Cathod active material for lithium secondary battery and manufacturing method therefor
A bimodal manganese-rich and high nickel-based cathode active material with dual redox capabilities and optimized particle sizes addresses the structural instability and cost issues of manganese-rich cathode materials, improving performance and safety while reducing gas generation and voltage decay.
Patent Information
- Application Number
- PCT/KR2024/001830
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-25
- Filing Date
- 2024-02-07
- Publication Date
- 2024-11-28
AI Technical Summary
Manganese-rich cathode active materials for lithium secondary batteries face challenges due to structural instability and continuous anion redox, leading to voltage decay and gas generation, which hinder commercialization, and are also affected by the volatile price of nickel.
A bimodal (Mn-rich) layered cathode active material with a high nickel-based NCM layered single crystal cathode material mixed at a certain ratio, utilizing dual redox mechanisms and specific particle size ratios to reduce gas generation and improve lifespan, while lowering raw material costs.
The solution significantly reduces gas generation and voltage decay, enabling commercialization by enhancing the performance and safety of manganese-rich cathode active materials, and achieves a cost reduction of at least 10% compared to traditional high nickel materials.
Smart Images

Figure KR2024001830_28112024_PF_FP_ABST
Abstract
Description
Cathode active material for lithium secondary batteries and method for producing the same
[0001] The present examples relate to a cathode active material for a lithium secondary battery and a method for producing the same, and more particularly, to a cathode active material for a lithium secondary battery including a manganese-rich cathode active material and a high-nickel cathode active material and a method for producing the same.
[0002]
[0003] NCM layered cathode active materials show a characteristic of linearly increasing capacity with increasing nickel content, and are known to be suitable materials for increasing the driving range of electric vehicles due to increased energy density. However, due to the instability of nickel supply and demand, the price of the cathode active material itself also has a disadvantage of greatly fluctuating prices every year. On the other hand, manganese is relatively inexpensive, so if the content of manganese is increased compared to nickel in the layered cathode material, a composite of Li2MnO3 and LiNi(Co,Mn,Al) is formed inside the cathode material particles, and when the initial charge voltage is charged at a high voltage of 4.5 V or higher, not only the cation redox of LiNi(Co,Mn,Al) on LiNiO2 but also oxygen redox on Li2MnO3 occurs simultaneously, so a high capacity of more than 250 mAh / g can be realized. However, these Mn-rich cathode active materials have been unable to be commercialized despite extensive research due to the structural instability that occurs during charge and discharge cycles, and the continuous generation of oxygen due to continuous anion redox.
[0004] The present invention is to solve the above problems, and the core of the present invention is to configure a bimodal form in which a manganese-rich layered cathode active material large particle and a high-nickel NCM layered single crystal cathode material are mixed at a certain ratio, and by having the advantage of the manganese-rich cathode active material, which is the dual redox using cation and anion redox, and the advantage of the single particle, which is the effect of reducing gas generation and improving life characteristics, it can improve the performance compared to the bimodal form in which the existing manganese-rich cathode active material large particle and small particle are mixed.
[0005]
[0006] The present invention aims to provide a cathode active material with improved performance that enables commercialization by significantly reducing gas generation and voltage decay due to continuous anion redox during charge and discharge cycles of manganese-rich cathode active materials, which were the biggest obstacles to commercialization in the past.
[0007] In addition, the present invention aims to provide a new concept cathode active material and a manufacturing method thereof, which have improved safety compared to cathode materials composed of high-nickel cathode active materials with large and small particle sizes, while reducing the raw material cost by at least 10%.
[0008]
[0009] A cathode active material for a lithium secondary battery according to one embodiment of the present invention may include a lithium manganese-rich first cathode active material represented by the following chemical formula 1; and a high-nickel single-particle second cathode active material represented by the following chemical formula 2; wherein the average particle size (D50_1) of the lithium manganese-rich first cathode active material is larger than the average particle size (D50_2) of the high-nickel single-particle second cathode active material.
[0010] [Chemical Formula 1]
[0011] Li 1+x1 (Ni (1-a1-b1) Co a1 Mn b1 )O2
[0012] (Here, -0.5≤x1≤0.5, 0≤a1≤0.5, 0.5≤b1≤1.)
[0013] [Chemical Formula 2]
[0014] Li 1+x2 (Ni(1-a2-b2-c2)Co a2 Mn b2 M c2 )O2
[0015] (Here, -0.5≤x2≤0.5, 0≤a2≤0.2, 0≤b2≤0.1, 0≤c2≤0.03,
[0016] M is one or more elements selected from the group consisting of Fe, Cr, Ti, Zn, V, Al, Mg, and Zr.)
[0017] The ratio D50_1 / D50_2 of the average particle size (D50_1) of the lithium manganese-rich first positive electrode active material to the average particle size (D50_2) of the high-nickel single-particle second positive electrode active material may be 2.5 to 4.5.
[0018] The average particle size (D50_1) of the lithium manganese-rich first positive electrode active material may be 7 µm to 15 µm, and the average particle size (D50_2) of the high-nickel single-particle second positive electrode active material may be 3 µm to 6 µm.
[0019] The above lithium manganese-rich first positive electrode active material may be a secondary particle composed of a plurality of primary particles.
[0020] The weight (w1) ratio of the lithium manganese-rich first positive electrode active material to the weight (w2) of the high-nickel single-particle second positive electrode active material may be 85:15 to 55:45, w1 / w2.
[0021] The manganese molar content (C) based on the total amount of metal excluding lithium in the above high-nickel single-particle second cathode active material Mn2 ) based on the total amount of metal excluding lithium in the first positive electrode active material of lithium manganese-rich system, manganese molar content (C Mn1 )Rain (CMn1 / C Mn2 ) can be between 15.0 and 70.0.
[0022] The manganese molar content (C) based on the total amount of metal excluding lithium in the first positive electrode active material Mn1 ) and manganese molar content (C) based on the total amount of metal excluding lithium in the second positive electrode active material Mn2 ) difference (C Mn1 -C Mn2 ) can be 50 mol% to 70 mol%.
[0023] Nickel molar content (C) based on the total amount of metal excluding lithium in the first positive electrode active material Ni1 ) Nickel molar content (C) based on the total amount of metal excluding lithium in the second positive electrode active material Ni2 ) Rain (C) Ni2 / C Ni1 ) can be 2.0 to 3.0.
[0024] Nickel molar content (C) based on the total amount of metal excluding lithium in the above second positive electrode active material Ni2 ) and nickel molar content (C) based on the total amount of metal excluding lithium in the first cathode active material Ni1 ) difference (C Ni2 -C Ni1 ) can be 45 mol% to 65 mol%.
[0025] The above lithium manganese-rich first cathode active material may be formed at a voltage of 4.6 V to 4.8 V.
[0026] The tap density of the positive electrode active material for the above lithium secondary battery is 1.90 g / cm 3 2.20g / cm 3 and the specific surface area is 2.0cm 2 / g to 3.0cm 2 / g may be.
[0027] In addition, the positive electrode active material for the lithium secondary battery can satisfy the following relationship 1.
[0028] [Relationship 1]
[0029] 0.77 ≤ m / B*10^4 ≤ 0.95
[0030] (Here, m is the tap density (g / cm) of the positive electrode active material for lithium secondary batteries. 3 ), and B is the specific surface area (m) of the positive electrode active material for lithium secondary batteries. 2 / g) is.)
[0031] In the second positive electrode active material, the nickel molar content based on the total amount of metals excluding lithium may be 80 mol% or more, and in the first positive electrode active material, the manganese molar content based on the total amount of metals excluding lithium may be 50 mol% or more.
[0032] A method for manufacturing a positive electrode active material for a lithium secondary battery according to another embodiment of the present invention may include: a step of preparing a lithium manganese-rich first positive electrode active material represented by the following chemical formula 1; a step of preparing a high-nickel single-particle second positive electrode active material represented by the following chemical formula 2; and a step of manufacturing a positive electrode active material by mixing the first positive electrode active material and the second positive electrode active material.
[0033] [Chemical Formula 1]
[0034] Li 1+x1 (Ni (1-a1-b1) Co a1 Mn b1 )O2
[0035] (Here, -0.5≤x1≤0.5, 0≤a1≤0.2, 0.5≤b1<1.)
