Method for forming photoresist thin film reactive to extreme ultraviolet rays, and photoresist thin film formed thereby

The method of forming a photoresist thin film using specific precursors and oxygen sources addresses the challenges of photon absorption and etching resistance, enhancing sensitivity and pattern resolution for extreme ultraviolet lithography.

WO2024242478A1PCT designated stage expired Publication Date: 2024-11-28DONGJIN SEMICHEM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/006980
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-05-23
Filing Date
2024-05-23
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Current photoresists using extreme ultraviolet light sources face challenges with poor photon absorption, etching resistance, and pattern resolution, limiting their ability to form fine patterns and meet the demands of next-generation semiconductor manufacturing.

Method used

A method involving the formation of a photoresist thin film using a first precursor and an oxygen source to create a hydrophilic layer, followed by modification with a second precursor to form a hydrophobic modified layer, enhancing photon absorption and etching resistance without direct metal-hydroxyl bonding, which improves hydrophobicity and sensitivity.

Benefits of technology

The method achieves improved photon absorption and etching resistance, enabling the formation of ultrafine patterns and enhancing sensitivity, thus addressing the limitations of existing photoresists for extreme ultraviolet lithography.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006980_28112024_PF_FP_ABST
    Figure KR2024006980_28112024_PF_FP_ABST
Patent Text Reader

Abstract

An embodiment of the present invention provides a method for forming a hydrophobic photoresist thin film, comprising the steps of: injecting a first precursor and an oxygen source into a chamber in which a substrate is located, so as to form a thin film having hydrophilic groups included therein; and injecting a second precursor to modify the thin film having the hydrophilic groups included therein and form a modified layer, wherein the photoresist thin film formed thereby does not contain hydroxyl groups and thus exhibits hydrophobicity.
Need to check novelty before this filing date? Find Prior Art

Description

Method for forming an extreme ultraviolet light-reactive photoresist thin film and a photoresist thin film formed thereby

[0001] The present invention relates to a method for forming a photoresist thin film and a photoresist thin film formed thereby, and more particularly, to a method for forming a thin film including a step of forming a thin film including a hydrophilic group using two types of precursors and then modifying the thin film to form a modified layer, and to a photoresist thin film formed thereby.

[0002]

[0003] Photoresist (PR) is a chemical substance whose properties change in response to light. In displays, it is used in the photolithography process, which forms fine circuits on thin-film transistors (TFTs).

[0004] Photoresist's chemical properties change when exposed to light. Depending on the type, it hardens or melts when exposed to light. Photolithography utilizes these changes in photoresist properties to selectively remove only the weakened portions, distinguishing between those that will be used as circuits and those that will not, and creates a fine, three-dimensional circuit pattern, much like a engraving.

[0005] Photolithography is a key process in the manufacture of thin-film transistors (TFTs). Here, a thin layer of photoresist is applied to the TFT substrate. A photomask, which separates the areas where the electronic circuit pattern will be drawn from the rest, is then placed over the photoresist. When light is applied, the photoresist develops different properties depending on the areas exposed to the light. This difference in solubility between the two regions is then exploited to remove the more soluble photoresist through a development process.

[0006] The deposited material remaining in the area where the photoresist has disappeared is removed through an etching process, and the deposited material remaining under the photoresist remains intact as it is protected by the photoresist.

[0007] As it became impossible to form fine patterns smaller than 50 nm using krypton fluoride (248 nm) and argon fluoride (193 nm) light sources and general photoresists, a lithography process was recently developed that integrates many circuits in a narrower area using a short-wavelength light source and a chemically amplified deep ultraviolet (DUV) photoresist that responds to the short wavelength.

[0008] The short-wavelength light sources that are emerging include extreme ultraviolet (13 nm) light sources, ion beams, and X-rays. When the extreme ultraviolet light source is used, it is expected that it will be possible to design circuits of 0.1㎛ or less, and thus manufacture semiconductors 100 times faster and with 100 times more capacity than the currently used process.

[0009] Organic-based chemically amplified resist (CAR), a representative photoresist, has been used as a standard material up to the argon fluoride generation. However, with the introduction of extreme ultraviolet light and the miniaturization of processes, ① the photon absorption efficiency is very poor due to the low cross-section of carbon and oxygen, the main components of CAR, for photons in the extreme ultraviolet wavelength band; ② the uniformity and roughness characteristics deteriorate due to acid diffusion; and ③ the pattern collapse occurs during the developing process due to the low mechanical strength of organic-based photoresists. Therefore, the need for the development of a new inorganic photoresist that can satisfy the RLS (Resolution, LER / LWR, Sensitivity) characteristics by ① having high photon absorbance in the extreme ultraviolet wavelength and ② having excellent mechanical strength and etching resistance has arisen.

[0010] Recently, inorganic photoresists utilizing liquid and vapor phase chemical reactions as a coating method are recognized globally as the only alternative technology for forming ultra-fine patterns. However, the development of fundamental technologies for related materials, processes, and equipment remains inadequate. Therefore, to secure a leading position in next-generation extreme ultraviolet patterning technology and secure technological competitiveness, the development of inorganic photoresist materials and processes is essential.

[0011]

[0012] The technical problem to be achieved by the present invention is to provide a method for forming a photoresist thin film having improved photon absorption rate of extreme ultraviolet rays and excellent etching resistance, and a photoresist thin film formed thereby.

