylate (14 g), methyl methacrylate (48 g), butyl methacrylate (3.3 g), and hydroxylethyl methacrylate (14 g) was added dropwise to the three-neck flask at a constant rate so that the addition was completed within 3 hours. Furthermore, a mixed solution consisting of V-501 (0.06 g), potassium bicarbonate (0.04 g), and water (6 g) was added in two portions, one immediately after the start of the addition of the monomer solution and the other 1.5 hours after the start of the addition of the monomer solution. After the addition of the monomer solution was completed, the mixture was stirred for 1 hour. Subsequently, a mixed solution consisting of V-501 (0.06 g), potassium bicarbonate (0.04 g), and water (6 g) was added to the resulting reaction mixture, and the mixture was stirred for an additional 3 hours. The resulting reaction mixture was filtered through a 50 μm mesh to obtain an aqueous dispersion 2 of resin particles.

[0180] <Preparation of Black Ink> The components were mixed according to the following formulation to obtain a mixed liquid: Next, coarse particles were removed from the mixed liquid using a 1 μm filter to obtain a black ink.

[0181] - Composition - (Pigments) Black pigment (product name "Pro-Jet Black APD1000": pigment dispersion containing carbon black (pigment concentration 14.3%, manufactured by FUJIFILM Imaging Colorants) ... amount such that the pigment content in the ink is 4.0 parts by mass Cyan pigment (product name "Pro-Jet Cyan APD1000": pigment dispersion containing Pigment Blue 15:3 (pigment concentration 14.1%, manufactured by FUJIFILM Imaging Colorants) ... amount such that the pigment content in the ink is 1.0 part by mass Magenta pigment (product name "Pro-Jet Magenta APD1000": pigment dispersion containing Pigment Red 122 (pigment concentration 14.0%, manufactured by FUJIFILM 4.0 parts by mass (Wax) - "AQUACER 531" manufactured by BYK Japan KK (solid content 45% by mass) ... amount to provide a wax content of 1.0 part by mass (Resin particles) - Dispersion liquid 2 of resin particles prepared above (solid content concentration 25% by mass) ... amount to provide a resin particle content of 1.0 part by mass (Surfactants) - "Surfynol 465" manufactured by Nissin Chemical Industry Co., Ltd. ... 1.0 part by mass - "Emulgen 120" manufactured by Kao Corporation ... 1.0 part by mass - "BYK-347" manufactured by BYK ... 0.5 parts by mass (Other additives) Urea (Nissan Chemical Industries, Ltd.) ... 3% by mass Water ... amount that makes the total amount 100 parts by mass

[0182] <Preparation of cyan ink> The components were mixed according to the following formulation to obtain a mixed liquid: Next, coarse particles were removed from the mixed liquid using a 1 μm filter to obtain a cyan ink.

[0183] - Composition - (Pigment) Cyan pigment (product name "Pro-Jet Cyan APD1000": pigment dispersion containing Pigment Blue 15:3 (pigment concentration 14.1%, manufactured by FUJIFILM Imaging Colorants) ... amount such that the pigment content in the ink was 3.0 parts by mass (Organic Solvents) Propylene glycol (PG) (manufactured by ADEKA Corporation) ... 25.0 parts by mass Diethylene glycol monoisopropyl ether (DEGmiPrE) (manufactured by Nippon Nyukazai Co., Ltd.) ... 13.0 parts by mass (Wax) "AQUACER 531" (solid content 45% by mass) manufactured by BYK Japan KK ... amount such that the wax content was 1.0 part by mass (Resin Particles) Resin particle dispersion 2 prepared above (solid content concentration 25% by mass) ... amount such that the resin particle content was 1.0 part by mass (Surfactants) "Surfynol 465" manufactured by Nissin Chemical Industry Co., Ltd. ... 1.0 part by mass "Emulgen 120" manufactured by Kao Corporation ... 1.0 part by mass "BYK-347" manufactured by BYK Corporation ... 0.5 part by mass (Other additives) Urea (manufactured by Nissan Chemical Industries, Ltd.) ... 3% by mass Water ... amount that makes the total amount 100 parts by mass

[0184] The ink thus obtained was used to evaluate the ejection properties and image quality using the same evaluation methods as in Example 1. As a result, both were rated A.

