Aqueous solution containing lithium and silicon, method for producing same, and method for producing active material for lithium secondary battery
The use of an aqueous solution with a specific lithium and silicon molar ratio to form a lithium orthosilicate coating on lithium ion battery active materials addresses interfacial resistance and capacity issues, improving battery performance by enhancing Li ion conductivity and uniformity.
Patent Information
- Application Number
- PCT/JP2024/017629
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-05-13
- Publication Date
- 2024-11-28
AI Technical Summary
Existing methods for producing lithium ion secondary battery active materials face issues such as high interfacial resistance and battery capacity deterioration due to the reaction between positive electrode active materials and solid electrolytes, and the use of organic solvents is prone to oxidative decomposition when in contact with transition metals, leading to performance degradation.
An aqueous solution containing lithium and silicon with a specific molar ratio and low absorbance is used to form a coating layer of lithium orthosilicate on the positive electrode active material, which improves Li ion conductivity and reduces interfacial resistance, using a method that involves mixing silicon and lithium compounds, adjusting the molar ratio, and heat-treating the solution to create a crystalline lithium orthosilicate coating.
The method enhances the performance of all-solid-state lithium ion secondary batteries by reducing interfacial resistance and maintaining battery capacity through the formation of a uniform, high-conductivity lithium orthosilicate coating on the positive electrode active material.
Smart Images

Figure JP2024017629_28112024_PF_FP_ABST
Abstract
Description
Aqueous solution containing lithium and silicon, method for producing same, and method for producing active material for lithium secondary battery
[0001] The present invention relates to an aqueous solution containing lithium and silicon for coating the surfaces of positive electrode active material particles of a lithium ion secondary battery with lithium orthosilicate as a solid electrolyte, a production method thereof, and a method for producing an active material for a lithium secondary battery having a coating layer containing lithium orthosilicate.
[0002] The positive electrode active material of lithium-ion secondary batteries has generally been composed of a composite oxide of lithium and a transition metal. Among them, lithium cobalt oxide (LiCoO), which is a composite oxide containing Co as a component, has been particularly popular. 2 ) is widely used. Recently, lithium nickel oxide (LiNiO 2 ), lithium manganese oxide (LiMn 2 O 4 ), or ternary (LiNi 1/3 Mn 1/3 Co 1/3 O 2 The use of these types of devices and their combinations is also increasing.
[0003] The electrolyte for lithium ion secondary batteries is LiPF 6 , LiBF 4 These electrolytes are primarily composed of lithium salts such as those listed above dissolved in a mixed solvent of a cyclic carbonate ester such as PC (propylene carbonate) or EC (ethylene carbonate) and a chain ester such as DMC (dimethyl carbonate), EMC (ethyl methyl carbonate), or DEC (diethyl carbonate). Such organic solvents are vulnerable to oxidative atmospheres and are prone to oxidative decomposition reactions, particularly when they come into contact with transition metals such as Co, Ni, or Mn on the positive electrode surface. This is likely due to the high potential of the positive electrode surface and the catalytic action of highly oxidized transition metals. Therefore, preventing contact between the electrolyte and the transition metals (e.g., one or more of Co, Ni, and Mn) that make up the positive electrode active material as much as possible is effective in maintaining the performance of the electrolyte.
[0004] Furthermore, as a method for fundamentally solving the problems of the organic solvent-based electrolyte, all-solid-state lithium-ion secondary batteries have been proposed, in which the electrolyte is replaced with a non-flammable solid electrolyte. Generally, the electrode reaction in a battery occurs at the interface between the electrode active material and the electrolyte. When a liquid electrolyte is used, the electrolyte penetrates the surface of the electrode active material present on the electrode, forming a reaction interface for charge transfer. In all-solid-state batteries, a solid electrolyte with ion conductivity serves as the electrolyte. However, since the solid electrolyte itself does not have the fluidity of a liquid, it is necessary to form a composite in advance by mixing the powder of the electrode active material with the solid electrolyte or by coating the powder of the electrode active material with the solid electrolyte before constructing the secondary battery.
[0005] However, in the case of all-solid-state lithium-ion secondary batteries, there has been a problem in that the resistance (hereinafter sometimes referred to as "interface resistance") that occurs when lithium ions move across the interface between the positive electrode active material and the solid electrolyte increases, and the performance of the all-solid-state lithium-ion secondary battery, such as battery capacity, is likely to decrease. The increase in the interface resistance is believed to be caused by the reaction between the positive electrode active material and the solid electrolyte, resulting in the formation of high-resistance sites on the surface of the positive electrode active material, and it is known that the interface resistance can be reduced by coating the surface of lithium cobalt oxide, which is the positive electrode active material, with lithium silicate.
