Production method for aluminum alloy ingot, continuously cast aluminum alloy rod, and forged aluminum alloy product

The method addresses the coarsening issue in aluminum alloy products by controlling element compositions and cooling rates during the production of aluminum alloy ingots and continuously cast rods, achieving enhanced mechanical properties and energy efficiency.

WO2024242137A1PCT designated stage expired Publication Date: 2024-11-28RESONAC CORP

Patent Information

Application Number
PCT/JP2024/018847
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-22
Filing Date
2024-05-22
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

The challenge is to produce aluminum alloy ingots, continuously cast rods, and forged products that utilize commercially available scrap materials while preventing the coarsening of Al-Fe-Mn-Si compounds, which deteriorate the mechanical properties due to impurities present in recycled aluminum alloy scraps.

Method used

A method involving specific composition ranges of elements like Cu, Mg, Si, Mn, Fe, Cr, Ti, B, and Zr in aluminum alloy ingots, with a primary and secondary melting process, and a high cooling rate during casting to control the microstructure and suppress coarsening, ensuring the ingots and rods have improved mechanical properties.

Benefits of technology

The method effectively suppresses coarsening, enhancing the mechanical properties and corrosion resistance of the aluminum alloy products, achieving proof stresses of 350 MPa or more in continuously cast rods and 370 MPa or more in forged products, while reducing energy consumption by utilizing high-purity aluminum alloy scrap.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018847_28112024_PF_FP_ABST
    Figure JP2024018847_28112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a production method for an aluminum alloy ingot containing additive elements of 0.30-1.0 mass% Cu, 0.80-1.8 mass% Mg, 0.90-1.9 mass% Si, 0.30-1.2 mass% Mn, 0.20-0.65 mass% Fe, up to 0.25 mass% Zn, 0.050-0.30 mass% Cr, 0.01-0.1 mass% Ti, 0.0010-0.030 mass% B, and 0.0010-0.050 mass% Zr, the method comprising: a first melting step for obtaining a primary melt by melting raw materials including aluminum alloy scrap and having the same composition range as that of the aluminum alloy ingot except that the Si content is 0.60-0.90 mass%; a primary casting step for solidifying the primary melt into an ingot; and a secondary melting step for adjusting the Si content to 0.90-1.9 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing aluminum alloy ingots, aluminum alloy continuous cast rods, and aluminum alloy forged products

[0001] The present invention relates to a method for manufacturing an aluminum alloy ingot, a continuously cast aluminum alloy rod, and an aluminum alloy forged product. This application claims priority to Japanese Patent Application No. 2023-084135, filed on May 22, 2023, the contents of which are incorporated herein by reference.

[0002] In recent years, with the global trend towards carbon neutrality, CO emissions in manufacturing processes have 2 Reducing CO emissions during aluminum production is an issue. 2 In order to reduce emissions, it is important to utilize scrap aluminum alloys, which have a lower melting point than pure aluminum (purity of 99.0% or more), in order to improve the energy consumption rate during melting.

[0003] Methods for producing aluminum alloys and aluminum alloy products using aluminum alloy scrap as a raw material are known (for example, Patent Documents 1 to 3). Aluminum alloy scrap is recovered from used aluminum products, and is produced as a recycled raw material by melting and adjusting the composition to be used as the raw material for aluminum alloys.

[0004] JP 2020-514556 A JP 2020-527653 A JP 2022-137762 A

[0005] When utilizing aluminum alloy scrap as raw material for aluminum alloys derived from recycled materials, for example, when using scrap for 6000-series alloys, high-purity materials such as 6063 sash scrap from building materials are preferred. However, impurities such as Si, Fe, and Mn are often mixed in with the scrap. If these compounds (e.g., Al-Fe-Mn-Si) grow into large particles and are present in the cast rod during the melting and casting process, the mechanical properties of the product are reduced.

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing a 6000 series aluminum alloy ingot, a continuously cast aluminum alloy rod, and an aluminum alloy forged product, which are capable of utilizing commercially available aluminum alloy scrap in the production of aluminum alloys while suppressing coarsening of Al-Fe-Mn-Si compounds that are generated by elements mixed in from the aluminum alloy scrap.

[0007] In order to solve the above problems, the present invention provides the following means.

