Coated active material, positive electrode, secondary battery, and method for manufacturing positive electrode

The coated active material with a halogen-containing layer and phosphorus-containing layer addresses the issue of side reactions in secondary batteries, ensuring sustained discharge capacity and battery longevity by preventing metal elution and electrolyte decomposition.

WO2024242000A1PCT designated stage expired Publication Date: 2024-11-28PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD

Patent Information

Application Number
PCT/JP2024/018040
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-15
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Conventional secondary batteries experience accelerated deterioration due to side reactions such as metal elution and electrolyte decomposition, which reduce discharge capacity and battery lifespan.

Method used

A coated active material is developed with a halogen-containing layer between the surface of the positive electrode active material and a phosphorus-containing layer, specifically a phosphoric acid compound, to prevent direct contact and suppress side reactions while maintaining discharge capacity.

Benefits of technology

The coated active material effectively suppresses side reactions at the positive electrode, enhancing battery durability and maintaining sufficient discharge capacity by preventing metal elution and electrolyte decomposition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018040_28112024_PF_FP_ABST
    Figure JP2024018040_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A coated active material 10 according to the present disclosure comprises: a positive electrode active material; a halogen-containing layer 12 that covers at least a part of the surface of a particle 11 of the positive electrode active material; and a phosphorus-containing layer 13 that covers at least a part of the surface of the halogen-containing layer 12. The halogen-containing layer 12 is positioned between the surface of the particle 11 and the phosphorus-containing layer 13. The halogen-containing layer 12 contains a halide and is in contact with the surface of the particle 11. The phosphorus-containing layer 13 contains a phosphoric acid compound.
Need to check novelty before this filing date? Find Prior Art

Description

Coated active material, positive electrode, secondary battery, and method for manufacturing positive electrode

[0001] The present disclosure relates to a coated active material, a positive electrode, a secondary battery, and a method for manufacturing a positive electrode.

[0002] It is known that conventional secondary batteries are subject to side reactions, such as reduction and elution of transition metals contained in the active material, which in turn cause decomposition of the electrolyte. These side reactions accelerate the deterioration of the secondary battery.

[0003] Non-Patent Document 1 describes a lithium-rich positive electrode material Li[Li 0.2 Ni 0.13 Mn 0.54 Co 0.13 ]O2, the addition of tristrimethylsilyl phosphate to the electrolyte is described to improve the cycle characteristics. Patent Document 1 discloses a cathode material including a cathode active material and a solid electrolyte material coating at least a portion of the surface of the cathode active material, the solid electrolyte material including Li, Ti, M1, and F, where M1 is at least one selected from the group consisting of Ca, Mg, Al, Y, and Zr. Patent Document 2 discloses a coated cathode active material having a coating containing at least one selected from a specific phosphonate ester and a specific phosphite triester. Patent Document 3 discloses a battery containing a phosphorus compound having a P—OH structure in at least one of the cathode and the electrolyte. Patent Document 4 discloses a nonaqueous electrolyte secondary battery in which the nonaqueous electrolyte contains at least one phosphorus compound selected from the group consisting of phosphine oxide, phosphonate ester, and phosphinate ester.

[0004] J. Zhang et al. “Artificial Interface Deriving from Sacrificial Tris(trimethylsilyl)phosphate Additive for Lithium Rich Cathode Materials” Electrochimica Acta 117 (2014) 99-104

[0005] International Publication No. 2021-187391 International Publication No. 2017-126276 JP 2013-152825 A JP 2013-055031 A

[0006] The present disclosure provides a coated active material that can suppress side reactions in the positive electrode while maintaining a sufficient discharge capacity of the battery.

[0007] The coated active material of the present disclosure includes: a positive electrode active material; a halogen-containing layer covering at least a portion of a surface of a particle of the positive electrode active material; and a phosphorus-containing layer covering at least a portion of the surface of the halogen-containing layer, wherein the halogen-containing layer is located between the surface of the particle and the phosphorus-containing layer, the halogen-containing layer contains a halide and is in contact with the surface of the particle, and the phosphorus-containing layer contains a phosphate compound.

[0008] The present disclosure provides a coated active material that can suppress side reactions in the positive electrode while maintaining a sufficient discharge capacity of the battery.

[0009] Fig. 1 is a cross-sectional view showing a schematic configuration of a coated active material 10 according to embodiment 1. Fig. 2A is a process diagram showing a method for manufacturing a positive electrode. Fig. 2B is a process diagram showing another method for manufacturing a positive electrode. Fig. 3 is a cross-sectional view showing a schematic configuration of a positive electrode 16 according to embodiment 3. Fig. 4 is a vertical cross-sectional view schematically showing a secondary battery 100 according to embodiment 4.

[0010] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. The present disclosure is not limited to the following embodiments.

[0011] (Embodiment 1) Fig. 1 is a cross-sectional view showing a schematic configuration of a coated active material 10 according to Embodiment 1. The coated active material 10 includes a positive electrode active material, a halogen-containing layer 12 that coats at least a portion of the surface of a particle 11 of the positive electrode active material, and a phosphorus-containing layer 13 that coats at least a portion of the surface of the halogen-containing layer 12. The halogen-containing layer 12 is located between the surface of the particle 11 and the phosphorus-containing layer 13. The halogen-containing layer 12 contains a halide and is in contact with the surface of the particle 11. The phosphorus-containing layer 13 contains a phosphate compound.

[0012] In a battery, contact between the positive electrode active material and the electrolyte causes side reactions such as metal elution from the positive electrode active material and gas generation due to electrolyte decomposition, resulting in battery degradation. On the other hand, forming a phosphate compound coating on the surface of the positive electrode active material in an acidic environment to prevent contact between the positive electrode active material and the electrolyte alters the surface of the positive electrode active material, reducing battery capacity. In the coated active material 10 of the present disclosure, a halogen-containing layer 12 coats the surface of the positive electrode active material particles 11 in contact with the surface, and a phosphorus-containing layer 13 coats the halogen-containing layer 12 on top of the surface. That is, the halogen-containing layer 12 is located between the surface of the positive electrode active material particles 11 and the phosphorus-containing layer 13. This configuration prevents contact between the phosphate compound and the positive electrode active material, suppresses deterioration of the positive electrode active material, and suppresses side reactions such as metal elution at the positive electrode. Therefore, side reactions at the positive electrode can be suppressed while maintaining a sufficient discharge capacity of the battery.

[0013] Examples of the positive electrode active material that can be used include lithium-containing transition metal oxides, lithium-containing transition metal phosphates, transition metal fluorides, polyanionic materials, fluorinated polyanionic materials, transition metal sulfides, transition metal oxysulfides, and transition metal oxynitrides. In particular, using a lithium-containing transition metal oxide or a lithium-containing transition metal phosphate as the positive electrode active material can reduce the manufacturing cost of the battery and increase the average discharge voltage. Examples of lithium-containing transition metal oxides include lithium cobalt oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide, and lithium nickel manganese oxide. Examples of lithium-containing transition metal phosphates include lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, and lithium nickel phosphate.

[0014] The positive electrode active material may contain lithium nickel oxide having a layered rock salt crystal structure. The proportion of Ni among metal elements other than Li contained in the lithium nickel oxide may be 50 atomic % or more. The lithium nickel oxide may contain other transition metals. Lithium nickel oxide is useful for achieving a high operating voltage. The configuration of the coated active material according to embodiment 1 can suppress the elution of metal ions from the positive electrode active material. Because nickel is easily eluted from the positive electrode active material, the technology of the present disclosure is particularly expected to be effective in suppressing elution.

