Method for producing multilayer ceramic electronic component

The method of alternately stacking and arranging laminates with exposed conductor layers and attaching a functional member addresses the challenge of forming uniform side margins in multilayer ceramic components, enhancing insulation and reducing defects, thereby improving the manufacturing efficiency and reliability of these components.

WO2024241888A1PCT designated stage expired Publication Date: 2024-11-28KYOCERA CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017180
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-25
Filing Date
2024-05-08
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional methods for manufacturing multilayer ceramic electronic components face challenges in forming uniform side margin portions, leading to potential insulation issues around internal electrodes, especially as component heights decrease, and tilting of green chips during the manufacturing process.

Method used

A method involving the alternately stacked first and second laminates with exposed conductor layers, where the first laminate has a shorter main surface distance than side surface distance, and the second laminate has a shorter main surface distance than end surface distance, are arranged to intersect perpendicularly, and a functional member is attached to the side surfaces, reducing the likelihood of defects by aligning the laminates to prevent mutual falling and ensure uniform attachment.

Benefits of technology

This approach enhances the formation of uniform side margin portions, reduces defects, and ensures reliable insulation around internal electrodes, improving the manufacturing efficiency and reliability of low-profile multilayer ceramic electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024017180_28112024_PF_FP_ABST
    Figure JP2024017180_28112024_PF_FP_ABST
Patent Text Reader

Abstract

This method for producing a multilayer ceramic electronic component comprises a preparation step, an arrangement step, and an attachment step. In the preparation step, a first laminate and a second laminate are prepared. The first laminate is configured such that a distance between a pair of first main surfaces is smaller than a distance between a pair of first side surfaces, and a plurality of first conductor layers are exposed from the first side surfaces. The second laminate is configured such that a distance between a pair of second main surfaces is smaller than a distance between a pair of second side surfaces, and a plurality of second conductor layers are exposed from the second side surfaces. In the arrangement step, the first laminate and the second laminate are arranged such that the first side surfaces and the second side surfaces are open surfaces, and a direction orthogonal to the first main surfaces and a direction orthogonal to the second main surfaces intersect each other. In the attachment step, functional members are attached to the first side surfaces and the second side surfaces, which are open surfaces.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method for multilayer ceramic electronic components

[0001] The present invention relates to a method for manufacturing a multilayer ceramic electronic component.

[0002] A conventional method for manufacturing a multilayer ceramic electronic component is described in, for example, Japanese Patent Application Laid-Open No. 2003-222999.

[0003] Japanese Patent Application Laid-Open No. 2012-209539

[0004] A method for manufacturing a multilayer ceramic electronic component according to one embodiment of the present disclosure includes: a preparation step of preparing a first laminate including a plurality of first conductor layers and a plurality of first ceramic layers stacked alternately, the first laminate having a pair of first main surfaces, a pair of first end surfaces, and a pair of first side surfaces, wherein the distance between the pair of first main surfaces is smaller than the distance between the pair of first side surfaces and the plurality of first conductor layers are exposed from the first side surfaces; and a second laminate including a plurality of second conductor layers and a plurality of second ceramic layers stacked alternately, the second laminate having a pair of second main surfaces, a pair of second end surfaces, and a pair of second side surfaces, wherein the distance between the pair of second main surfaces is smaller than the distance between the pair of second side surfaces and the plurality of second conductor layers are exposed from the second side surfaces; an arrangement step of arranging the first laminate and the second laminate so that the first side surfaces and the second side surfaces are open surfaces and a direction orthogonal to the first main surfaces intersects with a direction orthogonal to the second main surfaces; and an attachment step of attaching functional members to the first side surfaces and the second side surfaces that serve as the open surfaces.

[0005] Objects, features, and advantages of the present disclosure will become more apparent from the detailed description and drawings below.

[0023] FIG. 1 is a schematic diagram of a multilayer ceramic electronic component according to an embodiment of the present disclosure.

[0024] FIG. 2 is a schematic diagram of an element body according to an embodiment of the present disclosure.

[0025] FIG. 3 is a schematic diagram showing, in isolation, each component of an element body according to an embodiment of the present disclosure.

[0026] FIG. 4 is a flowchart showing a method for manufacturing a multilayer ceramic electronic component according to an embodiment of the present disclosure.

[0027] FIG. 5 is a schematic diagram showing ceramic sheets and conductor sheets arranged thereon according to an embodiment of the present disclosure.

[0028] FIG. 6 is a schematic diagram showing ceramic sheets and conductor sheets arranged thereon according to an embodiment of the present disclosure.

[0029] FIG. 7 is a perspective view schematically showing the lamination of a base laminate according to an embodiment of the present disclosure.

[0030] FIG. 8 is a schematic perspective view of a base laminate according to an embodiment of the present disclosure.

[0031] FIG. 9 is a schematic perspective view of a laminate according to an embodiment of the present disclosure.

[0032] FIG. 10 is a schematic diagram of a first laminate and a second laminate according to an embodiment of the present disclosure.

[0033] FIG. 11 is a diagram showing a housing member and the laminates housed in the housing member.

[0034] FIG. 12 is a diagram showing a housing member and the laminates housed in the housing member.

[0035] FIG. 13 is a diagram showing a rolling process using a magnet.

[0036] FIG. 14 is a diagram showing a rolling process using a magnet. FIG. 10 is a diagram schematically showing the step of rolling by a magnet. FIG. 11 is a diagram schematically showing the step of rolling by a magnet. FIG. 12 is a diagram schematically showing the process of the fifth step. FIG. 13 is a diagram schematically showing the process of the fifth step. FIG. 14 is a diagram schematically showing the process of the fifth step. FIG. 15 is a schematic perspective view of an element body precursor according to an embodiment of the present disclosure.

[0006] In recent years, with the miniaturization and high performance of electronic devices, there has been a growing demand for smaller, thinner, and higher-capacitance multilayer ceramic electronic components, such as multilayer ceramic capacitors, used in electronic devices. To meet this demand, for example, it is effective to enlarge the internal electrodes of multilayer ceramic capacitors. To enlarge the internal electrodes, it is necessary to thin the side margins around the internal electrodes to ensure insulation.

