Catalytic system for oxidizing ammonia (embodiments) and method of manufacturing same
The catalytic system for ammonia oxidation, featuring treated activated meshes, addresses the issue of platinum group metal losses by stabilizing gas flow and enhancing surface capture, thereby extending service life and maintaining efficiency.
Patent Information
- Application Number
- PCT/RU2024/050104
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-05-18
- Publication Date
- 2024-11-28
AI Technical Summary
Existing catalytic systems for ammonia oxidation suffer from significant mechanical losses of platinum group metals due to chemical and mechanical degradation, leading to reduced service life and efficiency, despite efforts to mitigate these losses through the use of catchers and anti-pulsation gaskets which often compromise catalytic activity.
A catalytic system comprising platinum-based catalyst meshes and palladium-based catching meshes, with activated meshes made from heat-resistant high-alloy or nichrome alloys, where the activated meshes are treated to enhance surface roughness and platinoid capture, stabilizing gas flow and reducing mechanical stress on the catalyst grids.
The solution significantly reduces platinum group metal losses, extends the service life of the catalytic system, maintains high ammonia conversion efficiency, and achieves uniform gas flow distribution, resulting in a longer operational run without increased precious metal investment.
Smart Images

Figure IMGF000017_0001 
Figure IMGF000025_0001 
Figure IMGF000026_0001
Abstract
Description
[0001] Catalytic system for ammonia oxidation (variants) and its manufacturing method
[0002] Field of technology
[0003] The claimed group of inventions relates to the field of catalytic elements, in particular to variants of catalytic systems that are used for the conversion of ammonia from a gas phase containing oxygen in units for producing nitric and hydrocyanic acids, as well as hydroxylamine sulfate.
[0004] State of the art
[0005] The catalytic system consists of a package of platinum-based catalytic grids and a package of palladium-based catching grids. The catalytic grids participate in the catalytic oxidation of ammonia, the catching grids are located downstream of the gas flow under the catalytic grids and catch sublimating platinum and rhodium from the catalytic grids, and also oxidize the ammonia that has not reacted on the catalytic grids. During operation of the catalytic system, inevitable chemical losses of precious metals occur, which cause the destruction of the catalytic and catching grids, which leads to mechanical losses of precious metals in the form of particles and wire fragments and, as a consequence, to a reduction in the service life.With an increase in the productivity of the units, the service life and a decrease in the platinum group inputs into the catalyst and catching grids, there is a sharp increase in the losses of platinum metals due to an increase in chemical losses, which lead to the weakening of the grids and an increase in mechanical losses in the form of particles and wire fragments. Reducing the losses of platinum metals while maintaining their efficiency throughout the entire run has always been an urgent task. The solution to this problem was carried out in several main directions, in particular, the use of platinum metal catchers and devices for equalizing the gas flow over the entire surface area of the grid.
[0006] In order to reduce losses of platinum group metals, the Russian patent No. RU 2392048 (“Platinum group metal trap from a gas mixture”, patent holder Valery Ivanovich Chernyshev, B01J 23 / 44, B01J 20 / 10, BOID 53 / 86, published 20.06.2010, [1]) describes the use of soft gaskets made of a gas-permeable material based on silicon oxide with a gasket thickness of 2-80 times the diameter of the wire of the trapping mesh, which are placed between the trapping and heat-resistant meshes. This arrangement of soft gaskets allows to significantly reduce the negative effects of turbulent pulsations of the gas flow passing through the grids, and thus prevent the rupture of the catching grids in the catcher package into separate pieces, which leads to the exclusion of ammonia breakthrough and, as a consequence, ensures the concentration of ammonia in the gas mixture behind the catcher package at an explosion-proof level of less than 0.03 vol.%.
[0007] The disadvantage of this solution is that a significant part of the active surface of the collecting grids is covered by more than 60% soft gaskets, which leads to a 2-3-fold decrease in the degree of collecting platinum and rhodium evaporating from the catalyst grids, and to increased losses of precious metals.
[0008] The closest solution for reducing mechanical losses of platinum group metals from catalyst gauzes is Russian patent No. RU 2155097 (“Catalytic element for ammonia conversion”, patent holder Pavel Ivanovich Khalzov, Vladimir Nikolaevich Zvyagin, Vladimir Andreevich Bokiy, Yuriy Yemelyanovich Volodin, published 08 / 27 / 2000, [2]), which describes the use of a catalytic element for ammonia conversion in the form of a package of mesh platinum group metals with separating anti-pulsation spacers made of non-metallic materials based on silica fiber, modified with an active phase based on platinum, or palladium, or chromium oxide, or cobalt oxide. The main function of the separating spacers is anti-pulsation protection of the platinum group catalyst gauzes, which help reduce losses of platinum group metals by acting as a kind of damper (shock absorber).
[0009] The disadvantage of the said catalytic element, revealed by the results of the analysis of the operational characteristics of the catalytic systems and the analysis of the surface of the spent catalyst gauzes on a scanning electron microscope, is the overlap of a significant part of the active surface of the catalyst gauzes up to 50-60% with silica inert fibers of the gasket material, which leads to a decrease in the degree of ammonia conversion and increased losses of precious metals from the remaining open surface of the catalyst gauzes, which experiences high tension and ammonia load per unit area. Subsequently, this disadvantage played a major role in the refusal to use anti-pulsation gaskets based on silica material between the catalyst gauzes.
[0010] Taking into account the above-mentioned shortcomings, the task was set to increase the strength of catalyst gauzes by reducing the mechanical losses of platinum group metals from precious metal gauzes while maintaining the high catalytic activity of these gauzes.