[0036] [Chemical Formula 2]
[0037] Li 1+x2 (Ni(1-a2-b2-c2)Co a2 Mn b2 M c2 )O2
[0038] (Here, -0.5≤x2≤0.5, 0≤a2<0.2, 0≤b2≤0.1, 0≤c2<0.03,
[0039] M is one or more elements selected from the group consisting of Fe, Cr, Ti, Zn, V, Al, Mg, and Zr.)
[0040] Meanwhile, the average particle size (D50_1) of the lithium manganese-rich first cathode active material is larger than the average particle size (D50_2) of the high-nickel single-particle second cathode active material.
[0041] The step of preparing the lithium manganese-rich first positive electrode active material may include a step of forming the lithium manganese-rich first positive electrode active material at a voltage of 4.6 V to 4.8 V.
[0042] The step of forming the lithium manganese-rich first cathode active material at a voltage of 4.6 V to 4.8 V may include a step of charging the first cathode active material to 4.6 V to 4.8 V at a temperature of 40° C. to 50° C. under a current condition of 0.1 C, and then applying a constant voltage to maintain the charging until the current drops to a condition of 1 / 20 C.
[0043] In addition, the step of forming the lithium manganese-rich first positive electrode active material under voltage conditions of 4.6 V to 4.8 V may include a step of discharging under current conditions of 0.1 C.
[0044] The step of preparing the lithium manganese-rich first positive electrode active material is to prepare a lithium manganese-rich first positive electrode active material having an average particle size (D50_1) in the range of 7 ㎛ to 15 ㎛, and the step of preparing the high-nickel-based single-particle second positive electrode active material is to prepare a high-nickel-based single-particle second positive electrode active material having an average particle size (D50_2) in the range of 3 ㎛ to 6 ㎛.
[0045] The step of manufacturing a positive electrode active material by mixing the first positive electrode active material and the second positive electrode active material is to mix the weight (w1) of the lithium manganese-rich first positive electrode active material to the weight (w2) of the high-nickel single-particle second positive electrode active material in a ratio w1 / w2 of 85:15 to 55:45.
[0046] The step of manufacturing a positive electrode active material by mixing the first positive electrode active material and the second positive electrode active material is to manufacture a positive electrode active material that satisfies the following relationship 1.
[0047] [Relationship 1]
[0048] 0.77 ≤ m / B*10^4 ≤ 0.95
[0049] (Here, m is the tap density (g / cm) of the positive electrode active material for lithium secondary batteries. 3 ), and B is the specific surface area (m) of the positive electrode active material for lithium secondary batteries. 2 / g) is.)
[0050] A positive electrode for a lithium secondary battery according to another embodiment of the present invention may include: a current collector; and a positive electrode active material layer positioned on at least one surface of the current collector and including the positive electrode active material for a lithium secondary battery.
[0051] A lithium secondary battery according to another embodiment of the present invention includes the above-described positive electrode for a lithium secondary battery.
[0052] Additionally, the lithium secondary battery may have an average voltage decay of 40 mV to 65 mV after 50 charging and discharging cycles.
[0053] The above lithium secondary battery satisfies the following relationship 2.
[0054] [Relationship 2]
[0055] 50 ≤△V / (m / B*10^4) ≤ 80
[0056] (Here, △V is the voltage decay after 50 cycles of charging and discharging compared to the initial charging and discharging of a lithium secondary battery, and m is the tap density (g / cm) of the positive electrode active material for a lithium secondary battery. 3 ), and B is the specific surface area (m) of the positive electrode active material for lithium secondary batteries. 2 / g) is.)
[0057] The above lithium secondary battery satisfies the following relationship 3.
[0058] [Relationship 3]
[0059] 3.0 ≤G / (m / B*10^4) ≤ 5.0
[0060] (Here, G is the gas generation amount of the lithium secondary battery, and m is the tap density (g / cm) of the positive electrode active material for the lithium secondary battery. 3 ), and B is the specific surface area (m) of the positive electrode active material for lithium secondary batteries. 2 / g) is.)
[0061] The above lithium secondary battery satisfies the following relationship 4.
[0062] [Relationship 4]
[0063] 250.0 ≤ (G / Em) / (m / B*10^4) ≤ 400.0
[0064] (Here, G is the gas generation amount of the lithium secondary battery, Em is the loading amount of the positive electrode active material in the positive electrode of the lithium secondary battery, and m is the tap density (g / cm) of the positive electrode active material for the lithium secondary battery. 3 ), and B is the specific surface area (m) of the positive electrode active material for lithium secondary batteries. 2 / g) is.)
[0065]
[0066] The cathode active material for a lithium secondary battery according to the present invention has the advantage of reducing gas generation and voltage drop.
[0067] In addition, the method for manufacturing a positive electrode active material for a lithium secondary battery according to the present invention has the advantage of being able to obtain a positive electrode active material for a lithium secondary battery with reduced gas generation and voltage drop.
[0068]
[0069] FIG. 1 shows a cross-sectional SEM image of a positive electrode plate including a positive electrode active material for a lithium secondary battery according to one embodiment.
[0070] Figure 2 shows the results of EDS (Energy-dispersive X-ray spectroscopy) analysis for the positive electrode active material according to Example 1.
[0071] Figure 3 shows a cross-sectional SEM image of a positive electrode plate after performing 100 charging and discharging cycles on a coin cell using a positive electrode active material according to Example 1.
[0072] Figure 4 shows a cross-sectional SEM image of a positive electrode plate after performing 100 charging and discharging cycles on a coin cell using a positive electrode active material according to Comparative Example 1.
[0073]
[0074] In the description of the present invention, terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, a first part, component, region, layer, or section described below may be referred to as a second part, component, region, layer, or section without departing from the scope of the present invention.
[0075] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the present invention. As used herein, the singular forms "singular" and "comprising" include plural forms as well, unless the context clearly dictates otherwise. The word "comprising" as used herein specifies a particular feature, region, integer, step, operation, element, and / or component, but does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, and / or components.
[0076] Although not defined otherwise, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with the relevant technical literature and the present disclosure, and are not to be construed as ideal or overly formal unless otherwise defined.
[0077] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and the present invention is not limited thereto, and the present invention is defined only by the scope of the claims set forth below.
[0078]
[0079] <Cathode active material for lithium secondary batteries>
[0080] A cathode active material for a lithium secondary battery according to one embodiment of the present invention may include a lithium manganese-rich first cathode active material and a high-nickel single-particle second cathode active material.
[0081] The above lithium manganese-rich first cathode active material may be a manganese-rich cathode active material, and the above high-nickel single-particle second cathode active material may be a high-nickel cathode active material.
[0082] The ratio D50_1 / D50_2 of the average particle size (D50_1) of the lithium manganese-rich first positive electrode active material to the average particle size (D50_2) of the high-nickel single-particle second positive electrode active material may be in the range of 1 to 10, specifically in the range of 1.5 to 5.0, and more specifically in the range of 2 to 4.
[0083] Meanwhile, the lithium manganese-rich first cathode active material may be a secondary particle composed of a plurality of primary particles, and may be represented by the following chemical formula 1.
[0084] [Chemical Formula 1]
[0085] Li 1+x1 (Ni (1-a1-b1) Co a1 Mn b1 )O2
[0086] Here, -0.5≤x1≤0.5, 0≤a1≤0.2, 0.5≤b1<1.
[0087]
[0088] The above high-nickel single-particle second positive electrode active material can be represented by the following chemical formula 2.
[0089] [Chemical Formula 2]
[0090] Li 1+x2 (Ni(1-a2-b2-c2)Co a2 Mn b2 M c2 )O2
[0091] Here, -0.5≤x2≤0.5, 0≤a2<0.2, 0≤b2≤0.1, 0≤c2<0.03,
[0092] M is one or more elements selected from the group consisting of Fe, Cr, Ti, Zn, V, Al, Mg, and Zr.
[0093] The above lithium manganese-rich first cathode active material may be a manganese-rich cathode active material, and has a manganese molar content (C) based on the total amount of metal excluding lithium. Mn1) may be 55 mol% or more. In addition, the average particle size (D50_1) of the secondary particles may be in the range of 7 ㎛ to 15 ㎛, and specifically, may be in the range of 8 ㎛ to 14 ㎛.