[0185] Example 102 Magenta ink and yellow ink were prepared.

[0186] <Preparation of Magenta Ink> The components were mixed according to the following formulation to obtain a mixed solution: Next, coarse particles were removed from the mixed solution using a 1 μm filter to obtain a magenta ink.

[0187] - Composition - (Pigment) Magenta pigment (product name "Pro-Jet Magenta APD1000": pigment dispersion containing Pigment Red 122 (pigment concentration 14.0%, manufactured by FUJIFILM Imaging Colorants) ... amount such that the pigment content in the ink was 5.0 parts by mass (Organic Solvents) Propylene glycol (PG) (manufactured by ADEKA Corporation) ... 25.0 parts by mass Diethylene glycol monoisopropyl ether (DEGmiPrE) (manufactured by Nippon Nyukazai Co., Ltd.) ... 8.0 parts by mass (Wax) "AQUACER 531" (solid content 45% by mass) manufactured by BYK Japan KK ... amount such that the wax content was 1.0 part by mass (Resin Particles) Dispersion 2 of the resin particles prepared above (solid content concentration 25% by mass) Amounts that make the resin particle content 1.0 part by mass (Surfactants) - "Surfynol 465" manufactured by Nissin Chemical Industry Co., Ltd. ... 1.0 part by mass - "Emulgen 120" manufactured by Kao Corporation ... 1.0 part by mass - "BYK-347" manufactured by BYK Corporation ... 0.5 part by mass (Antifoaming agents) - "BYK-094" manufactured by BYK Corporation ... 0.05 part by mass (Other additives) - Urea (manufactured by Nissan Chemical Industries Co., Ltd.) ... 3% by mass - Water ... amounts that make the total amount 100 parts by mass

[0188] <Preparation of Yellow Ink> The components were mixed according to the following formulation to obtain a mixed liquid: Next, coarse particles were removed from the mixed liquid using a 1 μm filter to obtain a yellow ink.

[0189] - Composition - (Pigment) Yellow pigment (product name "Pro-Jet Yellow APD4000": pigment dispersion containing Pigment Yellow 74 (pigment concentration 19.9%, manufactured by FUJIFILM Imaging Colorants) ... amount such that the pigment content in the ink was 4.0 parts by mass (Organic Solvents) Propylene glycol (PG) (manufactured by ADEKA Corporation) ... 25.0 parts by mass Diethylene glycol monoisopropyl ether (DEGmiPrE) (manufactured by Nippon Nyukazai Co., Ltd.) ... 8.0 parts by mass (Wax) "AQUACER 531" (solid content 45% by mass) manufactured by BYK Japan KK ... amount such that the wax content was 1.0 part by mass (Resin Particles) Resin particle dispersion 2 prepared above (solid content concentration 25% by mass) ... amount such that the resin particle content was 1.0 part by mass (Surfactants) "Surfynol 465" manufactured by Nissin Chemical Industry Co., Ltd. ... 1.0 part by mass "Emulgen 120" manufactured by Kao Corporation ... 1.0 part by mass "BYK-347" manufactured by BYK Corporation ... 0.5 part by mass (Antifoaming agent) "BYK-094" manufactured by BYK Corporation ... 0.05 part by mass (Other additives) Urea (manufactured by Nissan Chemical Industries, Ltd.) ... 3% by mass Water ... amounts that make the total amount 100 parts by mass

[0190] The ink thus obtained was used to evaluate the ejection properties and image quality using the same evaluation methods as in Example 1. As a result, both were rated A.

[0191] Example 103 Aqueous dispersion 3 of resin particles, black ink and cyan ink were prepared.