[0011] Disclosure of invention
[0012] The technical result provided by each invention is a reduction in the loss of platinum group metals from the catalytic system in ammonia oxidation units, which makes it possible to reduce the loss of platinum group metals and increase the service life while maintaining a high degree of conversion without increasing the investment of precious metals.
[0013] Another technical result is the equalization of the gas flow.
[0014] To achieve the stated technical result, a catalytic system for the oxidation of ammonia is proposed, which is distinguished by the fact that it contains the following installed along the gas flow:
[0015] - a catalyst mesh or a stack of catalyst meshes made of a first platinum-based alloy or a second platinum-based alloy,
[0016] - an activated mesh or a package of activated meshes; wherein the activated meshes are made of woven wire with a diameter of 0.07-3.00 mm, the material of the activated meshes is heat-resistant high-alloy or precision steel, or nichrome alloys; the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 0.1 wt. % to 50 wt. %, wherein the second alloy is made on the basis of a triple platinum-palladium-rhodium system with a palladium content from 0.1 wt. % to 95 wt. % and rhodium from 1 wt. % to 50 wt. %.
[0017] The double platinum-rhodium system is understood to be an alloy containing two main components (platinum and rhodium) and inevitable impurities (for example, palladium, iridium, etc., no more than 1 wt.%).
[0018] The triple platinum-palladium-rhodium system is an alloy containing three main components (platinum, palladium and rhodium) and inevitable impurities (for example, iridium, etc., no more than 1 wt.%).
[0019] A net pack is a set of 2 or more nets.
[0020] Preferably, the first alloy is made on the basis of a binary platinum-rhodium system with a rhodium content of 3 May % to 12 May %, preferably from 4 May % to 10 May %, while the second alloy is made on the basis of a ternary platinum-palladium-rhodium system with a palladium content of 3 May % to 70 %, preferably from 3 May % to 60 May %, and rhodium of 1 May % to 10 May %, preferably from 2 May % to 6 May %.
[0021] Preferably, the activated grids are made of intertwined wires with a diameter of 0.07-1.0 mm, preferably 0.15-0.41 mm, with the formation of cells in such a way that when the activated grid is illuminated, light penetrates no more than 15% of the total area of the grid, preferably no more than 10% of the total area of the grid. In this case, the area of the grid is understood to be its area obtained by multiplying the length by the width.
[0022] Preferably, the system additionally contains the following installed along the gas flow:
[0023] - a catalyst mesh or a package of catalyst meshes made of a second platinum-based alloy,
[0024] - an activated grid or a package of activated grids.
[0025] Preferably, the system further comprises a palladium-based catching grid package installed along the gas flow path and an activated grid or a package of activated grids.
[0026] Also, to achieve the stated technical result, a catalytic system for the oxidation of ammonia is proposed, which is distinguished by the fact that it contains the following installed along the gas flow:
[0027] - a catalyst mesh or a package of catalyst meshes made of the first platinum-based alloy,
[0028] - a catalyst mesh or a package of catalyst meshes made of a second platinum-based alloy,
[0029] - an activated grid or a package of activated grids,
[0030] - a package of palladium-based trapping grids,
[0031] - an activated mesh or a package of activated meshes; wherein the activated meshes are made of woven wire with a diameter of 0.07-3.00 mm, the material of the activated meshes is heat-resistant high-alloy or precision steel, or nichrome alloys; the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 0.1% to 50%, wherein the second alloy is made on the basis of a triple platinum-palladium-rhodium system with a palladium content from 0.1 wt. % to 95 wt. % and rhodium from 1 wt. % to 50 wt. %.
[0032] Preferably, the first alloy is made on the basis of a binary platinum-rhodium system with a rhodium content of 3 May % to 12 May %, preferably from 4 May % to 10 May %, while the second alloy is made on the basis of a ternary platinum-palladium-rhodium system with a palladium content of 3 May % to 70 May %, preferably from 3 May % to 60 May %, and rhodium of 1 May % to 10 May %, preferably from 2 May % to 6 May %.
[0033] Preferably, the activated grids are made of intertwined wires with a diameter of 0.07-1.0 mm, preferably 0.15-0.41 mm, with the formation of cells in such a way that when the activated grid is illuminated, light penetrates through no more than 15% of the total area of the grid, preferably no more than 10% of the total area of the grid. In this case, the area of the grid is understood to be its area obtained by multiplying the length by the width.
[0034] Also, to achieve the stated technical result, a catalytic system for the oxidation of ammonia is proposed, which is distinguished by the fact that it contains the following installed along the gas flow:
[0035] - a catalyst mesh or a package of catalyst meshes made of the first platinum-based alloy,
[0036] - a catalyst mesh or a package of catalyst meshes made of a second platinum-based alloy,
[0037] - a palladium-based collecting mesh package, - an activated mesh or a package of activated meshes; wherein the activated meshes are made of woven wire with a diameter of 0.07-3.00 mm, the material of the activated meshes is heat-resistant high-alloy or precision steel, or nichrome alloys; the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 0.1 May % to 50 May %, wherein the second alloy is made on the basis of a ternary platinum-palladium-rhodium system with a palladium content from 0.1 May % to 95 May % and rhodium from 1 May % to 50 May %.
[0038] Preferably, the first alloy is made on the basis of a binary platinum-rhodium system with a rhodium content of 3 May % to 12 May %, preferably from 4 May % to 10 May %, while the second alloy is made on the basis of a ternary platinum-palladium-rhodium system with a palladium content of 3 May % to 70 May %, preferably from 3 May % to 60%, and rhodium of 1 May % to 10 May %, preferably from 2 May % to 6 May %.
