Laser annealing method and method for manufacturing semiconductor device by using same

The laser annealing method using deuterium and ammonia in a pressurized atmosphere addresses the inefficiencies of existing heat treatment processes by rapidly passivating interface charges, enhancing the stability and reliability of semiconductor devices.

WO2024242334A1PCT designated stage expired Publication Date: 2024-11-28RNR LAB INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005398
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-04-22
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing heat treatment processes for manufacturing semiconductor devices, such as MOSFETs, are inefficient and prone to reactivation of interface charges, leading to performance and reliability issues due to long processing times and instability of the gate dielectric layer.

Method used

A laser annealing method using deuterium (D2), hydrogen (H2), and ammonia (NH3) in a pressurized gas atmosphere above 1 atmosphere, which rapidly heats the semiconductor device to 600°C to 2000°C for 0.01 μs to 10 seconds, effectively passivating interface charges between the semiconductor and dielectric layers.

Benefits of technology

This method significantly improves the performance, stability, and reliability of semiconductor devices by efficiently deactivating interface charges and enhancing the bonding between semiconductor and dielectric layers, suitable for high-integration semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005398_28112024_PF_FP_ABST
    Figure KR2024005398_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A laser annealing method and a method of manufacturing a semiconductor device by using same are disclosed. The disclosed laser annealing method is a laser annealing method for a semiconductor device unit including a transistor, and may comprise the steps of: providing a semiconductor device unit having a transistor, which includes a semiconductor and a dielectric that forms a bonding interface with the semiconductor; and, in order to passivate interface charges between at least the semiconductor and the dielectric, irradiating the semiconductor device unit with a laser under a pressure condition of being higher than 1 atmosphere in a gas atmosphere of at least one of deuterium (D2), hydrogen (H2), and ammonia (NH3) and laser annealing same.
Need to check novelty before this filing date? Find Prior Art

Description

Laser annealing method and method for manufacturing semiconductor devices using the same

[0001] The present invention relates to an annealing method for a workpiece and a method for manufacturing a device using the same, and more particularly, to a laser annealing method and a method for manufacturing a semiconductor device using the same.

[0002] The MOSFET (metal-oxide-semiconductor field effect transistor) is a device that controls the amount of current flowing between the source and drain by the voltage applied to the gate. Since its development in the 1960s, it has been used throughout industry and has played a groundbreaking role in technological advancement. MOSFETs are used as a core component in integrated circuits, and most semiconductor devices currently mass-produced are manufactured based on MOSFETs. Along with the advancement of semiconductor technology, the integration and performance of unit transistor devices such as MOSFETs have also continuously improved. In addition, development is being conducted on new (or modified) structures of FET devices that can overcome the problems and performance limitations caused by high integration (i.e., downscaling) of existing MOSFETs.

[0003] In the manufacturing of transistor devices such as MOSFETs, a heat treatment process is utilized to inactivate the interfacial charge present at the interface between the gate dielectric layer and the semiconductor channel, thereby reducing the effective interfacial charge density. This heat treatment process can improve the film quality of the gate dielectric layer, ultimately enhancing the performance and reliability of the transistor.

[0004] However, conventional heat treatment processes require relatively long processing times and present challenges in efficient process performance, as they involve heating the substrate under a forming gas atmosphere. Furthermore, even if dangling bonds at the interface between the gate dielectric layer and the semiconductor channel are deactivated by conventional heat treatment processes, defects can reoccur due to reactivation. These problems can occur not only at the interface but also within the gate dielectric layer.

[0005] Therefore, in the manufacturing of transistor devices such as MOSFETs, there is a growing need to develop technologies that can overcome the existing problems and limitations mentioned above, efficiently enhance transistor performance, and ensure stability. Furthermore, as transistor integration significantly increases and their shape, structure, and scale evolve, the development of technologies and processes to ensure performance and reliability is essential.

[0006] The technical problem to be achieved by the present invention is to provide a process technology (laser annealing method) that can efficiently passivate interface charges between a semiconductor and a dielectric in the manufacture of a semiconductor device including a transistor, while significantly improving the performance, stability, and reliability of the transistor.

[0007] In addition, the technical problem to be achieved by the present invention is to provide a method for manufacturing a semiconductor device by applying the above-described process technology (laser annealing method).

