Biaxially oriented polypropylene film and laminate
The biaxially oriented polypropylene film with a base layer of polypropylene resin and recycled raw materials addresses the challenge of using recycled materials by maintaining film performance and sustainability, achieving high rigidity and heat resistance through specific material properties.
Patent Information
- Application Number
- PCT/JP2024/017820
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-30
- Filing Date
- 2024-05-14
- Publication Date
- 2024-11-28
AI Technical Summary
Conventional biaxially oriented polypropylene films with high rigidity and heat resistance are not suitable for use with recycled raw materials due to performance deterioration caused by foreign materials, making it difficult to achieve both environmental sustainability and film performance.
A biaxially oriented polypropylene film with a base layer containing a mixture of polypropylene resin and recycled raw materials, where the recycled raw materials have specific properties such as a melt flow rate of 3.0 to 11.0 g/10 min, a melting peak temperature of 145 to 170°C, and an enthalpy of fusion of 87.0 J/g or more, ensuring excellent film formability and performance without impairing rigidity or heat resistance.
The film achieves excellent rigidity, heat resistance, and dimensional stability, enabling the effective use of recycled materials while reducing environmental impact, thus promoting sustainable film production.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Biaxially oriented polypropylene film and laminate
[0001] The present invention relates to a biaxially oriented polypropylene film and a laminate using this film.
[0002] Traditionally, oriented polypropylene films have been widely used in various applications, including packaging materials, taking advantage of their excellent transparency, mechanical strength, moisture resistance, rigidity, etc. In recent years, in order to reduce the environmental impact, efforts have been made to reduce the amount of polypropylene used, such as by reducing the thickness.
[0003] For thin stretched polypropylene films, users demand that they maintain rigidity so as not to impair the feel of use, and therefore, the rigidity must be significantly improved compared to conventional stretched polypropylene films. Furthermore, since stretched polypropylene films are subjected to printing and lamination processes, they are required to have sufficient heat resistance and dimensional stability while also having improved rigidity. Therefore, biaxially stretched polypropylene films that have high heat resistance, rigidity, etc., imparted by adjusting the thermal shrinkage rate in the machine direction (MD) and transverse direction (TD) of the film and the impact strength (impact resistance) are known (see, for example, Patent Document 1).
[0004] Furthermore, with the promotion of the Sustainable Development Goals (SDGs), efforts to realize an environmentally friendly recycling-oriented society include, for example, the use of renewable energy to reduce emissions of greenhouse gases such as carbon dioxide, which is considered one of the causes of global warming. Therefore, in the field of resin films, films that use plant-derived raw materials (biomass raw materials) instead of petroleum-derived raw materials have been proposed (see, for example, Patent Document 2). Plant-derived raw materials are carbon-neutral resources, and therefore are effective as resources that can contribute to reducing environmental impact compared to petroleum-derived raw materials.
[0005] Another environmentally friendly initiative is the use of recycled materials. Recycled materials that are expected to be used as materials to make up films include recycled film, as well as post-industrial recycled materials, which reuse materials generated in the manufacturing process before products are released to the market, such as scrap and surplus products generated during film production, and post-consumer recycled materials, which collect and recycle used products in the market. Furthermore, mechanical recycling, a method of crushing, melting, and forming into pellets before reuse, is commonly used to mold these recycled materials.
[0006] Among these mechanically recycled materials, those used for oriented polypropylene mainly use polypropylene as the main raw material. Polypropylene may contain various types of resins, additives such as antistatic agents and antiblocking agents, and resins used in masterbatches of these additives, all of which are different from the main resin. These different materials contained in recycled materials are technically and economically difficult to remove. Therefore, recycled materials are reused with the different materials remaining.
[0007] In biaxially oriented polypropylene films with high rigidity and high heat resistance that use such recycled materials, film performance such as film rigidity (e.g., elastic modulus) and heat resistance tends to be reduced due to the influence of other materials contained in the recycled materials. For this reason, it has not been suitable to use this type of recycled material in the production of biaxially oriented polypropylene films with high rigidity and high heat resistance, and it has not been put to practical use.
[0008] However, due to social demands for environmental consideration, there is a demand for the use of recycled materials in order to contribute to reducing greenhouse gas emissions and efficiently utilizing petroleum resources. Furthermore, the use of recycled materials is economically rational and is becoming increasingly useful. Therefore, the inventors conducted extensive research and invented a film that has excellent formability and does not impair the film performance even when using recycled materials containing different materials.
[0009] JP 2014-055283 A JP 2021-133509 A
[0010] The present invention has been made in consideration of the above points, and aims to provide a biaxially oriented polypropylene film and laminate that have excellent film formability without impairing rigidity or heat resistance even when made from recycled raw materials.
[0011] That is, the first invention relates to a laminated film comprising a base layer and a surface layer laminated on one or both sides of the base layer, the base layer containing recycled raw materials derived from molded articles mainly made of polypropylene resin, the laminated film having an elastic modulus of 2.0 GPa or more in the machine direction (MD) and an elastic modulus of 4.0 GPa or more in the transverse direction (TD) as measured in accordance with JIS K 7127 (1999), and a dimensional change rate L in the machine direction (MD) at 140°C when the temperature is increased from 30°C to 150°C at a rate of 20°C / min and a load of 0.32 N is applied in the machine direction (MD) as measured by a thermomechanical measuring apparatus (TMA). 140 (%) and dimensional change rate L at 120°C 120 (%) and the difference (L 140 -L 120the base layer is made of a resin blend containing at least two different resins, the resin blend including: 55% by weight or more of a polypropylene resin (A) having a mesopentad fraction (mmmm) of 95% or more; and 5 to 25% by weight of the recycled material (B) having a melt flow rate (MFR) of 3.0 to 11.0 g / 10 min, a melting peak temperature of 145 to 170°C as measured by a differential scanning calorimeter (DSC) in accordance with JIS K 7122 (2012) and a melting enthalpy (ΔH) of 87.0 J / g or more.
[0012] A second invention relates to the first invention, wherein the recycled raw material (B) is a biaxially oriented polypropylene film having a crystallization temperature of 105°C or higher as measured with a differential scanning calorimeter (DSC) in accordance with JIS K 7122 (2012).
[0013] A third invention relates to the first or second invention, wherein the recycled raw material (B) is a biaxially oriented polypropylene film having a molecular weight distribution (Mw / Mn, Mz+1 / Mw) determined by gel permeation chromatography (GPC) measurement that satisfies the relationship Mw / Mn<Mz+1 / Mw and Mz+1 / Mw≧4.7.
[0014] A fourth invention relates to the biaxially oriented polypropylene film according to the first or second invention, wherein the base layer contains 10% by weight or less of a propylene-α-olefin random copolymer (C).
[0015] A fifth aspect of the present invention relates to the biaxially oriented polypropylene film according to the third aspect of the present invention, wherein the base layer contains 10% by weight or less of a propylene-α-olefin random copolymer (C).
[0016] A sixth aspect of the present invention relates to a laminate in which a sealant film is laminated on the biaxially oriented polypropylene film according to the first or second aspect of the present invention.
