Production method for aluminum alloy ingot, continuously cast aluminum alloy rod, and forged aluminum alloy product
The method addresses the challenge of reducing CO2 emissions and improving mechanical properties in aluminum alloy production by using a controlled two-step melting process with specific alloying elements, resulting in high-strength aluminum alloy products with reduced energy consumption.
Patent Information
- Application Number
- PCT/JP2024/018838
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-05-22
- Publication Date
- 2024-11-28
AI Technical Summary
The challenge is to reduce CO2 emissions in aluminum production while utilizing aluminum alloy scrap, which introduces impurities like Si, Fe, and Mn, leading to deteriorated mechanical properties due to coarsely grown compounds during melting and casting, and increasing energy consumption.
A method for producing 6000 series aluminum alloy ingots and continuously cast rods that incorporates specific ranges of Cu, Mg, Si, Mn, Fe, Cr, Ti, B, and Zr, using a two-step melting process to control the Si content and refine microstructures, thereby suppressing coarsening and improving mechanical properties and energy efficiency.
The method effectively utilizes commercially available aluminum alloy scraps to produce high-strength aluminum alloy products with improved mechanical properties and reduced energy consumption, achieving a 0.2% proof stress of 350 MPa or more in continuously cast rods and 370 MPa or more in forged products.
Smart Images

Figure JP2024018838_28112024_PF_FP_ABST
Abstract
Description
Method for manufacturing aluminum alloy ingots, aluminum alloy continuously cast rods, and aluminum alloy forged products
[0001] The present invention relates to a method for manufacturing an aluminum alloy ingot, a continuously cast aluminum alloy rod, and an aluminum alloy forged product. This application claims priority to Japanese Patent Application No. 2023-083946, filed on May 22, 2023, the contents of which are incorporated herein by reference.
[0002] In recent years, with the global trend towards carbon neutrality, CO emissions in manufacturing processes have 2 Reducing CO emissions during aluminum production is an issue. 2 In order to reduce emissions, it is important to utilize scrap aluminum alloys, which have a lower melting point than pure aluminum (purity of 99.0% or more), in order to improve the energy consumption rate during melting.
[0003] Methods for producing aluminum alloys and aluminum alloy products using aluminum alloy scrap as a raw material are known (for example, Patent Documents 1 to 3). Aluminum alloy scrap is recovered from used aluminum products, and is produced as a recycled raw material by melting and adjusting the composition to be used as the raw material for aluminum alloys.
[0004] JP 2020-514556 A JP 2020-527653 A JP 2022-137762 A
[0005] When utilizing aluminum alloy scrap as raw material for aluminum alloys derived from recycled materials, for example, when using scrap for 6000-series alloys, high-purity materials such as 6063 sash scrap from building materials are preferred. However, impurities such as Si, Fe, and Mn are often mixed in with the scrap. If these compounds (e.g., Al-Fe-Mn-Si) grow into large particles and are present in the cast rod during the melting and casting process, the mechanical properties of the product are reduced.
[0006] The present invention has been made in view of the above circumstances, and aims to provide a method for producing a 6000 series aluminum alloy ingot, a continuously cast aluminum alloy rod, and an aluminum alloy forged product, which are capable of utilizing commercially available aluminum alloy scrap in the production of aluminum alloys, while suppressing the coarsening of Al-Fe-Mn-Si compounds that are produced by elements mixed in from the aluminum alloy scrap, and improving the fuel consumption rate in the melting step.
[0007] In order to solve the above problems, the present invention provides the following means.
