Positive electrode active material, preparation method therefor, secondary battery, and electrical apparatus
By designing interconnected pore structures and appropriate porosity in the positive electrode active material, the problem of breakage caused by volume changes during cycling was solved, thereby improving the battery's kinetic performance and cycle life.
Patent Information
- Application Number
- PCT/CN2023/097890
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-05
AI Technical Summary
The positive electrode active material of existing secondary batteries breaks down during cycling due to anisotropic volume changes, affecting battery performance and cycle life.
The positive electrode active material is designed as an agglomeration of primary particles containing pores. The longest interconnection distance of the pores is not less than 0.5 μm, and the porosity is 3% to 12%. The porosity decreases from the geometric center to the surface. The internal pores are interconnected by co-sintering the positive electrode active material precursor with a flux.
It improves the battery's dynamic performance and cycle life, enhances lithium-ion transport efficiency, reduces material breakage, and improves battery capacity and stability.
Smart Images

Figure CN2023097890_05122024_PF_FP_ABST
Abstract
Description
Positive electrode active material, preparation method thereof, secondary battery and electric device Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a positive electrode active material, a preparation method thereof, a secondary battery, and an electrical device. Background Art
[0002] In recent years, as secondary batteries have been widely used in energy storage power systems such as hydropower, thermal, wind and solar power stations, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields, the market's performance requirements for secondary batteries have become increasingly higher.
[0003] Electrode materials with high gram capacity often exhibit low material stability, which affects the battery cycle life. How to achieve simultaneous improvement in battery gram capacity and cycle life is a technical problem that urgently needs to be solved in this field.
[0004] Summary of the Invention
[0005] The present application is made in view of the above-mentioned problems, and its purpose is to provide a positive electrode active material to achieve a simultaneous improvement in battery capacity and cycle life.
[0006] The first aspect of the present application provides a positive electrode active material, which is an agglomerate of primary particles. The positive electrode active material contains pores between the primary particles, and the longest connection distance of the pores is not less than 0.5 μm, and can be optionally 1 μm-5 μm.
[0007] The pores between the primary particles inside the positive electrode active material provided by this application are interconnected, and the longest connection distance is not less than 0.5 μm, which can provide expansion space for the anisotropic volume change of the primary particles inside the positive electrode active material during the cycle, thereby improving the cycle life of the battery. At the same time, the interconnected pores are conducive to shortening the transmission path of active ions (such as lithium ions) inside the positive electrode active material, facilitating the deintercalation and embedding of metal ions, and can further improve the dynamic performance of the battery and maximize the capacity level of the battery.
[0008] In any embodiment, the cross-sectional diameter of the pore is 10 nm to 350 nm, and can be optionally 20 nm to 200 nm.
[0009] The cross-sectional diameter of the pores between primary particles is 10nm to 350nm, which is beneficial for improving the transmission and diffusion rate of active ions (such as lithium ions) in the electrode, improving the battery's first coulombic efficiency (referred to as "first efficiency"), helping to maximize the battery's capacity level and improve the battery's cycle life. When the pore diameter between primary particles is 20nm to 200nm, it can fully utilize the characteristics of high lithium ion diffusion efficiency and large battery capacity, while reducing the negative impact of large-diameter pores on cycle life, allowing the battery to have both excellent capacity level and cycle stability.
[0010] In any embodiment, the cross-sectional porosity of the positive electrode active material is 3% to 12%, and optionally 4% to 9%.
[0011] When the cross-sectional porosity of the positive electrode active material is 3% to 12%, it has sufficient ion transport channels, which is conducive to the rapid insertion / deinsertion of metal ions, helping to improve the initial efficiency and gram capacity of the battery. In addition, the appropriate cross-sectional porosity can provide sufficient space for the deformation of the positive electrode active material during the cycle process, thereby improving the cycle life of the battery. When the cross-sectional porosity of the positive electrode active material is 4% to 9%, it can fully utilize the characteristics of high lithium ion diffusion efficiency and large battery capacity, while reducing the negative impact of large porosity on battery cycle life, so that the battery has both excellent capacity level and cycle stability.
[0012] In any embodiment, the porosity of the positive electrode active material decreases in a direction from the geometric center of the positive electrode active material toward the surface of the positive electrode active material.
[0013] The metal ions at the center of the positive electrode active material require a longer diffusion distance, and the higher porosity within the positive electrode active material facilitates the diffusion of metal ions within the material, promoting the full utilization of the battery capacity. During the cycling process, the center of the positive electrode active material is subjected to strong stress and large strain. The decrease in the porosity of the positive electrode active material from the geometric center to the surface of the positive electrode active material helps the positive electrode active material maintain a stable morphology during the cycling process, making it less likely to develop cracks induced by the center of the positive electrode active material, thereby improving the battery cycle life.
[0014] In any embodiment, the relationship between the cross-sectional porosity Po(C100) within the 100% concentric circle range of the positive electrode active material and the cross-sectional porosity Po(C64) within the 64% concentric circle range of the positive electrode active material on the same cross section satisfies Po(C64) / Po(C100) ≥ 1.10. The 100% concentric circle range of the positive electrode active material is the area within a distance r from the geometric center of the positive electrode active material, where r represents the radius of the positive electrode active material. The 64% concentric circle range of the positive electrode active material is the area within a distance 0.8r from the geometric center of the positive electrode active material.
[0015] In any embodiment, the relationship between the cross-sectional porosity Po(C100) within a 100% concentric circle of the positive electrode active material and the cross-sectional porosity Po(C36) within a 36% concentric circle of the positive electrode active material on the same cross section satisfies Po(C36) / Po(C100)≥1.20. The 36% concentric circle of the positive electrode active material is the area within 0.6r from the geometric center of the positive electrode active material, where r represents the radius of the positive electrode active material.
[0016] In any embodiment, based on the total mass of the positive electrode active material, the residual lithium content of the positive electrode active material is 500 ppm to 3500 ppm, and optionally 1000 ppm to 2100 ppm.
[0017] The residual lithium amount within the appropriate range can clean the surface of the positive electrode active material while improving the retention of the morphology and structure of the positive electrode active material, thereby achieving a comprehensive improvement in battery capacity and cycle stability.
[0018] In any embodiment, the general formula of the positive electrode active material is as shown in Formula I: Li a Ni x M 1-x O 2-b Formula I
[0019] Wherein, M includes at least one of Co, Mn, Al, Y, W, Ta, Mo, Ce, La, Zr, Sr, Y, Sb, W, Ti, Mg, Nb, K, and Ca, 0.5≤a≤1.2, 0.5≤x<1.0, -0.1≤b≤0.1, optionally, 0.8≤a≤1.2, 0.8≤x<1.0.