[0192] <Preparation of Aqueous Dispersion 3 of Resin Particles> A 2-liter three-neck flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube was charged with water (932 g), 12-methacrylamidodecanoic acid (2.02 g), potassium hydrogen carbonate (0.76 g), 4-hydroxy-2,2,6,6-tetramethylpiperidine 1-oxyl free radical (0.42 mg), and Olfine E1020 (surfactant, manufactured by Nissin Chemical Industry Co., Ltd., 17 mg), and the mixture was heated to 80°C under a nitrogen stream and stirred until homogeneous. A mixed solution consisting of potassium persulfate (0.27 g), potassium hydrogen carbonate (0.22 g), and water (18.2 g) was added to the flask and stirred. Next, a monomer solution prepared by mixing methyl methacrylate (206.0 g), benzyl methacrylate (60.0 g), styrene (60.0 g), and n-butyl acrylate (14.0 g), and an aqueous monomer solution consisting of 12-methacrylamidodecanoic acid (23.2 g), potassium bicarbonate (8.62 g), 2-hydroxyethyl methacrylate (60 g), water (160 g), and p-methoxyphenol (15 mg) were added dropwise to the three-neck flask. Simultaneously with the start of the dropwise addition of the monomer solution and the aqueous monomer solution, a mixed solution consisting of potassium persulfate (1.44 g), potassium bicarbonate (1.11 g), and water (127 g) was added dropwise. After the dropwise addition of the monomer solution and the aqueous monomer solution was completed, the mixture was further stirred, and then water (58 g) and PROXCEL GXL(S) (benzoisothiazolin-3-one solution, manufactured by Arch Chemicals Japan, 0.4 g) were added. The resulting reaction mixture was filtered through a 50 μm mesh to obtain an aqueous dispersion 3 of resin particles.

[0193] <Preparation of Black Ink> The components were mixed according to the following formulation to obtain a mixed liquid: Next, coarse particles were removed from the mixed liquid using a 1 μm filter to obtain a black ink.

[0194] - Composition - (Pigments) Black pigment (product name "Pro-Jet Black APD1000": pigment dispersion containing carbon black (pigment concentration 14.3%, manufactured by FUJIFILM Imaging Colorants) ... amount such that the pigment content in the ink is 4.0 parts by mass Cyan pigment (product name "Pro-Jet Cyan APD1000": pigment dispersion containing Pigment Blue 15:3 (pigment concentration 14.1%, manufactured by FUJIFILM Imaging Colorants) ... amount such that the pigment content in the ink is 1.0 part by mass Magenta pigment (product name "Pro-Jet Magenta APD1000": pigment dispersion containing Pigment Red 122 (pigment concentration 14.0%, manufactured by FUJIFILM 1.0 parts by mass (Surfactants) - "Dynostix 100" manufactured by Imaging Colorants... amount such that the pigment content in the ink is 2.0 parts by mass (Organic solvents) - Propylene glycol (PG) (manufactured by ADEKA Corporation)... 20.0 parts by mass - Diethylene glycol monoethyl ether (DEGmEE) (manufactured by Daicel Corporation)... 8.0 parts by mass (Wax) - "Hitec E-6314" manufactured by Toho Chemical Industry Co., Ltd. (solid content 35% by mass)... amount such that the wax content is 1.0 part by mass (Resin particles) - Dispersion 3 of resin particles prepared above (solid content concentration 25% by mass)... amount such that the resin particle content is 1.0 part by mass (Surfactants) - "Dynostix 100" manufactured by Nissin Chemical Industry Co., Ltd.... 1.0 part by mass - "Emulgen 103" manufactured by Kao Corporation... 1.0 part by mass - "BYK-345" manufactured by BYK... 0.5 part by mass (Other additives) Urea (Nissan Chemical Industries, Ltd.) ... 3 mass % Water ... amount that makes the total amount 100 mass parts

[0195] <Preparation of cyan ink> The components were mixed according to the following formulation to obtain a mixed liquid: Next, coarse particles were removed from the mixed liquid using a 1 μm filter to obtain a cyan ink.