[0008] Aspect 1 of the present invention is an aluminum alloy for producing an aluminum alloy ingot containing additive elements of Cu in the range of 0.30 mass% to 1.0 mass% inclusive, Mg in the range of 0.80 mass% to 1.8 mass% inclusive, Si in the range of 0.90 mass% to 1.9 mass% inclusive, Mn in the range of 0.30 mass% to 1.2 mass% inclusive, Fe in the range of 0.20 mass% to 0.65 mass% inclusive, Zn in the range of 0.25 mass% inclusive, Cr in the range of 0.050 mass% to 0.30 mass% inclusive, Ti in the range of 0.01 mass% to 0.1 mass% inclusive, B in the range of 0.0010 mass% to 0.030 mass% inclusive, and Zr in the range of 0.0010 mass% to 0.050 mass% inclusive, with the balance being Al and unavoidable impurities. This method for producing an aluminum alloy ingot includes: a primary melting step in which raw materials containing aluminum alloy scrap and aluminum ingot are charged, the raw materials having the same compositional ranges as those of the aluminum alloy ingot except that the Si content is 0.60% by mass or more and 0.90% by mass or less, and the aluminum alloy scrap and aluminum ingot are charged in ascending order of melting point and melted to obtain a primary molten metal; and a secondary melting step in which metallic Si or a Si-containing alloy is added to the primary molten metal obtained in the primary melting step or to a molten metal obtained by melting an ingot obtained by solidifying the primary molten metal, to adjust the Si content to be within the range of 0.90% by mass or more and 1.9% by mass or less.
[0009] A second aspect of the present invention is the method for producing an aluminum alloy ingot according to the first aspect, wherein the aluminum alloy scrap comprises at least one of scrap containing a 3000 series alloy, scrap containing a 4000 series alloy, scrap containing a 5000 series alloy, and scrap containing a 6000 series alloy.
[0010] A third aspect of the present invention is a continuously cast aluminum alloy rod obtained from an aluminum alloy ingot produced by the method for producing an aluminum alloy ingot according to the first or second aspect, and having a 0.2% yield strength of 350 MPa or more.
[0011] A fourth aspect of the present invention is an aluminum alloy forging obtained by using the continuously cast aluminum alloy rod of the third aspect, and having a 0.2% yield strength of 370 MPa or more.
[0012] According to the method for producing an aluminum alloy ingot of the present invention, it is possible to provide a method for producing a 6000 series aluminum alloy ingot that utilizes aluminum alloy scrap available on the market, while suppressing coarsening of Al—Fe—Mn—Si compounds that are produced by elements mixed in from the aluminum alloy scrap.
[0013] 1A and 1B are conceptual diagrams showing a case where the primary molten metal obtained in the primary melting process is solidified into an ingot and the ingot is then introduced into a secondary melting process.
[0014] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. Note that the drawings used in the following description may show characteristic portions enlarged for convenience in order to make the features easier to understand, and the dimensional ratios of each component may not necessarily be the same as those in reality. Furthermore, the materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not necessarily limited thereto. Appropriate changes can be made within the scope that does not change the effects of the present invention.
[0015] [Method for manufacturing aluminum alloy ingot] An aluminum alloy ingot manufactured by the method for manufacturing an aluminum alloy ingot according to this embodiment will be described. The aluminum alloy ingot according to this embodiment contains additive elements in the range of 0.30% by mass to 1.0% by mass, 0.80% by mass to 1.8% by mass of Mg, 0.90% by mass to 1.9% by mass of Si, 0.30% by mass to 1.2% by mass of Mn, 0.20% by mass to 0.65% by mass of Fe, 0.25% by mass to 0.65% by mass of Zn, 0.050% by mass to 0.30% by mass of Cr, 0.01% by mass to 0.1% by mass of Ti, 0.0010% by mass to 0.030% by mass of B, and 0.0010% by mass to 0.050% by mass of Zr, with the balance being Al and inevitable impurities.
[0016] The aluminum alloy ingot of this embodiment corresponds to a forged product of a 6000 series aluminum alloy in that it contains Mg and Si.
[0017] (Cu: 0.30% by mass or more, 1.0% by mass or less) Cu has the effect of finely dispersing Mg-Si compounds in the aluminum alloy and improving the tensile strength of the aluminum alloy by precipitating as Al-Cu-Mg-Si compounds such as the Q phase. By ensuring that the Cu content is within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved.