[0006] For example, Non-Patent Document 1 discloses LiCoO deposited on a metal substrate. 2 Li was deposited on the positive electrode as a solid electrolyte using pulsed laser deposition. 4 SiO 4 (lithium orthosilicate) or Li 2 SiO 3 A thin-film lithium battery in which lithium metasilicate (lithium metasilicate) is vapor-deposited is disclosed. 4 SiO 4 The Li ion conductivity of 2 SiO 3As a technique for coating the surface of a positive electrode active material with lithium silicate as a solid electrolyte using a highly productive wet method, for example, Patent Document 1 discloses a positive electrode active material powder whose surface is coated with vitreous lithium silicate.
[0007] In Non-Patent Document 2, Li 4 SiO 4 The technology disclosed in Non-Patent Document 2 is a positive electrode active material powder coated with sodium metasilicate (Na 2 SiO 3 ) to the positive electrode active material powder. 2 After forming the coating, lithium acetate powder is reacted with the coating layer in the solid state to form Li 4 SiO 4 In Non-Patent Document 3, Li is formed on the surface of the positive electrode active material by a wet method. 4 SiO 4 Patent Document 2 discloses a technique for coating Li without using TEOS. 4 SiO 4 A technique is disclosed in which a precursor solution of lithium metasilicate is prepared by mixing an aqueous solution of lithium metasilicate with a lithium compound to form a reaction precursor, thereby obtaining lithium orthosilicate.
[0008] JP 2014-513392 A JP 2021-075406 A
[0009] Atsushi Nakagawa et al., 35th Solid State Ionics Conference Abstracts, p.82, 2009S. Yang et al., Front. Energy, 2017, 11(3) p.374-382Y. Xu et al., J. Materiomics, 2 (2016) p.265-272
[0010] The pulsed laser deposition method of Non-Patent Document 1 has limitations on the materials to be treated, lacks versatility, and has problems of poor productivity. 2 Si 5 O 11 (lithium polysilicate) or Li 2 SiO 3 and those lithium silicates are Li4 SiO 4 In Non-Patent Document 2, the Li ion conductivity is low compared to that of Li ions, and the output characteristics of the battery are reduced during operation. 4 SiO 4 There was a problem that high resistance portions were formed in areas where the formation of lithium was insufficient, resulting in a decrease in battery characteristics. In the technology disclosed in Non-Patent Document 3, an alcohol solution using lithium acetate and tetraethoxysilane (TEOS) as starting materials for the coating liquid is used, which increases the manufacturing cost. In addition, TEOS absorbs moisture from the atmosphere and is prone to hydrolysis, making it difficult to handle as a coating liquid, so a coating liquid that does not use TEOS has been desired. In the case of the technology disclosed in Patent Document 2, the molar ratio of lithium to silicon is Li 4 SiO 4 It was found that when the molar ratio of lithium to silicon (Li / Si) is 3.7 or more, fine particles are generated in the aqueous solution. When a coating is formed on the surface of an electrode active material using such an aqueous solution, the coating tends to be non-uniform, and Li 4 SiO 4 There was a problem that high resistance portions were formed in areas where the formation of the conductive layer was insufficient, resulting in a deterioration in battery characteristics.
[0011] In view of the above problems, the present invention provides a method for manufacturing a lithium ion secondary battery, comprising: forming a cathode active material particle on the surface thereof with a Li ion conductive material having good Li ion conductivity; 4 SiO 4 The present invention aims to provide an aqueous solution containing lithium and silicon and having low absorbance for coating (lithium orthosilicate), a method for producing the aqueous solution, and a method for producing a positive electrode active material for a lithium secondary battery having a coating layer containing lithium orthosilicate using the aqueous solution.