[0094] The above high-nickel single-particle second cathode active material may be a high-nickel (high Ni) cathode active material, and has a nickel molar content (C) based on the total amount of metal excluding lithium. Ni1 ) may be 80 mol% or more, and specifically, may be 85 mol% or more. In addition, the average particle size (D50_2) of the high-nickel single-particle second positive electrode active material may be in the range of 3 μm to 6 μm, and specifically, may be in the range of 3 μm to 5 μm.
[0095] Meanwhile, the ratio D50_1 / D50_2 of the average particle size (D50_1) of the lithium manganese-rich first positive electrode active material to the average particle size (D50_2) of the high-nickel single-particle second positive electrode active material may be 1.0 to 5.0, specifically 1.5 to 4.5, and more specifically 2.5 to 4.5.
[0096] In the present invention, the “average particle size (D50)” of the positive electrode active material may be measured by a general method using a particle size analyzer.
[0097] In the present invention, the metal composition and content of the positive electrode active material can be analyzed using ICP-OES (OPTIMA 8300, Perkin Elmer).
[0098]
[0099] The manganese molar content (C) based on the total amount of metal excluding lithium in the above high-nickel single-particle second cathode active material Mn2 ) based on the total amount of metal excluding lithium in the first positive electrode active material of lithium manganese-rich system, manganese molar content (C Mn1 )Rain (C Mn1 / C Mn2) may be 15.0 to 70.0, specifically 19.0 to 66.0, and more specifically 19.2 to 65.5.
[0100] The manganese molar content (C) based on the total amount of metal excluding lithium in the first positive electrode active material Mn1 ) and manganese molar content (C) based on the total amount of metal excluding lithium in the second positive electrode active material Mn2 ) difference (C Mn1 -C Mn2 ) may be 50 mol% to 70 mol%, and specifically 54 mol% to 65 mol%.
[0101] Nickel molar content (C) based on the total amount of metal excluding lithium in the first positive electrode active material Ni1 ) Nickel molar content (C) based on the total amount of metal excluding lithium in the second positive electrode active material Ni2 ) Rain (C) Ni2 / C Ni1 ) may be 2.0 to 3.0, and specifically 2.4 to 2.8. In addition, the nickel molar content (C) based on the total amount of metal excluding lithium in the second positive electrode active material Ni2 ) and nickel molar content (C) based on the total amount of metal excluding lithium in the first cathode active material Ni1 ) difference (C Ni2 -C Ni1 ) may be 45 mol% to 65 mol%, and specifically 48 mol% to 60 mol%.
[0102]
[0103] In addition, the weight (w1) ratio w1 / w2 of the lithium manganese-rich first positive electrode active material to the weight (w2) of the high-nickel single-particle second positive electrode active material may be in the range of 85:15 to 55:45, and specifically, may be 80:20 to 60:40.
[0104] When the lithium manganese-rich first cathode active material and the high-nickel single-particle second cathode active material satisfy the above-mentioned size range and ratio, the integration density of the cathode active material for a lithium secondary battery within a unit volume is improved, thereby increasing the energy density per unit volume.
[0105]
[0106] The lithium manganese-rich first cathode active material according to the present invention may be formed by a high voltage, and specifically, the active material may be formed by a voltage of 4.6 V to 4.8 V. In this way, the lithium manganese-rich first cathode active material, which is manganese-rich, can sufficiently release oxygen (O2) by being formed by a high voltage, and can significantly reduce gas generation and voltage decay due to continuous anion redox during charge and discharge cycles, which is advantageous in expressing high capacity.
[0107]
[0108] The tap density of the positive electrode active material for the above lithium secondary battery is 1.90 g / cm 3 2.20g / cm 3 It can be, specifically, 1.91g / cm 3 2.15g / cm 3 It could be.
[0109] In the present invention, “tap density” may be measured by dividing the weight of the positive electrode active material by the volume of the measured graduated cylinder after loading the graduated cylinder loaded with the positive electrode active material into a tap density measuring device and tapping it periodically more than 3,000 times.
[0110] When the tap density of the positive electrode active material for the lithium secondary battery satisfies the above range, there is an advantage in that the output characteristics and cycle life characteristics of the battery can be improved.
[0111]
[0112] A cathode active material for a lithium secondary battery comprising a lithium manganese-rich first cathode active material and a high-nickel single-particle second cathode active material according to one embodiment of the present invention has a specific surface area of 2.0 cm 2 / g to 3.0cm 2 / g can be, specifically 2.1cm 2 / g to 2.6cm 2 / g may be.
[0113] In the present invention, the “specific surface area” was measured using the Brunauer-Emmett-Teller Analysis method according to the nitrogen adsorption method, and a method of measuring the specific surface area of a material was adopted by measuring the adsorption amount according to partial pressure by adsorbing and desorbing nitrogen gas on the surface of a solid sample using the BET (Brunauer Emmett Teller) formula.
[0114] When the specific surface area of the positive electrode active material for the lithium secondary battery satisfies the above range, there is an advantage in that the output characteristics and cycle life characteristics of the battery can be improved.
[0115]
[0116] Meanwhile, a cathode active material for a lithium secondary battery including a lithium manganese-rich first cathode active material and a high-nickel single-particle second cathode active material according to one embodiment of the present invention can satisfy the following relationship 1.
[0117] [Relationship 1]
[0118] 0.77 ≤ m / B*10^4 ≤ 0.95
[0119] Here, m is the tap density (g / cm) of the positive electrode active material for lithium secondary batteries. 3 ), and B is the specific surface area (m) of the positive electrode active material for lithium secondary batteries. 2 / g) is.
[0120] The value of the above relational expression 1 of the positive electrode active material for a lithium secondary battery including the lithium manganese-rich first positive electrode active material and the high-nickel single-particle second positive electrode active material may be 0.77 to 0.95, and specifically, may be 0.82 to 0.95. When the value of the above relational expression 1 satisfies the above range, there is an advantage in that the output characteristics and cycle life characteristics of the excellent battery can be improved.
[0121]
[0122] <Method for manufacturing positive electrode active material for lithium secondary batteries>
[0123] Another embodiment of the present invention provides a method for producing a cathode active material for a lithium secondary battery, comprising the steps of: preparing a lithium manganese-rich first cathode active material; preparing a nickel-rich single-particle second cathode active material; and mixing the first cathode active material and the second cathode active material to produce a cathode active material.
[0124] The above lithium manganese-rich first cathode active material may be a manganese-rich cathode active material and may be represented by the following chemical formula 1. The above high-nickel single-particle second cathode active material may be a high-nickel cathode active material and may be represented by the following chemical formula 2.
[0125] The ratio D50_1 / D50_2 of the average particle size (D50_1) of the lithium manganese-rich first positive electrode active material to the average particle size (D50_2) of the high-nickel single-particle second positive electrode active material may be in the range of 1.5 to 5.0, and specifically, may be in the range of 2.5 to 3.5.
[0126] Meanwhile, the lithium manganese-rich first cathode active material may be a secondary particle composed of a plurality of primary particles, and may be represented by the following chemical formula 1.
[0127] [Chemical Formula 1]
[0128] Li 1+x1 (Ni (1-a1-b1) Co a1 Mn b1 )O2
[0129] Here, -0.5≤x1≤0.5, 0≤a1≤0.2, 0.5≤b1<1.
[0130]
[0131] The above high-nickel single-particle second positive electrode active material can be represented by the following chemical formula 2.
[0132] [Chemical Formula 2]
[0133] Li 1+x2 (Ni(1-a2-b2-c2)Co a2 Mn b2 M c2 )O2
[0134] Here, -0.5≤x2≤0.5, 0≤a2<0.2, 0≤b2≤0.1, 0≤c2<0.03,
[0135] M is one or more elements selected from the group consisting of Fe, Cr, Ti, Zn, V, Al, Mg, and Zr.