[0007] On the other hand, in a typical manufacturing method of a multilayer ceramic capacitor, it is difficult to form side margins of uniform thickness due to the precision of each process, such as patterning of the internal electrodes and cutting of the laminated sheet, etc. Therefore, in such a manufacturing method of a multilayer ceramic capacitor, the narrower the side margins are, the more difficult it becomes to ensure insulation around the internal electrodes.

[0008] For example, Patent Document 1 discloses a method of preparing a mother block including a plurality of ceramic green sheets and a plurality of internal electrode patterns, cutting the mother block, preparing green chips with the internal electrodes exposed on the cut side surfaces, and attaching ceramic green sheets for side surfaces to the cut side surfaces. According to the method of Patent Document 1, it is possible to form a thin and uniform side margin portion while ensuring insulation around the internal electrodes.

[0009] As the height of multilayer ceramic capacitors continues to decrease, the method described in Patent Document 1 could result in the green chip tilting during the process of attaching a side ceramic green sheet to the cut side of the green chip, which is an open surface, potentially causing problems with the side margins that are formed.

[0010] Hereinafter, with reference to the drawings, a description will be given of a multilayer ceramic electronic component 1 according to an embodiment of the present disclosure and a method for manufacturing the multilayer ceramic electronic component 1. Note that, although a multilayer ceramic capacitor will be described below as an example of the multilayer ceramic electronic component 1, the multilayer ceramic electronic component to which the present disclosure is directed is not limited to a multilayer ceramic capacitor and can be applied to various other multilayer ceramic electronic components such as a multilayer piezoelectric element, a multilayer thermistor element, a multilayer coil, and a multilayer ceramic multilayer substrate.

[0011] It should be noted that the drawings used in the following description are schematic, and the dimensional ratios and the like in the drawings do not necessarily correspond to the actual ones. Furthermore, each embodiment described in this specification is an example, and different embodiments and modified examples may be partially substituted with each other. Also, different embodiments and modified examples may be partially combined. Furthermore, in the following description, the expression "orthogonal" includes angles near 90°.

[0012] [Configuration of Multilayer Ceramic Electronic Component] Fig. 1 is a schematic diagram of a multilayer ceramic electronic component 1 according to an embodiment of the present disclosure. The multilayer ceramic electronic component 1 has an element body 2 and external electrodes 3. The shape of the element body 2 is set as appropriate, but as an example, the element body 2 has a substantially rectangular parallelepiped shape. As an example, the external electrodes 3 are located on a pair of end faces of the element body 2 and may be formed to extend around to other faces adjacent to the end faces. The external electrode located on one end face is referred to as external electrode 3a, and the external electrode located on the other end face is referred to as external electrode 3b.

[0013] For convenience, the drawings may be illustrated with a Cartesian coordinate system consisting of a first direction, a second direction, and a third direction. In the multilayer ceramic electronic component 1 according to the present disclosure, any direction may be the first direction, the second direction, or the third direction. For convenience, however, the stacking direction of the internal electrode layers 212 and the dielectric layers 211 (described later) is defined as the first direction. Furthermore, a direction intersecting the first direction and substantially parallel to the short sides of the element body 2, which has a substantially rectangular parallelepiped shape, is defined as the second direction. Furthermore, a direction intersecting the second direction and substantially parallel to the long sides of the element body 2, which has a substantially rectangular parallelepiped shape, is defined as the third direction. For convenience, the first direction may be referred to as the up-down direction, the second direction as the left-right direction, and the third direction as the front-rear direction.

[0014] The element body 2 has a substantially rectangular parallelepiped shape and six faces. The faces located at the top and bottom of the element body 2 in the first direction are defined as main faces, the faces located at the left and right of the element body 2 in the second direction are defined as side faces, and the faces located at the front and back of the element body 2 in the third direction are defined as end faces. The definitions of main face, side face, and end face are similarly defined for the laminate section 21 described below that constitutes the element body 2. The definitions of main face, side face, and end face are similarly defined for the element body precursor 200 before firing described below. The definitions of main face, side face, and end face are similarly defined for the laminate 50 before firing described below. The definitions of main face, side face, and end face are similarly defined for the mother laminate 500 before firing described below.

[0015] The low-profile components required for multilayer ceramic electronic components are components whose height when mounted is low, and as shown in FIG. 1 , the dimension in a first direction, which is the height when mounted, is relatively smaller than the dimension in a second direction.

[0016] In this specification, the "main surface" does not necessarily have to be strictly flat. For example, the main surface may be slightly warped as a whole, or may have some unevenness in part. The same applies to "side surface" and "end surface."

[0017] The external electrodes 3 are formed from a conductor and function as terminals of the multilayer ceramic electronic component 1. Examples of conductors that can form the external electrodes 3 include metals such as nickel (Ni), copper (Cu), palladium (Pd), tin (Sn), zinc (Zn), platinum (Pt), silver (Ag), and gold (Au), as well as alloys of these metals.

[0018] The external electrode 3 may have a single-layer structure or a multi-layer structure. For example, a multi-layer external electrode 3 may have a two-layer structure consisting of a base film and a surface film, or a three-layer structure consisting of a base film, an intermediate film, and a surface film. The base film may be a baked film made of a metal or alloy thereof, primarily composed of, for example, Ni, Cu, Pd, Pt, Ag, or Au. The intermediate film may be a plated film made of a metal or alloy primarily composed of, for example, Pt, Pd, Au, Cu, or Ni. The surface film may be a plated film made of a metal or alloy primarily composed of, for example, Cu, Sn, Pd, Au, Zn, or the like.

