Lithium secondary battery

The lithium secondary battery design with a coated lithium-nickel metal oxide and silicon-based active materials addresses stability and capacity issues, enhancing lifespan and high-temperature performance.

WO2024242370A1PCT designated stage expired Publication Date: 2024-11-28SK ON CO LTD

Patent Information

Application Number
PCT/KR2024/006135
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2024-05-08
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Lithium-nickel metal oxide batteries face reduced structural stability and deteriorated lifespan characteristics due to high nickel content, leading to capacity degradation during repeated charging and discharging.

Method used

A lithium secondary battery design incorporating a positive electrode with a lithium-nickel metal oxide coating layer containing lithium-phosphorus, lithium-sulfur, lithium-tungsten, or lithium-aluminum compounds, and a silicon-based negative electrode active material, enhancing structural stability and capacity maintenance.

Benefits of technology

The solution improves the battery's lifespan characteristics, especially at high temperatures, and maintains capacity retention during rapid charge/discharge cycles, while reducing gas generation and preventing performance degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006135_28112024_PF_FP_ABST
    Figure KR2024006135_28112024_PF_FP_ABST
Patent Text Reader

Abstract

A lithium secondary battery according to embodiments of the present disclosure comprises: a positive electrode containing a first positive electrode active material; and a negative electrode containing a silicon-based active material, wherein the first positive electrode active material comprises: lithium-nickel metal oxide particles; and a coating layer disposed on the surface of the lithium-nickel metal oxide particles and including at least one selected from the group consisting of a lithium-phosphorus-containing compound, a lithium-sulfur-containing compound, a lithium-tungsten-containing compound, and a lithium-aluminum-containing compound. The lithium secondary battery of the present disclosure can achieve improvements in high-temperature lifespan characteristics and rapid charge / discharge lifespan characteristics and a reduction in the amount of gas generated.
Need to check novelty before this filing date? Find Prior Art

Description

lithium secondary battery

[0001] The present disclosure provides a lithium secondary battery. More specifically, the present disclosure relates to a lithium secondary battery including a positive electrode and a negative electrode.

[0002]

[0003] Secondary batteries, which can be repeatedly charged and discharged, are widely used as power sources for portable electronic communication devices such as camcorders, mobile phones, and laptops, thanks to the advancements in the information and communication and display industries. Furthermore, battery packs containing secondary batteries are being developed and applied as power sources for eco-friendly vehicles such as hybrid vehicles.

[0004] Examples of secondary batteries include lithium secondary batteries, nickel-cadmium batteries, and nickel-hydrogen batteries. Among these, lithium secondary batteries are actively being researched and developed due to their high operating voltage and energy density per unit weight, as well as their advantages in charging speed and weight reduction.

[0005] A lithium secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator, and an electrolyte impregnating the electrode assembly. The lithium secondary battery may further include an outer packaging material, for example, in the form of a pouch, that accommodates the electrode assembly and the electrolyte.

[0006] Lithium-nickel metal oxide can be used as an active material for the positive electrode of a lithium secondary battery. An example of the lithium-nickel metal oxide is a nickel-based lithium metal oxide. Nickel-based lithium metal oxide can increase the capacity of the battery by containing a high nickel content.

[0007] However, nickel-based lithium metal oxide has a problem in that the structural stability of the battery is poor during repeated charging and discharging when the nickel content increases, which reduces the life characteristics of the battery.

[0008]

[0009] An object of the present disclosure is to provide a lithium secondary battery with improved life characteristics.

[0010]

[0011] According to exemplary embodiments, a lithium secondary battery is provided, comprising: a positive electrode including a positive current collector and a positive active material layer disposed on the positive current collector and including a first positive active material; and a negative electrode including a negative current collector and a negative active material layer disposed on the negative current collector and including a silicon-based active material, wherein the first positive active material comprises lithium-nickel metal oxide particles and a coating layer disposed on at least a portion of a surface of the lithium-nickel metal oxide particles and including at least one selected from the group consisting of a lithium-phosphorus-containing compound, a lithium-sulfur-containing compound, a lithium-tungsten-containing compound, and a lithium-aluminum-containing compound.

[0012] According to exemplary embodiments, the content of the first positive electrode active material may be 50 wt% to 99.0 wt% of the total weight of the positive electrode active material layer.

[0013] According to exemplary embodiments, the lithium-nickel metal oxide particle has a secondary particle structure in which a plurality of primary particles are aggregated, and the coating layer may be disposed on at least a portion of a surface of the secondary particle and on at least a portion of an interface of the plurality of primary particles inside the secondary particle.

[0014] According to exemplary embodiments, the lithium-nickel metal oxide further includes at least one of cobalt and manganese, and the content of nickel in the lithium-nickel metal oxide may be from 48 mol% to 98 mol% based on the total mole number of nickel, cobalt, and manganese.

[0015] According to exemplary embodiments, the positive electrode active material layer may further include a second positive electrode active material including lithium-nickel metal oxide particles having a secondary particle structure in which a plurality of primary particles are aggregated, and not including the coating layer.

[0016] According to exemplary embodiments, the positive electrode active material layer may further include a third positive electrode active material including lithium-nickel metal oxide particles having a crystal grain size of 250 nm to 1000 nm as measured by X-ray diffraction analysis (XRD) and calculated by Equation 1 below, and not including the coating layer.

[0017] [Formula 1]

[0018]

[0019] (In Equation 1, L is the grain size, λ is the X-ray wavelength, β is the half width of the peak on the (003) plane, and θ is the diffraction angle).

[0020] According to exemplary embodiments, the positive electrode active material layer includes a first positive electrode active material layer and a second positive electrode active material layer sequentially stacked on the positive electrode current collector, and the first positive electrode active material layer and the second positive electrode active material layer may each independently include at least one positive electrode active material selected from the group consisting of the first positive electrode active material, the second positive electrode active material, and the third positive electrode active material. The second positive electrode active material includes lithium-nickel metal oxide particles having a secondary particle structure in which a plurality of primary particles are aggregated, and does not include the coating layer, and the third positive electrode active material includes lithium-nickel metal oxide particles having a crystal grain size of 250 nm to 1000 nm as measured by X-ray diffraction analysis (XRD) and calculated by the following Equation 1, and may not include the coating layer. At least one of the type and content of the positive electrode active materials included in the first positive electrode active material layer and the second positive electrode active material layer may be different from each other.

[0021] [Formula 1]

[0022]

[0023] (In Equation 1, L is the grain size, λ is the X-ray wavelength, β is the half width of the peak on the (003) plane, and θ is the diffraction angle).

[0024] According to exemplary embodiments, the positive electrode active material layer includes a first positive electrode active material layer and a second positive electrode active material layer sequentially laminated on the positive electrode current collector, the first positive electrode active material layer and the second positive electrode active material layer each include a binder, and the content of the binder in the total weight of the first positive electrode active material layer may be greater than or equal to the content of the binder in the total weight of the second positive electrode active material layer.

[0025] According to exemplary embodiments, the content of the second positive electrode active material may be 10 wt% to 50 wt% of the total weight of the positive electrode active material layer.

[0026] According to exemplary embodiments, the content of the third positive electrode active material may be 10 wt% to 50 wt% of the total weight of the positive electrode active material layer.

[0027] According to exemplary embodiments, within a region of a depth of 10 nm to 30 nm from the surface of the primary particle of the second positive electrode active material, a region may exist in which the content of the layered structure is smaller than the sum of the contents of the cubic structure and the spinel structure.

[0028] According to exemplary embodiments, the silicon-based active material may include at least one selected from the group consisting of silicon, silicon alloy, silicon oxide, metal-doped silicon oxide, silicon carbide, silicon-carbon composite (Si-C), and silicon-containing core-shell structured particles.

[0029] According to exemplary embodiments, the content of the silicon-based active material may be 5 wt% to 30 wt% of the total weight of the negative electrode active material layer.

[0030] According to exemplary embodiments, the negative active material may further include artificial graphite.

[0031] According to exemplary embodiments, the negative electrode active material layer includes a first negative electrode active material layer and a second negative electrode active material layer sequentially laminated on the negative electrode current collector, and the first negative electrode active material layer and the second negative electrode active material layer each include a binder, and the content of the binder in the total weight of the first negative electrode active material layer may be greater than or equal to the content of the binder in the total weight of the second negative electrode active material layer.

[0032] According to exemplary embodiments, the negative electrode may further include a primer layer disposed between the negative electrode active material layer and the negative electrode current collector, the primer layer including a binder.

[0033]

[0034] A lithium secondary battery according to exemplary embodiments of the present disclosure may include lithium-nickel metal oxide particles including a coating layer containing at least one of a lithium-phosphorus-containing compound, a lithium-sulfur-containing compound, a lithium-tungsten-containing compound, and a lithium-aluminum-containing compound. Accordingly, even when the battery is repeatedly charged and discharged at high temperatures, electrode stability is maintained, and capacity retention can be improved. The lithium secondary battery includes a silicon-based active material, and rapid charge / discharge characteristics and capacity characteristics can be further improved.

[0035] According to some embodiments, the battery may include a first positive electrode active material and a second positive electrode active material that does not include the coating layer. Accordingly, the battery can have sufficient capacity while improving room temperature cycle characteristics or rapid cycle characteristics.

[0036] According to some embodiments, the positive or negative electrode may include a multi-layered active material layer. The active material layer adjacent to the current collector may contain a higher binder content, thereby improving the adhesion and mechanical stability of the active material layer.

[0037]

[0038] FIG. 1 is a schematic plan perspective view showing a lithium secondary battery according to an exemplary embodiment.

[0039] Figure 2 is a schematic cross-sectional view showing a lithium secondary battery according to an exemplary embodiment.

[0040] Figures 3a to 3c are primary particle TEM-SAED images of the second positive electrode active material manufactured in Synthesis Example 2-1.

[0041] Figures 4a and 4b are TEM images of the first positive electrode active material manufactured in Synthesis Example 1-1.

[0042] Fig. 5a is a cross-sectional SEM image of the particle of the first positive electrode active material manufactured in Synthesis Example 1-3, and Figs. 5b and 5c are EDS elemental mapping images of sulfur and tungsten elements, respectively, for the image of Fig. 5a.

[0043] Figures 6a to 6d are SSRM diffusion resistance distribution images of electrodes including the positive active materials of Synthesis Examples 1-3 and 1-1.

