Polyolefin resin composition and molded article produced therefrom

A polyolefin resin composition combining polypropylene copolymer, polyethylene, and maleic anhydride-modified polypropylene resins addresses the adhesion and electrolyte resistance challenges of polypropylene, ensuring strong bonding to polar substrates and stability in high-temperature electrolyte environments.

WO2024242390A1PCT designated stage expired Publication Date: 2024-11-28LOTTE CHEM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/006532
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-24
Filing Date
2024-05-14
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Polypropylene resin, commonly used for its rigidity and heat resistance, faces challenges in achieving strong adhesion to polar substrates due to its non-polar nature and poor flexibility, and its adhesive strength decreases when exposed to high temperatures in electrolyte environments.

Method used

A polyolefin resin composition comprising a blend of polypropylene copolymer resin, polyethylene resin, polyolefin-based elastomer, and maleic anhydride-modified polypropylene resins, optimized in molecular weight and modification ratios, to enhance adhesion and electrolyte resistance.

Benefits of technology

The composition achieves excellent adhesive strength to polar substrates and maintains resistance in electrolyte environments, even at elevated temperatures, as demonstrated by the measured peel strengths before and after immersion in lithium secondary battery electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

A polyolefin resin composition of the present invention comprises: about 100 parts by weight of a base material including about 60 wt% to about 98 wt% of a polypropylene copolymer resin, and about 1 wt% to about 30 wt% of a polyethylene resin, and about 1 wt% to about 30 wt% of a polyolefin-based elastomer; and about 3 parts by weight to about 15 parts by weight of a maleic anhydride-modified polypropylene resin including about 50 wt% to about 95 wt % of a first maleic anhydride-modified polypropylene having a weight average molecular weight of about 40,000 g / mol or more and a maleic anhydride modification ratio of about 1.5 wt % or more, and about 5 wt% to about 50 wt % of a second maleic anhydride-modified polypropylene having a weight average molecular weight of less than about 40,000 g / mol and a maleic anhydride modification ratio of about 1.5 wt % or more. The polyolefin resin composition has excellent adhesive strength in terms of adhering to a polar substrate, electrolyte resistance, and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Polyolefin resin composition and molded article manufactured therefrom

[0001] The present invention relates to a polyolefin resin composition and a molded article manufactured therefrom. More specifically, the present invention relates to a polyolefin resin composition having excellent adhesive strength to polar substrates, electrolyte resistance, etc., and a molded article manufactured therefrom.

[0002]

[0003] Among polyolefin resins, polypropylene resin boasts excellent rigidity, transparency, and heat resistance, making it widely used as a thermoplastic molding material. Because polypropylene resin is non-polar, it must be acid-modified to achieve adhesion to polar substrates. Furthermore, polypropylene resin lacks flexibility and wettability, preventing it from achieving sufficient adhesion. Therefore, an elastomer component is typically added to polypropylene resin to improve adhesion to polar substrates.

[0004] In this way, when an elastomer component is mixed into an acid-modified polypropylene resin, the adhesiveness at room temperature can be improved, but there is a problem that the adhesive strength may decrease when left at 80℃ or higher after being immersed in a battery electrolyte, etc.

[0005] Therefore, there is a need to develop a polyolefin resin composition with excellent adhesive strength and electrolyte resistance to polar substrates.

[0006] The background technology of the present invention is disclosed in Korean Patent No. 10-1200658, etc.

[0007]

[0008] The purpose of the present invention is to provide a polyolefin resin composition having excellent adhesive strength to polar substrates, electrolyte resistance, etc.

[0009] Another object of the present invention is to provide a molded article formed from the polyolefin resin composition.

[0010] The above and other objects of the present invention can all be achieved by the present invention described below.