[0039] Preferably, the activated grids are made of intertwined wires with a diameter of 0.07-1.0 mm, preferably 0.15-0.41 mm, with the formation of cells in such a way that when the activated grid is illuminated, light penetrates no more than 15% of the total area of the grid, preferably no more than 10% of the total area of the grid. In this case, the area of the grid is understood to be its area obtained by multiplying the length by the width.
[0040] Also, to achieve the stated technical result, a method for manufacturing the above-mentioned catalytic system for oxidizing ammonia is proposed, characterized in that, in order to obtain an activated mesh, the mesh surface is fired with a hydrogen or nitric-hydrogen, or propane flame, or the meshes are heat-treated at a temperature of 150-600°C, then the surface of the activated mesh is etched in a solution of sulfuric or hydrochloric acid, or nitric acid, or a mixture of hydrochloric and nitric acids, at a temperature of 20-90°C for 0.25-20 minutes with stirring, or processed by electrochemical etching with stirring.
[0041] Preferably, the surface of the activated mesh is etched in a solution with a hydrochloric acid concentration of 1-36% at a temperature of 20-90°C for 0.25-20 min with stirring.
[0042] Preferably, the surface of the activated mesh is etched in a solution of a mixture of hydrochloric and nitric acid with a total concentration of 1-50% at a temperature of 20-90°C for 0.10-20 min with stirring.
[0043] Preferably, the surface of the activated mesh is treated by electrochemical etching at a temperature of 20-80°C for 0.25-20 min with stirring.
[0044] Preferably, after etching, the surface of the activated meshes is mechanically processed using sandpaper or a brush with metal bristles, or by sandblasting.
[0045] Preferably, platinum group metals are applied to the surface of the activated mesh through an intermediate layer based on aluminum oxide.
[0046] Preferably, the surface of the mesh is fired with a hydrogen or nitric-hydrogen flame at a temperature of 500-700°C, or with a propane flame at a temperature of 500-1200°C, or the meshes are heat-treated in a furnace at a temperature of 150-600°C.
[0047] Preferably, the surface of the activated mesh is etched in a solution with a hydrochloric acid concentration of 1-36% at a temperature of 20-90°C for 0.25-20 min with stirring.
[0048] Preferably, the surface of the activated grid is etched in a solution of a mixture of hydrochloric and nitric acid with a total concentration of 1-50% at a temperature of 20-90°C for 0.10-20 min with stirring. Preferably, the surface of the activated grid is treated by electrochemical etching at a temperature of 20-80°C for 0.25-20 min with stirring.
[0049] Also, to achieve the stated technical result, it is proposed to use the above-mentioned catalytic system for the oxidation of ammonia in ammonia oxidation units.
[0050] According to one embodiment, the catalytic system: comprises a first catalytic grid made of a first platinum-based alloy, a first activated grid, a first catalytic grid made of a second platinum-based alloy, a second activated grid, a stack of palladium-based catching grids, and a third activated grid, installed along the gas flow path;
[0051] - activated grids are made of woven wire with a diameter of 0.07-3.00 mm, with cells that are not visible through the light, while the material of the activated grids is heat-resistant high-alloy or precision steel, or nichrome alloys;
[0052] - the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 0.1 wt. % to 50 wt. %, while the second alloy is made on the basis of a triple platinum-palladium-rhodium system with a palladium content from 0.1 wt. % to 95 wt. % and rhodium from 1 wt. % to 50 wt. %.
[0053] According to another embodiment of the catalytic system, instead of the first catalytic grid of the first platinum-based alloy, a pack of first catalytic grids of the first platinum-based alloy is installed. Instead of the first activated grid, a first pack of activated grids is installed. Instead of the first catalytic grid of the second platinum-based alloy, a pack of catalytic grids of the second platinum-based alloy is installed. Instead of the second activated grid, a second pack of activated grids is installed. Instead of the third activated grid, a third pack of activated grids is installed.
[0054] According to another embodiment, the catalytic system: comprises a first catalytic grid made of a first platinum-based alloy or a second platinum-based alloy, a first activated grid, a stack of palladium-based catching grids, and a second activated grid, installed along the gas flow path;
[0055] - activated grids are made of woven wire with a diameter of 0.07-3.00 mm, with cells that are not visible through the light, while the material of the activated grids is heat-resistant high-alloy or precision steel, or nichrome alloys;
[0056] - the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 0.1 wt. % to 50 wt. %, while the second alloy is made on the basis of a triple platinum-palladium-rhodium system with a palladium content from 0.1 wt. % to 95 wt. % and rhodium from 1 wt. % to 50 wt. %.
[0057] According to another embodiment of the catalytic system, instead of the first catalytic grid of the first platinum-based alloy, a package of catalytic grids of the first platinum-based alloy is installed, or instead of the first catalytic grid of the second platinum-based alloy, a package of catalytic grids of the second platinum-based alloy is installed. Instead of the first activated grid, the first package of activated grids is installed, instead of the second activated grid, the second package of activated grids is installed.
[0058] According to another embodiment, the catalytic system: comprises a first catalytic grid made of a first platinum-based alloy, a first activated grid, a first catalytic grid made of a second platinum-based alloy, and a second activated grid, installed along the gas flow path; - the activated grids are made of woven wire with a diameter of 0.07-3.00 mm, with cells that are absent when viewed through, and the material of the activated grids is heat-resistant high-alloy or precision steel, or nichrome alloys;
[0059] - the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 0.1 wt. % to 50 wt. %, while the second alloy is made on the basis of a triple platinum-palladium-rhodium system with a palladium content from 0.1 wt. % to 95 wt. % and rhodium from 1 wt. % to 50 wt. %.
[0060] According to another embodiment of the catalytic system, instead of the first catalytic grid of the first platinum-based alloy, a package of catalytic grids of the first platinum-based alloy is installed, instead of the first activated grid, a first package of activated grids is installed. Instead of the first catalytic grid of the second platinum-based alloy, a package of catalytic grids of the second platinum-based alloy is installed. Instead of the second activated grid, a second package of activated grids is installed.
