Polyester fiber, method for producing same, and fiber structure
By controlling the cross-sectional area and circularity of ultrafine polyester fibers through precise spinning and stretching processes, the challenges of dispersibility and surface smoothness in wet-laid nonwoven fabrics are addressed, achieving improved fiber performance and fabric quality.
Patent Information
- Application Number
- PCT/JP2024/018632
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-05-21
- Publication Date
- 2024-11-28
AI Technical Summary
Existing methods for producing ultrafine polyester fibers struggle with achieving good dispersibility regardless of fiber aspect ratio and producing wet-laid nonwoven fabrics with improved surface smoothness, due to limitations in fiber diameter variation and manufacturing instability of sea-island type composite fibers.
The production of ultrafine polyester fibers with controlled cross-sectional area and circularity, achieved through specific spinning and stretching processes, including flow stretching and necking stretching with low drawing tension, to ensure uniformity and reduce outliers in fiber diameter, resulting in fibers with improved dispersibility and surface smoothness of wet-laid nonwoven fabrics.
The approach results in ultrafine polyester fibers that exhibit excellent dispersibility and produce wet-laid nonwoven fabrics with enhanced surface smoothness and pore size uniformity, addressing the limitations of previous methods by maintaining low stretching tension and optimizing fiber cross-sectional characteristics.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Polyester fiber, its manufacturing method, and fiber structure Related Applications
[0001] This application claims priority to Japanese Patent Application No. 2023-084700 filed on May 23, 2023 in Japan, and Japanese Patent Application No. 2023-084701 filed on May 23, 2023 in Japan, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to ultrafine polyester fibers that can be used as fibers for papermaking, etc., a method for producing the same, and a fiber structure containing the polyester fibers.
[0003] Conventionally, cellulosic fibers such as pulp and rayon, polypropylene fibers, polyacrylonitrile fibers, polyvinyl alcohol fibers, etc. have been used as fibers for papermaking. However, in recent years, paper-like products made by a papermaking method using polyester fibers as part or all of the raw material have come to be widely used because of their excellent physical properties such as mechanical properties, electrical properties, heat resistance, dimensional stability, and hydrophobicity.
[0004] Fibers for papermaking are widely used in industrial materials such as filters, and recently, ultrafine fibers have been used in response to demands for improved flexibility, density, and thinness. For example, Patent Document 1 (Japanese Patent No. 6022054) discloses organic resin non-crimped staple fibers for wetlaid nonwoven fabrics, which have a fineness of 0.0001 to 0.6 decitex, a fiber length of 1.0 to 5.0 millimeters, a moisture regain of 10 to 100% by weight, a cut end coefficient of 1.00 to 1.07, and a relative coefficient of variation (CV%) of fiber length of 0.0 to 15.0%.
[0005] Furthermore, Patent Document 2 (JP 2012-92458 A) discloses ultrafine fibers for binders made of a thermoplastic resin, having an average fiber diameter of 10 to 2000 nm, a fiber diameter variation coefficient of 0 to 25%, and a crystallinity of 20% or less.
[0006] Patent Document 3 (JP 2012-193476 A) discloses polyester ultrafine fibers characterized by a single filament fiber diameter of 10 to 1,000 nm, a single filament fiber diameter variation (CV%) of 0 to 25%, a tensile strength as an ultrafine fiber bundle of 4.0 cN / dtex or more, a breaking elongation of 10 to 80%, and a dry heat shrinkage rate at 150°C of 5% or less.
[0007] Japanese Patent No. 6022054 Japanese Patent Application Laid-Open No. 2012-92458 Japanese Patent Application Laid-Open No. 2012-193476
[0008] However, although Patent Document 1 measures dispersibility, it states that as the aspect ratio of the fibers (the ratio of fiber length to fiber diameter) increases, entanglement of the fibers becomes more likely, and taking this into consideration, dispersibility is evaluated by changing the aspect ratio according to the fiber fineness. Therefore, Patent Document 1 does not mention improving fiber dispersibility regardless of the aspect ratio. Furthermore, Patent Document 1 does not actually produce a wetlaid nonwoven fabric using organic resin non-crimped staple fiber, and does not mention evaluation of the wetlaid nonwoven fabric.
[0009] Patent Document 2 describes that a uniform fiber diameter allows for uniform dispersion among the subject fibers during papermaking, while Patent Documents 2 and 3 describe fiber diameter variation. However, Patent Documents 2 and 3 describe the production of ultrafine fibers by removing the sea component from an islands-in-sea composite fiber with a multi-island structure. In such a production method, the flow of the island component polymer, which has been divided into countless pieces and ultrafinely divided, is very unstable. Since two types of polymers with different fluidities (viscosities) are composited, for example, even a slight fluctuation when inserting the island component polymer from the tips of multiple island component pipes in the spinneret into the sea component may cause the island component polymers to not enter the desired positions, resulting in adjacent island component polymers merging and becoming coarse, making it impossible to obtain a desired cross section. In other words, the production conditions, such as the polymer combination and sea-island component ratio, are extremely limited, and there is a limit to the improvement in fiber diameter variation.
[0010] Therefore, an object of the present invention is to provide ultrafine polyester fibers that can exhibit good dispersibility regardless of the aspect ratio of the fibers.
[0011] Another object of the present invention is to provide ultrafine polyester fibers that can be used to produce wetlaid nonwoven fabrics with improved surface smoothness.
[0012] As a result of intensive research to achieve the above-mentioned object, the inventors of the present invention found that, since the cross section of a single yarn of an ultrafine polyester fiber is very small, even slight differences in size and shape have a significant effect on the performance of the fiber, by adjusting the fiber cross section of the ultrafine polyester fiber, it is possible to achieve excellent dispersibility even when the aspect ratio of the fiber is large, and to improve the surface smoothness of a wetlaid nonwoven fabric obtained using such a fiber, and thus completed the present invention.