[0013] The technical problems to be solved by the present invention are not limited to the technical problems mentioned above, and other technical problems not mentioned can be clearly understood by a person having ordinary skill in the technical field to which the present invention belongs from the description below.

[0014]

[0015] In order to achieve the above technical task, one embodiment of the present invention provides a method for forming a hydrophobic photoresist thin film, including the steps of: injecting a first precursor and an oxygen source into a chamber in which a substrate is located to form a thin film including a hydrophilic group; and injecting a second precursor to modify the thin film including the hydrophilic group to form a modified layer.

[0016]

[0017] After forming a thin film including the hydrophilic group, a step of supplying a purge gas to the chamber to remove the unreacted oxygen source is further included.

[0018] After forming the above-mentioned modified layer, a step of supplying a purge gas to the chamber to remove unreacted second precursor is further included.

[0019] The step of forming the above modified layer does not include a reactant.

[0020] The thin film including the hydrophilic group includes a hydroxyl group.

[0021]

[0022] In an embodiment of the present invention, the first precursor comprises a structure represented by the following chemical formula 1.

[0023] [Chemical Formula 1]

[0024] (R1) a -M-(L) d

[0025] (Here 0≤a≤5, 0≤d≤5, 0 <a+d<5, a와 d는 정수이고, M은 5주기 금속이고, R1은 선형, 분지형 또는 고리형의 알킬기, 선형, 분지형 또는 고리형의 알케닐기 및 아릴기 중에 선택되는 것이며, L은 가수분해 가능한 리간드이다).

[0026] In an embodiment of the present invention, M is any one metal selected from Te, Sb, Sn, and In.

[0027] In an embodiment of the present invention, L is selected from an ester group, an amine group, an amide group, an alkoxy group, a carbonyl group, and an aldehyde group.

[0028]

[0029] In an embodiment of the present invention, the second precursor has a structure represented by the following chemical formula 2.

[0030] [Chemical Formula 2]

[0031] (R2) b -M * -(L1) e

[0032] (Here, 1≤b≤5, 0≤e≤5, 1≤b+e≤5, b and e are integers, and M *is a 5-period metal, R2 is selected from a linear, branched or cyclic alkyl group, a linear, branched or cyclic alkenyl group and an aryl group, and L1 is a hydrolyzable ligand.

[0033] In an embodiment of the present invention, the M * is any one metal selected from Te, Sb, Sn, and In.

[0034] The above L1 is selected from an ester group, an amine group, an amide group, an alkoxy group, a carbonyl group, and an aldehyde group. In an embodiment of the present invention, the oxygen source is one selected from water (H2O), oxygen (O2), ozone (O3), and hydrogen peroxide (H2O2).

[0035] At least one of the above M and M* may include Te.

[0036] Both M and M* above can be Te.

[0037] In order to achieve the above technical task, another embodiment of the present invention provides a photoresist thin film formed according to the above method.

[0038] In an embodiment of the present invention, the structure represented by the following chemical formula 3 is included.

[0039] [Chemical Formula 3]

[0040] [(M) a' O b' ] x O c' (M * ) d' (R2) e'

[0041] Here, M and M* are each independently a 5-period metal, R2 is selected from a linear, branched or cyclic alkyl group, a linear, branched or cyclic alkenyl group and an aryl group, and a' ≥ 4, b' ≥ 8, c' ≥ 4, d' ≥ 8, e' ≥ 8, x ≥ 1.

[0042] At least one of the above M and M* may include Te.

[0043] Both M and M* above can be Te.

[0044] The above R2 may include a branched alkyl group or a halogenated alkyl group.

[0045] In an embodiment of the present invention, the contact angle with water is 60° or more.

[0046] In an embodiment of the present invention, when measuring infrared spectroscopy, 3200-3400 cm -1 In this case, there is no hydroxy peak.

[0047]

[0048] According to an embodiment of the present invention, a method for forming a photoresist thin film having an increased photon absorption rate of extreme ultraviolet light and excellent etching resistance can be provided.

[0049] The desired thickness of the thin film can be formed through the first precursor.

[0050] By sequentially depositing the first precursor and the second precursor, the film can exhibit hydrophobicity because it does not contain direct bonds between metal and hydroxyl groups.

[0051] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the detailed description of the present invention or the composition of the invention described in the claims.

[0052]

[0053] Figure 1 is a schematic diagram of a method for forming a photoresist thin film according to the present invention.

[0054] Figure 2 is an infrared spectroscopy (IR) analysis graph within the hydroxyl group (OH) peak range.

[0055]

[0056] Hereinafter, the present invention will be described with reference to the attached drawings. However, the present invention can be implemented in various different forms and is therefore not limited to the embodiments described herein. In the drawings, irrelevant parts have been omitted for clarity of description, and similar parts have been designated with similar reference numerals throughout the specification.

[0057] Throughout the specification, when a part is said to be "connected (connected, contacted, or coupled)" to another part, this includes not only cases where it is "directly connected," but also cases where it is "indirectly connected" with another part in between. Furthermore, when a part is said to "include" a component, this does not exclude other components, but rather implies that it may include other components, unless otherwise specifically stated.