[0020] In any embodiment, the positive electrode active material satisfies at least one of the following conditions:
[0021] (i) The specific surface area of the positive electrode active material is 0.4 cm 2 / g~5cm 2 / g;
[0022] (ii) the average particle size of the primary particles is 10 nm to 200 nm;
[0023] (iii) The tap density of the positive electrode active material is 1.7 g / cm 3 ~2.3g / cm 3 .
[0024] The second aspect of the present application provides a method for preparing a positive electrode active material, comprising: mixing a positive electrode active material precursor, a lithium salt and a flux and conducting a sintering reaction to prepare the positive electrode active material; the positive electrode active material is an agglomerate of primary particles, and the positive electrode active material contains pores located between the primary particles, and the longest connecting distance of the pores is greater than 0.5 μm.
[0025] During the preparation of positive electrode active materials, the co-sintering of flux with positive electrode active material precursor and lithium salt can successfully prepare positive electrode active materials with interconnected internal pores and a maximum connection distance of not less than 0.5 μm, effectively improving the first efficiency, capacity and cycle life of the battery.
[0026] In any embodiment, the flux includes an alkali metal salt, which can be one or more of an alkali metal sulfate and an alkali metal acetate. Optionally, the flux includes one or more of potassium sulfate, lithium sulfate, sodium sulfate, potassium acetate, lithium acetate, and sodium acetate.
[0027] In any embodiment, the precursor of the positive electrode active material has the general formula shown in Formula II, Ni y M 1-y (OH)2 Formula II
[0028] Wherein, M includes at least one of Co, Mn, Al, Y, W, Ta, Mo, Ce, La, Zr, Sr, Y, Sb, W, Ti, Mg, Nb, K, and Ca, 0.5≤y<1.0,
[0029] Optionally, 0.8≤y<1.0.
[0030] In any embodiment, the molar ratio of the flux to the positive electrode active material precursor is (0.05-0.3):1, and can be optionally (0.08-0.2):1.
[0031] A molar ratio of 0.05-0.3:1 between the flux and the cathode active material precursor can provide the cathode active material with a suitable pore structure, thereby improving the battery's capacity and cycle life. A molar ratio of 0.08-0.2:1 between the flux and the cathode active material precursor can also achieve excellent battery capacity and cycle life.
[0032] In any embodiment, the temperature of the sintering reaction is 500° C. to 800° C., optionally 650° C. to 800° C., and / or the time of the sintering reaction is 10 h to 15 h, optionally 12 h to 14 h.
[0033] In any embodiment, the preparation method of the positive electrode active material specifically includes: mixing a positive electrode active material precursor, a lithium salt and a flux under an oxygen atmosphere, performing a sintering reaction, and then washing with water to obtain an intermediate product; and calcining the intermediate product under an oxygen atmosphere to prepare the positive electrode active material.
[0034] In any embodiment, the water washing temperature is 4°C to 10°C.
[0035] The water washing temperature has an important influence on battery performance. A water washing temperature higher than 10°C will enlarge the pores in the positive electrode active material and increase the porosity. At the same time, a water washing temperature higher than 10°C can easily cause over-washing of the positive electrode active material, resulting in changes in the composition and structure of the surface of the positive electrode active material. The electronic conductivity of materials with too low lithium content and too high nickel content decreases, which significantly increases the internal resistance of the battery and reduces the capacity level and cycle life. A water washing temperature lower than 4°C cannot guarantee the removal of impurities on the surface of the positive electrode active material, affects the interconnectivity of the pores, and the impurity compounds remaining on the surface have a negative impact on the subsequent production and preparation of the battery. A water washing temperature within an appropriate range can achieve the cleaning of the surface of the positive electrode active material while maintaining the product morphology and structure, thereby achieving a comprehensive improvement in battery capacity and cycle stability.
[0036] In any embodiment, the calcination temperature is 500° C.-650° C., and / or the calcination time is 2 h-5 h.
[0037] A third aspect of the present application provides a secondary battery, comprising a positive electrode plate, wherein the positive electrode plate comprises a positive electrode active material according to any embodiment or a positive electrode active material prepared by a preparation method according to any embodiment.
[0038] A fourth aspect of the present application provides an electrical device comprising a secondary battery according to any embodiment. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] FIG1 is a scanning electron microscope image of a cross section of the positive electrode active material of Example 9;
[0040] FIG2 is a scanning electron microscope image of a cross section of the positive electrode active material of Comparative Example 2;
[0041] FIG3 is a comparison of the first charge and discharge curves of the batteries of Example 9 and Comparative Example 2;
[0042] FIG4 is a comparison chart of battery cycle stability of Example 9 and Comparative Example 2;
[0043] FIG5 is a scanning electron microscope image of a cross section of the positive electrode sheet in Example 9 after 300 cycles of testing;
[0044] FIG6 is a scanning electron microscope image of a cross section of the positive electrode sheet in Comparative Example 2 after 300 cycles of testing;
[0045] FIG7 is a cross-sectional porosity analysis diagram of the positive electrode active materials of Comparative Example 2 and Example 9 within different concentric circle area ranges; wherein 1A, 1B, 1C, 1D, 1E, and 1F are cross-sectional analysis diagrams of the positive electrode active material in Comparative Example 2 within the concentric circle ranges of 100%, 81%, 64%, 49%, 36%, and 25%, respectively; and 2A, 2B, 2C, 2D, 2E, and 2F are cross-sectional analysis diagrams of the positive electrode active material in Example 9 within the concentric circle ranges of 100%, 81%, 64%, 49%, 36%, and 25%, respectively;
[0046] FIG8 is a schematic diagram of a battery pack according to an embodiment of the present application;
[0047] FIG9 is an exploded view of the battery pack according to one embodiment of the present application shown in FIG8 ;
[0048] FIG. 10 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.
[0049] Explanation of reference numerals: 1 battery pack; 2 upper case; 3 lower case; 4 battery module; 5 secondary battery; 51 housing; 52 electrode assembly; 53 top cover assembly. DETAILED DESCRIPTION
[0050] Below, the embodiments of the positive electrode active material, preparation method thereof, secondary battery and electric device of the present application are described in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0051] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0052] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0053] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0054] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0055] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0056] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0057] As the battery life and mileage of various electrical devices increase, higher requirements are placed on the capacity and cycle performance of secondary batteries. Positive electrode active materials with high gram capacity are prone to anisotropic volume changes during cycling, which can lead to anisotropic stress within the positive electrode active material, causing particle breakage, rapid deterioration of battery performance, and a reduction in battery cycle life.