[0011]

[0012] 1. One aspect of the present invention relates to a polyolefin resin composition. The polyolefin resin composition comprises: about 100 parts by weight of a base material including about 60 to about 98 wt% of a polypropylene copolymer resin, about 1 to about 30 wt% of a polyethylene resin, and about 1 to about 30 wt% of a polyolefin elastomer; and about 3 to about 15 parts by weight of a maleic anhydride-modified polypropylene resin including about 50 to about 95 wt% of a first maleic anhydride-modified polypropylene having a weight average molecular weight of about 40,000 g / mol or more and a maleic anhydride modification ratio of about 1.5 wt% or more, and about 5 to about 50 wt% of a second maleic anhydride-modified polypropylene having a weight average molecular weight of less than about 40,000 g / mol and a maleic anhydride modification ratio of about 1.5 wt% or more.

[0013] 2. In the above 1 specific example, the polypropylene copolymer resin may include at least one of a propylene / ethylene random copolymer and a propylene / ethylene / α-olefin copolymer.

[0014] 3. In the above 1 or 2 specific examples, the polypropylene copolymer resin may have a content of propylene-derived components of about 85 to about 99 mol%, a content of ethylene-derived components of about 1 to about 10 mol%, and a content of α-olefin-derived components of about 0 to about 8 mol%.

[0015] 4. In the above specific examples 1 to 3, the polypropylene copolymer resin may have a melting point (Tm) of about 120 to about 150°C.

[0016] 5. In the above 1 to 4 specific examples, the polyethylene resin may include at least one of low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and linear low-density polyethylene (LLDPE).

[0017] 6. In the above 1 to 5 specific examples, the polyethylene resin may include at least one of low-density polyethylene (LDPE) and linear low-density polyethylene (LLDPE).

[0018] 7. In the above 1 to 6 specific examples, the polyolefin-based elastomer may include at least one of ethylene-propylene rubber, ethylene-butene rubber, and ethylene-octene rubber.

[0019] 8. In the above 1 to 7 specific examples, the first maleic anhydride modified polypropylene may have a weight average molecular weight of about 45,000 to about 60,000 g / mol, and a maleic anhydride modification ratio of about 1.6 to about 6 wt%.

[0020] 9. In the above 1 to 8 specific examples, the second maleic anhydride modified polypropylene may have a weight average molecular weight of about 10,000 to about 39,000 g / mol, and a maleic anhydride modification ratio of about 1.6 to about 6 wt%.

[0021] 10. In the above 1 to 9 specific examples, the weight ratio of the first maleic anhydride-modified polypropylene and the second maleic anhydride-modified polypropylene may be about 1:0.06 to about 1:0.7.

[0022] 11. In the above 1 to 10 specific examples, the polyolefin resin composition is manufactured by using the polyolefin resin composition and the polypropylene resin, manufacturing a two-layer film composed of the polyolefin resin composition and the polypropylene resin with a multilayer film molding machine, laminating the polyolefin resin composition layer of the film manufactured with the multilayer film molding machine on aluminum in the form of a film to which nylon is laminated so that it is in contact, and then heating at 200°C for 5 minutes to manufacture a specimen, and then cutting the specimen to a length of 100 mm and a width of 15 mm, and using a universal testing machine (UTM) to peel the aluminum and polypropylene resin layers at a speed of 50 mm / min, the adhesive strength is about 15 to about 20 kgf / cm. 2 It could be.

[0023] 12. In the above 1 to 11 specific examples, the polyolefin resin composition is used to manufacture a two-layer film composed of the polyolefin resin composition and the polypropylene resin using a multilayer film molding machine, and the polyolefin resin composition layer of the film manufactured by the multilayer film molding machine is laminated on aluminum in the form of a film to which nylon is laminated so that it is in contact, and then heated at 200°C for 5 minutes to manufacture a specimen, and then the specimen is cut to a length of 100 mm and a width of 25 mm, and the cut specimen is immersed in a lithium secondary battery electrolyte at 85°C for 24 hours, and then both sides of the specimen are cut to a length of 100 mm and a width of 15 mm. The specimen manufactured by peeling the aluminum and the polypropylene resin layers at a speed of 50 mm / min using a universal testing machine (UTM) has an adhesive strength of about 8 to about 15 kgf / cm. 2 It could be.

[0024] 13. Another aspect of the present invention relates to a molded article. The molded article is characterized in that it is formed from a polyolefin resin composition according to any one of 1 to 12.