[0044] Figure 7 is a graph of the discharge capacity retention rate during high-temperature charge / discharge according to the number of cycles in Examples 1 to 3.

[0045] Figure 8 is a graph of the discharge capacity retention rate during high-temperature charge / discharge according to the number of cycles in Examples 1, 4, 5, and 11.

[0046] Figure 9 is a graph of the discharge capacity retention rate during high-temperature charge / discharge according to the number of cycles in Examples 1 and 6 to 8.

[0047] Figure 10 is a graph of the discharge capacity retention rate during high-temperature charge / discharge according to the number of cycles in Examples 1 and 9 to 10.

[0048] Figure 11 is a graph of the discharge capacity retention rate during high-temperature charge / discharge according to the number of cycles in Example 1 and Comparative Examples 1 to 3.

[0049] Figure 12 is a graph of the discharge capacity retention rate during rapid charge / discharge according to the number of cycles in Examples 1 to 3.

[0050] Figure 13 is a graph of the discharge capacity retention rate during rapid charge / discharge according to the number of cycles in Examples 1, 4, 5, and 11.

[0051] Figure 14 is a graph of the discharge capacity retention rate during rapid charge / discharge according to the number of cycles in Examples 1 and 6 to 8.

[0052] Figure 15 is a graph of the discharge capacity retention rate during rapid charge / discharge according to the number of cycles in Examples 1 and 9 to 10.

[0053] Figure 16 is a graph of the discharge capacity retention rate during rapid charge / discharge according to the number of cycles in Example 1 and Comparative Examples 1 to 3.

[0054]

[0055] According to exemplary embodiments, a high-capacity lithium secondary battery with improved rapid charging characteristics is provided.

[0056] Hereinafter, embodiments of the present disclosure will be described in more detail with reference to the drawings. However, the following drawings attached to this specification illustrate preferred embodiments of the present disclosure and, together with the contents of the invention described above, serve to further understand the technical concept of the present disclosure. Therefore, the present disclosure should not be interpreted as being limited to the matters described in the drawings.

[0057] FIG. 1 is a schematic plan perspective view showing a lithium secondary battery according to an exemplary embodiment, and FIG. 2 is a cross-sectional view of the lithium secondary battery according to an exemplary embodiment taken along line II' of FIG. 1.

[0058] Referring to FIGS. 1 and 2, a lithium secondary battery may include a negative electrode (130), a positive electrode (100) opposite to the negative electrode (130), and an electrolyte (not shown).

[0059] According to exemplary embodiments, the positive electrode (100) may include a positive electrode active material layer (110) on at least one surface of the positive electrode current collector (105). The positive electrode active material layer (110) may include a positive electrode active material. For example, the positive electrode active material may include lithium metal oxide particles capable of reversible insertion and deintercalation of lithium ions.

[0060] The above positive electrode active material may include a first positive electrode active material. The first positive electrode active material may include lithium-nickel metal oxide particles.

[0061] In exemplary embodiments, the lithium-nickel metal oxide may further include at least one of cobalt and manganese. In some embodiments, the lithium-nickel metal oxide may include lithium, nickel, cobalt, and manganese.

[0062] The content of nickel in the lithium-nickel metal oxide may be 48 mol% to 98 mol% based on the total moles of nickel, cobalt, and manganese. When nickel is included in a content within the above range, a high-capacity secondary battery can be realized.

[0063] In some embodiments, the lithium-nickel metal oxide may be represented by the following chemical formula:

[0064] [chemical formula]

[0065] Li x Ni (1-a) M a O y

[0066] In the above chemical formula, M is at least one of Co, Al, Zr, Ti, Cr, B, Mg, Mn, Ba, Si, Y, W, and Sr, and 0.9≤x≤1.2, 1.9≤y≤2.1, 0.02≤a≤0.52 may be satisfied.

[0067] In some embodiments, the lithium-nickel metal oxide may include a doping metal. For example, the doping metal may include at least one of Al, Zr, Ti, Cr, B, Mg, Ba, Si, Y, W, and Sr, and may be doped in a form that substitutes for lithium and / or nickel sites in the lithium-nickel metal oxide.

[0068] The first positive electrode active material may be disposed on at least a portion of the surface of the particle and may include a coating layer including at least one selected from the group consisting of a lithium-phosphorus-containing compound, a lithium-sulfur-containing compound, a lithium-tungsten-containing compound, and a lithium-aluminum-containing compound. In some embodiments, the coating layer may include at least one of a lithium-phosphorus-containing compound and a lithium-sulfur-containing compound, and at least one of a lithium-tungsten-containing compound and a lithium-aluminum-containing compound.

[0069] The coating layer may include a lithium-phosphorus-containing compound, a lithium-sulfur-containing compound, a lithium-tungsten-containing compound, and / or a lithium-aluminum-containing compound formed during the process of removing residual lithium from the first positive electrode active material. Accordingly, the amount of residual lithium within the first positive electrode active material may be reduced, and the capacity retention rate during high-temperature charge / discharge of a lithium secondary battery may be improved.

[0070] The lithium-phosphorus containing compound may include a lithium phosphate compound, for example, Li3PO4. The lithium-sulfur containing compound may include a lithium sulfate compound, for example, Li2SO4. The lithium-tungsten containing compound may include a lithium tungstate compound, for example, Li2WO4 and / or Li2W2O7. The lithium-aluminum containing compound may include LiAlO2.

[0071] According to exemplary embodiments, the coating layer may include a lithium-tungsten-containing compound. The coating layer including the lithium-tungsten-containing compound can improve the durability of the first positive electrode active material and, by reacting with LiOH on the surface of the active material, form a lithium tungsten coating material with excellent conductivity, thereby further reducing the amount of residual LiOH. Accordingly, even if the lithium secondary battery is operated for a long period of time, a significant decrease in capacity can be prevented, and battery performance can be improved, particularly when charged and discharged in a high-temperature environment or during high-speed charge and discharge.

[0072] According to exemplary embodiments, the coating layer may be disposed on at least a portion of the surface of the lithium-nickel metal oxide. For example, the coating layer may be in the form of microparticles including at least one selected from the group consisting of a lithium-phosphorus-containing compound, a lithium-sulfur-containing compound, a lithium-tungsten-containing compound, and a lithium-aluminum-containing compound, attached in the form of islands to the surface of the lithium-nickel metal oxide particles.

[0073] For example, the coating layer may be in a form that continuously covers at least a portion of the surface of the lithium-nickel metal oxide particles of the first positive electrode active material. In this case, the coating layer may include a lithium-tungsten-containing compound.

[0074] In some embodiments, the first positive electrode active material may include lithium-nickel metal oxide particles having a secondary particle structure in which a plurality of primary particles are aggregated. The secondary particles may include a plurality of primary particles, and an interface may exist within the secondary particles where the primary particles come into contact with each other.

[0075] In exemplary embodiments, the coating layer may be disposed on at least a portion of the surfaces of the primary particles and may be present on at least a portion of the interfaces of the primary particles present inside the secondary particles. The coating layer may also be present on at least a portion of the outer surface of the secondary particles, which is the surface of the primary particles exposed to the outside of the secondary particles.

[0076] The content of the first positive electrode active material may be 50 wt% to 99 wt% of the total weight of the positive electrode active material layer. According to some embodiments, the content of the first positive electrode active material may be 60 wt% to 99 wt% or 65 wt% to 99 wt% of the total weight of the positive electrode active material layer.

[0077] Within the above range, the high-temperature characteristics of lithium secondary batteries can be improved. For example, lifespan characteristics can be improved in environments that are relatively higher than room temperature, and even when stored for long periods at high temperatures, the amount of gas generated can be reduced, preventing battery performance degradation and damage.

[0078] According to exemplary embodiments, the first positive electrode active material can be manufactured by the following method.

[0079] According to exemplary embodiments, lithium-nickel metal oxide particles can be first manufactured. The lithium-nickel metal oxide particles may be in the form of secondary particles in which a plurality of primary particles are aggregated. The lithium-nickel metal oxide particles can be manufactured by a method known in the art. For example, the lithium-nickel metal oxide particles can be manufactured by reacting a transition metal precursor with a lithium raw material. The transition metal precursor (e.g., a Ni-Co-Mn hydroxide precursor) can be manufactured through a co-precipitation reaction.

[0080] For example, transition metal precursors can be prepared through a co-precipitation reaction of metal salts. The metal salts can include nickel salts, manganese salts, and cobalt salts.

[0081] Examples of the nickel salts include nickel sulfate, nickel hydroxide, nickel nitrate, nickel acetate, and hydrates thereof. Examples of the manganese salts include manganese sulfate, manganese acetate, and hydrates thereof.

[0082] Examples of the above cobalt salts include cobalt sulfate, cobalt nitrate, cobalt carbonate, and hydrates thereof.

[0083] The above metal salts can be mixed with a precipitant and / or a chelating agent in a ratio that satisfies the content or concentration ratio of each metal described with reference to Chemical Formula 1 to prepare an aqueous solution. The aqueous solution can be co-precipitated in a reactor to prepare a transition metal precursor.

[0084] The precipitant may include an alkaline compound such as sodium hydroxide (NaOH), sodium carbonate (Na2CO3), etc. The chelating agent may include, for example, ammonia water (e.g., NH3H2O), ammonium carbonate (e.g., NH3HCO3), etc.

[0085] The temperature of the above co-precipitation reaction can be controlled, for example, in the range of about 40°C to 60°C. The reaction time can be controlled in the range of about 24 to 72 hours.

[0086] The above lithium raw material may include, for example, lithium-containing carbonates (e.g., lithium carbonate, etc.), hydrates (e.g., lithium hydroxide I hydrate (LiOH·H2O)), hydroxides (e.g., lithium hydroxide, etc.), nitrates (e.g., lithium nitrate (LiNO3)), chlorides (e.g., lithium chloride (LiCl)), etc. These may be used alone or in combination of two or more.

[0087] According to exemplary embodiments, the lithium-nickel metal oxide may be manufactured by a method of manufacturing a mixture including a transition metal precursor and a lithium raw material, followed by a first firing. The mixture may further include a raw material including a doping metal element or an auxiliary metal element.