[0019] 2A and 2B are schematic diagrams of the element body 2. The element body 2 has a laminated portion 21, a side margin portion 22, and a cover portion 23. FIG. 2A is a schematic diagram showing the laminated portion 21, the side margin portion 22, and the cover portion 23 as a single unit, while FIG. 2B is a schematic diagram showing the laminated portion 21, the side margin portion 22, and the cover portion 23 in a separated state. FIGS. 2A and 2B are both diagrams showing the element body 2 before and after firing. Although the element body 2 after firing has shrunk due to firing, it has substantially the same structure as the element body 2 before firing.

[0020] The multilayer section 21 includes a plurality of dielectric layers 211 and a plurality of internal electrode layers 212 stacked in a first direction. The plurality of dielectric layers 211 may include various ceramic dielectrics. Examples of ceramic dielectrics include barium titanate (BaTiO 3 ) and calcium zirconate (CaZrO 3 ) etc.

[0021] The multiple internal electrode layers 212 may contain various metals such as Ni, Pd, Ag, Cu, etc. The multiple stacked internal electrode layers 212 are alternately exposed from a pair of end faces of the laminate portion 21 and connected to the external electrodes 3. Of the multiple internal electrode layers 212, those connected to the external electrode 3a are referred to as internal electrode layers 212a, and those connected to the external electrode 3b are referred to as internal electrode layers 212b.

[0022] The side margins 22 are located on both side surfaces of the laminated portion 21 in the second direction. The side margins 22 may contain various ceramic dielectrics. For example, the main component of the side margins 22 may be the same as the main component of the dielectric layer 211 of the laminated portion 21. In this case, manufacturing efficiency is improved, and internal stress in the element body 2 is reduced, improving reliability.

[0023] The cover portion 23 is located on both main surfaces of the laminate portion 21 in the first direction. The cover portion 23 may contain various ceramic dielectrics. For example, the main component of the cover portion 23 may be the same as the main component of the dielectric layer 211 of the laminate portion 21. In this case, manufacturing efficiency is improved, and internal stress in the element body 2 is reduced, improving reliability.

[0024] With the above configuration, when a voltage is applied between the external electrodes 3 a and 3 b in the multilayer ceramic electronic component 1, the voltage is applied to the plurality of dielectric layers 211 between the internal electrode layers 212 a and 212 b, causing the multilayer ceramic electronic component 1 to store electric charge according to the voltage between the external electrodes 3 a and 3 b.

[0025] The configuration of the multilayer ceramic electronic component 1 is not limited to a specific configuration, and any known configuration can be appropriately adopted depending on the size, performance, etc. required for the multilayer ceramic electronic component 1. For example, the number of stacked internal electrode layers 212 in the multilayer section 21 can be appropriately determined.

[0026] [Method of Manufacturing Multilayer Ceramic Electronic Component] Fig. 3 is a flowchart showing a method of manufacturing the multilayer ceramic electronic component 1. Figs. 4A to 10C are views showing the manufacturing steps of the multilayer ceramic electronic component 1. The method of manufacturing the multilayer ceramic electronic component 1 will be described below with reference to Figs. 4A to 10C.

[0027] (First Step: Preparation of Base Laminate) In the first step, a base laminate 500 is prepared in which a plurality of ceramic sheets 400 and a plurality of conductor sheets 410 are alternately laminated.

[0028] To prepare the base laminate 500, first, the first ceramic sheet 401, the second ceramic sheet 402, the third ceramic sheet 403, the first conductive sheet 411, and the second conductive sheet 412 are prepared.

[0029] 4A to 4C show ceramic sheets 400 and a conductive sheet 410 disposed thereon. Fig. 4A shows a first ceramic sheet 401 and a first conductive sheet 411, Fig. 4B shows a second ceramic sheet 402 and a second conductive sheet 412, and Fig. 4C shows a third ceramic sheet 403.

[0030] The first ceramic sheet 401 and the second ceramic sheet 402 become the dielectric layer 211 of the laminated portion 21 after firing. The third ceramic sheet 403 becomes the cover portion 23 after firing. The first conductor sheet 411 and the second conductor sheet 412 become the internal electrode layer 212 after firing. The first ceramic sheet 401, the second ceramic sheet 402, and the third ceramic sheet 403 may be collectively referred to as ceramic sheets 400. The first conductor sheet 411 and the second conductor sheet 412 may be collectively referred to as conductor sheets 410.

[0031] The ceramic sheet 400 is placed on, for example, a carrier film. This placement is performed using, for example, a die coater, but is not limited to this. For example, it may be performed using a doctor blade coater or a gravure coater. The thickness of the ceramic sheet 400 can be set as appropriate. For example, the thickness of the ceramic sheet 400 may be approximately 1 to 10 μm. The thinner the ceramic sheet, the higher the capacitance of the multilayer ceramic electronic component 1 can be.

[0032] The ceramic sheet 400 may be made of various ceramic dielectric materials. As an example, the ceramic sheet 400 may be made of BaTiO 3 The ceramic powder mixture with additives added is wet-pulverized and mixed in a bead mill, and the pulverized and mixed slurry is then mixed with a polyvinyl butyral binder, a plasticizer, and an organic solvent to produce the ceramic powder mixture.

[0033] 4A and 4B, a first conductor sheet 411, which will become the internal electrode layer 212a after firing, is placed at an interval on the first ceramic sheet 401. Also, a second conductor sheet 412, which will become the internal electrode layer 212b after firing, is placed at an interval on the second ceramic sheet 402.

[0034] 4A and 4B show a conductive sheet 410 printed with two types of conductive patterns with different polarities. The conductive sheet 410 can be formed by, for example, screen printing or gravure printing. The conductive sheet 410 may be made from conductive paste containing various metals.

[0035] The third ceramic sheet 403 corresponding to the cover portion 23 after firing may not necessarily have the conductive sheet 410 formed thereon. However, the present invention is not limited to this example, and for example, the third ceramic sheet 403 may have the conductive sheet 410 disposed thereon, which will become a dummy internal electrode layer after firing.

