Powder of composite metal oxide, vulcanizing agent for rubbers, and rubber composition
The composite metal oxide powder with a specific formula (Mg1-xZnxO) addresses the structural and efficiency issues in existing composite metal oxide powders by ensuring zinc oxide is both exposed and dissolved within magnesium oxide, enhancing vulcanization efficiency and aligning with sustainable development goals by reducing rubber granule production.
Patent Information
- Application Number
- PCT/JP2024/017975
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-05-15
- Publication Date
- 2024-11-28
AI Technical Summary
Existing composite metal oxide powders for rubber vulcanization, such as those disclosed in Patent Documents 1 and 2, lack a clear description of their structure and do not effectively utilize the properties of magnesium oxide and zinc oxide to enhance vulcanization processes, particularly in terms of agglomeration and dispersibility.
A composite metal oxide powder with a specific formula (Mg1-xZnxO) is developed, where x ranges from 0.02 to 0.5, exhibiting shifted diffraction angles for magnesium oxide peaks, allowing zinc oxide to act as a vulcanizing agent both inside and outside the magnesium oxide, promoting initial and latter stages of vulcanization, and potentially reducing the amount of rubber granules.
The composite metal oxide powder enhances vulcanization efficiency by ensuring zinc oxide is both exposed on the surface and dissolved within magnesium oxide, improving the initial and final stages of the vulcanization process, and contributes to sustainable development goals by minimizing rubber granule production.
Smart Images

Figure JP2024017975_28112024_PF_FP_ABST
Abstract
Description
Composite metal oxide powder, rubber vulcanizing agent, and rubber composition
[0001] The present disclosure relates to a composite metal oxide powder, a rubber vulcanizing agent, and a rubber composition.
[0002] In order to produce rubber products, a vulcanizing agent, such as zinc oxide, and a vulcanization aid, such as magnesium oxide, are added to rubber raw materials. In addition, to improve the tendency of magnesium oxide to aggregate and its poor dispersibility, composite metal oxides containing magnesium oxide and zinc oxide have been investigated.
[0003] For example, Patent Document 1 discloses the following composite metal oxide: Mg 1-x M 2+ x O (1) (wherein, M 2+ is Mn 2+ , Fe 2+ , Co 2+ , Ni 2+ , Cu 2+ and Zn 2+ wherein x is a number in the range of 0.001<x<0.5).
[0004] Patent Document 2 discloses the following composite metal oxide: Mg 1-x M 2+ x O (1) (wherein, M 2+ is Mn 2+ , Fe 2+ , Co 2+ , Ni 2+ , Cu 2+ and Zn 2+ and x is a number in the range of 0.001<x<0.5), and the BET specific surface area is 4 m 2 / g or less of a thermally conductive complex metal oxide that is a magnesium oxide-based solid solution.
[0005] JP-A-6-157032 JP-A-6-87979
[0006] However, Patent Documents 1 and 2 do not describe the structure of a composite metal oxide that is defined using XRD and has a specific peak according to the present disclosure. The present disclosure aims to provide a composite metal oxide powder that is particularly useful as a vulcanizing agent for rubber.
[0007] The present disclosure includes the following aspects. (First Disclosure) In this first disclosure, a composite metal oxide powder includes magnesium oxide and zinc oxide. In XRD, the powder has a peak of the zinc oxide and a peak of the magnesium oxide. In the powder, the diffraction angle of the magnesium oxide peak value is shifted to a lower angle side compared to the peak value of magnesium oxide single crystal.
[0008] (Second Disclosure) The second disclosure relates to the first disclosure, wherein the composite metal oxide is represented by the following formula (1): Mg 1-x Zn x O is represented by the formula (1): In formula (1), x satisfies 0.02≦x<0.5.
[0009] (Third Disclosure) The present third disclosure is a rubber vulcanizing agent including the first or second disclosure. (Fourth Disclosure) The present fourth disclosure is a rubber composition including the rubber vulcanizing agent according to the third disclosure and a rubber raw material.
[0010] The composite metal oxide powder according to the present disclosure is particularly useful as a vulcanizing agent for rubber.
[0011] Figure 1 shows powder X-ray diffraction data for Powder No. 1 and Powder No. 2. Figure 2 shows the results of a vulcanization test.