[0058] The terminology used herein is merely used to describe specific embodiments and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this specification, it should be understood that the terms "comprises" or "has" indicate the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but do not exclude in advance the possibility of the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0059] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings.

[0060]

[0061] The term "substituted or unsubstituted" as used herein means a group that is unsubstituted or substituted with one or more substituents selected from the group consisting of deuterium; halogen; cyano group; nitro group; hydroxy group; carbonyl group; ester group; imide group; amide group; amino group; carboxyl group; sulfonic acid group; sulfonamide group; phosphine oxide group; alkoxy group; alkylcarbonyl group; alkoxycarbonyl group; sulfonyloxy group; aryloxy group; alkylthioxy group; arylthioxy group; alkylsulfoxy group; arylsulfoxy group; silyl group; boron group; aryl group; and heteroaryl group, or a group that is unsubstituted or substituted with two or more substituents among the above-mentioned substituents linked to each other.

[0062] In this specification, examples of halogen include fluorine, chlorine, bromine or iodine.

[0063] In the present specification, the ester group may have the oxygen of the ester group substituted with a straight-chain, branched-chain, or cyclic-chain alkyl group having 1 to 25 carbon atoms or an aryl group having 6 to 25 carbon atoms.

[0064] In the present specification, specific examples of alkyl groups include methyl, ethyl, propyl, n-propyl, isopropyl (iPr), butyl, n-butyl, isobutyl, tert-butyl (tBu), sec-butyl, 1-methyl-butyl, 1-ethyl-butyl, pentyl, n-pentyl, isopentyl, neopentyl, tert-pentyl, hexyl, n-hexyl, 1-methylpentyl, 2-methylpentyl, 4-methyl-2-pentyl, 3,3-dimethylbutyl, 2-ethylbutyl, heptyl, n-heptyl, 1-methylhexyl, cyclopentylmethyl, cyclohectylmethyl, octyl, n-octyl, tert-octyl, 1-methylheptyl, 2-ethylhexyl, 2-propylpentyl, n-nonyl, 2,2-dimethylheptyl, 1-ethyl-propyl, Examples thereof include, but are not limited to, 1,1-dimethyl-propyl, isohexyl, 2-methylpentyl, 4-methylhexyl, and 5-methylhexyl. The alkyl group may be substituted or unsubstituted, and examples of the substituent when substituted are as described above.

[0065] In this specification, an alkoxy group is a functional group in which the aforementioned alkyl group is bonded to one end of an ether group (-O-), and the description of the aforementioned alkyl group may be applied to these groups, except that they are functional groups bonded to an ether group (-O-). For example, the alkyl group may be linear, branched, or cyclic. The number of carbon atoms in the alkoxy group is not particularly limited, but may be 1 to 20 carbon atoms. Specifically, there are, but are not limited to, methoxy, ethoxy, n-propoxy, isopropoxy, i-propyloxy, n-butoxy, isobutoxy, tert-butoxy, sec-butoxy, n-pentyloxy, neopentyloxy, isopentyloxy, n-hexyloxy, 3,3-dimethylbutyloxy, 2-ethylbutyloxy, n-octyloxy, n-nonyloxy, n-decyloxy, cycloheptoxy, benzyloxy, p-methylbenzyloxy, etc. The alkoxy group may be substituted or unsubstituted, and when substituted, examples of the substituent are as described above.

[0066] In the present specification, the amine group may be selected from the group consisting of -NH2, a monoalkylamine group, a dialkylamine group, an N-alkylarylamine group, a monoarylamine group, a diarylamine group, an N-arylheteroarylamine group, an N-alkylheteroarylamine group, a monoheteroarylamine group, and a diheteroarylamine group, and the number of carbon atoms is not particularly limited, but may be 1 to 30. Specific examples of amine groups include, but are not limited to, a methylamine group, a dimethylamine group, an ethylamine group, a diethylamine group, a phenylamine group, a naphthylamine group, a biphenylamine group, anthracenylamine group, a 9-methyl-anthracenylamine group, a diphenylamine group, a ditolylamine group, an N-phenylbiphenylamine group, an N-phenylnaphthylamine group, an N-biphenylnaphthylamine group, a ditolylamine group, an N-phenyltolylamine group, a triphenylamine group, an N-naphthylfluorenylamine group, an N-phenylphenanthrenylamine group, an N-biphenylphenanthrenylamine group, an N-phenylfluorenylamine group, an N-phenylterphenylamine group, an N-phenanthrenylfluorenylamine group, an N-biphenylfluorenylamine group, and the like. The amine group may be substituted or unsubstituted, and when substituted, examples of the substituent are as described above.

[0067] In the present specification, the amide group may be a group in which hydrogen, a straight-chain alkyl group having 1 to 30 carbon atoms, a branched-chain alkyl group having 3 to 30 carbon atoms, a cyclic alkyl group having 3 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or a combination thereof, is bonded to the nitrogen of the amide group.

[0068]

[0069] Figure 1 is a schematic diagram of a method for forming a photoresist thin film according to the present invention.

[0070] Referring to Figure 1, a method for forming a hydrophobic photoresist thin film according to an embodiment of the present invention is described below.