[0136] The above lithium manganese rich first cathode active material may be a manganese rich (Mn rich) cathode active material, and has a manganese molar content (C) based on the total amount of metal excluding lithium. Mn1 ) may be 55 mol% or more. In addition, the average particle size (D50_1) of the secondary particles may be in the range of 7 ㎛ to 15 ㎛, and specifically, may be in the range of 8 ㎛ to 14 ㎛.
[0137] The above high-nickel single-particle second cathode active material has a nickel molar content (C) based on the total amount of metal excluding lithium. Ni1 ) may be 80 mol% or more, and specifically, may be 85 mol% or more. In addition, the average particle size (D50_2) of the high-nickel single-particle second positive electrode active material may be in the range of 3 μm to 6 μm, and specifically, may be in the range of 3 μm to 5 μm.
[0138] The characteristics of the lithium manganese-rich first cathode active material and the high-nickel single-particle second cathode active material have been described in detail above, so they are omitted here.
[0139] In addition, the lithium manganese-rich first cathode active material and the high-nickel single-particle second cathode active material can be manufactured using a first cathode active material precursor and a second cathode active material precursor as raw materials, respectively, and there are no particular limitations on the manufacturing method and raw materials.
[0140] The above lithium manganese-rich first cathode active material can be formed under temperature conditions of 40°C to 50°C and voltage conditions of 4.6 V to 4.8 V.
[0141] Specifically, a lithium manganese-rich first cathode active material, which is a manganese-rich cathode active material, can be subjected to high-voltage formation processing in the following manner.
[0142] In order to form the initial lithium manganese-rich first cathode active material, the initial charge and discharge process can be performed in a separate formation device. The method of manufacturing a general electrode plate and then disassembling it to separate only the cathode active material is complicated and time-consuming, so a flow battery method can be adopted to quickly and easily form the initial formation of the manganese-rich lithium manganese-rich first cathode active material. The formation using the flow battery method prepares a first cathode active material slurry having a certain level of viscosity by mixing the lithium manganese-rich first cathode active material powder, a conductive agent, and an electrolyte. In addition, a cell having a cathode, an anode, and a separator separating them is manufactured. Here, the anode is an anode plate in which a graphite electrode is coated as a thick film on a copper current collector, and the separator is a polypropylene separator. The positive electrode has an Al current collector and a first positive electrode active material slurry inlet and outlet on the Al current collector, and a high voltage charge was performed by continuously circulating the positive electrode active material slurry to the catholyte portion where the positive electrode Al current collector is located by a motor. After the charge was completed, the direction of the applied current was changed again and a discharge was performed. In order to initially maximize the amount of oxygen generated, the formation was performed at a temperature of 40 to 50°C, and at this time, the charge voltage was 4.6 to 4.8 V under 0.1C current conditions, specifically, up to 4.65 V. Afterwards, a constant voltage was applied to ensure sufficient charging until the current dropped to 1 / 20C conditions. Thereafter, the discharge was performed by reversing the current direction, and the temperature of 40 to 50°C and 0.1C conditions were maintained in the same manner.The electrolyte used in the initial formation was 1M LiPF6 lithium salt and EC:EMC=3:7 (vol%) with 3 vol% FEC added. The conductive material was carbon black, and the 1C current standard was 200 mAh / g.
[0143] By performing the above formation in the above voltage range, Li2MnO3, which is a composition inside the positive electrode active material, is activated, which has the advantage of allowing oxygen (anion) to sufficiently participate in the reaction, and further, oxygen generated as a side reaction can be sufficiently removed at a high temperature of 45°C at an early stage, which has the advantage of reducing side reactions during the charging and discharging process of a lithium secondary battery and improving battery performance.
[0144]
[0145] After the formation is completed, the positive electrode active material slurry is recovered again, the electrolyte is separated, and then dried. The formed lithium manganese-rich positive electrode active material, which is a manganese-rich positive electrode active material, is mixed with a high-nickel single-particle second positive electrode active material, which is a high-nickel positive electrode active material. In order to uniformly mix the lithium manganese-rich first positive electrode active material and the high-nickel single-particle second positive electrode active material, a method such as mechanical stirring or mixing using an inert gas can be used. In the present invention, there is no particular limitation on the mixing method of the lithium manganese-rich first positive electrode active material and the high-nickel single-particle second positive electrode active material.
[0146] In this way, the lithium manganese-rich first cathode active material, which is manganese-rich, can sufficiently release oxygen (O2) by forming a high voltage, and can significantly reduce gas generation and voltage decay due to continuous anion redox during charge and discharge cycles, which is advantageous for expressing high capacity.
[0147] Meanwhile, in the step of manufacturing a positive electrode active material by mixing the first positive electrode active material and the second positive electrode active material, the manufactured positive electrode active material can satisfy the following relationship 1.
[0148] [Relationship 1]
[0149] 0.77 ≤ m / B*10^4 ≤ 0.95
[0150] Here, m is the tap density (g / cm) of the positive electrode active material for lithium secondary batteries. 3 ), and B is the specific surface area (m) of the positive electrode active material for lithium secondary batteries. 2 / g) is.
[0151] The value of the above relational expression 1 may be 0.77 to 0.95, and specifically, 0.82 to 0.95. When the value of the above relational expression 1 satisfies the above range, there is an advantage in that a positive electrode active material capable of improving the output characteristics and cycle life characteristics of an excellent battery can be manufactured.
[0152]
[0153] <Cathode for lithium secondary batteries and lithium secondary batteries>
[0154] Another embodiment of the present invention relates to a positive electrode for a lithium secondary battery, comprising: a current collector; and a positive electrode active material layer positioned on at least one surface of the current collector and including the positive electrode active material for a lithium secondary battery as described above.
[0155] The above-mentioned current collector may be selected from the group consisting of, for example, aluminum, copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, aluminum foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0156] The above positive electrode active material layer may further include a binder and a conductive material.
[0157] The above binder can serve to attach the positive electrode active material particles for the lithium secondary battery well to each other and also to attach the positive electrode active material for the lithium secondary battery well to the current collector.
[0158] The above-mentioned conductive material can be any material that does not cause chemical changes in the battery being constructed and is electronically conductive.
[0159] The above lithium secondary battery may include a negative electrode and a non-aqueous electrolyte.
[0160] The above negative electrode includes a current collector and a negative electrode active material layer formed on the current collector, and the negative electrode active material layer may include a negative electrode active material.
[0161] The above negative active material may include a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.
[0162] The material capable of reversibly intercalating / deintercalating the lithium ions may be, for example, a carbon material, and any carbon-based negative electrode active material generally used in the lithium secondary battery may be used. For example, crystalline carbon, amorphous carbon, or a combination thereof may be used.
[0163] As the above lithium metal alloy, an alloy of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn can be used.
[0164] Materials capable of doping and dedoping the lithium include, for example, Si, SiO. x(0 < x < 2), Si-Y alloy (wherein Y is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO2, Sn-Y (wherein Y is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn), etc.
[0165] Examples of the above transition metal oxide include vanadium oxide, lithium vanadium oxide, etc. The negative electrode active material layer also includes a binder and may optionally further include a conductive material.
[0166] The above binder can play a role in attaching the negative electrode active material particles well to each other and also attaching the negative electrode active material well to the current collector.
[0167] The above conductive material is used to provide conductivity to the electrode, and any electronically conductive material that does not cause chemical changes can be used in the battery being constructed.
[0168] The above-mentioned current collector may be selected from the group consisting of, for example, aluminum foil, nickel foil, stainless steel foil, titanium foil, nickel foam, aluminum foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0169] The above negative and positive electrodes can be manufactured by mixing an active material, a conductive material, and a binder in a solvent to manufacture an active material composition, and applying the composition to a current collector. The present invention does not limit the method for manufacturing the electrodes.
[0170] The above solvent may include, but is not limited to, N-methylpyrrolidone.
[0171] The above electrolyte may be a non-aqueous electrolyte or a solid electrolyte, and one in which a lithium salt is dissolved is used.
[0172] The non-aqueous electrolyte may include an organic solvent, and the non-aqueous organic solvent may serve as a medium through which ions involved in the electrochemical reaction of the battery can move.