[0015] The lithium nickel oxide may be represented by the following composition formula (I): Element Me1 is at least one selected from the group consisting of V, Co, and Mn. Element Me2 is at least one selected from the group consisting of Mg, Al, Ca, Ti, Cu, Zn, and Nb. Composition formula (I) satisfies 0.9≦α1≦1.10, −0.05≦β1≦0.05, 0.5≦x1<1, 0≦x2≦0.5, and 0≦1−x1−x2≦0.5. Li α1 Ni x1 Me1 x2 Me2 (1-x1-x2) O 2+β1 ...(I)

[0016] In composition formula (I), 0<x2≦0.5 may be satisfied, or 0<1−x1−x2≦0.5 may be satisfied.

[0017] There are no particular limitations on the shape of the positive electrode active material particles 11. The shape of the particles 11 is, for example, needle-like, scale-like, spherical, or oval-spherical.

[0018] Halogen-containing layer 12 is a layer containing a halide, and covers at least a portion of the surface of positive electrode active material particle 11 and is in contact with the surface of positive electrode active material particle 11. Halogen-containing layer 12 is formed by the halide being located in contact with at least a portion of the surface of positive electrode active material particle 11.

[0019] The halogen-containing layer 12 may contain a halide as a main component. Here, the "main component" refers to the component that is contained in the largest amount by mass.

[0020] The halogen-containing layer 12 may consist essentially of a halide. "The halogen-containing layer 12 consists essentially of a halide" means that the mass proportion of the halide in the halogen-containing layer 12 is 97 mass% or more. The mass proportion of the halide in the halogen-containing layer 12 may be 98 mass% or more, or may be 99 mass% or more. The halogen-containing layer 12 may consist solely of a halide, excluding inevitable impurities.

[0021] The halide may have lithium ion conductivity. The halide may be a halide solid electrolyte having lithium ion conductivity.

[0022] The halide may be a fluoride. Such a halide has excellent oxidation resistance. Therefore, the coated active material 10 including the halogen-containing layer 12 between the surface of the positive electrode active material particle 11 and the phosphorus-containing layer 13 can improve battery characteristics such as discharge capacity.

[0023] The halide may include Li, M1, M2, and F, where M1 is at least one selected from the group consisting of Ti and Nb, and M2 may be at least one selected from the group consisting of Ca, Mg, Al, Y, and Zr. In this configuration, the halide exhibits high ionic conductivity.

[0024] The halide may consist essentially of Li, M1, M2, and F. "The halide consists essentially of Li, M1, M2, and F" means that the molar ratio (i.e., molar fraction) of the total amount of substance of Li, M1, M2, and F to the total amount of substance of all elements constituting the halide is 90% or more. As an example, the molar ratio may be 95% or more.

[0025] M1 may contain Ti. M2 may contain Al. M1 may contain Ti and M2 may contain Al. That is, the halide may contain Li, Ti, Al, and F, or may consist essentially of Li, Ti, Al, and F. In this configuration, the halide exhibits high ionic conductivity.

[0026] The halide may have a composition represented by the following composition formula (II): In composition formula (II), α2, β2, γ2, and δ2 are each independently a value greater than 0. Li α2 M1 β2 M2 γ2 X δ2 ...Formula (II)

[0027] In the composition formula (II), δ2 may be a value greater than α2, δ2 may be a value greater than each of α2, β2, and γ2.

[0028] In composition formula (II), the following may be satisfied: 1.7≦α2≦3.7, 0<β2<1.5, 0<γ2<1.5, and 5≦δ2≦7.

[0029] In composition formula (II), 2.5≦α2≦3, 0.1≦β2≦0.6, 0.4≦γ2≦0.9, and δ2=6 may be satisfied.

[0030] According to this configuration, the halide exhibits high ionic conductivity, which can improve the battery characteristics.

[0031] The halide may be represented by the following composition formula (III): In composition formula (III), 0<x3<1 and 0<b3≦1.5 are satisfied. Li6-(4-x3)b3(Ti 1-x3 Al x3 ) b3 F6...Formula (III)

[0032] In order to increase the ionic conductivity of the first solid electrolyte, in composition formula (III), 0.1≦x3≦0.9 may be satisfied, or 0.1≦x≦0.7 may be satisfied.

[0033] The halide may have a composition represented by the following composition formula (IV): In composition formula (IV), x4, y4, and b4 satisfy the following conditions: 0<x4<1, 0<y4<1, 0<x4+y4≦1, and 0.8≦b4≦1.1, and m is the valence of M2. Li6-{5-x4-(5-m)y4}b4(Nb 1-x4-y4 Ti x4 M2 y4 )b4 F6...Formula (IV)

[0034] In the composition formula (IV), when M2 contains a plurality of elements, m is the sum of the products of the composition ratios of the respective elements and the valences of the elements. For example, when M2 contains an element Met1 and an element Met2, and the element Met1 has a composition ratio of a1 and a valence of m1, and the element Met2 has a composition ratio of a2 and a valence of m2, m is expressed as m1a1+m2a2.

[0035] The thickness of the halogen-containing layer 12 may be 1 nm or more and 1 μm or less, or may be 5 nm or more and 0.1 μm or less.

[0036] The mass ratio of the halogen-containing layer 12 to the positive electrode active material may be 0.01% or more and 20% or less, or 0.01% or more and 5% or less. The mass ratio of the halide contained in the halogen-containing layer 12 to the positive electrode active material may be 0.01% or more and 20% or less, or 0.01% or more and 5% or less.

[0037] The mass ratio of the halogen-containing layer 12 to the positive electrode active material can be measured, for example, by energy dispersive X-ray spectroscopy using a transmission electron microscope (TEM-EDX).

[0038] The phosphorus-containing layer 13 is a layer containing a phosphate compound, and covers at least a portion of the surface of the halogen-containing layer 12. The phosphorus-containing layer 13 is formed by the phosphate compound being located on at least a portion of the surface of the halogen-containing layer 12, which covers at least a portion of the surface of the positive electrode active material particles 11. The phosphorus-containing layer 13 may be in contact with the surface of the halogen-containing layer 12. The phosphorus-containing layer 13 does not have to be in contact with the surface of the positive electrode active material particles 11.

[0039] The phosphorus-containing layer 13 may be substantially composed of a phosphate compound. "The phosphorus-containing layer 13 is substantially composed of a phosphate compound" means that the mass ratio of the phosphate compound in the phosphorus-containing layer 13 is 97 mass% or more. The mass ratio of the phosphate compound in the phosphorus-containing layer 13 may be 98 mass% or more, or may be 99 mass% or more. The phosphorus-containing layer 13 may be composed only of a phosphate compound.

[0040] As used herein, "phosphate compound" refers to an oxoacid of phosphorus. Examples of phosphate compounds include phosphoric acid, phosphonic acid, phosphinic acid, pyrophosphoric acid, phosphate esters, phosphonic acid esters, phosphinic acid esters, derivatives thereof, and condensates thereof. The phosphate compound may be an organic phosphorus compound. As used herein, the organic phosphorus compound refers to a compound containing carbon and phosphorus. The phosphate compound may be a compound having a carbon-phosphorus bond.

[0041] The phosphate compound may contain a P-O-P bond. The phosphate compound may be polyphosphoric acid, a polyphosphate ester, or a derivative thereof.

[0042] The phosphate compound may contain a structure represented by chemical formula (1).

[0043]

[0044] In chemical formula (1), n1 and n2 are each independently an integer of 0 or greater. 1 , R 2 , R 4 , and R 5 are each independently -OR or -(CH2) m1 represents X1. 3 and R are each independently a direct bond to a halide in the halogen-containing layer 12, a hydrogen atom, or —(CH) m2 X2 represents a trimethylsilyl group or a triethylsilyl group. m1 is an integer of 0 to 15. m2 is a natural number of 1 to 3. X1 and X2 each independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxy group, a cyano group, or a fluorine atom. R 2 If there are multiple R 2 are independent of each other. 4 If there are multiple R 4 are independent of each other.

[0045] Because the phosphate compound has such a structure, it is relatively stable even under high voltage environments. Therefore, even when the upper limit voltage of the secondary battery is high, for example, even when it exceeds 4.3 V, it is possible to sufficiently suppress oxidative decomposition of the electrolyte and suppress side reactions such as metal elution from the positive electrode active material.