[0013] That is, the present invention can be configured in the following aspects: [Aspect 1] An average cross-sectional area (x) calculated from cross-sectional area data of a single yarn is 1 to 40 μm 2 (preferably 2 to 35 μm 2 , more preferably 5 to 30 μm 2 ) and the standard deviation (σ) of the cross-sectional area is 10 μm 2 less than (preferably 8 μm 2 Less than 7 μm, more preferably 2A polyester fiber according to Aspect 1, wherein the coefficient of variation of the cross-sectional area calculated from the cross-sectional area data of a single yarn is 50% or less (preferably 45% or less, more preferably 40% or less, and even more preferably 36% or less). [Aspect 3] A polyester fiber according to Aspect 1 or 2, wherein the average fiber diameter of a single yarn is 1 to 10 μm (preferably 1.5 to 9 μm, and more preferably 2 to 8 μm), and the circularity of the fiber cross section is 0.90 to 1.00 (preferably 0.91 to 1.00, more preferably 0.92 to 1.00, and even more preferably 0.93 to 1.00). [Aspect 4] The polyester fiber according to aspect 3, wherein the coefficient of variation of the circularity of the fiber cross section is 7% or less (preferably 6% or less, more preferably 5% or less, and even more preferably 4% or less). [Aspect 5] A polyester fiber having an average fiber diameter of a single yarn of 1 to 10 μm (preferably 1.5 to 9 μm, and more preferably 2 to 8 μm) and a circularity of the fiber cross section of 0.90 to 1.00 (preferably 0.91 to 1.00, more preferably 0.92 to 1.00, and even more preferably 0.93 to 1.00). [Aspect 6] The polyester fiber according to aspect 5, wherein the coefficient of variation of the circularity of the fiber cross section is 7% or less (preferably 6% or less, more preferably 5% or less, and even more preferably 4% or less). [Aspect 7] The polyester fiber according to any one of aspects 1 to 6, wherein the average fiber length is 0.1 to 110 mm (preferably 0.5 to 50 mm, and more preferably 1 to 20 mm). [Aspect 8] The polyester fiber according to any one of Aspects 1 to 7, having an aspect ratio of 100 or more (preferably 300 to 10,000, more preferably 500 to 3,000). [Aspect 9] A fiber structure comprising the polyester fiber according to any one of Aspects 1 to 8. [Aspect 10] The fiber structure according to Aspect 9, which is a wetlaid nonwoven fabric.[Aspect 11] A method for producing the polyester fiber according to any one of Aspects 1 to 8, comprising: a spinning step of melt-spinning a resin material containing a polyester-based resin; and a drawing step of drawing the fiber obtained by the spinning step, wherein the drawing step comprises flow drawing and subsequent necking drawing, and the drawing tension in at least the flow drawing is 0.01 cN / dtex or less (preferably 0.009 cN / dtex or less, more preferably 0.008 cN / dtex or less).
[0014] As used herein, the singular forms "a," "an," and "the" are intended to include the plural forms, including "at least one," unless the content clearly dictates otherwise. As used herein, the terms "and / or," "at least one," and "one or more" include any and all combinations of the associated listed items.
[0015] It should be noted that any combination of at least two elements disclosed in the claims and / or the specification is included in the present invention, and in particular any combination of two or more of the claims described in the claims is included in the present invention.
[0016] The polyester fibers of the present invention can have good dispersibility regardless of the aspect ratio of the fibers, and such fibers are useful for producing wetlaid nonwoven fabrics with improved surface smoothness.
[0017] [Polyester Fiber] The polyester fiber according to the first aspect of the present invention has an average cross-sectional area (x) of 1 to 40 μm calculated from the cross-sectional area data of a single yarn. 2 and the standard deviation (σ) of the cross-sectional area is 10 μm 2 or less, and the ratio (Ao / Ai) of the total value Ao of the cross-sectional areas of the data outside the range of x±2.5σ to the total value Ai of the cross-sectional areas of the data within the range of x±2.5σ is 10% or less.
[0018] In the present invention, since ultrafine polyester fibers have extremely small fiber cross sections, differences in size are expected to have a significant effect on fiber performance, and therefore, instead of fiber diameter, attention was focused on cross-sectional area, which can more clearly distinguish the difference. It was then discovered that the distribution of the cross-sectional area of single yarns has a significant effect on fiber dispersibility and the surface smoothness of wetlaid nonwoven fabrics produced using such fibers.
[0019] In this specification, the term "fiber cross section" refers to a cross section perpendicular to the fiber axis direction, and the cross-sectional area data for a single yarn is measured by the method described in the Examples below and is data on the measured cross-sectional areas of 250 single yarns. The average cross-sectional area (x) and standard deviation (σ) represent the average value and standard deviation, respectively, of the cross-sectional area data for a single yarn. Ai represents the total cross-sectional area of all data within the range of x±2.5σ (i.e., a range of 5 times the standard deviation (σ) centered on the average cross-sectional area (x); x-2.5σ or more and x+2.5σ or less), and Ao represents the total cross-sectional area of all data outside the range of x±2.5σ. The ratio of Ao to Ai (Ao / Ai) represents a numerical value expressed as a percentage obtained by dividing Ao by Ai (i.e., a numerical value calculated by dividing Ao by Ai and multiplying by 100). This is an index showing the extent to which cross-sectional area data (outliers) outside the range of x±2.5σ deviate from the average cross-sectional area, and the number of such numerical values present. In the present invention, by using the range of x±2.5σ as a standard, relatively small cross-sectional area data can be placed within this range, and outliers can be set to a range mainly consisting of cross-sectional area data larger than the upper limit value, so that the numerical value of Ao becomes a numerical value that can mainly identify single yarns with unusually large cross-sectional areas. Furthermore, since the coefficient of variation (CV value) of the fiber diameter of a single yarn as in Patent Documents 2 and 3 cannot identify the presence of outliers in the cross-sectional area data of a single yarn, the present invention uses the ratio of Ao to Ai (Ao / Ai) as an index for identifying the presence of single yarns with unusually large cross-sectional areas.