[0173] Examples of the organic solvent include cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and vinylene carbonate; chain carbonates such as dimethyl carbonate, methyl ethyl carbonate, and diethyl carbonate; esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ethers such as 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, 1,2-dioxane, and 2-methyltetrahydrofuran; nitriles such as acetonitrile; and amides such as dimethylformamide. These may be used singly or in combination. In particular, a mixed solvent of a cyclic carbonate and a chain carbonate can be preferably used.
[0174] Additionally, as an electrolyte, a gel polymer electrolyte impregnated with an electrolyte solution in a polymer electrolyte such as polyethylene oxide or polyacrylonitrile, or an inorganic solid electrolyte such as LiI or Li3N may be used.
[0175] The above lithium salt is a substance that is dissolved in an organic solvent and acts as a source of lithium ions within the battery, enabling the basic operation of a lithium secondary battery and promoting the movement of lithium ions between the positive and negative electrodes.
[0176] The lithium salt may be any one commonly used in the art without limitation as long as it does not impede the purpose of the present invention. For example, the lithium salt may be one selected from the group consisting of LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiSbF6, LiAlO4, LiAlCl4, LiCl, and LiI.
[0177] Depending on the type of the lithium secondary battery, a separator may be present between the positive and negative electrodes. Such separators may include polyethylene, polypropylene, polyvinylidene fluoride, or multilayer films of two or more layers thereof. Of course, mixed multilayer films such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may also be used.
[0178] Lithium secondary batteries can be classified into lithium ion batteries, lithium ion polymer batteries, and lithium polymer batteries depending on the type of separator and electrolyte used, and can be classified into cylindrical, square, coin, and pouch types depending on the shape, and can be divided into bulk type and thin film type depending on the size.
[0179] The structure and manufacturing method of the battery are not limited in the present invention.
[0180] According to one embodiment of the present invention, a lithium secondary battery may have an average voltage decay of 40 mV to 65 mV after 50 cycles of charging and discharging compared to the initial charging and discharging, and specifically, may have an average voltage decay of 45 mV to 65 mV.
[0181] The above lithium secondary battery can satisfy the following relationship 2.
[0182] [Relationship 2]
[0183] 50 ≤△V / (m / B*10^4) ≤ 80
[0184] Here, △V is the voltage decay after 50 cycles of charging and discharging compared to the initial charging and discharging of a lithium secondary battery, and m is the tap density (g / cm) of the positive electrode active material for a lithium secondary battery. 3 ), and B is the specific surface area (m) of the positive electrode active material for lithium secondary batteries. 2 / g) is.
[0185]
[0186] Meanwhile, the above lithium secondary battery can satisfy the following relationship 3.
[0187] [Relationship 3]
[0188] 3.0 ≤G / (m / B*10^4) ≤ 5.0
[0189] Here, G is the gas generation amount of the lithium secondary battery, and m is the tap density (g / cm) of the positive electrode active material for the lithium secondary battery. 3 ), and B is the specific surface area (m) of the positive electrode active material for lithium secondary batteries. 2 / g) is.
[0190] In the present invention, the measurement of the gas generation amount was performed as follows. After initially charging a coin cell using the positive electrode active material manufactured according to the above examples and comparative examples, the coin cell was disassembled and only the electrode was removed. The electrode was placed in a pouch with an electrolyte and sealed. When stored at 60°C for 4 weeks, the pouch expanded due to gas generation. The expanded volume was measured using the Archimedes method.
[0191]
[0192] In addition, the lithium secondary battery can satisfy the following relationship 4.
[0193] [Relationship 4]
[0194] 250.0 ≤ (G / Em) / (m / B*10^4) ≤ 400.0
[0195] Here, G is the gas generation amount of the lithium secondary battery, Em is the loading amount of the cathode active material in the cathode of the lithium secondary battery, and m is the tap density (g / cm) of the cathode active material for the lithium secondary battery. 3 ), and B is the specific surface area (m) of the positive electrode active material for lithium secondary batteries. 2 / g) is.
[0196] The above Em is calculated by considering the positive electrode loading amount and the content of positive electrode active material in the positive electrode.
[0197]
[0198] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples, and the present invention is not limited thereby, and the present invention is defined only by the scope of the claims set forth below.
[0199]
[0200] (Manufacturing Example 1: Manufacturing of lithium and manganese-rich first cathode active material)
[0201] Nickel cobalt manganese coprecipitation hydroxide was prepared using a 20 L coprecipitation reactor.
[0202] The solution for preparing the precursor was prepared by dissolving NiSO4·6H2O, CoSO4·7H2O, and MnSO4·H2O in DI water to prepare a 2.5 M metal salt aqueous solution. Then, N2 was purged to prevent oxidation of metal ions during the coprecipitation reaction, and the reactor temperature was maintained at 50℃. The metal salt aqueous solution and NH4(OH) as a coprecipitation chelating agent were added to the coprecipitation reactor, and NaOH was used to adjust the pH. The precursor was grown to an average particle size (D50) of 10㎛, and the prepared precursor was filtered, washed with DI water, and then vacuum dried in an oven at 100℃ for 24 h.
[0203] The first cathode active material precursor manufactured above and the lithium raw material LiOH·H2O were weighed according to the design value of the first cathode active material and mixed using a mixer. The mixture was loaded into a refractory (Saggar) and placed in a box furnace. The box furnace was heated to 850°C for 5 hours while injecting 180 LPH of air, and then fired at a temperature profile of maintaining the temperature at 850°C for 10 hours and then cooling to room temperature for 5 hours. The material obtained by firing was induced to be crushed and then classified through a 325 mesh to manufacture a lithium and manganese-rich first cathode active material.
[0204] The composition and average particle size (D50) of the manufactured lithium and manganese-rich first cathode active material are shown in Table 1.
[0205] The lithium and manganese-rich first cathode active material powder, a conductive agent, and an electrolyte are mixed to prepare a first cathode active material slurry having a certain level of viscosity. In addition, a cell having a cathode, an anode, and a separator separating them is manufactured. Here, the anode is a cathode plate in which a graphite electrode is thickly coated on a lithium metal or Cu current collector, and the separator is a polypropylene separator. The cathode is provided with an Al current collector and a cathode active material slurry inlet and outlet on the Al current collector, and a high-voltage charge is performed by continuously circulating the first cathode active material slurry to the catholyte portion where the cathode Al current collector is located by a motor. After charging is completed, the direction of the applied current is changed again to perform a discharge. In order to initially maximize the amount of oxygen generation, the formation was performed at a temperature of 45℃. At this time, the charging voltage was up to 4.65 V under 0.1C current conditions, and a constant voltage was applied to ensure sufficient charging until the current dropped to 1 / 20C conditions. Afterwards, the current direction was reversed and discharge was performed, and the temperature and 0.1C conditions were maintained in the same way. The electrolyte used for the initial formation was 1M LiPF6 lithium salt with EC:EMC=3:7 (vol %) and 3% FEC added, and the conductive material was carbon black, and the 1C current standard was 200mAh / g.
[0206] Table 1 below shows the composition and size of the lithium and manganese-rich first cathode active material, as well as the initial formation discharge capacity and tap density.
[0207]
[0208] Cathode active material compositionAverage particle size (D50, ㎛)Initial discharge capacity (4.65 V~2 V, mAh / g, 0.1 C, 45 ℃)Tap density (g / cm 3 )Li 1.13 Ni 0.3 Mn0.57 O282771.71Li 1.13 Ni 0.3 Mn 0.57 O2102751.83Li 1.13 Ni 0.3 Mn 0.57 O2142712.03Li 1.13 Ni 0.3 Mn 0.57 O252791.50Li 1.13 Ni 0.3 Mn 0.57 O232811.29Li 1.1 Ni 0.28 Co 0.1 Mn 0.52 O2102801.92Li 1.1 Ni 0.28 Co 0.1 Mn 0.52 O232851.32
[0209] Referring to Table 1 above, it can be seen that when Co is present, the initial discharge capacity is higher, and as the average particle size increases, the discharge capacity decreases, but the tap density increases.
[0210] After performing the initial discharge as described above, the first positive electrode active material slurry was recovered again, and the powder was dried while only the electrolyte was separated, to finally manufacture the first positive electrode active material with a large particle size.