[0058] [Positive electrode active material]
[0059] Based on this, the present application provides a positive electrode active material, which is an agglomerate of primary particles. The positive electrode active material contains pores between the primary particles, and the longest connection distance of the pores is not less than 0.5μm, and can be optionally 1μm-5μm.
[0060] In some embodiments, the longest connected distance of the pores may be 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, or any value therebetween.
[0061] The longest connection distance of the pores can be tested by methods known in the art. As an example, the longest connection distance of the pores can be determined by ultra-thin sectioning the positive electrode active material at a certain step length using a focused ion beam (FIB), and taking scanning electron microscope (SEM) images in sequence; 3D reconstruction software is used to align the collected focused ion beam-scanning electron microscope photos, and after alignment, three-dimensional reconstruction is performed to obtain a three-dimensional image of the positive electrode active material particles. According to the reconstruction results, the pore distribution in the three-dimensional image of the positive electrode active material is obtained, and the longest connection distance of the pores is read. The step length of ultra-thin sectioning of the positive electrode active material by the focused ion beam (FIB) can be selected as 20 nm. The pores between the primary particles inside the positive electrode active material provided in the present application are interconnected, and the longest connection distance is not less than 0.5 μm, which can provide expansion space for the anisotropic volume change of the primary particles in the positive electrode active material during the cycle, thereby improving the cycle life of the battery. At the same time, the interconnected pores are conducive to shortening the transmission path of metal ions (such as lithium ions) inside the positive electrode active material, facilitating the deintercalation and embedding of metal ions, and can further improve the battery's kinetic performance and maximize the battery's capacity level.
[0062] In some embodiments, the cross-sectional diameter of the pores between the primary particles is 10 nm to 350 nm, and optionally 20 nm to 200 nm.
[0063] In some embodiments, the cross-sectional diameter of the pores between the primary particles can be selected to be 10nm, 15nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm, 260nm, 270nm, 280nm, 290nm, 300nm, 310nm, 320nm, 330nm, 340nm, 350nm or any value therebetween.
[0064] The cross-sectional diameter of the pores between primary particles can be measured using methods known in the art. For example, the cross-sectional diameter of the pores between primary particles can be obtained by image processing and analysis of a cross-section of the positive electrode active material. The electrode sheet is subjected to triple ion beam sectioning to obtain a flat cross-section that exposes the cross-sectional surface of the positive electrode active material. The cross-sectional image is then photographed using a scanning electron microscope (SEM) to obtain a cross-sectional SEM image. The pore diameter between primary particles is then measured, with the longest diameter of each pore being used as the cross-sectional diameter of the pore.
[0065] Pores with a cross-sectional diameter of 10nm to 350nm between primary particles are beneficial for increasing the transmission and diffusion rate of metal ions (such as lithium ions) in the electrode, improving the initial efficiency of the battery, helping to maximize the battery capacity, and extending the battery's cycle life. When the pore diameter between primary particles is 20nm to 200nm, it can fully utilize the high lithium ion diffusion efficiency and large battery capacity, while reducing the negative impact of large-diameter pores on cycle life, allowing the battery to achieve both excellent capacity and cycle stability.
[0066] In some embodiments, the cross-sectional porosity of the positive electrode active material is 3% to 12%, and optionally 4% to 9%.
[0067] In some embodiments, the cross-sectional porosity of the positive electrode active material may be 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, or any value therebetween.
[0068] The cross-sectional porosity of the positive electrode active material can be tested using methods known in the art. As an example, the cross-sectional porosity of the positive electrode active material can be obtained by image processing and analysis of the cross-section of the positive electrode active material. The electrode piece is subjected to triple ion beam cutting to obtain a flat cross-section that exposes the internal structure of the positive electrode active material; a scanning electron microscope (SEM) is used to photograph a cross-sectional view, and the obtained scanned image representing the interior of the positive electrode active material is threshold segmented using ImageJ software. The gray-white contrast area is the particle, and the black contrast area is the pore. The ratio of the area of the black contrast area within the positive electrode active material to the total area of the positive electrode active material is used as the cross-sectional porosity of the positive electrode active material.
[0069] When the cross-sectional porosity of the positive electrode active material is 3% to 12%, it has sufficient ion transport channels, which is conducive to the rapid insertion / deinsertion of metal ions, helping to improve the initial efficiency and gram capacity of the battery. In addition, the appropriate cross-sectional porosity can provide sufficient space for the deformation of the positive electrode active material during the cycle process, thereby improving the cycle life of the battery. When the cross-sectional porosity of the positive electrode active material is 4% to 9%, it can fully utilize the characteristics of high lithium ion diffusion efficiency and large battery capacity, while reducing the negative impact of large porosity on battery cycle life, so that the battery has both excellent capacity level and cycle stability.
[0070] In some embodiments, the porosity of the positive electrode active material decreases in a direction from the geometric center of the positive electrode active material toward the surface of the positive electrode active material.
[0071] The porosity of the positive electrode active material can be tested using any known method. To facilitate statistical analysis of the porosity of different regions within the positive electrode active material, the concentric circle method can be used for characterization. As an example, the positive electrode active material is ultrathinly sliced at a certain step length using a focused ion beam (FIB) microscope, and scanning electron micrographs (SEM) are taken sequentially. The FIB-SEM results are then reconstructed in three dimensions using 3D reconstruction software to obtain a three-dimensional image of the interior of the positive electrode active material. The three-dimensional image of the positive electrode active material is cut through its geometric center to obtain a cross-section of the interior of the positive electrode active material. Using the geometric center of the positive electrode active material particle as the center, circles with different radii are drawn, and the cross-sectional porosity within different radius ranges within the same cross-sectional image is calculated. For the same cross-sectional image, the cross-sectional porosity within a small radius range is greater than the cross-sectional porosity within a large radius range, indicating that the porosity of the positive electrode active material decreases from the geometric center of the positive electrode active material toward the surface of the positive electrode active material.
[0072] The metal ions at the center of the positive electrode active material require a longer diffusion distance, and the higher porosity within the positive electrode active material facilitates the diffusion of metal ions within the material, promoting the full utilization of the battery capacity. During the cycling process, the center of the positive electrode active material is subjected to strong stress and large strain. The decrease in the porosity of the positive electrode active material from the geometric center to the surface of the positive electrode active material helps the positive electrode active material maintain a stable morphology during the cycling process, making it less likely to develop cracks induced by the center of the positive electrode active material, thereby improving the battery cycle life.