[0088] The raw material containing the above doping metal element or auxiliary metal element is Al2O3, TiO2, Ti2O3, ZrO2, B2O3, SrO2, SrAl2O4, SrTiO3, SrWO4, BaO, WO3, (NH4)0H2(W2O7)6, MgO, Ta2O5, Nb2O5, MoO3, H4[W12SiO 40 ], H4SiO4·12MoO3 and (NH4)2MoO4. In this case, the metal oxide is sufficiently converted into a metal hydroxide, so that a secondary battery having excellent life characteristics and low resistance can be realized.

[0089] The above first firing can be performed at a temperature of about 600°C to 1000°C for about 5 to 15 hours, and can be performed in an oxygen atmosphere.

[0090] Next, a coating layer can be formed on the surface of the lithium-nickel metal oxide particles. During the process of forming the coating layer, residual lithium can be removed.

[0091] According to an exemplary embodiment, a preliminary coating can be formed on the surface of the lithium-nickel metal oxide particles. The preliminary coating can be formed by dry mixing the lithium-nickel metal oxide particles with a metal-containing raw material for preliminary coating.

[0092] The metal-containing raw material for the pre-coating may include an oxide of the metal for the pre-coating. For example, the metal-containing raw material for the pre-coating may include aluminum oxide, tungsten oxide, etc., and preferably tungsten oxide. In exemplary embodiments, when the metal-containing raw material for the pre-coating includes tungsten oxide, excellent low resistance and rapid lifespan can be improved.

[0093] The above metal-containing raw material for preliminary coating can be used in an amount of 0.001 mol to 0.01 mol per 1 mol of the lithium-nickel metal oxide.

[0094] Next, the lithium-nickel metal oxide particles having a pre-coated surface can be treated with an aqueous solution to remove residual lithium. The aqueous solution may contain a compound capable of reacting with lithium compounds, such as lithium carbonate, remaining on the lithium-nickel metal oxide.

[0095] To improve the yield of lithium-nickel metal oxide particles or ensure the stability of the synthesis process, a lithium precursor (lithium salt) may be used in excess. In this case, a lithium precursor including lithium hydroxide (LiOH) and / or lithium carbonate (Li2CO3) may remain on the surface of the lithium-nickel metal oxide particles.

[0096] Additionally, as the Ni content of the lithium-nickel metal oxide increases, the first sintering can be performed at a lower temperature. In this case, the residual lithium content on the surface of the lithium-nickel metal oxide particles can increase.

[0097] The residual lithium can be removed by washing the lithium-nickel metal oxide with water in a substantially equal amount (water washing treatment). However, in this case, the surface of the lithium-nickel metal oxide particles may be oxidized, and a side reaction of the lithium-nickel metal oxide with water may occur, resulting in damage or collapse of the layered structure of the particles.

[0098] In addition, when the layered structure is transformed into a face-centered cubic structure, spinel structure, and / or rock salt structure instead of a hexagonal close-packed structure by water, the lithium-nickel metal oxide may be hydrolyzed to generate nickel impurities such as NiO or Ni(OH)2. In this case, the transformed structures are irreversibly transformed and may hinder lithium movement during battery charging and discharging. Accordingly, the initial capacity and capacity retention rate of the secondary battery may decrease.

[0099] According to exemplary embodiments, the aqueous solution treatment can implement passivation by a compound for removing residual lithium on the surface of lithium-nickel metal oxide particles, thereby securing the initial capacity of the battery and preventing a significant decrease in capacity even when repeating charge and discharge. In exemplary embodiments, the aqueous solution can include an aqueous solvent and a compound for removing residual lithium. The aqueous solvent can include deionized water, and the compound for removing residual lithium can include a sulfur-containing compound, a phosphorus-containing compound, or the like.

[0100] For example, the sulfur-containing compound may include a sulfonyl compound, and may include at least one selected from the group consisting of (NH4)2SO4, SO3NH3, NH4SO3NH2, Al2(SO4)3, AlK(SO4)2, AlNH4(SO4)2, Ti(SO4)2, TiOSO4, SrSO4, KHSO4, NaHSO4, and KHSO4.

[0101] For example, the phosphorus-containing compound may include a phosphate compound, for example, NH4H2PO4, (NH4)2HPO4, (NH4)3PO4, Mg3(PO4)2, AlPO4, Co3(PO4)2, (C2H5O)2P(O)H, (C4H9O)2P(O)OH, Ni3(PO4)2, NaNH4HPO4, (NH4)MgPO4(6H2O), Na2H2P2O7, Na4P2O7, and (NaPO3) n (n>0) may include at least one selected from.

[0102] The content of the compound for removing residual lithium in the above aqueous solution may be 5 to 30 parts by weight or 10 to 15 parts by weight per 100 parts by weight of the aqueous solvent.

[0103] The lithium-nickel metal oxide particles having the above dry coating formed can be mixed with the above aqueous solution to prepare a mixture. The mixture can contain 2 to 20 parts by weight of an aqueous solvent based on 100 parts by weight of the lithium-nickel metal oxide particles having the above pre-coating formed. In this case, a lithium-sulfur compound can be sufficiently formed at locations where residual lithium existed on the surface and inside of the lithium-nickel metal oxide particles, while substantially preventing damage or collapse of the layered structure of the primary particles, as in the case of a water-washing treatment.

[0104] In some embodiments, the mixture may include 0.5 to 1.8 parts by weight of a residual lithium removal compound relative to 100 parts by weight of the lithium-nickel metal oxide particles having the pre-coated particles. In this case, a sufficient amount of the residual lithium removal compound can react with the residual lithium to form, for example, a lithium-sulfur compound, while preventing the sulfur content in the positive electrode active material from becoming excessively high. Accordingly, the battery's lifespan characteristics can be improved while maintaining its output characteristics.

[0105] Next, the mixture may be subjected to a second firing to produce a first cathode active material. During the second firing process, the metal included in the pre-coating and the residual lithium removal compound included in the aqueous solution may react with the residual lithium to form a coating layer on the surface of the lithium-nickel metal oxide particles. For example, when the mixture includes a sulfur-containing compound, the sulfur-containing compound may react with the residual lithium present on the surface of the lithium-nickel metal oxide particles to be converted into a lithium-sulfur compound. Accordingly, the residual lithium may be removed, thereby improving the lifespan characteristics of the secondary battery.

[0106] For example, sulfur-containing compounds can react with residual lithium and moisture, converting some of the metal oxides contained in the pre-coating into metal hydroxides with stronger bonding energies. This can improve the high-temperature lifespan and stability of secondary batteries.

[0107] In some embodiments, when the compound for removing residual lithium includes a sulfur-containing compound, some of the sulfur-containing compound may react with residual lithium present on the surface of the lithium-nickel metal oxide particles to convert into a lithium-sulfur compound, and the remainder may convert the metal oxide included in the pre-coating into a metal hydroxide. Accordingly, a coating including the lithium-sulfur-containing compound and the hydroxide of the metal included in the pre-coating may be formed on the surface of the lithium-nickel metal oxide particles.

[0108] In addition, since no water washing treatment is performed, for example, the lithium-nickel metal oxide particles may not include primary particles of a face-centered cubic structure, and residual lithium can be effectively removed while preventing oxidation and layered structure damage due to water on the particle surface.

[0109] In exemplary embodiments, the second firing may be performed at a temperature of about 250° C. to 550° C. for about 5 to 15 hours. In this case, the metal oxide of the preliminary coating may be sufficiently converted into a metal hydroxide to form a coating while sufficiently removing residual lithium.

[0110] Additionally, performing firing within the above temperature range can prevent excessively high temperatures from causing the metal hydroxide to be converted back into a metal oxide. Consequently, the battery's lifespan and capacity characteristics can be improved.

[0111] According to exemplary embodiments, the positive electrode active material layer may further include a positive electrode active material different from the first positive electrode active material.

[0112] According to exemplary embodiments, the positive electrode active material layer may include lithium-nickel metal oxide particles having a secondary particle structure in which a plurality of primary particles are aggregated, and a second positive electrode active material that does not include the coating layer. For example, the second positive electrode active material may be manufactured by manufacturing the lithium-nickel metal oxide particles and then washing them with water.

[0113] The lithium-nickel metal oxide particles of the second positive electrode active material have a secondary particle structure and may have a single-crystalline or polycrystalline particle structure.

[0114] In exemplary embodiments, within a region from the surface of the primary particle of the second positive electrode active material to a depth of 10 nm to 30 nm, there may exist a region in which the content of the layered structure is less than the sum of the contents of the cubic phase structure and the spinel structure. For example, when the crystal structure of the primary particle of the second positive electrode active material is confirmed by transmission electron microscopy (TEM) and selected area electron diffraction (SAED) analysis, there may exist a region in which the content of the layered structure is less than the sum of the contents of the cubic phase structure and the spinel structure within a region from the surface of the primary particle to a depth of 10 nm or 20 nm.

[0115] For example, in a region of a depth of 3 nm, 4 nm, 5 nm, or 10 nm from the surface of the primary particle of the second positive electrode active material, the content of the layered structure may be less than the sum of the contents of the cubic structure and the spinel structure.

[0116] According to exemplary embodiments, the positive electrode active material layer may include a third positive electrode active material including single-crystalline lithium-nickel metal oxide particles without the coating layer. The third positive electrode active material may have relatively large crystal grain sizes, and thus, the number of crystal grains contained in one particle may be small.

[0117] The crystal grain size of the lithium-nickel metal oxide particles of the third positive electrode active material is about 250 nm to 1000 nm, and can be obtained by calculating it using the Scherrer equation (Equation 1 below) using the full width at half maximum (FWHM) obtained through XRD analysis.

[0118] [Formula 1]

[0119]

[0120] In Equation 1, L is the grain size, λ is the X-ray wavelength, β is the half width of the peak on the (003) plane, and θ is the diffraction angle.

[0121] In exemplary embodiments, the XRD analysis can be performed on dried powder of lithium-nickel metal oxide particles using Cu Kα rays as a diffraction light source, at a diffraction angle (2θ) range of 10° to 120°, at a scan rate of 0.0065° / s.

[0122] In some embodiments, β in Equation 1 above may be a half-width corrected for the equipment-derived value. In one embodiment, Si may be used as a standard material to reflect the equipment-derived value. In this case, a value corrected by subtracting the half-width of the peak of the (220) plane of Si may be used as β.