[0025]

[0026] The present invention has the effect of providing a polyolefin resin composition having excellent adhesive strength to a polar substrate, electrolyte resistance, etc., and a molded article formed therefrom.

[0027]

[0028] Hereinafter, the present invention will be described in detail as follows.

[0029] A polyolefin resin composition according to the present invention comprises (A) a base material comprising a polypropylene copolymer resin, a polyethylene resin, and a polyolefin-based elastomer; and (B) a maleic anhydride-modified polypropylene resin comprising a first maleic anhydride-modified polypropylene and a second maleic anhydride-modified polypropylene.

[0030] In this specification, “a to b” indicating a numerical range is defined as “≥a and ≤b”.

[0031]

[0032] (A) Basic materials

[0033] According to one specific example of the present invention, a base material comprises a polypropylene copolymer resin, a polyethylene resin, and a polyolefin-based elastomer, and is applied together with a maleic anhydride-modified polypropylene resin comprising first and second maleic anhydride-modified polypropylenes having a specific range of weight average molecular weight and maleic anhydride modification ratio (graft ratio), thereby improving the adhesive strength, electrolyte resistance, etc. of the polyolefin resin composition to a polar substrate.

[0034] In a specific example, the polypropylene copolymer resin may include at least one of a propylene / ethylene random copolymer and a propylene / ethylene / α-olefin copolymer.

[0035] In a specific example, the polypropylene copolymer resin may have a content of a propylene-derived component of about 85 to about 99 mol%, for example, about 90 to about 98 mol%, an ethylene-derived component of about 1 to about 10 mol%, for example, about 2 to about 5 mol%, and an α-olefin-derived component of about 0 to about 8 mol%, for example, about 0 to about 5 mol%. Here, when the content of the α-olefin-derived component is 0 mol%, the polypropylene copolymer resin is a propylene / ethylene random copolymer. Within the above range, the polyolefin resin composition may have excellent processability, film formability, etc.

[0036] In a specific example, the polypropylene copolymer resin may have a melting point (Tm) of about 120 to about 150°C, for example, about 125 to about 145°C. Within this range, the adhesiveness (adhesive strength to a polar substrate) of the polyolefin resin composition may be excellent.

[0037] In a specific example, the polypropylene copolymer resin may be included in an amount of about 60 to about 98 wt%, for example, about 65 to about 90 wt%, for example, about 75 to about 85 wt%, based on 100 wt% of the base material. If the content of the polypropylene copolymer resin is outside the above range, there is a concern that the mechanical properties, processability, etc. of the polyolefin resin composition may deteriorate.

[0038] In a specific example, the polyethylene resin may include one or more of low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and linear low-density polyethylene (LLDPE). For example, the polyethylene resin may be low-density polyethylene (LDPE) and / or linear low-density polyethylene (LLDPE).

[0039] In a specific example, the polyethylene resin may have a melt-flow index of about 0.5 to about 15 g / 10 min, for example, about 1 to about 10 g / 10 min, measured under conditions of 190°C and a load of 2.16 kg according to ASTM D1238. Within this range, the film formability of the polyolefin resin composition may be excellent.

[0040] In a specific example, the polyethylene resin may be included in an amount of about 1 to about 30 wt%, for example, about 5 to about 25 wt%, for example, about 5 to about 10 wt%, of 100 wt% of the base material. If the content of the polyethylene resin is outside the above range, there is a concern that the mechanical properties, processability, etc. of the polyolefin resin composition may deteriorate.

[0041] In a specific example, the polyolefin-based elastomer can improve adhesive strength to a polar substrate, electrolyte resistance, etc., and a polyolefin-based elastomer used in a typical polyolefin resin composition can be used.

[0042] In specific examples, the polyolefin-based elastomer may include ethylene-propylene rubber, ethylene-butene rubber, ethylene-octene rubber, combinations thereof, and the like, and may be, for example, ethylene-propylene rubber.

[0043] In a specific example, the polyolefin-based elastomer may have a melt-flow index of about 0.1 to about 5 g / 10 min, for example, about 0.5 to about 3 g / 10 min, measured under conditions of 190°C and a load of 2.16 kg according to ASTM D1238. Within this range, the wettability, mechanical properties, etc. of the polyolefin resin composition may be excellent.

