Quenched and partitioned steel for automobiles and gradient partitioning preparation method therefor

By optimizing chemical composition and process design and adopting gradient partitioning technology, the problem of insufficient plasticity index of quenched partitioning steel is solved, and quenched partitioning steel for automobiles with high yield strength, tensile strength and elongation is achieved, which is suitable for more complex automotive structures and reduce production costs and process difficulty.

WO2024244041A1PCT designated stage expired Publication Date: 2024-12-05ANGANG STEEL CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/099156
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2023-06-08
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The plasticity index of existing quenched partitioned steel is difficult to reach more than 25%, limiting its application possibility in more complex structural parts.

Method used

By optimizing chemical composition and process design, a quenched steel for automobiles is provided, whose chemical composition includes elements such as C, Mn, Si, Al, Ti, P, S, and other elements, and is prepared with alloy elements such as Ni, Cr, Mo, and Nb. The methods include continuous casting, hot rolling, pickling, cold rolling and continuous retraction or continuous retraction galvanizing, and adopt a gradient partitioning process to improve the yield strength, tensile strength and elongation of the steel plate.

Benefits of technology

High-performance steel plate with yield strength of 600~700MPa, tensile strength of 980~1100MPa and elongation of 25~30%, surpassing the performance of steel plates of the same level, can be applied to more complex automotive structural parts, while reducing production costs and Process difficulty.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023099156_05122024_PF_FP_ABST
    Figure CN2023099156_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of cold-rolled high-strength steel for automobiles, and specifically relates to a quenched and partitioned steel for automobiles and a gradient partitioning preparation method therefor. The chemical composition of the steel comprises, by mass percentage: C: 0.17-0.24%, Mn: 1.60-2.40%, Si: 0.80-1.80%, Al: 0.05-0.80%, Ti: 0.015-0.025%, P: 0.007-0.012%, and S: 0.001-0.004%, the remainder being Fe and unavoidable impurities. The method comprises the following steps: continuous casting, hot rolling, pickling, cold rolling, and continuous annealing / continuous annealing galvanizing. The present invention makes a breakthrough in the mechanism of action of QP steel by means of reasonable composition and process design, and proposes a gradient partitioning process idea. The prepared QP steel product exceeds the international leading level compared with steel plates of the same grade, and can be applied to more complex automotive structural members.
Need to check novelty before this filing date? Find Prior Art

Description

Quenching and partitioning steel for automobiles and gradient partitioning preparation method thereof Technical Field

[0001] The invention belongs to the technical field of cold-rolled high-strength steel for automobiles, and particularly relates to a quenching and partitioning steel for automobiles and a gradient partitioning preparation method thereof. Background Art

[0002] The quenching and partitioning (Q&P) process, proposed by Speer et al. in 2003, is a novel process for producing high-strength, high-ductility steels with a mixed microstructure of martensite and retained austenite. The process involves the following steps: First, the steel is austenitized or partially austenitized steel and then quenched to a temperature between the start (Ms) and end (Mf) temperatures of the martensite transformation. The steel is then briefly held at this temperature to produce a certain content of martensite and untransformed austenite. Subsequently, the steel is isothermally partitioned at or above the quenching temperature to facilitate carbon diffusion and enrichment from the supersaturated martensite into the untransformed austenite, thereby stabilizing the austenite. Finally, the steel is cooled to room temperature, resulting in a final microstructure of either a mixed martensite and retained austenite or a mixed ferrite, martensite, and retained austenite. Among third-generation advanced high-strength steels, high-strength steels using the Q&P process are considered Q&P steels. With the global push for energy conservation and emissions reduction, and the continued advancement of lightweighting in automobiles, the use of third-generation advanced high-strength steel (AHSS) in body-in-white (BIW) vehicles is steadily increasing. For example, the proportion of AHSS in vehicles from brands like BMW, Toyota, and Mercedes-Benz has risen from approximately 5% around 2017 to over 15% by 2022. In Chinese automakers like BYD and Geely, the proportion of AHSS in newly released models has even risen to approximately 30%. This increasing use of AHSS is primarily driven by the continuous optimization and advancement of AHSS production and manufacturing technologies. Q&P steel represents the most widely used, best-recognized, and most mature AHSS product globally.