[0008] The problems to be solved by the present invention are not limited to the problems mentioned above, and other problems not mentioned can be understood by those skilled in the art from the description below.

[0009] According to one embodiment of the present invention, a laser annealing method for a semiconductor device including a transistor is provided, comprising the steps of: providing a semiconductor device including a transistor including a semiconductor and a dielectric forming a bonding interface with the semiconductor; and performing laser annealing by irradiating a laser to the semiconductor device under a pressure condition higher than 1 atmosphere in an atmosphere of at least one gas among deuterium (D2), hydrogen (H2), and ammonia (NH3) for passivating interface charges between at least the semiconductor and the dielectric.

[0010] The above pressure conditions may be conditions of about 100 atmospheres or less.

[0011] The above pressure conditions may be conditions exceeding about 1 atm and less than about 100 atm.

[0012] The above transistor can be formed on a substrate, and the laser annealing can be performed while the temperature of the substrate is controlled in a range from room temperature to about 550°C.

[0013] The laser annealing can be performed while the temperature of the substrate is controlled within a range of room temperature to approximately 550°C.

[0014] The above laser annealing can be performed in a deuterium (D2) gas atmosphere.

[0015] The above laser annealing can be performed so that the temperature of the surface of the semiconductor element portion is increased to about 600°C to 2000°C.

[0016] The above laser annealing can be performed for about 0.01 μs to 10 seconds.

[0017] The semiconductor may include a channel of the transistor, and the dielectric may include a gate dielectric layer of the transistor.

[0018] The step of preparing the semiconductor element may include a step of forming a wiring member electrically connected to the transistor, and the laser annealing may be performed before or after the step of forming the wiring member.

[0019] The laser may include any one of ultraviolet ray, visible ray, infrared ray, and microwave.

[0020] According to another embodiment of the present invention, a method for manufacturing a semiconductor device using the above-described laser annealing method is provided.

[0021] According to embodiments of the present invention, in the manufacture of a semiconductor device including a transistor, a process technology (laser annealing method) can be implemented that can efficiently passivate the interface charge between the semiconductor and the dielectric while significantly improving the performance, stability, and reliability of the transistor. According to one embodiment, by performing a high-speed annealing process using laser irradiation under a pressure condition higher than 1 atm in a gas atmosphere such as deuterium (D2) having a high binding energy for a semiconductor element (e.g., silicon), a passivation process for removing the interface charge can be efficiently performed, and the performance, stability, and reliability of the semiconductor device can be significantly improved. In addition, the process technology (laser annealing method) according to an embodiment of the present invention can be usefully utilized in the manufacture of a highly integrated semiconductor device.

[0022] By applying the laser annealing method according to embodiments of the present invention, it is possible to manufacture a semiconductor device having high integration and excellent performance, stability, and reliability.

[0023] However, the effects of the present invention are not limited to the above effects, and can be expanded in various ways without departing from the technical spirit and scope of the present invention.

[0024] FIGS. 1A to 1C are cross-sectional views illustrating a laser annealing method for a semiconductor device including a transistor according to one embodiment of the present invention.

[0025] FIGS. 2A and 2B are cross-sectional views illustrating a laser annealing method for a semiconductor device including a transistor according to another embodiment of the present invention.

[0026] FIGS. 3A to 3D are cross-sectional views illustrating a laser annealing method for a semiconductor device including a transistor according to another embodiment of the present invention.

[0027] FIG. 4 is a plan view exemplarily showing the form of a pattern that a plurality of nano dots constituting the heating layer described in FIGS. 3a and 3b can have.

[0028] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings.

[0029] The embodiments of the present invention described below are provided to more clearly explain the present invention to a person having ordinary skill in the art, and the scope of the present invention is not limited by the following embodiments, and the following embodiments can be modified in various other forms.

[0030] The terminology used herein is used to describe particular embodiments and is not intended to limit the present invention. The singular forms used herein may include the plural forms unless the context clearly dictates otherwise. In addition, the terms "comprise" and / or "comprising" used herein specify the presence of a stated feature, step, number, operation, element, element, and / or group thereof, but do not exclude the presence or addition of one or more other features, steps, numbers, operations, elements, elements, and / or groups thereof. In addition, the term "connected" used herein not only means that certain elements are directly connected, but also includes a concept that indirectly connects elements by interposing another element between them.