[0044] In a specific example, the polyolefin-based elastomer may be included in an amount of about 1 to about 30 wt%, for example, about 5 to about 25 wt%, for example, about 10 to about 15 wt%, based on 100 wt% of the base material. If the content of the polyolefin-based elastomer is outside the above range, there is a concern that the adhesive strength of the polyolefin resin composition to a polar substrate, electrolyte resistance, etc. may be reduced.

[0045]

[0046] (B) Maleic anhydride modified polypropylene resin

[0047] According to one specific example of the present invention, a maleic anhydride-modified polypropylene resin comprises a first maleic anhydride-modified polypropylene and a second maleic anhydride-modified polypropylene having a weight average molecular weight and a maleic anhydride modification ratio (graft ratio) within a specific range, and is applied together with the base material to improve the adhesive strength, electrolyte resistance, etc. of the polyolefin resin composition to a polar substrate.

[0048] In a specific example, the first maleic anhydride-modified polypropylene may be a maleic anhydride-modified polypropylene having a weight average molecular weight of about 40,000 g / mol or more and a maleic anhydride modification ratio of about 1.5 wt% or more.

[0049] In a specific example, the first maleic anhydride-modified polypropylene may have a weight average molecular weight of about 40,000 g / mol or more, for example, about 45,000 to about 60,000 g / mol, as measured by gel permeation chromatography (GPC). When the weight average molecular weight of the first maleic anhydride-modified polypropylene is less than about 40,000 g / mol, there is a concern that the adhesive strength of the polyolefin resin composition to a polar substrate, electrolyte resistance, etc. may be reduced.

[0050] In a specific example, the first maleic anhydride-modified polypropylene may have a maleic anhydride modification ratio of about 1.5 wt% or more, for example, about 1.6 to about 6 wt%, for example, about 1.7 to about 3 wt%. If the maleic anhydride modification ratio of the first maleic anhydride-modified polypropylene is less than about 1.5 wt%, there is a concern that the adhesive strength of the polyolefin resin composition to a polar substrate, electrolyte resistance, etc. may be reduced.

[0051] In a specific example, the first maleic anhydride-modified polypropylene may be included in an amount of about 50 to about 95 wt%, for example, about 65 to about 94 wt%, based on 100 wt% of the total maleic anhydride-modified polypropylene resin. If the content of the first maleic anhydride-modified polypropylene is outside the above range, there is a concern that the adhesive strength of the polyolefin resin composition to a polar substrate, electrolyte resistance, etc. may be reduced.

[0052] In a specific example, the second maleic anhydride-modified polypropylene may be a maleic anhydride-modified polypropylene having a weight average molecular weight of less than about 40,000 g / mol and a maleic anhydride modification ratio of about 1.5 wt% or more.

[0053] In a specific example, the second maleic anhydride-modified polypropylene may have a weight average molecular weight of less than about 40,000 g / mol, for example, about 10,000 to about 39,000 g / mol, as measured by gel permeation chromatography (GPC). When the weight average molecular weight of the second maleic anhydride-modified polypropylene is about 40,000 g / mol or more, there is a concern that the adhesive strength of the polyolefin resin composition to a polar substrate, electrolyte resistance, etc. may be reduced.

[0054] In a specific example, the second maleic anhydride-modified polypropylene may have a maleic anhydride modification ratio of about 1.5 wt% or more, for example, about 1.6 to about 6 wt%, for example, about 2.5 to about 4.5 wt%. If the maleic anhydride modification ratio of the second maleic anhydride-modified polypropylene is less than about 1.5 wt%, there is a concern that the adhesive strength of the polyolefin resin composition to a polar substrate, electrolyte resistance, etc. may be reduced.

[0055] In a specific example, the second maleic anhydride-modified polypropylene may be included in an amount of about 5 to about 50 wt%, for example, about 6 to about 35 wt%, based on 100 wt% of the total maleic anhydride-modified polypropylene resin. If the content of the second maleic anhydride-modified polypropylene is outside the above range, there is a concern that the adhesive strength of the polyolefin resin composition to a polar substrate, electrolyte resistance, etc. may be reduced.