[0211]
[0212] (Manufacturing Example 2: Manufacturing of high-nickel single-particle second cathode active material)
[0213] A high-nickel single-particle second cathode active material precursor was manufactured using the same method as the above lithium and manganese-rich first cathode active material precursor manufacturing method.
[0214] The above-mentioned manufactured second cathode active material precursor and lithium raw material LiOH·H2O and Al(OH)3 precursor were weighed according to the design value of the high-nickel single-particle second cathode active material, and then mixed using a mixer to prepare a mixture. The mixture was loaded into a refractory (Saggar) and placed in a box furnace. 200 LPH of oxygen (O2) was added to the box furnace, and the temperature was raised to 750°C to 850°C for 5 hours, maintained at the temperature for 10 hours, and then cooled to room temperature for 5 hours, and then fired with a temperature profile. The material obtained by firing was induced to be crushed and then classified through 325 mesh, thereby producing a high-nickel single-particle second cathode active material with a small particle size.
[0215] The composition and average particle size (D50) of the manufactured second positive electrode active material are shown in Table 2.
[0216]
[0217] (Manufacturing of positive electrode active materials for lithium secondary batteries)
[0218] A high-nickel single-particle second cathode active material having a small particle size manufactured according to Manufacturing Example 2 and a lithium and manganese-rich first cathode active material having a large particle size manufactured according to Manufacturing Example 1 were uniformly mixed according to design values to manufacture a cathode active material for a lithium secondary battery.
[0219] Table 2 below shows the composition and mixing ratio of the formed large-particle lithium and manganese-rich first cathode active material and the small-particle high-nickel single-particle second cathode active material included in the cathode active material for lithium secondary batteries manufactured according to the examples and comparative examples.
[0220] Meanwhile, in Comparative Example 1, a lithium and manganese-rich cathode active material with a small particle size was used as the second cathode active material with a small particle size.
[0221]
[0222] Classification Large particle size First positive electrode active material Small particle size Second positive electrode active material Mixed weight ratio (large particle size: small particle size) Chemical formula Average particle size (D50, ㎛) Chemical formula Average particle size (D50, ㎛) Example 1 Li 1.13 Ni 0.3 Mn 0.57 O210LiNi 0.94 Co 0.04 Mn 0.01 Al 0.01 O2380:20 Example 2Li 1.13 Ni 0.3 Mn 0.57 O210LiNi 0.91 Co 0.06 Mn 0.02 Al 0.01 O2380:20 Example 3Li 1.13 Ni 0.3 Mn 0.57 O210LiNi 0.86 Co 0.09 Mn 0.03 Al 0.02 O2380:20 Example 4Li 1.13 Ni 0.3 Mn 0.57 O210LiNi 0.83 Co 0.12 Mn 0.03 Al 0.02 O2380:20 Example 5Li 1.13 Ni 0.3 Mn 0.57 O214LiNi 0.94 Co 0.04 Mn 0.01 Al 0.01 O2580:20 Example 6Li 1.13 Ni 0.3 Mn 0.57 O210LiNi 0.86 Co 0.09 Mn 0.03 Al 0.02 O2370:30 Example 7Li 1.1 Ni 0.28 Co 0.1 Mn 0.52 O210LiNi 0.86 Co 0.09 Mn 0.03 Al 0.02 O2380:20 Example 8Li 1.13 Ni 0.3 Mn0.57 O28LiNi 0.86 Co 0.09 Mn 0.03 Al 0.02 O2380:20 Example 9Li 1.13 Ni 0.3 Mn 0.57 O210LiNi 0.94 Co 0.04 Mn 0.01 Al 0.01 O2360:40 Comparative Example 1Li 1.13 Ni 0.3 Mn 0.57 O210Li 1.13 Ni 0.3 Mn 0.57 O2380:20 Comparative Example 2Li 1.1 Ni 0.28 Co 0.1 Mn 0.52 O210Li 1.1 Ni 0.28 Co 0.1 Mn 0.52 O2380:20 Comparative Example 3Li 1.13 Ni 0.3 Mn 0.57 O26LiNi 0.94 Co 0.04 Mn 0.01 Al 0.01 O2380:20 Comparative Example 4Li 1.13 Ni 0.3 Mn 0.57 O210LiNi 0.94 Co 0.04 Mn 0.01 Al 0.01 O2280:20 Comparative Example 5Li 1.13 Ni 0.3 Mn 0.57 O210LiNi 0.94 Co 0.04 Mn 0.01 Al 0.01 O2350:50 Comparative Example 6Li 1.13 Ni 0.3 Mn 0.57 O210LiNi 0.94 Co 0.04 Mn 0.01 Al 0.01 O2390:10 Comparative Example 7Li 1.14 Ni 0.43 Mn 0.43O210LiNi 0.94 Co 0.04 Mn 0.01 Al 0.01 O2380:20 Comparison Example 8 Formation Li 1.13 Ni 0.3 Mn 0.57 O210LiNi 0.94 Co 0.04 Mn 0.01 Al 0.01 O2380:20
[0223] (Characteristic Analysis 1 - SEM Analysis)
[0224] An SEM image of a cross-section of an electrode manufactured using a positive electrode active material for a lithium secondary battery manufactured according to Example 1 was analyzed and is shown in Fig. 1.
[0225] Referring to Figure 1, it can be confirmed that the first cathode active material with a large particle size and the second cathode active material with a small particle size are uniformly distributed. At this time, the large spherical particles are a composition rich in lithium and manganese, and the small particles randomly located around them are small-diameter high-nickel single particles.
[0226]
[0227] (Characterization 2 - EDS Analysis)
[0228] FIG. 2 shows the results of measuring the main composition of the positive electrode active material according to Example 1 using an element mapping method using EDS (Energy-dispersive X-ray spectroscopy) for the square area of FIG. 1.
[0229] Referring to Figure 2, Ni was found to be more distributed in particles of small particle size, and Mn was found to be relatively more distributed in particles of large particle size.
[0230]
[0231] Table 3 below shows the tap density and BET analysis results of the positive electrode active materials manufactured according to the examples and comparative examples, and the calculated values of the correlation between the tap density and BET.
[0232] Tap density (m) (g / cm) 3 )BET (B)(m 2 / g)Relationship 1m / B*10^4(g) 2 / cm 5 ) Example 12.032.450.83 Example 22.012.560.79 Example 32.022.480.81 Example 42.022.560.79 Example 52.152.510.86 Example 62.032.210.92 Example 72.032.480.82 Example 81.912.460.78 Example 91.922.130.90 Comparative Example 11.823.580.51 Comparative Example 21.933.640.53 Comparative Example 31.772.550.69 Comparative Example 41.922.540.76 Comparative Example 51.822.470.74 Comparative Example 61.883.040.62Comparative example 72.072.540.81Comparative example 81.972.440.81
[0233] (Coin-shaped half-cell manufacturing)
[0234] Using the positive electrode active material manufactured according to the above examples and comparative examples, a CR2032 coin cell was manufactured and then electrochemical evaluation was conducted.
[0235] The slurry for manufacturing the electrode plate was mixed with the above materials in a weight ratio (wt%) of positive electrode active material: conductive material (Denka Black): binder (PVDF, KF1100) = 92.5:3.5:4, and the viscosity of the slurry was adjusted by adding NMP (N-Methyl-2-pyrrolidone) so that the solid concentration was approximately 30 wt%. The manufactured slurry was coated on a 15 μm thick Al foil using a doctor blade, dried, and then rolled. At this time, the electrode loading was approximately 14 mg / cm 2 The electrolyte used was 1M LiPF6 in EC:EMC=3:7 (vol%) with 3% FEC added. After manufacturing a coin cell using a PP separator and a lithium anode (200um, Honzo metal), it was aged at room temperature for 10 hours and then charge and discharge tests were performed.
[0236] Charge and discharge tests were conducted under 4.4 V charge and 2.5 V discharge conditions, and the electrochemical evaluation results are shown in Table 4 below.
[0237] In Table 4 below, the loading amount of the positive electrode active material, Em, is 14 mg / cm of the positive electrode. 2 And in the slurry for manufacturing the electrode plate, considering the mixing ratio of the positive electrode active material of 92.5 wt% in the mixture of the positive electrode active material, conductive material (denka black) and binder (PVDF, KF1100), 12.95 mg / cm 2 was calculated as
[0238]
[0239]
[0240]
[0241] Referring to Table 4 above, it can be confirmed that the battery using the positive electrode active material manufactured according to Examples 1 to 9 of the present invention has a capacity of 95% or more for one cycle in 50 cycles.