[0031] In addition, when it is said in this specification that a certain element is located "on" another element, this includes not only cases where a certain element is in contact with another element, but also cases where another element exists between the two elements. The term "and / or" as used in this specification includes any one of the listed items and any and all combinations of one or more of them. In addition, terms of degree such as "about", "substantially", etc. as used in this specification are used to mean a range of or close to the numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly using the disclosure that mentions exact or absolute numbers provided to help the understanding of this specification.

[0032] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. The sizes and thicknesses of areas or parts depicted in the attached drawings may be somewhat exaggerated for clarity and convenience of explanation. Like reference numbers designate like components throughout the detailed description.

[0033] FIGS. 1A to 1C are cross-sectional views illustrating a laser annealing method for a semiconductor device including a transistor according to one embodiment of the present invention.

[0034] Referring to FIG. 1A, a laser annealing method according to one embodiment of the present invention may include a step of preparing a semiconductor device having a transistor. The transistor may include a semiconductor and a dielectric forming a bonding interface with the semiconductor.

[0035] According to an example, the semiconductor may include or correspond to a channel portion (110) of the transistor, and the dielectric may include or correspond to a gate dielectric layer (120) of the transistor. According to a specific embodiment, the transistor may include a channel portion (110) made of a semiconductor material and a gate dielectric layer (120) bonded to the channel portion (110). The gate dielectric layer (120) may be disposed on the channel portion (110), and a gate electrode (130) may be disposed on the gate dielectric layer (120). A source (140A) electrically connected to or in contact with a first region (e.g., a first end) of the channel portion (110) may be provided, and a drain (140B) electrically connected to or in contact with a second region (e.g., a second end) of the channel portion (110) may be provided. The channel portion (110) may be referred to as a channel member or a channel region. The source (140A) may be referred to as a source member or a source region, and similarly, the drain (140B) may be referred to as a drain member or a drain region.

[0036] According to an example, the transistor may be formed on a predetermined substrate (100). A channel portion (110) and a source (140A) and a drain (140B) may be defined or formed within a surface portion of the substrate (100). The channel portion (110) may be defined between the source (140A) and the drain (140B). The source (140A) and the drain (140B) may be regions that are highly doped (ion-implanted) with conductive impurities.

[0037] The substrate (100) may be, as a non-limiting example, a group IV interlayer compound substrate such as a silicon (Si) substrate, a germanium (Ge) substrate, or a silicon (Si)-germanium (Ge) substrate, or a group III-V or group II-VI compound substrate, and may be a semiconductor substrate having a layered structure such as silicon-on-insulator (SOI) to suppress a body effect, or a semiconductor layer obtained through epitaxial growth. An insulating region such as a shallow trench isolation (STI) may be provided on the substrate (100) to define an active region, and a well region having a suitable conductivity type may be formed for implementing an n-type metal-oxide-semiconductor (NMOS) transistor or a p-type metal-oxide-semiconductor (PMOS) transistor.

[0038] The channel portion (110) may include, as a non-limiting example, a group IV intermetallic compound such as silicon (Si), germanium (Ge) or silicon (Si)-germanium (Ge), or a group III-V compound or a group II-VI compound.

[0039] The gate dielectric layer (120) may include, for example, silicon oxide (e.g., SiO2), silicon oxynitride (e.g., SiON), or silicon nitride (e.g., Si3N4), or may include a high-k material having a higher dielectric constant than silicon nitride. The gate dielectric layer (120) may also include a laminated structure composed of two or more different dielectric material layers. Any material that can be used as a gate dielectric (insulating) material in a general transistor device may be applied as the material of the gate dielectric layer (120). The gate dielectric layer (120) may be referred to as a gate insulating layer.

[0040] The gate electrode (130) may be formed of a predetermined conductive material, such as a conductive polysilicon doped with impurities, a metal, or a metal compound, and may be adjusted to have a suitable work function. Although not shown, a sidewall insulating layer may be further formed on both sides of the gate stack including the gate dielectric layer (120) and the gate electrode (130).

[0041] The semiconductor element portion may further include an insulating layer (150) formed on the substrate (100) to cover the gate electrode (130). The insulating layer (150) may be formed to cover the source (140A), the drain (140B) and the gate electrode (130). After depositing a predetermined insulating material layer, a planarization process may be performed on the upper surface thereof to form the insulating layer (150). The insulating layer (150) may include, as a non-limiting example, silicon oxide (e.g., SiO2), silicon oxynitride (e.g., SiON), or silicon nitride (e.g., Si3N4), or may include other insulating materials, and may be composed of one or more insulating materials. The insulating layer (150) may be referred to as an interlayer insulating film.