[0073] In some embodiments, the relationship between the cross-sectional porosity Po(C100) within a 100% concentric circle of the positive electrode active material and the cross-sectional porosity Po(C64) within a 64% concentric circle of the positive electrode active material on the same cross-section satisfies Po(C64) / Po(C100)≥1.10. The 100% concentric circle of the positive electrode active material is the region within a distance r from the geometric center of the positive electrode active material, and the 64% concentric circle of the positive electrode active material is the region within a distance 0.8r from the geometric center of the positive electrode active material, where r represents the radius of the positive electrode active material.
[0074] In some embodiments, the relationship between the cross-sectional porosity Po(C100) within a 100% concentric circle of the positive electrode active material and the cross-sectional porosity Po(C36) within a 36% concentric circle of the positive electrode active material on the same cross-section satisfies Po(C36) / Po(C100)≥1.20. The 36% concentric circle of the positive electrode active material is the area within 0.6r of the geometric center of the positive electrode active material, where r represents the radius of the positive electrode active material.
[0075] In some embodiments, based on the total mass of the positive electrode active material, the residual lithium content of the positive electrode active material is 500 ppm to 3500 ppm, and optionally 1000 ppm to 2100 ppm.
[0076] In some embodiments, the residual lithium content of the positive electrode active material may be 500 ppm, 1000 ppm, 1500 ppm, 2000 ppm, 2100 ppm, 2500 ppm, 3000 ppm, 3500 ppm, or any value therebetween, based on the total mass of the positive electrode active material.
[0077] The residual lithium content of the positive electrode active material can be tested according to GB / T 9736-2008, General method for determination of acidity and alkalinity of chemical reagents. Weigh 10g-30g of the positive electrode active material, add 100ml of pure water, and stir for 30 minutes. Let it stand for 10 minutes, filter, and remove a certain amount of the filtrate. Use 0.05mol / L hydrochloric acid standard solution, drain the burette to remove any bubbles, and then select the appropriate sensor and program start potential for titration. The residual lithium content is calculated by dividing the sum of the measured masses of lithium carbonate and lithium bicarbonate by the mass of the positive electrode active material.
[0078] The amount of residual lithium on the surface of the positive electrode active material has an important impact on the battery performance. In the preparation process of high-nickel positive electrode active materials, an excess lithium source is often added to avoid the increase in cation mixing caused by lithium evaporation during the calcination process. However, the excess lithium source will be converted into residual lithium compounds such as lithium carbonate and lithium bicarbonate and remain on the surface of the positive electrode active material. The residual lithium compounds on the surface of the positive electrode active material will cause the slurry to gel, making coating difficult, and side reactions will occur during the electrochemical reaction, causing the electrochemical performance to deteriorate and causing safety problems. Residual lithium compounds such as lithium carbonate and lithium bicarbonate are easily soluble in water. Therefore, water washing is an effective means to remove residual lithium from the positive electrode active material. Although transitional cleaning helps to effectively remove residual lithium on the surface of the positive electrode active material, it will also cause changes in the composition and structure of the surface of the positive electrode active material. The electronic conductivity of the positive electrode active material with too low a lithium content and too high a nickel content will decrease, which will significantly increase the internal resistance of the battery and reduce the capacity level and cycle life.
[0079] The residual lithium amount within the appropriate range can clean the surface of the positive electrode active material while improving the retention of the morphology and structure of the positive electrode active material, thereby achieving a comprehensive improvement in battery capacity and cycle stability.
[0080] In some embodiments, the general formula of the positive electrode active material is as shown in Formula I: Li a Ni x M 1-x O 2-b Formula I
[0081] Wherein, M includes at least one of Co, Mn, Al, Y, W, Ta, Mo, Ce, La, Zr, Sr, Y, Sb, W, Ti, Mg, Nb, K, and Ca, 0.5≤a≤1.2, 0.5≤x<1.0, and -0.1≤b≤0.1. Optionally, 0.8≤a≤1.2, and 0.8≤x<1.0.
[0082] In some embodiments, a can be selected from 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, or any value therebetween.
[0083] In some embodiments, x can be selected from 0.5, 0.6, 0.7, 0.8, 0.9, or any value therebetween.
[0084] In some embodiments, b can be selected as -0.1, -0.005, 0, 0.005, or 0.1.
[0085] In some embodiments, the specific surface area of the positive electrode active material is 0.4 cm 2 / g~5cm 2 / g.
[0086] The specific surface area of the positive electrode active material can be measured using any known method. For example, the specific surface area of the positive electrode active material can be measured with reference to GB / T 19587-2017, "Determination of the Specific Surface Area of Solid Substances by the BET Method for Gas Adsorption." As an example, the specific surface area of the positive electrode active material is measured using a TriStar II 3020 instrument. The positive electrode active material is dispersed in a dispersant, such as ethanol, and ultrasonicated for 30 minutes. The material is then dried in a vacuum drying oven and finally measured using a specific surface area meter.
[0087] In some embodiments, the specific surface area of the positive electrode active material may be 0.4 cm 2 / g, 0.6cm 2 / g, 0.8cm 2 / g, 1cm 2 / g, 1.5cm 2 / g, 2cm 2 / g, 2.5cm 2 / g, 3cm 2 / g, 3.5cm 2 / g, 4cm 2 / g, 4.5cm 2 / g, 5cm 2 / g or any value therebetween.
[0088] The positive electrode active material provided by the present disclosure has a high specific surface area, which is conducive to the efficient transmission of metal ions and improves the overall performance of the battery.
[0089] In some embodiments, the average particle size of the primary particles is 10 nm to 200 nm.
[0090] In some embodiments, the average particle size of the primary particles is 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, or any value therebetween.
[0091] The average particle size of the primary particles can be measured by any known method. As an example, the average particle size test method of the primary particles is as follows. The positive electrode active material is cut by an ion beam milling instrument (CP) to obtain a sample in which the cross section of the primary particles of the positive electrode active material can be observed, and the cross section is photographed using a scanning electron microscope (SEM) to obtain a cross-sectional scanning electron microscope image, and 100 primary particles are randomly selected from the obtained scanning electron microscope image; the particle boundaries of the selected 100 primary particles are observed to determine the shape of the primary particles; the longest diameter of each of the 100 primary particles is counted, and their average value is used as the average particle size of the primary particles.