[0020] In ultrafine polyester fibers, when there are many single yarns having a cross-sectional area outside the range of x±2.5σ where x is the average cross-sectional area and σ is the standard deviation of the cross-sectional area, when the fibers are dispersed in water, the single yarns having a cross-sectional area larger than x+2.5σ act as nuclei to cause entanglement, resulting in a deterioration in the surface smoothness of the resulting wetlaid nonwoven fabric. Therefore, in the present invention, the dispersibility can be improved by adjusting the ultrafine polyester fibers to reduce the number of such thick single yarns, and by making the ratio (Ao / Ai) of the total cross-sectional areas Ao of the data outside the range of x±2.5σ to the total cross-sectional areas Ai of the data within x±2.5σ to be 10% or less. It has been found that this makes it possible to improve the dispersibility and to improve the surface smoothness of wetlaid nonwoven fabrics obtained using such fibers.
[0021] The average cross-sectional area (x) of the polyester fiber in the first aspect of the present invention is 1 to 40 μm from the viewpoint of improving the dispersibility of the fiber. 2 and preferably 2 to 35 μm 2 , more preferably 5 to 30 μm 2 may be.
[0022] The standard deviation (σ) of the cross-sectional area of the polyester fiber in the first aspect of the present invention is 10 μm or less from the viewpoint of improving the surface smoothness of the obtained wetlaid nonwoven fabric. 2 less than or equal to 8 μm, preferably 2 Less than 7 μm, more preferably 2 The lower limit of the standard deviation of the cross-sectional area is not particularly limited, but may be, for example, 1 μm 2 It may be to some extent.
[0023] In the first aspect of the present invention, the ratio of Ao to Ai of the polyester fiber (Ao / Ai) may be 10% or less, preferably 8% or less, and more preferably 6% or less, from the viewpoint of improving the dispersibility of the fiber and the surface smoothness of the obtained wetlaid nonwoven fabric. The lower limit of Ao / Ai is not particularly limited, but may be, for example, about 0.1%.
[0024] In the polyester fiber according to the first aspect of the present invention, from the viewpoint of improving the surface smoothness and pore size uniformity of the resulting wetlaid nonwoven fabric, the coefficient of variation of the cross-sectional area calculated from the cross-sectional area data of single yarns may be 50% or less, preferably 45% or less, more preferably 40% or less, and even more preferably 36% or less. The lower limit of the coefficient of variation of the cross-sectional area is not particularly limited, but may be, for example, about 0.1%. In this specification, the coefficient of variation of the cross-sectional area can be calculated by the standard deviation of the cross-sectional area (σ) / average cross-sectional area (x)×100.
[0025] The polyester fiber in the second embodiment of the present invention has an average fiber diameter of a single yarn of 1 to 10 μm and a circularity of the fiber cross section of 0.90 to 1.00.
[0026] In the case of ultrafine fibers, the fiber cross section is very small, and even slight differences in the circularity of the fiber cross section significantly affect the fiber shape, which may affect the dispersibility of the fibers. Furthermore, the circularity of the fiber cross section also affects the surface smoothness of the wetlaid nonwoven fabric produced using the fibers. Therefore, the present invention has discovered that by adjusting the fiber cross section of ultrafine polyester fibers to be closer to a perfect circle, it is possible to achieve excellent dispersibility even when the fiber aspect ratio is large, and to improve the surface smoothness of the wetlaid nonwoven fabric produced using such fibers.
[0027] The average fiber diameter of a single yarn of the polyester fiber in the second aspect of the present invention may be preferably 1.5 to 9 μm, more preferably 2 to 8 μm. In this specification, the average fiber diameter of a single yarn means the average value of the circumscribed circle diameter (i.e., the maximum diameter) of the fiber cross section, and is a value measured by the method described in the examples below.
[0028] The lower limit of the circularity of the cross section of the polyester fiber in the second aspect of the present invention may be preferably 0.91 or more, more preferably 0.92 or more, and even more preferably 0.93 or more. The closer the fiber cross section is to a perfect circle, the better. There is no particular limitation on the upper limit of the circularity, but it may be, for example, 0.99 or less, or 0.98 or less. In this specification, the circularity of the fiber cross section is the ratio of the maximum diameter to the minimum diameter (minimum diameter / maximum diameter) of the cross section perpendicular to the fiber axis direction, and is a value measured by the method described in the Examples below.
[0029] In the polyester fiber according to the second aspect of the present invention, from the viewpoint of improving the surface smoothness and pore size uniformity of the resulting wetlaid nonwoven fabric, the coefficient of variation of the circularity of the fiber cross section may be 7% or less, preferably 6% or less, more preferably 5% or less, and even more preferably 4% or less. The lower limit of the coefficient of variation of the circularity of the fiber cross section is not particularly limited, but may be, for example, about 0.1%. In this specification, the coefficient of variation of the circularity of the fiber cross section can be calculated by dividing the standard deviation of the circularity by the average value of the circularity, and is a value measured by the method described in the Examples below.
[0030] The polyester fiber according to the first aspect of the present invention may have the configuration of the polyester fiber according to the second aspect. For example, the polyester fiber according to the present invention may have an average cross-sectional area (x) of 1 to 40 μm, calculated from the cross-sectional area data of a single yarn. 2 and the standard deviation (σ) of the cross-sectional area is 10 μm 2 or less, the ratio (Ao / Ai) of the sum of the cross-sectional areas Ao of the data outside the range of x±2.5σ to the sum of the cross-sectional areas Ai of the data within the range of x±2.5σ may be 10% or less, the average fiber diameter of the single yarn may be 1 to 10 μm, and the circularity of the fiber cross section may be 0.90 to 1.00.