[0123] When the content of Ni in the particles increases, the mechanical strength and chemical stability of the positive electrode active material may deteriorate, and for example, particle cracks may occur during the pressing process for forming the positive electrode active material layer (110). Accordingly, the electrolyte may penetrate into the particles, causing gas generation due to a side reaction.

[0124] In addition, as charge and discharge are repeated, the volume of the positive electrode active material undergoes repeated shrinkage / expansion, and thus, particle cracks may become more severe in the case of high-Ni positive electrode active materials.

[0125] When the crystal grain size is within the above range, the strength of the third positive electrode active material can be increased, and the inter-crystal grain or inter-particle boundary area can be reduced, thereby reducing particle cracks.

[0126] Therefore, gas generation resulting from repeated charge / discharge cycles can be suppressed, and cracking due to volume shrinkage / expansion can be reduced. Therefore, stable capacity characteristics can be achieved even in high-temperature environments, and the lifespan characteristics of lithium secondary batteries can be improved.

[0127] The second positive electrode active material and the third positive electrode active material may not include the coating layer. In some embodiments, the second positive electrode active material and the third positive electrode active material may not include the coating layer included in the first positive electrode active material, and may include a coating layer that is not identical to the coating layer included in the first positive electrode active material.

[0128] According to some embodiments, the second positive electrode active material and the third positive electrode active material may not be identical to each other. Furthermore, the second positive electrode active material and the third positive electrode active material may not be identical to each other as the first positive electrode active material. "Not identical" may mean that at least one of the following properties is different: the composition of the lithium-nickel metal oxide, the size of the crystal grains, the structure of the primary particle agglomeration, the size of the primary particles and the secondary particles, whether a coating layer is included, and the composition of the coating layer. The "same" may mean substantially the same within a range including a general measurement error.

[0129] For example, when the first positive electrode active material includes a lithium-sulfur compound and a lithium-aluminum compound, the second positive electrode active material may include a coating layer including a lithium-aluminum compound, and the second positive electrode active material may not be identical to the first positive electrode active material.

[0130] In exemplary embodiments, when the positive electrode active material layer includes the second positive electrode active material, the content of the second positive electrode active material may be 10 wt% to 50 wt% of the total weight of the positive electrode active material layer. In some embodiments, the content of the second positive electrode active material may be 15 wt% to 35 wt% or 20 wt% to 30 wt% of the total weight of the positive electrode active material layer.

[0131] In exemplary embodiments, when the positive electrode active material layer includes the third positive electrode active material, the content of the third positive electrode active material may be 10 wt% to 50 wt% of the total weight of the positive electrode active material layer. In some embodiments, the content of the third positive electrode active material may be 15 wt% to 35 wt% or 20 wt% to 30 wt% of the total weight of the positive electrode active material layer.

[0132] Within the above range, when the first positive electrode active material, the second positive electrode active material and / or the third positive electrode active material are used together, the high-temperature life characteristics of the improved lithium secondary battery can be further improved.

[0133] According to exemplary embodiments, the positive electrode active material layer (110) may further include a binder, a conductive agent, a dispersant, etc.

[0134] For example, the positive electrode (100) can be manufactured by mixing and stirring a positive electrode active material, a binder, a conductive agent, a dispersion medium, etc. to prepare a positive electrode slurry, then applying the positive electrode slurry onto a positive electrode current collector (105), drying the dispersion medium, and then rolling.

[0135] The above binder may include an organic binder such as polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyacrylonitrile, polymethylmethacrylate, and an aqueous binder such as styrene-butadiene rubber (SBR).

[0136] The above conductive material may include a carbon-based conductive material such as graphite, carbon black, graphene, carbon nanotubes, etc.; a metal-based conductive material such as perovskite materials such as tin, tin oxide, titanium oxide, LaSrCoO3, LaSrMnO3, etc.

[0137] For example, the positive electrode collector (105) may include stainless steel, nickel, aluminum, titanium, copper, or an alloy thereof.

[0138] According to exemplary embodiments, the positive electrode active material layer (110) may include a first positive electrode active material layer and a second positive electrode active material layer sequentially laminated on at least one surface of the positive electrode current collector (not shown). The first positive electrode active material layer and the second positive electrode active material layer may each include a positive electrode active material, a binder, a conductive material, etc. At least one of the type and content of each component included in the first positive electrode active material layer and the second positive electrode active material layer may be different from each other.

[0139] According to some embodiments, the first positive electrode active material layer and the second positive electrode active material layer may each independently include at least one positive electrode active material selected from the group consisting of the first positive electrode active material, the second positive electrode active material, and the third positive electrode active material. In this case, at least one of the type and content of the positive electrode active material included in the first positive electrode active material layer and the second positive electrode active material layer may be different from each other.

[0140] For example, the first positive electrode active material layer may include a first positive electrode active material, and the second positive electrode active material layer may include a second positive electrode active material. Alternatively, the first positive electrode active material layer and the second positive electrode active material layer may include a first positive electrode active material, and the content of the first positive electrode active material included in each layer may be different.

[0141] In some embodiments, the content of the binder in the total weight of the first positive electrode active material layer may be greater than or equal to the content of the binder in the total weight of the second positive electrode active material layer. For example, the content of the binder in the first positive electrode active material layer may be 0.9 wt% to 1.5 wt% of the total weight of the first positive electrode active material layer, and the content of the binder in the second positive electrode active material layer may be 0.1 wt% to 0.8 wt% of the total weight of the second positive electrode active material layer.

[0142] Accordingly, the first positive electrode active material layer adjacent to the positive electrode current collector (105) can be more firmly attached to the current collector, thereby securing the durability of the positive electrode, and the second positive electrode active material layer can have a relatively increased amount of positive electrode active material while reducing the content of the binder, thereby increasing the capacity of the battery.

[0143] According to exemplary embodiments, the first positive electrode active material layer and the second positive electrode active material layer may each independently include at least one of the first positive electrode active material and the second positive electrode active material. However, at least one of the first positive electrode active material layer and the second positive electrode active material layer may include the first positive electrode active material.

[0144] For example, the first positive electrode active material layer may include a first positive electrode active material, and the second positive electrode active material layer may include a second positive electrode active material.

[0145] According to exemplary embodiments, the total weight of the first positive electrode active material layer and the second positive electrode active material layer may refer to the total weight of the positive electrode active material layers. For example, when the thicknesses of the first positive electrode active material layer and the second positive electrode active material layer are the same and the content of the first positive electrode active material in the first positive electrode active material layer is about 90 wt% and the content of the first positive electrode active material in the second positive electrode active material layer is about 40 wt%, the content of the first positive electrode active material in the total weight of the positive electrode active material layers may be calculated to be about 65 wt%.

[0146] According to exemplary embodiments, the ratio of the content of the first positive electrode active material to the content of the second positive electrode active material with respect to the total weight of the positive electrode active material layer may be 1 to 4. In some embodiments, the ratio of the content of the first positive electrode active material to the content of the second positive electrode active material with respect to the total weight of the positive electrode active material layer may be 1 to 2.5.

[0147] Within the above range, the positive electrode active material layer can improve the high-temperature characteristics of the battery by including a higher content of the first positive electrode active material, which is more stable at high temperatures, than the second positive electrode active material.

[0148] According to exemplary embodiments, the negative electrode (130) may include a negative electrode active material layer (120) on at least one surface of the negative electrode current collector (125). The negative electrode active material layer (120) may include a negative electrode active material. For example, the negative electrode active material may include a material capable of absorbing and desorbing lithium ions.

[0149] In exemplary embodiments, the negative electrode active material may include a silicon-based active material. The silicon-based active material may be incorporated into the negative electrode active material layer to enhance the capacity and lifespan characteristics of the negative electrode. Accordingly, the lifespan characteristics of the battery, particularly the capacity retention characteristics during rapid charge / discharge, may be improved.

[0150] For example, the silicon-based active material may include silicon, silicon alloy, silicon oxide, metal-doped silicon oxide, silicon carbide, silicon-carbon composite (Si-C), silicon-containing core-shell structured particles, etc. These may be used alone or in combination of two or more.

[0151] In exemplary embodiments, the silicon-based active material may include a doping metal. For example, the doping metal may include at least one of Li, Mg, Al, Ca, Fe, Ti, and V, and may be doped in a form that substitutes for a silicon site in the silicon-based active material.

[0152] According to exemplary embodiments, the content of the silicon-based active material may be 5 wt% to 30 wt% of the total weight of the negative electrode active material layer. According to some embodiments, the content of the silicon-based active material may be 10 wt% to 20 wt% or 10 wt% to 15 wt% of the total weight of the negative electrode active material layer.

[0153] Within the above range, the battery characteristics can be maintained similar to the initial state when the battery is charged and discharged under harsh conditions (high temperature environment, ultra-fast charging, etc.) without deteriorating the long-term durability of the negative electrode.

[0154] In addition to silicon-based active materials, the above-mentioned negative electrode active material may further include materials known in the art capable of absorbing and desorbing lithium ions. For example, carbon-based materials such as crystalline carbon, amorphous carbon, carbon composites, and carbon fibers; lithium alloys; and the like may be used.

[0155] Examples of the above amorphous carbon include hard carbon, coke, mesocarbon microbeads (MCMB) calcined at 1500°C or lower, and mesophase pitch-based carbon fibers (MPCF).

[0156] Examples of the above crystalline carbon include graphite-based carbons such as artificial graphite, natural graphite, graphitized coke, graphitized MCMB, and graphitized MPCF.

[0157] Elements included in the above lithium alloy include aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium, or indium.

[0158] Preferably, the negative active material may further include artificial graphite.

[0159] According to exemplary embodiments, the negative active material layer (120) may further include a binder, a conductive agent, a dispersant, etc.

[0160] For example, the negative electrode (130) can be manufactured by mixing and stirring a negative electrode active material, a binder, a conductive agent, a dispersion medium, etc. to prepare a negative electrode slurry, then applying the negative electrode slurry onto a negative electrode current collector (125), drying the dispersion medium, and then rolling.

[0161] Materials substantially identical or similar to those described above for the positive electrode may be used as the binder and conductive material. In some embodiments, the binder for forming the negative electrode may include, for example, an aqueous binder such as styrene-butadiene rubber (SBR) for compatibility with the carbon-based active material, and may be used together with a thickener such as carboxymethyl cellulose (CMC).

[0162] According to an exemplary embodiment, the negative electrode current collector (125) may include, for example, gold, stainless steel, nickel, aluminum, titanium, copper or an alloy thereof, and preferably may include copper or a copper alloy.