[0056] In a specific example, the weight ratio of the first maleic anhydride-modified polypropylene and the second maleic anhydride-modified polypropylene (first maleic anhydride-modified polypropylene: second maleic anhydride-modified polypropylene) may be from about 1:0.06 to about 1:0.7, for example, from about 1:0.07 to about 1:0.6. In this range, the adhesive strength of the polyolefin resin composition to a polar substrate, electrolyte resistance, etc. may be more excellent.

[0057] In a specific example, the content of the maleic anhydride-modified polypropylene resin may be about 3 to about 15 parts by weight, for example, about 5 to about 10 parts by weight, for example, about 5.5 to about 7.5 parts by weight, based on about 100 parts by weight of the base material. If the content of the maleic anhydride-modified polypropylene resin is outside the above range, there is a concern that the adhesive strength, electrolyte resistance, film formability, etc. of the polyolefin resin composition to a polar substrate may be reduced.

[0058]

[0059] A polyolefin resin composition according to one specific embodiment of the present invention may further include additives included in conventional polyolefin resin compositions. Examples of the additives include, but are not limited to, antioxidants, stabilizers, flame retardants, anti-drip agents, lubricants, release agents, nucleating agents, antistatic agents, stabilizers, pigments, dyes, and mixtures thereof. When the additives are used, the content thereof may be about 0.001 to about 20 parts by weight, for example, about 0.1 to about 10 parts by weight, based on about 100 parts by weight of the base material, but is not limited thereto.

[0060]

[0061] A polyolefin resin composition according to one specific example of the present invention may be in the form of pellets obtained by mixing the above components and melt-extruding them at about 150 to about 230°C, for example, about 170 to about 210°C, using a conventional twin-screw extruder.

[0062] In a specific example, a two-layer film composed of the polyolefin resin composition and the polypropylene resin is manufactured using a multilayer film molding machine using the polyolefin resin composition and the polypropylene resin, and the polyolefin resin composition layer of the film manufactured by the multilayer film molding machine is laminated on aluminum in the form of a film to which nylon is laminated so that it is in contact, and then heated at 200°C for 5 minutes to manufacture a specimen, and then the specimen is cut into a length of 100 mm and a width of 15 mm, and the aluminum and polypropylene resin layers are peeled off at a speed of 50 mm / min using a universal testing machine (UTM), and the adhesive strength is measured to be about 15 to about 20 kgf / cm. 2 , for example, about 15 to about 19 kgf / cm 2 It could be.

[0063] In a specific example, the polyolefin resin composition is manufactured by using the polyolefin resin composition and the polypropylene resin, manufacturing a two-layer film composed of the polyolefin resin composition and the polypropylene resin with a multilayer film molding machine, laminating the polyolefin resin composition layer of the film manufactured with the multilayer film molding machine on aluminum in the form of a film to which nylon is laminated so that it is in contact, and then heating at 200°C for 5 minutes to manufacture a specimen, and then cutting the specimen to a length of 100 mm and a width of 25 mm, and immersing the cut specimen in a lithium secondary battery electrolyte at 85°C for 24 hours, and then cutting both sides of the specimen to a length of 100 mm and a width of 15 mm, and measuring the adhesive strength of the specimen manufactured by peeling the aluminum and the polypropylene resin layer at a speed of 50 mm / min using a universal testing machine (UTM) of about 8 to about 15 kgf / cm 2 , for example, about 9 to about 13 kgf / cm 2 It could be.

[0064]

[0065] The molded article according to the present invention is formed from the polyolefin resin composition. The polyolefin resin composition can be manufactured in the form of pellets, and the manufactured pellets can be manufactured into various molded articles (products) through various molding methods such as injection molding, extrusion molding, vacuum molding, and casting molding. Such molding methods are well known to those skilled in the art to which the present invention pertains. The molded article has excellent adhesive strength to polar substrates, electrolyte resistance, etc., and is useful as an adhesive film, adhesive sheet, etc. for bonding to polar substrates (aluminum, steel, ethylene vinyl alcohol (EVOH), polyamide, etc.).