[0017] A seventh aspect of the present invention relates to a laminate in which a sealant film is laminated on the biaxially oriented polypropylene film according to the third aspect of the present invention.
[0018] An eighth aspect of the present invention relates to a laminate in which a sealant film is laminated on the biaxially oriented polypropylene film according to the fourth aspect of the present invention.
[0019] A ninth aspect of the present invention relates to a laminate in which a sealant film is laminated on the biaxially oriented polypropylene film according to the fifth aspect of the present invention.
[0020] A tenth invention relates to the laminate of the sixth invention, wherein the sealant film is an unstretched polypropylene film.
[0021] An eleventh invention relates to the laminate of the seventh invention, wherein the sealant film is an unstretched polypropylene film.
[0022] A twelfth invention relates to the laminate of the eighth invention, wherein the sealant film is an unstretched polypropylene film.
[0023] A thirteenth invention relates to the laminate of the ninth invention, wherein the sealant film is an unstretched polypropylene film.
[0024] According to the biaxially oriented polypropylene film of the first invention, among the laminated films comprising a base layer and a surface layer laminated on one or both sides of the base layer, wherein recycled raw materials derived from molded products mainly made of polypropylene resin are blended into the base layer, the laminated film has an elastic modulus in the machine direction (MD) of 2.0 GPa or more and an elastic modulus in the transverse direction (TD) of 4.0 GPa or more, as measured in accordance with JIS K 7127 (1999), and a dimensional change rate L in the machine direction (MD) at 140°C when the temperature is increased from 30°C to 150°C at a rate of 20°C / min and a load of 0.32 N is applied in the machine direction (MD), as measured by a thermomechanical analyzer (TMA). 140 (%) and dimensional change rate L at 120°C 120 (%) and the difference (L 140 -L 120) is 15 or less, and the thermal shrinkage rates in the machine direction (MD) and the transverse direction (TD) when heated at 150°C for 5 minutes are each 10% or less, and the base layer is made of a resin mixture containing at least two different resins, the resin mixture including 55% by weight or more of a polypropylene resin (A) having a mesopentad fraction (mmmm) of 95% or more, and 5 to 25% by weight of the recycled raw material (B) having a melt flow rate (MFR) of 3.0 to 11.0 g / 10 min, a melting peak temperature of 145 to 170°C as measured by a differential scanning calorimeter (DSC) in accordance with JIS K 7122 (2012) and a melting enthalpy (ΔH) of 87.0 J / g or more. Therefore, excellent film formability can be obtained without impairing film properties such as rigidity and heat resistance, regardless of the presence or absence of other materials in the recycled raw material.
[0025] According to the biaxially oriented polypropylene film of the second invention, in the first invention, the recycled raw material (B) has a crystallization temperature of 105°C or higher as measured with a differential scanning calorimeter (DSC) in accordance with JIS K 7122 (2012), and therefore the crystallization rate is increased and good rigidity can be obtained.
[0026] According to the biaxially oriented polypropylene film of the third invention, in the first or second invention, the recycled raw material (B) has a molecular weight distribution (Mw / Mn, Mz+1 / Mw) determined by gel permeation chromatography (GPC) measurement that satisfies the relationship Mw / Mn<Mz+1 / Mw and Mz+1 / Mw≧4.7, and therefore can maintain high rigidity.
[0027] According to the biaxially oriented polypropylene film of the fourth invention, in the first or second invention, the base layer contains 10% by weight or less of the propylene-α-olefin random copolymer (C), which widens the temperature range in which the film can be stretched, thereby reducing the reject rate due to uneven stretching and improving production efficiency.
[0028] According to the biaxially oriented polypropylene film of the fifth invention, since the base layer in the third invention contains 10% by weight or less of propylene-α-olefin random copolymer (C), the temperature range in which the film can be stretched can be widened, the reject rate due to stretching unevenness can be reduced, and production efficiency can be improved.
[0029] According to the laminate of the sixth invention, a sealant film is laminated to the biaxially oriented polypropylene film described in the first or second invention, so that film performance such as rigidity and heat resistance is not impaired even when recycled raw materials are blended, and the laminate can be suitably used as a film product such as a packaging film that aims to reduce the environmental load.
[0030] According to the laminate of the seventh invention, a sealant film is laminated to the biaxially oriented polypropylene film described in the third invention, so that even when recycled raw materials are blended, the film performance such as rigidity and heat resistance is not impaired, and the laminate can be suitably used as a film product such as a packaging film that aims to reduce the environmental load.
[0031] According to the laminate of the eighth invention, a sealant film is laminated to the biaxially oriented polypropylene film described in the fourth invention, so that even when recycled raw materials are blended, the film performance such as rigidity and heat resistance is not impaired, and the laminate can be suitably used as a film product such as a packaging film that aims to reduce the environmental load.
[0032] According to the laminate of the ninth invention, a sealant film is laminated to the biaxially oriented polypropylene film described in the fifth invention, so that even when recycled raw materials are blended, the film performance such as rigidity and heat resistance is not impaired, and the laminate can be suitably used as a film product such as a packaging film that aims to reduce the environmental load.
[0033] According to the laminate of the tenth invention, since the sealant film in the sixth invention is an unstretched polypropylene film, excellent recyclability and heat seal strength can be obtained.
[0034] According to the laminate of the eleventh invention, in the seventh invention, the sealant film is an unstretched polypropylene film, and therefore excellent recyclability and heat seal strength can be obtained.
[0035] According to the laminate of the twelfth invention, in the eighth invention, the sealant film is an unstretched polypropylene film, so that excellent recyclability and heat seal strength can be obtained.
[0036] According to the laminate of the thirteenth invention, in the ninth invention, the sealant film is an unstretched polypropylene film, so that excellent recyclability and heat seal strength can be obtained.
[0037] A biaxially oriented polypropylene film according to one embodiment of the present invention is a laminated film having a base layer and a surface layer laminated on one or both sides of the base layer. This biaxially oriented polypropylene film contains recycled materials in the base layer. The biaxially oriented polypropylene film of the present invention is produced by a known film production method such as the T-die method. This film is suitable for use as a packaging film for, for example, food, daily necessities, miscellaneous goods, cosmetics, medicines, and other products. The packaging film can also be appropriately made into a packaging bag.
[0038] The biaxially oriented polypropylene film has physical properties required for various applications such as packaging films, such as a modulus of elasticity in the machine direction (MD) of 2.0 GPa or more and a modulus of elasticity in the transverse direction (TD) of 4.0 GPa or more, and a dimensional change rate in the machine direction (MD) of 1.0 GPa or more. 140 )% and the dimensional change rate at 120 ° C (L 120 ) % difference (L 140 -L 120 ) is 15 or less, and the heat shrinkage rates in the machine direction (MD) and transverse direction (TD) are each 10% or less.