[0036] The thickness of the conductive sheet 410 can be set as appropriate. As long as the characteristics of the capacitor are ensured, the thinner the conductive sheet 410, the more likely it is to prevent internal defects due to internal stress. For example, in a capacitor with a high number of layers, the thickness of the conductive sheet 410 may be 1 μm or less. Furthermore, the spacing between the first conductive sheet 411 and the second conductive sheet 412 does not necessarily have to be constant and can be set as appropriate. For example, the spacing between the first conductive sheet 411 and the second conductive sheet 412 may be different.

[0037] The first ceramic sheet 401 on which the first conductive sheet 411 is formed may be referred to as the first sheet, the second ceramic sheet 402 on which the second conductive sheet 412 is formed may be referred to as the second sheet, and the third ceramic sheet 403 may be referred to as the third sheet.

[0038] Next, the prepared first, second, and third sheets are stacked to produce a base laminate 500. FIG. 5 is a schematic perspective view of the base laminate 500. For ease of explanation, each ceramic sheet 400 is shown exploded in FIG. 5. However, in actuality, the base laminate 500 is formed by compressing and integrating the ceramic sheets 400 using hydrostatic pressure, uniaxial pressure, or the like. This results in a high-density base laminate 500.

[0039] In the base laminate 500, first sheets and second sheets corresponding to the laminated portion 21 after firing are alternately stacked in the first direction. In addition, in the base laminate 500, third sheets corresponding to the cover portion 23 after firing are stacked on the top and bottom surfaces in the first direction of the alternately stacked first and second sheets. The numbers of the first sheets, second sheets, and third sheets can each be changed as appropriate.

[0040] (Second Step: Cutting) In the second step, the base laminate 500 is cut so as to form an unfired laminate 50 having side and end faces from which the conductive sheets 410 are exposed.

[0041] 6A and 6B are perspective views of a base laminate 500 and an individual laminate 50. FIG. 6A shows the base laminate 500, which is cut along cutting lines CL1 and CL2 while attached to tape as a holding member. This results in the base laminate 500 being cut into individual laminates 50 as shown in FIG. 6B. The resulting multiple laminates 50 include a first laminate 51 and a second laminate 52, which will be described later.

[0042] The cut surfaces of the base laminate 500 formed by cutting along the cutting line CL1 become the side surfaces in the second direction of the laminate 50. The cut surfaces of the base laminate 500 formed by cutting along the laminate cutting line CL2 become the end surfaces in the third direction of the laminate 50. The conductive sheet 410 is exposed from the side surfaces and end surfaces of the laminate 50.

[0043] The configuration of the cutting blade used to cut the base laminate 500 in the second step may be changed as appropriate. For example, the cutting blade may be a push-cutting blade or a rotary blade. Furthermore, techniques that do not require a cutting blade may be used to cut the base laminate 500, such as laser cutting or water jet cutting.

[0044] (Third Step: Preparation of Laminate) In the third step, the first laminate 51 and the second laminate 52 cut in the second step are prepared. The first laminate 51 and the second laminate 52 are shown in FIG.

[0045] The first laminate 51 includes a plurality of first ceramic layers 511 and a plurality of first conductor layers 512 that are alternately stacked. The first ceramic layers 511 correspond to the ceramic sheets 400 in the base laminate 500. The first conductor layers 512 correspond to the conductor sheets 410 in the base laminate 500.

[0046] The first laminate 51 has a main surface, an end surface, and a side surface referred to as a first main surface, a pair of first end surfaces, and a pair of first side surfaces. In other words, the first laminate 51 has a pair of first main surfaces, a pair of first end surfaces, and a pair of first side surfaces. As shown in FIG. 7 , the distance L1M between the pair of first main surfaces of the first laminate 51 is smaller than the distance L1S between the pair of first side surfaces. In other words, L1M<L1S. Furthermore, the distance L1M between the pair of first main surfaces of the first laminate 51 may be smaller than the distance L1T between the pair of first end surfaces. In other words, L1M<L1T.

[0047] If the first main surface is not a plane and there are multiple L1Ms, the largest distance can be defined as L1M. Also, if there are multiple L1Ss and L1Ts, they can be defined in the same way as L1M.

[0048] The plurality of first conductor layers 512 are exposed from both sides of the pair of first side surfaces of the first laminate 51 formed by cutting in the second step. Furthermore, the plurality of stacked first conductor layers 512 are alternately exposed from both sides of the pair of first end surfaces of the first laminate 51 formed by cutting in the second step.

[0049] The second laminate 52 includes a plurality of alternately stacked second ceramic layers 521 and a plurality of second conductor layers 522. The second ceramic layers 521 correspond to the ceramic sheets 400 in the base laminate 500. The second conductor layers 522 correspond to the conductor sheets 410 in the base laminate 500.

[0050] The second laminate 52 has a main surface, an end surface, and a side surface referred to as the second main surface, a pair of second end surfaces, and a pair of second side surfaces. In other words, the second laminate 52 has a pair of second main surfaces, a pair of second end surfaces, and a pair of second side surfaces. As shown in FIG. 7 , the distance L2M between the pair of second main surfaces of the second laminate 52 is smaller than the distance L2S between the pair of second side surfaces. In other words, L2M<L2S. Furthermore, the distance L2M between the pair of second main surfaces of the second laminate 52 may be smaller than the distance L2T between the pair of second end surfaces. In other words, L2M<L2T.

[0051] If the second principal surface is not a plane and there are multiple L2Ms, the smallest distance can be represented by L2M. Also, if there are multiple L2Ss and L2Ts, they can be defined in the same way as L2M.

[0052] The plurality of second conductive layers 522 are exposed from both sides of the pair of second side surfaces of the second laminate 52 formed by cutting in the second step. Furthermore, the plurality of stacked second conductive layers 522 are alternately exposed from both sides of the pair of second end surfaces of the second laminate 52 formed by cutting in the second step.

[0053] (Step 4: Arrangement) In step 4, the first laminate 51 and the second laminate 52 are arranged so that one first side surface of the first laminate 51 and one second side surface of the second laminate 52 are open surfaces. In addition, at this time, the first laminate 51 and the second laminate 52 are arranged so that a direction D1 perpendicular to the first main surface of the first laminate 51 and a direction D2 perpendicular to the second main surface of the second laminate 52 intersect.