[0012] [1] To achieve the above object, the present invention provides an aqueous solution containing lithium and silicon, which contains 0.1% by mass to 3.0% by mass of lithium and 0.1% by mass to 3.0% by mass of silicon, has a lithium to silicon molar ratio Li / Si of 3.70 to 5.20, and has an absorbance of 0.10 or less at a wavelength of 660 nm. [2] The aqueous solution containing lithium and silicon according to the above item [1] is dried and then heat-treated at 750°C in an air atmosphere for 5 hours to obtain a fired powder, which is mainly composed of lithium orthosilicate (Li 4 SiO 4) crystals. [3] The aqueous solution containing lithium and silicon according to the above item [1] preferably has a lithium content of 0.5% by mass or more and 2.0% by mass or less. [4] The aqueous solution containing lithium and silicon according to the above item [1] preferably has a silicon content of 0.5% by mass or more and 2.0% by mass or less. [5] The aqueous solution containing lithium and silicon according to the above item [1] preferably has a lithium to silicon molar ratio Li / Si of 3.70 or more and 5.00 or less. [6] The aqueous solution containing lithium and silicon according to the above item [1] preferably has an absorbance of 0.07 or less at a wavelength of 660 nm. [7] The present invention also provides a method for producing an aqueous solution containing lithium and silicon according to item [1], comprising the steps of mixing an aqueous solution containing a silicon compound with an aqueous solution containing a lithium compound to obtain an aqueous solution having a lithium to silicon molar ratio Li / Si of 3.70 or more and 5.20 or less, and maintaining the aqueous solution containing lithium and silicon at 45° C. or more and 60° C. [8] The present invention further provides a method for producing an active material for a lithium secondary battery having a coating layer containing lithium orthosilicate, comprising the steps of: an aqueous solution coating step of coating a surface of a positive electrode active material for a lithium secondary battery with the aqueous solution containing lithium and silicon obtained by the production method according to item [7]; a coating layer forming step of drying the positive electrode active material for a lithium secondary battery coated with the aqueous solution containing lithium and silicon to form a coating layer containing lithium and silicon; and a heat treatment step of subjecting the positive electrode active material for a lithium secondary battery having the coating layer containing lithium and silicon to a heat treatment. [9] The present invention further provides a method for producing an active material for a lithium secondary battery having a coating layer containing lithium orthosilicate, the method comprising: an aqueous solution coating step of coating a surface of a positive electrode active material for a lithium secondary battery with the aqueous solution containing lithium and silicon described in the above item [1]; a coating layer forming step of drying the positive electrode active material for a lithium secondary battery coated with the aqueous solution containing lithium and silicon to form a coating layer containing lithium and silicon; and a heat treatment step of heat treating the positive electrode active material for a lithium secondary battery having the coating layer containing lithium and silicon.
[0013] When the aqueous solution containing lithium and silicon obtained by the manufacturing method of the present invention is used, even if the molar ratio of lithium to silicon in the aqueous solution is Li / Si 3.70 or more, Li is mainly deposited on the surface of the electrode active material. 4 SiO 4 Therefore, the present invention can contribute to improving the performance of all-solid-state lithium ion secondary batteries.
[0014] 1 shows an X-ray diffraction pattern of a powder obtained by drying and calcining the aqueous solution obtained in Example 5.
[0015] [Positive Electrode Active Material] Examples of the positive electrode active material to be coated with the aqueous solution containing lithium and silicon according to the present invention include the following. The positive electrode active material is made of a composite oxide of Li and a transition metal M, and is not limited to materials conventionally used in lithium ion secondary batteries, such as lithium cobalt oxide (Li 1+X CoO 2 , -0.1≦X≦0.3), Li 1+X NiO 2 , Li 1+X Mn 2 O 4 , Li 1+X Ni 1/2 Mn 1/2 O 2 , Li 1+X Ni 1/3 Co 1/3 Mn 1/3 O 2 (-0.1≦X≦0.3 in both cases), Li 1+X [Ni Y Li 1/3-2Y/3 Mn 2/3-Y/3 ]O 2 (0≦X≦1, 0<Y<1 / 2), etc., and lithium transition metal oxides in which part of these Li or transition metal elements is replaced with Al or other elements, and Li 1+X FePO 4 , Li 1+X MnPO 4 (in all cases, -0.1≦X≦0.3) and lithium manganese oxide (LiMnO 4) and those in which a part of Mn is replaced with Al, Ti, Cr, Fe, Zr, Y, W, Ta, Nb, Ni, Co, Fe, etc. (LiAl 0.1 Mn 0.9 O 4 , LiNi 0.5 Mn 1.5 O 4 etc.)
[0016] [Li Source] In the aqueous solution containing lithium and silicon of the present invention, water-soluble lithium hydroxide (LiOH), lithium chloride (LiCl), lithium sulfate, lithium nitrate, etc. can be used as the Li source. It is preferable to use LiOH as the Li source, which is less likely to leave impurities when a coating layer containing lithium orthosilicate is finally formed on the surface of the positive electrode active material. LiOH may be anhydrous or hydrated. The LiOH added to the aqueous solution is Li + and OH - The solution dissociates into a LiOH solution and exhibits strong alkalinity. A strong alkalinity is preferred because it stabilizes the aqueous solution and suppresses the generation of fine particles in the aqueous solution. In this specification, an aqueous solution in which an additional Li source such as LiOH is dissolved is referred to as Solution A. In the present invention, an aqueous solution containing lithium and silicon is prepared by adding Solution A containing additional Li to Solution B described below. The lithium concentration in the aqueous solution after preparation is 0.1% by mass or more and 3.0% by mass or less in terms of Li. If the lithium concentration is 0.1% by mass or more, the concentration of the coating layer components in the aqueous solution increases, making it easier to achieve a uniform coating in the coating layer formation process. Furthermore, if the Li concentration is 3.0% by mass or less, the generation of a large amount of fine particles in the aqueous solution is suppressed, making it easier to achieve a uniform coating in the coating layer formation process. The lithium concentration is preferably 0.5% by mass or more and 2.0% by mass or less.