[0008] Aspect 1 of the present invention is a method for producing an aluminum alloy ingot containing additive elements in the range of 0.30 mass% to 1.0 mass% Cu, 0.80 mass% to 1.8 mass% Mg, 0.90 mass% to 1.9 mass% Si, 0.30 mass% to 1.2 mass% Mn, 0.20 mass% to 0.65 mass% Fe, 0.25 mass% to 0.65 mass% Zn, 0.050 mass% to 0.30 mass% Cr, 0.01 mass% to 0.1 mass% Ti, 0.0010 mass% to 0.030 mass% B, and 0.0010 mass% to 0.050 mass% Zr, with the balance being Al and inevitable impurities. and a primary casting step of solidifying the primary molten metal obtained in the primary melting step into an ingot, the primary molten metal being obtained in the primary melting step, wherein the primary molten metal is cooled from the liquidus temperature to the solidus temperature of the final solidification portion of the ingot at a cooling rate of 10°C / sec or more, and the secondary melting step of adding metallic Si or a Si-containing alloy to the molten metal obtained in the primary casting step, thereby adjusting the Si content to be within the range of 0.90% by mass or more and 1.9% by mass or less.

[0009] A second aspect of the present invention is the method for producing an aluminum alloy ingot according to the first aspect, wherein the aluminum alloy scrap comprises at least one of scrap containing a 3000 series alloy, scrap containing a 4000 series alloy, scrap containing a 5000 series alloy, and scrap containing a 6000 series alloy.

[0010] A third aspect of the present invention is a continuously cast aluminum alloy rod obtained from an aluminum alloy ingot produced by the method for producing an aluminum alloy ingot according to the first or second aspect, and having a 0.2% yield strength of 350 MPa or more.

[0011] A fourth aspect of the present invention is an aluminum alloy forging obtained by using the continuously cast aluminum alloy rod of the third aspect, and having a 0.2% yield strength of 370 MPa or more.

[0012] According to the method for producing an aluminum alloy ingot of the present invention, it is possible to provide a method for producing a 6000 series aluminum alloy ingot that utilizes aluminum alloy scrap available on the market, while suppressing coarsening of Al—Fe—Mn—Si compounds that are produced by elements mixed in from the aluminum alloy scrap.

[0013] Fig. 1 is a conceptual diagram of a case where a primary molten metal obtained in a primary melting step is solidified into an ingot and the ingot is then introduced into a secondary melting step. Fig. 2 is a schematic cross-sectional view of a continuous casting mold for a vertical continuous casting apparatus. Fig. 3 is a schematic cross-sectional view of a horizontal continuous casting apparatus. Fig. 4 is a schematic diagram for explaining a structural observation site of a continuously cast aluminum alloy rod of the present embodiment. Fig. 5 is a schematic diagram for explaining a site for evaluating tensile properties of a continuously cast aluminum alloy rod of the present embodiment. Fig. 6 is a schematic diagram for explaining the preparation of a forged product for evaluating tensile properties of an aluminum alloy forged product of the present embodiment.

[0014] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. Note that the drawings used in the following description may show characteristic portions enlarged for convenience in order to make the features easier to understand, and the dimensional ratios of each component may not necessarily be the same as those in reality. Furthermore, the materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not necessarily limited thereto. Appropriate changes can be made within the scope that does not change the effects of the present invention.

[0015] [Method for manufacturing aluminum alloy ingot] An aluminum alloy ingot manufactured by the method for manufacturing an aluminum alloy ingot according to this embodiment will be described. The aluminum alloy ingot according to this embodiment contains additive elements in the range of 0.30% by mass to 1.0% by mass, 0.80% by mass to 1.8% by mass of Mg, 0.90% by mass to 1.9% by mass of Si, 0.30% by mass to 1.2% by mass of Mn, 0.20% by mass to 0.65% by mass of Fe, 0.25% by mass to 0.65% by mass of Zn, 0.050% by mass to 0.30% by mass of Cr, 0.01% by mass to 0.1% by mass of Ti, 0.0010% by mass to 0.030% by mass of B, and 0.0010% by mass to 0.050% by mass of Zr, with the balance being Al and inevitable impurities.

[0016] The aluminum alloy ingot of this embodiment corresponds to a forged product of a 6000 series aluminum alloy in that it contains Mg and Si.

[0017] (Cu: 0.30% by mass or more, 1.0% by mass or less) Cu has the effect of finely dispersing Mg-Si compounds in the aluminum alloy and improving the tensile strength of the aluminum alloy by precipitating as Al-Cu-Mg-Si compounds such as the Q phase. By ensuring that the Cu content is within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved.