[0039] The elastic modulus is a value measured by a tensile property test method conforming to JIS K 7127 (1999). The elastic modulus is used as one of the indicators of film rigidity. A film with a higher elastic modulus value has higher rigidity and a stronger firmness. By having a biaxially oriented polypropylene film with a modulus of elasticity in the machine direction (MD) of 2.0 GPa or more and a modulus of elasticity in the transverse direction (TD) of 4.0 GPa or more, excellent processability for various applications such as packaging films can be obtained. If the modulus of elasticity in the machine direction (MD) or the transverse direction (TD) is too low, the film may have poor processability and be prone to deformation, which may result in reduced productivity.
[0040] The dimensional change rate indicates the rate at which a film deforms due to temperature rise and is used as an index of dimensional stability such as the film's elongation performance. In particular, this dimensional stability assumes a state in which the film expands or contracts due to tension applied to the film during secondary processing such as deposition of metal or inorganic oxide layers, printing, and lamination.
[0041] In the biaxially stretched polypropylene film of the present invention, the temperature was increased from 30°C to 150°C at a rate of 20°C / min, and a load of 0.32 N was applied in the machine direction (MD), and the dimensional change rate in the machine direction (MD) at 140°C was measured using a thermomechanical analyzer (TMA). 140 (%), the dimensional change rate at 120°C is L 120 (%), dimensional change rate L 140 and dimensional change rate L 120 The difference between (L 140 -L 120 ) is required to be 15 or less. A difference in dimensional change rate (dimensional stability) of 15 or less indicates that the rate of deformation due to temperature rise is small and the dimensional stability is excellent. If the difference in dimensional change rate is too large, the film is likely to deform due to temperature rise, resulting in poor dimensional stability. This may lead to reduced productivity, such as the occurrence of wrinkles during secondary processing such as printing, or a deterioration in appearance.
[0042] The heat shrinkage rate indicates the rate at which a film shrinks at a given temperature and is used as an index of dimensional stability, such as the shrinkage performance of the film. The biaxially oriented polypropylene film of the present invention is required to have a heat shrinkage rate of 10% or less in both the machine direction (MD) and the transverse direction (TD) when heated at 150°C for 5 minutes. A heat shrinkage rate of 10% or less indicates that the film is less likely to shrink at high temperatures and has excellent dimensional stability. If the heat shrinkage rate in either or both the machine direction (MD) and the transverse direction (TD) is too high, the film is more likely to shrink at high temperatures and has poor dimensional stability. This may result in wrinkles during the packaging process, poor appearance, and reduced productivity.
[0043] Furthermore, the biaxially oriented polypropylene film of the present invention preferably has the transparency required for applications such as packaging films. The transparency of the film is expressed by the haze value measured in accordance with JIS K 7136 (2000). The preferred haze value for the film is 5.0% or less. If the haze value is too high, the transparency generally required for packaging films and the like will be insufficient, which is undesirable.
[0044] The base layer is made of a resin mixture of at least two different resins containing 55% by weight or more of polypropylene resin (A) and 5 to 25% by weight of recycled material (B). In addition to the polypropylene resin (A) and recycled material (B), additives such as a propylene-α-olefin random copolymer (C) and a masterbatch containing an antistatic agent, an antiblocking agent, etc. are mixed into the base layer as needed.
[0045] The polypropylene resin (A) must have a mesopentad fraction (mmmm) of 95% or more. The mesopentad fraction (mmmm) is an index of stereoregularity obtained by high-temperature nuclear magnetic resonance (NMR) measurement. The mesopentad fraction (mmmm) is measured using an FT-NMR device (manufactured by JEOL RESONANCE, Inc., "JNM-ECA400"), 13C-NMR measurement was carried out. 0.6 mL of a mixture of deuterated orthodichlorobenzene: deuterated benzene = 8:2 (volume ratio) was added to 120 mg of sample, and the mixture was heated to 135°C to dissolve, and measurement was carried out at 135°C. The mesopentad fraction was calculated by the method described in "Zambelli et al., Macromolecules, Vol. 6, p. 925 (1973)", and peak assignment was based on the corrected version of the above literature described in "Macromolecules, Vol. 8, p. 687 (1975)". Observation nuclei: 13 C (100 MHz) Measurement mode: Single pulse proton broadband decoupling Pulse interval: 5 seconds Pulse width: 45° Shift reference: Solvent-derived signal = 132.39 ppm Number of accumulations: 11,000
[0046] The pentad fraction, which indicates the degree of stereoregularity, is 13 This shows the proportion of isotactic sequences in pentad units in polypropylene molecular chains measured using C-NMR. This pentad fraction is the fraction (mmmm) of propylene monomers at the center of a chain in which five consecutive propylene units are meso-bonded. Specifically, 13 The intensity fraction of the mmmm peak among all absorption peaks in the methyl carbon region of the C-NMR spectrum is taken as the isotactic pentad unit.
[0047] When the base layer is mainly composed of a polypropylene resin with a mesopentad fraction (mmmm) of 95% or more, the crystallinity is improved, resulting in a resin layer with excellent rigidity and heat resistance. If the blending ratio of this polypropylene resin is too low, the rigidity, heat resistance, etc. of the film may be reduced. Similarly, if the mesopentad fraction of the polypropylene film is less than 95%, the rigidity, heat resistance, etc. of the film may be reduced.
[0048] The recycled raw material (B) is a resin material derived from polypropylene resin molded products, such as film molded products, scraps and surplus products generated during film production, and other resin products, and is obtained by re-pelletizing and other recycling processes. This recycled raw material also includes resin molded products containing residual materials that are different from the resin used as the main raw material, additives such as antistatic agents and antiblocking agents, and resins used in masterbatches of these additives, which are difficult to remove from the main raw material. When recycled raw materials containing residual materials from such resin molded products are used as a constituent material for biaxially oriented polypropylene film, this usually causes a decrease in film performance, such as film rigidity (e.g., modulus of elasticity) and heat resistance. Furthermore, since the main raw material for the base layer of the biaxially oriented polypropylene film of the present invention is a highly crystalline polypropylene resin, the presence of a low-crystalline resin in the recycled raw material can also cause a decrease in film performance.
[0049] Therefore, in the biaxially oriented polypropylene film of the present invention, by focusing on the melt flow rate, peak melting temperature, and enthalpy of melting of the recycled raw materials to be blended, and by using recycled raw materials having melt flow rate, peak melting temperature, and enthalpy within specified conditions, it has been found that it is possible to obtain excellent film-forming properties without impairing film properties such as rigidity and heat resistance, regardless of the presence or absence of foreign materials that cause a decrease in film properties.
[0050] That is, the recycled raw material must have a melt flow rate (MFR) of 3.0 to 11.0 g / 10 min, a peak melting temperature of 145 to 170° C., and a melting enthalpy (ΔH) of 87.0 J / g or more. The preferable conditions of the melt flow rate (MFR), peak melting temperature, and melting enthalpy (ΔH) of the recycled raw material are all set taking into consideration the inclusion of different materials.
[0051] The melt flow rate (MFR) is used as an indicator of the fluidity of a resin. A higher MFR value indicates better fluidity. Using recycled raw materials with too low an MFR may result in poor film formability due to insufficient fluidity. Using recycled raw materials with too high an MFR may result in poor film formability due to excessive fluidity. By using recycled raw materials with an MFR of 3.0 to 11.0 g / 10 min, good film formability can be achieved even if the recycled raw materials contain other materials.