[0003] The Chinese standard GB / T20564.9 specifies Q&P 980 properties as yield strength ≥550 MPa, tensile strength ≥980 MPa, and elongation ≥18%. It can be used in complex body structural parts or reinforcements, such as inner and outer B-pillar panels and bumpers. However, Q&P steel's limited plasticity clearly makes it difficult to meet the requirements for more complex structural applications, such as replacing DP780, 420LA, or even DP590. The Japan Advanced Materials Research Institute (JRI) has set a plasticity target of 35% for 980 MPa-grade advanced high-strength steel. At that point, 980 MPa-grade products could replace nearly all existing body structural parts from a formability perspective. Of course, achieving a plasticity target of 35% requires new, innovative design mechanisms and correspondingly upgraded equipment and processes. Therefore, currently, achieving a plasticity of over 25% to around 30% is a feasible goal in the short term.

[0004] Chinese patent CN202010319605.2 discloses a method for manufacturing 980 MPa cold-rolled Q&P steel with excellent ductility. The steel's components, by weight, are as follows: C: 0.18-0.21%, Mn: 1.8-2.1%, Si: 1.4-1.6%, Al: 0.02-0.06%, P ≤ 0.02%, S ≤ 0.01%, Nb: 0.04-0.06%, with the balance being Fe and other unavoidable impurities. The preparation method includes smelting, hot rolling, annealing, pickling, cold rolling, and continuous annealing, resulting in a steel plate with a tensile strength of 982-1065 MPa and an elongation of 18.8-24.9%.

[0005] Chinese patent CN201810144307.7 discloses 980 MPa-grade cold-rolled high-strength Q&P steel for automotive use and its production method. The steel's alloy composition is C: 0.18-0.24%, Si: 0.6-1.3%, Mn: 1.6-2.4%, Nb: 0.04-0.07%, Als: 0.5-1.0%, P: 0.02-0.04%, S ≤ 0.005%, with the balance being Fe and other unavoidable impurities. The preparation method includes smelting, hot rolling, annealing, pickling, cold rolling, and continuous annealing. The resulting steel plate has yield strength ≥ 550 MPa, tensile strength ≥ 980 MPa, and elongation ≥ 18%. The maximum elongation in the embodiment is 23.5%. This shows that, based on the existing composition and process system, Q&P steel is difficult to achieve a plasticity index exceeding 25%.

[0006] Summary of the Invention

[0007] In order to solve the above technical problems, the present invention provides a quenching and partitioning steel for automobiles and a gradient partitioning preparation method thereof. Based on the existing equipment conditions, higher-dimensional plasticity indicators of Q&P steel products are achieved, thereby greatly improving the possibility of Q&P steel products being applied in vehicle bodies.

[0008] In order to achieve the above object, the technical solution of the present invention is as follows:

[0009] On one hand, the present invention provides a quenching and partitioning steel for automobiles. The chemical composition of the steel comprises, by mass percentage, the following: C: 0.17% to 0.24%, Mn: 1.60% to 2.40%, Si: 0.80% to 1.80%, Al: 0.05% to 0.80%, Ti: 0.015% to 0.025%, P: 0.007% to 0.012%, S: 0.001% to 0.004%, and the balance being Fe and unavoidable impurities.

[0010] In the above technical solution, further, the chemical composition of the steel may also include one or more of Ni, Cr, Mo, and Nb; wherein, in terms of mass percentage, Ni: 0.1% to 0.30%, Cr: 0.1% to 0.30%, Mo: 0.05% to 0.30%, and Mn+Ni+Cr+Mo≤2.50%, Nb: 0.01% to 0.025%.

[0011] In the above technical solution, further, the steel has a yield strength of 600-700 MPa, a tensile strength of 980-1100 MPa, and an elongation of 25%-30%.