[0017] [Si Source] In the aqueous solution containing lithium and silicon of the present invention, the starting material of Si is not particularly limited as long as it is soluble in water, but it is preferable to use an aqueous solution containing lithium and silicon that also serves as a Li source. For example, Li 2 Si 5 O 11 Aqueous solution, Li 2 Si 14 O 29Aqueous solution, Li 2 Si 18 O 37 It is preferable to use an aqueous solution of lithium polysilicate in which the molar ratio of lithium to silicon (Li / Si) in the aqueous solution is 0.1 or more. Although it is possible to solubilize Si on the acidic side by using fluoride ions or the like, this is not preferable because the coated positive electrode active material dissolves on the acidic side. In this specification, Li 2 Si 5 O 11 The aqueous solution in which the above-mentioned Li is dissolved is referred to as Solution B. In the present invention, the Li-containing Solution A is added to Solution B to prepare an aqueous solution containing lithium and silicon, and the silicon concentration in the aqueous solution after preparation is 0.1 mass% or more and 3.0 mass% or less in terms of Si. If the silicon concentration is 0.1 mass% or more, the concentration of the coating layer components in the aqueous solution increases, making it easier to achieve a uniform coating in the coating layer formation process. If the silicon concentration is 3.0 mass% or less, the generation of a large amount of fine particles in the aqueous solution is suppressed, making it easier to achieve a uniform coating in the coating layer formation process. The silicon concentration is preferably 0.5 mass% or more and 2.0 mass% or less.
[0018] In the aqueous solution containing lithium and silicon of the present invention, the molar ratio Li / Si of lithium to silicon in the aqueous solution is 3.70 or more and 5.20 or less. By setting the Li / Si value to 3.70 or more and 5.20 or less, Li with high Li ion conductivity can be obtained. 4 SiO 4 Furthermore, if the Li / Si molar ratio exceeds 5.20, fine particles are likely to be generated in an amount exceeding the soluble concentration. The value of the lithium to silicon molar ratio Li / Si is preferably 3.70 or more and 5.00 or less. The aqueous solution containing lithium and silicon may contain an organic solvent such as alcohol, as long as the effect is not impaired.
[0019] [Absorbance] The absorbance value at a wavelength of 660 nm of the aqueous solution containing lithium and silicon according to the present invention is preferably 0.1 or less. Here, the absorbance of the aqueous solution at a wavelength of 660 nm is an index indicating the intensity of scattered light caused by microparticles present in the aqueous solution, and a high absorbance at that wavelength indicates a high concentration of microparticles present in the aqueous solution. Furthermore, when an aqueous solution with a high concentration of microparticles is applied to an electrode active material, the microparticles adhere to the surface of the electrode active material, making the coating layer uneven and prone to unevenness in thickness. This unevenness in the coating layer thickness can result in thin sections with insufficient thickness or even uncoated areas, resulting in a reduced coverage rate. According to the inventors' studies, if the absorbance value of the aqueous solution at a wavelength of 660 nm is 0.10 or less, the amount of microparticles in the aqueous solution is sufficiently small, minimizing adverse effects on the uniformity of the coating layer thickness and coverage rate. The absorbance value is preferably 0.07 or less. The absorbance value was measured using an ultraviolet-visible spectrophotometer at a wavelength of 660 nm, with the aqueous solution temperature at 25°C. The lower limit of absorbance was 0.000. However, the detection limit of the ultraviolet-visible spectrophotometer used for the absorbance measurement was 0.001.
[0020] [Carbon Content] If the aqueous solution containing lithium and silicon of the present invention contains carbon, it may remain as an impurity when a coating layer containing lithium orthosilicate is finally formed on the surface of the positive electrode active material, potentially reducing battery performance. Therefore, it is preferable that the aqueous solution containing lithium and silicon of the present invention contains a low content of organic matter that does not volatilize even when fired. The carbon content in the aqueous solution can be reduced to 5 mg / L or less in terms of total organic carbon (TOC). Furthermore, by using reagents with 1000 ppm or less of inevitable impurities, excluding Li, Si, and water, as the Si source and Li source of the aqueous solution containing lithium and silicon of the present invention, the TOC can be reduced to 5 mg / L or less. The carbon content in the aqueous solution can be reduced to 3 mg / L or less, more preferably 2 mg / L or less.
[0021] [Production Method] In the method for producing an aqueous solution containing lithium and silicon according to the present invention, as described above, a mixed solution containing lithium and silicon is prepared by adding a solution A containing Li to a solution B containing Si. This mixed solution generates fine particles and becomes cloudy. 2 Si 5 O 11 When an aqueous solution of lithium polysilicate (LiSi) is used as Solution A and an aqueous solution of lithium hydroxide (LiOH) is used as Solution B, the mixed solution will essentially contain only lithium ions, silicate ions, and unavoidable impurities. Solution B may also be added to Solution A. Subsequently, the mixed solution is stirred using a known mechanical stirring means while maintaining the temperature of the aqueous solution at 45°C or higher and 60°C or lower, whereby the fine particles dissolve and an aqueous solution containing lithium and silicon is obtained.