[0242] The average voltage decrease after cycle charging and discharging was measured, and the voltage drop after 50 cycles of charging and discharging was converted into a numerical value compared to the initial measurement results.
[0243] In the present invention, when a coin half-cell is subjected to one charge / discharge cycle in the 4.4 V - 2.5 V range, the discharge curve is integrated, and the voltage at the 50% point of energy is defined as the initial voltage. The charge / discharge cycle is continuously performed up to 50 times, and the discharge curve at the final 50th cycle is identically integrated, and the voltage at the point where the energy becomes 50% is measured, and this is defined as the final voltage. In addition, the voltage drop is defined by measuring the final voltage and the initial voltage.
[0244] Referring to Table 4 above, in the case of coin cells using the positive electrode active material manufactured according to Examples 1 to 9 of the present invention, the voltage drop after 50 cycles of charging and discharging was 70 mV or less, specifically 40 mV to 65 mV, more specifically 45 mV to 65 mV, whereas in the case of coin cells using the positive electrode active material manufactured according to Comparative Examples 1 to 8 of the present invention, the voltage drop after 50 cycles of charging and discharging was 70 mV or more, indicating a relatively large voltage drop.
[0245] Meanwhile, in the case of coin cells using the positive electrode active material manufactured according to Examples 1 to 9, the value of the relational expression 2 △V / (M / B*10^4) was 50 or more and 80 or less at the same time, whereas in the case of Comparative Examples 1 to 8, the value of the relational expression 2 was found to be greater than 80.
[0246] In addition, the amount of gas generated from the battery using the positive electrode active material manufactured according to the above examples and comparative examples was measured and shown in Table 4 above.
[0247] Referring to Table 4 above, when the positive electrode active materials manufactured according to Examples 1 to 9 were applied, the G / (M / B*10^4) value of equation 3 was 3.0 to 5.0, specifically 3.5 to 4.9, whereas in the case of Comparative Examples 1 to 8, the value of equation 3 was found to be greater than 5.0.
[0248] In addition, the (G / Em) / (m / B*10^4) value of equation 4, which represents the amount of gas generated according to the loading amount of the positive electrode active material manufactured according to the examples and comparative examples, was found to be in the range of 250.0 to 400.0, specifically 270.0 to 380, in the case of examples 1 to 9, and the value of equation 4 was found to be greater than 400 in the case of comparative examples 1 to 8.
[0249] Fig. 3 shows a cross-sectional SEM image of a positive electrode plate after performing 100 charges and discharges of a coin cell using a positive electrode active material according to Example 1, and Fig. 4 shows a cross-sectional SEM image of a positive electrode plate after performing 100 charges and discharges of a coin cell using a positive electrode active material according to Comparative Example 1. When high-nickel single particles were applied as the small-particle second positive electrode active material of Example 1, it was confirmed that the degree of crack occurrence in the large-particle first positive electrode active material was greatly reduced after performing 100 charges and discharges compared to when lithium and manganese-rich secondary particles were applied as the small-particle second positive electrode active material of Comparative Example 1.
[0250] Meanwhile, referring to FIG. 3, when high-nickel single particles were applied as the small-diameter second positive electrode active material of Example 1, it can be confirmed that there was almost no occurrence of cracks in the positive electrode active material after 100 charging and discharging cycles.
[0251] On the other hand, referring to Fig. 4, when lithium and manganese-rich secondary particles were applied as the small-particle second cathode active material of Comparative Example 1, it can be confirmed that cracks occurred not only in the large-particle first cathode active material but also in the small-particle second cathode active material after 100 cycles of charging and discharging. These cracks cause the specific surface area of the cathode active material to continuously increase during the charging and discharging process, thereby promoting the reaction with the electrolyte, thereby causing problems of accelerated gas generation and deterioration of the battery life.
[0252]
[0253] The present invention is not limited to the above-described embodiments, but can be manufactured in a variety of different forms. Those skilled in the art will appreciate that the present invention can be implemented in other specific forms without altering the technical spirit or essential characteristics of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.
Claims
1. A first positive electrode active material comprising a lithium manganese-rich group represented by the following chemical formula 1; and Contains a second positive electrode active material of high nickel single particle type represented by the following chemical formula 2; The average particle size (D50_1) of the lithium manganese-rich first cathode active material is larger than the average particle size (D50_2) of the high-nickel single-particle second cathode active material. Cathode active material for lithium secondary batteries. [Chemical Formula 1] Li 1+x1 (Ni (1-a1-b1) Co a1 Mr b1 )O2 (Here, -0.5≤x1≤0.5, 0≤a1≤0.5, 0.5≤b1≤1.) [Chemical formula 2] <h2 style=";text-align:left;direction:ltr">Li<h2 style=";text-align:left;direction:ltr"> 1+x2 <h2 style=";text-align:left;direction:ltr"> (Ni(1-a2-b2-c2)Co<h2 style=";text-align:left;direction:ltr"> a2 <h2 style=";text-align:left;direction:ltr"> Mn<h2 style=";text-align:left;direction:ltr"> b2 <h2 style=";text-align:left;direction:ltr"> M<h2 style=";text-align:left;direction:ltr"> c2 <h2 style=";text-align:left;direction:ltr"> O2) (Here, -0.5≤x2≤0.5, 0≤a2≤0.2, 0≤b2≤0.1, 0≤c2≤0.03, M is one or more elements selected from the group consisting of Fe, Cr, Ti, Zn, V, Al, Mg, and Zr.) 2. In paragraph 1, The ratio D50_1 / D50_2 of the average particle size (D50_1) of the lithium manganese-rich first cathode active material to the average particle size (D50_2) of the high-nickel single-particle second cathode active material is 2.5 to 4.
5. Cathode active material for lithium secondary batteries.
3. In paragraph 1, The average particle size (D50_1) of the lithium manganese-rich first cathode active material is 7 ㎛ to 15 ㎛. Cathode active material for lithium secondary batteries.
4. In paragraph 1, The average particle size (D50_2) of the above-mentioned high-nickel single-particle second cathode active material is 3 ㎛ to 6 ㎛. Cathode active material for lithium secondary batteries.
5. In paragraph 1, The above lithium manganese-rich first cathode active material is a secondary particle composed of a plurality of primary particles. Cathode active material for lithium secondary batteries.
6. In paragraph 1, The weight ratio (w1) of the lithium manganese-rich first cathode active material to the weight (w2) of the nickel-based single-particle second cathode active material is w1 / w2, which is 85:15 to 55:
45. Cathode active material for lithium secondary batteries.
7. In paragraph 1, The manganese mole content (C) based on the total amount of metal excluding lithium in the above high-nickel single particle second cathode active material Mn2 ) The manganese mole content (C) based on the total amount of metal excluding lithium in the first cathode active material of the lithium manganese-rich system Mn1 )Rain (C Mn1 / C Mn2 ) is 15.0 to 70.0, Cathode active material for lithium secondary batteries.
8. In paragraph 1, The manganese mole content (C) based on the total amount of metal excluding lithium in the first positive electrode active material Mn1 ) and manganese mole content (C) based on the total amount of metal excluding lithium in the second cathode active material Mn2 ) difference (C Mn1 -C Mn2 ) is 50 mol% to 70 mol%, Cathode active material for lithium secondary batteries.
9. In paragraph 1, Nickel molar content (C) based on the total amount of metal excluding lithium in the first positive electrode active material Ni1 ) Nickel molar content (C) based on the total amount of metal excluding lithium in the second cathode active material Ni2 ) Rain (C) Ni2 / C Ni1 ) is between 2.0 and 3.0, Cathode active material for lithium secondary batteries.
10. In paragraph 1, Nickel molar content (C) based on the total amount of metal excluding lithium in the above second cathode active material Ni2 ) and nickel molar content (C) based on the total amount of metal excluding lithium in the first cathode active material Ni1 ) difference (C Ni2 -C Ni1 ) is 45 mol% to 65 mol%, Cathode active material for lithium secondary batteries.