[0163] According to an exemplary embodiment, the negative electrode active material layer (120) may include a first negative electrode active material layer and a second negative electrode active material layer sequentially laminated on at least one surface of the negative electrode current collector (not shown). The first negative electrode active material layer and the second negative electrode active material layer may each include a negative electrode active material, a binder, a conductive material, etc. At least one of the type and content of each component included in the first negative electrode active material layer and the second negative electrode active material layer may be different from each other.

[0164] According to some embodiments, the weight-based content of the binder in the first negative electrode active material layer may be greater than or equal to the weight-based content of the binder in the second negative electrode active material layer. For example, the weight-based content of the binder in the first negative electrode active material layer may be 1.0 wt% to 5.0 wt% of the total weight of the first negative electrode active material layer, and the weight-based content of the binder in the second negative electrode active material layer may be 0.1 wt% to 1.0 wt% of the total weight of the second negative electrode active material layer.

[0165] Accordingly, the first negative electrode active material layer adjacent to the negative electrode current collector (125) can be more firmly attached to the current collector, thereby securing the durability of the negative electrode, and the second negative electrode active material layer can relatively increase the amount of the negative electrode active material while reducing the binder content, thereby increasing the capacity of the battery. In addition, the electrode pore resistance of the second negative electrode active material layer can be lowered, thereby improving the rapid performance.

[0166] According to an exemplary embodiment, the negative electrode may further include a primer layer (not shown) disposed between the negative electrode active material layer (120) and the negative electrode current collector (125) and including a binder. The primer layer is a layer that is relatively thinner than the negative electrode active material layer, may be substantially made of a binder, and may function as an adhesive layer that firmly attaches the negative electrode current collector (125) and the negative electrode active material layer (120). Accordingly, the amount of the negative electrode active material layer may be relatively increased while the content of the binder is reduced, thereby increasing the capacity of the battery. In addition, the electrode pore resistance of the second negative electrode active material layer may be lowered, thereby improving rapid performance.

[0167] In some embodiments, the area of ​​the negative electrode (130) may be larger than the area of ​​the positive electrode (100). In this case, lithium ions generated from the positive electrode (100) may smoothly move to the negative electrode (130) without being precipitated in the middle.

[0168] According to exemplary embodiments, a separator (140) may be interposed between the anode (100) and the cathode (130).

[0169] For example, the separator (140) may include a porous polymer film made of a polyolefin polymer, such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, an ethylene / methacrylate copolymer, etc. In addition, for example, the separator (140) may include a nonwoven fabric arranged with high-melting-point glass fibers, polyethylene terephthalate fibers, etc.

[0170] For example, an electrode cell can be configured including an anode (100), a cathode (130), and a separator (140).

[0171] For example, a plurality of electrode cells can be stacked to form an electrode assembly (150).

[0172] For example, an electrode assembly (150) can be formed by winding, lamination, z-folding, etc. of electrode cells including an anode (100), a cathode (130), and a separator (140).

[0173] A lithium secondary battery according to exemplary embodiments may include an electrolyte. For example, the electrode assembly (150) and the electrolyte described above may be housed together in a case (160) to form a lithium secondary battery.

[0174] According to exemplary embodiments, the electrolyte may be a non-aqueous electrolyte. The electrolyte may include a lithium salt as an electrolyte.

[0175] The above lithium salt is, for example, Li +X - is expressed as and the anion of the lithium salt (X - ) as F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - Examples include:

[0176] Examples of the organic solvent that can be used include propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethylmethyl carbonate (EMC), methylpropyl carbonate, dipropyl carbonate, dimethylsulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, sulfolane, gamma-butyrolactone, propylene sulfite, and tetrahydrofuran. These may be used alone or in combination of two or more.

[0177] According to exemplary embodiments, the electrolyte may further include an additive. The additive may further include dimethylsulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, sulfolane, gamma-butyrolactone, propylene sulfite, and tetrahydrofuran.

[0178] A lithium secondary battery according to exemplary embodiments may include an electrode lead (107, 127) connected to an electrode (100, 130) and protruding outward from a case (160).

[0179] For example, it may include a positive lead (107) connected to the positive electrode (100) and protruding outward from the case (160); and a negative lead (127) connected to the negative electrode (130) and protruding outward from the case (160).

[0180] For example, the positive electrode (100) and the positive electrode lead (107) may be electrically connected. Similarly, the negative electrode (130) and the negative electrode lead (127) may be electrically connected.

[0181] For example, the positive electrode lead (107) may be electrically connected to the positive electrode collector (105). Additionally, the negative electrode lead (127) may be electrically connected to the negative electrode collector (125).

[0182] The positive electrode current collector (105) of the positive electrode (100) and the negative electrode current collector (125) of the negative electrode (130) may each include a notching portion. The notching portion may be provided as an electrode tab, for example. The notching portion may include a positive electrode notching portion protruding from the positive electrode current collector (105) and a negative electrode notching portion protruding from the negative electrode current collector (125).

[0183] For example, the positive electrode current collector (105) may include a protrusion (positive electrode tab) on one side. The positive electrode active material layer (110) may not be arranged on the positive electrode tab. The positive electrode tab may be integral with the positive electrode current collector (105) or may be connected by welding or the like. The positive electrode current collector (105) and the positive electrode lead (107) may be electrically connected through the positive electrode tab.

[0184] The negative electrode current collector (125) may include a protrusion (negative electrode tab) on one side. The negative electrode active material layer (120) may not be arranged on the negative electrode tab. The negative electrode tab may be integral with the negative electrode collector (125) or may be connected by welding or the like. The negative electrode collector (125) and the negative electrode lead (127) may be electrically connected through the negative electrode tab.

[0185] In one embodiment, the electrode assembly (150) may include a plurality of positive electrodes and a plurality of negative electrodes. For example, the plurality of positive electrodes and the plurality of negative electrodes may be arranged alternately with each other, and a separator may be interposed between the positive electrodes and the negative electrodes. Accordingly, the lithium secondary battery according to one embodiment may include a plurality of positive electrode tabs and a plurality of negative electrode tabs protruding from each of the plurality of positive electrodes and the plurality of negative electrodes.

[0186] In one embodiment, the positive tabs (or negative tabs) can be laminated, pressed, and welded to form a positive tab laminate (or negative tab laminate). The positive tab laminate can be electrically connected to the positive lead (107). Additionally, the negative tab laminate can be electrically connected to the negative lead (127).

[0187] The above lithium secondary battery can be manufactured in, for example, a cylindrical shape, a square shape, a pouch shape, or a coin shape.

[0188] Hereinafter, embodiments of the present disclosure will be further described with reference to specific experimental examples. The examples and comparative examples included in the experimental examples are merely illustrative of the present disclosure and do not limit the scope of the appended claims. It will be apparent to those skilled in the art that various changes and modifications to the examples are possible within the scope and technical idea of ​​the present disclosure, and it is also natural that such changes and modifications fall within the scope of the appended claims.

[0189]

[0190] Synthesis Example 1-1

[0191] (1) Manufacturing of lithium-nickel metal oxide particles

[0192] NiSO4, CoSO4, and MnSO4 were mixed in a ratio (mol) of 0.55:0.12:0.33 using distilled water that had been bubbled with N2 for 24 hours to remove internal dissolved oxygen. The solution was put into a reactor at 50°C, and a coprecipitation reaction was performed for 48 hours using NaOH and NH3H2O ​​as precipitants and chelating agents to obtain Ni as a transition metal precursor. 0.55 Co 0.12 Mn 0.33 (OH)2 was obtained. The obtained precursor was dried at 80°C for 12 hours and then re-dried at 110°C for 12 hours.

[0193] Lithium hydroxide and the above transition metal precursor were added to a dry high-speed mixer at a ratio of 1.01:1 and mixed uniformly for 5 minutes.

[0194] The above mixture was placed in a kiln and heated to 730 to 750°C at a rate of 2°C / min, and maintained at 730 to 750°C for 10 hours. During the heating and maintenance, oxygen was continuously passed at a flow rate of 20 L / min. After the kiln was completed, natural cooling was performed to room temperature, and LiNi was produced through pulverization and classification. 0.55 Co 0.12 Mn 0.33 Lithium-nickel metal oxide particles having a composition of O2 and a secondary particle structure in which primary particles are aggregated were obtained.

[0195] (2) Formation of coating layer

[0196] The lithium-nickel metal oxide particles and Al2O3 powder prepared above were dry mixed to form a preliminary coating on the surface of the lithium-nickel metal oxide particles. At this time, the Al2O3 was added in an amount of 0.3 mol% relative to the total molar number of the lithium-nickel metal composite oxide particles.

[0197] Ammonium sulfate ((NH4)2SO4) powder was added at 1.2 wt% relative to the total weight of the lithium-nickel metal oxide particles to 10 wt% of pure water relative to the total weight of the above-mentioned pre-coated lithium-nickel metal oxide particles, and stirred to prepare a sulfur-containing compound aqueous solution.

[0198] The above-described sulfur-containing compound aqueous solution was added to and mixed with the above-described pre-coated lithium-nickel metal oxide particles to prepare a mixture. The prepared mixture was placed in a calcination furnace, and while supplying oxygen at a flow rate of 20 L / min, the temperature was increased to 400°C at a heating rate of 2°C / min, and maintained at the elevated temperature for 10 hours. After calcination, the first positive electrode active material was obtained by sieving through a 325 mesh.

[0199]

[0200] Synthesis Example 1-2

[0201] In Synthesis Example 1-1, a first positive electrode active material was obtained in the same manner as Synthesis Example 1, except that ammonium phosphate ((NH4)2HPO4) was used instead of ammonium sulfate.

[0202]

[0203] Synthesis Example 1-3

[0204] In Synthesis Example 1-1, a first positive electrode active material was obtained in the same manner as Synthesis Example 1, except that WO3 was used instead of Al2O3 as a metal oxide in the preliminary coating arrangement.

[0205]

[0206] Synthesis Example 2-1

[0207] In (1) of the above synthesis example 1, Ni is used as a transition metal precursor. 0.88 Co 0.06 Mn 0.06 LiNi was prepared in the same manner as (1) of Synthesis Example 1, except that (OH)2 was prepared. 0.88 Co 0.06 Mn 0.06 Lithium-nickel metal oxide particles of O2 were prepared.