[0022] By setting the holding temperature for dissolving the microparticles at 45° C. or higher and 60° C. or lower, the microparticles are dissolved, and the absorbance value of the resulting aqueous solution at a wavelength of 660 nm can be set to 0.10 or lower. It is preferable to hold the temperature of the aqueous solution at 45° C. or higher and 60° C. or lower while stirring the mixed solution using a known mechanical stirring means, because this prevents a local temperature drop due to the addition of Solution A and shortens the time required for dissolving the microparticles.
[0023] In the present invention, the retention time for dissolving the microparticles is not particularly specified, but from an economical viewpoint, it is preferably 3 hours or less. The retention time can also be, for example, 15 minutes or more. The time when the absorbance of the aqueous solution obtained in the above step becomes 0.10 or less is regarded as the time when the dissolution of the microparticles is completed.
[0024] In the method for producing an aqueous solution containing lithium and silicon according to the present invention, a step of filtering the resulting aqueous solution containing lithium and silicon using a known filtration method may be performed after the step of dissolving the fine particles. The mixed solution may be maintained at 45°C to 60°C by mixing aqueous solution A containing lithium and aqueous solution B containing silicon at a temperature below 45°C, and then heating the resulting solution to 45°C to 60°C. Alternatively, aqueous solution A containing lithium and aqueous solution B containing silicon may be mixed at a temperature of 45°C to 60°C, and the temperature may be adjusted to 45°C to 60°C. The lithium-to-silicon molar ratio (Li / Si) of the aqueous solution containing lithium and silicon obtained by dissolving the fine particles is set to 3.70 to 5.20. The silicon concentration in the aqueous solution after the adjustment is preferably 0.1% by mass to 3.0% by mass in terms of Si, and the lithium concentration is preferably 0.1% by mass to 3.0% by mass in terms of Li.
[0025] In the method for producing an aqueous solution containing lithium and silicon of the present invention, a step of filtering the obtained aqueous solution containing lithium and silicon using a known filtering means may be provided after the step of dissolving the fine particles.
[0026] The aqueous solution containing lithium and silicon of the present invention is dried and then heat-treated at 750°C in an air atmosphere for 5 hours to obtain a calcined powder, which is mainly composed of lithium orthosilicate (Li 4 SiO 4 ) crystals, that is, those having the crystals as the main phase. 4 SiO 4 The term "having a crystal of Li as the main phase" means that the X-ray diffraction pattern obtained by X-ray diffraction measurement of the sintered powder shows that Li 4 SiO 4 The diffraction peak intensity with the highest peak intensity among the diffraction peaks identified in the crystal is designated as I 0 and heterogeneous phase (Li 4 SiO 4 The diffraction peak intensity with the highest peak intensity among the diffraction peaks (peaks that could not be identified in the crystalline phase) was defined as I 1 When the diffraction peak intensity ratio I 1 / I 0 In I 1 / I0 < 1.0. If no other phase is detected, 1 = 0, and the above I 1 / I 0 <1.0. The presence of different phases is permitted within a range that does not impair the effects of the present invention, but it is preferable that the amount of different phases present is small. For example, I 1 / I 0 More preferably, I≦0.50. 1 / I 0 It is more preferable that the ratio is ≦0.15. As a method for drying the aqueous solution, for example, spray drying method can be used.
[0027] [Coating Treatment] The following is an embodiment of the coating treatment of the positive electrode active material for a lithium ion secondary battery using an aqueous solution containing lithium and silicon according to the present invention. The positive electrode active material to be coated has a specific surface area of 0.1 to 2 m. 2 / g can be used. Since the specific surface area of a positive electrode active material is inversely proportional to its particle size, the specific surface area of the positive electrode active material is appropriately selected depending on the application of the lithium ion secondary battery. The thickness of the coating layer coated on the positive electrode active material is preferably 3 to 20 nm, more preferably 5 to 15 nm. For the coating treatment, known methods such as a tumbling fluidized bed coating method or a high-velocity airflow collision shear method are used, and a positive electrode active material having a coating layer containing lithium orthosilicate can be obtained by contacting the positive electrode active material with the aqueous solution of the present invention, drying it, and then heat-treating it.
[0028] [Measurement of Lithium and Silicon Contents] 15 mL of pure water and 5 mL of hydrochloric acid were added to a 0.1 g portion of the solution sample, and then 2 mL of hydrogen peroxide solution was added to dissolve the lithium and silicon. The resulting solution was adjusted to a constant volume using a measuring flask and then diluted appropriately as necessary. The lithium and silicon concentrations in the diluted solution were measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES, CP-720 manufactured by Agilent Technologies, Inc.), and the lithium and silicon contents in the solution sample were calculated.