[0018] (Mg: 0.80 mass % or more, 1.8 mass % or less) Mg has the effect of improving the tensile strength of the aluminum alloy. Mg dissolves in the aluminum matrix or forms a Mg-Si compound (Mg 2 Si) or Q phase and other Al-Cu-Mg-Si compounds (AlCuMgSi), which contribute to strengthening the aluminum alloy. 2 Si is the CuAl in the aluminum alloy. 2 It has the effect of suppressing the formation of CuAl phase. 2 By suppressing the formation of the phase, the corrosion resistance of the aluminum alloy ingot is improved. By having the Mg content within the above range, the corrosion resistance as well as the mechanical properties at room temperature of the aluminum alloy ingot can be improved.

[0019] (Si: 0.90% by mass or more, 1.9% by mass or less) Like Mg, Si has the effect of improving the corrosion resistance as well as the mechanical properties of an aluminum alloy ingot at room temperature. However, if excessive Si is added to an aluminum alloy, coarse primary Si grains may crystallize, potentially reducing the tensile strength of the aluminum alloy. By keeping the Si content within the above range, it is possible to improve the corrosion resistance as well as the mechanical properties of an aluminum alloy ingot at room temperature while suppressing the crystallization of primary Si.

[0020] (Mn: 0.30% by mass or more, 1.2% by mass or less) Mn forms fine granular precipitates containing intermetallic compounds such as Al-Mn-Fe-Si and Al-Mn-Cr-Fe-Si in the aluminum alloy, thereby improving the tensile strength of the aluminum alloy. By ensuring that the Mn content is within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved.

[0021] (Fe: 0.20 mass% or more, 0.65 mass% or less) Fe crystallizes in the aluminum alloy as fine crystals containing intermetallic compounds such as Al-Mn-Fe-Si, Al-Mn-Cr-Fe-Si, Al-Fe-Si, Al-Cu-Fe, and Al-Mn-Fe, thereby improving the tensile strength of the aluminum alloy. When the Fe content is within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved. The Fe / Mn relationship is less than 1.4. When the Fe / Mn relationship is less than 1.4, the crystallization of AlFeSi-based compounds of 2.0 μm or more can be suppressed, and the mechanical properties can be improved.

[0022] (Cr: 0.050% by mass or more, 0.30% by mass or less) Cr forms fine granular crystallized products containing intermetallic compounds such as Al-Mn-Cr-Fe-Si and Al-Fe-Cr in the aluminum alloy, thereby improving the tensile strength of the aluminum alloy. By ensuring that the Cr content is within the above range, the mechanical properties of the aluminum alloy ingot at room temperature can be improved.

[0023] (Ti: 0.010% by mass or more, 0.10% by mass or less) Ti has the effect of refining the crystal grains of an aluminum alloy and improving its wrought workability. If the Ti content is less than 0.010% by mass, the effect of refining the crystal grains may not be sufficiently obtained. On the other hand, if the Ti content exceeds 0.10% by mass, coarse crystals may be formed, which may reduce the wrought workability. Furthermore, if a large amount of coarse crystals containing Ti are mixed into an aluminum alloy ingot, the toughness may be reduced. Therefore, the Ti content is set to 0.010% by mass or more, and 0.10% by mass or less. The Ti content is preferably 0.015% by mass or more, and 0.050% by mass or less.

[0024] (B: 0.0010% by mass or more, 0.030% by mass or less) B has the effect of refining the crystal grains of an aluminum alloy and improving its wrought workability. Adding B to an aluminum alloy together with the above-mentioned Ti improves the effect of refining the crystal grains. If the B content is less than 0.0010% by mass, the effect of refining the crystal grains may not be sufficient. On the other hand, if the B content exceeds 0.030% by mass, coarse crystals may be formed and may be mixed into the aluminum alloy ingot as inclusions. Furthermore, if a large amount of coarse crystals containing B are mixed into the final aluminum alloy product, the toughness may be reduced. Therefore, the B content is set to 0.0010% by mass or more, and 0.030% by mass or less. The B content is preferably 0.0050% by mass or more, and 0.025% by mass or more.