[0012] In the above technical solution, further, the microstructure of the steel is composed of 40% to 60% ferrite, 20% to 30% martensite, 10% to 20% bainite and 10% to 20% retained austenite by volume percentage, wherein the ferrite is intercritical ferrite and oriented epitaxial ferrite.

[0013] The selection principles and content design reasons of the chemical components of the steel of the present invention are as follows:

[0014] C: C is the most economical strong element in steel, which improves the hardenability of steel plates and thus increases the strength of steel plates. In the Q&P steel of the present invention, C is the most critical factor, affecting the phase transformation behavior of supercooled austenite. The relatively enriched C in the supercooled austenite during the cooling stage ensures the content of martensite transformed during the transformation process. At the same time, the untransformed supercooled austenite relies on the C diffusion of the surrounding martensite to improve stability during the isothermal partitioning stage, and is then retained as residual austenite. However, too high a C content will increase the risk of hot-rolled edge cracking and cold-rolled edge cracking in industrial production. In addition, too high a C content will lead to the formation of a high proportion of twin martensite at the spot welding nugget, deteriorating the welding performance. Therefore, the present invention controls the C element content to 0.17% to 0.24%.

[0015] Mn: Mn is a common economical strengthening element in steel, which improves the solid solution strengthening effect and the hardenability of the steel plate, thereby improving the overall strength of the steel plate. In the Q&P steel of the present invention, the Mn element mainly plays a role in reducing the cooling rate in the critical zone and increasing the proportion of martensite in the rapid cooling stage; at the same time, it is combined with the addition of C to improve the stability of the austenite phase. However, the added content of the Mn element should not exceed the scope of the present invention, considering the problem of C / Mn segregation caused by excessive Mn content. Therefore, the present invention controls the Mn element content to 1.60% to 2.40%.

[0016] Si: Si is a common economical strengthening element that ensures the matrix strength of ferrite. Simultaneously, Si addition increases the AC3 point of the steel plate, effectively adjusting the annealing process window during the continuous annealing stage and ensuring an appropriate ferrite-austenite ratio in the critical zone at industrial continuous annealing temperatures. In the Q&P steel of the present invention, the primary role of Si addition is that sufficient Si addition can inhibit the formation of carbides during the over-aging stage, preventing the steel plate from degrading due to carbide precipitation. It is worth noting that in the production of galvanized products, excessive Si content can lead to "skipping" on the galvanized surface, affecting surface quality. Therefore, the present invention controls the Si content to between 0.80% and 1.80%.

[0017] Al: Al is added to conventional steel plates in limited quantities, generally serving as a deoxidizer during the smelting process. In the present invention, a relatively high content of Al is added during the galvanized product manufacturing stage to replace Si, inhibiting carbide precipitation. However, excessive Al substitution should not be excessively high, as this can lead to difficulties in tapping during the continuous casting crystallization phase, an upward shift in the soaking window during continuous annealing and galvanizing, and increased production complexity. In the present invention, the Al content is controlled between 0.05% and 0.80%.

[0018] Ti: In conventional steel plates, Ti acts as a nitrogen binder. In the present invention, Ti is appropriately added to supplement strength. If some planned components fail to meet strength requirements, Ti precipitation can be used to refine the original austenite grains, strengthening them and providing precipitation strengthening to supplement strength. In the present invention, the Ti content is controlled to 0.015-0.025%.

[0019] P: P is an impurity element in steel that easily segregates at grain boundaries. When the P content is high, Fe2P particles are easily formed, reducing the plasticity and toughness of the steel. Therefore, the lower the P content, the better. In the present invention, the P content is controlled to 0.070% to 0.012%.

[0020] S: S is an impurity element in steel. It easily combines with Mn to form MnS inclusions, which deteriorates the plasticity of the steel plate. Therefore, the lower its content, the better. In the present invention, the S content is controlled to 0.001% to 0.004%.

[0021] You can also add elements:

[0022] Ni: A solid solution strengthening element, like C and Mn, it improves austenite stability. Ni also improves the corrosion resistance of the steel plate to a certain extent. Ni can be added to the optional components of the present invention in appropriate amounts to improve corrosion resistance. In this invention, the Ni content is controlled to 0.10% to 0.30%.