[0029] [Absorbance Measurement] Qualitative evaluation of the amount of insoluble fine particles in an aqueous solution was performed by measuring absorbance at a wavelength of 660 nm using an ultraviolet-visible spectrophotometer (Shimadzu Corporation, UV-1800). Absorbance measurements were performed at 25°C using a quartz cell (10 mm x 10 mm x 45 mm) and pure water (ion-exchanged water) as a reference sample. [X-ray Diffraction Measurement] Powder samples obtained by spray-drying the aqueous solution were heat-treated at 750°C and then subjected to X-ray diffraction measurement. The measurement conditions were as follows: tube: Cu, tube voltage: 40 kV, tube current: 30 mA, divergence slit: 1.0°, scattering slit: 1.0°, receiving slit: 0.3 mm, scan speed: 2.0° / min, step width: 0.02. Peak search was performed using Shimadzu Corporation's XRD-6100 software under the following conditions: Smoothing processing: Automatic Background processing: Automatic Ka1-a2 ratio: 50 Peak search: Automatic
[0030] [Carbon measurement] The carbon amount in the aqueous solution was measured by the TC-IC method. The TC-IC method is a method in which the total carbon amount (TC) and inorganic carbon amount (IC) in a sample are measured separately, and the total organic carbon amount (TOC) is calculated from the difference. A total organic carbon meter (TOC-LCHS, manufactured by Shimadzu Corporation) was used for the measurement. TC measurement: The sample was injected into a combustion tube (680°C) filled with an oxidation catalyst, and carbon dioxide (CO 2 ) is detected in the analysis section. IC measurement: The sample is acidified (pH 3 or less) and aerated to remove CO from carbonates, etc. 2 is released and detected in the analytical section.
[0031] [Example 1] LiOH·H 2 5.99 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 59.94 g of ion-exchanged water were added and stirred at room temperature for 10 minutes to dissolve the solution, which was designated as Solution A. 2 Si 5 O 1111.02 g of an aqueous solution (manufactured by Sigma-Aldrich Corporation, concentration 20% by mass) and 34.04 g of ion-exchanged water were added and maintained at 50°C with stirring, and this was designated as Solution B. Solution A was added to Solution B at a rate of 5 g / min while stirring and maintained at 50°C, and white fine particles were generated in the mixed solution after the addition. The mixed solution was then maintained at 50°C and stirring was continued for 120 minutes, whereupon the fine particles dissolved to obtain a transparent aqueous solution.
[0032] The amounts of lithium and silicon contained in the resulting aqueous solution were measured by ICP-AES, and the absorbance of the resulting aqueous solution at a wavelength of 660 nm was also measured. The lithium and silicon contents were approximately equal to the amounts charged as raw materials, and the Li / Si molar ratio was 4.70. The absorbance was 0.03, and the TOC was 1 mg / L.
[0033] The aqueous solution obtained in this example was spray-dried using a spray dryer (SD-1000 manufactured by Tokyo Rikakikai Co., Ltd.) to obtain a white dry powder. The spray-drying conditions were an inlet temperature of 180°C, an outlet temperature of 90°C, and a solution addition rate of 10 g / min. The dried powder was heat-treated in an air atmosphere at 750°C for 5 hours and then crushed in a mortar to obtain a 750°C-fired powder. X-ray diffraction measurement of the 750°C-fired powder revealed that Li 4 SiO 4 Diffraction peaks due to the crystals of lithium orthosilicate were observed. 4 SiO 4 Diffraction peak intensity I originating from (lithium orthosilicate) crystals 0 was the diffraction peak with the highest peak intensity in the obtained X-ray diffraction pattern. 4 SiO 4 The diffraction peak intensity I is the highest among the diffraction peaks (peaks that could not be identified in the crystalline phase of 1 = 0. Therefore, I 1 / I 0 <1.0, the obtained fired powder is lithium orthosilicate (Li 4 SiO 4Therefore, the aqueous solution containing lithium and silicon obtained in this example is a precursor of lithium orthosilicate, and by coating the aqueous solution on a positive electrode active material, drying, and heat-treating the coating at 750°C, a positive electrode active material for a lithium secondary battery having a coating layer containing lithium orthosilicate can be obtained.
[0034] The conditions for preparing the aqueous solution in this example are shown in Table 1, and the composition of the resulting aqueous solution and the results of X-ray diffraction measurement of the powder calcined at 750° C. are shown in Table 2.