[0092] The average particle size of the primary particles is within this range, so that the diffusion distance of lithium ions will not be too long, which is conducive to the deintercalation and intercalation of lithium ions and is beneficial to the improvement of battery capacity and cycle performance.
[0093] In some embodiments, the tap density of the positive electrode active material is 1.7 g / cm 3 ~2.3g / cm 3 .
[0094] In some embodiments, the tap density of the positive electrode active material is 1.7 g / cm 3 , 1.8g / cm 3 , 1.9g / cm 3 , 2.0g / cm 3 , 2.1g / cm 3 , 2.2g / cm 3 , 2.3g / cm 3 or any value in between.
[0095] The tap density of the positive electrode active material can be measured using any known method. For example, the tap density of the positive electrode active material can be measured with reference to GB / T 5162-2006 "Determination of Tap Density of Metal Powders" using a Dandong Better BT-300 tap density meter.
[0096] The positive electrode active material with a tap density within the above range can not only enable the battery to have a certain load capacity and ensure the volume energy density of the battery, but also realize the rapid transmission of metal ions, which is beneficial to the performance of the battery capacity level and improves the overall performance of the battery.
[0097] The second aspect of the present application provides a method for preparing a positive electrode active material, comprising: mixing a positive electrode active material precursor, a lithium salt and a flux for a sintering reaction to prepare a positive electrode active material; the positive electrode active material is an agglomerate of primary particles, and the positive electrode active material contains pores between the primary particles, and the longest connecting distance of the pores is greater than 0.5 μm.
[0098] In some embodiments, the flux includes an alkali metal salt, which may be one or more of an alkali metal sulfate and an alkali metal acetate. Alternatively, the flux includes one or more of potassium sulfate, lithium sulfate, sodium sulfate, potassium acetate, lithium acetate, and sodium acetate.
[0099] Alkali metal salts are acid salts composed of six alkali metal elements: lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), and francium (Fr). Alkali metal sulfates include lithium sulfate, sodium sulfate, and potassium sulfate, while alkali metal acetates include lithium acetate, sodium acetate, and potassium acetate.
[0100] During the preparation of positive electrode active materials, the co-sintering of flux with positive electrode active material precursor and lithium salt can successfully prepare positive electrode active materials with interconnected internal pores and a maximum connection distance of not less than 0.5 μm, effectively improving the first efficiency, capacity and cycle life of the battery.
[0101] In some embodiments, the precursor of the positive electrode active material is represented by Formula II, Ni y M 1-y (OH)2 Formula II
[0102] Wherein, M includes at least one of Co, Mn, Al, Y, W, Ta, Mo, Ce, La, Zr, Sr, Y, Sb, W, Ti, Mg, Nb, K, and Ca, and 0.5≤y<1.0. Optionally, 0.8≤y<1.0.
[0103] In some embodiments, y can be selected from 0.5, 0.6, 0.7, 0.8, 0.9, or any value therebetween.
[0104] In some embodiments, the molar ratio of the flux to the positive electrode active material precursor is (0.05-0.3):1, and can be optionally (0.08-0.2):1.
[0105] In some embodiments, the molar ratio of the flux to the positive electrode active material precursor can be selected to be 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, or any value therebetween.
[0106] A molar ratio of 0.05-0.3:1 between the flux and the cathode active material precursors allows for a suitable pore structure, improving the battery's capacity and cycle life. A molar ratio of 0.08-0.2:1 between the flux and the cathode active material precursors allows for both excellent capacity and cycle life.
[0107] In some embodiments, the sintering reaction temperature is 500° C. to 800° C., and may be 650° C. to 800° C., and the sintering reaction time is 10 h to 15 h, and may be 12 h to 14 h.
[0108] In some embodiments, the temperature of the sintering reaction may be selected to be 500° C., 550° C., 600° C., 650° C., 700° C., 750° C., 800° C., or any value therebetween.
[0109] In some embodiments, the sintering reaction time may be 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, or any value therebetween.
[0110] In some embodiments, the method for preparing the positive electrode active material specifically includes: mixing the positive electrode active material precursor, lithium salt and flux in an oxygen atmosphere, performing a sintering reaction, and then washing with water to obtain an intermediate product; and calcining the intermediate product in an oxygen atmosphere to prepare the positive electrode active material.
[0111] To reduce the impact of flux impurities on the surface of the positive electrode active material on battery performance, a simple water washing process is required to remove the flux. However, the water washing process introduces oxygen-containing functional groups on the surface of the positive electrode active material. The calcination process after water washing can effectively remove the oxygen-containing functional groups introduced by the water washing process on the surface of the positive electrode active material, reducing the negative impact of oxygen-containing functional groups on battery performance.
[0112] In some embodiments, the water washing temperature is 4°C to 10°C.
[0113] In some embodiments, the water washing temperature may be 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, or 10°C.
[0114] The water washing temperature has an important influence on battery performance. A water washing temperature higher than 10°C will enlarge the pores in the positive electrode active material and increase the porosity. At the same time, a water washing temperature higher than 10°C can easily cause the positive electrode active material to be overwashed, resulting in changes in the composition and structure of the surface of the positive electrode active material. The electronic conductivity of materials with too low lithium content and too high nickel content decreases, which significantly increases the internal resistance of the battery and reduces the capacity level and cycle life. A water washing temperature lower than 4°C cannot guarantee the removal of impurities on the surface of the positive electrode active material, affecting the interconnectivity of the pores, and the impurity compounds remaining on the surface have a negative impact on the subsequent production and preparation of the battery. A water washing temperature within an appropriate range can achieve the cleaning of the surface of the positive electrode active material while maintaining the product morphology and structure, thereby achieving a comprehensive improvement in battery capacity and cycle stability.
[0115] In some embodiments, the calcination temperature is 500° C.-650° C., and / or the calcination time is 2 h-5 h.
[0116] In some embodiments, the calcination temperature may be 500° C., 550° C., 600° C., 650° C., or any value therebetween.
[0117] In some embodiments, the calcination time may be 2 h, 3 h, 4 h, 5 h, or any value therebetween.
[0118] In one embodiment of the present application, a secondary battery is provided, including a positive electrode plate, wherein the positive electrode plate includes the positive electrode active material of any embodiment or the positive electrode active material prepared by the preparation method of any embodiment.
[0119] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During the battery's charge and discharge processes, active ions are inserted and removed between the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator, located between the positive and negative electrodes, primarily prevents short circuits between the positive and negative electrodes while allowing ions to pass through.