[0052] The melting peak temperature is a value measured using a differential scanning calorimeter (DSC) in accordance with JIS K 7122 (2012). The melting peak temperature is used as an index of the heat resistance of a resin. Using recycled raw materials with too low a melting peak temperature can result in insufficient heat resistance, resulting in a large thermal shrinkage rate and increased susceptibility to thermal deformation, potentially reducing the rigidity and dimensional stability of the film. Furthermore, since there are almost no examples of resin molded products usable as recycled raw materials having a melting peak temperature exceeding 170°C, a realistic upper limit of 170°C is considered appropriate. Therefore, by using recycled raw materials with a melting peak temperature of 145 to 170°C, good heat resistance can be achieved, even when the recycled raw materials contain other materials, and thermal deformation of the film can be suppressed, while deterioration of the film's rigidity and dimensional stability can be suppressed.
[0053] The fusion enthalpy (ΔH) is the energy required to melt a resin, measured using a differential scanning calorimeter (DSC) in accordance with JIS K 7122 (2012). The fusion enthalpy is used as an index of the heat resistance of a resin. If recycled raw materials with too low a fusion enthalpy are used, the heat resistance may be insufficient, making the film prone to thermal deformation and reducing the rigidity and dimensional stability of the film. From the viewpoint of thermal stability, the fusion enthalpy of recycled raw materials must be 87.0 J / g or more. This ensures good heat resistance even when the recycled raw materials contain different materials, suppressing thermal deformation of the film and preventing deterioration of the rigidity and dimensional stability of the film.
[0054] Furthermore, the recycled raw material preferably has a crystallization temperature of 105°C or higher. The crystallization temperature is a value measured using a differential scanning calorimeter (DSC) in accordance with JIS K 7122 (2012). The crystallization temperature affects the rigidity, heat resistance, formability, etc. of the biaxially oriented polypropylene film. If the crystallization temperature of the recycled raw material is too low, the heat resistance decreases and the film becomes more susceptible to thermal deformation, which may result in a decrease in the rigidity, dimensional stability, etc. of the film. If the crystallization temperature of the recycled raw material is 105°C or higher, the crystallization rate increases, good rigidity can be obtained, and deterioration of the dimensional stability of the film can be suppressed.
[0055] Furthermore, the recycled raw material preferably has a molecular weight distribution (Mw / Mn, Mz+1 / Mw) determined by gel permeation chromatography (GPC) measurement that satisfies the following relationship: Mw / Mn<Mz+1 / Mw and Mz+1 / Mw≧4.7. In the molecular weight distribution, Mw is the weight-average molecular weight, which is the average value obtained by multiplying the number of molecules by the molecular weight. Mn is the number-average molecular weight, which is the value obtained by simply averaging the molecular composition by number.
[0056] Mz+1 (Z+1 average molecular weight) is influenced by the portion with an even higher molecular weight than Mz, which is a value that is more susceptible to the presence of a higher molecular weight than Mw. Mz+1 is defined by the following formula (i), and Mz (Z average molecular weight) is defined by the following formula (ii): Mz+1 = Σ(Ni·Mi 4 ) / Σ(Ni·Mi 3 ) … (i) Mz=Σ(Ni・Mi 3 ) / Σ(Ni·Mi 2 ) … (ii)
[0057] Mw / Mn is an index representing the molecular weight distribution of each molecule. Furthermore, Mz+1 / Mw is an index representing the molecular weight distribution of high molecular weight components. In terms of molecular weight distribution, when Mw / Mn<Mz+1 / Mw, this means that the molecular weight distribution of high molecular weight components is broad, very high molecular weight components are present, and the component proportion is high. By using recycled raw materials with a high content of such high molecular weight components, high rigidity can be maintained in biaxially oriented polypropylene films. Furthermore, Mz+1 / Mw in this case is 4.7 or higher. If Mz+1 / Mw is too low, the component proportion of high molecular weight components may be insufficient, making it impossible to maintain high rigidity.
[0058] The propylene-α-olefin random copolymer (C) is a resin material that is blended as needed to broaden the temperature range in which the film can be stretched, thereby reducing the rate of defects due to stretching unevenness and improving production efficiency. Blending the propylene-α-olefin random copolymer into the base layer of the film makes it easier to adjust the dimensional change rate in the MD direction in TMA measurement. When blended, the proportion of the propylene-α-olefin random copolymer is preferably 10% by weight or less. If the amount of the propylene-α-olefin random copolymer is too high, the rigidity, heat resistance, etc. of the film may be reduced.
[0059] The propylene-α-olefin random copolymer blended in the base layer is a random copolymer of propylene and an appropriate α-olefin other than propylene. Examples of α-olefins include ethylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, and 1-octene. These copolymers may be used alone or in combination of two or more. Among propylene-α-olefin random copolymers, propylene-ethylene random copolymer, propylene-ethylene-1-butene random copolymer, and propylene-1-butene random copolymer are preferred, with propylene-ethylene-1-butene random copolymer being more preferred.
[0060] The surface layer is a resin layer laminated on one or both sides of the base layer. The surface layer is a layer on which secondary film processing such as vapor deposition, printing, and lamination is performed. From the viewpoint of recyclability, the resin material constituting the surface layer is preferably primarily made of polypropylene resin, which is the same resin material as the base layer. The polypropylene resin may be the same type of polypropylene resin as the base layer, or a different type of polypropylene resin. For example, when the surface layer is laminated on one side of the base layer, the film can have a one-type two-layer structure or a two-type two-layer structure. Furthermore, when the surface layer is laminated on both sides of the base layer, the film can have a one-type three-layer structure, a two-type three-layer structure, or a three-type three-layer structure. Furthermore, as a biaxially stretched film with three or more layers, an optional layer such as an intermediate layer may be laminated between the base layer and the surface layer as needed.
[0061] In the surface layer, from the viewpoint of ensuring the rigidity, heat resistance, dimensional stability, etc. of the film, it is preferable that the pentad fraction of the polypropylene resin used is 90% or more. Furthermore, when it is necessary to effectively bleed out antistatic properties or to impart heat sealing properties, it is also possible to use a low-crystalline resin within a range that does not impair the desired physical properties of the laminated film. Examples of low-crystalline resins include random copolymers of propylene and α-olefins (excluding propylene), such as propylene-ethylene random copolymers, propylene-ethylene-1-butene random copolymers, and propylene-1-butene random copolymers.
[0062] Additives may be added to biaxially oriented polypropylene films as needed. Examples of additives include antioxidants, UV absorbers, antistatic agents, lubricants, nucleating agents, adhesives, antifogging agents, flame retardants, antiblocking agents, and inorganic or organic fillers. Examples of antistatic agents include aliphatic amine compounds such as lauryl diethanolamine, myristyl diethanolamine, and oleyl diethanolamine, aliphatic amide compounds such as lauryl diethanolamide, myristyl diethanolamide, and oleyl diethanolamide, and polyhydric alcohols. The antistatic agent may be added by a known method. For example, a high-concentration masterbatch may be prepared separately and mixed in any step, or may be premixed with polyolefin powder or polyolefin pellets. The high-concentration masterbatch may be prepared by, for example, heat-kneading a polyolefin resin and an antistatic agent using a known mixer or extruder, such as a Banbury mixer, Henschel mixer, tumbler mixer, single-screw extruder, or multi-screw extruder.