[0018] (Mg: 0.80 mass % or more, 1.8 mass % or less) Mg has the effect of improving the tensile strength of the aluminum alloy. Mg dissolves in the aluminum matrix or forms a Mg-Si compound (Mg 2 Si) or Q phase and other Al-Cu-Mg-Si compounds (AlCuMgSi), which contribute to strengthening the aluminum alloy. 2 Si is the CuAl in the aluminum alloy. 2 It has the effect of suppressing the formation of CuAl phase. 2By suppressing the formation of the phase, the corrosion resistance of the aluminum alloy ingot is improved. By having the Mg content within the above range, the corrosion resistance as well as the mechanical properties at room temperature of the aluminum alloy ingot can be improved.
[0019] (Si: 0.90% by mass or more, 1.9% by mass or less) Like Mg, Si has the effect of improving the corrosion resistance as well as the mechanical properties of an aluminum alloy ingot at room temperature. However, if excessive Si is added to an aluminum alloy, coarse primary Si grains may crystallize, potentially reducing the tensile strength of the aluminum alloy. By keeping the Si content within the above range, it is possible to improve the corrosion resistance as well as the mechanical properties of an aluminum alloy ingot at room temperature while suppressing the crystallization of primary Si.
[0020] (Mn: 0.30% by mass or more, 1.2% by mass or less) Mn forms fine granular precipitates containing intermetallic compounds such as Al-Mn-Fe-Si and Al-Mn-Cr-Fe-Si in the aluminum alloy, thereby improving the tensile strength of the aluminum alloy. By ensuring that the Mn content is within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved.
[0021] (Fe: 0.20 mass% or more, 0.65 mass% or less) Fe crystallizes in the aluminum alloy as fine crystals containing intermetallic compounds such as Al-Mn-Fe-Si, Al-Mn-Cr-Fe-Si, Al-Fe-Si, Al-Cu-Fe, and Al-Mn-Fe, thereby improving the tensile strength of the aluminum alloy. When the Fe content is within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved. The Fe / Mn relationship is less than 1.4. When the Fe / Mn relationship is less than 1.4, the crystallization of AlFeSi-based compounds of 2.0 μm or more can be suppressed, and the mechanical properties can be improved.
[0022] (Cr: 0.050% by mass or more, 0.30% by mass or less) Cr forms fine granular crystallized products containing intermetallic compounds such as Al-Mn-Cr-Fe-Si and Al-Fe-Cr in the aluminum alloy, thereby improving the tensile strength of the aluminum alloy. By ensuring that the Cr content is within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved.
[0023] (Ti: 0.010% by mass or more, 0.10% by mass or less) Ti has the effect of refining the crystal grains of an aluminum alloy and improving its wrought workability. If the Ti content is less than 0.010% by mass, the effect of refining the crystal grains may not be sufficiently obtained. On the other hand, if the Ti content exceeds 0.10% by mass, coarse crystals may be formed, which may reduce the wrought workability. Furthermore, if a large amount of coarse crystals containing Ti are mixed into an aluminum alloy ingot, the toughness may be reduced. Therefore, the Ti content is set to 0.010% by mass or more, and 0.10% by mass or less. The Ti content is preferably 0.015% by mass or more, and 0.050% by mass or less.
[0024] (B: 0.0010% by mass or more, 0.030% by mass or less) B has the effect of refining the crystal grains of an aluminum alloy and improving its wrought workability. Adding B to an aluminum alloy together with the above-mentioned Ti improves the effect of refining the crystal grains. If the B content is less than 0.0010% by mass, the effect of refining the crystal grains may not be sufficient. On the other hand, if the B content exceeds 0.030% by mass, coarse crystals may be formed and may be mixed into the aluminum alloy ingot as inclusions. Furthermore, if a large amount of coarse crystals containing B are mixed into the final aluminum alloy product, the toughness may be reduced. Therefore, the B content is set to 0.0010% by mass or more, and 0.030% by mass or less. The B content is preferably 0.0050% by mass or more, and 0.025% by mass or more.