[0054] In this specification, the term "open surface" refers to a surface that is located opposite to the surface that contacts the placement surface of a component such as a storage component or a sheet component when the laminate 50 is placed on the placement surface of the component, and that does not contact the placement surface of the component.

[0055] For example, in the fourth step, the arrangement of the first laminate 51 and the second laminate 52 may be performed using the accommodation member 6 and the magnet 7. Figures 8A and 8B show the accommodation member 6 and the laminate 50 accommodated in the accommodation member 6 after the accommodation step.

[0056] The housing member 6 has a first recess 61 and a second recess 62. The first laminate 51 is housed in the first recess 61, and the second laminate 52 is housed in the second recess 62. The housing member 6 may have a plurality of first recesses 61, or a plurality of second recesses 62. Fig. 8A shows a state in which the first laminate 51 is housed in the first recess 61, and the second laminate 52 is housed in the second recess 62. Fig. 8B shows a state after the first laminate 51 and the second laminate 52 have been rolled by the magnet 7.

[0057] The shapes of the first recess 61 and the second recess 62 may be set as appropriate. For example, as shown in Figures 8A and 8B, the first recess 61 may be a rectangular parallelepiped having a first short side wall 611 and a first long side wall 612 that is longer than the first short side wall 611. The second recess 62 may be a rectangular parallelepiped having a second short side wall 621 and a second long side wall 622 that is longer than the second short side wall 621. In this case, the first short side wall 611 and the second short side wall 621 intersect, and the first long side wall 612 and the second long side wall 622 intersect.

[0058] 9A to 9D show the rolling process using the magnet 7, with the laminate 50 rolling in the order shown in FIGS. 9A to 9D. Note that FIGS. 9A to 9D are cross-sectional views taken along line VIV-VIV in FIG. 8A. As shown in FIGS. 9A to 9D, the first short wall 611 and the first long wall 612 of the first recess 61 are connected via the first bottom surface 610. The second short wall 621 and the second long wall 622 of the second recess 62 are connected via the second bottom surface 620.

[0059] The length of the first longitudinal wall 612 may be greater than L1S and less than L1T. In this case, the longitudinal direction of the first laminate 51 is accommodated along the first longitudinal wall 612 of the first recess 61. Similarly, the length of the second longitudinal wall 622 may be greater than L2S and less than L2T. In this case, the longitudinal direction of the second laminate 52 is accommodated along the second longitudinal wall 622 of the second recess 62.

[0060] However, when the laminate 50 is randomly placed in the first recess 61 and the second recess 62, it will be placed either with the first main surface of the first laminate 51 facing the first bottom surface 610 of the first recess 61, or with the first side surface of the first laminate 51 facing the first bottom surface 610.

[0061] Similarly, the second recess 62 can be in one of two states: the second laminate 52 is accommodated so that the second main surface faces the second bottom surface 620, or the second laminate 52 is accommodated so that the second side surface faces the second bottom surface 620.

[0062] Here, since the side surfaces of the stack 50 are often processed, it is necessary to align the orientation of all the stacks so that the side surfaces are open. In other words, the stacks need to be housed so that the first side surfaces face the first bottom surface 610, and the second side surfaces face the second bottom surface 620.

[0063] Next, a magnetic field is applied using magnets 7 to cause the stack 50 to roll. Two magnets 7 are arranged above and below the housing member 6 so that their opposite magnetic poles face each other. In the example shown in Figures 9B and 9C, the lower surface of the upper magnet 7 is the south pole, and the upper surface of the lower magnet 7 is the north pole. With the magnets 7 arranged in this manner, a magnetic field is generated in which magnetic flux lines point from the lower north pole to the upper south pole. By using two magnets 7, parallel magnetic flux lines can be generated over a wide area.

[0064] When such a magnetic field is applied, the first laminate 51 and the second laminate 52 rotate about their longitudinal axes so that the plane direction of the conductive layers is parallel to the magnetic flux lines. As a result, the first side surface of the first laminate 51 in the first recess 61 becomes an open surface due to the rotation, while the first laminate 51 that originally had an open first side surface remains as it is. Therefore, the first side surfaces of all the first laminates 51 can be aligned so that they are open.

[0065] Furthermore, the second laminate 52 rotates in the second recess 62 so that the second side surface becomes an open surface, while the second laminate 52 that originally had the second side surface as an open surface remains as is. Therefore, the second side surfaces of all the second laminates 52 can be aligned so that they are open surfaces. This allows the side surfaces of all the laminates 50, including the first laminate 51 and the second laminate 52, to be aligned so that they are open surfaces.

[0066] 8B , after rolling, the first laminate 51 contacts the first short-side wall 611 and the first long-side wall 612. In other words, after rolling, the first main surface of the first laminate 51 contacts the first long-side wall 612, and the first end surface of the first laminate 51 contacts the first short-side wall 611. After rolling, the second laminate 52 contacts the second short-side wall 621 and the second long-side wall 622. In other words, after rolling, the second main surface of the second laminate 52 contacts the second long-side wall 622, and the second end surface of the second laminate 52 contacts the second short-side wall 621. In this case, the first short wall 611 and the second short wall 621 intersect, and the first long wall 612 and the second long wall 622 intersect, so that the direction D1 perpendicular to the first main surface of the first laminate 51 after rolling and the direction D2 perpendicular to the second main surface of the second laminate 52 intersect.

[0067] Next, the lid member 63 is removed, and the adhesive sheet 8 is attached to the side of the laminate 50 that has become the open surface. When pressure is applied in the vertical direction to the laminate 50 when attaching the laminate 50 to the adhesive sheet 8, a force is applied that rotates the laminate so that it falls over. The first laminate 51 has a structure in which L1M<L1S, and is narrower in width than in height when viewed from the first edge surface. Therefore, the moment of inertia is smaller when the first main surface rotates in a direction inclined relative to the adhesive sheet 8, so the first laminate 51 tends to fall over uniformly in the direction D1. The second laminate 52, like the first laminate 51, also has a structure in which L2M<L2S, and is narrower in width than in height when viewed from the second edge surface. Therefore, the moment of inertia is smaller when the second main surface rotates in a direction inclined relative to the adhesive sheet 8, so the second laminate 52 tends to fall over uniformly in the direction D2.