[0061] According to another embodiment, the catalytic system: comprises a first catalytic grid made of a first platinum-based alloy or a second platinum-based alloy, and an activated grid, installed in the direction of gas flow;
[0062] - the activated mesh is made of woven wire with a diameter of 0.07-3.00 mm, with cells that are not visible through the light, while the material of the activated mesh is heat-resistant high-alloy or precision steel, or nichrome alloys;
[0063] - the first alloy is made on the basis of a binary platinum-rhodium system with a rhodium content from 0.1 May % to 50 May %, wherein the second alloy is made on the basis of a ternary platinum-palladium-rhodium system with a palladium content from 0.1 May % to 95 May % and rhodium from 1 May % to 50 May %. According to another embodiment of the catalytic system, instead of the first catalytic gauze of the first platinum-based alloy, a stack of catalytic gauze of the first platinum-based alloy is installed, or instead of the first catalytic gauze of the second platinum-based alloy, a stack of catalytic gauze of the second platinum-based alloy is installed. Instead of the first activated gauze, the first pack of activated gauze is installed.
[0064] According to another embodiment, the catalytic system: comprises, installed along the gas flow path, a first catalytic grid made of a first platinum-based alloy, a first catalytic grid made of a second platinum-based alloy, a first activated grid, a stack of palladium-based catching grids, and a second activated grid;
[0065] - activated grids are made of woven wire with a diameter of 0.07-3.00 mm, with cells that are not visible through the light, while the material of the activated grids is heat-resistant high-alloy or precision steel, or nichrome alloys;
[0066] - the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 0.1 wt. % to 50 wt. %, while the second alloy is made on the basis of a triple platinum-palladium-rhodium system with a palladium content from 0.1 wt. % to 95 wt. % and rhodium from 1 wt. % to 50 wt. %.
[0067] According to another embodiment of the catalytic system, instead of the first catalytic grid made of the first platinum-based alloy, a package of catalytic grids made of the first platinum-based alloy is installed. In this case, instead of the first catalytic grid made of the second platinum-based alloy, a package of catalytic grids made of the second platinum-based alloy is installed. Instead of the first activated grid, a first package of activated grids is installed, instead of the second activated grid, a second package of activated grids is installed. According to another embodiment, the catalytic system: comprises a first catalytic grid made of the first platinum-based alloy, a first catalytic grid made of the second platinum-based alloy, a package of catching grids based on palladium, an activated grid, installed along the gas flow;
[0068] - activated grids are made of woven wire with a diameter of 0.07-3.00 mm, with cells that are not visible through the light, while the material of the activated grids is heat-resistant high-alloy or precision steel, or nichrome alloys;
[0069] - the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 0.1 wt. % to 50 wt. %, while the second alloy is made on the basis of a triple platinum-palladium-rhodium system with a palladium content from 0.1 wt. % to 95 wt. % and rhodium from 1 wt. % to 50 wt. %.
[0070] According to another embodiment of the catalytic, instead of the first catalytic grid of the first platinum-based alloy, a stack of catalytic grids of the first platinum-based alloy is installed. Instead of the first catalytic grid of the second platinum-based alloy, a stack of catalytic grids of the second platinum-based alloy is installed. Instead of the first activated grid, a first stack of activated grids is installed.
[0071] The essence of the claimed method is that in the method for manufacturing all the above-mentioned versions of the device for reducing mechanical losses of platinum group metals from a catalytic system for oxidizing ammonia, activated meshes are fired with a hydrogen or nitrogen-hydrogen, or propane flame, or the activated meshes are thermally treated at a temperature of 150-600°C. Then the surface of the wire of the activated mesh is etched in a solution of diluted sulfuric or hydrochloric acids, or nitric acid, or a mixture of hydrochloric and nitric acids, at a temperature of 20-90°C for 0.25-20 minutes with stirring, or treated by electrochemical etching with stirring.
[0072] In special cases, it is permissible to perform the method as follows.
[0073] The surface of the activated mesh wire can be etched in a solution with a hydrochloric acid concentration of 1-36% at a temperature of 20-90°C for 0.25-20 min with stirring.
[0074] The surface of the activated mesh wire can be etched in a solution of a mixture of hydrochloric and nitric acid with a total concentration of 1-50% at a temperature of 20-90°C for 0.10-20 min with stirring.
[0075] The surface of the activated mesh wire is preferably treated by electrochemical etching at a temperature of 20-80°C for 0.25-20 min with stirring.
[0076] After etching, the surface of the activated meshes can be mechanically processed using sandpaper or a brush with metal bristles, or sandblasted.
[0077] Platinum group metals can be applied to the surface of the activated mesh through an intermediate layer.
[0078] Brief description of the drawings
[0079] Figure 1 shows a diagram of the arrangement of activated grids in the device according to embodiment 1; Fig. 2 is a diagram of the arrangement of activated grids in the device according to embodiment 2; Fig. 3 is a diagram of the arrangement of activated grids in the device according to embodiment 3; Fig. 4 is a diagram of the arrangement of activated grids in the device according to embodiment 4; Fig. 5 is a diagram of the arrangement of activated grids in the device according to embodiment 5; Fig. 6 is a diagram of the arrangement of activated grids in the device according to embodiment 6; Fig. 7 is an activated grid, Fig. 8 is an activated grid (side view); Fig. 9 is an activated grid (top view); Fig. 10 is a cell of the activated grid; Fig. 11 is a section A-A of Fig. 3, Fig. 12 is a section B-B of Fig. 3.