[0066]

[0067] Hereinafter, the present invention will be described in more detail through examples; however, these examples are for the purpose of explanation only and should not be construed as limiting the present invention.

[0068]

[0069] Example

[0070] Below, the specifications of each component used in the examples and comparative examples are as follows.

[0071] (A) Basic materials

[0072] (A1) Polypropylene copolymer resin (propylene-ethylene-1-butene terpolymer, manufacturer: Lotte Chemical, product name: SFC-750, melting point (Tm): approximately 132°C) was used.

[0073] (A2-1) Polyethylene resin (linear low-density polyethylene (LLDPE), manufacturer: Lotte Chemical, product name: UT-404) was used.

[0074] (A2-2) Polyethylene resin (low-density polyethylene (LDPE), manufacturer: Lotte Chemical, product name: XL-610S) was used.

[0075] (A3) Polyolefin elastomer

[0076] Ethylene-propylene rubber (manufacturer: ExxonMobil, product name: Vistalon 722) was used.

[0077] (B) Maleic anhydride modified polypropylene resin

[0078] (B1) First maleic anhydride modified polyolefin

[0079] Maleic anhydride-modified polypropylene (maleic anhydride modification ratio: approximately 2 wt%, weight average molecular weight: approximately 53,000 g / mol) was used.

[0080] (B2) Second maleic anhydride modified polyolefin

[0081] (B2-1) Maleic anhydride-modified polypropylene (maleic anhydride modification ratio: approximately 4 wt%, weight average molecular weight: approximately 19,000 g / mol) was used.

[0082] (B2-2) Maleic anhydride-modified polypropylene (maleic anhydride modification ratio: approximately 3 wt%, weight average molecular weight: approximately 38,000 g / mol) was used.

[0083]

[0084] Examples 1 to 8 and Comparative Examples 1 to 5

[0085] After adding each of the above components in the amounts described in Tables 1 and 2 below, pellets were manufactured by extrusion at a barrel temperature of approximately 170°C. The extrusion was performed using a twin-screw extruder with an L / D of 40 and a diameter of 19 mm, and the manufactured pellets were dried at approximately 80°C for approximately 4 hours or more, and then specimens were manufactured using a multilayer film molding machine according to the method for measuring physical properties described below. The physical properties of the manufactured specimens were evaluated using the following method, and the results are shown in Tables 1 and 2 below.

[0086]

[0087] Method of measuring physical properties

[0088] (1) Adhesive strength (peel strength, unit: kgf / cm) 2 ): Using the polyolefin resin composition and polypropylene resin (manufacturer: Lotte Chemical, product name: SFC550), a two-layer film composed of the polyolefin resin composition and the polypropylene resin was manufactured using a multilayer film molding machine, and the polyolefin resin composition layer among the films manufactured using the multilayer film molding machine was laminated on top of aluminum (thickness: approximately 113 μm) in the form of a film to which nylon was laminated so that it was in contact, and then heated at 200°C for 5 minutes to manufacture a specimen, and then the specimen was cut into 100 mm in length and 15 mm in width, and the adhesive strength was measured by peeling the aluminum and polypropylene resin layers at a speed of 50 mm / min using a universal testing machine (UTM, manufacturer: ZwickRoell, device name: Z020).

[0089] (2) Adhesive strength after immersion in electrolyte (electrolyte resistance, peel strength, unit: kgf / cm)2 ): Using the above polyolefin resin composition and polypropylene resin (manufacturer: Lotte Chemical, product name: SFC550), a two-layer film composed of the polyolefin resin composition and the polypropylene resin was manufactured using a multilayer film molding machine, and the polyolefin resin composition layer among the films manufactured using the multilayer film molding machine was laminated on aluminum (thickness: about 113 μm) in the form of a film to which nylon was laminated so that it was in contact, and then heated at 200°C for 5 minutes to manufacture a specimen, and then the specimen was cut into 100 mm in length and 25 mm in width, and the cut specimen was immersed in a lithium secondary battery electrolyte at 85°C in which lithium salt (LiPF6) was dissolved at a concentration of 1 M in a solvent in which ethylene carbonate (EC): dimethyl carbonate (DMC): diethyl carbonate (DEC) was mixed at a volume ratio of 1: 1: 1 for 24 hours, and then both sides of the specimen were cut to length The adhesive strength was measured by peeling the aluminum and polypropylene resin layers at a speed of 50 mm / min using a universal testing machine (UTM, manufacturer: ZwickRoell, device name: Z020) on a specimen manufactured to be 100 mm long and 15 mm wide.