[0196] - Composition - (Pigment) Cyan pigment (product name "Pro-Jet Cyan APD1000": pigment dispersion containing Pigment Blue 15:3 (pigment concentration 14.1%, manufactured by FUJIFILM Imaging Colorants) ... amount such that the pigment content in the ink was 3.0 parts by mass (Organic Solvents) Propylene glycol (PG) (manufactured by ADEKA Corporation) ... 25.0 parts by mass Diethylene glycol monoethyl ether (DEGmEE) (manufactured by Daicel Corporation) ... 13.0 parts by mass (Wax) "Hitec E-6314" manufactured by Toho Chemical Industry Co., Ltd. (solid content 35% by mass) ... amount such that the wax content was 1.0 part by mass (Resin Particles) Resin particle dispersion 3 prepared above (solid content concentration 25% by mass) ... amount such that the resin particle content was 1.0 part by mass (Surfactant) "Dynol 604" manufactured by Nissin Chemical Industry Co., Ltd.: 1.0 part by mass "Emulgen 103" manufactured by Kao Corporation: 1.0 part by mass "BYK-345" manufactured by BYK Corporation: 0.5 part by mass (Other additives) Urea (manufactured by Nissan Chemical Industries Co., Ltd.): 3% by mass Water: Amount that makes the total amount 100 parts by mass

[0197] The ink thus obtained was used to evaluate the ejection properties and image quality using the same evaluation methods as in Example 1. As a result, both were rated A.

[0198] Example 104 Magenta ink and yellow ink were prepared.

[0199] <Preparation of Magenta Ink> The components were mixed according to the following formulation to obtain a mixed solution: Next, coarse particles were removed from the mixed solution using a 1 μm filter to obtain a magenta ink.

[0200] - Composition - (Pigment) Magenta pigment (product name "Pro-Jet Magenta APD1000": pigment dispersion containing Pigment Red 122 (pigment concentration 14.0%, manufactured by FUJIFILM Imaging Colorants) ... amount such that the pigment content in the ink was 5.0 parts by mass (Organic solvent) Propylene glycol (PG) (manufactured by ADEKA Corporation) ... 25.0 parts by mass Diethylene glycol monoethyl ether (DEGmEE) (manufactured by Daicel Corporation) ... 8.0 parts by mass (Wax) "Hitec E-6314" (solid content 35% by mass) manufactured by Toho Chemical Industry Co., Ltd. ... amount such that the wax content was 1.0 part by mass (Resin particles) Dispersion 3 of resin particles prepared above (solid content concentration 25% by mass) ... amount such that the resin particle content was 1.0 part by mass (Surfactant) "Dynol 604" manufactured by Nissin Chemical Industry Co., Ltd. ... 1.0 part by mass "Emulgen 103" manufactured by Kao Corporation ... 1.0 part by mass "BYK-345" manufactured by BYK Corporation ... 0.5 part by mass (Antifoaming agent) "BYK-094" manufactured by BYK Corporation ... 0.05 part by mass (Other additives) Urea (manufactured by Nissan Chemical Industries, Ltd.) ... 3% by mass Water ... amount that makes the total amount 100 parts by mass

[0201] <Preparation of Yellow Ink> The components were mixed according to the following formulation to obtain a mixed liquid: Next, coarse particles were removed from the mixed liquid using a 1 μm filter to obtain a yellow ink.

[0202] - Composition - (Pigment) Yellow pigment (product name "Pro-Jet Yellow APD4000": pigment dispersion containing Pigment Yellow 74 (pigment concentration 19.9%, manufactured by FUJIFILM Imaging Colorants) ... amount such that the pigment content in the ink was 4.0 parts by mass (Organic solvent) Propylene glycol (PG) (manufactured by ADEKA Corporation) ... 25.0 parts by mass Diethylene glycol monoethyl ether (DEGmEE) (manufactured by Daicel Corporation) ... 8.0 parts by mass (Wax) "Hitec E-6314" (solid content 35% by mass) manufactured by Toho Chemical Industry Co., Ltd. ... amount such that the wax content was 1.0 part by mass (Resin particles) Dispersion 3 of resin particles prepared above (solid content concentration 25% by mass) ... amount such that the resin particle content was 1.0 part by mass (Surfactant) "Dynol 604" manufactured by Nissin Chemical Industry Co., Ltd. ... 1.0 part by mass "Emulgen 103" manufactured by Kao Corporation ... 1.0 part by mass "BYK-345" manufactured by BYK Corporation ... 0.5 part by mass (Antifoaming agent) "BYK-094" manufactured by BYK Corporation ... 0.05 part by mass (Other additives) Urea (manufactured by Nissan Chemical Industries, Ltd.) ... 3% by mass Water ... amount that makes the total amount 100 parts by mass

[0203] The ink thus obtained was used to evaluate the ejection properties and image quality using the same evaluation methods as in Example 1. As a result, both were rated A.