[0080] Implementation of the invention. The best embodiment of the invention
[0081] Catalytic system variant number
[0082] Accepted abbreviations: "KS" - catalyst grid; "US" - palladium-based catching grid package with separating grids; "SAT" - activated grid
[0083] Implementation of the technical solution according to option 1.
[0084] It is known that uneven distribution of gas flow over the surface of the catalytic system (see patent RU 2100068, [3]) leads to various pressure drops, increased tension on the grids and, as a consequence, to increased losses of platinum metals.
[0085] In variant 1 and in other variants, the stack may contain two or more gauzes, the first alloy being an alloy based on a double platinum-rhodium system with a rhodium content from 0.1 wt. % to 50 wt. %, the second alloy being an alloy based on a triple platinum-palladium-rhodium system with a palladium content from 0.1 wt. % to 95 wt. % and rhodium from 1 wt. % to 50 wt. %. In order to increase the strength of the catalytic system, a stack of catalyst gauzes made of a first platinum-based alloy, a first stack of activated gauzes, a stack of catalyst gauzes made of a second platinum-based alloy, a second stack of activated gauzes, a stack of catching gauzes based on palladium, and a third stack of activated gauzes are installed along the gas flow (Fig. 1).
[0086] Implementation of the technical solution according to option 2.
[0087] In order to increase the strength of the catalytic system, a package of catalyst grids made of a first platinum-based alloy or a second platinum-based alloy, a first package of activated grids, a package of palladium-based catching grids, and a second package of activated grids are installed along the gas flow path (Fig. 2).
[0088] Implementation of the technical solution according to option 3.
[0089] In order to increase the strength of the catalytic system, a package of catalyst meshes made of a first platinum-based alloy, a first package of activated meshes, a package of catalyst meshes made of a second platinum-based alloy, and a second package of activated meshes are installed along the gas flow path (Fig. 3).
[0090] Implementation of the technical solution according to option 4.
[0091] In order to increase the strength of the catalytic system, a package of catalyst grids made of a first platinum-based alloy or a second platinum-based alloy and a package of activated grids are installed along the gas flow path (Fig. 4).
[0092] Implementation of the technical solution according to option 5.
[0093] In order to increase the strength of the catalytic system, a package of catalyst grids made of a first platinum-based alloy, a package of catalyst grids made of a second platinum-based alloy, a first package of activated grids, a package of catching grids based on palladium, and a second package of activated grids are installed along the gas flow (Fig. 5).
[0094] Implementation of the technical solution according to variant 6. In order to increase the strength of the catalytic system, a package of catalyst grids made of a first alloy based on platinum, a package of catalyst grids made of a second alloy based on platinum, a package of catching grids based on palladium, and a package of activated grids are installed along the gas flow (Fig. 6).
[0095] In all variants, the activated grids (Fig. 7, 8, 9) are made woven from wire with a diameter of 0.07-3.00 mm, with the formation of cells in such a way that when the activated grid is illuminated, light penetrates no more than 15% of the total area of the grid, preferably no more than 10% of the total area of the grid. In this case, the area of the grid is understood to be its area obtained by multiplying the length by the width.
[0096] The material of the activated grids is:
[0097] - heat-resistant high-alloy or precision steel;
[0098] - nichrome alloys.
[0099] It is preferable to make activated meshes from steel grade X23Yu5T.
[0100] Activated grids stabilize the gas flow over the entire surface area of the grid due to the preferential redistribution of the normal component of the gas flow, directed vertically to the surface of the grids, to the tangential component - along the surface of the grids (see Figs. 10, 11, 12).
[0101] Implementation of the method for manufacturing the device according to options 1-6.
[0102] To activate the surface of the mesh, it is fired with a hydrogen or nitric-hydrogen or propane flame, or the mesh is heat treated at a temperature of 500-700°C.
[0103] Then the surface of the activated mesh wire is etched in a solution of diluted sulfuric or hydrochloric acids, or nitric acid, or a mixture of hydrochloric and nitric acids, at a temperature of 20-90°C for 0.25-20 min with stirring, or processed by electrochemical etching with stirring. Preferably, the surface of the mesh wire is etched in a solution with a sulfuric acid content of 1-50%.
[0104] The surface of the activated mesh wire can be etched in a solution with a hydrochloric acid concentration of 1-36% at a temperature of 20-90°C for 0.25-20 minutes with stirring.
[0105] The surface of the activated mesh wire can be etched in a solution of a mixture of hydrochloric and nitric acid with a total concentration of 1-50% at a temperature of 20-90°C for 0.10-20 min with stirring.
[0106] The surface of the activated mesh wire can be treated by electrochemical etching at a temperature of 20-80°C for 0.25-20 min with stirring.
[0107] After etching, the surface of the activated meshes is mechanically processed with sandpaper or a brush with metal bristles, or by sandblasting. As a result of such processing, lubricants from equipment parts containing carbon, which blocks the surface of the wire, are almost completely removed from the surface of the wire, the surface of the mesh becomes rough, which leads to an increase in the strength of the mechanical adhesion of platinoid particles evaporating from the platinoid meshes. The degree of capture increases by 5-10% for activated meshes compared to similar meshes made of smooth wire.
[0108] In order to increase the activity of the catalytic system and maintain the efficiency of operation throughout the entire run, platinoids are applied to the surface of the activated grid through the intermediate layer using any of the known methods (in particular, Russian patent RU 2169614, [4]). Platinoids on the activated grids further oxidize the unreacted ammonia from the catalyst grids and thus evenly distribute the ammonia oxidation reaction over the depth of the catalytic system package.