[0071] A method for forming a hydrophobic photoresist thin film according to one embodiment of the present invention comprises the steps of: injecting a first precursor and an oxygen source into a chamber in which a substrate is positioned to form a thin film including a hydrophilic group; and injecting a second precursor to modify the thin film including the hydrophilic group, thereby forming a modified layer. The first step is a step of forming a thin film including a hydrophilic group by injecting a first precursor and an oxygen source into a chamber in which a substrate is positioned.

[0072] After forming the thin film including the hydrophilic group, a step of supplying a purge gas to the chamber to remove the unreacted oxygen source may be further included.

[0073] The thin film including the hydrophilic group includes a hydroxyl group.

[0074] The above first precursor includes a structure represented by the following chemical formula 1 and can be represented by the following chemical formula 1.

[0075] [Chemical Formula 1]

[0076] (R1) a -M-(L) d

[0077] Here, a and d are integers, 0≤a≤5, 0≤d≤5, 0 <a+d<5를 만족하고, M은 5주기 금속이고, R1은 선형, 분지형 또는 고리형의 알킬기, 선형, 분지형 또는 고리형의 알케닐기 및 아릴기 중에 선택되는 것이며, L은 가수분해 가능한 리간드이다.

[0078] More specifically, a can be an integer from 0 to 4, and d can be an integer from 0 to 4. Specifically, when a+d=4, more specifically, when a=0, d=4, and when a=1, d=3.

[0079] Specifically, the M may be any one metal selected from among Te, Sb, Sn, and In among the 5th period metals. More specifically, the M may be Te or Sn. In the photoresist, the higher the absorbance, the better the sensitivity, and in this respect, the order of In, Sn, Sb, and Te may be excellent.

[0080] R1 may be selected from a linear, branched or cyclic alkyl group, a linear, branched or cyclic alkenyl group and an aryl group.

[0081] Specifically, the R1 is selected from hydrogen, a substituted or unsubstituted linear alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted branched alkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted cyclic alkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 30 carbon atoms.

[0082] Alkyl and aryl groups can be halogenated. In this case, the precursor is -(CH2) n CF3, -(CH2) n I, -(CH2) m It has functional groups such as CHCH2, but these are exemplary and not limited thereto.

[0083] Alkyl groups have the characteristic of being advantageous for bonding with metals when exposed to extreme ultraviolet light. Branched alkyl groups exhibit greater bonding with metals, potentially enhancing sensitivity. In the absence of R1, the group exhibits excellent reactivity with water, which can be advantageous for forming metal oxide films.

[0084] That is, when R1 is unsubstituted, the more branched the alkyl group, the more favorable the bonding with the metal during EUV exposure, resulting in superior sensitivity. Specifically, sensitivity may be superior when it is isopropyl or tert-butyl, and more specifically, sensitivity may be superior when it is tert-butyl.

[0085]

[0086] An alkenyl group is a straight-chain or branched-chain aliphatic hydrocarbon group, and refers to an aliphatic unsaturated alkenyl group containing one or more double bonds.

[0087] An aryl group is a substituent in which all atoms of a cyclic substituent have p-orbitals, and these p-orbitals form conjugation, and may include a monocyclic or fused ring polycyclic (i.e., a ring that shares adjacent pairs of carbon atoms) functional group.

[0088] In the case of aryl groups, the effect may be similar to that of linear alkyls.

[0089] L is a hydrolyzable ligand that can be selected from an ester group, an amine group, an amide group, an alkoxy group, a carbonyl group, and an aldehyde group.

[0090] Specifically, the ester group may be selected from a formate group, an acetyl group, a propionate group, and a phenyl acetate group.

[0091] Specifically, the amine group may be selected as a dialkylamine group. More specifically, the amine group may be selected as a dimethylamine group.

[0092] At this time, the amine group may have the best reactivity with water.

[0093] The above oxygen source may be one selected from water, oxygen, ozone and hydrogen peroxide.

[0094] The first precursor deposition is performed through the chemical vapor deposition (CVD) process. This process can be categorized into heat, plasma, and light, depending on the external energy used in CVD. This process involves placing a wafer in a vacuum chamber, sealed from the outside world, and supplying a gas containing the raw materials for the desired thin film. This process deposits a thin film without altering the substrate's properties through plasma, heat, or other factors.

[0095] In the step of depositing the first precursor, oxide particles are formed at intervals and are physically or chemically adsorbed.

[0096] The above first precursor can control the thickness of the photoresist thin film.

[0097] After the above step, a purge step can be further performed, and the purge step is a step of supplying a purge gas to the chamber to remove the unreacted oxygen source.

[0098]

[0099] The next step is to form a modified layer by introducing a second precursor to modify the thin film containing the hydrophilic group. After forming the modified layer, a step of supplying a purge gas to the chamber to remove unreacted second precursor may be further included.

[0100] The step of forming the above modified layer does not include a reactant.

[0101] The above second precursor includes a structure represented by the following chemical formula 2 and can be represented by the following chemical formula 2.

[0102]

[0103] [Chemical Formula 2]

[0104] (R2) b -M * -(L1) e

[0105] Here, 1≤b≤5, 0≤e≤5, 1≤b+e≤5, b and e are integers, and M * is a 5-period metal, R2 is selected from a linear, branched or cyclic alkyl group, a linear, branched or cyclic alkenyl group and an aryl group, and L1 is a hydrolyzable ligand.

[0106] Specifically, when b is an integer from 0 to 4, e can be an integer from 0 to 4. More specifically, b+e=4. When b=3, e=1. Also, b+e=2. When b=1, e=1.