[0204] Example 105 Black ink and cyan ink were prepared in the same manner as in Example 103, except that the magenta pigment used in <Preparation of Black Ink> in Example 103 was changed to the following magenta pigment and the water content was adjusted. Magenta pigment (product name "Pro-Jet Magenta APD4000": pigment dispersion containing Pigment Red 122 (pigment concentration 20.0%, solid content concentration 26.0%, manufactured by FUJIFILM Imaging Colorants)...amount that would result in a pigment content of 4.0 parts by mass in the ink

[0205] The ink thus obtained was used to evaluate the ejection properties and image quality using the same evaluation methods as in Example 1. As a result, both were rated A.

[0206] Example 106 A magenta ink and a yellow ink were prepared in the same manner as in Example 104, except that the magenta pigment used in the magenta ink of Example 104 was changed to the magenta pigment shown below and the water content was adjusted, and the magenta pigment used in the yellow ink of Example 104 was changed to the yellow pigment shown below. Magenta pigment (product name "Pro-Jet Magenta APD4000": pigment dispersion containing Pigment Red 122 (pigment concentration 20.0%, solid content concentration 26.0%, manufactured by FUJIFILM Imaging Colorants)... amount that results in a pigment content of 4.0 parts by mass in the ink. Yellow pigment (product name "Pro-Jet Yellow APD1000-TP": pigment dispersion containing Pigment Yellow 74 (pigment concentration 15.0%, solid content concentration 21.0%, manufactured by FUJIFILM Imaging Colorants)... amount that results in a pigment content of 4.0 parts by mass in the ink.

[0207] The ink thus obtained was used to evaluate the ejection properties and image quality using the same evaluation methods as in Example 1. As a result, both were rated A.

[0208] Example 107 Black ink and cyan ink were prepared in the same manner as in Example 101, except that the black pigment used in <Preparation of Black Ink> in Example 101 was changed to the following black pigment: Black pigment (product name "Pro-Jet Black APD4000": pigment dispersion containing carbon black (pigment concentration 15.0%, manufactured by FUJIFILM Imaging Colorants)...amount that would result in a pigment content of 4.0 parts by mass in the ink

[0209] The ink thus obtained was used to evaluate the ejection properties and image quality using the same evaluation methods as in Example 1. As a result, both were rated A.

[0210] Example 108 Ink was prepared in the same manner as in Example 101. Treatment liquid A was prepared in the following manner.

[0211] <Preparation of Treatment Liquid A> The components of the following composition were mixed to obtain treatment liquid A. - Composition of Treatment Liquid A - DEGmBE (diethylene glycol monobutyl ether)... 6.0 mass % Malonic acid... 5.6 mass % Malic acid... 3.83 mass % Phosphoric acid 85 mass % aqueous solution... 3.37 mass % Water-soluble polymer 1 below... 0.4 mass % Antifoaming agent (TSA-739 (15%) manufactured by Momentive Performance Materials Japan LLC; emulsion-type silicone antifoaming agent)... 0.0083 mass % as silicone oil Teika Power BN2070M (surfactant manufactured by Teika Corporation)... 0.42 mass % as active ingredient Benzotriazole... 1.0 mass % Ion-exchanged water... balance to make the total 100 mass %

[0212] <Synthesis of Water-Soluble Polymer 1> Water-soluble polymer 1 to be used as a component in the treatment liquid was synthesized. This synthesis was carried out in accordance with paragraphs 0200 to 0204 and 0229 of JP 2013-001854 A. The structure of water-soluble polymer 1 is shown below. In the water-soluble polymer 1 shown below, the numbers to the bottom right of each structural unit represent the mass ratio (% by mass), and Mw represents the weight-average molecular weight.