[0109] When the gas flow is stabilized, a uniform pressure drop occurs over the entire surface area of the grids, which leads to a decrease in mechanical stress, less cracking and destruction of the catalyst and catching grids and, in general, to a decrease in the loss of platinum group metals from the precious metal grids. A catalytic system with lower losses of platinum group metals retains its strength characteristics longer during operation, withstands high ammonia loads and has an increased service life.
[0110] Activated grids are made of intertwined wires with a diameter of 0.07-1.0 mm, forming cells in such a way that when the activated grid is illuminated, light penetrates no more than 15% of the total grid area, preferably no more than 10% of the total grid area. The grid area is understood to be its area obtained by multiplying the length by the width.
[0111] The catching effect is achieved due to the high contact area of the surface of the activated meshes with the platinum group particles in the gas flow, evaporating from the catalyst meshes, which is more than 5 times greater than the surface of woven meshes with cells per transmission made of the same diameter of the warp and weft wire (see Fig. 8). The degree of catching of platinum group metals by the activated meshes is up to 30%.
[0112] The catching effect is also achieved, as described above, due to the high contact area of the activated mesh surface with the platinum group particles when the gas flow flows around the surface of the wire of the catching mesh. The degree of catching of platinum group metals by activated meshes is up to 30%.
[0113] When studying the pressure drop under activated nets made of nichrome alloys or steel grade X23Yu5T made of wire with a diameter of 0.07-3.00 mm in a wind tunnel at an absolute pressure of 3-4 atm., almost complete equalization of the gas flow in the cross-section of the tube occurs, as well as a low value of the pressure drop of about 14 mm H2O, which is more than 3 times less under catalyst nets in medium-pressure units (see patent RU 2145935, [5]). At the same time, such equalization of the flow was not detected on woven nets with an open cell.
[0114] Studies were conducted during operation and after operation in a contact oxidation apparatus of a package of catalyst grids with activated grids installed underneath them, and the following results were obtained:
[0115] - uniform infrared glow of the catalyst grids during operation, which is due to uniform heating of the grids;
[0116] - uniform wear of the wire of the catalyst meshes from the edge to the center of the mesh, which is associated with the same ammonia load in the radial direction of the contact apparatus;
[0117] - reduction of platinum group metal losses from catalyst meshes, which may be due to reduction of mechanical losses due to uniform loading across the entire cross-section;
[0118] - the presence of numerous platinum group particles on the activated surface of the grids, which may be associated with the condensation of volatile platinum oxides and mechanical adhesion of platinum group particles to the activated surface of the grids, made in such a way that when the activated grid is illuminated, light penetrates through no more than 15% of the cell area, preferably no more than 10% of the cell area.
[0119] Examples of specific implementation.
[0120] Example 1. Catalytic system according to variant 4a. In the contact apparatus of the nitric acid production unit at atmospheric pressure, a grid of Kh23Yu5 steel with a diameter of 2900 mm made of warp wire with a diameter of 0.22 mm and weft wire with a diameter of 0.16 mm, activated by a hydrogen flame at a temperature of 700°C, was placed under a catalyst grid of PlRd 95-5 alloy (95 wt. % platinum and 5 wt. % rhodium) with a diameter of 2900 mm in the direction of gas flow. After operation for 9000 hours, the catalyst grid retained its integrity without the formation of tears and cracks, the degree of capture of platinum group metals after refining processing of the activated grid was more than 10%. The overrun of the catalyst grid relative to the standard value of 7920 hours was more than 1000 hours while maintaining the degree of ammonia conversion at the level of 95.5-97% during the entire run.
[0121] Example 2. Catalytic system according to variant 6b. Two grids made of Kh23Yu5T steel with a diameter of 3850 mm, made of 0.30 mm diameter warp wire and 0.20 mm diameter weft wire, activated by propane flame at a temperature of 1200°C, were installed in the contact apparatus of the nitric acid production unit at an average pressure of AK-72 in the direction of gas flow under a pack of catalyst grids, in which in the direction of gas flow the 2 upper grids are made of PlRd 95-5 alloy and 4 lower grids are made of PlPdRd 81-16-3 alloy (81 wt. % platinum, 16 wt. % palladium and 3 wt. % rhodium), and a pack of collecting grids is made of PdN-5 alloy (95 wt. % palladium and 5 wt. % nickel). After 8000 hours of operation, the catalyst and collecting meshes retained their integrity, and the degree of platinum group metal capture after refining of activated meshes was more than 7%.The catalytic system overrun relative to the standard value of 5500-6000 hours was more than 2000 hours while maintaining the degree of ammonia conversion at the level of 94.0-95.5% throughout the entire run.
[0122] Example 3. Catalytic system according to variant 4b. Four 1600 mm diameter grids made of Kh23Yu5T steel, made of 0.35 mm diameter warp wire and 0.22 mm diameter weft wire, activated by hydrogen flame at a temperature of 700°C, were installed in the contact apparatus of a nitric acid production unit at high pressure (8-10 absolute atm.) in the direction of gas flow under a stack of catalyst grids, in which in the direction of gas flow the 6 upper grids were made of PlPdRd 60-37-3 (60 wt. % platinum, 37 wt. % palladium and 3 wt. % rhodium). After operation for 2400 hours, the catalyst grids retained their integrity, the degree of platinum group metal capture after refining processing of the activated grids was more than 5%. The overrun of the catalyst grids relative to the standard value of 2160 hours was more than 200 hours while maintaining the calculated degree of ammonia conversion at the level of 90.0-92% throughout the entire run. Example 4. Catalytic system according to variant 4b.Three 1200 mm diameter nichrome gauzes of the Kh20N80 grade, made of 0.40 mm diameter warp wire and 0.28 mm diameter weft wire, activated by firing in a slot furnace at a temperature of 400°C, were installed in the contact apparatus of the hydrocyanic acid production unit along the gas flow path under a stack of catalyst gauzes, in which, along the gas flow path, the 4 upper gauzes were made of PlRd 92-8 alloy (92 wt. % platinum and 8 wt. % rhodium) and the 4 lower gauzes were made of PlRd 95-5 alloy. After operation for 2600 hours, the catalyst gauzes retained their integrity, the degree of platinum group metal capture after refining processing of the activated gauzes was more than 8%. The overrun of the catalyst gauzes relative to the standard value of 2200 hours was more than 400 hours, while maintaining the conversion of ammonia into HCN at the level of 60-62%.