[0063] The thickness of the biaxially stretched polypropylene film is appropriately set depending on the application, etc. For example, it is preferably 9 to 100 μm, more preferably 10 to 80 μm, even more preferably 12 to 60 μm, and particularly preferably 12 to 50 μm. In addition, in the biaxially stretched polypropylene film, the thickness of the surface layer is appropriately adjusted within a range that does not impair the desired physical properties of the film. For example, it is preferably 0.1 to 10 μm, more preferably 0.5 to 8 μm.
[0064] As described above, the biaxially oriented polypropylene film of the present invention is a laminated film that reduces environmental impact by incorporating recycled material (B) into the base layer. In particular, the recycled material to be incorporated satisfies the following conditions: a melt flow rate (MFR) of 3.0 to 11.0 g / 10 min, a peak melting temperature of 145 to 170°C, and a melting enthalpy (ΔH) of 87.0 J / g or greater, and is incorporated at a ratio of 5 to 25 wt%. Conventionally, when recycled materials are used as film constituents, film properties such as rigidity and heat resistance can be reduced due to the influence of other materials in the recycled material. However, by incorporating an appropriate amount of recycled material that meets all of the above conditions into the base layer, it is possible to achieve excellent film formability without compromising film properties such as rigidity and heat resistance, regardless of the presence or absence of other materials in the recycled material. Therefore, this technology can promote the reuse of recycled materials in the field of resin films, where the use of recycled materials has been difficult, and significantly contribute to reducing environmental impact.
[0065] In the biaxially oriented polypropylene film of the present invention, a laminate can be formed by laminating a sealant film on the surface layer or the base layer on the side not provided with a surface layer. As the sealant film, a single-layer or multi-layer resin film having heat sealability is preferably used.
[0066] Any suitable resin material having heat sealing properties can be used for the sealant film, but from the viewpoint of recyclability, it is preferable that the sealant film be primarily made of polypropylene resin, which is the same resin material as the base layer and surface layer. The polypropylene resin can be selected from general polypropylene-based resins. For example, it can be selected from at least one of propylene homopolymer, propylene-α-olefin random copolymer such as propylene-ethylene random copolymer or propylene-ethylene-butene random copolymer, or propylene-ethylene block copolymer.
[0067] The sealant film is preferably an unstretched polypropylene film using the above polypropylene resin. Unstretched films have reduced film orientation, resulting in high heat seal strength, making them suitable for sealant films. Note that "unstretched" refers to a state in which no intentional stretching has been applied, and includes cases in which unavoidable stretching has been applied during film production, etc.
[0068] The laminate obtained in this manner comprises a biaxially oriented polypropylene film containing recycled raw materials and a sealant layer, and can therefore be suitably used as a film product such as a packaging film that aims to reduce the environmental impact.
[0069] [Preparation of Biaxially Stretched Polypropylene Film] In preparing the biaxially oriented polypropylene films of Examples 1 to 24, the materials described below were mixed and melted in predetermined proportions (by weight), and co-extruded using a T-die method to obtain a three-layer structure consisting of a base layer and a first and second surface layers laminated on both sides of the base layer. The raw sheet was then stretched 5.0 times in the machine direction (MD) and then 8.0 times in the transverse direction (TD) to obtain a biaxially oriented polypropylene film consisting of the first surface layer, base layer, and second surface layer. The blending ratios of the resin materials used in each layer of Examples 1 to 24 are shown in Tables 1 to 4 below.
[0070] [Materials Used] The following resins were used as the resin material for each layer. For each material, the melt flow rate (MFR) was measured using a melt indexer (G-01, manufactured by Toyo Seiki Seisakusho Co., Ltd.) in accordance with JIS K 7210 (2014) at a test temperature of 230 ° C. The crystallization temperature (° C.), melting peak temperature (° C.), and melting enthalpy (J / g) of the recycled raw material were each measured using a differential scanning calorimeter (DSC214 Polymer, manufactured by NETZSCH). In this measurement, the sample was heated from 20°C to 200°C at a rate of 10°C / min under a nitrogen stream, held at 200°C for 3 minutes, and then cooled from 200°C to 20°C at a rate of 10°C / min (1st Run). The sample was then held at 20°C for 3 minutes, and then heated from 20°C to 200°C at a rate of 10°C / min (2nd Run). The exothermic peak temperature from the DSC curve obtained in the 1st Run was taken as the crystallization temperature (°C), and the melting peak temperature and melting enthalpy were determined from the DSC curve in the 2nd Run. When multiple melting peaks were present, the highest melting peak temperature was used, and the melting enthalpy was determined by setting a baseline connecting the DSC curve from 50°C to 180°C with a straight line.
[0071] The molecular weight and molecular weight distribution of each material were measured using a high-temperature GPC system ("HLC-8321GPC-HT" manufactured by Tosoh Corporation) under the following conditions: Column: TSKgel GMHHR-H(20)HT x 3 (7.8 mm ID x 300 mm x 3) Eluent: 1,2,4-trichlorobenzene (0.05% BHT added) Flow rate: 1.0 mL / min Detector: RI detector (polarity: -) Column temperature: 140°C Injection volume: 300 μL Molecular weight standard: Standard polystyrene
[0072] <Polypropylene Resin (A)> Resin A1: Propylene homopolymer (mesopentad fraction (mmmm) 96.1%, MFR 3.5 g / 10 min, peak melting temperature 166°C) Resin A2: Propylene homopolymer (mesopentad fraction (mmmm) 95.8%, MFR 4.6 g / 10 min, peak melting temperature 166°C) Resin A3: Propylene homopolymer (mesopentad fraction (mmmm) 91.0%, MFR 3.0 g / 10 min, peak melting temperature 163°C)
[0073] <Recycled Raw Materials (B)> Resin B1: Recycled raw material consisting of biaxially oriented polypropylene film (commercially available product, resin composition: 99.4% by weight of polypropylene resin, 0.6% by weight of polyethylene resin) (MFR 5.4 g / 10 min, melting peak temperature 162°C, melting enthalpy 100.2 J / g, crystallization temperature 112°C, Mw / Mn: 4.3, Mz+1 / Mw 5.0) Resin B2: Recycled raw material consisting of biaxially oriented polypropylene film (commercially available product, resin composition: 97.0% by weight of polypropylene resin, 3.0% by weight of polyethylene resin) (MFR 5.7 g / 10 min, melting peak temperature 161°C, melting enthalpy 100.5 J / g, crystallization temperature 114°C, Mw / Mn 4.3, Mz+1 / Mw 4.8) Resin B3: Recycled raw material consisting of unstretched polypropylene film (commercially available product, resin composition: 98.5% by weight of polypropylene resin, 1.5% by weight of polyethylene resin) (MFR 10.1 g / 10 min, melting peak temperature 150°C, melting enthalpy 87.6 J / g, crystallization temperature 117°C, Mw / Mn 4.6, Mz+1 / Mw 4.9) Resin B4: Recycled raw material consisting of polypropylene bottle (commercially available product, resin composition: mainly polypropylene resin (details unknown)) (MFR 10.1 g / 10 min, melting peak temperature 140°C, melting enthalpy 86.8 J / g, crystallization temperature 102°C, Mw / Mn 4.8, Mz+1 / Mw 4.6)
[0074] <Propylene / α-olefin random copolymer (C)> Resin C1: propylene / α-olefin random copolymer (MFR 6.0 g / 10 min, melting peak temperature 162° C.)