[0046] In chemical formula (1), n1 and n2 may be, independently of each other, 1 or greater. At least one selected from the group consisting of n1 and n2 may be 1 or greater. n1 and n2 may be, independently of each other, 500 or less. X1 may be a hydrogen atom. X2 may be a hydrogen atom.

[0047] In chemical formula (1), m1 may be an integer of 0 to 11, or an integer of 0 to 6. When m1 is an integer of 0 to 6, side reactions can be further suppressed.

[0048] In the chemical formula (1), m2 may be 1 or 2.

[0049] The phosphate compound may be, for example, silyl phosphite, phosphonic acid, phosphoric acid, pyrophosphate, or a condensate thereof. The phosphate compound may contain Si. The phosphate compound may be silyl phosphite, tristrimethylsilyl phosphate (TMSP), or a compound derived from TMSP, such as a condensate of TMSP. In the chemical formula (1), R 1 , R 2 , R 4 , and R 5 are each independently -OR, and R 3 and R may each independently represent a direct bond to a halide in the halogen-containing layer 12, a hydrogen atom, or a trimethylsilyl group.

[0050] In the chemical formula (1), R 3 may represent a direct bond to the halide.

[0051] The phosphorus-containing layer 13 may contain one or more types of phosphoric acid compounds.

[0052] The phosphorus-containing layer 13 covers at least a portion of the surface of the halogen-containing layer 12, which in turn covers the surfaces of the positive electrode active material particles 11. This configuration prevents direct contact between the phosphate compound and the positive electrode active material. This prevents deterioration of the positive electrode active material, thereby maintaining a sufficient discharge capacity and suppressing side reactions such as metal elution in the positive electrode.

[0053] The phosphorus-containing layer 13 may cover the entire surface of the halogen-containing layer 12 .

[0054] The phosphorus-containing layer 13 may be in contact with the halogen-containing layer 12. As described above, the phosphorus-containing layer 13 does not have to be in contact with the surface of the particles 11 of the positive electrode active material.

[0055] The phosphate compound may or may not form a chemical bond with the halide in the halogen-containing layer 12. The phosphate compound may be physically attached to the halogen-containing layer 12.

[0056] The mass ratio of P (phosphorus) contained in the phosphorus-containing layer 13 to the positive electrode active material may be 0.1% or more. With such a configuration, contact between the positive electrode active material and the electrolyte solution can be sufficiently prevented, and side reactions at the interface between the surface of the positive electrode active material and the electrolyte solution can be suppressed.

[0057] The mass ratio of P contained in the phosphorus-containing layer 13 relative to the positive electrode active material can be measured using, for example, TEM-EDX. For example, the location and abundance ratio of P can be confirmed by TEM-EDX, and then the mass can be measured by inductively coupled plasma atomic emission spectrometry (ICP-AES) to determine the mass of P contained in the phosphorus-containing layer 13. The mass of the positive electrode active material can also be measured by, for example, ICP-AES. From the above, the mass ratio of P contained in the phosphorus-containing layer 13 can be calculated. For example, when the phosphate compound is an organic phosphorus compound, the phosphorus-containing layer 13 can be identified by TEM-EDX elemental mapping as a region with high concentrations of P and C on the surface of the halogen-containing layer 12 that coats the surface of the positive electrode active material particles 11.

[0058] In the coated active material 10, the mass ratio of P contained in the phosphorus-containing layer 13 to the positive electrode active material may be 3 mass% or less, or may be 2 mass% or less. The mass ratio of P contained in the phosphorus-containing layer 13 to the positive electrode active material may be 0.1 mass% or more and 2 mass% or less.

[0059] The ratio of the mass of P at the interface between the surface of the positive electrode active material particle 11 and the halogen-containing layer 12 to the mass of P at the particle surface of the coated active material 10 may be 3% or less. The ratio of the mass of the phosphate compound at the interface between the surface of the positive electrode active material particle 11 and the halogen-containing layer 12 to the mass of the phosphate compound at the particle surface of the coated active material 10 may be 3% or less. The phosphate compound may not be present at the interface between the surface of the positive electrode active material particle 11 and the halogen-containing layer 12.

[0060] The thickness of the phosphorus-containing layer 13 may be 0.001 μm or more and 2 μm or less, or may be 0.001 μm or more and 1 μm or less.

[0061] The coated active material 10 has, for example, a particle shape. There are no particular limitations on the particle shape of the coated active material 10. The particle shape of the coated active material 10 is needle-like, scale-like, spherical, or oval-spherical.

[0062] (Method for Producing Coated Active Material) The coated active material 10 can be produced, for example, by the following method.

[0063] The halogen-containing layer 12 is obtained by attaching a halide to the surfaces of the positive electrode active material particles 11. For example, raw material powders are mixed to prepare a halide. Then, the halide is attached to the surfaces of the positive electrode active material particles 11.

[0064] The method for attaching a halide to the surface of the positive electrode active material particles 11 is not particularly limited. For example, a halide is coated on a powder of the positive electrode active material by a mechanochemical method, thereby forming a halogen-containing layer 12 on the surface of the positive electrode active material particles 11. The positive electrode active material and the halide are mixed in an appropriate ratio to obtain a mixture, which is then milled to impart mechanical energy to the mixture. A mixing device such as a ball mill can be used for the milling process. Examples of devices that can impart mechanical energy include processing devices (particle composite devices) such as a ball mill, "Mechanofusion" (manufactured by Hosokawa Micron), "Nobilta" (manufactured by Hosokawa Micron), and "Balance Gran" (manufactured by Freund Turbo).

[0065] Next, a solution containing a phosphoric acid compound and a solvent is prepared.

[0066] As described above, the phosphate compound includes, for example, a structure represented by chemical formula (1). The phosphate compounds in the raw material stage are in a state before they can condense with each other and / or bond with halides, and can be distinguished from the phosphate compounds contained in the phosphorus-containing layer 13. The phosphate compounds in the raw material stage include, for example, a structure represented by chemical formula (2).

[0067]

[0068] In chemical formula (2), R 7 is a hydrogen atom, -(CH2) k1 Y1 represents a trimethylsilyl group or a triethylsilyl group. 6 and R 8 are each independently -OR or -(CH2) k2 Y2 represents a hydrogen atom, -(CH2) k3 Y3 represents a trimethylsilyl group or a triethylsilyl group. k1 and k3 are each independently a natural number from 1 to 3. k2 is an integer from 0 to 15. Y1, Y2, and Y3 are each independently a hydrogen atom, a hydroxyl group, an amino group, a carboxy group, a cyano group, or a fluorine atom.

[0069] The phosphoric acid compound in the raw material stage may include at least one selected from the group consisting of silyl phosphite and phosphoric acid. The silyl phosphite may be TMSP.

[0070] Examples of solvents that can be used include cyclic carbonates, chain carbonates, and cyclic carboxylic acid esters. Examples of cyclic carbonates include propylene carbonate (PC), ethylene carbonate (EC), and fluoroethylene carbonate (FEC). Examples of chain carbonates include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Examples of cyclic carboxylic acid esters include γ-butyrolactone (GBL), γ-valerolactone (GVL), and the like. One solvent may be used alone, or two or more solvents may be used in combination. From the viewpoint of the production process, a solvent with a high boiling point is preferred. The boiling point of the solvent is, for example, 200°C or higher.

[0071] The concentration of the phosphate compound in the solution may be 0.1% by mass or more and 20% by mass or less.

[0072] Next, the prepared solution is brought into contact with the particles 11 of the positive electrode active material having the halogen-containing layer 12 formed on the surface thereof. The contact may be performed by immersing the particles in the solution. Alternatively, the solution may be applied to the particles, for example, by spraying. The positive electrode active material containing the particles may be formed into a layer, and the solution may be applied onto the layer or impregnated into the solution, thereby bringing the positive electrode active material particles into contact with the solution. The contact time with the solution is, for example, 15 minutes or more and 120 minutes or less, and the temperature is, for example, 20°C or more and 60°C or less.