[0031] The polyester fiber of the present invention may be a non-composite fiber or a solid fiber.
[0032] The polyester fibers of the present invention may be short fibers depending on the type of fiber structure, etc., and may have, for example, an average fiber length of 0.1 to 110 mm, preferably 0.5 to 50 mm, and more preferably 1 to 20 mm. When producing a paper-like material, which is an example of a wetlaid nonwoven fabric, the average fiber length of the polyester fibers may be preferably 0.1 to 50 mm, more preferably 0.5 to 25 mm, and even more preferably 1 to 20 mm, from the viewpoint of improving the processability of the production process and the physical properties of the resulting paper-like material, such as strength. Furthermore, in the production of drylaid nonwoven fabrics using a carding machine or the like, a web composed of fibers must pass through the line continuously without breaking in the direction of travel. Therefore, the average fiber length of the polyester fibers used in the production of drylaid nonwoven fabrics may be preferably 10 to 110 mm, more preferably 15 to 100 mm, and even more preferably 20 to 90 mm. In this specification, the average fiber length is a value measured by the method described in the Examples below.
[0033] The polyester fiber of the present invention may have an aspect ratio of 100 or more, preferably 300 to 10,000, and more preferably 500 to 3,000. In this specification, the aspect ratio means the ratio of the average fiber length to the average fiber diameter (average fiber length / average fiber diameter).
[0034] The polyester fiber of the present invention is made of a polyester-based resin, which is a polycondensate of a dicarboxylic acid and a diol, and examples of the dicarboxylic acid include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, and 4,4'-biphenyldicarboxylic acid, and aliphatic dicarboxylic acids such as azelaic acid and sebacic acid, and examples of the diol include aliphatic diols such as ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, polyethylene glycol, and polytetramethylene glycol, aromatic diols such as ethylene oxide adducts of bisphenol A or bisphenol S, and alicyclic diols such as cyclohexanedimethanol.
[0035] The polyester resin constituting the polyester fiber of the present invention is preferably a polyester resin containing an aromatic dicarboxylic acid as the main dicarboxylic acid component, such as polyethylene terephthalate, polytrimethylene terephthalate, polytetramethylene terephthalate, polycyclohexanedimethylene terephthalate, polyethylene naphthalate, or polytetramethylene terephthalate. These polyester resins may be copolymers in which another diol or another dicarboxylic acid such as isophthalic acid is copolymerized as a third component. Among these, polyethylene terephthalate is more preferred.
[0036] The polyester fiber of the present invention may contain a thermoplastic resin within a range that does not impair the effects of the present invention. Furthermore, the polyester fiber of the present invention may contain, as necessary, a matting agent, a heat stabilizer, an ultraviolet absorber, an antistatic agent, an end terminator, a fluorescent whitening agent, etc.
[0037] The polyester fiber of the present invention may contain 50% by weight or more of a polyester resin, preferably 80% by weight or more, more preferably 90% by weight or more, and even more preferably 95% by weight or more.
[0038] From the viewpoint of improving the mechanical properties of the fiber structure, the polyester fiber of the present invention is preferably a drawn fiber. For example, the polyester fiber may be a polyester fiber in which the amorphous component is crystallized by drawing, and no crystallization peak is observed in a DSC curve during the temperature rise process obtained by differential scanning calorimetry (DSC). In this specification, when the crystallization peak (exothermic peak) is very broad and cannot be clearly determined as a peak, it may be determined that no crystallization peak is observed.
[0039] [Method for producing polyester fiber] The method for producing a polyester fiber of the present invention may include a spinning step of melt-spinning a resin material containing a polyester-based resin, and a drawing step of drawing the fiber obtained in the spinning step.
[0040] (Spinning Process) The spinning process can be carried out by melt spinning using a known method, and for example, a known spinning device can be used. Specifically, the resin material in the form of pellets, powder, or the like, which serves as the raw material for the polyester fiber, is placed in a hopper and fed to an extruder via a feeder. The polyester resin contained in the resin material can be any of the polyester resins described above. From the viewpoints of spinnability and the physical properties of the resulting fiber, the intrinsic viscosity of the polyester resin may be 0.4 to 1.0 dL / g, preferably 0.45 to 0.9 dL / g, and more preferably 0.5 to 0.8 dL / g.
[0041] As the extruder, known extruders such as single-screw extruders and multi-screw extruders (two or more screws) can be used. For example, in a twin-screw extruder, the resin material is melt-kneaded and transported from upstream to downstream by the rotation of two parallel screws rotatably supported in a cylinder, and the resin material is heated and melted using known heating means such as a heater installed in the cylinder to form a molten resin. The temperature during melt-kneading depends on the type of polyester-based resin, but may be 260 to 320°C, preferably 270 to 310°C, in order to melt-knead the resin material evenly and stably and to spin it stably.
[0042] The molten resin is then metered using a gear pump, introduced into a spinning head, and discharged through a nozzle outlet to form a filament. The filament is then taken up to obtain an undrawn fiber (raw spun yarn). Depending on the melt viscosity of the resin material, the average fiber diameter of the resulting undrawn fiber can be set as desired by adjusting the nozzle outlet size, discharge rate, take-up speed (spinning speed), and other factors. For example, the nozzle outlet hole diameter may be 0.05 to 0.30 mm, and the discharge rate per hole may be 0.01 to 2.0 g / min. The take-up speed may be 500 to 3,000 m / min, preferably 600 to 2,000 m / min, and more preferably 800 to 1,500 m / min.