[0120] [Positive electrode]
[0121] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, and the positive electrode film layer includes the positive electrode active material of the first aspect of the present application.
[0122] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0123] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0124] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), a vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, a vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, a tetrafluoroethylene-hexafluoropropylene copolymer, and a fluorine-containing acrylate resin.
[0125] In some embodiments, the positive electrode film layer may further include a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0126] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0127] [Negative electrode]
[0128] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0129] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0130] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0131] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery that is well known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0132] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0133] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0134] In some embodiments, the negative electrode film layer may optionally further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0135] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0136] [Electrolytes]
[0137] The electrolyte conducts ions between the positive and negative electrodes. This application does not specify the type of electrolyte, and the electrolyte can be selected based on the needs. For example, the electrolyte can be liquid, gel, or solid.
[0138] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0139] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0140] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0141] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0142] [Isolation film]
[0143] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.
[0144] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0145] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.
[0146] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0147] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the outer packaging of the secondary battery can be a soft shell, such as a pouch-type soft shell. The soft shell can be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0148] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG8 shows a secondary battery 5 having a square structure as an example.
[0149] In some embodiments, referring to Figure 9, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0150] In addition, the present application also provides an electrical device, which includes the secondary battery provided in the present application. The secondary battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.
[0151] As the electrical device, a secondary battery can be selected according to its usage requirements.
[0152] FIG10 shows an example of an electric device, which may be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle.
[0153] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.
[0154] Example
[0155] Below, the embodiment of the present application is described. The embodiment described below is exemplary and is only used to explain the present application, and is not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. Reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0156] 1. Preparation method
[0157] Example 1
[0158] 1) Preparation of positive electrode active materials
[0159] Nickel sulfate, cobalt sulfate, and manganese sulfate were prepared into a 2 mol / L metal salt solution according to the molar ratio of Ni, Co, and Mn elements of 0.95:0.04:0.01. Subsequently, the metal salt solution, 8 mol / L ammonia water, and 5 mol / L NaOH solution were continuously added into the reactor to react. The pH value during the reaction was controlled to be 11.30, the ammonia concentration was 4.0 g / L, the reaction time was 20 h, and the stirring rate was 300 r / min. The precursor of the positive electrode active material (Ni) was prepared by the hydroxide coprecipitation method. 0.95 Co 0.04 Mn 0.01 (OH)2).
[0160] The positive electrode active material precursor Ni prepared above 0.95 Co 0.04 Mn0.01 (OH)2, lithium salt LiOH·H2O, and flux K2SO4 were mixed uniformly at a molar ratio of 1:1.05:0.10. The mixed powder was then added to a corundum boat and placed in a tube furnace. Pure oxygen was introduced at a flow rate of 0.2 liters / minute. The temperature was raised to 650°C at a rate of 5°C / minute. After being held at 650°C for 12 hours, the temperature was lowered to room temperature at a rate of 5°C / minute. The cooled powder was removed, mechanically crushed, and deionized water was added to dissolve the K2SO4. The mixture was then filtered and washed once at 8°C for 10 minutes. After washing twice, the mixture was filtered again to obtain an intermediate product.
[0161] The intermediate product was dried by blast drying at 60°C. The dried powder was added to a corundum porcelain boat again and placed in a tube furnace. Pure oxygen was introduced at a flow rate of 0.2 liters / minute. The temperature was raised to 500°C at a rate of 5°C / min. After being kept at 500°C for 2 hours, the temperature was lowered to room temperature at a rate of 5°C / min to prepare a positive electrode active material. The cross-sectional diameter of the pore structure of the positive electrode active material is 100nm, the porosity of the cross-sectional area of the positive electrode active material is 6.2%, and the specific surface area of the positive electrode active material is 2.0m 2 / g, the longest pore connection distance of the positive electrode active material is 3.0μm, the primary particle size of the positive electrode active material is 120nm, the secondary particle size of the positive electrode active material is 4μm, and the tap density of the positive electrode active material is 2.1g / cm 3 .
[0162] 2) Preparation of positive electrode sheet
[0163] The above-mentioned positive electrode active material, conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) are added to N-methylpyrrolidone in a mass ratio of 97:1:2, and mixed and stirred for 0.5-6 hours to obtain a positive electrode slurry; then the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil to prepare a positive electrode film layer, which is dried, cold pressed, and cut to obtain a positive electrode sheet.
[0164] 3) Preparation of negative electrode sheet
[0165] The negative electrode is a lithium plate.
[0166] 4) Electrolyte
[0167] In an argon atmosphere glove box (H2O <0.1ppm, O2 <0.1ppm), lithium salt LiPF6 was dissolved in an organic solvent of dimethyl carbonate / ethylene carbonate (volume ratio of 1:1) and stirred evenly to obtain an electrolyte with a lithium salt concentration of 1 mol / L.
[0168] 5) Isolation film
[0169] Polypropylene film is used as the isolation film.
[0170] 6) Preparation of button cells
[0171] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), the positive electrode sheet, separator, electrolyte and lithium sheet were assembled in sequence to form the button cell of Example 1.
[0172] 7) Preparation of batteries
[0173] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator positioned between the positive and negative electrode sheets to provide isolation. The cells are then wound to obtain a bare cell. The tabs are welded to the bare cell and placed in an aluminum shell. The cells are then baked at 80°C to remove moisture. The electrolyte is then injected and sealed to obtain an uncharged battery. The uncharged battery then undergoes a series of steps, including resting, hot and cold pressing, formation, shaping, and capacity testing, to obtain the lithium battery product of Example 1.
[0174] In Examples 2-5, the molar ratio of the flux to the positive electrode active material precursor was adjusted. Other steps were the same as in Example 1. The specific parameters are shown in Table 1.
[0175] In Example 6, the type of flux was adjusted, and the other steps were the same as in Example 1. The specific parameters are shown in Table 1.
[0176] In Examples 7, 8, 10-12, the water washing temperature was adjusted, and the other steps were the same as in Example 1. The specific parameters are shown in Table 1.
[0177] In Example 9, the type of positive electrode active material precursor was adjusted to Ni 0.83 Co 0.12 Mn 0.05 (OH)2, and the other steps are the same as in Example 1, and the specific parameters are shown in Table 1.