[0068] Here, for example, if the direction D1 of the first laminate 51 and the direction D2 of the second laminate 52 housed in the housing member 6 are aligned in the same direction, there is a possibility that a problem will occur in which the first laminate 51 and the second laminate 52 are likely to tip over in the same direction when being attached to the adhesive sheet 8 as shown in Fig. 9D . If the functional member 404 is pressed against the side surface of the laminate 50 in the fifth step described below while the laminate 50 is in an upturned state, there will be portions on the side surface of the laminate 50 where the pressure applied to the functional member 404 is insufficient, and the functional member 404 will not be formed uniformly, which may result in a problem in the side margin portion 22 after firing.

[0069] On the other hand, in the fourth step of the present disclosure, the first stack 51 and the second stack 52 are arranged so that the direction D1 of the first stack 51 after rolling and the direction D2 of the second stack 52 after rolling intersect. In this case, the direction D1 in which the first stack 51 is likely to tip over does not coincide with the direction D2 in which the second stack 52 is likely to tip over. Therefore, tipping of the first stack 51 can be reduced. Furthermore, the direction D2 in which the second stack 52 is likely to tip over does not coincide with the direction D1 in which the first stack 51 is likely to tip over. Therefore, tipping of the second stack 52 can be reduced.

[0070] In this way, when the direction in which the first laminate 51 is likely to tip over and the direction in which the second laminate 52 is likely to tip over intersect, the presence of each other can reduce the tipping of the first laminate 51 and the second laminate 52. Therefore, in the fifth step described below, the entire side surface of the laminate 50 can be sufficiently pressed against the functional member 404, and the functional member 404 can be uniformly formed on the side surface of the laminate 50, thereby reducing the possibility of defects occurring in the side margin portion 22 after firing.

[0071] 8A, 8B, and 9A to 9D, after the stack 50 is accommodated in the accommodation member 6, the lid member 63 is placed on the accommodation member 6. This allows the first stack 51 to be reliably held in the first recess 61, and the second stack 52 to be reliably held in the second recess 62.

[0072] The first short side wall 611 and the second short side wall 621 may be perpendicular to each other, and the first long side wall 612 and the second long side wall 622 may be perpendicular to each other. In other words, the first long side wall 612 and the second short side wall 621 may be parallel to each other, and the first short side wall 611 and the second long side wall 622 may be parallel to each other. This makes the direction D1 of the first stack 51 after rolling and the direction D2 of the second stack 52 after rolling perpendicular to each other, thereby further reducing the occurrence of tipping over.

[0073] 8A , 8B , and 9A to 9D show an example in which the first stack 51 after rolling contacts both the first short-side wall 611 and the first long-side wall 612, and the second stack 52 after rolling contacts both the second short-side wall 621 and the second long-side wall 622. However, this is not limiting. For example, the first stack 51 after rolling may not contact the first short-side wall 611 and the first long-side wall 612. The second stack 52 may not contact the second short-side wall 621 and the second long-side wall 622. Even in this case, if the direction D1 of the first stack 51 after rolling and the direction D2 of the second stack 52 after rolling intersect, the occurrence of tipping over can be reduced.

[0074] Furthermore, after rolling, the first laminate 51 may be in contact with either the first short wall 611 or the first long wall 612, and the second laminate 52 after rolling may be in contact with either the second short wall 621 or the second long wall 622.

[0075] Specifically, for example, the first end surface of the first laminate 51 after rolling may contact only the first short-side wall 611, and the second main surface of the second laminate 52 after rolling may contact only the second long-side wall 622. In this case, if the first short-side wall 611 and the second long-side wall 622 are parallel, the laminates can be arranged so that the direction D1 of the first laminate 51 after rolling and the direction D2 of the second laminate 52 after rolling intersect with each other. Therefore, compared to a case in which the first laminate 51 does not contact the first short-side wall 611 and the first long-side wall 612 and the second laminate 52 does not contact the second short-side wall 621 and the second long-side wall 622 after rolling, tipping over of each other can be more effectively reduced.

[0076] Furthermore, for example, the first main surface of the first laminate 51 after rolling may contact only the first long wall 612, and the second end surface of the second laminate 52 after rolling may contact only the second short wall 621. In this case, if the first long wall 612 and the second short wall 621 are parallel, the laminates can be arranged so that the direction D1 of the first laminate 51 after rolling and the direction D2 of the second laminate 52 after rolling intersect with each other. Therefore, compared to a case in which the first laminate 51 does not contact the first short wall 611 and the first long wall 612 after rolling and the second laminate 52 does not contact the second short wall 621 and the second long wall 622 after rolling, tipping over of each other can be more effectively reduced.

[0077] Furthermore, as in the examples shown in Figures 8A, 8B and 9A to 9D, the first laminate 51 after rolling may be in contact with both the first short wall 611 and the first long wall 612, and the second laminate 52 after rolling may be in contact with both the second short wall 621 and the second long wall 622.

[0078] Specifically, for example, the first end face of the first laminate 51 after rolling may be in contact with the first short side wall 611, the first main face may be in contact with the first long side wall 612, and the second main face of the second laminate 52 after rolling may be in contact with the second long side wall 622, and the second end face may be in contact with the second short side wall 621. In this case, if the first short side wall 611 and the second long side wall 622 are parallel and the first short side wall 611 and the second long side wall 622 are parallel, the direction D1 of the first laminate 51 after rolling and the direction D2 of the second laminate 52 after rolling can be more reliably arranged to be perpendicular or nearly perpendicular. Therefore, the occurrence of tipping over of each other can be more effectively reduced compared to when the first stack 51 after rolling contacts either the first short wall 611 or the first long wall 612, and the second stack 52 after rolling contacts either the second short wall 621 or the second long wall 622.