[0073] The particles of the positive electrode active material that have been brought into contact with the solution are dried. The drying time may be, for example, 5 minutes to 48 hours. In this manner, the coated active material 10 according to the first embodiment is obtained. The drying may be vacuum drying. Vacuum drying refers to drying at a pressure lower than atmospheric pressure.

[0074] After contact with the solution, the particles of the positive electrode active material may be washed before vacuum drying. For example, the particles of the positive electrode active material may be washed using a solvent. The solvent used for washing may be the same solvent used in the solution containing the phosphoric acid compound and the solvent, such as DMC. This makes it possible to remove by-products such as decomposition products of the phosphoric acid compound. This makes it possible to suppress gas generation at the positive electrode due to the reaction between the by-products and the electrolyte.

[0075] (Embodiment 2) A method for producing a positive electrode according to Embodiment 2 satisfies at least one selected from the group consisting of (A) and (B) below: (A) forming a halogen-containing layer on at least a portion of the surface of particles of a positive electrode active material, forming a positive electrode active material layer on a positive electrode current collector, the particles having the halogen-containing layer formed thereon, contacting the positive electrode active material layer with a solution containing a phosphate compound and a solvent, and drying the positive electrode active material layer after the contact; (B) forming a halogen-containing layer on at least a portion of the surface of particles of a positive electrode active material, contacting the particles having the halogen-containing layer formed thereon with a solution containing a phosphate compound and a solvent, and drying the particles after the contact, and forming a positive electrode active material layer on a positive electrode current collector, the dried particles being included.

[0076] FIG. 2A is a process diagram showing a method for producing a positive electrode.

[0077] In step S1, a halogen-containing layer is formed on at least a portion of the surface of particles of a positive electrode active material.

[0078] The halogen-containing layer is a layer containing a halide, such as the halide described above in the first embodiment.

[0079] In step S1, the halogen-containing layer may be formed by a mechanochemical method.

[0080] In step S2, a positive electrode active material layer including particles on which a halogen-containing layer has been formed is formed on the positive electrode current collector. In step S2, the positive electrode active material layer is formed, for example, as follows.

[0081] A positive electrode slurry containing the positive electrode active material obtained in step S1 is prepared, for example, by dispersing the positive electrode active material, a binder, and a conductive additive in a dispersion medium.

[0082] A positive electrode active material layer is formed by applying a positive electrode slurry to a positive electrode current collector. Specifically, the positive electrode slurry is applied to a positive electrode current collector to form a coating film. The positive electrode active material layer is obtained by removing the dispersion medium from the coating film. One method for removing the dispersion medium is to heat the coating film. For example, N-methyl-2-pyrrolidone (NMP) or the like is used as the dispersion medium. In this way, a positive electrode active material layer is formed on the positive electrode current collector.

[0083] In step S3, the positive electrode active material layer is contacted with a solution containing a phosphate compound and a solvent. In step S3, the positive electrode active material layer may be contacted with the solution by impregnating the positive electrode active material layer formed on the positive electrode current collector with the solution, or by applying the solution to the positive electrode active material layer. The contact time is, for example, from 15 minutes to 120 minutes.

[0084] The solution containing the phosphate compound and the solvent is, for example, the solution described in embodiment 1. That is, the phosphate compound may have a structure represented by the above chemical formula (2). The phosphate compound may include TMSP. The solvent may be the solvent described above in embodiment 1.

[0085] In step S4, the positive electrode active material layer is dried. In step S4, the drying time may be, for example, 5 minutes or more and 48 hours or less.

[0086] After step S3 and before step S4, the positive electrode active material layer may be washed. For example, the positive electrode active material layer is washed using a solvent. The solvent used for washing may be the solvent used in the solution containing the phosphate compound and the solvent, such as DMC. This makes it possible to remove by-products such as decomposition products of the phosphate compound. This makes it possible to suppress gas generation at the positive electrode due to a reaction between the by-products and the electrolyte.

[0087] FIG. 2B is a process diagram showing another method for producing a positive electrode.

[0088] In step ST1, a halogen-containing layer is formed on at least a part of the surface of the particles of the positive electrode active material in the same manner as in step S1.

[0089] In step ST2, a solution containing a phosphate compound and a solvent is brought into contact with the particles of the positive electrode active material obtained in step ST1. The contact of the solution with the particles of the positive electrode active material may be carried out by immersing the particles of the positive electrode active material in the solution, or by applying the solution to the particles of the positive electrode active material, for example by spraying the solution onto the particles of the positive electrode active material.

[0090] In step ST3, the particles of the positive electrode active material obtained in step ST2 are dried. In step ST3, the drying time may be, for example, 5 minutes to 48 hours. The drying may be vacuum drying. Vacuum drying refers to drying at a pressure lower than atmospheric pressure.

[0091] In step ST4, a positive electrode active material layer is formed on the positive electrode current collector using the positive electrode active material particles obtained in step ST3 in the same manner as in step S2.

[0092] After step ST2 and before step ST3, the particles of the positive electrode active material may be washed.

[0093] The method for producing a positive electrode according to the present disclosure may satisfy the above-mentioned (A).

[0094] The method for producing a positive electrode of the present disclosure may satisfy both of the above (A) and (B). The method for producing a positive electrode of the present disclosure may include forming a halogen-containing layer on at least a portion of the surface of particles of a positive electrode active material, contacting the particles on which the halogen-containing layer has been formed with a solution containing a phosphate compound and a solvent, drying the particles after the contact, forming a positive electrode active material layer containing the obtained dried particles on a positive electrode current collector, further contacting the positive electrode active material layer with a solution containing a phosphate compound and a solvent, and drying the positive electrode active material layer after the contact. That is, in the method for producing a positive electrode of the present disclosure, steps S3 and S4 may be performed after steps ST1 to ST4.

[0095] The mass ratio of P contained in the phosphate compound to the positive electrode active material may be 0.1% or more. That is, the mass ratio of P contained in the phosphate compound to the positive electrode active material in the solution brought into contact with the positive electrode active material layer or the positive electrode active material particles may be 0.1% or more.

[0096] 3 is a cross-sectional view showing a schematic configuration of a positive electrode 16 according to embodiment 3. The positive electrode 16 includes a positive electrode current collector 14 and a positive electrode active material layer 15 supported on the positive electrode current collector 14. The positive electrode active material layer 15 includes the coated active material according to embodiment 1.

[0097] The positive electrode active material layer 15 may contain only the coated active material according to embodiment 1 as the positive electrode active material, or may contain a positive electrode active material different from the coated active material according to embodiment 1. The positive electrode active material layer 15 may contain the coated active material according to embodiment 1 on its surface.

[0098] The positive electrode active material layer 15 may further contain other materials such as a binder, an ion conductor, and a conductive additive.

[0099] For example, a metal foil can be used for the positive electrode current collector 14. Examples of metals that form the positive electrode current collector 14 include aluminum, titanium, alloys containing these metal elements, and stainless steel.

[0100] The positive electrode 16 is manufactured by, for example, the manufacturing method according to the second embodiment.

[0101] (Embodiment 4) A secondary battery according to embodiment 4 includes the positive electrode according to embodiment 3, a negative electrode, and an electrolyte. By using the positive electrode according to embodiment 3, the characteristics of the secondary battery, such as charge / discharge efficiency, can be improved.

[0102] 4 is a longitudinal cross-sectional view schematically illustrating a secondary battery 100 according to embodiment 4. The secondary battery 100 is a cylindrical battery including a cylindrical battery case, a wound electrode group 24, and an electrolyte (not shown). The electrode group 24 is housed in the battery case and is in contact with the electrolyte.