[0107] Above M * M* may be any one metal selected from Te, Sb, Sn, and In among the 5th period metals. More specifically, M* may be Sn and Te.

[0108] The above M and M* may be the same or different. At least one of the above M and M* may include Sn. At least one of the above M and M* may include Te. Both the above M and M* may be Te. Specifically, when M is Sn, M* may be Te. When M is Te, M* may be Sn. When M is Te, M* may be Te. When M is Sn, M* may be Sn. In a photoresist, the higher the absorbance, the better the sensitivity, and in this respect, the order of In, Sn, Sb, and Te may be excellent.

[0109] In photoresists, the higher the absorbance, the better the sensitivity, and in this respect, ln, Sn, Sb, and Te are excellent in that order.

[0110] The above R2 may be selected from a linear, branched or cyclic alkyl group, a linear, branched or cyclic alkenyl group and an aryl group. In addition, when R2 includes a halogenated alkyl group or a branched alkyl group, the sensitivity may be excellent.

[0111] Specifically, R2 is selected from hydrogen, a substituted or unsubstituted linear alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted branched alkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted cyclic alkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 30 carbon atoms.

[0112] Specifically, R2 may comprise a branched alkyl group or a halogenated alkyl group.

[0113] More specifically, R2 may comprise tert-butyl or -CH2CH2I.

[0114]

[0115] Alkyl groups have the characteristic of being advantageous in bonding with metals when exposed to extreme ultraviolet light. In this case, bonding with metals is advantageous when the alkyl group is branched rather than linear or cyclic.

[0116] An alkenyl group is a straight-chain or branched-chain aliphatic hydrocarbon group, and refers to an aliphatic unsaturated alkenyl group containing one or more double bonds.

[0117] An aryl group is a substituent in which all atoms of a cyclic substituent have p-orbitals, and these p-orbitals form conjugation, and may include a monocyclic or fused ring polycyclic (i.e., a ring that shares adjacent pairs of carbon atoms) functional group.

[0118] In the case of aryl groups, the effect may be similar to that of linear alkyls.

[0119] L1 is a hydrolyzable ligand that can be selected from an ester group, an amine group, an amide group, an alkoxy group, a carbonyl group, and an aldehyde group.

[0120] Specifically, the ester group may be selected from a formate group, an acetyl group, a propionate group, and a phenyl acetate group.

[0121] Specifically, the amine group may be selected as a dialkylamine group. More specifically, the amine group may be selected as a dimethylamine group.

[0122] L1 is removed by hydrolysis reaction during thin film formation.

[0123] In the step of depositing the second precursor, the second precursor may penetrate into the gap to remove the hydroxo moiety and form a side chain.

[0124] The second precursor can retain oxo and remove hydroxo. As a result, the final thin film formed exhibits hydrophobicity.

[0125] The ALD (Atomic Layer Deposition) process involves precursor supply, purge, reactant supply, and purge, and then undergoes a deposition process. However, the present invention performs only the precursor supply and purge steps without the inclusion of reactants. This process can improve sensitivity and storage stability.

[0126] In this case, if the reactant is injected and the purging process is further performed, a metal oxide film is formed.

[0127]

[0128] According to the present invention, a process of forming a thin film including a hydrophilic group by introducing a first precursor and an oxygen source into a chamber where a substrate is located, purging, introducing a second precursor to modify the thin film including the hydrophilic group to form a modified layer, and purging is defined as one cycle, and such cycle can be repeated 5 to 300 times. The hydrophobic photoresist thin film thus deposited can be formed to have a thickness in the range of 10 to 600 nm. If the thickness of the thin film is controlled to be thin, it can be used not only as a photoresist thin film but also as an underlying film.

[0129]

[0130] A photoresist thin film according to one embodiment of the present invention can be formed according to the above-described forming method, and can also be formed by a method other than the above-described forming method.

[0131] The above photoresist thin film includes a structure represented by the following chemical formula 3 and can be represented by the following chemical formula 3.

[0132] [Chemical Formula 3]

[0133] [(M) a' O b' ] x O c' (M * ) d' (R2) e'

[0134] Here, M and M* are each independently a 5-period metal, R2 is selected from a linear, branched or cyclic alkyl group, a linear, branched or cyclic alkenyl group and an aryl group, and a' ≥ 4, b' ≥ 8, c' ≥ 4, d' ≥ 8, e' ≥ 8, x ≥ 1.

[0135] The above M and M* may each independently be any one metal selected from Te, Sb, Sn, and In among the 5th period metals. In the photoresist, the higher the absorbance, the better the sensitivity, and in this respect, In, Sn, Sb, and Te may be superior in that order.

[0136] Specifically, when M is selected from Sn and Te, M* can be selected from Sn and Te.

[0137] The above M and M* may include at least Te.

[0138] More specifically, when M is Sn, M* can be Sn, when M is Sn, M* can be Te, when M is Te, M* can be Te, and when M is Te, M* can be Sn.

[0139] The above R2 may be selected from a linear, branched or cyclic alkyl group, a linear, branched or cyclic alkenyl group and an aryl group.