[0025] (Zr: 0.0010 mass % or more, 0.050 mass % or less) When Zr is 0.050 mass % or less, Al 3 Precipitation in the form of Zr and Al-(Ti,Zr) contributes to improving the strength of aluminum alloy ingots through recrystallization suppression effects and precipitation strengthening. However, if the Zr content exceeds 0.050 mass%, coarse Zr compounds may crystallize, potentially leading to a decrease in the corrosion resistance of the aluminum alloy ingot. For this reason, the Zr content is set to 0.050 mass% or less. Furthermore, in order to obtain the above-mentioned recrystallization suppression effects and the effects of improving the strength of forged products through precipitation strengthening, the Zr content is preferably 0.0010 mass% or more.

[0026] (Zn: 0.250 mass% or less) Zn may be 0.250 mass% or less. If the Zn content exceeds 0.250 mass%, MgZn 2 The Zn content is preferably 0.250 mass% or less, or is preferably zero.

[0027] (Inevitable impurities) Inevitable impurities are impurities that are inevitably mixed into the aluminum alloy from the raw materials or manufacturing process of the aluminum alloy ingot. Examples of inevitable impurities include Ni, Sn, and Be. The content of these inevitable impurities preferably does not exceed 0.1% by mass.

[0028] [Method for manufacturing aluminum alloy ingot] Next, a method for manufacturing the aluminum alloy ingot of this embodiment will be described. The aluminum alloy ingot of this embodiment can be manufactured, for example, by a method including a melting (molten metal formation) step and a casting step. Here, the aluminum alloy ingot of this embodiment is characterized in that the melting step has two sub-steps (a primary melting step and a secondary melting step), and the casting step also has two sub-steps (a primary casting step and a secondary casting step (main casting step)). These sub-steps are performed in the order of the primary melting step → the primary casting step → the secondary melting step → the secondary casting step.

[0029] Both the primary casting process and the secondary melting process have in common that they are processes for forming a molten aluminum alloy. Both the primary casting process and the secondary casting process have in common that they are processes for producing an aluminum alloy ingot (rod).

[0030] <Primary Melting Step> In the primary melting step, a raw material containing aluminum alloy scrap, in which the content ratios of the above-described additive elements (Cu, Mg, Mn, Fe, Zn, Cr, Ti, B, Zr) are in the same compositional range as that of the aluminum alloy ingot to be produced, except that the content ratio of Si is 0.60 mass % or more and 0.90 mass % or less, is melted to obtain a primary molten metal.

[0031] 1 is a conceptual diagram illustrating a part of the method for producing an aluminum alloy ingot according to the present embodiment. Specifically, the diagram conceptually illustrates a flow in which raw materials including blended aluminum alloy scrap are prepared (raw material preparation step), the raw materials are then charged into a primary melting furnace and a primary melting step is performed to obtain a primary molten metal (primary melting step), the primary molten metal is temporarily solidified into an ingot (primary melt solidification (casting) step), and the ingot is then used as a raw material in a secondary melting furnace and a secondary melting step is performed to obtain a secondary molten metal (secondary melting step).

[0032] The primary melting process is carried out under conditions such that the input raw materials (feedstock) are completely melted. Examples of raw materials include aluminum alloy scrap, aluminum ingot (aluminum bullion), Cu scrap, and master alloys. The melting is carried out, for example, at a temperature of 780 to 850°C. Examples of aluminum alloy scrap include scrap of Al-Mn-based (3000 series) alloys such as aluminum cans and recycled aluminum can blocks, scrap of Al-Si-based (4000 series) alloys such as ADC12 and A356, scrap of Al-Mg-based (5000 series) alloys such as 5052 and 5083, and scrap of Al-Mg-Si-based (6000 series) alloys such as 6063 and 6061. Aluminum bullion (pure aluminum) is classified into normal purity bullion, high purity bullion, and alloy bullion based on its purity and composition, and can be divided into ingots (cast ingots for general raw materials), slabs (cast ingots prepared for rolling), billets (cast ingots prepared for extrusion), etc. based on its shape and use.

[0033] If the Si content is less than 0.60% by mass, for example, metallic Si or a Si-containing alloy is added to adjust the Si content to a range of 0.60% by mass to 0.90% by mass. Metallic Si is preferred as the additive material due to ease of adjustment. If the Si content exceeds 0.90% by mass, aluminum ingot or aluminum alloy scrap with a low Si content is added to adjust the Si content to a range of 0.60% by mass to 0.90% by mass. Examples of aluminum alloy scrap with a low Si content include 3000-series alloy scrap, scrap containing 5000-series alloy, and scrap containing 6000-series alloy. The Si content (component analysis) can be performed, for example, by optical emission spectroscopy.