[0042] Referring to FIG. 1B, a laser annealing method according to an embodiment of the present invention may include a step of performing laser annealing (i.e., laser heat treatment) by irradiating a laser (L10) to the semiconductor element portion under a pressure condition higher than 1 atm in a gas atmosphere of at least one of deuterium (D2), hydrogen (H2), and ammonia (NH3). The semiconductor element portion may be placed in a predetermined chamber, and the laser annealing may be performed by irradiating the semiconductor element portion with a laser (L10) in a state where a pressure higher than 1 atm is formed in the chamber with the gas atmosphere. The laser annealing may be for passivating at least interface charges between the semiconductor and the dielectric. In the present embodiment, the semiconductor may be a channel portion (110), and the dielectric may be a gate dielectric layer (120).

[0043] The gas used to form the above-described gas atmosphere may include at least an element for passivating the interface charge between the semiconductor and the dielectric, i.e., the interface charge between the channel portion (110) and the gate dielectric layer (120). In one example, the element of the gas may play a role in inactivating (i.e., passivating) the interface charge generated by a dangling bond or the like by forming Si-D bonding or Si-H bonding, etc., at or around the bonding interface between the channel portion (110) and the gate dielectric layer (120) through the heat treatment process using the laser annealing described above. At this time, not only the interface charge but also fixed charges existing around the interface may be inactivated (passivated) by a similar principle as above. Accordingly, the interface characteristics between the channel portion (110) and the gate dielectric layer (120) and the physical properties of the gate dielectric layer (120) are improved, and as a result, the performance, stability, and reliability of the transistor element can be improved.

[0044] In particular, when deuterium is used in the above gas atmosphere, since deuterium has a higher bonding energy with semiconductors such as silicon than hydrogen, the stability and reliability of the transistor element can be further improved. For example, since more energy is required to break a Si-D bond than a Si-H bond, the use of deuterium can be more effective in lowering the trap level at the bonding interface and performing the passivation process. In this respect, it may be preferable to perform the laser annealing in a deuterium (D2) gas atmosphere. The laser annealing can be performed in a 100% deuterium (D2) gas atmosphere, or in a gas atmosphere containing about 10% or more or about 40% or more deuterium (D2). However, in some cases, other gases than deuterium (D2) gas, that is, other passivation gases such as hydrogen (H2) gas or ammonia (NH3) gas, may be used.

[0045] In the above-described laser annealing, the pressure formed within the chamber may be greater than 1 atm (760 Torr). For example, the pressure may be greater than 1 atm and less than or equal to 100 atm. More preferably, the pressure may be 3 atm or more and 100 atm or less, or 3 atm or more and 50 atm or less. In the above-described laser annealing, by forming a relatively high pressure condition, the element of the gas (passivation gas) can be made to bond better with a semiconductor element such as silicon. That is, by using a relatively high pressure condition, the element of the gas (passivation gas) can bond better with a semiconductor element such as silicon at the interface between the channel portion (110) and the gate dielectric layer (120) and the surrounding area thereof. In particular, when the gas contains deuterium, the bonding promotion effect (bonding promotion effect between elements) due to the high pressure can be further enhanced. Additionally, when the above pressure is about 3 atm or more, the effect of promoting bonding between elements can be enhanced.

[0046] The laser (L10) used in the above laser annealing may be, for example, a laser (laser beam) generated from any one of a YAG (yttrium aluminum garnet) laser generator, a CO2 laser generator, a diode laser generator, and a fiber laser generator. The laser (L10) may include any one of ultraviolet ray, visible ray, infrared ray, and microwave. The laser (L10) may have, for example, a wavelength of about 0.02 μm to about 11 μm.

[0047] In the above laser annealing, the laser (L10) can be irradiated from above the semiconductor element portion to the surface of the insulating layer (150). The laser annealing can be performed so that the temperature of the surface portion of the semiconductor element portion is increased to about 600°C to 2000°C. Since the laser (L10) is used, the temperature of the surface portion of the semiconductor element portion can be increased to a considerably high temperature in a short period of time, and the heat treatment process for the above-described passivation can be performed efficiently and easily. In particular, the process of deactivating interface charges and fixed charges, etc. can be performed efficiently and effectively in a short period of time by promoting the penetration and bonding of elements due to the instantaneous heating and pressurization conditions caused by the laser irradiation.