[0140] R2 is selected from hydrogen, a substituted or unsubstituted linear alkyl group having 1 to 20 carbon atoms, a substituted or unsubstituted branched alkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted cyclic alkyl group having 3 to 20 carbon atoms, a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 30 carbon atoms.

[0141] Specifically, R2 may comprise a branched alkyl group or a halogenated alkyl group.

[0142] More specifically, R2 may comprise a tert-butyl group (tBu) or -CH2CH2I.

[0143] a' ≥ 4, b' ≥ 8, c' ≥ 4, d' ≥ 8, e' ≥ 8, x ≥ 1.

[0144] Specifically, a' ≥ 12, b' ≥ 24, c' ≥ 12, d' ≥ 24, e' ≥ 24, x ≥ 3.

[0145] More specifically, 12≤a'≤80, 24≤b'≤160, 12≤c'≤80, 24≤d'≤160, 24≤e'≤480, 3 ≤ x ≤ 20.

[0146]

[0147] The above [chemical formula 3] may have a repeating unit as in the following [chemical formula 4] as an example.

[0148] [Chemical Formula 4]

[0149]

[0150]

[0151] At this time, b is an integer from 1 to 3.

[0152] The repeating unit of the above [chemical formula 4] can grow in the transverse direction, the longitudinal direction, or both directions.

[0153] The following [Chemical Formula 5], [Chemical Formula 6], [Chemical Formula 7], and [Chemical Formula 8] are examples of thin film structures when x=1, x=2, x=3, and x=4, respectively. The form in which the thin film grows is not limited to this, and various modifications are possible. The bond angles for each atom may be different.

[0154] [Chemical Formula 5]

[0155]

[0156]

[0157] [Chemical Formula 6]

[0158]

[0159]

[0160] [Chemical Formula 7]

[0161]

[0162]

[0163] [Chemical Formula 8]

[0164]

[0165]

[0166] The photoresist thickness of the present invention may be 5 nm to 30 nm (50 Å to 300 Å). In [Chemical Formula 3], when a'=4, b'=4, c'=8, d'=8, e'=8 or 16 or 24, it may be expressed in the form of [Chemical Formula 4]. When X=1, the length of the unit body may be 1.6 nm to 2.0 nm.

[0167]

[0168] The contact angle of the above photoresist thin film with water can be 60° or more. R2 must be present for extreme ultraviolet photoreaction. The contact angle refers to the angle between the water droplet and the solid interface when water is dropped on the solid. When the contact angle is small, it has high wettability and hydrophilicity, and when the contact angle is large, it has low wettability and hydrophobicity.

[0169] In general, the contact angle of a metal oxide film is hydrophilic and lower than 50°. However, the thin film according to the present invention exhibits hydrophobicity, which is low wettability, with a contact angle of 60° or higher.

[0170] In the case of the photoresist thin film according to the present invention, since it does not contain a direct bond between a metal and a hydroxyl group, the infrared spectroscopy measurement shows a wavelength of 3200-3400 cm -1 In this case, a hydroxy peak may not exist. This means that the photoresist thin film according to the present invention exhibits hydrophobicity.

[0171]

[0172] Hereinafter, embodiments and experimental examples of the present invention will be described in detail. However, the following examples are intended only to illustrate the present invention and are not intended to limit the invention to these embodiments.

[0173]

[0174] <Example 1>

[0175] A first precursor (MeSn(OCOEt)3) and water were simultaneously injected into a chamber where a silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, a second precursor (Me2(tBu)Sn(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0176]

[0177] <Example 2>

[0178] The first precursor (MeSn(OCOEt)3) and water were simultaneously injected into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor (Me2(CH2CH2I)Sn(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0179]

[0180] <Example 3>

[0181] The first precursor (MeSn(OCOEt)3) and water were simultaneously injected into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor ((nBu)3Sn(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0182]

[0183] <Example 4>

[0184] The first precursor (MeSn(OCOEt)3) and water were simultaneously injected into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor ((nBu)2(CH2CH2I)Sn(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0185]

[0186]

[0187] <Example 5>

[0188] The first precursor (MeSn(OCOEt)3) and water were simultaneously introduced into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor (tBuSn(NMe2)) was introduced for 20 seconds and purged. This process was performed 300 cycles.

[0189]

[0190] <Example 6>

[0191] The first precursor (iPrSn(OCOEt)3) and water were simultaneously injected into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor (Me2(tBu)Sn(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0192]

[0193] <Example 7>

[0194] The first precursor (tBuSn(OCOEt)3) and water were simultaneously injected into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor (Me2(tBu)Sn(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0195]

[0196] <Example 8>

[0197] The first precursor (C3H4Sn(OCOEt)3) and water were simultaneously injected into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor (Me2(tBu)Sn(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0198]

[0199] <Example 9>

[0200] The first precursor (C7H7Sn(OCOEt)3) and water were simultaneously injected into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor (Me2(tBu)Sn(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0201]

[0202] <Example 10>

[0203] The first precursor (tBuSn(OC(CH3)2Et)3) and water were simultaneously injected into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor (Me2(tBu)Sn(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0204]

[0205] <Example 11>

[0206] The first precursor (MeSn(NH2)3) and water were simultaneously injected into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor (Me2(tBu)Sn(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0207]

[0208] <Example 12>

[0209] The first precursor (MeTe(OCOEt)3) and water were simultaneously injected into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor (Me2(tBu)Sn(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0210]

[0211] <Example 13>

[0212] The first precursor (MeSn(OCOEt)3) and water were simultaneously injected into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor (Me2(tBu)Te(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0213]

[0214] <Example 14>

[0215] The first precursor (MeTe(OCOEt)3) and water were simultaneously introduced into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor (Me2(tBu)Te(NMe2)) was introduced for 20 seconds and purged. This process was performed 300 cycles.