[0208] The second positive electrode active material was obtained by washing and drying using water having a weight equal to the weight of the manufactured lithium-nickel metal oxide particles.

[0209]

[0210] Synthesis Example 3-1

[0211] In (1) of the above synthesis example 1, Ni is used as a transition metal precursor. 0.88 Co 0.06 Mn 0.06 (OH)2 was manufactured and calcined for 13 hours to obtain LiNi 0.88 Co 0.06 Mn 0.06 A third positive electrode active material was obtained in the same manner as (1) of Synthesis Example 1, except that lithium-nickel metal oxide particles of O2 were prepared.

[0212] For the third cathode active material, the crystal grain size calculated using Equation 1 described above through XRD analysis was approximately 300 nm. Detailed XRD analysis equipment and measurement conditions are as described in Table 1 below.

[0213] XRD (X-Ray Diffractometer) EmpyreanmakerPanalyticalanode MaterialCuk-Alpha 1 WAVELENGTH1.540598ågenerator Voltage45 kvtube current40 mascan Range10 ~ 120 ° SCAN STEP SIZE0.0065 ° DIVERGENCE Slit1 / 4 ° Antiscatter Slit1 / 2 °

[0214]

[0215] Experimental Example 1: Confirmation of the layered structure of the surface

[0216] To analyze the crystal phase of the primary particles of the second positive electrode active material manufactured in Synthesis Example 2-1, TEM-SAED (Transmission Electron Microscopy-Selected Area Electron Diffraction) analysis was performed. After FIB processing of the second positive electrode active material manufactured in Synthesis Example 2-1 to produce a specimen, a TEM was used to specify a selected area aperture for the cross-section, and then the diffraction image was acquired by entering diffraction mode.

[0217] Figures 3a to 3c show primary particle TEM-SAED images of the second positive electrode active material manufactured in Synthesis Example 2-1. Enlarged images of points 1 and 2 in Figure 3a are shown in Figures 3b and 3c, respectively.

[0218] Referring to Figures 3a to 3c, the SAED images showed a cubic phase, not a layered structure, at two locations close to the particle surface. Given that the cubic phase was observed at locations close to the surface, it can be inferred that, in the case of the second positive electrode active material of Synthesis Example 2-1, there is a greater area of ​​the cubic phase than the layered structure within a region approximately 20 nm deep from the primary particle surface.

[0219]

[0220] Experimental Example 2: Confirmation of the coating layer

[0221] To confirm the coating layer of the first positive electrode active material manufactured in Synthesis Example 1-1, TEM images were taken. The process was performed in the same manner as Experimental Example 1, and TEM images of the first positive electrode active material manufactured in Synthesis Example 1-1 are shown in FIGS. 4a and 4b. The magnification of FIG. 4b is higher than that of FIG. 4a.

[0222] For the indicated points 1 and 2 in Fig. 4a, they correspond to Li2SO4 and lithium-nickel metal oxide, respectively. That is, it can be confirmed that a coating layer containing Li2SO4 is arranged at the interface of the primary particles. Fig. 4b is a TEM image taken at a higher magnification of the surface of the primary particles, in which a coating layer containing Li2SO4 is provided on the surface of the lithium-nickel metal oxide (NCM) particles. In the first positive electrode active material of Synthesis Example 1-1, a coating layer containing Li2SO4 was formed on the surface of the primary particles, i.e., at the interface of the primary particles inside the secondary particles.

[0223] In addition, an SEM image of a particle cross-section of the first positive electrode active material manufactured in Synthesis Example 1-3 was taken, and an EDS element mapping image was obtained to confirm the element distribution for the cross-section.

[0224] Fig. 5a shows a cross-sectional SEM image of the first positive electrode active material manufactured in Synthesis Example 1-3, and Figs. 5b and 5c show EDS element mapping images of sulfur and tungsten elements, respectively, for the image of Fig. 5a.

[0225] Referring to FIGS. 5a to 5c, a coating layer was formed on the outer surface of the particles of the first positive electrode active material manufactured in Synthesis Example 1-3, and it was observed that sulfur element was included in the coating layer and that some sulfur element was also distributed at the interface of the primary particles inside the secondary particles. In addition, tungsten element appears to be distributed both inside and outside the particles, indicating that a tungsten and sulfur-containing coating layer was formed at the interface of the primary particles inside the secondary particles.

[0226]

[0227] Experimental Example 3: Surface Resistance Measurement and Evaluation

[0228] The positive electrode active materials manufactured in Synthesis Examples 1-1 and 1-3 were mixed with a binder (PVDF) and coated on Al foil to produce an electrode. In order to analyze the inherent conductivity of the positive electrode active material and to exclude the effect of enhancing conductivity by a conductive agent, the electrode was manufactured by mixing only a minimum amount (1 wt%) of binder, unlike the components of general electrodes.

[0229] For the cut cross-section of the above electrode, analysis was conducted in SSRM mode using AFM to confirm the electrical resistance distribution.

[0230] Specifically, the electrode was cut, and a tip coated with a conductive material (contact area radius of 30 nm) was contacted using Bruker's AFM over a 200 nm x 200 nm area of ​​the cross-section, and a voltage of 3 V was applied to perform analysis in SSRM mode to obtain a diffusion resistance distribution image.

[0231] Figures 6a to 6d show SSRM diffusion resistance distribution images of electrodes including the first positive active material of Synthesis Example 1-3 and Synthesis Example 1-1. Figure 6a is an SSRM image of an electrode including the first positive active material of Synthesis Example 1-3, Figure 6b is a high-magnification SSRM image of an electrode including the first positive active material of Synthesis Example 1-3, Figure 6c is an SSRM image of an electrode including the first positive active material of Synthesis Example 1-1, and Figure 6d is an SSRM image of an electrode including the first positive active material of Synthesis Example 1-1.

[0232] Referring to FIGS. 6a to 6d, it can be seen that the internal resistance of the positive electrode active material is lowered because the first positive electrode active material includes a tungsten-containing coating layer.

[0233]

[0234] Example 1

[0235] A slurry was prepared by adding N-methyl pyrrolidone (NMP) to a mixture containing 98.08 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1, 0.72 wt% of MWCNT (including 20 wt% of a CNT dispersing agent) as a conductive agent, and 1.2 wt% of polyvinylidene fluoride (PVdF) as a binder, which was then uniformly applied to a 12 ㎛ thick aluminum foil, dried, and rolled to a density of 3.6 g / cc to manufacture a positive electrode for a secondary battery.

[0236] Artificial graphite (D50: 17 ㎛) 81.45 wt%, SiO as silicon-based active material x (0 <x<2) 15 중량%, 도전재로 SWCNT(CNT 분산용 제제 60 중량% 포함) 0.25 중량%, 증점제로 CMC 1.3 중량%, 바인더로 SBR 2 중량%, (고형분 총 합 100 중량%)를 포함하는 혼합물에 물을 첨가하여 음극 슬러리를 제조하였다. 구리 집전체(8 ㎛ 두께의 구리박)의 일 면 상에 상기 제조된 음극 슬러리를 코팅, 건조 및 1.6g / cc 밀도로 압연한 음극 활물질층을 형성하여 음극을 제조하였다.

[0237] The positive and negative electrodes were notched to a predetermined size, stacked, and a separator (polyethylene, 13 μm thick) was interposed between the positive and negative electrodes to form an electrode cell. The tab portions of the positive and negative electrodes were then welded. The welded positive / separator / negative electrode assembly was placed in a pouch and sealed on three sides except for the electrolyte injection side. At this time, the part with the electrode tab was included in the sealing part. The electrolyte was injected through the electrolyte injection side, and the remaining sides were sealed, and then impregnated for more than 12 hours.

[0238] The electrolyte was prepared by dissolving 1.1 M LiPF6 in a mixed solvent of ethyl carbonate, ethyl methyl carbonate, and ethyl acetate (EC / EMC=25 / 75, volume ratio), to which 7 wt% of fluoroethylene carbonate (FEC), 0.5 wt% of 1,3-propene sultone (PRS), 0.5 wt% of 1,3-propane sultone (PS), and 0.5 wt% of ethylene sulfate (ESA) were added.

[0239] Afterwards, Heat Press Pre-charging was performed for 60 minutes at an average current of 0.5C. After stabilization for more than 12 hours, degassing was performed and aging was performed for more than 24 hours, followed by Mars charge / discharge (charge condition CC-CV 0.25C 4.2V 0.05C CUT-OFF, discharge condition CC 0.25C 2.5V CUTOFF).

[0240] Afterwards, standard charge / discharge was performed (charge condition CC-CV 0.33 C 4.2V 0.05C CUT-OFF, discharge condition CC 0.33C 2.5V CUT-OFF).

[0241]

[0242] Example 2

[0243] A lithium secondary battery sample was manufactured in the same manner as Example 1, except that the first positive electrode active material manufactured in Synthesis Example 1-2 was used instead of the first positive electrode active material manufactured in Synthesis Example 1-1.

[0244]

[0245] Example 3

[0246] A lithium secondary battery sample was manufactured in the same manner as Example 1, except that the first positive electrode active material manufactured in Synthesis Example 1-3 was used instead of the first positive electrode active material manufactured in Synthesis Example 1-1.

[0247]

[0248] Example 4

[0249] A lithium secondary battery sample was manufactured in the same manner as Example 1, except that 68.656 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1 and 29.424 wt% of the second positive electrode active material manufactured in Synthesis Example 2-1 were used instead of 98.08 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1.

[0250]

[0251] Example 5

[0252] A lithium secondary battery sample was manufactured in the same manner as Example 1, except that 68.656 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1 and 29.424 wt% of the third positive electrode active material manufactured in Synthesis Example 3-1 were used instead of 98.08 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1.

[0253]

[0254] Example 6

[0255] A slurry for a first positive electrode active material layer was prepared by adding N-methyl pyrrolidone (NMP) to a mixture containing 98.08 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1, 0.72 wt% of MWCNT (including 20 wt% of a CNT dispersing agent) as a conductive agent, and 1.2 wt% of polyvinylidene fluoride (PVdF) as a binder.

[0256] A slurry for a second positive electrode active material layer was prepared by adding N-methyl pyrrolidone (NMP) to a mixture containing 98.68 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1, 0.72 wt% of MWCNT (including 20 wt% of a CNT dispersing agent) as a conductive material, and 0.6 wt% of polyvinylidene fluoride (PVdF) as a binder.