[0012] The composite metal oxide powder according to the present disclosure (hereinafter sometimes referred to as the "powder according to the present disclosure"), the rubber vulcanizing agent, and the rubber composition are described in detail below. The powder according to the present disclosure is a composite metal oxide powder and contains magnesium oxide and zinc oxide. In the present disclosure, the composite metal oxide refers to a metal oxide that combines magnesium oxide and zinc oxide. In other words, the composite metal oxide does not include a mixture of magnesium oxide and zinc oxide.
[0013] The powder according to the present disclosure has a zinc oxide peak and a magnesium oxide peak in powder X-ray diffraction (XRD). In the powder, the magnesium oxide peak value is shifted to a lower diffraction angle compared to the peak value of magnesium oxide single crystal. The powder X-ray diffraction can be measured using CuKα radiation as an X-ray source, with a measurement range of 5 to 70°, a step width of 0.026°, and a measurement speed of 10 seconds / step. An example of an instrument for performing the powder X-ray diffraction (XRD) is the Empyrean-DY1356 manufactured by Malvern Panalytical.
[0014] In the above powder, the peak value of the diffraction angle (2θ) on the (200) plane of magnesium oxide is shifted lower than the peak value of the diffraction angle (2θ) on the (200) plane of magnesium oxide single crystal by preferably at least 0.05°, more preferably at least 0.10°, and even more preferably at least 0.15°. Furthermore, in the above powder, the peak value of the diffraction angle (2θ) on the (200) plane of magnesium oxide is shifted lower than the peak value of the diffraction angle (2θ) on the (200) plane of magnesium oxide single crystal by preferably at most 1.00°, more preferably at most 0.50°, and even more preferably at most 0.30°. Therefore, when the above powder is used as a vulcanizing agent for rubber, for example, the zinc oxide solid-solved in the magnesium oxide can act as a vulcanizing agent in the latter half of vulcanization.
[0015] In the powder, the peak value of the diffraction angle (2θ) of zinc oxide may or may not be shifted from the peak value of the diffraction angle (2θ) of zinc oxide single crystal. In the powder, the peak value of the diffraction angle (2θ) of zinc oxide is preferably within a range of ±0.05° from the diffraction angle (2θ) of zinc oxide single crystal. As a result, when the powder is used as a vulcanizing agent for rubber, for example, the zinc oxide exposed on the outside of the magnesium oxide can promote initial vulcanization.
[0016] Furthermore, when the above powder is used as a rubber vulcanizing agent, the zinc oxide exposed on the outside of the magnesium oxide promotes initial vulcanization, and the zinc oxide dissolved inside the magnesium oxide can act as a vulcanizing agent in the latter half of vulcanization, which allows the amount of rubber granules to be reduced, thereby contributing to the achievement of the SDGs (Sustainable Development Goals) adopted at the United Nations Summit.
[0017] The composite metal oxide is preferably represented by the following formula (1): Mg 1-x Zn x O is represented by formula (1). x preferably satisfies 0.02≦x, more preferably 0.05≦x, and even more preferably 0.15≦x. Also, x preferably satisfies x<0.5, more preferably x≦0.25, and even more preferably x≦0.15. This makes it easier for zinc oxide to be exposed to the outside of magnesium oxide and easier for zinc oxide to form a solid solution inside magnesium oxide.
[0018] The composite metal oxide is preferably a metal oxide represented by the following formula (2): 1-n(Mg 1-m Zn m O).nZnO Formula (2) where m preferably satisfies 0.05≦m, and more preferably 0.10≦m. Also, m preferably satisfies m≦0.45, and more preferably m≦0.35. n preferably satisfies 0.05≦n, and more preferably 0.15≦n. Also, n preferably satisfies n≦0.45, and more preferably n≦0.40. This makes it easier for zinc oxide to be exposed to the outside of magnesium oxide and easier for zinc oxide to form a solid solution inside magnesium oxide.
[0019] The particle size of the powder can be any particle size, and the preferred range varies depending on the application. For example, when the powder is used as a rubber vulcanizing agent, the powder preferably has a D50 of 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.6 μm or more. Also, when the powder is used as a rubber vulcanizing agent, the powder preferably has a D50 of 100 μm or less, more preferably 60 μm or less, and even more preferably 50 μm or less.
[0020] In this specification, D50 means the 50% particle size on a volume basis, and can be measured by a laser diffraction method. An example of an instrument used in the laser diffraction method is the laser diffraction scattering particle size distribution analyzer LMS-2000e manufactured by Seishin Enterprises.