[0090]

[0091] Example 12345678(A) (weight%)(A1)8580808080807580(A2-1)5101010101010-(A2-2)-------10(A3)101010101010101510(B) (weight part)5.55.55.57.56.06.05.55.5(B) (weight%)(B1)90.990.990.993.383.366.790.990.9(B2-1)9.19.1-6.716.733.39.19.1(B2-2)--9.1-----Adhesive strength15.116.417.217.016.817.518.515.5Electrolyte Adhesive strength after immersion9.810.29.911.511.510.711.312.1

[0092] * Weight parts: (A) Weight parts for approximately 100 weight parts of basic material

[0093]

[0094] Comparative Example 12345 (A) (weight %) (A1) 9090808080 (A2-1) -10101010 (A2-2)----- (A3) 10-101010 (B) (weight part) 5.5 5.5 5.5 5.0 6.0 (B) (weight %) (B1) 90.9 90.9 -100 16.7 (B2-1) 9.19 19.1 -83.3 (B2-2) --90.9 --Adhesive strength 13.6 8.7 7.5 14.8 8.7 Adhesive strength after immersion in electrolyte 4.4 1.5 1.2 7.13.6

[0095] * Weight parts: (A) Weight parts for approximately 100 weight parts of basic material

[0096]

[0097] From the above results, it can be seen that the polyolefin resin composition of the present invention has excellent adhesive strength to polar substrates, electrolyte resistance, etc.

[0098] On the other hand, in Comparative Example 1 where no polyethylene resin was applied (the content of the polyethylene resin is less than the range of the present invention), in Comparative Example 2 where no polyolefin elastomer was applied (the content of the polyolefin elastomer is less than the range of the present invention), in Comparative Example 3 where no first maleic anhydride-modified polypropylene was applied (the weight average molecular weight of the first maleic anhydride-modified polypropylene is less than the range of the present invention), in Comparative Example 4 where no second maleic anhydride-modified polypropylene was applied (the weight average molecular weight of the second maleic anhydride-modified polypropylene exceeds the range of the present invention), and in Comparative Example 5 where the content of the first maleic anhydride-modified polypropylene is less than the range of the present invention and the content of the second maleic anhydride-modified polypropylene exceeds the range of the present invention, it can be seen that the adhesive strength to a polar substrate, electrolyte resistance, etc. are all reduced.

[0099]

[0100] The present invention has been described with reference to exemplary embodiments. Those skilled in the art will appreciate that the present invention can be implemented in modified forms without departing from its essential characteristics. Therefore, the disclosed embodiments should be considered illustrative rather than limiting. The scope of the present invention is set forth in the claims, not the foregoing description, and all differences within the scope equivalent thereto should be construed as being encompassed by the present invention.

Claims

1. About 100 parts by weight of a base material comprising about 60 to about 98 wt% of a polypropylene copolymer resin, about 1 to about 30 wt% of a polyethylene resin, and about 1 to about 30 wt% of a polyolefin elastomer; and A polyolefin resin composition comprising about 3 to about 15 parts by weight of a maleic anhydride-modified polypropylene resin, comprising about 50 to about 95 parts by weight of a first maleic anhydride-modified polypropylene having a weight average molecular weight of about 40,000 g / mol or more and a maleic anhydride modification ratio of about 1.5 wt% or more, and about 5 to about 50 parts by weight of a second maleic anhydride-modified polypropylene having a weight average molecular weight of less than about 40,000 g / mol and a maleic anhydride modification ratio of about 1.5 wt% or more.

2. A polyolefin resin composition according to claim 1, characterized in that the polypropylene copolymer resin comprises at least one of a propylene / ethylene random copolymer and a propylene / ethylene / α-olefin copolymer.