[0178] Table 1
[0179] Comparative Example 1
[0180] The battery of Comparative Example 1 was prepared in a similar manner to that of Example 1, but the positive electrode active material was prepared as follows:
[0181] The positive electrode active material precursor Ni 0.95 Co 0.04 Mn 0.01(OH)2 and lithium salt LiOH·H2O were mixed evenly in a molar ratio of 1:1.05, and then the mixed powder was added to a corundum porcelain boat, placed in a tube furnace, and pure oxygen was introduced at a flow rate of 0.2 liters / minute. The temperature was raised to 650°C at a rate of 5 degrees / minute. After being kept at 650°C for 12 hours, the temperature was cooled to room temperature at a rate of 5 degrees / minute to obtain a positive electrode active material. The porosity of the cross section of the positive electrode active material and the specific surface area of the positive electrode active material are 0.3m 2 / g, the primary particles of the positive electrode active material are 120nm, the secondary particles of the positive electrode active material are 4μm, and the tap density of the positive electrode active material is 2.8g / cm 3 .
[0182] The positive electrode active material and the battery of Comparative Example 2 are prepared in a similar manner to the battery of Comparative Example 1, but the positive electrode active material precursor is Ni 0.83 Co 0.12 Mn 0.05 (OH)2.
[0183] 2. Performance Testing
[0184] 1) First Coulombic efficiency test
[0185] At 2.8-4.25V, charge the button battery at 0.1C to 4.3V, then charge at constant voltage at 4.3V to a current ≤ 0.05mA, let it stand for 2 minutes, and the charging capacity at this time is recorded as C0. Then discharge it at 0.1C to 2.8V, and the discharge capacity at this time is the initial gram capacity recorded as D0. The first efficiency is calculated as D0 / C0*100%.
[0186] 2) Gram capacity test
[0187] Under a constant temperature environment of 25℃, let it stand for 5 minutes, discharge at 1 / 3C to 2.8V, let it stand for 5 minutes, charge at 1 / 3C to 4.25V, then charge at constant voltage at 4.25V to a current ≤0.05C, let it stand for 5 minutes, and then discharge at 1 / 3C to 2.8V. The discharge capacity at this time is the initial gram capacity, recorded as D0.
[0188] 3) Low temperature DC internal resistance test
[0189] In a constant temperature environment of 25℃, let it stand for 5 minutes, discharge at 1 / 3C to 2.8V, let it stand for 5 minutes, charge at 1 / 3C to 4.25V, then charge at constant voltage at 4.25V to a current ≤0.05C, let it stand for 5 minutes, and then discharge at 1 / 3C to 2.8V. The discharge capacity at this time is recorded as D0.
[0190] In a constant temperature environment of 25℃, let it stand for 30 minutes, charge to 4.25V at a current of 1 / 3D0, then charge at a constant voltage at 4.25V to a current ≤0.05D0, let it stand for 30 minutes, then discharge to the capacity position of 0.5D0 at a current of 1 / 3D0, and let it stand for 10 minutes.
[0191] The battery was placed in a constant temperature environment of -25°C for 120 minutes, discharged at a current of 0.36D0 for 10 seconds, and the voltage change ΔU at this time was recorded. According to Ohm's formula, the DC internal resistance at 50% SOC at -25°C was calculated as R50% = ΔU / (0.36D0). The lower this value, the better the battery dynamics.
[0192] 4) Battery cycle capacity retention test
[0193] At 45°C, charge at a constant current of 1C to 4.25V, then charge at a constant voltage of 4.25V until the current drops to 0.05C, and then discharge at a constant current of 1C to 2.8V. This is the first-cycle discharge capacity (Cd1). Repeat this charge and discharge cycle for the 300th cycle, and the discharge capacity after n cycles is recorded as Cdn. Capacity retention (Reten%) = discharge capacity after n cycles (Cdn) / first-cycle discharge capacity (Cd1).
[0194] 3. Analysis of test results of various embodiments and comparative examples
[0195] Batteries of various examples and comparative examples were prepared according to the above methods, and various performance parameters were measured. The results are shown in Tables 2 and 3.
[0196] Table 2
[0197] Table 3
[0198] Figure 1 is a scanning electron microscope image of a cross-section of the positive electrode active material of Example 9. Figure 2 is a scanning electron microscope image of a cross-section of the positive electrode active material of Comparative Example 2. As can be seen from the scanning electron microscope image, the positive electrode active material provided by the present disclosure is an agglomerate of primary particles, which contains pores between the primary particles. As can be seen from Figures 1, 2 and Table 1, the positive electrode active material provided by the present disclosure has a higher cross-sectional porosity and a larger pore cross-sectional diameter than the positive electrode active material in the prior art, so that the internal pores are interconnected and have a long pore connection distance.
[0199] From the comparison of the examples and comparative examples in FIG3 and Tables 2-3, it can be seen that compared with the positive electrode active materials of the same components in the prior art, the positive electrode active materials provided by the present disclosure enable the battery to have a higher specific capacity.
[0200] Figure 4 is a comparison chart of the battery cycle stability of Example 9 and Comparative Example 2. Figure 5 is a cross-sectional scanning electron microscope image of the positive electrode sheet in Example 9 after 300 cycle tests. Figure 6 is a cross-sectional scanning electron microscope image of the positive electrode sheet in Comparative Example 2 after 300 cycle tests. As can be seen from the arrows in the figure, the particles of the positive electrode active material in Comparative Example 2 are severely broken and the morphology collapses after the cycle. From the comparison of the embodiments and the comparative examples in Figures 4-6 and Tables 2-3, it can be seen that compared with the positive electrode active materials of the same components in the prior art, the positive electrode active materials provided by the present disclosure enable the battery to have high cycle stability. After 300 cycles, the positive electrode active materials of the same components in the prior art have obvious cracks inside the positive electrode active materials, resulting in serious breakage of the secondary particles of the positive electrode active materials. However, after 300 cycles, the particle morphology of the positive electrode active material provided by the present disclosure has not changed significantly.
[0201] Figure 7 shows cross-sectional porosity analysis of the positive electrode active materials of Comparative Example 2 and Example 9 within different concentric circle area ranges. Figures 1A-1F in Figure 7 show cross-sectional views of the positive electrode active material of Comparative Example 2 within concentric circle areas of 100%, 81%, 64%, 49%, 36%, and 25%, respectively, while Figures 2A-2F show cross-sectional views of the positive electrode active material of Example 9 within concentric circle areas of 100%, 81%, 64%, 49%, 36%, and 25%, respectively. The cross-sectional porosity of the positive electrode active material in Comparative Example 2 within the concentric circles of 100%, 81%, 64%, 49%, 36%, and 25% was 2.08%, 2.04%, 2.08%, 2.08%, 2.10%, and 1.94%, respectively; the cross-sectional porosity of the positive electrode active material in Example 9 within the concentric circles of 100%, 81%, 64%, 49%, 36%, and 25% was 6.25%, 7.29%, 7.71%, 8.31%, 8.98%, and 9.60%, respectively. A comparison of the examples and comparative examples in Figure 7 and Table 1 shows that the positive electrode active material provided by the present disclosure is different from the positive electrode active material in the prior art in that its porosity decreases from the geometric center of the positive electrode active material toward the surface of the positive electrode active material. This helps to further improve the diffusion and migration of lithium ions within the positive electrode active material, improve the capacity level of the battery, and help the positive electrode active material maintain the stability of its morphology and structure during the cycle.