[0034] When Si, Fe, and Mn are mixed in scrap and melted, Al-Fe-Mn-Si compounds are generated within a certain temperature range during the melting process. The amount of this compound generated is particularly affected by the amount of Si. If the amount generated increases, the melting temperature must be set to 850°C or higher to melt them. This is undesirable because it increases the energy used during melting. Furthermore, if the Si content falls below 0.6% by mass, too much Si is added in the secondary melting process, which takes time to completely melt the added Si, resulting in energy loss. Therefore, the Si content of the alloy composition obtained in the primary melting process must be 0.60% by mass or more and 0.90% by mass or less.

[0035] The higher the usage ratio (blending ratio) of aluminum alloy scrap in the raw materials, the more preferable it is in terms of improving the energy consumption rate during melting. The blending ratio of aluminum alloy scrap can be, for example, 50% or more. For example, it can be 60% or more, 70% or more, 80% or more, 90% or more, or 100%. On the other hand, although the effect of improving the energy consumption rate during melting is lower, the blending ratio of aluminum alloy scrap can also be less than 50%, for example, 40%, 30%, 20%, or 10%.

[0036] The melting point of pure aluminum is approximately 660°C. In contrast, ADC12, for example, has a melting point of 570°C, and other aluminum alloys have melting points of 650°C or less, which is 10°C or more lower. Therefore, it melts easily, and by utilizing this, the energy consumption rate during melting can be improved.

[0037] Aluminum alloy scrap can be used within the composition ranges listed below. Examples of aluminum alloy scrap include Al-Si (4000 series) alloys such as ADC12 and A356, which contain 4% to 12% by weight of Si and 0.01% to 3.0% by weight of Cu; Al-Mn (3000 series) alloys such as other aluminum cans and recycled aluminum can blocks, which contain 0.7% to 1.4% by weight of Mn and 0.5% to 1.4% by weight of Mg; Al-Mg (5000 series) alloys such as 5052 and 5083, which contain 2.0% to 5.0% by weight of Mg; and Al-Mg-Si (6000 series) alloys such as 6063 and 6061, which contain 0.2% to 0.8% by weight of Si and 0.45% to 1.2% by weight of Mg. Aluminum can scrap is usually subjected to a heat treatment process at 400 to 500°C to remove paint from the can surface before being melted. By adding an Al-Si alloy, the amount of Si added in the secondary melting step can be reduced, so it is preferable to use this in combination with scrap of other alloy types.

[0038] <Primary Casting Step> The primary casting step is a step in which the primary molten metal obtained in the primary melting step is solidified into an ingot. During this step, the cooling rate from the liquidus temperature to the solidus temperature of the final solidification portion of the ingot is set to 10°C / sec or more. The cooling rate of the final solidification portion was calculated by measuring the temperature of the central portion of the ingot, which is the final solidification portion, using a thermocouple. For example, a K-type thermocouple (positive electrode: chromel, negative electrode: alumel) can be used.

[0039] Here, as is well known, the "final solidification portion" of the ingot refers to the portion of the molten metal where solidification is complete. When the molten metal is poured into a mold, it cools and solidifies starting from the vicinity of the wall surface of the mold, and the portion of the molten metal at the opening surface of the mold solidifies last. This final solidification portion is the portion of the molten metal that finally solidifies after 95% of the volume of the molten metal in the mold has solidified. In this specification, the "final solidification portion" refers to the portion of the molten metal that finally solidifies after 95% of the volume of the molten metal in the mold has solidified.

[0040] The approximate position of the "final solidification zone" is shown using the vertical continuous casting apparatus shown in FIG. 2 and the horizontal (horizontal) continuous casting apparatus shown in FIG.

[0041] The continuous casting mold 200 of the vertical continuous casting machine shown in FIG. 2 is cylindrical with a circular cross-section molding hole 11 open at both ends. It is composed of a cylindrical mold body 200A and a cylindrical carbon ring 200B fitted into the molding hole 11 and attached to the inner peripheral surface 200Aa of the mold body 200A. One end of the molding hole 11 is an inlet 12 for molten metal M, and the other end is a casting outlet 13 for an ingot S. The mold body 200A also has a cavity 21 through which cooling water C flows. An inlet 22 leading to the cavity 21 is provided at the top, and a jet outlet 23 is provided surrounding the casting outlet 13. The cooling water C introduced through the inlet 22 is primarily cooled and solidified through the carbon ring 200B, and is then sprayed onto the ingot S being cast from the jet outlet 23, thereby secondary cooling the ingot S. In addition, a recess 26 having a thickness equivalent to the thickness of the carbon ring 200B is formed in the inner peripheral surface 200Aa of the mold body 200A except for a portion on the casting outlet 13 side. fは The final solidification portion is indicated by the symbol T h indicates the location where the temperature is measured with a thermocouple to measure the cooling rate of the final solidification portion.