[0023] Cr and Mo: Cr and Mo are solid solution strengthening elements that strengthen the steel plate. In the present invention, Cr and Mo can improve the hardenability of the steel plate, delay the formation of pearlite and bainite during the cooling stage, and promote the formation of martensite. At the same time, Cr and Mo can change the type of iron oxide scale during the coiling process, limit the oxidation process within the steel plate, and improve the surface quality of the steel plate. In the present invention, Cr and Mo are added after Mn is added to balance the problems of hot-rolled edge cracking and cold-rolled edge cracking. Therefore, in the present invention, the Cr content is controlled at 0.10% to 0.30%, and the Mo content is controlled at 0.05% to 0.30%.

[0024] As mentioned above, alloying elements such as Ni, Cr, and Mo are all substitutes for Mn. Their primary function in the present invention is to enhance and stabilize austenite. However, considering multiple factors, including cost, difficulty in casting steel, hot rolling, and cold rolling, their overall addition should meet the integrated goals of low cost, easy production, and high yield. Therefore, the Mn+Ni+Cr+Mo content of the present invention is ≤ 2.5%.

[0025] Nb: Nb is a microalloying strengthening element that refines grains and increases strength. In the present invention, Nb is added in conjunction with Ti to partially compensate for the low strength of the designed composition. However, excessive Nb content should not be added, as it will lead to excessively fine grains during hot rolling, excessively high hot-rolled coil strength, and increased difficulty in cold rolling. In the present invention, the Nb content is controlled to 0.01% to 0.025%.

[0026] Another aspect of the present invention provides a method for preparing the above-mentioned quenching and partitioning steel for automobiles by gradient partitioning, the method comprising the following steps: continuous annealing or continuous annealing galvanizing;

[0027] The specific steps of the method are as follows:

[0028] Continuous retreat:

[0029] The cold-rolled sheet is heated to 800-830°C, held isothermal for 80-180s, slowly cooled to 700-740°C at a cooling rate of 1.2-3.6°C / s, and then rapidly cooled to 250-280°C at a rate of 15-25°C / s. The sheet is then heated to 380-410°C at a rate of more than 20°C / s for a first-stage over-aging treatment, with an isothermal time of 120-280s. As the sheet temperature rises, the sheet enters a second-stage over-aging treatment, with an aging temperature of 300-380°C and an isothermal time of 120-280s.

[0030] Or continuous galvanizing:

[0031] The cold-rolled sheet is heated to 820-860°C, held at this temperature for 60-120 seconds, and then slowly cooled to 700-740°C at a cooling rate of 1.2-3.6°C / s. The sheet is then rapidly cooled to 250-280°C at a rate of 18-25°C / s. The sheet is then heated to 480-510°C at a rate of more than 20°C / s for over-aging treatment. The isothermal time is 20-40 seconds. After over-aging treatment, the sheet enters the zinc pot at a temperature of 450-470°C and is kept in the zinc pot for 2-5 seconds.

[0032] In the above technical solution, further, the thickness of the cold-rolled steel plate is 1.4 / 1.6 / 1.8 mm, the 1.4 mm plate thickness corresponds to the 2.8 mm hot-rolled steel plate, and the 1.6 mm and 1.8 mm plate thicknesses correspond to the 3.0-3.5 mm hot-rolled steel plate.

[0033] The reasons for designing the preparation steps of the present invention are as follows:

[0034] During the soaking stage of continuous annealing / continuous galvanizing (continuous annealing temperature 800-830℃, isothermal 80-180s or continuous annealing 820-860℃, isothermal 60-120s), 35%-45% critical zone ferrite structure is obtained to balance the strength of the steel plate and ensure the C concentration in the austenite under the austenitization degree; slowly cool to 700-740℃ at a rate of 1.2-3.6℃ / s to obtain 5%-10% oriented epitaxial ferrite to prevent ferrite from containing Too high austenite content leads to reduced strength, while too low a ferrite content leads to excessively high strength. More importantly, the C concentration gradient of the supercooled austenite after slow cooling and before rapid cooling is guaranteed, which in turn determines the transformation amount of bainite and martensite in the subsequent process. Subsequently, the steel is cooled to 250-280°C at a higher cooling rate to obtain 25%-30% martensite structure and the remaining untransformed supercooled austenite structure. Too low a martensite content leads to reduced strength of the steel plate, while too high a martensite content leads to a reduction in the retained austenite content.