3. A polyolefin resin composition according to claim 1 or 2, characterized in that the polypropylene copolymer resin has a content of a propylene-derived component of about 85 to about 99 mol%, a content of an ethylene-derived component of about 1 to about 10 mol%, and a content of an α-olefin-derived component of about 0 to about 8 mol%.

4. A polyolefin resin composition according to any one of claims 1 to 3, wherein the polypropylene copolymer resin has a melting point (Tm) of about 120 to about 150°C.

5. A polyolefin resin composition according to any one of claims 1 to 4, characterized in that the polyethylene resin comprises at least one of low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and linear low-density polyethylene (LLDPE).

6. A polyolefin resin composition according to any one of claims 1 to 5, characterized in that the polyethylene resin comprises at least one of low-density polyethylene (LDPE) and linear low-density polyethylene (LLDPE).

7. A polyolefin resin composition according to any one of claims 1 to 6, characterized in that the polyolefin-based elastomer comprises at least one of ethylene-propylene rubber, ethylene-butene rubber, and ethylene-octene rubber.

8. A polyolefin resin composition according to any one of claims 1 to 7, wherein the first maleic anhydride-modified polypropylene has a weight average molecular weight of about 45,000 to about 60,000 g / mol and a maleic anhydride modification ratio of about 1.6 to about 6 wt%.

9. A polyolefin resin composition according to any one of claims 1 to 8, wherein the second maleic anhydride-modified polypropylene has a weight average molecular weight of about 10,000 to about 39,000 g / mol and a maleic anhydride modification ratio of about 1.6 to about 6 wt%.

10. A polyolefin resin composition according to any one of claims 1 to 9, wherein the weight ratio of the first maleic anhydride-modified polypropylene and the second maleic anhydride-modified polypropylene is about 1:0.06 to about 1:0.

7.

11. In any one of claims 1 to 10, the polyolefin resin composition is manufactured by using the polyolefin resin composition and the polypropylene resin to manufacture a two-layer film composed of the polyolefin resin composition and the polypropylene resin with a multilayer film molding machine, and the polyolefin resin composition layer of the film manufactured with the multilayer film molding machine is laminated on aluminum in the form of a film to which nylon is laminated so that it is in contact, and then heating at 200°C for 5 minutes to manufacture a specimen, and then the specimen is cut into a length of 100 mm and a width of 15 mm, and the aluminum and polypropylene resin layers are peeled off at a speed of 50 mm / min using a universal testing machine, and the adhesive strength is measured to be about 15 to about 20 kgf / cm. 2 A polyolefin resin composition characterized by:

12. In any one of claims 1 to 11, the polyolefin resin composition is manufactured by using the polyolefin resin composition and the polypropylene resin, manufacturing a two-layer film composed of the polyolefin resin composition and the polypropylene resin with a multilayer film molding machine, laminating the polyolefin resin composition layer of the film manufactured with the multilayer film molding machine on aluminum in the form of a film to which nylon is laminated so that it is in contact, and then heating at 200°C for 5 minutes to manufacture a specimen, and then cutting the specimen to a length of 100 mm and a width of 25 mm, and immersing the cut specimen in a lithium secondary battery electrolyte at 85°C for 24 hours, and then cutting both sides of the specimen to a length of 100 mm and a width of 15 mm, and using a universal testing machine to peel off the aluminum and the polypropylene resin layer at a speed of 50 mm / min, the adhesive strength measured is about 8 to about 15 kgf / cm. 2 A polyolefin resin composition characterized by:

13. A molded product characterized by being formed from a polyolefin resin composition according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Sizing Composition for Glassfiber

    KR101863488B1

  • Polypropylene resin composition with excellent coating property for painting car bumper, including low molecular weight polypropylene resin modified by unsaturated carboxylic acid

    KR1019990066058A

  • Thermoplastic olefin composition comprising maleic anhydride modified polymer and polymeric additive for inject molded products

    KR1019990070174A

  • Low hardness Thermoplastic elastomer resin composition and article using the same

    KR1020160114994A

  • Maleic anhydride functionalization of polypropylene via solid-state shear pulverization

    US9624320B2