[0042] The horizontal continuous casting apparatus 2000 shown in Figure 3 includes a molten metal receiving section (not shown) with a tap port on its side wall, a molten metal pouring nozzle 20 with a circular molten metal pouring passage, and a continuous casting mold 400 having a cylindrical mold body 400A with a circular shaped molding hole 41. The continuous casting mold 400 shown in Figure 3 includes a cylindrical mold body 400A with a molten metal pouring inlet 12 at one end and an ingot pouring outlet 13 at the other end, and a carbon ring 400B fitted into the molding hole 41 and disposed on the inner circumferential surface 400Aa of the mold body 400A. A lubricating oil supply pipe 43 opening into the molding hole 41 is provided at the inlet side of the molding hole 41. The mold body 400A has a cavity 42 therein through which cooling water C flows, and a jetting port 44 is provided surrounding the casting outlet 13. Cooling water C introduced from an inlet (not shown) flows through the cavity 42, primarily cooling and solidifying the molten metal M in the forming hole 41 via the mold body 400A and the carbon ring 400B, and is then sprayed onto the ingot S being cast out from the nozzle 44, thereby secondary cooling the ingot S. In addition, a recess corresponding to the thickness of the carbon ring 400B is formed in the inner peripheral surface 400Aa of the mold body 400A, except for a portion on the casting outlet 13 side. In FIG. 3, the symbol S fは The final solidification portion is indicated by the symbol T h indicates the location where the temperature is measured with a thermocouple to measure the cooling rate of the final solidification portion.

[0043] Specifically, the primary casting process involves pouring the molten metal obtained in the primary melting process into a mold made of cast iron or the like to solidify the ingot. The mold temperature is controlled so that the cooling rate of the final solidification portion of the ingot is 10°C / sec or higher. Casting can be performed by pouring the molten metal into a stationary mold and solidifying it, or by vertical continuous casting. When casting the molten metal into a stationary mold, the mold temperature can be 200°C or lower, preferably 100°C or lower. If the cooling rate exceeds 10°C / sec, Al-Fe-Mn-Si compounds grow coarsely in the final solidification portion, and these compounds cannot be decomposed unless they are melted at a temperature exceeding 800°C in the secondary melting process. If the secondary melting process and casting are performed without decomposition, the undissolved Al-Fe-Mn-Si compounds will remain in the product and impair its mechanical properties. When melting is carried out at a temperature exceeding 800°C, oxidation consumption during melting is accelerated, resulting in a large loss of material.

[0044] <Second Melting Step> The second melting step is a step of adding metallic Si or a Si-containing alloy to the molten metal obtained by melting the ingot obtained in the first casting step to adjust the Si content to 0.90% by mass or more and 1.9% by mass. Metallic Si is preferred as the additive material because it is easy to adjust.

[0045] The composition adjustment here is carried out at a temperature between 700°C and 800°C. If the temperature is below 700°C, the temperature drop in the molten metal path when the molten metal is cast causes the Al-Fe-Mn-Si compounds to grow coarsely, impairing the mechanical properties of the product. Also, if the temperature exceeds 800°C, the amount of hydrogen dissolved in the atmosphere into the molten aluminum increases, increasing the amount of hydrogen gas in the molten metal, resulting in the generation of porosity in the cast product and impairing the mechanical properties. Therefore, the temperature range of 700°C to 800°C is preferable.

[0046] <Secondary Casting Step (Main Casting Step)> The molten metal obtained in the secondary melting step is subjected to flux treatment and then GBF (gas bubbling filtration) treatment before being poured into a casting mold. The poured molten metal is then continuously cast by either vertical or horizontal continuous casting to produce a continuously cast aluminum alloy rod.

[0047] [Continuously Cast Aluminum Alloy Rod] The continuously cast aluminum alloy rod according to this embodiment is produced by continuous casting, either vertical (vertical) continuous casting or horizontal (horizontal) continuous casting, using an aluminum alloy ingot obtained by the method for producing an aluminum alloy ingot according to this embodiment, and has a 0.2% yield strength of 350 MPa or more.