[0103] The battery case is composed of a case body 25, which is a cylindrical metal container with a bottom, and a sealing body 26 that seals the opening of the case body 25. A gasket 37 is disposed between the case body 25 and the sealing body 26. The gasket 37 ensures the airtightness of the battery case. Within the case body 25, insulating plates 27 and 28 are disposed on both ends of the electrode group 24 in the direction of the winding axis of the electrode group 24, respectively.

[0104] Case body 25 has, for example, a step portion 31. Step portion 31 can be formed by partially pressing the side wall of case body 25 from the outside. Step portion 31 may be formed in an annular shape on the side wall of case body 25 along the circumferential direction of an imaginary circle defined by case body 25. In this case, sealing body 26 is supported by, for example, the surface of step portion 31 on the opening side.

[0105] Sealing body 26 includes a filter 32, a lower valve body 33, an insulating member 34, an upper valve body 35, and a cap 36. These components are stacked in this order in sealing body 26. Sealing body 26 is attached to the opening of case body 25 so that cap 36 is located on the outside of case body 25 and filter 32 is located on the inside of case body 25.

[0106] Each of the above-mentioned members constituting the sealing body 26 has, for example, a disk or ring shape. The above-mentioned members, except for the insulating member 34, are electrically connected to one another.

[0107] The electrode group 24 has a positive electrode 21, a negative electrode 22, and a separator 23. The positive electrode 21, the negative electrode 22, and the separator 23 are all strip-shaped. The width direction of the strip-shaped positive electrode 21 and negative electrode 22 is, for example, parallel to the winding axis of the electrode group 24. The separator 23 is disposed between the positive electrode 21 and the negative electrode 22. The positive electrode 21 and the negative electrode 22 are spirally wound with the separator 23 interposed between these electrodes.

[0108] When observing a cross section of the secondary battery 100 in a direction perpendicular to the winding axis of the electrode group 24, the positive electrodes 21 and negative electrodes 22 are stacked alternately in the radial direction of an imaginary circle defined by the case body 25, with a separator 23 interposed between these electrodes.

[0109] The positive electrode 21 is electrically connected to a cap 36, which also serves as a positive electrode terminal, via a positive electrode lead 29. One end of the positive electrode lead 29 is connected, for example, to near the center of the positive electrode 21 in the longitudinal direction of the positive electrode 21. The positive electrode lead 29 passes through a through-hole formed in the insulating plate 27 and extends from the positive electrode 21 to the filter 32. The other end of the positive electrode lead 29 is welded, for example, to the surface of the filter 32 on the electrode group 24 side.

[0110] The negative electrode 22 is electrically connected to the case body 25, which also serves as a negative electrode terminal, via a negative electrode lead 30. One end of the negative electrode lead 30 is connected to, for example, an end of the negative electrode 22 in the longitudinal direction of the negative electrode 22. The other end of the negative electrode lead 30 is welded to, for example, the inner bottom surface of the case body 25.

[0111] Each component of the secondary battery 100 will be specifically described below.

[0112] The positive electrode 21 is the positive electrode according to the third embodiment.

[0113] The negative electrode 22 includes a material having the property of absorbing and releasing metal ions (e.g., lithium ions). The negative electrode 22 includes, for example, a negative electrode active material. The negative electrode may include a negative electrode current collector and a negative electrode active material layer supported on the surface of the negative electrode current collector.

[0114] The negative electrode current collector is, for example, a foil made of a metal material such as stainless steel, nickel, a nickel alloy, copper, or a copper alloy.

[0115] The negative electrode active material layer includes a negative electrode active material, which can be a material capable of absorbing and releasing lithium ions, such as lithium titanate, graphite, silicon, a silicon compound, or a NiBi alloy.

[0116] The negative electrode active material layer may contain other materials such as a conductive additive, an ion conductor, and a binder.

[0117] The electrolyte may contain a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. The concentration of the lithium salt in the electrolyte may be, for example, 0.5 mol / L or more and 2 mol / L or less. By controlling the lithium salt concentration within the above range, an electrolyte having excellent ionic conductivity and appropriate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.

[0118] The non-aqueous solvent may be a cyclic carbonate, a chain carbonate, a cyclic ether, a chain ether, a nitrile, an amide, etc. One selected from these solvents may be used, or two or more may be used in combination.

[0119] Examples of lithium salts that can be used include lithium hexafluorophosphate (LiPF), lithium tetrafluoroborate (LiBF), lithium perchlorate (LiClO), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bisperfluoroethylsulfonylimide (LiN(SO2C2F5)2), LiAsF6, LiCF3SO3, and lithium difluoro(oxalato)borate. One selected from these electrolyte salts may be used, or two or more may be used in combination.

[0120] The electrolyte may further include a phosphate compound, such as TMSP. The electrolyte may be phosphorus-free.

[0121] It is usually desirable to interpose a separator between the positive electrode and the negative electrode. The separator 23 has high ion permeability and adequate mechanical strength and insulating properties. The separator 23 may be made of a microporous thin film, a woven fabric, a nonwoven fabric, or the like. The separator 23 may be made of a polymer, for example. The polymer may be a polyolefin such as polypropylene or polyethylene.

[0122] In the secondary battery of the present disclosure, the electrolyte may be impregnated into a polymer provided as a separator, for example, that is, the secondary battery of the present disclosure may have a structure in which the electrolyte and the polymer are used in combination.

[0123] The secondary battery of the present disclosure may further include a solid electrolyte as an electrolyte. That is, the secondary battery of the present disclosure may have a hybrid structure in which an electrolytic solution and a solid electrolyte are used in combination. Examples of solid electrolyte materials include halide solid electrolytes, sulfide solid electrolytes, oxide solid electrolytes, and organic polymer solid electrolytes. In the present disclosure, a "halide solid electrolyte" refers to a solid electrolyte containing a halogen element as the main anion component. A "sulfide solid electrolyte" refers to a solid electrolyte containing sulfur as the main anion component. An "oxide solid electrolyte" refers to a solid electrolyte containing oxygen as the main anion component. The "main anion component" refers to the anion with the largest substance amount among all the anions constituting the solid electrolyte. The secondary battery of the present disclosure may include a halide solid electrolyte.

[0124] In the present disclosure, as an example of the structure of a secondary battery according to embodiment 3, the configuration example shown in FIG. 4 is described, i.e., a secondary battery in which a stacked electrode group formed by stacking positive and negative electrodes with a separator interposed therebetween and an electrolyte solution are housed in an exterior body. However, the secondary battery according to the present disclosure is not limited to this configuration example. The secondary battery according to the present disclosure may have any shape, such as a cylindrical shape, a prismatic shape, a coin shape, a button shape, or a laminate shape. Furthermore, instead of a stacked electrode group in the secondary battery according to the present disclosure, an electrode group of another shape, such as an electrode group formed by winding positive and negative electrodes with a separator interposed therebetween, may be used.

[0125] The application of the coated active material and positive electrode of the present disclosure is not limited to the secondary battery 100. In addition to lithium secondary batteries, the coated active material and positive electrode of the present disclosure can be applied to various secondary batteries such as sodium secondary batteries and magnesium secondary batteries.

[0126] (Other Embodiments) (Additional Notes) The above description of the embodiments discloses the following techniques.

[0127] (Technology 1) A coated active material comprising: a positive electrode active material; a halogen-containing layer covering at least a portion of a surface of a particle of the positive electrode active material; and a phosphorus-containing layer covering at least a portion of a surface of the halogen-containing layer, wherein the halogen-containing layer is located between the surface of the particle and the phosphorus-containing layer, the halogen-containing layer contains a halide and is in contact with the surface of the particle, and the phosphorus-containing layer contains a phosphate compound.

[0128] This configuration makes it possible to suppress side reactions at the positive electrode while maintaining a sufficient discharge capacity of the battery.

[0129] (Technology 2) The coated active material according to Technology 1, wherein the halide has lithium ion conductivity. With this configuration, it is possible to suppress side reactions in the positive electrode while maintaining a sufficient discharge capacity of the battery.