[0043] In the present invention, the undrawn fiber obtained in the spinning step may be once wound up and then unwound and drawn, or may be drawn directly after spinning without being wound up after spinning, but from the viewpoint of adjusting the drawing tension in the drawing step as described below, it is preferable to once wind up the undrawn fiber and then subject it to the drawing step. For example, the average fiber diameter of the once wound undrawn fiber may be 8 to 17 μm, preferably 9 to 16 μm, and more preferably 10 to 15 μm.
[0044] (Drawing step) In the present invention, it is preferable to draw undrawn fibers to obtain ultrafine polyester fibers, and in the drawing step, flow drawing is performed, which can reduce the fiber size while maintaining a low molecular orientation, and the drawing tension is adjusted within a specific range, thereby making it possible to uniformize the size and shape of the fiber cross section. Specifically, in the drawing step, the obtained undrawn fibers are subjected to flow drawing and then necking drawing, and it is preferable that the drawing tension is 0.01 cN / dtex or less.
[0045] In general, polyester fibers can be made finer by drawing undrawn fibers at a high drawing ratio. However, in the present invention, it was found that the application of a high drawing tension during the drawing process makes it impossible to draw a plurality of fibers uniformly, resulting in the resulting polyester fibers containing single yarns with a specifically large cross-sectional area and a deformed fiber cross-sectional shape. Furthermore, after examining the conditions for the drawing process, it was found that by performing flow drawing, which can achieve a finer fiber size while maintaining a low molecular orientation, and adjusting the drawing tension within a specific range so as not to apply tension to the polyester fibers, it is possible to achieve a finer fiber size and control the size and shape of the fiber cross-section.
[0046] In the drawing step, the multifilament obtained in the spinning step may be drawn as it is, or from the viewpoint of improving productivity, a plurality of multifilaments may be bundled together to form a fiber bundle (tow) and then drawn.
[0047] Flow drawing is a method in which the undrawn fibers obtained are drawn at a temperature higher than their glass transition point (Tg), and can reduce the fiber size while maintaining the molecular orientation of the undrawn fibers. In the present invention, such flow drawing is performed under a low drawing tension, which is thought to enable the application of a slight and more uniform tensile tension in the fiber axial direction, thereby enabling the size and shape of the fiber cross section to be controlled. Flow drawing can be performed under heating in various modes described below. The drawing tension can be monitored upstream of the heating zone and can be adjusted by the drawing speed, etc. The drawing tension is preferably 0.01 cN / dtex or less, more preferably 0.009 cN / dtex or less, and even more preferably 0.008 cN / dtex or less. From the viewpoint of productivity, it may also be 0.001 cN / dtex or more.
[0048] In the present invention, the flow drawing is not particularly limited as long as it can draw the undrawn polyester fiber at a temperature higher than the glass transition point under a specific low drawing tension, and may be performed by hot bath drawing, dry heat drawing, or wet heat drawing, but hot bath drawing is preferred from the viewpoint of uniform heating. As a heat medium for the hot bath, a liquid such as water or an organic solvent (various oils, etc.) can be used, but a hot water bath is preferred from the viewpoint of thermal conductivity, washability, etc.
[0049] The temperature in the flow drawing is not particularly limited as long as it is higher than the glass transition point (Tg) of the undrawn polyester fiber, and may be Tg+5° C. to Tg+45° C., preferably Tg+10° C. to Tg+40° C. Depending on the type of polyester resin, the temperature may be, for example, 80 to 120° C., preferably 85 to 115° C. Furthermore, from the viewpoint of lowering the drawing tension and performing more stable drawing, the temperature in the flow drawing is more preferably 90 to 110° C.
[0050] The draw ratio in flow drawing may be 1.5 to 10 times, preferably 2.0 to 8.0 times, and more preferably 2.5 to 6.0 times, from the viewpoint of achieving finer fibers and controlling the size and shape of the fiber cross section.
[0051] After flow drawing, necking drawing of the flow-drawn fiber can further reduce the fineness, change the crystallinity, and improve the mechanical strength. Necking drawing can be performed by drawing at a temperature equal to or lower than the glass transition point of the polyester fiber, and may be performed by, for example, hot bath drawing, dry heat drawing, or wet heat drawing, but hot bath drawing is preferred from the viewpoint of uniform heating. As the heat medium for the hot bath, a liquid such as water or an organic solvent (various oils, etc.) can be used, but a hot water bath is preferred from the viewpoint of thermal conductivity, washability, etc., as in flow drawing.
[0052] The temperature in the necking stretching may be a temperature equal to or lower than the glass transition point (Tg) of the polyester fiber, or may be Tg-50° C. to Tg, preferably Tg-30° C. to Tg-1° C., and more preferably Tg-20° C. to Tg-5° C. From the viewpoint of improving the molecular orientation and performing more stable stretching, the temperature may be, for example, 30 to 80° C., preferably 50 to 75° C., and more preferably 60 to 73° C.
[0053] The draw ratio in the necking drawing may be 1.1 to 5.0 times, preferably 1.5 to 4.0 times, and more preferably 2.0 to 3.5 times, from the viewpoints of achieving finer fibers, improving mechanical strength, and controlling the size and shape of the fiber cross section.
[0054] Flow drawing and necking drawing may be performed separately for each drawing. For example, the fiber may be temporarily wound after flow drawing, and then necking drawing may be performed using a different drawing device. When the fiber is temporarily wound after flow drawing and then necking drawing is performed using a different drawing device, it is preferable to adjust the drawing tension in the necking drawing as in the above-mentioned flow drawing. Alternatively, both flow drawing and necking drawing may be performed using a continuous drawing device. From the viewpoint of improving production efficiency and adjusting the drawing tension, it is preferable to perform both flow drawing and necking drawing using a continuous drawing device.