[0079] The fourth step may further include a tilting step of tilting the accommodating member 6. By tilting the accommodating member 6, the first stack 51 after rolling can be brought into contact with the first short-side wall 611, the first long-side wall 612, or both. Furthermore, by tilting the accommodating member 6, the second stack 52 after rolling can be brought into contact with the second short-side wall 621, the second long-side wall 622, or both. For example, when the accommodating member 6 is tilted in a direction in which the first end face of the first stack 51 after rolling contacts the first short-side wall 611, the second main surface of the second stack 52 after rolling will simultaneously contact the second long-side wall 622. Furthermore, when the accommodating member 6 is tilted in a direction in which the first main surface of the first stack 51 after rolling contacts the first long-side wall 612, the second end face of the second stack 52 after rolling will simultaneously contact the second short-side wall 621.

[0080] The tilting step may be performed simultaneously with or after the accommodation step of accommodating the stack 50 in the accommodation member 6. The tilting step may also be performed simultaneously with or after the rolling step of rolling the stack 50 by the magnet 7.

[0081] 9B and 9C show an example in which a magnetic field is generated by two magnets 7 arranged above and below the housing member 6, but this is not limiting. For example, one magnet 7 may be arranged either above or below the housing member 6. In this case, the orientation of the north and south poles of the magnet 7 may be set as appropriate. In other words, the direction of the magnetic flux lines from the north pole to the south pole in the next time may be set as appropriate.

[0082] (Fifth Step: Attaching Functional Member) In the fifth step, a functional member 404 is attached to the side of the laminate 50 placed on the adhesive sheet 8 in the fourth step. FIGS. 10A to 10C are diagrams that schematically show the process of the fifth step, and the process progresses in the order of FIGS. 10A to 10C. First, as shown in FIG. 10A, the functional member 404 is placed on a flat plate 420. The laminate 50 is placed with the open side facing the functional member 404. The flat plate 420 may be a rigid body such as metal or resin, or an elastic body such as rubber, and can be selected appropriately according to the properties of the functional member 404.

[0083] Examples of the functional member 404 include a protective ceramic green sheet, a protective ceramic paste, and a terminal electrode paste. For example, the functional member 404 may be made of various ceramic dielectric materials, similar to the ceramic sheet 400 prepared in the first step. In one example, the functional member 404 is made of the same material as the ceramic sheet 400. The functional member 404 is formed into a sheet using, for example, a roll coater or a doctor blade.

[0084] Next, as shown in FIG. 10B , the side surface of the laminate 50 is pressed against the functional member 404. This causes the functional member 404 to adhere to the side surface of the laminate 50. Thereafter, as shown in FIG. 10C , when the laminate 50 is lifted up from the functional member 404, only the functional member 404 attached to the side surface is separated from the elastic body and remains on the laminate 50 side. Alternatively, the flat plate 420 may be made of an elastic material so that the functional member 404 is punched out when the side surface of the laminate 50 is pressed against the functional member 404. This allows the functional member 404, which will become the side margin portion 22 after firing, to be provided on one side surface of the laminate 50. Note that the functional member 404 is also provided on the other side surface of the laminate 50 using the same or a similar process.

[0085] The above steps can produce an element body precursor 200 as shown in Fig. 11. After firing, the element body precursor 200 becomes the element body 2. The shape and size of the element body precursor 200 can be set appropriately depending on the shape and properties of the element body 2 after firing.

[0086] (Sixth Step: Firing) In the sixth step, the obtained unfired element precursor 200 is fired to produce the element 2 as shown in Fig. 2. The firing can be carried out, for example, in a reducing atmosphere or a low oxygen partial pressure atmosphere.

[0087] (Seventh Step: Formation of External Electrodes) In the seventh step, external electrodes 3 are formed on the end faces of the element body 2 obtained in the sixth step.

[0088] In the seventh step, first, an unsintered electrode material is applied to cover both end faces in the third direction of the element body 2. The unsintered electrode material applied to the element body 2 is baked, for example, in a reducing atmosphere or a low-oxygen partial pressure atmosphere, to form a base film on the element body 2. Then, an intermediate film and a surface film are formed on the base film baked on the element body 2 by a plating process such as electrolytic plating, to complete the external electrode 3.

[0089] Note that part of the treatment in Step 7 may be performed before Step 6. For example, before Step 6, unsintered electrode material may be applied to both end faces in the third direction of the unsintered element precursor 200, and in Step 6, the unsintered electrode material may be baked simultaneously with the firing of the element precursor 200 to form the base layer of the external electrode 3.

[0090] By carrying out the first to seventh steps as described above, the multilayer ceramic electronic component 1 shown in FIG. 1 can be obtained.

[0091] According to the above-described method for manufacturing a multilayer ceramic electronic component, it is possible to reduce the occurrence of defects in the formed side margin portions.

[0092] The present disclosure can be implemented in the following aspects (1) to (7).

[0093] (1) A method for manufacturing a multilayer ceramic electronic component, comprising: a preparation step of preparing a first laminate comprising a plurality of first conductor layers and a plurality of first ceramic layers stacked alternately, the first laminate having a pair of first main surfaces, a pair of first end surfaces, and a pair of first side surfaces, the distance between the pair of first main surfaces being smaller than the distance between the pair of first side surfaces, and the plurality of first conductor layers being exposed from the first side surfaces; and a second laminate comprising a plurality of second conductor layers and a plurality of second ceramic layers stacked alternately, the second laminate having a pair of second main surfaces, a pair of second end surfaces, and a pair of second side surfaces, the distance between the pair of second main surfaces being smaller than the distance between the pair of second side surfaces, and the plurality of second conductor layers being exposed from the second side surfaces; an arrangement step of arranging the first laminate and the second laminate so that the first side surfaces and the second side surfaces are open surfaces and so that a direction orthogonal to the first main surfaces intersects with a direction orthogonal to the second main surfaces; and an attachment step of attaching functional members to the first side surfaces and the second side surfaces that are open surfaces.