[0035] The key processes of continuous annealing / continuous galvanizing are: 1. Rapid heating rate (above 20°C / s). Slow heating will inhibit the transformation of the remaining supercooled austenite in the steel sheet to bainite. This is because the carbon concentration required for the bainite phase transformation termination line T0 gradually decreases during the slow heating process. 2. Gradient partitioning: The present invention adopts a two-stage partitioning process, with the temperature of the first stage higher than that of the second stage, forming a cooling gradient. This is because the slow cooling process (the steel sheet cools naturally in the furnace) will significantly shift the bainite phase transformation termination line T0 to the right, increasing the carbon concentration at the required termination point, delaying the end of the bainite transformation, and significantly increasing the retained austenite content of the steel sheet to over 15%. The retained secondary martensite content is theoretically the lowest, significantly improving the steel sheet's formability. As a result, after the pre-processing, 25% to 30% of the supercooled austenite forms 12% to 15% of bainite and 15% to 18% of retained austenite, thereby achieving an elongation of over 25%.

[0036] In the above technical solution, further, the method for preparing the cold-rolled sheet comprises the following steps: continuous casting, hot rolling, pickling, and cold rolling;

[0037] The specific steps of the method are as follows:

[0038] (1) Continuous casting: Continuous casting is carried out according to the chemical composition of steel;

[0039] (2) Hot rolling: heating temperature is 1230-1280℃, furnace time is 180-240min, rough rolling temperature is 1150-1200℃, intermediate billet thickness is 50-80mm, finishing rolling temperature is 1070-1130℃, final rolling temperature is above 920℃, coiling temperature is 450-520℃, and hot rolled steel plate thickness is 2.8-3.5mm;

[0040] (3) Pickling and cold rolling: After pickling, cold rolling is performed, and the cold rolling reduction rate is 46.7% to 48.6%.

[0041] In the above technical solution, further, in step (1), the casting temperature is 1580-1620°C, and the thickness of the ingot is 220-280 mm.

[0042] The reasons for designing each step of cold-rolled sheet preparation of the present invention are as follows:

[0043] In step (2), the heating temperature is controlled at 1230-1280°C and the furnace time is 180-240 minutes, in order to promote full solid solution of the alloy and control the banded structure caused by segregation. The finishing rolling stage is divided into two stages to promote the recrystallization behavior of the original austenite grains and inhibit the coarsening of the unrecrystallized austenite grains; the coiling temperature is controlled at 450-520°C to prevent the formation of Si-rich oxides on the surface of the steel plate after the addition of Si content, which in turn leads to the formation of internal oxide layers and grain boundary oxide layers.

[0044] In step (3), too low a rolling reduction rate cannot ensure sufficient cold rolling deformation energy storage, resulting in insufficient ferrite recrystallization effect in the continuous annealing stage; too high a rolling reduction rate greatly increases the load of the cold rolling mill and cannot ensure the target thickness is achieved.

[0045] The beneficial effects of the present invention are:

[0046] (1) The present invention breaks through the plasticity limitation mechanism of QP steel through reasonable composition and process design, proposes a gradient partitioning process idea, gives full play to the advantages of bainite matrix configuration, realizes the optimal design of retained austenite content and the best coordinated deformation ability of the organization, and the QP steel product produced by the present invention has a yield strength of 600-660MPa, a tensile strength of 980-1100MPa, and an elongation of 25-31%. Compared with the same grade steel plate, it exceeds the international leading level and can be used in more complex automotive structural parts;

[0047] (2) The present invention is based on existing equipment conditions and has the advantages of low production cost and stable production process;

[0048] (3) The QP steel product of the present invention can achieve lightweighting of automobiles, reduce weight and exhaust emissions from the application end, and meet the dual carbon strategy. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] FIG1 is a scanning structure of Example 1 of the present invention. DETAILED DESCRIPTION

[0050] The present invention will be described in more detail by way of examples. These examples are merely descriptions of the best mode of carrying out the present invention and do not limit the scope of the present invention in any way.