[0075] <Additives> A master batch of an antistatic agent (Resin D1: MFR 7.8 g / 10 min) was used as an additive. The concentration of the antistatic agent was adjusted to 9% based on Resin A3.
[0076] [Prototype Example 1] Prototype Example 1 is a film obtained by blending 100% by weight of Resin A3, which is a polypropylene resin, as a first surface layer, 80% by weight of Resin A1, which is a polypropylene resin, 10% by weight of Resin B1, which is a recycled raw material, and 10% by weight of Resin D1, which is an additive (master batch of antistatic agent), as a base layer, and 100% by weight of Resin A3, which is a polypropylene resin, as a second surface layer, and forming it into a film with a thickness of 20 μm.
[0077] [Prototype Example 2] Prototype Example 2 is a film obtained by film formation in the same manner as Prototype Example 1, except that the base layer contained 75 wt % of Resin A1 and 15 wt % of Resin B1.
[0078] [Prototype Example 3] Prototype Example 3 is a film obtained by film formation in the same manner as Prototype Example 1, except that the base layer contained 70 wt % of Resin A1 and 20 wt % of Resin B1.
[0079] [Prototype Example 4] Prototype Example 4 is a film obtained by film formation in the same manner as Prototype Example 1, except that the base layer contained 65 wt % of Resin A1 and 25 wt % of Resin B1.
[0080] [Prototype Example 5] Prototype Example 5 is a film obtained by film-forming in the same manner as Prototype Example 1, except that the recycled raw material of the base layer of Prototype Example 1 was changed from Resin B1 to Resin B2, and the base layer contained 85% by weight of Resin A1 and 5% by weight of Resin B2.
[0081] [Prototype Example 6] Prototype Example 6 is a film obtained by film production in the same manner as in Prototype Example 1, except that the recycled raw material for the substrate layer was changed from Resin B1 to Resin B2.
[0082] [Prototype Example 7] Prototype Example 7 is a film obtained by film production in the same manner as in Prototype Example 2, except that the recycled raw material for the substrate layer was changed from Resin B1 to Resin B2.
[0083] [Prototype Example 8] Prototype Example 8 is a film obtained by film production in the same manner as in Prototype Example 3, except that the recycled raw material for the substrate layer was changed from Resin B1 to Resin B2.
[0084] [Prototype Example 9] Prototype Example 9 is a film obtained by film production in the same manner as in Prototype Example 4, except that the recycled raw material for the substrate layer was changed from Resin B1 to Resin B2.
[0085] [Prototype Example 10] Prototype Example 10 is a film obtained by film formation in the same manner as Prototype Example 1, except that the polypropylene resin in the base layer of Prototype Example 1 was changed from Resin A1 to Resin A2, and 2 wt% of Resin C1, a propylene-α-olefin random copolymer, was blended into the base layer, making Resin A2 78 wt%.
[0086] [Prototype Example 11] Prototype Example 11 is a film obtained by producing the film in the same manner as Prototype Example 10, except that the film thickness was 18 μm.
[0087] [Prototype Example 12] Prototype Example 12 is a film obtained by film formation in the same manner as Prototype Example 10, except that the base layer contained 68 wt% of Resin A2 and 20 wt% of Resin B1, and the film thickness was 16 μm.
[0088] [Prototype Example 13] Prototype Example 13 is a film obtained by blending 15% by weight of Resin A3, which is a polypropylene resin, into the base layer of Prototype Example 10, making Resin A2 58% by weight, and Resin B1 15% by weight, with the rest remaining the same.
[0089] [Prototype Example 14] Prototype Example 14 is a film obtained by film-forming in the same manner as Prototype Example 10, except that the polypropylene resin of the base layer of Prototype Example 10 was changed from Resin A2 to Resin A1, and the recycled raw material was changed from Resin B1 to Resin B3, and the base layer contained 83 wt% Resin A1 and 5 wt% Resin B3.
[0090] [Prototype Example 15] Prototype Example 15 is a film obtained by film formation in the same manner as Prototype Example 14, except that the base layer contained 78 wt % of Resin A1 and 10 wt % of Resin B3.
[0091] [Prototype Example 16] Prototype Example 16 is a film obtained by film formation in the same manner as Prototype Example 14, except that the base layer contained 68 wt % of Resin A1 and 20 wt % of Resin B3.
[0092] [Prototype Example 17] Prototype Example 17 is a film obtained by forming the base layer using a blend of 87 wt% of Resin A1, 3 wt% of Resin C1, and 10 wt% of Resin D1 without incorporating recycled raw materials, but in the same manner as Prototype Example 1 except for the above.
[0093] [Prototype Example 18] Prototype Example 18 is a film obtained by film formation in the same manner as Prototype Example 1, except that the base layer contained 87 wt % of Resin A1 and 3 wt % of Resin B1.
[0094] [Prototype Example 19] Prototype Example 19 is a film obtained by film formation in the same manner as Prototype Example 5, except that the base layer contained 60 wt % of Resin A1 and 30 wt % of Resin B2.
[0095] [Prototype Example 20] Prototype Example 20 is a film obtained by film production in the same manner as Prototype Example 2, except that the recycled raw material for the substrate layer was changed from Resin B1 to Resin B4.
[0096] [Prototype Example 21] Prototype Example 21 is a film obtained by film production in the same manner as in Prototype Example 3, except that the recycled raw material for the substrate layer was changed from Resin B1 to Resin B4.
[0097] [Prototype Example 22] Prototype Example 22 is a film obtained by forming the same film as Prototype Example 1, except that no recycled raw materials were blended in the base layer and 90 wt % of Resin A3 was blended.
[0098] [Prototype Example 23] Prototype Example 23 is a film obtained by film production in the same manner as in Prototype Example 1, except that the propylene resin in the substrate layer was changed from Resin A1 to Resin A3.
[0099] [Prototype Example 24] Prototype Example 24 is a film obtained by film formation in the same manner as Prototype Example 14, except that the base layer contained 58 wt % of Resin A1 and 30 wt % of Resin B3.
[0100]
[0101]
[0102]
[0103]
[0104] The performance of the biaxially oriented polypropylene films of Examples 1 to 24 was evaluated for haze, heat shrinkage, tensile modulus, dimensional stability, and film formability. The results and evaluations of each test are shown in Tables 5 to 8 below, along with the physical properties of the recycled raw materials in each example.