[0202] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A positive electrode active material, characterized in that: The positive electrode active material is an aggregate of primary particles. The positive electrode active material contains pores between the primary particles. The longest connection distance of the pores is not less than 0.5 μm and can be selected from 1 μm to 5 μm.
2. The positive electrode active material according to claim 1, characterized in that The cross-sectional diameter of the pores is 10 nm to 350 nm, and can be optionally 20 nm to 200 nm.
3. The positive electrode active material according to claim 1 or 2, characterized in that: The cross-sectional porosity of the positive electrode active material is 3% to 12%, and may be 4% to 9%.
4. The positive electrode active material according to any one of claims 1 to 3, characterized in that The porosity of the positive electrode active material decreases in a direction from a geometric center of the positive electrode active material toward a surface of the positive electrode active material.
5. The positive electrode active material according to any one of claims 1 to 4, characterized in that The relationship between the cross-sectional porosity Po(C100) within the 100% concentric circle range of the positive electrode active material and the cross-sectional porosity Po(C64) within the 64% concentric circle range of the positive electrode active material on the same cross section satisfies Po(C64) / Po(C100)≥1.10; and / or, The relationship between the cross-sectional porosity Po(C100) within the 100% concentric circle range of the positive electrode active material and the cross-sectional porosity Po(C36) within the 36% concentric circle range of the positive electrode active material on the same cross section satisfies Po(C36) / Po(C100)≥1.20, The 100% concentric circle range of the positive electrode active material is the area within a distance r from the geometric center of the positive electrode active material. The 64% concentric circle range of the positive electrode active material is the area within 0.8r from the geometric center of the positive electrode active material. The 36% concentric circle range of the positive electrode active material is a region within 0.6r of the geometric center of the positive electrode active material, where r represents the radius of the positive electrode active material.
6. The positive electrode active material according to any one of claims 1 to 5, characterized in that Based on the total mass of the positive electrode active material, the residual lithium content of the positive electrode active material is 500 ppm to 3500 ppm, and can be optionally 1000 ppm to 2100 ppm.
7. The positive electrode active material according to any one of claims 1 to 6, characterized in that The general formula of the positive electrode active material is shown in Formula I: Li a Ni x M 1-x O 2-b Formula I Among them, M includes at least one of Co, Mn, Al, Y, W, Ta, Mo, Ce, La, Zr, Sr, Y, Sb, W, Ti, Mg, Nb, K, and Ca, 0.5≤a≤1.2, 0.5≤x<1.0, -0.1≤b≤0.1, and optionally, 0.8≤a≤1.2, 0.8≤x<1.
0.
8. The positive electrode active material according to any one of claims 1 to 7, characterized in that The positive electrode active material satisfies at least one of the following conditions: (i) The specific surface area of the positive electrode active material is 0.4 cm 2 / g~5cm 2 / g; (ii) the average particle size of the primary particles is 10 nm to 200 nm; (iii) The tap density of the positive electrode active material is 1.7 g / cm 3 ~2.3g / cm 3 .
9. A method for preparing a positive electrode active material, characterized in that: include: Mixing a positive electrode active material precursor, a lithium salt and a flux and performing a sintering reaction to prepare the positive electrode active material; The positive electrode active material is an aggregate of primary particles. The positive electrode active material contains pores between the primary particles. The longest connection distance of the pores is greater than 0.5 μm.
10. The preparation method according to claim 9, characterized in that: The flux includes an alkali metal salt, which may be one or more of an alkali metal sulfate and an alkali metal acetate. Optionally, the flux includes one or more of potassium sulfate, lithium sulfate, sodium sulfate, potassium acetate, lithium acetate, and sodium acetate.
11. The preparation method according to claim 9 or 10, characterized in that: The general formula of the precursor of the positive electrode active material is shown in Formula II, Ni y M 1-y (OH)2 Formula II Wherein, M includes at least one of Co, Mn, Al, Y, W, Ta, Mo, Ce, La, Zr, Sr, Y, Sb, W, Ti, Mg, Nb, K, and Ca, 0.5≤y<1.0, optionally, 0.8≤y<1.
0.
12. The preparation method according to any one of claims 9 to 11, characterized in that: The molar ratio of the flux to the positive electrode active material precursor is (0.05-0.3):1, and can be optionally (0.08-0.2):
1.
13. The preparation method according to any one of claims 9 to 12, characterized in that: The sintering reaction temperature is 500°C to 800°C, and can be 650°C to 800°C, and / or, The sintering reaction time is 10 hours to 15 hours, and can be optionally 12 hours to 14 hours.
14. The preparation method according to any one of claims 9 to 13, characterized in that: The method for preparing the positive electrode active material specifically comprises: In an oxygen atmosphere, a cathode active material precursor, a lithium salt and a flux are mixed, sintered, and then washed with water to obtain an intermediate product; The intermediate product is calcined under an oxygen atmosphere to prepare the positive electrode active material.
15. The preparation method according to claim 14, characterized in that: The water washing temperature is 4°C to 10°C.
16. The preparation method according to claim 14 or 15, characterized in that: The calcination temperature is 500° C.-650° C., and / or the calcination time is 2 h-5 h.
17. A secondary battery, characterized in that: The invention comprises a positive electrode sheet, wherein the positive electrode sheet comprises the positive electrode active material according to any one of claims 1 to 8 or the positive electrode active material prepared by the preparation method according to any one of claims 9 to 16.
18. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to claim 17.
Citation Information
Patent Citations
Cathode active material and lithium ion secondary battery containing the same
CN101414675A
Lithium battery positive electrode material, preparation method thereof and lithium battery using positive electrode material
CN107768639A
Lithium ion secondary battery
JP2012178244A
Positive electrode active substance for non-aqueous electrolyte secondary battery, method for producing same, and non-aqueous electrolyte secondary battery
US20190252680A1