[0021] The powder may have any BET specific surface area, and the preferred range may vary depending on the application. For example, when the powder is used as a vulcanizing agent for rubber, the powder preferably has a BET specific surface area of 10 m 2 / g or more, more preferably 15m 2 / g or more, and more preferably 20m 2 For example, when the powder is used as a vulcanizing agent for rubber, the powder preferably has a BET specific surface area of 300 m 2 / g or less, more preferably 280m 2 / g or less, and more preferably 250m 2 The BET specific surface area is measured, for example, by a high-speed specific surface area / pore distribution measuring device NOVA2000 manufactured by Yuasa Ionics Co., Ltd.
[0022] The powder according to the present disclosure may not be surface-treated, and the particle surfaces may be surface-treated with a surface treatment agent, for example, to improve dispersibility in the rubber raw material. Examples of the surface treatment agent include anionic surfactants, cationic surfactants, phosphate ester treatment agents, silane coupling agents, titanate coupling agents, aluminum coupling agents, silicone treatment agents, silicic acid, and water glass. Particularly preferred surface treatment agents are one or more selected from the group consisting of oleic acid, stearic acid, octanoic acid, and octylic acid. The amount of the surface treatment agent is 0.01 to 20% by mass, and preferably 0.1 to 15% by mass, based on the powder.
[0023] The surface treatment with the surface treatment agent can be carried out by a conventional means, for example, by adding the powder to a Henshiel mixer, and while stirring the powder at high speed, adding dropwise the surface treatment agent either as is or diluted with a solvent, and mixing the powder and the surface treatment agent.
[0024] The rubber vulcanizing agent according to the present disclosure includes the above powder, in which zinc oxide is present both as a solid solution inside magnesium oxide and exposed on the outside of the magnesium oxide, and therefore when used as a rubber vulcanizing agent, the zinc oxide exposed on the outside of the magnesium oxide promotes initial vulcanization, while the zinc oxide dissolved in the magnesium oxide acts as a vulcanizing agent in the latter half of vulcanization, resulting in excellent vulcanization smoothness.
[0025] The rubber composition according to the present disclosure includes the rubber vulcanizing agent and a rubber raw material, such as synthetic rubbers, including acrylic rubber, ethylene propylene rubber (EPDM), butyl rubber, isoprene rubber, styrene butadiene rubber (SBR), nitrile rubber (NBR), and halogen-containing rubbers, including chlorosulfonated polyethylene, fluororubber, brominated butyl rubber, and epichlorohydrin rubber.
[0026] In the rubber composition, the ratio of the rubber raw material to the rubber vulcanizing agent may vary depending on the type of rubber (rubber raw material) to be formed. The rubber vulcanizing agent is added in an amount of, for example, 0.001 to 20 parts by mass, preferably 0.01 to 10 parts by mass, per 100 parts by mass of the rubber raw material.
[0027] The rubber composition may further contain other additives in addition to the rubber vulcanizing agent, such as antioxidants, ultraviolet absorbers, antistatic agents, pigments, lubricants, crosslinking agents, heat stabilizers for vinyl chloride such as organic acid salts of zinc, β-diketones, organotins, phosphites, and partial esters of polyhydric alcohols, foaming agents, plasticizers, and fillers.
[0028] The rubber vulcanizing agent according to the present disclosure is capable of vulcanizing raw materials of rubber without adding other vulcanizing agents, vulcanization accelerators, etc., but the rubber composition according to the present disclosure may further contain other vulcanizing agents, other vulcanization accelerators, etc. known in the art.
[0029] The mixing of the rubber raw material and the rubber vulcanizing agent is not particularly limited as long as they can be mixed, and examples thereof include a single-screw extruder, a twin-screw extruder, a roll, a Banbury mixer, etc. The rubber composition can be molded by known molding means, such as injection molding, extrusion molding, blow molding, press molding, rotational molding, calendar molding, sheet forming molding, transfer molding, lamination molding, vacuum molding, etc.
[0030] The powder according to the present disclosure has the same functions as conventional magnesium oxide-based solid solutions, and therefore can be used not only as the rubber vulcanizing agent described above, but also in applications where magnesium oxide is used, such as an acid acceptor for resins, an acid acceptor for rubber, an acid neutralizer, a thickener for FRP, a heat stabilizer, a deodorizer, a light resistance improver, and a resin curing agent.