[0094] (2) The method for producing a multilayer ceramic electronic component according to the above aspect (1), wherein in the arranging step, a direction perpendicular to the first main surface and a direction perpendicular to the second main surface are perpendicular to each other.

[0095] (3) The method for manufacturing a multilayer ceramic electronic component according to the above aspect (1) or (2), wherein the distance between the pair of first main surfaces in the first laminate is smaller than the distance between the pair of first end faces, and the distance between the pair of second main surfaces in the second laminate is smaller than the distance between the pair of second end faces.

[0096] (4) A method for manufacturing a multilayer ceramic electronic component according to any one of the above aspects (1) to (3), wherein the stacked first conductive layers are alternately exposed from both sides of the pair of first end faces of the first laminate in the preparation step, and the stacked second conductive layers are alternately exposed from both sides of the pair of second end faces of the second laminate.

[0097] (5) The method for manufacturing a multilayer ceramic electronic component according to any one of the above aspects (1) to (4), wherein in the arranging step, a housing member having a first recess and a second recess is prepared, the first laminate is housed in the first recess, the second laminate is housed in the second recess, and a magnetic field is applied to roll the first laminate and the second laminate.

[0098] (6) A method for manufacturing a multilayer ceramic electronic component according to the above aspect (5), wherein the first recess has a first short-side wall and a first long-side wall that is longer than the first short-side wall, the second recess has a second short-side wall and a second long-side wall that is longer than the second short-side wall, the first long-side wall and the second short-side wall are parallel, and in the arranging step, one of the pair of first main surfaces of the first laminate after rolling contacts the first long-side wall, and one of the pair of second end surfaces of the second laminate after rolling contacts the second short-side wall.

[0099] (7) A method for manufacturing a multilayer ceramic electronic component according to the above aspect (6), wherein the first short-side wall and the second long-side wall are parallel to each other, and in the arranging step, one of the pair of first end faces of the first laminate after rolling contacts the first short-side wall, and one of the pair of second main surfaces of the second laminate after rolling contacts the second long-side wall.

[0100] 1: Multilayer ceramic electronic component 2: Element body 21: Lamination portion 211: Dielectric layer 212: Internal electrode layer 22: Side margin portion 23: Cover portion 200: Element body precursor 3, 3a, 3b: External electrode 400: Ceramic sheet 404: Functional member 410: Conductive sheet 420: Flat plate 50: Laminate 51: First laminate 511: First ceramic layer 512: First conductive layer 52: Second laminate 521: Second ceramic layer 522: Second conductive layer 500: Base laminate 6: Housing member 61: First recess 611: First short-side wall 612: First long-side wall 62: Second recess 621: Second short-side wall 622: Second long-side wall 63: Lid member 7: Magnet 8: Adhesive sheet

Claims

1. A method for manufacturing a multilayer ceramic electronic component, comprising: a preparation step of preparing a first laminate comprising a plurality of first conductor layers and a plurality of first ceramic layers stacked alternately, the first laminate having a pair of first main surfaces, a pair of first end surfaces and a pair of first side surfaces, the distance between the pair of first main surfaces being smaller than the distance between the pair of first side surfaces, and the plurality of first conductor layers being exposed from the first side surfaces; and a second laminate comprising a plurality of second conductor layers and a plurality of second ceramic layers stacked alternately, the second laminate having a pair of second main surfaces, a pair of second end surfaces and a pair of second side surfaces, the distance between the pair of second main surfaces being smaller than the distance between the pair of second side surfaces, and the plurality of second conductor layers being exposed from the second side surfaces; an arrangement step of arranging the first laminate and the second laminate such that the first side surfaces and the second side surfaces are open surfaces and a direction perpendicular to the first main surface intersects with a direction perpendicular to the second main surface; and an attachment step of attaching a functional member to the first side surfaces and the second side surfaces that are open surfaces.

2. The method for producing a multilayer ceramic electronic component according to claim 1, wherein in said arranging step, a direction perpendicular to said first main surface and a direction perpendicular to said second main surface are perpendicular to each other.

3. A method for manufacturing a multilayer ceramic electronic component as described in claim 1 or 2, wherein the distance between a pair of the first main surfaces in the first laminate is smaller than the distance between a pair of the first end faces, and the distance between a pair of the second main surfaces in the second laminate is smaller than the distance between a pair of the second end faces.

4. A method for manufacturing a multilayer ceramic electronic component as described in any one of claims 1 to 3, wherein the plurality of stacked first conductive layers are alternately exposed from both sides of a pair of first end faces of the first laminate in the preparation step, and the plurality of stacked second conductive layers are alternately exposed from both sides of a pair of second end faces of the second laminate.

5. A method for manufacturing a multilayer ceramic electronic component as described in any one of claims 1 to 4, wherein in the arranging step, a container member having a first recess and a second recess is prepared, the first laminate is contained in the first recess, the second laminate is contained in the second recess, and a magnetic field is applied to roll the first laminate and the second laminate.

6. A method for manufacturing a multilayer ceramic electronic component as described in claim 5, wherein the first recess has a first short wall and a first long wall longer than the first short wall, the second recess has a second short wall and a second long wall longer than the second short wall, the first long wall and the second short wall are parallel, and during the arranging step, one of the pair of first main surfaces of the first laminate after rolling is in contact with the first long wall, and one of the pair of second end faces of the second laminate after rolling is in contact with the second short wall.

7. A method for manufacturing a multilayer ceramic electronic component as described in claim 6, wherein the first short wall and the second long wall are parallel, and during the arranging process, one of the pair of first end faces of the first laminate after rolling contacts the first short wall, and one of the pair of second main faces of the second laminate after rolling contacts the second long wall.

Citation Information

Patent Citations

  • Alignment method of orientation of chip component

    JP2003007574A

  • Alignment method of chip component and magnet

    JP2019175902A