[0035] [Examples 2 to 5] In Examples 2 and 3, the amount of LiOH·H used to obtain Solution A was 2 The amounts of O and ion-exchanged water and the amount of ion-exchanged water used to prepare Solution B were changed to obtain transparent aqueous solutions containing dissolved fine particles, with a different Li / Si molar ratio from that of Example 1. Table 1 shows the preparation conditions for the aqueous solutions in these examples, and Table 2 shows the compositions of the resulting aqueous solutions and the results of X-ray diffraction measurements of the powders calcined at 750°C. The results of X-ray diffraction measurements of the powders calcined at 750°C obtained from the aqueous solutions of Examples 2 and 3 all showed that Li 4 SiO 4 Diffraction peaks due to the crystals of lithium orthosilicate were observed. 4 SiO 4 Diffraction peak intensity I originating from (lithium orthosilicate) crystals 0 was the diffraction peak with the highest peak intensity in the obtained X-ray diffraction pattern. 4 SiO 4 The diffraction peak intensity with the highest peak intensity among the diffraction peaks of the crystal is I 0 The diffraction peak intensity with the highest peak intensity among the diffraction peaks of the different phases is I 1 When the diffraction peak intensity ratio I 1 / I 0 I 1 / I 0 <1.0, the obtained fired powder is lithium orthosilicate (Li 4 SiO 4 ) crystals as the main phase. In Example 2, a different phase was detected, and the diffraction peak intensity ratio I 1 / I 0= 0.09. In Example 3, no heterophase was detected.
[0036] In Examples 4 and 5, the LiOH·H 2 The amounts of O and ion-exchanged water and the amount of ion-exchanged water used to obtain Solution B were changed, the Li / Si molar ratio was changed from that of Example 1, and the holding temperature in the microparticle dissolving step was changed to obtain transparent aqueous solutions containing dissolved microparticles according to Examples 4 and 5. The preparation conditions for the aqueous solutions of these Examples are shown in Table 1, and the compositions of the obtained aqueous solutions and the results of X-ray diffraction measurements of the powders calcined at 750°C are shown in Table 2. The results of X-ray diffraction measurements of the powders calcined at 750°C obtained from the aqueous solutions according to Examples 4 and 5 all showed that Li 4 SiO 4 Diffraction peaks due to the crystals of lithium orthosilicate were observed. Figure 1 shows the X-ray diffraction pattern obtained by X-ray diffraction measurement of the powder obtained by drying and calcining the aqueous solution obtained in Example 5 using the method described above. 4 SiO 4 Peaks due to lithium orthosilicate are observed. 4 SiO 4 Diffraction peak intensity I originating from (lithium orthosilicate) crystals 0 was the diffraction peak with the highest peak intensity in the obtained X-ray diffraction pattern. 4 SiO 4 The diffraction peak intensity with the highest peak intensity among the diffraction peaks of the crystal is I 0 The diffraction peak intensity with the highest peak intensity among the diffraction peaks of the different phases is I 1 When the diffraction peak intensity ratio I 1 / I 0 I 1 / I 0 <1.0, the obtained fired powder is lithium orthosilicate (Li 4 SiO 4 ) crystals as the main phase. In Example 4, a different phase was detected, and the diffraction peak intensity ratio I 1 / I 0 In Example 5, a different phase was detected, and the diffraction peak intensity ratio I 1 / I 0=0.09.
[0037] [Comparative Example 1] LiOH·H 2 8.76 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 87.59 g of ion-exchanged water were added and stirred at room temperature for 10 minutes to dissolve the mixture, which was designated as Solution A. 2 Si 5 O 11 11.02 g of an aqueous solution (Sigma-Aldrich Corporation, concentration 20% by mass) and 3.63 g of ion-exchanged water were added and kept at 50°C while stirring, and this was designated as Solution B. Solution A was added to Solution B while stirring and kept at 50°C at a rate of 5 g / min, and white fine particles were generated in the mixed solution after the addition. In this case, the Li / Si molar ratio was 5.98. The mixed solution containing the fine particles was then kept at 50°C and stirring was continued for 120 minutes, but the fine particles did not dissolve and the absorbance was 1.00. In this case, it is believed that the amount of fine particles generated exceeded the soluble concentration, and the fine particles did not completely dissolve. Because the fine particles did not dissolve, a powder calcined at 750°C was not prepared.
[0038] [Comparative Examples 2 and 3] The LiOH·H 2 The amounts of O and ion-exchanged water and the amount of ion-exchanged water used to obtain solution B were changed to change the Li / Si molar ratio, and the holding temperature in the microparticle dissolution step was also changed to obtain aqueous solutions of Comparative Examples 2 and 3. In these cases, the Li / Si ratio was within the range of the present invention, but the generated microparticles did not dissolve. In this case, it is believed that the holding temperature was inappropriate, which is why the microparticles did not dissolve. Since the microparticles did not dissolve, no powder was produced that was fired at 750°C. The preparation conditions for the aqueous solutions of these comparative examples are shown in Table 1, and the compositions of the obtained aqueous solutions are shown in Table 2.