[0055] The total draw ratio in the drawing step (the product of the draw ratio in flow drawing and the draw ratio in necking drawing) depends on the average fiber diameter of the raw spinning yarn (undrawn fiber) and the average fiber diameter of the desired drawn fiber, but may be, for example, 2.0 to 20 times, preferably 5.0 to 18 times, and more preferably 7.0 to 15 times.
[0056] The ratio of the stretching ratio of flow stretching to the stretching ratio of necking stretching in the stretching step (flow stretching / necking stretching) may be, for example, 0.3 to 5.0, preferably 0.4 to 4.0, and more preferably 0.5 to 3.0.
[0057] In the method for producing a polyester fiber of the present invention, various known oil agents may be applied by a known method during the spinning step, before the drawing step, and / or after the drawing step, for example, to improve the collectability of the fiber, prevent fluffing, thread breakage, and the like, and prevent the fibers from sticking together.
[0058] In the method for producing polyester fibers of the present invention, the drawn fibers may be cut to a predetermined fiber length by a known method depending on the application.
[0059] [Fiber Structure] The polyester fiber of the present invention can be used as the main fiber of a fiber structure. The form of the fiber structure is not limited as long as it contains at least polyester fiber, and examples thereof include various types of fabrics such as nonwoven fabrics, woven fabrics, and knitted fabrics, with nonwoven fabrics being preferred. The fiber structure may also contain fibers other than the polyester fiber of the present invention. For example, the fiber structure may contain cellulose-based fibers such as pulp and rayon, polyolefin-based fibers formed from polyolefin-based resins such as polyethylene and polypropylene, polyamide-based fibers formed from polyamide-based resins such as polyamide 6, polyamide 66, polyamide 11, polyamide 12, polyamide 610, and polyamide 612, polyacrylonitrile-based fibers, polyvinyl alcohol-based fibers, etc. Furthermore, if necessary, the fiber structure may contain binder fibers such as water-soluble polymer fibers such as polyvinyl alcohol-based fibers and heat-fusible fibers such as polyester-based fibers.
[0060] The fiber structure of the present invention can be adjusted in terms of basis weight and thickness depending on the type, application, etc. For example, the basis weight is 1 to 120 g / m2 and preferably 3 to 100 g / m 2 , more preferably 5 to 90 g / m 2 may be.
[0061] The fiber structure of the present invention is preferably a wetlaid nonwoven fabric, and more preferably may be a paper-like material. Paper-like materials obtained using the polyester fibers of the present invention have excellent surface smoothness. For example, the surface roughness may be 9.0 μm or less, preferably 8.5 μm or less, and more preferably 8.3 μm or less. The lower limit is not particularly limited, and the surface roughness may be 1.0 μm or more. In this specification, the surface roughness refers to the arithmetic mean roughness Ra measured in accordance with ISO 1997, and is a value measured by the method described in the Examples below.
[0062] When a wetlaid nonwoven fabric is produced as the fiber structure, it may contain binder fibers. The mass ratio of the polyester fiber of the present invention to the binder fibers (e.g., polyester binder fibers) constituting the wetlaid nonwoven fabric (polyester fiber / binder fiber) may be 95 / 5 to 5 / 95, preferably 80 / 20 to 20 / 80, more preferably 75 / 25 to 25 / 75, even more preferably 70 / 30 to 30 / 70, and still more preferably 70 / 30 to 50 / 50.
[0063] The polyester fiber of the present invention has excellent dispersibility and can therefore be used particularly in the production of wetlaid nonwoven fabrics. A wetlaid nonwoven fabric can be obtained by forming a web using water in the production process, drying the web as needed, and then heating the web to bond the fibers with binder fibers. Specific methods for forming a web using water in the production process include a papermaking method in which fibers are dispersed in water to produce a paper-like web, and a hydroentanglement method in which a web is formed without using water and then the fibers in the web are entangled using water.
[0064] As the papermaking method, known methods can be used, such as cylinder papermaking, Fourdrinier papermaking, and short wire papermaking.
[0065] After forming the paper-like web, the web may be dried using a known device, and after drying the web, it may be subjected to a press treatment at high temperature.
[0066] The wetlaid nonwoven fabric containing the polyester fiber of the present invention has excellent surface smoothness, breathability and liquid permeability, and can therefore be used as various industrial materials such as filters, separators, supports for reverse osmosis membranes, wiping materials, artificial leather and various types of functional paper.
[0067] The present invention will be described in more detail below with reference to examples, but the present invention is not limited by these examples. In the following examples and comparative examples, various physical properties were measured by the following methods.
[0068] (Intrinsic Viscosity) The intrinsic viscosity (dL / g) of the resin before spinning was measured using an automatic viscosity measuring device (SS-600-L1 model, manufactured by Shibayama Scientific Instruments Manufacturing Co., Ltd.) A phenol / tetrachloroethane (volume ratio 1 / 1) mixed solvent at 30°C was used as the measurement solvent.
[0069] (Glass transition point) 3 to 8 mg of undrawn polyester fiber (raw spun yarn) was weighed as a measurement sample, and measurement was performed using a differential scanning calorimeter (DSC-60, manufactured by Shimadzu Corporation) in a nitrogen atmosphere at a temperature increase rate of 10°C / min from room temperature to 300°C. In the obtained DSC curve, the glass transition point was determined as the temperature at the intersection of a straight line extending the low-temperature side baseline to the high-temperature side and a tangent drawn at the point where the gradient of the curve in the stepwise change portion of the glass transition is maximum.
[0070] (Stretching Tension) Using a handheld tension meter (manufactured by Nidec-Shimpo Corporation), the tension (cN / dtex) of the fiber tow immediately before being introduced into the stretching bath was measured.