[0216]

[0217] <Example 15>

[0218] The first precursor (Sn(NH2)4) and water were simultaneously injected into the chamber where the silicon wafer substrate was located at a temperature of 50°C to 100°C (preferably 75°C) for 15 seconds and purged. Thereafter, the second precursor (Me2(tBu)Sn(NMe2)) was injected for 20 seconds and purged. This process was performed 300 cycles.

[0219]

[0220] <Comparative Example 1>

[0221] In the process of introducing the second precursor, the process was performed as a process including a reactant, rather than an example process that did not include a reactant, and other conditions were the same as in Example 1.

[0222]

[0223] Comparative Example 2

[0224] The first precursor (MeSn(OCOEt)3) was used as a single precursor without a second precursor, and other conditions were the same as in Example 1.

[0225]

[0226] <Comparative Example 3>

[0227] In the process of introducing the second precursor, the process was performed as a process including a reactant, rather than an example process that did not include a reactant, and other conditions were the same as in Example 13.

[0228]

[0229] <Experimental Example>

[0230] The results of the experimental evaluation of the present invention are shown in Table 1 below.

[0231]

[0232] Thin film thickness (nm) Contact angle sensitivity with water (mJ / cm) -1 )Hydroxy peak Example 124.772.414.78O Example 2258914.69O Example 3258314.93O Example 424.88814.84O Example 524.975.214.61O Example 623.977.614.69O Example 724.578.114.59O Example 824.976.914.65O Example 924.879.214.81O Example 1025.178.514.76O Example 112577.914.75O Example 1225.379.314.37O Example 1325.278.414.39O Example 1424.878.114.31O Example 152578.114.58O Comparative Example 125.235 Not Evaluable X Comparative Example 225.13715.04 X Comparative Example 325.342.3 Not Evaluable X

[0233]

[0234] <Experimental Example 1> Thin Film Thickness Measurement

[0235] The thickness of the photoresist thin film produced by performing the processes of Examples 1 to 15 and Comparative Examples 1 to 3 was measured using an ellipsometer, and the measured thickness was approximately 20 to 30 nm.

[0236]

[0237]

[0238] <Experimental Example 2> Water contact angle

[0239] Typically, the contact angle of a metal oxide film is lower than 50°. However, the photoresist film according to the present invention has a contact angle of 60° or higher. The film of the present invention exhibits relatively hydrophobicity compared to a metal oxide film because the hydroxo is removed and an alkyl chain is present in the side chain portion.

[0240]

[0241] <Experimental Example 3> Coating properties and sensitivity

[0242] The photoresist thin films produced by performing the processes of Examples 1 to 15 and Comparative Examples 1 to 3 were exposed to EUV radiation. After exposure, they were baked at 170°C for 120 seconds (post-exposure bake, PEB). The baked thin films were immersed in a developer and washed to form negative tone images. The residual resist thickness was measured using an elipsometer, and the sensitivity (Dose to gel) for each type of resist is shown in Table 1. Referring to Table 1, Examples 1 to 15 had superior sensitivity to Comparative Example 2, which performed the CVD process using only a single precursor.

[0243] Example 15 did not include a reactant in the step of forming a modified layer, and thus had a better sensitivity than Comparative Example 3, which included a reactant in the step of forming a modified layer.

[0244] In photoresists, the higher the absorbance, the better the sensitivity. In this respect, the order of excellence is ln, Sn, Sb, and Te. Examples 12 to 14, which include Te among the metals, had better sensitivity than Example 1, which includes only Sn among the metals.

[0245] Comparative Examples 1 and 3 were performed including the reactant, so a metal oxide film without an alkyl group to photoreact was formed, making it impossible to evaluate sensitivity.

[0246]

[0247] <Experimental Example 4> Infrared Spectroscopy (IR) Analysis

[0248] The results of infrared spectroscopy (IR) analysis performed on photoresist thin films produced by performing the processes of Examples 1 to 15 and Comparative Examples 1 to 3 at room temperature (typically, 15 to 25°C) using a Bruker Vertex 70 device are shown in Table 1 and Fig. 2.

[0249] Examples 1 to 15 are 3200 cm -1 ~ 3400cm -1 In Table 1 below, no hydroxy peak was observed, and Comparative Examples 1 to 3 showed the presence of a hydroxy peak.

[0250] Figure 2 is an IR analysis graph of Example 1 and Comparative Example 2. The hydroxo peak is 3232.36 cm -1 , and Example 1 is represented by a solid line, and Comparative Example 2 is represented by a dotted line. Example 1 uses the first precursor (MeSn(OCOEt)3) and the second precursor (Me2(tBu)Sn(NMe2)), and Comparative Example 2 uses the first precursor (MeSn(OCOEt)3) as a single precursor without the second precursor.

[0251] Referring to Figure 2, the IR analysis results show that the photoresist thin film according to the present invention has a range of hydroxy peaks (wavelength 3232.36 cm -1 ) can be confirmed that no peak appears within the sample. This indicates that the hydroxyl group has been removed.