[0039] [Comparative Example 4] LiOH·H 245.40 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 272.43 g of ion-exchanged water were added and stirred at room temperature for 10 minutes to dissolve. This was designated as Solution A. A 500 mL beaker was filled with lithium silicate solution (manufactured by Nippon Chemical Industry Co., Ltd., lithium silicate 35, SiO 2 :20.9% by mass, LiO 2 95.95 g of Li-based ammonium hydroxide (Li content: 2.9% by mass, molar ratio: 3.55) was added and maintained at 40°C with stirring, resulting in Liquid B. Liquid A was added to Liquid B at a rate of 5 g / min while stirring and maintained at 40°C. White fine particles were generated in the mixed solution after addition. In this case, the Li content was 2.13% by mass, the Si content was 2.27% by mass, and the Li / Si molar ratio was 3.80. The mixed solution was then maintained at 40°C and stirring was continued for 70 minutes, but the fine particles did not dissolve. Since the fine particles did not dissolve, a powder calcined at 750°C was not prepared. The preparation conditions for the aqueous solution of Comparative Example 4 are shown in Table 1, and the composition of the resulting aqueous solution is shown in Table 2.
[0040] From the above results, it is clear that by using the production method of the present invention, an aqueous solution containing lithium and silicon can be obtained that can be used as a precursor for forming a coating layer containing lithium orthosilicate on the surface of a positive electrode active material for a lithium secondary battery.
[0041]
[0042]
Claims
1. An aqueous solution containing lithium and silicon, the aqueous solution containing 0.1% by mass or more and 3.0% by mass or less of lithium and 0.1% by mass or more and 3.0% by mass or less of silicon, the molar ratio of lithium to silicon Li / Si being 3.70 or more and 5.20 or less, and the absorbance at a wavelength of 660 nm being 0.10 or less.
2. The aqueous solution was dried and then heat-treated at 750°C for 5 hours in an air atmosphere to obtain a calcined powder, which was mainly composed of lithium orthosilicate (Li 4 SiO 4 2. The aqueous solution containing lithium and silicon according to claim 1, wherein the aqueous solution is composed of crystals of the formula (I).
3. The aqueous solution containing lithium and silicon according to claim 1, wherein the lithium content in the aqueous solution is 0.5% by mass or more and 2.0% by mass or less.
4. The aqueous solution containing lithium and silicon according to claim 1, wherein the silicon content in the aqueous solution is 0.5% by mass or more and 2.0% by mass or less.
5. The aqueous solution containing lithium and silicon according to claim 1, wherein the molar ratio Li / Si of lithium to silicon in said aqueous solution is 3.70 or more and 5.00 or less.
6. The aqueous solution containing lithium and silicon according to claim 1, wherein the aqueous solution has an absorbance of 0.07 or less at a wavelength of 660 nm.
7. A method for producing an aqueous solution containing lithium and silicon according to claim 1, comprising the steps of: mixing an aqueous solution containing a silicon compound with an aqueous solution containing a lithium compound to obtain an aqueous solution having a lithium to silicon molar ratio Li / Si of 3.70 or more and 5.20 or less; and maintaining the aqueous solution containing lithium and silicon at 45°C or more and 60°C or less.
8. A method for producing an active material for a lithium secondary battery having a coating layer containing lithium orthosilicate, comprising: an aqueous solution coating step of coating a surface of a positive electrode active material for a lithium secondary battery with an aqueous solution containing lithium and silicon obtained according to claim 7; a coating layer forming step of drying the positive electrode active material for a lithium secondary battery coated with the aqueous solution containing lithium and silicon to form a coating layer containing lithium and silicon; and a heat treatment step of subjecting the positive electrode active material for a lithium secondary battery having a coating layer containing lithium and silicon to a heat treatment.
9. A method for producing an active material for a lithium secondary battery having a coating layer containing lithium orthosilicate, comprising: an aqueous solution coating step of coating a surface of a positive electrode active material for a lithium secondary battery with the aqueous solution containing lithium and silicon as defined in claim 1; a coating layer forming step of drying the positive electrode active material for a lithium secondary battery coated with the aqueous solution containing lithium and silicon to form a coating layer containing lithium and silicon; and a heat treatment step of subjecting the positive electrode active material for a lithium secondary battery having the coating layer containing lithium and silicon to a heat treatment.
Citation Information
Patent Citations
Positive electrode active material for lithium secondary batteries and manufacturing method thereof, and lithium secondary battery arranged by use of such positive electrode active material
JP2014082219A
Positive electrode active material composite for lithium ion secondary battery and method for manufacturing the same
JP2018147554A
CO2 ABSORBING MATERIAL AND PRODUCTION METHOD THEREOF
JP2018528851A
Lithium-containing oxide precursor solution for electrode active material coating and manufacturing method for the same
JP2023021925A