[0105] [Haze] Haze (%) is an index of transparency, and was measured using a haze meter (NDH-8000, manufactured by Nippon Denshoku Industries Co., Ltd.) according to a test method in accordance with JIS K 7136 (2000). For the biaxially oriented polypropylene films of Prototype Examples 1 to 24, a haze value of 5.0% or less was determined to be good, as it is the transparency required for a packaging film.
[0106] [Heat Shrinkage] The heat shrinkage (%) was measured based on a heat shrinkage test in accordance with JIS Z 1712 (2009). In this test, test specimens (15 mm wide, 150 mm long) were cut from the films of each of the prototypes 1 to 24, and marks were placed at 100 mm intervals in the center of the specimen. The specimens were then heated at 150°C for 5 minutes, and the lengths between the marks in the machine direction (MD) and the transverse direction (TD) of the test specimens after heating were measured. The heat shrinkage (%) was calculated as the percentage change from the measured machine direction and transverse direction lengths after heating to the machine direction and transverse direction lengths before heating. A heat shrinkage (%) of 10% or less was considered to be a good product.
[0107] [Tensile Modulus] The tensile modulus (GPa) was measured using a tensile tester (RTF-1310, manufactured by Orientec Co., Ltd.) based on the test method for tensile properties of plastics in accordance with JIS K 7127 (1999). 15 mm x 200 mm test pieces were cut from the films obtained in Prototype Examples 1 to 24. Next, the tensile modulus of each film in the machine direction (MD) and the transverse direction (TD) was measured using a tensile tester (RTF-1310, manufactured by Orientec Co., Ltd.) based on the test method for tensile properties of plastics in accordance with JIS K 7127 (1999). The tensile modulus of each film in the machine direction (MD) and the transverse direction (TD) was measured at a chuck distance of 100 mm and a pulling speed of 200 mm / min. A product was judged to be good if the measurement results satisfied both the machine direction (MD) modulus of 2.0 GPa or more and the transverse direction modulus of 4.0 GPa or more.
[0108] [Dimensional Stability] Using a thermomechanical measuring device (manufactured by TA Instruments Japan, Ltd., Q400), the dimensional change rates (%) in the machine direction (MD) at 120°C and 140°C were calculated according to the procedure described below. 140 ) and the dimensional change rate at 120 ° C (L 120 ) and the difference (L 140 -L 120 ) was calculated as the dimensional stability. A dimensional stability of 15 or less was judged to be a non-defective product.
[0109] To measure the dimensional change rate, test specimens (width 4 mm, length 25 mm) were cut from the films of Prototype Examples 1 to 24 in the machine direction (MD). The machine direction of the test specimen was set as the tensile direction, and the specimen was set in the sample holder so that the distance between the chucks was approximately 8 mm, and fixed to the probe of the thermomechanical device. A load of 0.32 N was applied to the test specimen, and the length (L 0 While applying a load of 0.32 N in the longitudinal direction of the test piece, the temperature was raised from 30°C to 150°C at a temperature rising rate of 20°C / min, and the length (L) in the machine direction (MD) of the test piece at the time when it reached 120°C was measured. 1 ) and the length (L) of the test piece in the machine direction (MD) when it reached 140 ° C. 2 The length (L) of the test piece before and after heating was measured. 0 ), (L 1 ) (L2 ) into the following formulas (iii) and (iv), and the dimensional change rate (L 120 ) and dimensional change rate at 140 ° C (L 140 ) was calculated. 120 (%) = {(L 1 -L 0 ) / L 0}×100... (iii) L 140 (%) = {(L 2 -L 0 ) / L 0}×100... (iv)
[0110] [Film-forming property] In the judgment of film-forming property, the films of Prototype Examples 1 to 24 were visually checked for defects in appearance such as uneven stretching during film formation, and the film was judged as "○" when a good appearance was obtained, and "×" when a poor appearance was confirmed.
[0111]
[0112]
[0113]
[0114]
[0115] [Results and Discussion] Prototype 17 is a biaxially oriented polypropylene film with a resin composition that does not contain recycled materials and is mainly composed of a highly crystalline polypropylene resin (resin A1). As shown in Table 7, Prototype 17 has good film performance in all aspects, including haze, heat shrinkage, tensile modulus, dimensional stability, and film formability. It is preferable that other films containing recycled materials have film performance similar to that of the film of Prototype 17.
[0116] Prototypes 1 to 4 and 18 are examples in which a highly crystalline polypropylene resin (resin A1) is used as the main raw material for the base layer, and resin B1 is used as the recycled raw material, with the blending amount adjusted. Similarly, prototypes 5 to 9 and 19 are examples in which resin B2 is used as the recycled raw material, with the blending amount adjusted. Prototypes 14 to 16 and 24 are examples in which resin B3 is used as the recycled raw material, with the blending amount adjusted. Prototypes 20 and 21 are examples in which resin B4 is used as the recycled raw material, with the blending amount adjusted.
[0117] Among the films of the above-mentioned prototypes, the films that did not exhibit sufficient film performance were prototypes 19 to 21 and 24. Comparing the films of prototypes 19 and 24 with other films that exhibited good film performance, the films of prototypes 19 and 24 contained an excess amount of recycled material compared to the other films. On the other hand, prototypes 20 and 21 were equivalent to films with a good proportion of recycled material. From these findings, it is believed that the physical properties of resin B4 incorporated into prototypes 20 and 21 are not suitable as a recycled material.
[0118] Therefore, by comparing the physical properties of the recycled raw materials (resins B1, B2, and B3) for which good results were obtained with those of the recycled raw material for resin B4, it is believed that the recycled raw materials have preferable physical properties of an MFR of 11.0 g / 10 min or less, a melting peak temperature of 145°C or more, a melting enthalpy of 87.0 J / g or more, and a crystallization temperature of 105°C or more. Of these physical properties, the lower limit of the MFR is thought to be about 3 g / 10 min, taking into account the fluidity of the resin. The upper limit of the melting peak temperature is thought to be about 170°C, taking into account practically usable resin molded products. Furthermore, by comparing resins B1, B2, and B3 with resin B4, it is believed that the molecular weight distribution (Mw / Mn, Mz+1 / Mw) determined by GPC measurement preferably satisfies the relationship Mw / Mn<Mz+1 / Mw and Mz+1 / Mw≧4.7.
[0119] Next, we consider the preferred blending ratio of recycled raw materials. It is believed that the blending ratios of prototypes 19 (resin B2) and 24 (resin B3) were excessive. Therefore, based on prototypes 1-4 and 18 (resin B1), prototypes 5-9 (resin B2), and prototypes 14-16 (resin B3), which yielded favorable results, it is believed that the preferred blending ratio of recycled raw materials is 25% by weight or less. Taking into consideration the reduction of environmental impact, it is preferable that the blending ratio of recycled raw materials be approximately 5% by weight. Therefore, it is believed that the preferred blending ratio of recycled raw materials that achieves both good film performance and environmental contribution is approximately 5-25% by weight.