[0123] Example 5. Catalytic system according to variant 4b. In the contact apparatus of the hydroxylamine sulfate production unit, two Kh23Yu5T steel meshes with a diameter of 2900 mm, made of 0.28 mm diameter warp wire and 0.18 mm diameter weft wire, activated by propane flame at a temperature of 1200°C, were placed in the direction of gas flow under a stack of catalyst meshes, in which, in the direction of gas flow, the two upper meshes were made of PlRd 92.5-7.5 alloy (92.5 wt. % platinum and 7.5 wt. % rhodium) and the lower mesh was made of PlRd 95-5 alloy. After operation for 9000 hours, the catalyst meshes retained their integrity without the formation of tears and cracks, the degree of platinum group metal capture after refining processing of the activated meshes was more than 15%. The overrun of the catalyst grid relative to the standard value of 7920 hours amounted to more than 1000 hours while maintaining the degree of ammonia conversion at the level of 92-94% throughout the entire run.
[0124] Example 6. Similar to example 3, but additionally platinum was applied to the surface of the activated gauzes by any of the known methods, in particular by the method described in Russian patent RU 2169614 (passed into the public domain), in which platinum group metals are applied to the carrier through an intermediate layer based on modified aluminum oxide. After operation for 2300 hours, the catalyst gauzes retained their integrity, the degree of platinum group metals capture after refining processing of the activated gauzes was more than 6%. The overrun of the catalyst gauzes relative to the standard value of 2160 hours was more than 100 hours, while maintaining the calculated degree of ammonia conversion at a high level of 91.0-92% throughout the entire run.
[0125] The test results are shown below.
[0126]
[0127] Notes:
[0128] *Abbreviations: "ABC" - ammonia-air mixture; "KA" - contact apparatus; "abs. atm" - absolute pressure in atmospheres; "KS" - catalyst grid; "US" - a pack of collecting grids with separating grids; "SAT" - activated grid; "MPG" - platinum group metals; "AK" - nitric acid; "SK" hydrocyanic acid; "GAS" - hydroxylamine sulfate; "NNS" - nitrite-nitrate salts.
[0129] ** Alloy composition, wt. %:
[0130] PlRd 95-5 contains 95% platinum and 5% rhodium;
[0131] PlRd 92.5-7.5 contains 92.5% platinum and 7.5% rhodium;
[0132] PlRd 92-8 contains 92% platinum and 8% rhodium;
[0133] PlPdRd 81-16-3 contains 81% platinum, 16% palladium and 3% rhodium;
[0134] PlPdRd 60-37-3 contains 60% platinum, 37% palladium and 3% rhodium
[0135] PDN-5 contains 95% palladium and 5% nickel.
[0136] Variants of the method for producing a catalytic system for the oxidation of ammonia were also investigated.
[0137] Notes: * after etching, additional mechanical treatment of the surface of the activated meshes is carried out with sandpaper or a brush with metal bristles.
[0138] In all embodiments of the invention, the resulting devices were used in ammonia oxidation units, where they made it possible to reduce the loss of platinum group metals from the catalytic system and equalize the gas flow.
[0139] The claimed invention ensured a reduction in the loss of platinum group metals from the catalytic system in ammonia oxidation units, an increase in the service life while maintaining a high degree of conversion without increasing the investment of precious metals, and also the equalization of the gas flow.
Claims
34 Invention formula 1. A catalytic system for the oxidation of ammonia, characterized in that it contains the following installed along the gas flow path: - a catalyst mesh or a stack of catalyst meshes made of a first platinum-based alloy or a second platinum-based alloy, - an activated mesh or a package of activated meshes; the activated meshes are made of woven wire with a diameter of 0.07-3.0 mm, the material of the activated meshes is heat-resistant high-alloy or precision steel, or nichrome alloys; the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 0.1 May. % to 50 May. %, while the second alloy is made on the basis of a ternary platinum-palladium-rhodium system with a palladium content from 0.1 May. % to 95 May. % and rhodium from 1 May. % to 50 May. %.
2. The system according to claim 1, characterized in that the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 3 May % to 12 May %, preferably from 4 May % to 10 May %, while the second alloy is made on the basis of a ternary platinum-palladium-rhodium system with a palladium content from 3 May % to 70%, preferably from 3 May % to 60 May %, and rhodium from 1 May % to 10 May %, preferably from 2 May % to 6 May %.
3. The system according to claim 1, characterized in that the activated grids are made of interwoven wires with a diameter of 0.07-1.0 mm, preferably 0.15-0.41 mm, with the formation of cells in such a way that when the activated grid is illuminated, light penetrates through no more than 15% of the grid area, preferably no more than 10% of the grid area.
4. The system according to item 1, characterized in that the system additionally contains the following installed along the gas flow path: 35 - a catalyst mesh or a package of catalyst meshes made of a second platinum-based alloy, - an activated grid or a package of activated grids.
5. The system according to item 1 or item 4, characterized in that the system additionally contains a package of palladium-based catching grids installed along the gas flow path and an activated grid or a package of activated grids.