[0048] [Aluminum Alloy Forgings] The aluminum alloy forgings according to this embodiment are produced using the continuously cast aluminum alloy rod according to this embodiment, and have a 0.2% proof stress of 370 MPa or more. For example, the aluminum alloy forgings according to this embodiment can be produced by subjecting the continuously cast aluminum alloy rod according to this embodiment to a homogenization heat treatment step, a forging step, a solution treatment step, a quenching treatment step, and an aging treatment step.

[0049] Next, specific examples of the present invention will be described, but the present invention is not limited to these examples.

[0050] (Examples of Aluminum Alloy Scrap) Aluminum alloy scrap obtained from a secondary alloy manufacturer and a scrap manufacturer was analyzed by optical emission spectroscopy to obtain component analysis values ​​(mass%) for each scrap, which are shown in Table 1. The component analysis was carried out in accordance with the optical emission spectroscopy analysis of aluminum and aluminum alloys specified in JIS H1305 2005.

[0051]

[0052] (Examples 1 to 6, Comparative Examples 1 to 6) The compositions of the samples of Examples 1 to 6 and Comparative Examples 1 to 6 are as follows: In Examples 1 to 6, the combinations (mixtures) of aluminum alloy scrap and aluminum ingot shown in Table 1, or only aluminum alloy scrap, were used as raw materials. In both the examples and comparative examples, the contents of additive elements other than Si were as follows: Cu in the range of 0.30% by mass to 1.0% by mass, Mg in the range of 0.80% by mass to 1.8% by mass, Mn in the range of 0.30% by mass to 1.2% by mass, Fe in the range of 0.20% by mass to 0.65% by mass, Zn in the range of 0.25% by mass, Cr in the range of 0.050% by mass to 0.30% by mass, Ti in the range of 0.01% by mass to 0.1% by mass, B in the range of 0.0010% by mass to 0.030% by mass, and Zr in the range of 0.0010% by mass to 0.050% by mass, with the balance being Al and inevitable impurities. Furthermore, in the examples, the Si content was in the range of 0.60% by mass to 0.90% by mass. On the other hand, in the comparative examples, the Si content was blended so as to be outside the range of 0.60 mass % or more and 0.90 mass % or less.

[0053] In both the examples and comparative examples, the melting and casting processes were performed using a vertical continuous casting machine. In the examples, the molten metal obtained in the primary melting process was first poured into a cast iron mold to perform pour casting, thereby obtaining an ingot. When casting into an ingot, casting was performed so that the cooling rate of the final solidification portion was 10°C / sec or higher. Specifically, a 5 kg ingot was cast at a mold temperature of 200°C or lower. On the other hand, in the comparative example, when casting into an ingot from the molten metal obtained in the primary melting process, casting was performed so that the cooling rate of the final solidification portion exceeded 10°C / sec. Specifically, a 5 kg ingot was cast at a mold temperature exceeding 200°C. The cooling rate of the final solidification portion was measured using a K-type thermocouple at the center of the ingot, which is the final solidification portion, as shown in Figure 2, and the cooling rate from the liquidus temperature to the solidus temperature was calculated.

[0054] For each of the Examples and Comparative Examples, the ingots obtained in the primary casting step were used in the secondary melting step, where melting and composition adjustment were carried out. The secondary melting was carried out at 780°C. After the raw materials were melted, the presence or absence of hearth sediment (remaining material on the hearth) was confirmed using a jig. The resulting molten metal was then cast in the main casting step to obtain continuously cast rods.

[0055] The casting conditions in this casting process were as follows: Casting diameter: 82 mm Casting speed: 230 mm / min Cooling water amount: 30 L / min Casting temperature: 720°C

[0056] <Evaluation after secondary melting step> As described above, the presence or absence of hearth bottom sediment (Al-Fe-Mn-Si compounds) was confirmed after secondary melting at 780°C. Those without hearth bottom sediment were marked with a "good" and those with hearth bottom sediment were marked with an "x." An iron stirring tool was used to check for hearth bottom sediment. When the stirring tool came into contact with the hearth bottom sediment, it felt like hitting a pebble.

[0057] <Evaluation of Continuously Cast Rods (Tensile Properties)> The tensile properties of the obtained continuously cast aluminum alloy rods 10 were measured by the following method. The tensile properties were evaluated in accordance with ASTM-E8 standard. That is, referring to FIGS. 4( a) and 4(b), tensile test specimens with a gauge length of 25.4 mm and a parallel portion diameter of 6.4 mm were taken from the central region 10b extending in the casting direction of the continuously cast aluminum alloy rod 10. The obtained test specimens were subjected to a tensile test at room temperature (25°C) at a rate of 2 mm / min to measure the 0.2% proof stress. The results are shown in Table 2.