[0252]

[0253] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will readily appreciate that the present invention can be readily modified into other specific forms without altering the technical spirit or essential characteristics of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single entity may be implemented in a distributed manner, and similarly, components described as distributed may be implemented in a combined manner.

[0254] The scope of the present invention is indicated by the claims described below, and all changes or modifications derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.

Claims

1. A step of forming a thin film including a hydrophilic group on the substrate by injecting a first precursor and an oxygen source into a chamber where the substrate is located; and A method for forming a hydrophobic photoresist thin film, comprising a step of forming a modified layer by modifying a thin film including the hydrophilic group by introducing a second precursor.

2. In paragraph 1, A method for forming a hydrophobic photoresist thin film, further comprising the step of supplying a purge gas to the chamber after forming a thin film including the hydrophilic group to remove the unreacted oxygen source.

3. In paragraph 1, A method for forming a hydrophobic photoresist thin film, further comprising a step of supplying a purge gas to the chamber after forming the modified layer to remove unreacted second precursor.

4. In paragraph 1, A method for forming a hydrophobic photoresist thin film, wherein the step of forming the above-mentioned modified layer does not include a reactant.

5. In paragraph 1, A method for forming a hydrophobic photoresist thin film, wherein the thin film including the hydrophilic group includes a hydroxyl group.

6. In paragraph 1, A method for forming a hydrophobic photoresist thin film, wherein the first precursor comprises a structure represented by the following chemical formula 1: [Chemical Formula 1] (R1) a -M-(L) d (Here 0≤a≤5, 0≤d≤5, 0 <a+d<5, a와 d는 정수이고, M은 5주기 금속이고, R1은 선형, 분지형 또는 고리형의 알킬기, 선형, 분지형 또는 고리형의 알케닐기 및 아릴기 중에 선택되는 것이며, L은 각각 독립적으로 가수분해 가능한 리간드이다.).

7. In paragraph 6, A method for forming a hydrophobic photoresist thin film, wherein the above M is any one metal selected from Te, Sb, Sn, and In.

8. In paragraph 6, A method for forming a hydrophobic photoresist thin film, wherein the above L is selected from an ester group, an amine group, an amide group, an alkoxy group, a carbonyl group, and an aldehyde group.

9. In paragraph 6, A method for forming a hydrophobic photoresist thin film, wherein the above R1 comprises a branched alkyl group.

10. In paragraph 1, A method for forming a hydrophobic photoresist thin film, wherein the second precursor comprises a structure represented by the following chemical formula 2: [Chemical Formula 2] (R2) b -M * -(L1)e (Here, 1≤b≤5, 0≤e≤5, 1≤b+e≤5, b and e are integers, and M * is a 5-period metal, R2 is selected from a linear, branched or cyclic alkyl group, a linear, branched or cyclic alkenyl group and an aryl group, and L1 is a hydrolyzable ligand.

11. In paragraph 10, Above M * A method for forming a hydrophobic photoresist thin film, wherein the metal is one selected from Te, Sb, Sn and In.

12. In paragraph 10, A method for forming a hydrophobic photoresist thin film, wherein the above L1 is selected from an ester group, an amine group, an amide group, an alkoxy group, a carbonyl group, and an aldehyde group.

13. In paragraph 1, A method for forming a hydrophobic photoresist thin film, wherein the oxygen source is one selected from water, oxygen, ozone, and hydrogen peroxide.

14. In either of paragraph 6 or paragraph 10, A method for forming a hydrophobic photoresist thin film, wherein at least one of the above M and M* comprises Te.

15. In paragraph 14, A method for forming a hydrophobic photoresist thin film, wherein both M and M* are Te.

16. A hydrophobic photoresist thin film comprising a structure represented by the following chemical formula 3: [Chemical Formula 3] [(M) a' O b' ] x O c' (M * ) d' (R2) e' Here, M and M* are each independently a 5-period metal, R2 is selected from a linear, branched or cyclic alkyl group, a linear, branched or cyclic alkenyl group and an aryl group, and a'≥4, b'≥8, c'≥4, d'≥8, e'≥8, x≥1.

17. In paragraph 16, A hydrophobic photoresist thin film with a contact angle with water of 60° or more.

18. In paragraph 16, 3200-3400cm when measured by infrared spectroscopy -1 A hydrophobic photoresist thin film in which no hydroxy peak exists.

19. In paragraph 16, A hydrophobic photoresist thin film, wherein the above R2 comprises a tert-butyl group or -CH2CH2I.

20. In paragraph 16, A hydrophobic photoresist thin film, wherein at least one of the above M and M* comprises Te.

21. In paragraph 20, A hydrophobic photoresist thin film in which both M and M* are Te.

Citation Information

Patent Citations

  • Metal oxide layer composition control by atomic layer deposition for thin film transistor

    KR1020150113041A

  • Organometallic solution based high resolution patterning compositions

    KR1020160082969A

  • Apparatus, Method, and Computer-Readable Recording Medium for Enhancing Memory Using Picture Data

    KR1020220128576A

  • Electronic device including a waterproof structure

    KR1020230039400A

  • Extreme Ultraviolet Lithography Patterning Method

    US20230054125A1