[0120] Prototype 10 is a film in which the main raw material of the substrate layer is changed to another highly crystalline polypropylene resin (resin A2) compared to Prototype 1, and a propylene-α-olefin random copolymer (resin C1) is also blended. Prototype 10 obtained film performance almost equivalent to that of Prototype 1. Thus, no deterioration in film performance was observed even when a small amount of propylene-α-olefin random copolymer was blended into the substrate layer. The propylene-α-olefin random copolymer can be added in an amount sufficient to ensure that the blending amount of the propylene resin is not insufficient, and for example, 10 wt % or less is considered to be preferable.
[0121] Furthermore, Prototype Examples 11 to 13 are films in which some modifications were made to the film of Prototype Example 10. Prototype Example 11 is a film with a reduced thickness. Prototype Example 12 is a film in which the recycled material (resin B1) content was increased. Prototype Example 13 is a film in which a small amount of low-crystalline polypropylene resin (resin A3) was added to the substrate layer. All of Prototype Examples 11 to 13 exhibited good film performance. Prototype Example 11 suggests that there will be no significant change in film performance if the thickness is adjusted within the required thickness range. Prototype Example 12 demonstrates that even in a film containing a small amount of propylene-α-olefin random copolymer in the substrate layer, good film performance can be achieved by increasing the amount of recycled material within the range of 5 to 25 wt%. Prototype Example 13 demonstrates that good film performance can be achieved even when a small amount of low-crystalline polypropylene resin is added to a substrate layer primarily composed of a high-crystalline polypropylene resin.
[0122] To study the main raw material, polypropylene resin, in Prototype 22, a low-crystalline polypropylene resin (Resin A3) was used as the main raw material, and a biaxially oriented polypropylene film containing no recycled materials was produced. The film of Prototype 22 had an insufficient tensile modulus in the transverse (TD) direction, and therefore did not achieve the required rigidity. Furthermore, the dimensional stability was also insufficient. This is thought to be due to the low crystallinity of the polypropylene resin, which reduced the rigidity and heat resistance of the film.
[0123] Furthermore, Prototype 23 is a film obtained by blending 10% by weight of resin B1 as a recycled raw material with Prototype 22, and corresponds to a film in which the high crystalline polypropylene resin (resin A1) of the base layer of Prototype 1 was changed to a low crystalline polypropylene resin (resin A3). Dimensional stability was insufficient in Prototype 23. This is thought to be due to the low crystallinity of the polypropylene resin as in Prototype 22, which reduced heat resistance, etc., and is thought to indicate that the crystallinity of the polypropylene resin, the main raw material of the film, affected the film performance, regardless of whether recycled raw materials were used or not.
[0124] Based on the evaluation of each prototype, it was shown that, in order to ensure that the performance of films containing recycled materials is not impaired, including the longitudinal and transverse modulus of elasticity, dimensional stability (the difference between the longitudinal dimensional change rate at 140°C and the dimensional change rate at 120°C), and longitudinal and transverse heat shrinkage, the main raw material of the base layer should be 55% by weight or more of a high-crystalline polypropylene resin with a mesopentad fraction of 95% or more, and the recycled raw material should satisfy all of the following: MFR of 3.0 to 11.0 g / 10 min, peak melting temperature of 145 to 170°C, and melting enthalpy of 87.0 J / g or more, and the blending ratio should be 5 to 25% by weight. Furthermore, it was shown that even when a propylene-α-olefin random copolymer is blended, film performance is not impaired as long as the blending ratio is approximately 10% by weight or less.
[0125] In the biaxially oriented polypropylene film of the present invention, by using recycled raw materials that satisfy all of the specified conditions for melt flow rate, melting peak temperature, and melting enthalpy, it is possible to obtain excellent film formability without impairing film properties such as rigidity and heat resistance. Therefore, it is possible to provide a biaxially oriented polypropylene film and a laminate using this film that can contribute to reducing environmental load, and they are promising as alternatives to conventional biaxially oriented polypropylene films and their laminates.
Claims
1. A laminated film comprising a base layer and a surface layer laminated on one or both sides of the base layer, the base layer containing recycled materials derived from a molded product mainly made of polypropylene resin, the elastic modulus in the machine direction (MD) measured in accordance with JIS K 7127 (1999) being 2.0 GPa or more and the elastic modulus in the transverse direction (TD) being 4.0 GPa or more, and the dimensional change rate L in the machine direction (MD) at 140°C when the temperature is increased from 30°C to 150°C at 20°C / min and a load of 0.32 N is applied in the machine direction (MD) measured using a thermomechanical measuring device (TMA). 140 (%) and dimensional change rate L at 120°C 120 (%) and the difference (L 140 -L 120 % of the recycled material (B) having a melt flow rate (MFR) of 3.0 to 11.0 g / 10 min, a melting peak temperature of 145 to 170°C as measured by a differential scanning calorimeter (DSC) in accordance with JIS K 7122 (2012) and a melting enthalpy (ΔH) of 87.0 J / g or more.
2. The biaxially oriented polypropylene film according to claim 1, wherein the recycled raw material (B) has a crystallization temperature of 105°C or higher as measured with a differential scanning calorimeter (DSC) in accordance with JIS K 7122 (2012).
3. The biaxially oriented polypropylene film according to claim 1 or 2, wherein the recycled raw material (B) has a molecular weight distribution (Mw / Mn, Mz+1 / Mw) determined by gel permeation chromatography (GPC) measurement that satisfies Mw / Mn<Mz+1 / Mw and Mz+1 / Mw≧4.
7. Mw: weight average molecular weight Mn: number average molecular weight Mz+1: Z+1 average molecular weight 4. The biaxially oriented polypropylene film according to claim 1 or 2, wherein the base layer contains 10% by weight or less of a propylene-α-olefin random copolymer (C).
5. The biaxially oriented polypropylene film according to claim 3, wherein the base layer contains 10% by weight or less of a propylene-α-olefin random copolymer (C).
6. A laminate comprising the biaxially oriented polypropylene film according to claim 1 or 2 and a sealant film laminated thereon.
7. A laminate comprising the biaxially oriented polypropylene film according to claim 3 and a sealant film laminated thereon.
8. A laminate comprising the biaxially oriented polypropylene film according to claim 4 and a sealant film laminated thereon.
9. A laminate comprising the biaxially oriented polypropylene film according to claim 5 and a sealant film laminated thereon.
10. The laminate of claim 6, wherein said sealant film is a non-oriented polypropylene film.
11. The laminate according to claim 7, wherein said sealant film is a non-oriented polypropylene film.
12. The laminate according to claim 8, wherein said sealant film is a non-oriented polypropylene film.
13. The laminate according to claim 9, wherein said sealant film is a non-oriented polypropylene film.
Citation Information
Patent Citations
Olefinic building sheet
JP2000238187A
Polyolefin-based multilayered shrink film
JP2009101682A
Polypropylene-based multilayered shrink film
JP2010064369A
Packaging film for food product, and package for food product
JP2020007443A
Biaxially oriented laminated polypropylene film
JP2023013958A