[0031] The powder according to the present disclosure can be produced, for example, as follows: - a coprecipitation step of mixing a water-soluble magnesium salt, a water-soluble zinc salt, and an alkali to obtain a coprecipitate containing magnesium hydroxide and zinc hydroxide; - an aging step of aging the coprecipitate; - a grinding step of pulverizing the aged coprecipitate; and - a calcination step of calcining the pulverized coprecipitate to form the composite metal oxide powder.
[0032] In the coprecipitation step, a water-soluble magnesium salt, a water-soluble zinc salt, and an alkali are mixed to obtain a coprecipitate containing magnesium hydroxide and zinc hydroxide. Examples of the water-soluble magnesium salt include, but are not limited to, magnesium chloride, magnesium nitrate, magnesium acetate, magnesium sulfate, etc. From the viewpoint of suppressing aggregation of primary particles, the water-soluble magnesium salt is preferably magnesium chloride, magnesium nitrate, or magnesium acetate.
[0033] Examples of the water-soluble zinc salt include zinc chloride, zinc nitrate, etc. Examples of the alkali include hydroxides of alkali metals such as sodium hydroxide, potassium hydroxide, and lithium hydroxide, and hydroxides of alkaline earth metals such as calcium hydroxide.
[0034] The ratio of the water-soluble magnesium salt to the water-soluble zinc salt can be appropriately adjusted in accordance with the preferred molar ratio of Mg and Zn in the composite metal oxide. 1-x Zn x When the compound has the formula O, the water-soluble magnesium salt and the water-soluble zinc salt can be mixed in a ratio such that the molar ratio of Mg:Zn is (1-x):x.
[0035] The alkali can be added in an amount appropriate for the water-soluble magnesium salt and water-soluble zinc salt to form magnesium hydroxide and zinc hydroxide. If the amount of alkali required theoretically for the water-soluble magnesium salt and water-soluble zinc salt to completely form magnesium hydroxide and zinc hydroxide is taken as 100 mol % (1.0 equivalent), the alkali is preferably added in an amount of 80 mol % (0.8 equivalent) or more, more preferably 90 mol % (0.9 equivalent) or more, and even more preferably 95 mol % (0.95 equivalent) or more. The alkali may be added in an amount of 100 mol % (1.0 equivalent) or more, but from the viewpoint of facilitating washing of the coprecipitate, it is preferably added in an amount of 100 mol % (1.0 equivalent) or less.
[0036] The coprecipitate can be washed with deionized water or the like, filtered, and resuspended in water, an organic solvent, or the like, as needed, to remove impurities such as alkali metals, alkaline earth metals, etc. A homogenizer or the like can be used for the resuspension.
[0037] In the aging step, the coprecipitate is aged to form an aged coprecipitate. The aging temperature in the aging step is preferably 40°C or higher, more preferably 45°C or higher, and even more preferably 48°C or higher. The aging temperature is preferably 200°C or lower, more preferably lower than 100°C, and even more preferably 95°C or lower. This makes it easier to obtain the composite metal oxide powder. When the aging temperature is 100°C or higher, the aging step can be carried out under high pressure using an autoclave or the like.
[0038] The aging temperature in the aging step is preferably 1 hour or more, more preferably 2 hours or more, and even more preferably 3 hours or more. The aging temperature is preferably 10 hours or less, more preferably 8 hours or less, and even more preferably 6 hours or less. The aged coprecipitate can be dehydrated (filtered), dried, etc., as necessary.
[0039] In the grinding step, the aged coprecipitate is ground to form a ground coprecipitate. The grinding of the aged coprecipitate can be carried out using grinders known in the art. Examples of grinders include jaw crushers, gyratory crushers, cone crushers, impact crushers, roll crushers, cutter mills, stamp mills, ring mills, roller mills, jet mills, hammer mills, pin mills, rotary mills, vibratory mills, planetary mills, and ball mills.
[0040] In the calcination step, the pulverized coprecipitate is calcined to obtain a composite metal oxide powder. Calcination of the coprecipitate can be carried out by a method known in the art. Calcination of the coprecipitate can be carried out at a temperature of preferably 300°C or higher, and more preferably 350°C or higher. Calcination of the coprecipitate can be carried out at a temperature of preferably 600°C or lower, and more preferably 550°C or lower. Calcination of the coprecipitate can be carried out for a time period of preferably 0.1 hour or longer, more preferably 0.5 hour or longer, and preferably 10 hours or shorter, and more preferably 6 hours or shorter.