[0025] (Zr: 0.0010 mass % or more, 0.050 mass % or less) When Zr is 0.050 mass % or less, Al 3Precipitation in the form of Zr and Al-(Ti,Zr) contributes to improving the strength of aluminum alloy ingots through recrystallization suppression effects and precipitation strengthening. However, if the Zr content exceeds 0.050 mass%, coarse Zr compounds may crystallize, potentially leading to a decrease in the corrosion resistance of the aluminum alloy ingot. For this reason, the Zr content is set to 0.050 mass% or less. Furthermore, in order to obtain the above-mentioned recrystallization suppression effects and the effects of improving the strength of forged products through precipitation strengthening, the Zr content is preferably 0.0010 mass% or more.
[0026] (Zn: 0.250 mass% or less) Zn may be 0.250 mass% or less. If the Zn content exceeds 0.250 mass%, MgZn 2 The Zn content is preferably 0.250 mass% or less, or is preferably zero.
[0027] (Inevitable impurities) Inevitable impurities are impurities that are inevitably mixed into the aluminum alloy from the raw materials or manufacturing process of the aluminum alloy ingot. Examples of inevitable impurities include Ni, Sn, and Be. The content of these inevitable impurities preferably does not exceed 0.1% by mass.
[0028] [Method for manufacturing aluminum alloy ingot] Next, a method for manufacturing the aluminum alloy ingot of this embodiment will be described. The aluminum alloy ingot of this embodiment can be manufactured, for example, by a method including a melting (molten metal formation) step and a casting step.
[0029] (Melting Step) In the melting (molten metal formation) step, a molten aluminum alloy is formed. In the method for producing an aluminum alloy ingot according to this embodiment, the melting (molten metal formation) step is comprised of two sub-steps (a primary melting step and a secondary melting step).
[0030] <Primary Melting Step> In the primary melting step, raw materials including aluminum alloy scrap and aluminum ingot (aluminum bullion), which have the same content ratios of the above-described additive elements (Cu, Mg, Mn, Fe, Zn, Cr, Ti, B, Zr) as those of the aluminum alloy ingot to be produced, except that the content ratio of Si is 0.60% by mass or more and 0.90% by mass or less, are charged. When these raw materials are charged, the aluminum alloy scrap and aluminum ingot are charged in ascending order of melting point, and melted to obtain a primary molten metal.
[0031] The primary molten metal obtained in the primary melting step may be solidified into an ingot, or may be transferred directly to a melting furnace for performing the secondary melting step. Figures 1A and 1B are diagrams conceptually illustrating such a configuration. Figure 1A is a diagram conceptually illustrating a flow for solidifying the primary molten metal obtained in the primary melting step into an ingot. First, a raw material containing blended aluminum alloy scrap is prepared (raw material preparation step). Next, the raw material is charged into a primary melting furnace and the primary melting step is performed to obtain the primary molten metal (primary melting step). Next, the primary molten metal is solidified into an ingot (primary molten metal solidification step). After that, the secondary melting step is performed in a secondary melting furnace using the ingot as the raw material to obtain the secondary molten metal (secondary melting step). On the other hand, Figure 1B is a diagram conceptually illustrating a flow for transferring the primary molten metal obtained in the primary melting step directly to a melting furnace for performing the secondary melting step. First, a raw material containing blended aluminum alloy scrap is prepared (raw material preparation step). Next, the raw materials are charged into a primary melting furnace and a primary melting process is carried out to obtain a primary molten metal (primary melting process).The primary molten metal is then transferred directly to a secondary melting furnace via a trough and a secondary melting process is carried out to obtain a secondary molten metal (secondary melting process).