[0130] (Technology 3) The coated active material according to Technology 1 or 2, wherein the halide contains Li, M1, M2, and F, wherein M1 is at least one selected from the group consisting of Ti and Nb, and M2 is at least one selected from the group consisting of Ca, Mg, Al, Y, and Zr. With this configuration, it is possible to suppress side reactions in the positive electrode while maintaining a sufficient discharge capacity of the battery.

[0131] (Technology 4) The halide has a composition represented by the following composition formula (IV): Li6-{5-x4-(5-m)y4}b4(Nb 1-x4-y4 Ti x4 M2 y4 ) b4 F6 ... Formula (IV) wherein M2 is at least one selected from the group consisting of Ca, Mg, Al, Y, and Zr, x4, y4, and b4 satisfy 0 < x4 < 1, 0 < y4 < 1, 0 < x4 + y4 ≦ 1, and 0.8 ≦ b4 ≦ 1.1, and m is the valence of M2. This configuration makes it possible to suppress side reactions in the positive electrode while maintaining a sufficient discharge capacity of the battery.

[0132] (Technology 5) The coated active material according to any one of Technologies 1 to 4, wherein the mass ratio of the halogen-containing layer to the positive electrode active material is 0.01% or more and 20% or less.

[0133] (Technology 6) The coated active material according to any one of Technologies 1 to 5, wherein the phosphate compound is an organic phosphorus compound. With this configuration, it is possible to suppress side reactions in the positive electrode while maintaining a sufficient discharge capacity of the battery.

[0134] (Technology 7) The coated active material according to any one of Technologies 1 to 6, wherein the phosphate compound contains a P-O-P bond. With this configuration, it is possible to suppress side reactions in the positive electrode while maintaining a sufficient discharge capacity of the battery.

[0135] (Technology 8) The coated active material according to any one of Technologies 1 to 7, wherein the phosphate compound includes a structure represented by chemical formula (1). In the chemical formula (1), n1 and n2 are each independently an integer of 0 or more, and R 1 , R 2 , R 4 , and R 5 are each independently -OR or -(CH2) m1 represents X1, and R 3 and R are each independently a direct bond to the halide, a hydrogen atom, -(CH2) m2 X2 represents a trimethylsilyl group or a triethylsilyl group, m1 represents an integer of 0 to 15, m2 represents a natural number of 1 to 3, X1 and X2 each independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxy group, a cyano group, or a fluorine atom, R 2 If there are multiple R 2 are independent of each other, and R 4 If there are multiple R 4 are independent of each other.

[0136] Because the phosphate compound has such a structure, it is relatively stable even under high voltage conditions, and therefore, even when the upper limit voltage of the battery is high, it can sufficiently suppress oxidative decomposition of the electrolyte and suppress side reactions such as metal elution from the positive electrode active material. Furthermore, the effect of suppressing side reactions can be maintained for a longer period of time.

[0137] (Technology 9) In the chemical formula (1), R 1 , R 2 , R 4 , and R 5 are each independently -OR, and R 3 and R each independently represent a direct bond to the halide, a hydrogen atom, or a trimethylsilyl group. According to this configuration, side reactions in the positive electrode can be further suppressed.

[0138] (Technology 10) The coated active material according to any one of Technologies 1 to 9, wherein the positive electrode active material contains lithium nickel oxide, and the proportion of Ni in the metal elements other than Li contained in the lithium nickel oxide is 50 atomic % or more. With this configuration, a high operating voltage of the battery can be achieved.

[0139] (Technology 11) A positive electrode comprising: a positive electrode current collector; and a positive electrode active material layer supported on the positive electrode current collector, wherein the positive electrode active material layer contains the coated active material according to any one of Technologies 1 to 10.

[0140] This configuration can suppress side reactions at the positive electrode, thereby improving the battery characteristics.

[0141] (Technology 12) A secondary battery comprising: the positive electrode according to Technology 11; a negative electrode; and an electrolyte.

[0142] This configuration can improve the characteristics of the secondary battery.

[0143] (Technology 13) A method for manufacturing a positive electrode including a positive electrode current collector and a positive electrode active material layer supported on the positive electrode current collector, the method satisfying at least one selected from the group consisting of (A) and (B) below: (A) forming a halogen-containing layer on at least a portion of the surface of particles of a positive electrode active material, forming the positive electrode active material layer containing the particles on the positive electrode current collector, contacting the positive electrode active material layer with a solution containing a phosphoric acid compound and a solvent, and drying the positive electrode active material layer after the contact; (B) forming a halogen-containing layer on at least a portion of the surface of particles of a positive electrode active material, contacting the particles with the halogen-containing layer formed thereon with a solution containing a phosphoric acid compound and a solvent, and drying the particles after the contact; and forming the positive electrode active material layer containing the dried particles on the positive electrode current collector.

[0144] According to the configuration of Technique 13, the positive electrode of the present disclosure can be produced efficiently.

[0145] (Technology 14) The method for producing a positive electrode according to Technology 13, further comprising washing the positive electrode active material layer after the contact with the solution and before the drying when the condition (A) is satisfied, and further comprising washing the particles after the contact with the solution and before the drying when the condition (B) is satisfied. This configuration makes it possible to produce a positive electrode that can further suppress side reactions such as oxidative decomposition of the electrolyte.

[0146] (Technology 15) The method for producing a positive electrode according to Technology 13 or 14, wherein the halogen-containing layer is formed by a mechanochemical method. With this configuration, the positive electrode of the present disclosure can be produced efficiently.

[0147] (Technology 16) The method for producing a positive electrode according to any one of Techniques 13 to 15, wherein the phosphate compound includes a structure represented by chemical formula (2). In chemical formula (2), R 7 is a hydrogen atom, -(CH2) k1 Y1 represents a trimethylsilyl group or a triethylsilyl group; R 6 and R 8are each independently -OR or -(CH2) k2 Y2, R is a hydrogen atom, -(CH2) k3 Y3 represents a trimethylsilyl group or a triethylsilyl group; k1 and k3 each independently represent a natural number from 1 to 3; k2 is an integer from 0 to 15; and Y1, Y2, and Y3 each independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxy group, a cyano group, or a fluorine atom.

[0148] When the phosphate compound has such a structure, it is possible to efficiently produce a positive electrode that can sufficiently suppress oxidative decomposition of the electrolyte and suppress side reactions such as metal elution from the positive electrode active material, even when the upper limit voltage is high.

[0149] (Technology 17) The method for producing a positive electrode according to any one of Techniques 13 to 16, wherein the phosphate compound includes tristrimethylsilyl phosphate. With this configuration, a positive electrode in which side reactions are suppressed while maintaining a sufficient discharge capacity of the battery can be produced more efficiently.

[0150] (Technology 18) The method for producing a positive electrode according to any one of Techniques 13 to 17, wherein a mass ratio of P contained in the phosphate compound to the positive electrode active material is 0.1% or more. With this configuration, a positive electrode in which side reactions are suppressed while maintaining a sufficient discharge capacity of the battery can be produced.

[0151] The present disclosure will be described in more detail below using examples. The following examples are merely examples of embodiments, and are not intended to limit the scope of the present disclosure.

[0152] (Example 1) In an argon glove box with a dew point of -60°C or less, raw material powders LiF, TiF4, and AlF3 were weighed in a molar ratio of LiF:TiF4:AlF3 = 3:0.33:0.67. These were pulverized and mixed in a mortar to obtain a mixture. The obtained mixed powder was milled for 12 hours at 500 rpm using a planetary ball mill. In this way, halide powder was obtained. The halide was Li, 2.7 Ti 0.3 Al 0.7F6 (hereinafter referred to as "LTAF").

[0153] LiNi 0.8 Mn 0.2 A powder of a positive electrode active material having a composition of O2 and LTAF were weighed to a mass ratio of positive electrode active material:LTAF = 100:3. These materials were placed in a dry particle compositing apparatus (Nobilta, manufactured by Hosokawa Micron Co., Ltd.) and subjected to compositing treatment at 6000 rpm for 30 minutes. The temperature inside the apparatus was maintained below 20°C. In this way, a positive electrode active material coated with LTAF was obtained.