[0048] The laser annealing may be performed for, for example, about 0.01 μs to 10 seconds. More preferably, the laser annealing may be performed for about 0.1 μs to 1 second. However, the time range of the laser annealing is not limited to the above-described time range and may be adjusted in various ways depending on the case.

[0049] According to one embodiment of the present invention, the laser annealing may be performed while the temperature of the substrate (100) is controlled to a range of room temperature (e.g., about 25°C) to about 550°C. More specifically, the laser annealing may be performed while the temperature of the substrate (100) is controlled to a range of room temperature to about 550°C or a range of about 350°C to about 450°C. When the laser annealing is performed while the substrate (100) is heated to a predetermined temperature, passivation of the interface charge may be performed more efficiently. However, when the temperature of the substrate (100) is high, such as about 550°C or higher or about 450°C or higher, there is a possibility that an undesirable reaction that deteriorates the characteristics of the transistor may occur in the substrate (100) portion. Therefore, the heating temperature of the substrate (100) may be preferably about 550°C or lower or about 450°C or lower.

[0050] Referring to FIG. 1C, a wiring member (200) may be formed on an insulating layer (150). The wiring member (200) may be a member electrically connected to the transistor. For example, the wiring member (200) may be formed to be electrically connected to the gate electrode (130). Here, one wiring member (200) is illustrated, but a plurality of wiring members may be formed. A wiring member electrically connected to the source (140A) may be further provided, and a wiring member electrically connected to the drain (140B) may be further provided. The wiring member (200) may be considered a component included in the transistor.

[0051] The wiring member (200) may include at least one of a metal and a metal compound. Therefore, the process of forming the wiring member (200) may be referred to as a type of metallization process. Materials for common electrodes, contact layers, and wiring used in semiconductor processes may be applied to the wiring member (200). The wiring member (200) does not necessarily have to have a line shape, and its shape may vary. The wiring member (200) may be referred to as a metallic member or metal wiring including a metal or a metal compound.

[0052] Although the embodiments of FIGS. 1A to 1C have described cases where the laser annealing process is performed before the metallization process, according to another embodiment of the present invention, the laser annealing process may be performed after the metallization process. This other embodiment will be described with reference to FIGS. 2A and 2B.

[0053] FIGS. 2A and 2B are cross-sectional views illustrating a laser annealing method for a semiconductor device including a transistor according to another embodiment of the present invention.

[0054] Referring to FIG. 2A, a laser annealing method according to an embodiment of the present invention may include a step of preparing a semiconductor device having a transistor. The semiconductor device of FIG. 2A may include the configuration of the transistor described in FIG. 1A. That is, the semiconductor device of FIG. 2A may include a substrate (101), a channel portion (111), a gate dielectric layer (121), a gate electrode (131), a source (141A), a drain (141B), and an insulating layer (151). The substrate (101), the channel portion (111), the gate dielectric layer (121), the gate electrode (131), the source (141A), the drain (141B), and the insulating layer (151) may respectively correspond to the substrate (100), the channel portion (110), the gate dielectric layer (120), the gate electrode (130), the source (140A), the drain (140B), and the insulating layer (150) of FIG. 1A.

[0055] In this embodiment, before performing laser annealing, a wiring member (201) may be formed on an insulating layer (151) by a metallization process. The wiring member (201) may be the same as or similar to the wiring member (200) described in FIG. 1C.

[0056] Referring to FIG. 2b, the laser annealing method according to the present embodiment may include a step of performing laser annealing (i.e., laser heat treatment) by irradiating a laser (L11) to the semiconductor element under a pressure condition higher than 1 atm in a gas atmosphere of at least one of deuterium (D2), hydrogen (H2), and ammonia (NH3). The semiconductor element may be placed in a predetermined chamber, and the laser annealing may be performed by irradiating the semiconductor element with a laser (L11) in a state where a pressure higher than 1 atm is formed in the chamber with the gas atmosphere. The laser annealing may be for passivating at least interface charges between the semiconductor and the dielectric. The semiconductor may be a channel portion (111), and the dielectric may be a gate dielectric layer (121).