[0032] In the primary melting step, aluminum alloy scrap and aluminum ingot are charged first, starting with the one with the lowest melting point. After the first scrap is completely melted, the next aluminum alloy scrap and aluminum ingot, whichever has the lowest melting point, is charged, and after the first scrap is completely melted, the next aluminum alloy scrap and aluminum ingot, whichever has the lowest melting point, is charged. After the first aluminum alloy scrap and aluminum ingot are completely melted, additive metals such as Cu scrap and mother alloy are charged. Examples of aluminum alloy scrap include scrap of Al-Mn-based (3000-series) alloys such as aluminum cans and recycled aluminum can ingots, scrap of Al-Si-based (4000-series) alloys such as ADC12 and A356, scrap of Al-Mg-based (5000-series) alloys such as 5052 and 5083, and scrap of Al-Mg-Si-based (6000-series) alloys such as 6063 and 6061. Aluminum ingots (pure aluminum) are classified into normal purity ingots, high purity ingots, and alloy ingots based on their purity and composition, and can be divided into ingots (cast ingots for general raw materials), slabs (cast ingots prepared for rolling), billets (cast ingots prepared for extrusion), and the like based on their shape and use.
[0033] If the Si content is less than 0.60% by mass, for example, metallic Si or a Si-containing alloy is added to adjust the Si content to a range of 0.60% by mass to 0.90% by mass. Metallic Si is preferred as the additive material due to ease of adjustment. If the Si content exceeds 0.90% by mass, aluminum bullion or aluminum alloy scrap with a low Si content is added to adjust the Si content to a range of 0.60% by mass to 0.90% by mass. Examples of aluminum alloy scrap with a low Si content include 3000-series alloy scrap, scrap containing 5000-series alloy, and scrap containing 6000-series alloy. The Si content (component analysis) can be performed, for example, by optical emission spectroscopy.
[0034] When Si, Fe, and Mn are mixed in scrap and melted, Al-Fe-Mn-Si compounds are generated within a certain temperature range during the melting process. The amount of this compound generated is particularly affected by the amount of Si. If the amount generated increases, the melting temperature must be set to 850°C or higher to melt them. This is undesirable because it increases the energy used during melting. Furthermore, if the Si content falls below 0.6% by mass, too much Si is added in the secondary melting process, which takes time to completely melt the added Si, resulting in energy loss. Therefore, the Si content of the alloy composition obtained in the primary melting process must be 0.60% by mass or more and 0.90% by mass or less.
[0035] The higher the usage ratio (blending ratio) of aluminum alloy scrap in the raw materials, the more preferable it is in terms of improving the energy consumption rate during melting. The blending ratio of aluminum alloy scrap can be, for example, 50% or more. For example, it can be 60% or more, 70% or more, 80% or more, 90% or more, or 100%. On the other hand, although the effect of improving the energy consumption rate during melting is lower, the blending ratio of aluminum alloy scrap can also be less than 50%, for example, 40%, 30%, 20%, or 10%.
[0036] The melting point of pure aluminum is approximately 660°C. In contrast, ADC12, for example, has a melting point of 570°C, and other aluminum alloys have melting points of 650°C or less, which is 10°C or more lower. Therefore, it melts easily, and by utilizing this, the energy consumption rate during melting can be improved.
[0037] Aluminum alloy scrap can be used within the composition ranges listed below. Examples of aluminum alloy scrap include Al-Si (4000 series) alloys such as ADC12 and A356, which contain 4% to 12% by weight of Si and 0.01% to 3.0% by weight of Cu; Al-Mn (3000 series) alloys such as other aluminum cans and recycled aluminum can blocks, which contain 0.7% to 1.4% by weight of Mn and 0.5% to 1.4% by weight of Mg; Al-Mg (5000 series) alloys such as 5052 and 5083, which contain 2.0% to 5.0% by weight of Mg; and Al-Mg-Si (6000 series) alloys such as 6063 and 6061, which contain 0.2% to 0.8% by weight of Si and 0.45% to 1.2% by weight of Mg. Aluminum can scrap is usually subjected to a heat treatment process at 400 to 500°C to remove paint from the can surface before being melted. By adding an Al-Si alloy, the amount of Si added in the secondary melting step can be reduced, so it is preferable to use this in combination with scrap of other alloy types.