[0154] The positive electrode active material coated with LTAF, acetylene black (AB), and polyvinylidene fluoride (PVDF) were mixed with N-methyl-2-pyrrolidone (NMP) and stirred to prepare a positive electrode slurry. The mass ratio of these materials in the positive electrode active material layer was positive electrode active material:AB:PVDF=96:2:2.

[0155] The positive electrode slurry was applied to the surface of an aluminum foil (1.45 cm × 1.45 cm), the coating was dried, and then rolled to form a positive electrode active material layer. In this way, an electrode plate in which the positive electrode active material layer was supported on the positive electrode current collector was obtained.

[0156] A 0.2% by mass TMSP solution was prepared by adding tristrimethylsilyl phosphate (TMSP) to a mixed solvent of dimethyl carbonate (DMC) and ethanol (EtOH) in a volume ratio of 90:10.

[0157] The electrode plate was immersed in 200 μL of TMSP solution. After immersion for 1 hour, the electrode plate was removed and washed twice with DMC. The washed electrode plate was placed in a desiccator and dried under vacuum for 5 minutes. In this way, a phosphorus-containing layer was formed.

[0158] This resulted in the production of the positive electrode of Example 1. The positive electrode thus produced contained a coated active material provided, at least near the surface thereof, with a halogen-containing layer covering the particle surface of the positive electrode active material and a phosphorus-containing layer covering at least a portion of the surface of the halogen-containing layer.

[0159] A laminate half-cell was fabricated as an evaluation cell for Example 1 using the positive electrode, Li metal foil as a counter electrode, a separator, and an electrolyte solution from Example 1. A PP / PE / PP separator was used as the separator. The concentration of LiPF6 in the electrolyte solution was 1.35 mol / L. The solvent for the electrolyte solution contained ethylene carbonate (EC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), and DMC in a volume ratio of EC:FEC:EMC:DMC = 10:10:5:75. The volume of the electrolyte solution was 150 μL.

[0160] (Example 2) In forming the phosphorus-containing layer, the TMSP concentration in the TMSP solution was set to 2 mass %. Except for the above, a positive electrode of Example 2 was fabricated in the same manner as in Example 1. Using the positive electrode of Example 2, an evaluation cell of Example 2 was fabricated in the same manner as in Example 1.

[0161] (Comparative Example 1) LiNi 0.8 Mn 0.2 A positive electrode slurry was prepared by adding N-methyl-2-pyrrolidone (NMP) to a positive electrode active material having a composition of O, acetylene black (AB), and polyvinylidene fluoride (PVDF). The mass ratio of these materials in the positive electrode active material layer was positive electrode active material:AB:PVDF=96:2:2.

[0162] The positive electrode slurry was applied to the surface of an aluminum foil (1.45 cm x 1.45 cm), the coating was dried, and then rolled to form a positive electrode active material layer. In this manner, the positive electrode of Comparative Example 1 was produced. That is, the positive electrode of Comparative Example 1 did not include a coated active material having a halogen-containing layer and a phosphorus-containing layer.

[0163] An evaluation cell for Comparative Example 1 was fabricated in the same manner as in Example 1 using the positive electrode of Comparative Example 1.

[0164] (Comparative Example 2) LiNi was used in the same manner as in Example 1. 0.8 Mn 0.2The surface of a positive electrode active material having a composition of O was coated with LTAF. Using the positive electrode active material coated with LTAF, a positive electrode active material layer was formed on a positive electrode current collector in the same manner as in Comparative Example 1. In this manner, a positive electrode of Comparative Example 2 was produced.

[0165] An evaluation cell for Comparative Example 2 was fabricated in the same manner as in Example 1 using the positive electrode of Comparative Example 2.

[0166] (Comparative Example 3) LiNi 0.8 Mn 0.2 A positive electrode slurry was prepared by adding N-methyl-2-pyrrolidone (NMP) to a positive electrode active material having a composition of O, acetylene black (AB), and polyvinylidene fluoride (PVDF). The mass ratio of these materials in the positive electrode active material layer was positive electrode active material:AB:PVDF=96:2:2.

[0167] The positive electrode slurry was applied to the surface of an aluminum foil (1.45 cm × 1.45 cm), the coating was dried, and then rolled to form a positive electrode active material layer. In this way, an electrode plate in which the positive electrode active material layer was supported on the positive electrode current collector was obtained.

[0168] The electrode plate was immersed in a TMSP solution, washed with DMC, and then vacuum dried in the same manner as in Example 1. In this way, a positive electrode of Comparative Example 3 was obtained.

[0169] An evaluation cell for Comparative Example 3 was fabricated in the same manner as in Example 1 using the positive electrode of Comparative Example 3.

[0170] (Comparative Example 4) LiNi 0.8 Mn 0.2 A positive electrode slurry was prepared by adding N-methyl-2-pyrrolidone (NMP) to a positive electrode active material having a composition of O, acetylene black (AB), and polyvinylidene fluoride (PVDF). The mass ratio of these materials in the positive electrode active material layer was positive electrode active material:AB:PVDF=96:2:2.

[0171] The positive electrode slurry was applied to the surface of an aluminum foil (1.45 cm × 1.45 cm), the coating was dried, and then rolled to form a positive electrode active material layer. In this way, an electrode plate in which the positive electrode active material layer was supported on the positive electrode current collector was obtained.

[0172] The electrode plate was immersed in a TMSP solution, washed with DMC, and then vacuum dried in the same manner as in Example 2. This gave a positive electrode of Comparative Example 4. That is, the positive electrode of Comparative Example 4 was obtained in the same manner as in Comparative Example 1, except that the concentration of the TMSP solution was 2 mass%.

[0173] An evaluation cell of Comparative Example 4 was fabricated in the same manner as in Example 1 using the positive electrode of Comparative Example 4.

[0174] [Charge / Discharge Test] The evaluation cells of Examples 1 and 2 and Comparative Examples 1 to 4 were charged at a constant current of 0.2 C at an ambient temperature of 25°C until the voltage reached 4.5 V, and then charged at a constant voltage of 4.5 V. Charging was terminated at a current of 0.02 C. After a 20-minute pause, constant current discharge was performed at a current of 0.2 C until the voltage reached 2.5 V, and then a 20-minute pause was performed. The above charge / discharge cycle was repeated twice. The initial discharge capacity was evaluated.

[0175] The cells that had undergone the above charge and discharge were then changed to an ambient temperature of 55°C. These cells were then subjected to constant current charging at a current value of 0.2 C until the voltage reached 4.5 V (hereinafter referred to as "first charging"), and the charge capacity was confirmed. Next, charging was performed at an ambient temperature of 55°C, maintaining a voltage of 4.5 V for 72 hours (hereinafter referred to as "second charging"). Thereafter, constant current discharging was performed at a current value of 0.2 C until the voltage reached 2.5 V, and the discharge capacity was confirmed.

[0176] The evaluation results of the charge-discharge test are shown in Table 1. In Table 1, the capacity X is calculated using the formula: X = (C1 + C2) - D1, where C1 is the charge capacity in the first charge, C2 is the amount of further charge in the second charge, and D1 is the discharge capacity in the constant-current discharge after the second charge. In other words, the value of capacity X corresponds to the amount of current that flowed in excess of the original battery capacity during the second charge. This current is thought to be due to a side reaction, such as metal elution from the positive electrode active material, that occurred during the second charge. Therefore, capacity X correlates with the amount of side reaction.