[0051] Examples 1-10

[0052] The chemical compositions of the automotive quenching and partitioning steels provided in Examples 1-10 are shown in Table 1.

[0053] Table 1 Chemical composition of steels of Examples 1-10, wt%

[0054] The gradient partitioning preparation method of the quenching and partitioning steel for automobiles comprises the following steps: continuous casting, hot rolling, pickling, cold rolling, continuous annealing or continuous annealing galvanizing;

[0055] The specific steps are as follows:

[0056] (1) Continuous casting: Continuous casting is carried out according to the chemical composition of the steel, with a casting temperature of 1580-1620°C and a billet thickness of 220-280 mm;

[0057] (2) Hot rolling: heating temperature is 1230-1280℃, furnace time is 180-240min, rough rolling temperature is 1150-1200℃, intermediate billet thickness is 50-80mm, finishing rolling temperature is 1070-1130℃, final rolling temperature is above 920℃, coiling temperature is 450-520℃, and hot rolled steel plate thickness is 2.8-3.5mm;

[0058] (3) Pickling and cold rolling: After pickling, cold rolling is carried out. The thickness of the cold rolled steel plate is 1.4 / 1.6 / 1.8 mm. The thickness of 1.4 mm corresponds to the hot rolled steel plate of 2.8 mm, and the thickness of 1.6 and 1.8 mm corresponds to the hot rolled steel plate of 3.0-3.5 mm. The cold rolling reduction rate is 46.7-48.6%.

[0059] (4) Continuous retreat:

[0060] The cold-rolled sheet is heated to 800-830°C, held isothermal for 80-180s, slowly cooled to 700-740°C at a cooling rate of 1.2-3.6°C / s, and then rapidly cooled to 250-280°C at a rate of 15-25°C / s. The sheet is then heated to 380-410°C at a rate of more than 20°C / s for a first-stage over-aging treatment, with an isothermal time of 120-280s. As the sheet temperature rises, the sheet enters a second-stage over-aging treatment, with the aging temperature controlled at 300-380°C and an isothermal time of 120-280s.

[0061] Or continuous galvanizing:

[0062] The cold-rolled sheet is heated to 820-860°C, held at this temperature for 60-120 seconds, and then slowly cooled to 700-740°C at a cooling rate of 1.2-3.6°C / s. The sheet is then rapidly cooled to 250-280°C at a rate of 18-25°C / s. The sheet is then heated to 480-510°C at a rate of more than 20°C / s for over-aging treatment. The isothermal time is 20-40 seconds. After over-aging treatment, the sheet enters the zinc pot at a temperature of 450-470°C and is kept in the zinc pot for 2-5 seconds.

[0063] Table 2 lists the continuous casting and hot rolling process parameters of the steels of Examples 1-10, and Table 3 lists the cold rolling and continuous annealing / continuous annealing galvanizing process parameters of the example steels.

[0064] Table 2 Continuous casting and hot rolling process parameters of steels of Examples 1-10

[0065] Table 3 Cold rolling and continuous annealing / continuous annealing galvanizing process parameters of steels in Examples 1-10

[0066] Table 4 lists the mechanical properties of the steels of Examples 1-10.

[0067] Table 4 Mechanical properties of steels in Examples 1-10

[0068] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. The scope of protection of the present invention shall be determined by the scope defined in the claims. Other variations or modifications may be made based on the above description. Obvious variations or modifications derived therefrom shall remain within the scope of protection of the present invention.

Claims

1. A quenching and partitioning steel for automobiles, characterized in that: The chemical composition of the steel includes, by mass percentage, C: 0.17% to 0.24%, Mn: 1.60% to 2.40%, Si: 0.80% to 1.80%, Al: 0.05% to 0.80%, Ti: 0.015% to 0.025%, P: 0.007% to 0.012%, S: 0.001% to 0.004%, and the balance is Fe and unavoidable impurities.