[0057] Specific conditions, characteristics, effects, etc. of the above laser annealing may be similar to those described with reference to FIG. 1B. The pressure condition may be a condition of about 100 atm or less. More preferably, the pressure condition may be a condition of about 1 atm or more and 100 atm or less, or a condition of about 3 atm or more and 100 atm or less. The laser annealing may be preferably performed in a gas atmosphere including deuterium (D2). The laser annealing may be performed so that the temperature of the surface of the semiconductor element portion is increased to about 600°C to 2000°C. The laser annealing may be performed for, for example, about 0.01 μs to 10 seconds. The laser may include any one of ultraviolet ray, visible ray, infrared ray, and microwave. The above laser annealing can be performed while the temperature of the substrate (101) is controlled to a range of about room temperature to about 550°C. For example, the above laser annealing can be performed while the temperature of the substrate (101) is controlled to a range of about room temperature to about 550°C. In addition, specific conditions, characteristics, effects, etc. of the laser annealing can be referred to as described with reference to Fig. 1b.

[0058] According to an example, the temperature at which the surface of the semiconductor element is heated by the laser annealing in the present embodiment may be lower than the temperature at which the surface of the semiconductor element is heated by the laser annealing in the embodiment of Fig. 1b. When the laser annealing is performed in a state where the wiring member (201) is formed, the heating temperature of the surface may be controlled so that the wiring member (201) is not damaged by the laser annealing. In addition, it may be preferable to form the wiring member (201) with a relatively high melting point, such as a metal or a metal compound.

[0059] In the case of the embodiment described with reference to FIGS. 2a and 2b, since the laser annealing is performed in a state where the wiring member (201) is formed in advance to passivate the interface charge between the channel portion (111) and the gate dielectric layer (121), after the passivation, the interface area between the channel portion (111) and the gate dielectric layer (121) may not be affected by the process for forming the wiring member (201).

[0060] FIGS. 3A to 3D are cross-sectional views illustrating a laser annealing method for a semiconductor device including a transistor according to another embodiment of the present invention.

[0061] Referring to FIG. 3A, a laser annealing method according to an embodiment of the present invention may include a step of preparing a semiconductor device having a transistor. The semiconductor device of FIG. 3A may include the configuration of the transistor described in FIG. 1A. That is, the semiconductor device of FIG. 3A may include a substrate (102), a channel portion (112), a gate dielectric layer (122), a gate electrode (132), a source (142A), a drain (142B), and an insulating layer (152). The substrate (102), the channel portion (112), the gate dielectric layer (122), the gate electrode (132), the source (142A), the drain (142B), and the insulating layer (152) may respectively correspond to the substrate (100), the channel portion (110), the gate dielectric layer (120), the gate electrode (130), the source (140A), the drain (140B), and the insulating layer (150) of FIG. 1A.

[0062] In the present embodiment, before performing laser annealing, a heating layer (162) may be formed on the insulating layer (152). The heating layer (162) may include at least one of a metal and a metal compound. For example, the heating layer (162) may include at least one of TiN, Ti, TiSi, Ta, TaN, Co, CoSi, Ni, NiSi, Ru, W, WSi, Cu, Re, Mo, Nb, and Cr. It may be desirable for the heating layer (162) to have a thickness of about 30 Å to 4000 Å to improve its function, but the present embodiment is not limited thereto, and the appropriate thickness of the heating layer (162) may vary depending on the case. The heating layer (162) may have a relatively high absorption rate for the laser, and may serve to transfer or trap heat toward the insulating layer (152). In this regard, the heating layer (162) may be referred to as a ‘laser absorption layer (high absorption layer)’ or a ‘heat transfer layer.’

[0063] According to one embodiment, the heating layer (162) may have a nano pattern structure or a nano dot array structure. For example, the heating layer (162) may include a nano dot array including a plurality of nano dots (12). The plurality of nano dots (12) may be formed of a metallic material such as a metal or a metal compound. When the heating layer (162) has a nano dot array structure, in a subsequent laser annealing step, the heating layer (162) can effectively perform the role of absorbing laser and transmitting heat while effectively allowing gas to pass through. However, in some cases, the heating layer (162) may not have a nano dot array structure, and may have a continuous layer structure. When the heating layer (162) has a continuous layer structure, the gas permeation characteristics can be adjusted by appropriately controlling the thickness thereof.