[0038] <Second Melting Step> The second melting step is a step of adding metallic Si or a Si-containing alloy to the primary molten metal obtained in the first melting step or to a molten metal obtained by melting an ingot obtained from the primary molten metal, thereby adjusting the Si content to 0.90% by mass or more and 1.9% by mass. Metallic Si is preferred as the additive material because of its ease of adjustment.
[0039] The composition adjustment here is carried out at a temperature of 700°C or higher and 800°C or lower. If the temperature is below 700°C, the temperature drop in the molten metal path when the molten metal is cast causes the Al-Fe-Mn-Si compounds to grow coarsely, impairing the mechanical properties of the product. Also, if the temperature exceeds 800°C, the amount of hydrogen dissolved in the atmosphere into the molten aluminum increases, increasing the amount of hydrogen gas in the molten metal, resulting in the generation of porosity in the cast product and impairing the mechanical properties. Therefore, the temperature range of 700°C or higher and 800°C or lower is preferable.
[0040] (Casting process) The molten metal obtained in the secondary melting process is subjected to flux treatment and then GBF (gas bubbling filtration) treatment before being poured into a casting mold. The poured molten metal is then continuously cast by either vertical (vertical) continuous casting or horizontal (horizontal) continuous casting to produce a continuously cast aluminum alloy rod.
[0041] In the method for manufacturing an aluminum alloy ingot according to this embodiment, a melting facility may be used in which a melting furnace for performing a primary melting step and a melting furnace for adjusting the composition are arranged in series and connected by a trough, and the primary molten metal obtained in the primary melting step can be transferred to the melting furnace for adjusting the composition without casting.
[0042] [Continuously Cast Aluminum Alloy Rod] The continuously cast aluminum alloy rod according to this embodiment is produced by continuous casting, either vertical (vertical) continuous casting or horizontal (horizontal) continuous casting, using an aluminum alloy ingot obtained by the method for producing an aluminum alloy ingot according to this embodiment, and has a 0.2% yield strength of 350 MPa or more.
[0043] [Aluminum Alloy Forgings] The aluminum alloy forgings according to this embodiment are produced using the continuously cast aluminum alloy rod according to this embodiment, and have a 0.2% proof stress of 370 MPa or more. For example, the aluminum alloy forgings according to this embodiment can be produced by subjecting the continuously cast aluminum alloy rod according to this embodiment to a homogenization heat treatment step, a forging step, a solution treatment step, a quenching treatment step, and an aging treatment step.
[0044] Next, specific examples of the present invention will be described, but the present invention is not limited to these examples.
[0045] (Example of Aluminum Alloy Scrap) Aluminum alloy scrap obtained from a secondary alloy manufacturer and a scrap manufacturer was analyzed by optical emission spectroscopy to obtain component analysis values (mass%) for each scrap, which are shown in Table 1. The component analysis was carried out in accordance with the optical emission spectroscopy analysis of aluminum and aluminum alloys specified in JIS H1305 2005. The melting point was measured by differential scanning calorimetry (DSC) to determine the melting temperature of the sample.
[0046]
[0047] (Example, Comparative Examples 1 and 2) In the example and Comparative Examples 1 and 2, the combinations (blends) of aluminum alloy scrap and aluminum ingot shown in Table 1 were made using raw materials with blending ratios shown in Table 2.
[0048]
[0049] In both the examples and comparative examples 1 and 2, the contents of the additive elements other than Si were: Cu in the range of 0.30% by mass to 1.0% by mass, Mg in the range of 0.80% by mass to 1.8% by mass, Mn in the range of 0.30% by mass to 1.2% by mass, Fe in the range of 0.20% by mass to 0.65% by mass, Zn in the range of 0.25% by mass, Cr in the range of 0.050% by mass to 0.30% by mass, Ti in the range of 0.01% by mass to 0.1% by mass, B in the range of 0.0010% by mass to 0.030% by mass, and Zr in the range of 0.0010% by mass to 0.050% by mass, with the balance being Al and inevitable impurities. Furthermore, in the examples, the Si content was in the range of 0.60% by mass to 0.90% by mass. On the other hand, in the comparative examples, the Si content was blended so as to be outside the range of 0.60 mass % or more and 0.90 mass % or less.