[0257] Using a slot die concept coating facility equipped with a dual shim consisting of upper and lower layers, the slurry for the first positive electrode active material layer and the slurry for the second positive electrode active material layer were uniformly applied at the same weight ratio on one side of a 12 μm thick aluminum foil, dried, and then rolled to a density of 3.6 g / cc to manufacture a positive electrode for a secondary battery. At this time, the slurry for the first positive electrode active material layer formed a first positive electrode active material layer in direct contact with the aluminum foil, and the slurry for the second positive electrode active material layer formed a second positive electrode active material layer on the first positive electrode active material layer.

[0258] A lithium secondary battery sample was manufactured in the same manner as in Example 1, except that the positive electrode was manufactured as described above.

[0259] At this time, the content of the first positive electrode active material manufactured in Synthesis Example 1-1 among the total weight of the first positive electrode active material layer and the second positive electrode active material layer was 98.38 wt%.

[0260]

[0261] Example 7

[0262] A slurry for a first positive electrode active material layer was prepared by adding N-methyl pyrrolidone (NMP) to a mixture containing 69.656 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1, 29.424 wt% of the third positive electrode active material manufactured in Synthesis Example 3-1, 0.72 wt% of MWCNT (including 20 wt% of a CNT dispersing agent) as a conductive agent, and 1.2 wt% of polyvinylidene fluoride (PVdF) as a binder.

[0263] A slurry for a second positive electrode active material layer was prepared by adding N-methyl pyrrolidone (NMP) to a mixture containing 69.076 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1, 29.604 wt% of the third positive electrode active material manufactured in Synthesis Example 3-1, 0.72 wt% of MWCNT (including 20 wt% of a CNT dispersing agent) as a conductive agent, and 0.6 wt% of polyvinylidene fluoride (PVdF) as a binder.

[0264] A lithium secondary battery sample was prepared in the same manner as in Example 6, except that the slurries were prepared as described above.

[0265] At this time, the content of the first positive electrode active material manufactured in Synthesis Example 1-1 among the total weight of the first positive electrode active material layer and the second positive electrode active material layer was 68.866 wt%.

[0266]

[0267] Example 8

[0268] A slurry for a first positive electrode active material layer was prepared by adding N-methyl pyrrolidone (NMP) to a mixture containing 39.232 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1, 58.848 wt% of the third positive electrode active material manufactured in Synthesis Example 3-1, 0.72 wt% of MWCNT (including 20 wt% of a CNT dispersing agent) as a conductive agent, and 1.2 wt% of polyvinylidene fluoride (PVdF) as a binder.

[0269] A slurry for a second positive electrode active material layer was prepared by adding N-methyl pyrrolidone (NMP) to a mixture containing 98.68 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1, 0.72 wt% of MWCNT (including 20 wt% of a CNT dispersing agent) as a conductive material, and 0.6 wt% of polyvinylidene fluoride (PVdF) as a binder.

[0270] A lithium secondary battery sample was prepared in the same manner as in Example 6, except that the slurries were prepared as described above.

[0271] At this time, the content of the first positive electrode active material manufactured in Synthesis Example 1-1 among the total weight of the first positive electrode active material layer and the second positive electrode active material layer was 68.956 wt%.

[0272]

[0273] Example 9

[0274] 80.45 wt% artificial graphite, SiO as silicon-based active material x (0 <x<2) 15 중량%, 도전재로 SWCNT(CNT 분산용 제제 60 중량% 포함) 0.25 중량%, 증점제로 CMC 1.3 중량%, 바인더로 SBR 3 중량%를 포함하는 혼합물에 물을 첨가하여 제1 음극 활물질층용 음극 슬러리를 제조하였다.

[0275] 82.45 wt% artificial graphite, SiO as silicon-based active material x (0 <x<2) 15 중량%, 도전재로 SWCNT(CNT 분산용 제제 60 중량% 포함) 0.25 중량%, 증점제로 CMC 1.3 중량%, 바인더로 SBR 1 중량%를 포함하는 혼합물에 물을 첨가하여 제2 음극 활물질층용 음극 슬러리를 제조하였다.

[0276] Using a slot die concept coating facility equipped with a dual shim consisting of upper and lower layers, the slurry for the first negative electrode active material layer and the slurry for the second negative electrode active material layer were coated on one side of a copper current collector (8 μm thick copper foil) at the same weight ratio, dried, and rolled to a density of 1.6 g / cc to manufacture an anode for a lithium secondary battery. At this time, a first negative electrode active material layer in direct contact with the aluminum foil was formed using the slurry for the first negative electrode active material layer, and a second negative electrode active material layer was formed on the first negative electrode active material layer using the slurry for the second negative electrode active material layer.

[0277] A lithium secondary battery sample was manufactured in the same manner as in Example 1, except that the negative electrode was manufactured as described above.

[0278]

[0279] Example 10

[0280] An SBR aqueous solution was applied to one side of a copper current collector (8 ㎛ thick copper foil) and dried to form a primer layer.

[0281] Artificial graphite (D50: 17 ㎛) 81.45 wt%, SiO as silicon-based active material x (0 <x<2) 15 중량%, 도전재로 SWCNT(CNT 분산용 제제 60 중량% 포함) 0.25 중량%, 증점제로 CMC 1.3 중량%, 바인더로 SBR 2 중량%, (고형분 총 합 100 중량%)를 포함하는 혼합물에 물을 첨가하여 음극 슬러리를 제조하였다.

[0282] The negative electrode slurry prepared above was coated on the primer layer, dried, and rolled to a density of 1.6 g / cc to form a negative electrode active material layer, thereby preparing a negative electrode.

[0283] A lithium secondary battery sample was manufactured in the same manner as in Example 1, except that the negative electrode was manufactured as described above.

[0284] At this time, the weight of the primer layer was 1.5 parts by weight with respect to 100 parts by weight of the negative electrode active material layer.

[0285]

[0286] Example 11

[0287] A lithium secondary battery sample was manufactured in the same manner as Example 1, except that 39.232 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1 and 58.848 wt% of the second positive electrode active material manufactured in Synthesis Example 2-1 were used instead of 98.08 wt% of the first positive electrode active material manufactured in Synthesis Example 1-1.

[0288]

[0289] Comparative Example 1

[0290] A lithium secondary battery sample was manufactured in the same manner as Example 1, except that the second positive electrode active material manufactured in Synthesis Example 2-1 was used instead of the first positive electrode active material manufactured in Synthesis Example 1-1.

[0291]

[0292] Comparative Example 2

[0293] A lithium secondary battery sample was manufactured in the same manner as Example 1, except that a silicon-based active material was not used in the manufacture of the negative electrode slurry, artificial graphite was used at 93.7 wt%, and a carbon-based conductive material was used at 3.0 wt% instead of 0.1 wt% of SWCNT as the conductive material.

[0294]

[0295] Comparative Example 3

[0296] A lithium secondary battery sample was manufactured in the same manner as Example 1, except that the second positive electrode active material manufactured in Synthesis Example 2-1 was used instead of the first positive electrode active material manufactured in Synthesis Example 1-1, the silicon-based active material was not used when manufacturing the negative electrode slurry, artificial graphite was used at 93.7 wt%, and a carbon-based conductive material was used at 3.0 wt% instead of 0.1 wt% of SWCNT as the conductive material.

[0297]

[0298] The contents and / or types of active materials, binders, and conductive agents in each of the positive electrode active material layer and negative electrode active material layer of Examples 1 to 11 and Comparative Examples 1 to 3 are shown in Table 2 below. When types are also indicated, the contents are indicated in parentheses, and the unit is weight%. In addition, in Examples 6 to 10, the composition of the first active material layer of the multilayer structure is described below, and the composition of the second active material layer is described above.

[0299] Positive active material layer Negative active material layer Positive active material Binder Artificial graphite Silicon-based active material Binder Conductive material Example 1A-1 (98.08) 1.28 1.45 152 D-1 (0.1) Example 2A-2 (98.08) 1.28 1.45 152 D-1 (0.1) Example 3A-3 (98.08) 1.28 1.45 152 D-1 (0.1) Example 4A-1 (68.656) B-1 (29.424) 1.28 1.45 152 D-1 (0.1) Example 5A-1 (68.656) C-1 (29.424) 1.28 1.45 152 D-1 (0.1) Example 6A-1(98.68)0.681.45152D-1 (0.1)A-1(98.08)1.2Example 7A-1(69.076)C-1(29.604)0.681.45152D-1 (0.1)A-1(68.656)C-1(29.424)1.2Example 8A-1(98.68)0.681.45152D-1 (0.1)A-1(39.232)C-1(58.848)1.2Example 9A-1(98.08)1.282.45151D-1 (0.1)80.45153D-1 (0.1)Example 10A-1(98.08)1.281.45150.5D-1 (0.1)--1.5*-Example 11A-1(39.232)B-1(58.848)1.281.45152D-1 (0.1)Comparative Example 1B-1(98.08)1.281.45152D-1(0.1)Comparative Example 2A-1(98.08)1.293.7-2D-23.0Comparative Example 3B-1(98.08)1.281.45-2D-23.0

[0300] *In the case of Example 10, the unit of content of the binder as a primer layer is parts by weight relative to 100 parts by weight of the negative electrode active material layer.

[0301] A-1: First positive electrode active material manufactured in Synthesis Example 1-1

[0302] A-2: First positive electrode active material manufactured in Synthesis Example 1-2

[0303] A-3: First positive electrode active material manufactured in Synthesis Example 1-3

[0304] B-1: Second positive electrode active material manufactured in Synthesis Example 2-1

[0305] C-1: Third positive electrode active material manufactured in Synthesis Example 3-1

[0306] D-1: SWCNT challenge material

[0307] D-2: Carbon-based conductive material

[0308]

[0309] The characteristics of the lithium secondary battery samples of the above examples and comparative examples were evaluated according to the following experimental examples, and the results are shown in Table 3.

[0310]

[0311] Experimental Example 4: Evaluation of High-Temperature Lifetime Characteristics

[0312] For the lithium secondary battery samples of Examples and Comparative Examples, the batteries were charged at 0.3 C under constant current / constant voltage (CC / CV) conditions at a temperature of 45 ℃ to a voltage corresponding to SOC98, cut off at 0.05 C, and then discharged at 0.5 C under constant current (CC) conditions to a voltage corresponding to SOC4, and the discharge capacity was measured. This was repeated 1000 times, and the capacity retention rate was calculated as the percentage of the discharge capacity after 800 and 1000 cycles divided by the discharge capacity at one cycle.