11. In paragraph 1, The above lithium manganese-rich first cathode active material is formed at a voltage of 4.6 V to 4.8 V. Cathode active material for lithium secondary batteries.
12. In paragraph 1, The tap density of the above positive electrode active material for lithium secondary batteries is 1.90 g / cm 3 2.20g / cm2 3 It is, Cathode active material for lithium secondary batteries.
13. In paragraph 1, The specific surface area of the positive electrode active material for the above lithium secondary battery is 2.0 cm 2 / g to 3.0cm 2 / g is, Cathode active material for lithium secondary batteries.
14. In paragraph 1, The above-mentioned positive electrode active material for a lithium secondary battery satisfies the following relationship 1: Cathode active material for lithium secondary batteries. [Relationship 1] 0.77 ≤ m / B*10^4 ≤ 0.95 (Here, m is the tap density (g / cm) of the positive electrode active material for lithium secondary batteries. 3 ), and B is the specific surface area (m) of the cathode active material for lithium secondary batteries. 2 / g) is.) 15. In paragraph 1, In the above second positive electrode active material, the nickel molar content based on the total amount of metal excluding lithium is 80 mol% or more. Cathode active material for lithium secondary batteries.
16. In paragraph 1, In the above first positive electrode active material, the manganese molar content based on the total amount of metal excluding lithium is 50 mol% or more. Cathode active material for lithium secondary batteries.
17. A step of preparing a lithium manganese-rich first positive electrode active material represented by the following chemical formula 1; A step for preparing a high-nickel single-particle second positive electrode active material represented by the following chemical formula 2; and A step of manufacturing a positive electrode active material by mixing the first positive electrode active material and the second positive electrode active material; comprising; The average particle size (D50_1) of the lithium manganese-rich first cathode active material is larger than the average particle size (D50_2) of the high-nickel single-particle second cathode active material. A method for producing a cathode active material for a lithium secondary battery. [Chemical Formula 1] Li 1+x1 (Ni (1-a1-b1) Co a1 Mr b1 )O2 (Here, -0.5≤x1≤0.5, 0≤a1≤0.2, 0.5≤b1<1.) [Chemical formula 2] <h2 style=";text-align:left;direction:ltr">Li<h2 style=";text-align:left;direction:ltr"> 1+x2 <h2 style=";text-align:left;direction:ltr"> (Ni(1-a2-b2-c2)Co<h2 style=";text-align:left;direction:ltr"> a2 <h2 style=";text-align:left;direction:ltr"> Mn<h2 style=";text-align:left;direction:ltr"> b2 <h2 style=";text-align:left;direction:ltr"> M<h2 style=";text-align:left;direction:ltr"> c2 <h2 style=";text-align:left;direction:ltr"> O2) (Here, -0.5≤x2≤0.5, 0≤a2<0.2, 0≤b2≤0.1, 0≤c2<0.03, M is one or more elements selected from the group consisting of Fe, Cr, Ti, Zn, V, Al, Mg, and Zr.) 18. In paragraph 17, The step of preparing the above lithium manganese-rich first cathode active material is: A step of forming the lithium manganese-rich first cathode active material at a voltage of 4.6 V to 4.8 V is included. A method for producing a cathode active material for a lithium secondary battery.
19. In Article 17, The step of forming the first positive electrode active material of the lithium manganese-rich system at a voltage of 4.6 V to 4.8 V is as follows. It is performed at a temperature of 40℃ to 50℃. A method for producing a cathode active material for a lithium secondary battery.
20. In paragraph 17, The step of forming the lithium manganese-rich first cathode active material under voltage conditions of 4.6 V to 4.8 V is as follows. Charge to 4.6 V to 4.8 V under 0.1 C current conditions, A step of applying a constant voltage and maintaining the charge until the current drops to a 1 / 20C condition, A method for producing a cathode active material for a lithium secondary battery.
21. In paragraph 17, The step of forming the lithium manganese-rich first cathode active material under voltage conditions of 4.6 V to 4.8 V is as follows. Including a step of discharging under 0.1C current conditions, A method for producing a cathode active material for a lithium secondary battery.
22. In paragraph 17, The step of preparing the above lithium manganese-rich first cathode active material is: A lithium manganese-rich first cathode active material having an average particle size (D50_1) of 7 ㎛ to 15 ㎛ is prepared. A method for producing a cathode active material for a lithium secondary battery.
23. In paragraph 17, The step of preparing the above-mentioned high-nickel single-particle second cathode active material is as follows. A high-nickel single-particle second cathode active material is prepared, having an average particle size (D50_2) of 3 ㎛ to 6 ㎛. A method for producing a cathode active material for a lithium secondary battery.
24. In paragraph 17, The step of manufacturing a positive electrode active material by mixing the first positive electrode active material and the second positive electrode active material is as follows: The weight (w1) of the lithium manganese-rich first cathode active material to the weight (w2) of the nickel-based single particle second cathode active material is mixed in a ratio w1 / w2 of 85:15 to 55:
45. A method for producing a cathode active material for a lithium secondary battery.
25. In paragraph 17, The step of manufacturing a positive electrode active material by mixing the first positive electrode active material and the second positive electrode active material is as follows: A method for manufacturing a positive electrode active material satisfying the following relational expression 1, A method for producing a cathode active material for a lithium secondary battery. [Relationship 1] 0.77 ≤ m / B*10^4 ≤ 0.95 (Here, m is the tap density (g / cm) of the positive electrode active material for lithium secondary batteries. 3 ), and B is the specific surface area (m) of the cathode active material for lithium secondary batteries. 2 / g) is.) 26. The whole house; and A cathode active material layer, which is located on at least one side of the entire body and includes a cathode active material for a lithium secondary battery according to any one of claims 1 to 16; Cathode for lithium secondary batteries.
27. Containing a positive electrode for a lithium secondary battery of Article 26, Lithium secondary battery.
28. In paragraph 27, The average voltage decay after 50 charging and discharging cycles is 40 mV to 65 mV. Lithium secondary battery.
29. In paragraph 27, It satisfies the following relation 2, Lithium secondary battery. [Relationship 2] 50 ≤△V / (m / B*10^4) ≤ 80 (Here, △V is the voltage decay after 50 cycles of charging and discharging compared to the initial charging and discharging of a lithium secondary battery, and m is the tap density (g / cm) of the cathode active material for a lithium secondary battery. 3 ), and B is the specific surface area (m) of the cathode active material for lithium secondary batteries. 2 / g) is.) 30. In paragraph 27, It satisfies the following relation 3, Lithium secondary battery. [Relationship 3] 3.0 ≤G / (m / B*10^4) ≤ 5.0 (Here, G is the gas generation amount of the lithium secondary battery, and m is the tap density of the cathode active material for the lithium secondary battery (g / cm 3 ), and B is the specific surface area (m) of the cathode active material for lithium secondary batteries. 2 / g) is.) 31. In paragraph 27, It satisfies the following relation 4, Lithium secondary battery. [Relationship 4] 250.0 ≤ (G / Em) / (m / B*10^4) ≤ 400.0 (Here, G is the gas generation amount of the lithium secondary battery, Em is the loading amount of the cathode active material in the cathode of the lithium secondary battery, and m is the tap density (g / cm) of the cathode active material for the lithium secondary battery. 3 ), and B is the specific surface area (m) of the cathode active material for lithium secondary batteries. 2 / g) is.)
Citation Information
Patent Citations
Cathode active material for secondary battery with improved durability and lithium secondary battery including same
KR1020140098433A
Positive electrode active material for secondary battery, method for preparing the same, and secondary battery comprising the same
KR1020170063387A
Encapsulation coposition of Oil-soluble vitamin support-based and prepatarion method thereof
KR1020210149255A
Method for avoiding output limit of battery for vehicle
KR1020240167266A
Apparatus and method for drying electrode sheet for battery
KR102388446B1
Cited By
Battery cell, battery device and electric device
CN121366871A
Positive electrode active material, positive electrode containing the same, and lithium secondary battery
JP2026528890A
Positive electrode active material and method for manufacturing a positive electrode active material
WO2026125216A1