[0177]

[0178] (Discussion) Examples 1 and 2 had sufficient initial discharge capacities of 206 mAh / g or more, and small capacity X values ​​of 15.00 mAh / g or less. In Examples 1 and 2, the capacity X values ​​were significantly reduced without a significant decrease in discharge capacity compared to Comparative Example 1, in which the positive electrode active material was not coated. In Examples 1 and 2, the initial discharge capacity was larger and the capacity X values ​​were reduced compared to Comparative Example 2, in which a coated active material having only a halogen-containing layer was used. In Examples 1 and 2, the capacity X values ​​were reduced without a significant decrease in discharge capacity compared to Comparative Example 3, in which a coated active material having only a phosphorus-containing layer formed with a 0.2 mass% TMSP solution was used. In Comparative Example 4, in which a coated active material having only a phosphorus-containing layer formed with a 2 mass% TMSP solution was used, the capacity X values ​​were relatively small but the discharge capacity was insufficient. On the other hand, in Example 2, in which a phosphorus-containing layer was formed with a 2 mass% TMSP solution like Comparative Example 4, the discharge capacity was almost unchanged and the capacity X values ​​were suppressed compared to Example 1. From the above, in Examples 1 and 2, side reactions were suppressed while maintaining a sufficient initial discharge capacity. This is because the phosphorus-containing layer suppresses side reactions that occur due to contact between the positive electrode active material and the electrolyte, while the halogen-containing layer suppresses deterioration of the positive electrode active material that occurs due to contact between the phosphate compound and the positive electrode active material. Therefore, similar effects can be obtained even when substances different from those used in the Examples are used as the positive electrode active material, halide, and phosphate compound. In batteries using coated active materials with a halogen-containing layer and a phosphorus-containing layer, adjusting the TMSP concentration allowed for further suppression of side reactions without significantly reducing the initial discharge capacity.

[0179] The technology of the present disclosure is useful for secondary batteries used as power sources for mobile communication devices, portable electronic devices, electric vehicles, and the like.

Claims

1. A coated active material comprising a positive electrode active material, a halogen-containing layer covering at least a part of the surface of the particles of the positive electrode active material, and a phosphorus-containing layer covering at least a part of the surface of the halogen-containing layer, wherein the halogen-containing layer is located between the surface of the particles and the phosphorus-containing layer, the halogen-containing layer contains a halide and is in contact with the surface of the particles, and the phosphorus-containing layer contains a phosphate compound.

2. The coated active material according to claim 1, wherein the halide has lithium ion conductivity.

3. The coated active material according to claim 1, wherein the halide contains Li, M1, M2, and F, M1 is at least one selected from the group consisting of Ti and Nb, and M2 is at least one selected from the group consisting of Ca, Mg, Al, Y, and Zr.

4. The halide has a composition represented by the following compositional formula (IV): Li6-{5-x4-(5-m)y4}b4(Nb 1-x4-y4 Ti x4 M2 y4 ) b4 F6 ··· Formula (IV) Here, M2 is at least one selected from the group consisting of Ca, Mg, Al, Y, and Zr, and x4, y4, and b4 satisfy 0 < x4 < 1, 0 < y4 < 1, 0 < x4 + y4 ≦ 1, and 0.8 ≦ b4 ≦ 1.1, and m is the valence of M2. The coated active material according to claim 1.

5. The coated active material according to claim 1, wherein the mass ratio of the halogen-containing layer to the positive electrode active material is 0.01% or more and 20% or less.

6. The coated active material according to claim 1, wherein the phosphate compound is an organic phosphorus compound.

7. The coated active material according to claim 1, wherein the phosphate compound contains a P—O—P bond.

8. The phosphate compound contains a structure represented by Chemical Formula (1), and is the coating active material according to Claim 1. n1 and n2 are each independently an integer of 0 or more, and R 1 , R 2 , R 4 , and R 5 each independently represent -OR or -(CH2) m1 X1; R 3 and R each independently represent a direct bond with the halide, a hydrogen atom, -(CH2) m2 X2, a trimethylsilyl group, or a triethylsilyl group; m1 is an integer from 0 to 15; m2 is a natural number from 1 to 3; X1 and X2 each independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxy group, a cyano group, or a fluorine atom; when there are a plurality of R 2 , the plurality of R 2 are independent of each other; when there are a plurality of R 4 , the plurality of R 4 are independent of each other.

9. In the chemical formula (1), R 1 , R 2 , R 4 , and R 5 each independently represent -OR, and R 3 and R each independently represent a direct bond with the halide, a hydrogen atom, or a trimethylsilyl group. The coating active material according to claim 8.

10. The coated active material according to claim 1, wherein the positive electrode active material contains lithium nickel oxide, and the proportion of Ni in the metal elements other than Li contained in the lithium nickel oxide is 50 atomic% or more.

11. A positive electrode comprising a positive electrode current collector and a positive electrode active material layer supported on the positive electrode current collector, wherein the positive electrode active material layer contains the coated active material according to any one of claims 1 to 10.

12. A secondary battery comprising the positive electrode according to claim 11, a negative electrode, and an electrolyte.

13. A method for manufacturing a positive electrode including a positive electrode current collector and a positive electrode active material layer supported on the positive electrode current collector, the method for manufacturing a positive electrode satisfying at least one selected from the group consisting of the following (A) and (B). (A) Forming a halogen-containing layer on at least a part of the surface of the particles of the positive electrode active material; forming the positive electrode active material layer containing the particles on the positive electrode current collector; bringing a solution containing a phosphate compound and a solvent into contact with the positive electrode active material layer; and drying the positive electrode active material layer after the contact. (B) Forming a halogen-containing layer on at least a part of the surface of the particles of the positive electrode active material; bringing a solution containing a phosphate compound and a solvent into contact with the particles having the halogen-containing layer formed thereon; drying the particles after the contact; and forming the positive electrode active material layer containing the dried particles on the positive electrode current collector.

14. When satisfying (A), the method for manufacturing a positive electrode according to claim 13 further includes washing the positive electrode active material layer after the contact of the solution and before the drying. When satisfying (B), the method for manufacturing a positive electrode according to claim 13 further includes washing the particles after the contact of the solution and before the drying.

15. The method for manufacturing a positive electrode according to claim 13, wherein the halogen-containing layer is formed by a mechanochemical method.

16. The method for manufacturing a positive electrode according to claim 13, wherein the phosphate compound contains a structure represented by chemical formula (2). R 7 represents a hydrogen atom, -(CH2) k1 Y1, a trimethylsilyl group, or a triethylsilyl group, and R 6 and R 8 each independently represent -OR or -(CH2) k2 Y2, and R represents a hydrogen atom, -(CH2) k3 Y3, a trimethylsilyl group, or a triethylsilyl group, k1 and k3 are each independently a natural number from 1 to 3, k2 is an integer from 0 to 15, and Y1, Y2, and Y3 each independently represent a hydrogen atom, a hydroxyl group, an amino group, a carboxy group, a cyano group, or a fluorine atom.

17. The method for manufacturing a positive electrode according to claim 13, wherein the phosphate compound includes tris(trimethylsilyl) phosphate.

18. The mass ratio of P contained in the phosphate compound to the positive electrode active material is 0.1% or more, and the method for manufacturing a positive electrode according to claim 13.

Citation Information

Patent Citations

  • Nonaqueous electrolytic solution, nonaqueous electrolyte secondary battery, battery pack, electronic device, electric vehicle, power storage device, and electric power system

    JP2013055031A

  • Battery, battery pack, electronic device, electrically-powered vehicle, power storage device and electric power system

    JP2013152825A

  • Positive electrode active material for lithium secondary cell, positive electrode for lithium secondary cell, lithium secondary cell, and methods for manufacturing same

    WO2017126276A1

  • Positive electrode material, and battery

    WO2021187391A1

  • Positive electrode active material particles comprising a core containing lithium cobalt oxide and a shell containing lithium cobalt phosphate, and method for producing the same

    JP2019523978A

Cited By

  • Modified ternary positive electrode material and preparation method thereof, positive electrode plate and lithium battery

    CN120184219A

  • Modified ternary positive electrode material, preparation method therefor, positive electrode sheet, and lithium battery

    WO2026218423A1