[0313] When measuring capacity by repeating cycles, if the capacity retention rate reaches 80% or the battery is damaged due to a vent, etc., the number of cycles at which the problem occurred is recorded in Table 3.

[0314] Figures 7 to 11 show graphs of the discharge capacity retention rate during high-temperature charge / discharge according to the number of cycles of examples and comparative examples.

[0315]

[0316] Experimental Example 5: Evaluation of Rapid Charge / Discharge Lifetime Characteristics

[0317] For the lithium secondary battery samples of the examples and comparative examples, 3.0C / 2.75C / 2.5C / 2.25C / 2.0C / 1.75C / 1.5C / 1.25C / 1.0C / 0.75C / 0.5C at a temperature of 25 ℃

[0318] After charging to reach DOD72 within 35 minutes according to the Step charging method at C-rate, it was discharged at 0.5C. The above charging and discharging were considered as one cycle, and the cycle was repeated 400 times. The capacity retention rate was calculated as the percentage of the discharge capacity after 400 cycles divided by the discharge capacity at one cycle.

[0319] Figures 12 to 16 show graphs of the discharge capacity retention rate during rapid charge / discharge according to the number of cycles of examples and comparative examples.

[0320]

[0321] Experimental Example 6: Evaluation of High-Temperature Storage Characteristics

[0322] The lithium secondary battery samples of the examples and comparative examples were placed in an oven at 60°C and left for 40 weeks, and the time at which venting occurred was observed.

[0323]

[0324] High temperature charge / discharge capacity retention rateRapid charge / discharge capacity retention rate(%)High temperature storage event occurrence time(Note)800cyc1000cyc400cycExample 184.981.887.332Example 283.780.886.9Not measuredExample 386.282.191.734Example 482.979.388.028Example 588.886.283.835Example 684.681.392.232Example 786.483.486.835Example 887.484.986.334Example 984.080.893.4Not measuredExample 1083.880.793.9Not measuredExample 1178.8-89.325 Comparison Example 180 (520cyc)-90.215 Comparison Example 283.8 Vent (943cyc) Sharp Drop 20 Comparison Example 380 (620cyc) Vent (689cyc)- Sharp Drop 9

[0325]

[0326] Referring to Table 3 and FIGS. 7 to 16, the lithium secondary batteries of the examples have a positive electrode including a first positive electrode active material and a negative electrode including a silicon-based active material, and thus have improved high-temperature lifespan characteristics by maintaining a high capacity even when charge and discharge are repeated at high temperatures. In addition, the lithium secondary batteries of the examples have improved rapid charge and discharge lifespan characteristics by maintaining a high discharge capacity even when rapid charge and discharge is repeated.

[0327] It can be confirmed that the batteries of the examples have improved high-temperature storage characteristics as they do not vent for more than 25 weeks when stored at high temperatures.

[0328] In Example 3, the high-temperature life characteristics and rapid charge / discharge life characteristics were further improved by using the first positive electrode active material further including an additional coating layer containing lithium tungstate.

[0329] In the case of Example 5, the third positive electrode active material having a large crystal grain size was used together with the first positive electrode active material, thereby further improving the high-temperature life characteristics in particular.

[0330] The battery of Example 6 further improved rapid charge / discharge cycle life characteristics by including a positive electrode including a first positive electrode active material layer and a second positive electrode active material layer having different binder contents.

[0331] The batteries of Examples 7 and 8 had a positive electrode including a first positive electrode active material layer and a second positive electrode active material layer having different binder contents, and further included a third positive electrode active material, thereby further increasing the capacity retention rate during high-temperature charge / discharge.

[0332] The battery of Example 9 includes a negative electrode including a first negative electrode active material layer and a second negative electrode active material layer having different binder contents, and the battery of Example 10 includes a negative electrode including a primer layer, so that the rapid charge / discharge capacity retention rate is particularly greatly increased.

[0333] On the other hand, since the positive electrode of the battery of Comparative Example 1 did not contain the first positive electrode active material, the capacity rapidly decreased when charging and discharging were repeated in a high-temperature environment, and a vent occurred in the pouch of the battery after about 15 weeks at a temperature of 60°C.

[0334] The negative electrode of the battery of Comparative Example 2 did not contain a silicon-based active material, so the capacity retention rate during rapid charge / discharge rapidly deteriorated to 75% in only about 100 cycles (see Fig. 16).

[0335] The positive electrode of the battery of Comparative Example 3 did not include the first positive electrode active material, and the negative electrode did not include a silicon-based active material, so all the problems that appeared in Comparative Examples 1 and 2 were observed.

Claims

1. A positive electrode including a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector and including a first positive electrode active material; and A negative electrode comprising a negative current collector and a negative active material layer disposed on the negative current collector and including a silicon-based active material, A lithium secondary battery, wherein the first positive electrode active material comprises lithium-nickel metal oxide particles and a coating layer disposed on at least a portion of the surface of the lithium-nickel metal oxide particles and comprising at least one selected from the group consisting of a lithium-phosphorus-containing compound, a lithium-sulfur-containing compound, a lithium-tungsten-containing compound, and a lithium-aluminum-containing compound.

2. A lithium secondary battery according to claim 1, wherein the content of the first positive electrode active material is 50 wt% to 99 wt% of the total weight of the positive electrode active material layer.

3. In the first paragraph, the lithium-nickel metal oxide particles have a secondary particle structure in which a plurality of primary particles are aggregated, A lithium secondary battery, wherein the coating layer is disposed on at least a portion of the surface of the secondary particle and at least a portion of the interface of the plurality of primary particles inside the secondary particle.

4. A lithium secondary battery according to claim 1, wherein the lithium-nickel metal oxide further comprises at least one of cobalt and manganese, and the content of nickel in the lithium-nickel metal oxide is 48 mol% to 98 mol% based on the total mole number of nickel, cobalt, and manganese.

5. A lithium secondary battery according to claim 1, wherein the positive electrode active material layer comprises lithium-nickel metal oxide particles having a secondary particle structure in which a plurality of primary particles are aggregated, and further comprises a second positive electrode active material that does not include the coating layer.

6. In the first paragraph, the positive electrode active material layer is A lithium secondary battery comprising lithium-nickel metal oxide particles having a crystal grain size of 250 nm to 1000 nm as measured by X-ray diffraction analysis (XRD) and calculated by the following equation 1, and further comprising a third positive electrode active material not including the coating layer. [Formula 1] (In Equation 1, L is the grain size, λ is the X-ray wavelength, β is the half width of the peak on the (003) plane, and θ is the diffraction angle).

7. In the first paragraph, the positive electrode active material layer includes a first positive electrode active material layer and a second positive electrode active material layer sequentially laminated on the positive electrode current collector, The first positive electrode active material layer and the second positive electrode active material layer each independently include at least one selected from the group consisting of the first positive electrode active material, the second positive electrode active material, and the third positive electrode active material, The second positive electrode active material includes lithium-nickel metal oxide particles having a secondary particle structure in which a plurality of primary particles are aggregated, and does not include the coating layer. The third cathode active material comprises lithium-nickel metal oxide particles having a crystal grain size of 250 nm to 1000 nm as measured by X-ray diffraction analysis (XRD) and calculated by the following equation 1, and does not include the coating layer. A lithium secondary battery, wherein at least one of the types and contents of the positive electrode active material included in the first positive electrode active material layer and the second positive electrode active material layer are different from each other: [Formula 1] (In Equation 1, L is the grain size, λ is the X-ray wavelength, β is the half width of the peak on the (003) plane, and θ is the diffraction angle).

8. A lithium secondary battery in accordance with claim 5, wherein the content of the second positive electrode active material is 10 wt% to 50 wt% of the total weight of the positive electrode active material layer.

9. A lithium secondary battery in claim 6, wherein the content of the third positive electrode active material is 10 wt% to 50 wt% of the total weight of the positive electrode active material layer.

10. A lithium secondary battery in accordance with claim 5, wherein, within a region of a depth of 10 nm to 30 nm from the surface of the primary particle of the second positive electrode active material, there exists a region in which the content of the layered structure is smaller than the sum of the contents of the cubic structure and the spinel structure.

11. In the first paragraph, the positive electrode active material layer includes a first positive electrode active material layer and a second positive electrode active material layer sequentially laminated on the positive electrode current collector, The first positive electrode active material layer and the second positive electrode active material layer each include a binder, A lithium secondary battery, wherein the content of the binder in the total weight of the first positive electrode active material layer is greater than or equal to the content of the binder in the total weight of the second positive electrode active material layer.

12. A lithium secondary battery according to claim 1, wherein the silicon-based active material comprises at least one selected from the group consisting of silicon, silicon alloy, silicon oxide, metal-doped silicon oxide, silicon carbide, silicon-carbon composite (Si-C), and silicon-containing core-shell structured particles.

13. A lithium secondary battery according to claim 1, wherein the content of the silicon-based active material is 5 wt% to 30 wt% of the total weight of the negative electrode active material layer.

14. A lithium secondary battery according to claim 1, wherein the negative active material further comprises artificial graphite.

15. In the first paragraph, the negative electrode active material layer includes a first negative electrode active material layer and a second negative electrode active material layer sequentially laminated on the negative electrode current collector, The first negative electrode active material layer and the second negative electrode active material layer each include a binder, A lithium secondary battery, wherein the content of the binder in the total weight of the first negative electrode active material layer is greater than or equal to the content of the binder in the total weight of the second negative electrode active material layer.

16. A lithium secondary battery according to claim 1, wherein the negative electrode is disposed between the negative electrode active material layer and the negative electrode current collector, and further includes a primer layer including a binder.

Citation Information

Patent Citations

  • Secondary battery and vehicle

    JP2008258055A

  • Hemostatic agent with film and method for preparing thereof

    KR1020230164270A

  • Cathode active material for lithium secondary battery and lithium secondary battery including the same

    KR102293034B1

  • Method and system for managing cloud access and accounts

    KR102551891B1

  • KR20220126129A

Cited By

  • Cathode active material for lithium secondary battery and lithium secondary battery including the same

    EP4790025A1