[0058] <Evaluation of Forged Products (Tensile Properties)> As shown in Figure 5, a continuously cast aluminum alloy rod 10 with a diameter of 82 mm was upset from its side to a thickness of 41 mm to produce a 50% upset product. The product underwent T6 treatment under the following conditions and a tensile test was then performed: forging conditions: forging temperature 520°C; T6 treatment conditions: 3 hours at 540°C (solution treatment), followed by quenching (water temperature 40°C), followed by 6 hours at 180°C (aging treatment). The 0.2% proof stress of this tensile test specimen was measured by tensile testing at room temperature (25°C) at a rate of 2 mm / min. The results are shown in Table 2.

[0059]

[0060] As can be seen from Table 2, after the secondary melting step, none of the Examples had hearth bottom sediment (Al-Fe-Mn-Si compounds), whereas all of the Comparative Examples had hearth bottom sediment (Al-Fe-Mn-Si compounds). Furthermore, all of the continuously cast aluminum alloy rods of the Examples had a 0.2% yield strength of 350 MPa or more, whereas all of the continuously cast aluminum alloy rods of the Comparative Examples had a 0.2% yield strength of less than 350 MPa. Furthermore, all of the aluminum alloy forged products of the Examples had a 0.2% yield strength of 370 MPa or more, whereas all of the aluminum alloy forged products of the Comparative Examples had a 0.2% yield strength of less than 350 MPa.

[0061] 10. Aluminum alloy continuously cast rod

Claims

1. A method for producing an aluminum alloy ingot containing additive elements of Cu in the range of 0.30 mass% to 1.0 mass%, Mg in the range of 0.80 mass% to 1.8 mass%, Si in the range of 0.90 mass% to 1.9 mass%, Mn in the range of 0.30 mass% to 1.2 mass%, Fe in the range of 0.20 mass% to 0.65 mass%, Zn in the range of 0.25 mass% or less, Cr in the range of 0.050 mass% to 0.30 mass%, Ti in the range of 0.01 mass% to 0.1 mass%, B in the range of 0.0010 mass% to 0.030 mass%, and Zr in the range of 0.0010 mass% to 0.050 mass%, with the balance being Al and unavoidable impurities, 1. A method for producing an aluminum alloy ingot, comprising: a primary melting step of melting a raw material containing aluminum alloy scrap, the raw material having the same composition range as that of the aluminum alloy ingot except that the Si content is 0.60% by mass or more and 0.90% by mass or less, to obtain a primary molten metal; a primary casting step of solidifying the primary molten metal obtained in the primary melting step into an ingot, the primary casting step being a cooling rate from the liquidus temperature to the solidus temperature of a final solidification portion of the ingot of 10° C. / sec or more; and a secondary melting step of adding metallic Si or a Si-containing alloy to the molten metal obtained by melting the ingot obtained in the primary casting step to adjust the Si content to be within the range of 0.90% by mass or more and 1.9% by mass or less.

2. The method for producing an aluminum alloy ingot as set forth in claim 1, wherein the aluminum alloy scrap comprises at least one of scrap containing a 3000 series alloy, scrap containing a 4000 series alloy, scrap containing a 5000 series alloy, and scrap containing a 6000 series alloy.

3. A continuously cast aluminum alloy rod obtained using an aluminum alloy ingot produced by the method for producing an aluminum alloy ingot according to claim 1 or 2, and having a 0.2% yield strength of 350 MPa or more.

4. An aluminum alloy forging obtained by using the aluminum alloy continuously cast rod described in claim 3 and having a 0.2% yield strength of 370 MPa or more.

Citation Information

Patent Citations

  • High-strength and high-toughness aluminum alloy forged material

    JP2000144296A

  • Automobile chassis parts and its manufacturing method

    JP2008163445A

  • Aluminum alloy for die casting with improved corrosion resistance, frequency filter and method for manufacturing communication equipment parts

    JP2017538031A

  • Aluminum alloy recycling method and its refinement

    JP2020531685A

  • Aluminum alloy forging and method for producing the same

    JP2022093988A

Cited By

  • Al-Mg-Zn-Zr aluminum alloy round cast ingot and preparation method thereof

    CN119710388A