6. A catalytic system for the oxidation of ammonia, characterized in that it contains the following installed along the gas flow path: - a catalyst mesh or a package of catalyst meshes made of the first platinum-based alloy, - a catalyst mesh or a package of catalyst meshes made of a second platinum-based alloy, - an activated grid or a package of activated grids, - a package of palladium-based trapping meshes, - an activated mesh or a package of activated meshes; the activated meshes are made of woven wire with a diameter of 0.07-3.00 mm, the material of the activated meshes is heat-resistant high-alloy or precision steel, or nichrome alloys; the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 0.1 May. % to 50 May. %, while the second alloy is made on the basis of a ternary platinum-palladium-rhodium system with a palladium content from 0.1 May. % to 95 May. % and rhodium from 1 May. % to 50 May. %.
7. The system according to item 6, characterized in that the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 3 May. % to 12 May. %, preferably from 4 May. % to 10 May. %, while the second alloy is made on the basis of a ternary platinum-palladium-rhodium system with palladium content from 3 May % to 70 May %, preferably from 3 May % to 60 May %, and relative from 1 May % to 10 May %, preferably from 2 May % to 6 May %.
8. The system according to claim 7, characterized in that the activated grids are made of interwoven wires with a diameter of 0.07-1.0 mm, preferably 0.15-0.41 mm, with the formation of cells in such a way that when the activated grid is illuminated, light penetrates through no more than 15% of the grid area, preferably no more than 10% of the grid area.
9. A catalytic system for the oxidation of ammonia, characterized in that it contains the following installed along the gas flow path: - a catalyst mesh or a package of catalyst meshes made of the first platinum-based alloy, - a catalyst mesh or a package of catalyst meshes made of a second platinum-based alloy, - a package of palladium-based trapping meshes, - an activated mesh or a package of activated meshes; the activated meshes are made of woven wire with a diameter of 0.07-3.00 mm, the material of the activated meshes is heat-resistant high-alloy or precision steel, or nichrome alloys; the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 0.1 May. % to 50 May. %, while the second alloy is made on the basis of a ternary platinum-palladium-rhodium system with a palladium content from 0.1 May. % to 95 May. % and rhodium from 1 May. % to 50 May. %.
10. The system according to item 9, characterized in that the first alloy is made on the basis of a double platinum-rhodium system with a rhodium content from 3 May. % to 12 May. %, preferably from 4 May. % to 10 May. %, while the second alloy is made on the basis of a ternary platinum-palladium-rhodium system with palladium content from 3 May % to 70 May %, preferably from 3 May % to 60 May %, and relative from 1 May % to 10 May %, preferably from 2 May % to 6 May %.
11. The system according to claim 9, characterized in that the activated grids are made of interwoven wires with a diameter of 0.07-1.0 mm, preferably 0.15-0.41 mm, with the formation of cells in such a way that when the activated grid is illuminated, light penetrates through no more than 15% of the grid area, preferably no more than 10% of the grid area.
12. A method for producing a catalytic system for oxidizing ammonia according to any of paragraphs. 1-11, characterized in that in order to obtain an activated mesh, the surface of the mesh is fired with a hydrogen or nitric-hydrogen, or propane flame, or the mesh is thermally treated at a temperature of 150-600°C, then the surface of the activated mesh is etched in a solution of sulfuric or hydrochloric acid, or nitric acid, or a mixture of hydrochloric and nitric acids, at a temperature of 20-90°C for 0.25-20 minutes with stirring, or processed by electrochemical etching with stirring.
13. The method according to item 12, characterized in that the surface of the activated mesh is etched in a solution with a hydrochloric acid concentration of 1–36% at a temperature of 20–90°C for 0.25–20 minutes with stirring.
14. The method according to item 12, characterized in that the surface of the activated mesh is etched in a solution of a mixture of hydrochloric and nitric acid with a total concentration of 1-50% at a temperature of 20-90°C for 0.10-20 min with stirring.
15. The method according to item 12, characterized in that the surface of the activated mesh is treated by electrochemical etching at a temperature of 20-80°C for 0.25-20 minutes with stirring.
16. The method according to item 12, characterized in that after etching, the surface of the activated meshes is mechanically processed. 38 sandpaper or a wire brush, or sandblasting.
17. The method according to claim 12, characterized in that platinum group metals are applied to the surface of the activated mesh through an intermediate layer based on aluminum oxide.
18. The method according to item 12, characterized in that the surface of the mesh is fired with a hydrogen or nitric-hydrogen flame at a temperature of 500-700°C, or with a propane flame at a temperature of 500-1200°C, or the mesh is heat-treated in an oven at a temperature of 150-600°C.
20. The method according to claim 12, characterized in that the surface of the activated mesh is etched in a solution with a hydrochloric acid concentration of 1–36% at a temperature of 20–90°C for 0.25–20 minutes with stirring.
21. The method according to paragraph 12, characterized in that the surface of the activated mesh is etched in a solution of a mixture of hydrochloric and nitric acid with a total concentration of 1-50% at a temperature of 20-90°C for 0.10-20 minutes with stirring.
22. The method according to paragraph 12, characterized in that the surface of the activated mesh is treated by electrochemical etching at a temperature of 20-80°C for 0.25-20 minutes with stirring.
25. Use of a catalytic system for oxidation of ammonia according to any of claims 1-11 in ammonia oxidation units.
Citation Information
Patent Citations
Catalyst system and method for the catalytic combustion of ammonia to form nitrogen oxides in a medium pressure system
EP3680015A1
Catalyst for gas phase oxidation reactions and processes effected therewith
GB785657A
Device for trapping platinoids in catalytic oxidation of ammonia
RU2119381C1
Catalytic element for ammonia conversion
RU2155097C1
Method for catalytic oxidation of ammonia