[0041] The present disclosure will be described below using examples, but the present disclosure is not limited to these examples. [Example 1] 3.0 L of a mixed solution of magnesium chloride and zinc chloride (magnesium concentration: 0.82 mol / L, zinc concentration: 0.2 mol / L) was added to a reaction vessel. While stirring the mixed solution, 2.0 mol / L of sodium hydroxide was added to the reaction vessel in an amount of 0.95 equivalents, the total equivalent of magnesium and zinc, to obtain Coprecipitate No. 1. Coprecipitate No. 1 was washed with deionized water, filtered, and then added with deionized water and resuspended using a homogenizer to obtain Resuspended Coprecipitate No. 1.
[0042] The resuspended coprecipitate No. 1 was aged at 80°C for 4 hours, filtered, dried, pulverized in a ball mill, and then calcined at 450°C for 1 hour to obtain composite metal oxide powder No. 1. The composition formula of composite metal oxide powder No. 1 was Mg 0.8 Zn 0.2The D50 and BET specific surface area of composite metal oxide powder No. 1 are shown in Table 1. Powder X-ray diffraction (XRD) data for composite metal oxide powder No. 1 is shown in Figure 1 together with powder X-ray diffraction (XRD) data for magnesium oxide single crystal (Kyowamag 150, manufactured by Kyowa Chemical Industry Co., Ltd.).
[0043] [Example 2] Composite metal oxide powder No. 2 was obtained in the same manner as in Example 1, except that the mixed solution of magnesium chloride and zinc chloride was changed so that the magnesium concentration was 0.77 mol / L and the zinc concentration was 0.25 mol / L, and the aging conditions and firing conditions were changed as shown in Table 1. The composition formula of composite metal oxide powder No. 2 was Mg 0.75 Zn 0.25 The D50 and BET specific surface area of composite metal oxide powder No. 2 are shown in Table 1. Powder X-ray diffraction (XRD) data for composite metal oxide powder No. 2 is shown in Figure 1 together with powder X-ray diffraction (XRD) data for magnesium oxide single crystal (Kyowamag 150, manufactured by Kyowa Chemical Industry Co., Ltd.).
[0044] Comparative Example 1 Composite metal oxide powder No. 3 was produced in accordance with Example 1 of Patent Document 1. The specific production method is as follows: 3.0 L of a mixed solution of magnesium chloride and zinc chloride (magnesium concentration: 0.96 mol / L, zinc concentration: 0.05 mol / L) was charged into a reaction vessel. While stirring the mixed solution, 2.0 mol / L of sodium hydroxide was charged into the reaction vessel in an amount of 0.95 equivalents, the total equivalent of magnesium and zinc, to obtain coprecipitate No. 3. Coprecipitate No. 3 was washed with deionized water, filtered, and then deionized water was added and resuspended using a homogenizer to obtain resuspended coprecipitate No. 3.
[0045] The resuspended coprecipitate No. 3 was aged in an autoclave at 175°C for 12 hours, filtered, dried, pulverized in a ball mill, and then calcined at 450°C for 1 hour to obtain composite metal oxide powder No. 3. The composition formula of composite metal oxide powder No. 3 was Mg 0.95 Zn 0.05The D50 and BET specific surface area of composite metal oxide powder No. 3 are shown in Table 1.
[0046]
[0047] Example 3 100 parts by mass of chloroprene resin (PS-40A, manufactured by Denka Co., Ltd.), 0.5 parts by mass of stearic acid, 30 parts by mass of carbon black, and 4.0 parts by mass of Powder No. 1 were kneaded using a roll mill to form Rubber Composition No. 1. Note that when Rubber Composition No. 1 was formed, most of the Rubber Composition No. 1 did not adhere to the roll.
[0048] The storage stability of Rubber Composition No. 1 was measured in accordance with JIS K6300-1:2013, Unvulcanized Rubber - Physical Properties - Part 1: Determination of Viscosity and Scorch Time Using a Mooney Viscometer. The test temperature was 125°C. The results are shown in Table 2. "Vm" refers to the minimum Mooney viscosity. "t5" refers to the scorch time (minutes) at which the Mooney reading rises 5M above Vm. "t35" refers to the scorch time (minutes) at which the Mooney reading rises 35M above Vm.