[0050] In the examples, the raw materials were charged into a 15-ton melting furnace in the order of lowest melting point, and the entire amount was melted at a melting temperature of 780°C. On the other hand, in the comparative examples, the raw materials were charged into a 15-ton melting furnace in the order of highest melting point (Comparative Example 1), or in a random order, neither in the order of lowest nor highest melting point (Comparative Example 2), and the entire amount was melted at a melting temperature of 780°C. The amount of LNG used when melting 1 ton in the examples and comparative examples (unit: [m3 / Ton]) was measured. 3 / Ton] or less is 〇, 100 [m 3 / Ton] or more was judged as ×. The results are shown in Table 3.
[0051]
[0052] From Table 3, in the example, the amount of LNG used is 85 [m 3 / Ton], whereas in Comparative Example 1 it was 120 [m 3 / Ton], and in Comparative Example 2 it was 115 [m 3 It was demonstrated that feeding aluminum alloy scrap and aluminum ingot raw materials into a melting furnace in order of decreasing melting point improves the energy consumption during melting compared to feeding the raw materials in order of increasing melting point, or feeding them randomly, neither in order of decreasing nor increasing melting point.
Claims
1. A method for producing an aluminum alloy ingot containing additive elements of Cu in the range of 0.30 mass% to 1.0 mass%, Mg in the range of 0.80 mass% to 1.8 mass%, Si in the range of 0.90 mass% to 1.9 mass%, Mn in the range of 0.30 mass% to 1.2 mass%, Fe in the range of 0.20 mass% to 0.65 mass%, Zn in the range of 0.25 mass% or less, Cr in the range of 0.050 mass% to 0.30 mass%, Ti in the range of 0.01 mass% to 0.1 mass%, B in the range of 0.0010 mass% to 0.030 mass%, and Zr in the range of 0.0010 mass% to 0.050 mass%, with the balance being Al and unavoidable impurities, 1. A method for producing an aluminum alloy ingot, comprising: a primary melting step in which raw materials including aluminum alloy scrap and aluminum ingot are charged, the raw materials having the same compositional range as that of the aluminum alloy ingot except for a Si content of 0.60% by mass or more and 0.90% by mass or less, and the aluminum alloy scrap and the aluminum ingot are charged in order of decreasing melting point to obtain a primary molten metal by melting the raw materials; and a secondary melting step in which metallic Si or a Si-containing alloy is added to the primary molten metal obtained in the primary melting step or to a molten metal obtained by melting an ingot obtained by solidifying the primary molten metal, to adjust the Si content to within a range of 0.90% by mass or more and 1.9% by mass or less.
2. The method for producing an aluminum alloy ingot as set forth in claim 1, wherein the aluminum alloy scrap comprises at least one of scrap containing a 3000 series alloy, scrap containing a 4000 series alloy, scrap containing a 5000 series alloy, and scrap containing a 6000 series alloy.
3. A continuously cast aluminum alloy rod obtained using an aluminum alloy ingot produced by the method for producing an aluminum alloy ingot according to claim 1 or 2, and having a 0.2% yield strength of 350 MPa or more.
4. An aluminum alloy forging obtained by using the aluminum alloy continuously cast rod described in claim 3 and having a 0.2% yield strength of 370 MPa or more.
Citation Information
Patent Citations
Eutectic high-entropy alloy with low notch sensitivity and preparation method thereof
CN111321336A
High-strength and high-toughness aluminum alloy forged material
JP2000144296A
Automobile chassis parts and its manufacturing method
JP2008163445A
Aluminum alloy recycling method and its refinement
JP2020531685A
Aluminum alloy forging and method for producing the same
JP2022093988A