[0213]

[0214] In the inkjet recording of Example 1, the treatment liquid A was applied in advance to a substrate using a bar coater (K ​​hand coater, No. 1, RK Print Coat Instruments Ltd.) in an amount of 6.7 g / m 2 An image recording material was prepared in the same manner as in Example 1, except that the coating was carried out so that the image recording material was

[0215] Using the obtained image recording matter, the ejection performance and image quality were evaluated using the same evaluation methods as in Example 1, and both were rated A. [Example 109] Aqueous dispersion 4 of resin particles, black ink, and cyan ink were prepared.

[0216] <Preparation of Aqueous Dispersion 4 of Resin Particles> A 20-liter three-neck flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube was charged with water (9,320 g), 12-methacrylamidodecanoic acid (20.2 g), potassium bicarbonate (7.6 g), 4-hydroxy-2,2,6,6-tetramethylpiperidine 1-oxyl free radical (4.20 mg), and Olfine E1020 (surfactant, manufactured by Nissin Chemical Industry Co., Ltd., 170 mg), and the mixture was heated to 80°C under a nitrogen stream and stirred until homogenous. A mixed solution consisting of potassium persulfate (2.7 g), potassium bicarbonate (2.2 g), and water (182 g) was added to the flask and stirred for 1 minute. Next, a monomer solution prepared by mixing methyl methacrylate (2,200 g), benzyl methacrylate (750 g), styrene (750 g), and n-butyl acrylate (140 g), and an aqueous monomer solution consisting of 12-methacrylamidodecanoic acid (58 g), potassium bicarbonate (86.2 g), 2-hydroxyethyl methacrylate (600 g), water (1,600 g), and p-methoxyphenol (150 mg) were added dropwise to the three-neck flask at a constant rate so that the addition would be completed within one hour. Simultaneously with the start of the addition of the monomer solution and the aqueous monomer solution, a mixed solution consisting of potassium persulfate (14.4 g), potassium bicarbonate (11.1 g), and water (1,270 g) was added dropwise so that the addition would be completed within one hour. After the dropwise addition of the monomer solution and the aqueous monomer solution was completed, the mixture was further stirred, and then water (580 g) and PROXCEL GXL(S) (4.0 g of a benzisothiazolin-3-one solution, manufactured by Arch Chemicals Japan Co., Ltd.) were added. The resulting reaction mixture was filtered through a 100 μm mesh and then further filtered through a 50 μm mesh to obtain an aqueous dispersion 4 of resin particles.

[0217] <Preparation of Black Ink> A black ink was prepared in the same manner as in <Preparation of Black Ink> of Example 101, except that diethylene glycol monoisopropyl ether (DEGmiPrE) in Example 101 was replaced with the following component, the water content was adjusted, and Resin particle dispersion liquid 4 was used instead of Resin particle dispersion liquid 2: Ethylene glycol monohexyl ether (EGmHE) (manufactured by Nippon Nyukazai Co., Ltd.) ... 4.0 parts by mass

[0218] <Preparation of Cyan Ink> A cyan ink was prepared in the same manner as in <Preparation of Cyan Ink> in Example 101, except that diethylene glycol monoisopropyl ether (DEGmiPrE) in Example 101 was replaced with the following component, the water content was adjusted, and Resin Particle Dispersion 4 was used instead of Resin Particle Dispersion 2: Ethylene glycol monohexyl ether (EGmHE) (manufactured by Nippon Nyukazai Co., Ltd.) ... 4.0 parts by mass

[0219] The ink thus obtained was used to evaluate the ejection properties and image quality using the same evaluation methods as in Example 1. As a result, both were rated A.

[0220] Example 110 Magenta ink and yellow ink were prepared.