[0071] (Single Yarn Cross-Sectional Area) The fibers obtained in the Examples and Comparative Examples were solidified with paraffin and cut using a microtome in a direction perpendicular to the fiber axis to prepare measurement samples. The cut surfaces of the measurement samples were observed using a digital microscope (Keyence Corporation, VHX-5000), and the automatic area measurement function was used. In order to eliminate inclined fibers, 250 cross sections of single yarns that had a high uniformity in shadow (outline appearance) and existed alone were selected, and the cross-sectional area of each single yarn was measured. From the cross-sectional area data obtained for the 250 points, the average value and standard deviation were calculated, and these were defined as the average cross-sectional area x and the standard deviation of the cross-sectional area σ, respectively. The coefficient of variation of the cross-sectional area was also calculated using the following formula: coefficient of variation of cross-sectional area = standard deviation of cross-sectional area σ / average cross-sectional area x × 100
[0072] Of the cross-sectional area data obtained for 250 points, the total value Ai of the cross-sectional areas of all data within the range of x±2.5σ based on the average cross-sectional area x and standard deviation σ, and the total value Ao of the cross-sectional areas of all data outside this range were calculated. Then, the ratio of Ao to Ai was calculated using the following formula: Ratio of Ao to Ai = Ao / Ai × 100
[0073] (Circularity) The fibers obtained in the examples and comparative examples were solidified with paraffin and cut perpendicular to the fiber axis direction using a microtome to prepare measurement samples. The cut surface of the measurement sample was observed with a digital microscope (Keyence Corporation, VHX-5000), and the maximum and minimum diameters in the fiber cross section were measured using an automatic area measurement function, and the circularity was calculated using the following formula. In order to exclude inclined fibers, 50 fiber cross sections that had a high uniformity of shadow (outline appearance) and existed alone were selected, and the average circularity calculated from these fiber cross sections was used. Circularity = Minimum diameter / Maximum diameter
[0074] Furthermore, the standard deviation of circularity was calculated from the data on circularity of 50 fibers, and the coefficient of variation of circularity was calculated using the following formula: Coefficient of variation of circularity = standard deviation of circularity / average circularity
[0075] (Average Fiber Diameter) The average value of the maximum diameters of the 50 selected fibers measured in the fiber cross section during the measurement of circularity was taken as the average fiber diameter (µm).
[0076] (Average Fiber Length) The fiber lengths of 50 randomly selected fibers were measured, and the average of the measured values was taken as the average fiber length.
[0077] (Aspect Ratio) The aspect ratio was calculated from the average fiber diameter and average fiber length measured above according to the following formula: Aspect ratio = average fiber length / average fiber diameter
[0078] (Crystallization Peak) As a measurement sample, 3 to 8 mg of the fibers obtained in the Examples and Comparative Examples were weighed out, and measurement was carried out using a differential scanning calorimeter (DSC-60, manufactured by Shimadzu Corporation) in a nitrogen atmosphere at a temperature increase rate of 10°C / min from room temperature to 300°C. From the obtained DSC curve, the presence or absence of a crystallization peak resulting from crystallization during temperature increase, originating from the polyester resin, was read.
[0079] (Dispersibility) The fibers obtained in the examples and comparative examples were dispersed in water to prepare a 0.1% slurry, which was then stirred and made into paper. The resulting paper was visually inspected and evaluated according to the following criteria: ◯: Single fibers are uniformly dispersed; ×: Bundle threads (fibers in a bundle) and binding threads (fibers tangled and not dispersed) are present as undispersed fibers.
[0080] (Arithmetic mean roughness Ra) Using a small surface roughness measuring instrument (Mitutoyo Corporation, Surftest SJ-410), both surfaces of the wetlaid nonwoven fabrics obtained in the Examples and Comparative Examples were measured with reference to ISO 1997, and the arithmetic mean roughness Ra was calculated. For the measurement, a needle with a conical tip shape having a taper angle of 60 degrees and a tip curvature radius of 2 μm was used. With a reference length of 0.8 mm, measurements were taken five times at different locations on each surface, and the average value was calculated.
[0081] Example 1 Polyethylene terephthalate pellets with an intrinsic viscosity of 0.65 dL / g were fed into a twin-screw extruder, melt-kneaded at 300°C, and extruded through a die with 150 holes (hole diameter: 0.12 mm) at a throughput rate of 20 g / min. The extruded material was taken up at a speed (spinning speed) of 1,000 m / min to obtain unstretched polyester fibers with an average fiber diameter of 11 μm. The glass transition temperature of the unstretched polyester fibers was 76.3°C. The unstretched polyester fibers were aligned to form a fiber tow, and the stretching tension of the fiber tow was adjusted to 0.006 cN / dtex. The fiber tow was flow-stretched at 3.0 times in a 99°C hot water bath, followed by necking stretching at 3.0 times in a 70°C hot water bath. An oil was then applied to the fiber tow, which was then squeezed to a moisture content of approximately 20% by weight and cut to a length of 3 mm with a cutter to obtain polyester fibers. The physical properties of the polyester fibers obtained were evaluated and the results are shown in Table 1.
[0082] 60% by mass of the obtained polyester fiber and 40% by mass of binder fiber (N720H, manufactured by Kuraray Co., Ltd., single fiber fineness: 2.2 dtex, fiber length: 5 mm) were put into the water bath of a disintegrator (manufactured by Tester Sangyo Co., Ltd.). The fibers were disintegrated in water for 6,000 times at 3,000 rpm, and then the fibers were split into fibers having a basis weight of 10 g / m using a Tappy paper machine (manufactured by Kumagai Riki Kogyo Co., Ltd.). 2 Then, using a press (manufactured by Kumagai Riki Kogyo Co., Ltd.), the paper was pressed at 3.0 kg / cm 2 The wet-laid nonwoven fabric was dried at 120°C for 1 minute in a rotary dryer (manufactured by Kumagai Riki Kogyo Co., Ltd.) to obtain a paper-like wet-laid nonwoven fabric. The physical properties of the obtained wet-laid nonwoven fabric were evaluated and the results are shown in Table 1.