[0064] Referring to FIG. 3b, the laser annealing method according to the present embodiment may include a step of performing laser annealing (i.e., laser heat treatment) by irradiating a laser (L12) to the semiconductor element under a pressure condition higher than 1 atm in a gas atmosphere of at least one of deuterium (D2), hydrogen (H2), and ammonia (NH3). The semiconductor element may be placed in a predetermined chamber, and the laser annealing may be performed by irradiating the semiconductor element with a laser (L12) in a state where a pressure higher than 1 atm is formed in the chamber with the gas atmosphere. The laser annealing may be for passivating at least interface charges between the semiconductor and the dielectric. The semiconductor may be a channel portion (112), and the dielectric may be a gate dielectric layer (122).

[0065] The specific conditions, characteristics, effects, etc. of the laser annealing may be the same as or similar to those described with reference to FIG. 1B. The pressure condition may be a condition of about 100 atm or less. More preferably, the pressure condition may be a condition of about 1 atm or more and 100 atm or less, or a condition of about 3 atm or more and 100 atm or less. The laser annealing may be preferably performed in a gas atmosphere including deuterium (D2). The laser annealing may be performed so that the temperature of the surface of the semiconductor element portion is increased to about 600°C to 2000°C. The laser annealing may be performed for, for example, about 0.01 μs to 10 seconds. The laser may include any one of ultraviolet ray, visible ray, infrared ray, and microwave. The above laser annealing can be performed while the temperature of the substrate (102) is controlled to a range of about room temperature to about 550°C. For example, the above laser annealing can be performed while the temperature of the substrate (102) is controlled to a range of about room temperature to about 550°C. In addition, specific conditions, characteristics, effects, etc. of the above laser annealing can be referred to as described with reference to FIG. 1B.

[0066] After the step of Fig. 3b, the heating layer (162) can be removed. The result is shown in Fig. 3c.

[0067] Referring to FIG. 3d, a wiring member (202) can be formed on an insulating layer (152) through a metallization process. The wiring member (202) can be the same as or similar to the wiring member (200) described in FIG. 1c.

[0068] FIG. 4 is a plan view exemplarily showing the shape of a pattern that a plurality of nano dots (12) constituting the heating layer (162) described in FIGS. 3a and 3b can have.

[0069] Referring to Fig. 4, if the dimensions of a plurality of nano dots (12) and the spacing between them are appropriately controlled, the heating layer (162) including them can have a discontinuous layer structure while easily absorbing heat energy by a laser and effectively allowing the penetration of gas. In this regard, the diameter of a plurality of nano dots (12) is about 5 nm to 10 3 nm may be desirable, and the spacing between multiple nano dots (12) is about 5 nm to 10 2 It may be desirable that the diameter and spacing of the plurality of nano dots (12) be on the order of nm. However, the range of appropriate diameters and spacings of the plurality of nano dots (12) may vary depending on the wavelength of the laser being used. In addition, the arrangement of the plurality of nano dots (12) is not limited to that shown in FIG. 4 and may vary. In addition, the heating layer (162) may have various nano pattern shapes other than a nano dot array structure, and in some cases, may have a continuous layer shape.

[0070] The 'transistor' described in the above-described embodiments may have a MOSFET structure, but may also have various other transistor structures. For example, the transistor may have various transistor structures such as a GAA (gate-all-around) FET structure, a fin FET structure, a tunneling FET structure, a spin FET structure, and a recess transistor structure. In addition, the 'transistor' described in the above-described embodiments may be a transistor as a general switching element or a driving element, and in some cases, may also be a memory transistor. When the transistor is a memory transistor, for example, a tunnel insulating layer (dielectric layer), a charge storage layer (charge trap layer), and a blocking insulating layer may be sequentially disposed between a semiconductor channel and a gate electrode (control gate electrode). In this case, the laser annealing process may be a process that improves the performance, stability, and reliability of the device by passivating at least an interface charge between the semiconductor channel and the tunnel insulating layer (dielectric layer). The term transistor as used herein may be interpreted broadly.

[0071] According to an embodiment of the present invention, a method for manufacturing a semiconductor device using the aforementioned laser annealing method is provided. Here, the semiconductor device may be a memory device or a non-memory device. The semiconductor device may encompass various electronic devices.