2. The quenching and partitioning steel for automobiles according to claim 1, characterized in that: The chemical composition of the steel may also include one or more of Ni, Cr, Mo, and Nb; wherein, by mass percentage, Ni: 0.10% to 0.30%, Cr: 0.10% to 0.30%, Mo: 0.05% to 0.30%, and Mn+Ni+Cr+Mo≤2.50%, Nb: 0.01% to 0.025%.

3. The quenching and partitioning steel for automobiles according to claim 1, characterized in that: The steel has a yield strength of 600-700 MPa, a tensile strength of 980-1100 MPa, and an elongation of 25%-30%.

4. The quenching and partitioning steel for automobiles according to claim 1, characterized in that: The microstructure of the steel consists of 40% to 60% ferrite, 20% to 30% martensite, 10% to 20% bainite and 10% to 20% residual austenite by volume percentage, wherein the ferrite is intercritical ferrite and oriented epitaxial ferrite.

5. A method for preparing a gradient partitioning of a quenching and partitioning steel for automobiles according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: continuous annealing or continuous galvanizing; The specific steps of the method are as follows: Continuous retreat: The cold-rolled sheet is heated to 800-830°C, isothermal for 80-180s, slowly cooled to 700-740°C at a cooling rate of 1.2-3.6°C / s, and then rapidly cooled to 250-280°C at a rate of 15-25°C / s, and then heated to 380-410°C at a rate of more than 20°C / s for a first-stage over-aging treatment, with an isothermal time of 120-280s; the second-stage over-aging treatment is carried out with the sheet temperature, with an aging temperature of 300-380°C and an isothermal time of 120-280s; Or continuous galvanizing: The cold-rolled sheet is heated to 820-860°C, kept isothermal for 60-120s, slowly cooled to 700-740°C at a cooling rate of 1.2-3.6°C / s, and then rapidly cooled to 250-280°C at a rate of 18-25°C / s, and then heated to 480-510°C at a rate of more than 20°C / s for aging treatment. The isothermal time is 20-40s. After aging treatment, it enters the zinc pot at a temperature of 450-470°C and stays in the zinc pot for 2-5s.

6. The preparation method according to claim 5, characterized in that: The thickness of the cold-rolled steel plate is 1.4 / 1.6 / 1.8 mm, the thickness of 1.4 mm corresponds to the hot-rolled steel plate of 2.8 mm, and the thickness of 1.6 mm and 1.8 mm corresponds to the hot-rolled steel plate of 3.0-3.5 mm.

7. The preparation method according to claim 5, characterized in that: The method for preparing the cold-rolled sheet comprises the following steps: continuous casting, hot rolling, pickling, and cold rolling; The specific steps of the method are as follows: (1) Continuous casting: Continuous casting is carried out according to the chemical composition of steel; (2) Hot rolling: heating temperature is 1230-1280°C, furnace time is 180-240 min, rough rolling temperature is 1150-1200°C, intermediate billet thickness is 50-80 mm, finishing rolling temperature is 1070-1130°C, final rolling temperature is above 920°C, coiling temperature is 450-520°C, and hot rolled steel plate thickness is 2.8-3.5 mm; (3) Pickling and cold rolling: After pickling, cold rolling is performed, and the cold rolling reduction rate is 46.7% to 48.6%.

8. The preparation method according to claim 7, characterized in that: In step (1), the casting temperature is 1580-1620°C, and the thickness of the ingot is 220-280 mm.

Citation Information

Patent Citations

  • Q-P (quenching and partitioning) steel plate and twice partitioning preparation method thereof

    CN105734213A

  • Method for producing high strength steel sheet having improved ductility and formability, and obtained steel sheet

    CN108474057A

  • Preparation method of martensite matrix 1,100-MPa-grade rare earth Q and P steel

    CN109136779A

  • Q&P steel plate with high strength-elongation product and excellent welding performance and preparing method thereof

    CN110093552A

  • 980 MPa grade quenching distribution steel and preparation method thereof

    CN111118397A