[0083] [Example 2] A polyester fiber was obtained in the same manner as in Example 1, except that the drawing conditions were such that the drawing tension of the fiber tow was adjusted to 0.005 cN / dtex, and the fiber was flow-drawn at 2.5 times in a hot water bath at 99°C, followed by consecutive necking drawing at 3.0 times in a hot water bath at 70°C. The evaluation results of the physical properties of the obtained polyester fiber are shown in Table 1. Furthermore, a paper-like wetlaid nonwoven fabric was obtained using the obtained polyester fiber in the same manner as in Example 1. The evaluation results of the physical properties of the obtained wetlaid nonwoven fabric are shown in Table 1.
[0084] [Example 3] A polyester fiber was obtained in the same manner as in Example 1, except that the drawing conditions were such that the drawing tension of the fiber tow was adjusted to 0.006 cN / dtex, and the fiber was flow-drawn at 4.0 times in a warm water bath at 99°C, followed by consecutive necking drawing at 3.0 times in a warm water bath at 70°C. The evaluation results of the physical properties of the obtained polyester fiber are shown in Table 1. Furthermore, a paper-like wetlaid nonwoven fabric was obtained using the obtained polyester fiber in the same manner as in Example 1. The evaluation results of the physical properties of the obtained wetlaid nonwoven fabric are shown in Table 1.
[0085] Comparative Example 1 A polyester fiber was obtained in the same manner as in Example 1, except that the drawing tension of the fiber tow was adjusted to 0.15 cN / dtex, and the fiber was flow-drawn at 3.0 times in a warm water bath at 97°C, followed by consecutive necking drawing at 3.0 times in a warm water bath at 70°C. The evaluation results of the physical properties of the obtained polyester fiber are shown in Table 1. Furthermore, a paper-like wetlaid nonwoven fabric was obtained using the obtained polyester fiber in the same manner as in Example 1. The evaluation results of the physical properties of the obtained wetlaid nonwoven fabric are shown in Table 1.
[0086]
[0087] As shown in Table 1, in Examples 1 to 3, the drawing tension was adjusted to a low level and flow drawing and necking drawing were performed, which made it possible to highly thin the fibers while reducing the number of unusually thick single yarns outside the range of x±2.5σ, and to make the fiber cross section closer to a perfect circle. Such polyester fibers have good dispersibility, and wetlaid nonwoven fabrics (paper) made using these polyester fibers have excellent surface smoothness.
[0088] On the other hand, in Comparative Example 1, although flow drawing and necking drawing were performed at the same draw ratio as in Example 1, drawing was performed under a higher drawing tension than in Examples 1 to 3, and therefore, single yarns having a cross-sectional area specifically larger than the average cross-sectional area were mixed in, resulting in low circularity. The obtained polyester fiber had poor dispersibility despite having a lower aspect ratio than in Examples 1 to 3, and a wetlaid nonwoven fabric (paper) produced using such polyester fiber had inferior surface smoothness compared to Examples 1 to 3.
[0089] The polyester fiber of the present invention can be used for various fabrics (particularly wetlaid nonwoven fabrics) such as nonwoven fabrics, woven fabrics, knitted fabrics, etc. For example, wetlaid nonwoven fabrics containing the polyester fiber of the present invention can be used as various industrial materials such as filters, separators, supports for reverse osmosis membranes, wiping materials, and various other functional papers.
[0090] As described above, the preferred embodiment of the present invention has been described, but various additions, modifications, or deletions can be made without departing from the spirit of the present invention, and such additions, modifications, or deletions are also included within the scope of the present invention.
Claims
1. The average cross-sectional area x calculated from the cross-sectional area data of single yarn is 1 to 40 μm. 2 and the standard deviation σ of the cross-sectional area is 10 μm 2 or less, and a ratio Ao / Ai of a sum of cross-sectional areas Ao of data outside the range of x±2.5σ to a sum of cross-sectional areas Ai of data within the range of x±2.5σ is 10% or less.
2. The polyester fiber according to claim 1, wherein the coefficient of variation of the cross-sectional area calculated from the cross-sectional area data of a single yarn is 50% or less.
3. The polyester fiber according to claim 1, wherein the average fiber diameter of the single yarn is 1 to 10 μm, and the circularity of the fiber cross section is 0.90 to 1.
00.
4. The polyester fiber according to claim 3, wherein the coefficient of variation of the circularity of the fiber cross section is 7% or less.
5. A polyester fiber having an average fiber diameter of a single yarn of 1 to 10 μm and a circularity of the fiber cross section of 0.90 to 1.
00.
6. The polyester fiber according to claim 5, wherein the coefficient of variation of the circularity of the fiber cross section is 7% or less.
7. The polyester fiber according to any one of claims 1 to 6, having an average fiber length of 0.1 to 110 mm.
8. The polyester fiber according to any one of claims 1 to 6, having an aspect ratio of 100 or more.
9. A fiber structure comprising the polyester fiber according to any one of claims 1 to 6.
10. The fiber structure according to claim 9, which is a wet-laid nonwoven fabric.
11. A method for producing a polyester fiber according to any one of claims 1 to 6, comprising a spinning step of melt-spinning a resin material containing a polyester-based resin, and a drawing step of drawing the fiber obtained by the spinning step, wherein in the drawing step, flow drawing and subsequent necking drawing are performed, and the drawing tension in at least the flow drawing is 0.01 cN / dtex or less.
Citation Information
Patent Citations
Ultrafine fiber for binder
JP2012092458A
Polyester microfiber
JP2012193476A
Organic resin non-crimped staple fiber and method for producing the same
JP6022054B2
JP1974036923A
JP1974094919A
Cited By
Method for producing insolubilized polypeptide molded article having reduced swelling-shrinkage rate, insolubilized fibroin molded article, and insolubilized polypeptide molded article