[0072] According to the embodiments of the present invention described above, in the manufacture of a semiconductor device including a transistor, a process technology (laser annealing method) can be implemented that can efficiently passivate the interface charge between the semiconductor and the dielectric while significantly improving the performance, stability, and reliability of the transistor. According to one embodiment, by performing a high-speed annealing process using laser irradiation under a pressure condition higher than 1 atm in a gas atmosphere such as deuterium (D2) having a high binding energy for a semiconductor element (e.g., silicon), a passivation process for removing the interface charge can be efficiently performed, and the performance, stability, and reliability of the semiconductor device can be significantly improved. In addition, the process technology (laser annealing method) according to the embodiments of the present invention can be usefully utilized in the manufacture of highly integrated semiconductor devices. By applying the laser annealing method according to the embodiments of the present invention, it can be possible to manufacture a semiconductor device having a high degree of integration while also having excellent performance, stability, and reliability.

[0073] In this specification, preferred embodiments of the present invention have been disclosed, and although specific terms have been used, they have been used in a general sense only to easily explain the technical contents of the present invention and to help the understanding of the invention, and are not intended to limit the scope of the present invention. It will be apparent to those skilled in the art that other modifications based on the technical idea of ​​the present invention can be implemented in addition to the embodiments disclosed herein. Those skilled in the art will appreciate that the laser annealing method according to the embodiments described with reference to FIGS. 1A to 4 and the method for manufacturing a semiconductor device using the same can be variously substituted, changed, and modified without departing from the technical idea of ​​the present invention. Therefore, the scope of the invention should not be defined by the described embodiments, but by the technical idea described in the claims.

[0074] Embodiments of the present invention can be applied to an annealing method for a workpiece and the manufacture of devices using the method. Embodiments of the present invention can be applied to a laser annealing method and the manufacture of semiconductor devices using the method.

Claims

1. A laser annealing method for a semiconductor device including a transistor, A step of providing a semiconductor device having a transistor including a semiconductor and a dielectric forming a bonding interface with the semiconductor; and A laser annealing method for a semiconductor device, comprising the step of performing laser annealing by irradiating a laser to the semiconductor device under a pressure condition higher than 1 atmosphere in an atmosphere of at least one gas among deuterium (D2), hydrogen (H2), and ammonia (NH3) for passivating at least interface charges between the semiconductor and the dielectric.

2. In paragraph 1, The above pressure condition is a laser annealing method for a semiconductor element under conditions of 100 atm or less.

3. In paragraph 1, A laser annealing method for a semiconductor device, wherein the above pressure conditions are more than 1 atm and less than 100 atm.

4. In paragraph 1, The above transistor is formed on a substrate, A laser annealing method for a semiconductor device, wherein the laser annealing is performed while the temperature of the substrate is controlled within a range from room temperature to 550°C.

5. In paragraph 1, The above laser annealing is a laser annealing method for a semiconductor device performed in a deuterium (D2) gas atmosphere.

6. In paragraph 1, A laser annealing method for a semiconductor device, wherein the above laser annealing is performed so that the temperature of the surface of the semiconductor device is increased to 600°C to 2000°C.

7. In paragraph 1, A laser annealing method for a semiconductor device, wherein the above laser annealing is performed for 0.01 μs to 10 seconds.

8. In paragraph 1, The semiconductor comprises a channel of the transistor, The above dielectric is a laser annealing method for a semiconductor element including a gate dielectric layer of the transistor.

9. In paragraph 1, The step of providing the semiconductor element portion includes the step of forming a wiring member electrically connected to the transistor, A laser annealing method for a semiconductor device, wherein the laser annealing is performed before or after the step of forming the wiring member.

10. In paragraph 1, A laser annealing method for a semiconductor device, wherein the laser includes any one of ultraviolet ray, visible ray, infrared ray, and microwave.

11. A method for manufacturing a semiconductor device using the laser annealing method described in any one of claims 1 to 10.

Citation Information

Patent Citations

  • Method for manufacturing thin film semiconductor device

    JP3169309B2

  • Method for forming SOI mosfet by annealing in high-pressure hydrogen ambient

    KR100771229B1

  • Lateral diffusion MOS device and method for manufacturing the device

    KR101581690B1

  • Method of manufacturing a transistor having a trenchtype gate in a semiconductor device

    KR1020050079555A

  • Transistors with a gate insulation layer having a channel depleting interfacial charge and related fabrication methods

    US20110049530A1