[0049] Rubber Composition No. 1 was molded into a thickness of 2 mm, press-vulcanized at 153°C for 30 minutes, and then allowed to stand at room temperature for 24 hours to form Sheet No. 1. The properties of Sheet No. 1 were measured in accordance with JIS K6251, "Vulcanized rubber and thermoplastic rubber - Determination of tensile properties." The results are shown in Table 2.
[0050] In the tensile properties, "Tb" means "tensile strength at break." "Eb" means "elongation at break." "Se" means "tensile stress at a given elongation." For example, Se100 means tensile stress at 100% elongation.
[0051] The heat resistance of Sheet No. 1 was measured in accordance with JIS K6257:2017, "Vulcanized rubber and thermoplastic rubber - Determination of heat aging characteristics." The heating conditions were 153°C and 0.5 hours. The results are shown in Table 2.
[0052] The Shore A hardness of Sheet No. 1 was measured in accordance with JIS K6253-3:2012, Vulcanized and thermoplastic rubbers - Determination of hardness - Part 3: Durometer hardness. The results are shown in Table 2. The compression set (CS) of Sheet No. 1 was measured in accordance with JIS K6262:2013, Vulcanized and thermoplastic rubbers - Determination of compression set at room temperature, high temperature, and low temperature. The test temperature was 120°C, and the test time was 72 hours. The results are shown in Table 2.
[0053] [Examples 4 and 5] Rubber compositions No. 2 and No. 3 and sheets No. 2 and No. 3 were formed according to Example 3, except that the amount of powder No. 1 was as shown in Table 2. Their properties are shown in Table 2. When rubber compositions No. 2 and No. 3 were kneaded, they generally did not adhere to the roll.
[0054] Examples 6 to 8 Rubber compositions No. 4 to No. 6 and sheets No. 4 to No. 6 were formed in the same manner as in Example 3, except that powder No. 1 was replaced with powder No. 2 in the amounts shown in Table 2. The properties of these compositions are shown in Table 2. When rubber compositions No. 4 to No. 6 were kneaded, they generally did not adhere to the roll.
[0055] Comparative Example 2 Rubber Composition No. 7 and Sheet No. 7 were formed in the same manner as in Example 3, except that Powder No. 1 was replaced with Powder No. 3 in the amounts shown in Table 2. The properties of these compositions are shown in Table 2.
[0056] Comparative Example 3 100 parts by mass of chloroprene resin (PS-40A, manufactured by Denka Company Ltd.), 0.5 parts by mass of stearic acid, 30 parts by mass of carbon black, 5 parts by mass of zinc oxide (zinc oxide type 2, manufactured by Seido Chemical Industry Co., Ltd.), and 4 parts by mass of magnesium oxide (Kyowamag 150, manufactured by Kyowa Chemical Industry Co., Ltd.) were kneaded using a roll mill to obtain rubber composition No. 8. Note that when rubber composition No. 8 was kneaded, a portion of rubber composition No. 8 adhered to the roll.
[0057] Sheet No. 8 was formed from rubber composition No. 8 in the same manner as in Example 3. The properties of rubber composition No. 8 and sheet No. 8 are shown in Table 2.
[0058]
[0059] [Example 9 and Comparative Example 4] Rubber composition No. 2 and rubber composition No. 8 were each subjected to a vulcanization test in accordance with JIS K6300-2:2001, "Unvulcanized rubber - Physical properties - Part 2: Determination of vulcanization characteristics using a vibration-type vulcanization tester." The results are shown in Figure 2.
Claims
1. A powder of a composite metal oxide containing magnesium oxide and zinc oxide, characterized in that in an XRD, it has a peak for the zinc oxide and a peak for the magnesium oxide, and the diffraction angle of the peak value of the magnesium oxide is shifted to the lower angle side compared to the peak value of magnesium oxide single crystal.
2. The composite metal oxide is represented by the following formula (1): Mg 1-x Zinc x The powder according to claim 1 , which is represented by the formula: O Formula (1) wherein x satisfies 0.02≦x<0.
5.
3. A rubber vulcanizing agent comprising the powder according to claim 1 or 2.
4. A rubber composition comprising the rubber vulcanizing agent according to claim 3 and a rubber raw material.
Citation Information
Patent Citations
Hollow hexahedral Zn-Mg oxide and application thereof in degrading rhodamine B through cooperation with hydrogen peroxide
CN113511668A
Composite metal oxide, its production and its use
JP1994157032A
Semiconductor film manufacturing method
WO2014002574A1
Zinc-containing hydrotalcite
WO2023135927A1