[0221] <Preparation of Magenta Ink> A magenta ink was prepared in the same manner as in <Preparation of Magenta Ink> in Example 102, except that diethylene glycol monoisopropyl ether (DEGmiPrE) in Example 102 was replaced with the following component, the water content was adjusted, and Resin Particle Dispersion 4 was used instead of Resin Particle Dispersion 2: Ethylene glycol monohexyl ether (EGmHE) (manufactured by Nippon Nyukazai Co., Ltd.) ... 4.0 parts by mass

[0222] <Preparation of Yellow Ink> A yellow ink was prepared in the same manner as in <Preparation of Yellow Ink> in Example 102, except that diethylene glycol monoisopropyl ether (DEGmiPrE) in Example 102 was changed to the following component, the water content was adjusted, and Resin Particle Dispersion 4 was used instead of Resin Particle Dispersion 2: Ethylene glycol monohexyl ether (EGmHE) (manufactured by Nippon Nyukazai Co., Ltd.) ... 4.0 parts by mass

[0223] The ink thus obtained was used to evaluate the ejection properties and image quality using the same evaluation methods as in Example 1. As a result, both were rated A.

[0224] The disclosure of Japanese Patent Application No. 2023-085716, filed on May 24, 2023, is incorporated herein by reference in its entirety. In addition, all documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually indicated to be incorporated by reference.

Claims

1. A method for producing a printing ink comprising: ejecting a first ink from a first inkjet head located upstream in a conveying direction onto a substrate conveyed at a conveying speed of 80 m / min or more; ejecting a second ink from a second inkjet head located downstream in the conveying direction onto the substrate; a distance between the first inkjet head and the second inkjet head is 100 mm to 500 mm; both the first ink and the second ink contain a pigment and an organic solvent; and an SP value for the pigment content in the first ink is 28 MPa. 1/2 the mass ratio S1 of the content of the organic solvent is 0.5 to 1.6, and the SP value of the second ink relative to the content of the pigment is 28 MPa or less. 1/2 a mass ratio S2 of the content of the organic solvent, which is greater than 1.6 and not greater than 5.0, 2. The ink jet recording method according to claim 1, wherein the mass ratio S1 is 1.0 to 1.4, and the mass ratio S2 is 3.5 to 4.

5.

3. The inkjet recording method according to claim 1 or 2, wherein the difference between the mass ratio S1 and the mass ratio S2 is 1.5 to 4.

0.

4. An inkjet recording method according to claim 1 or claim 2, wherein both the first ink and the second ink contain resin particles, the content of the resin particles in the first ink is 0.1% by mass to 1.8% by mass relative to the total amount of the first ink, and the content of the resin particles in the second ink is 0.1% by mass to 4.0% by mass relative to the total amount of the second ink.

5. An inkjet recording method according to claim 1 or claim 2, wherein both of the first ink and the second ink contain wax, a mass ratio T1 of the content of resin particles to the content of wax in the first ink is 0.1 to 2.0, and a mass ratio T2 of the content of resin particles to the content of wax in the second ink is 0.1 to 6.

0.

6. The ink jet recording method according to claim 5, wherein the mass ratio T1 is 0.5 to 1.6, and the mass ratio T2 is 0.5 to 4.

5.

7. The inkjet recording method according to claim 1 or 2, wherein the first ink and the second ink each have a viscosity D of 10 mPa·s to 100 mPa·s when the volatile components are evaporated to reduce the mass by 45%.

8. The ink jet recording method according to claim 7, wherein the viscosity D of each of the first ink and the second ink is 20 mPa·s to 50 MPa·s.

9. An inkjet recording method according to claim 1 or 2, wherein both of the first ink and the second ink contain a surfactant, and the surfactant contains at least one selected from the group consisting of a polyoxyalkylene alkyl ether compound, an acetylene compound, and a silicone compound.

10. An inkjet recording method according to claim 1 or 2, wherein the pigments contained in the first ink and the second ink are both at least partially coated with a resin having a crosslinked structure.

11. The ink jet recording method according to claim 1 or 2, wherein the first ink is a black ink, and the second ink is a cyan ink.

Citation Information

Patent Citations

  • Photopolymerization composition, photopolymerizable color composition and color filter

    JP2002012607A

  • Actinic energy ray-curable ink-jet ink

    JP2002188025A

  • Recording liquid

    JP2003026978A

  • Black ink for ink-jet recording and method for forming image

    JP2003342503A

  • Ink set and image forming method

    JP2013001854A