Isotropic low-yield-ratio high-toughness bridge steel and manufacturing method therefor

By optimizing chemical composition and production process, the shortcomings of bridge steel plates in terms of high strength, low temperature toughness, weather resistance and weldability are solved, high strength, low yield and excellent weather resistance are achieved, and construction efficiency and safety performance are improved.

WO2024244043A1PCT designated stage expired Publication Date: 2024-12-05ANGANG STEEL CO LTD
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/099169
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2023-06-08
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing bridge steel plates have shortcomings in high strength, low temperature toughness, weather resistance, weldability and isotropy, resulting in low construction efficiency, poor safety performance, complex production process and high cost.

Method used

By optimizing chemical composition and production processes, low C and low Mn are used to improve welding performance and toughness, Nb and Ti elements are used to refine grains, increase Cr and Mo and other elements to improve weather resistance and hardenability, combined with specific smelting and heating , rolling and heat treatment processes to produce isotropic steel plates with high strength, low yield ratio, excellent weather resistance and welding properties.

Benefits of technology

The high strength, low yield-strength ratio, good weather resistance and welding performance of steel plates are achieved, production costs are reduced, construction efficiency and safety performance are improved, and the needs of large-span bridges are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023099169_05122024_PF_FP_ABST
    Figure CN2023099169_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are an isotropic low-yield-ratio high-toughness bridge steel and a manufacturing method therefor. The chemical composition weight percentages thereof are: C: 0.02-0.05%, Si: 0.25-0.45%, Mn: 1.00-1.40%, P≤0.01%, S≤0.003%, Nb: 0.02-0.05%, Ni: 0.40-0.70%, Cu: 0.25-0.45%, Mo: 0.10-0.20%, Cr: 0.50-0.80%, Ti: 0.005-0.02%, B: 0.001-0.0025%, Al: 0.01-0.04%, CEV: 0.36-0.52%, Pcm: 0.13-0.20%, and I≥6.30, the balance being iron and unavoidable impurities. The steel of the present invention has excellent weather resistance and welding performance, the performance of an entire plate is uniform, and the difference between transverse and longitudinal performance is extremely small.
Need to check novelty before this filing date? Find Prior Art

Description

Isotropic low-yield-to-strength ratio high-toughness bridge steel and manufacturing method thereof Technical Field

[0001] The present invention belongs to the field of metal materials, and in particular relates to an isotropic low-yield-to-strength ratio high-toughness bridge steel and a manufacturing method thereof. Background Art

[0002] As large steel bridges develop towards fully welded structures and high parameters, the safety and reliability requirements for bridge structures are becoming increasingly stringent. This not only places higher demands on designers, but also on the quality of steel plates. Specifically, they must not only have high strength to meet lightweight structural requirements, but also possess excellent low-temperature toughness, weldability, and corrosion resistance to meet the safety, reliability, and longevity requirements of steel structures.

[0003] Traditional high-strength bridge steel not only has poor impact toughness, weldability, yield strength ratio, and isotropy, but also lacks resistance to atmospheric corrosion. At the same time, different bridge structure types require a large amount of cutting and welding of equal-section steel plates, which seriously affects construction efficiency and quality. Therefore, domestic and foreign material workers have put forward higher requirements for the new generation of bridge steel. In addition to having higher strength, the steel's weldability, low-temperature toughness, seismic resistance, processability, corrosion resistance, performance uniformity, etc. have been greatly improved.

[0004] At present, existing bridge steels can already meet most of the market demands in the bridge field, but special steels with high strength levels and excellent comprehensive performance are still the development goals of countries around the world. Ultra-high-strength steel plates with high service safety have high scientific research difficulties, strict production processes, high equipment requirements, and are difficult to develop. The complexity and diversity of technical characteristics and indicators have significantly increased the difficulty of research and development of isotropic low-yield ratio and high-toughness bridge steels. First, the increase in steel plate thickness will lead to large differences in deformation from the surface to the core of the steel plate during rolling, reduced cooling uniformity in the thickness direction, and poor isotropy. Thirdly, for variable-section bridge steels, due to the different rolling temperatures and deformation amounts at the thin and thick ends, their strength and toughness uniformity is also difficult to control. At the same time, bridge steels need to have good corrosion resistance and welding properties, and further optimization of the composition is required.

[0005] At present, there are some studies on high-strength, toughness, weather-resistant bridge steel plates at home and abroad. After searching, some patents and literature were found, but the contents recorded therein are obviously different from the composition, production method, performance, product category and other aspects described in the technical solution of the present invention.

[0006] Patent CN 109797342 A discloses a high-strength, high-toughness, atmospheric corrosion-resistant steel plate for steel structure production and its manufacturing method. The chemical composition, calculated by mass fraction, includes: C: 0.03% to 0.10%, Si: 0.30% to 0.50%, Mn: 1.10% to 1.50%, P < 0.010%, S < 0.003%, Cr: 0.45% to 0.70%, Cu: 0.25% to 0.40%, Ni: 0.30% to 0.40%, Alt: ≥ 0.030%, Ti: 0.006% to 0.030%, V: 0.040% to 0.080%, Mo: 0.02%~0.08%, Ca: 0.0010%~0.0030%, N: 0.0020%~0.0080%, B: 0.0002%~0.0030%, Ce: 0.001%~0.010%, atmospheric corrosion resistance index I>6.5, CEV<0.54, Pcm<0.27, the balance is Fe and unavoidable impurities. This patent adopts chemical composition design and steel plate modulation process to obtain high-performance steel plates with bainite structure, which can be used in the production of steel structures such as bridges and high-rise buildings. However, the steel plates obtained by this patent do not have a low yield strength ratio and poor safety performance. The addition of rare elements such as Ca, B, and Ce makes smelting difficult, increasing production costs. In addition, the carbon equivalent is too high, the welding performance is poor, and tempering treatment is required, which is a complicated process.

[0007] Patent CN 107557665 A discloses a rare earth weathering bridge steel plate with a yield strength of 345 MPa and a production method thereof. The chemical composition, calculated by mass fraction, includes: C: 0.04% to 0.06%, Si: 0.20% to 0.30%, Mn: 1.10% to 1.30%, P < 0.015%, S < 0.008%, Cr: 0.40% to 0.50%, Cu: 0.25% to 0.35%, Ni: 0.30% to 0.40%, Als: 0.024% to 0.034%, Nb: 0.01% to 0.02%, Ce: 0.0005% to 0.0030%, and the balance is Fe and unavoidable impurities. This steel plate has the advantages of low yield ratio, good corrosion resistance, low-temperature toughness, cold forming performance, welding performance, and can be used without painting; but its strength is low and cannot meet the requirements of large-span steel bridges. The addition of rare earth elements makes smelting difficult and increases production costs.

[0008] Patent CN 110541117 A discloses a 620MPa-grade, high-performance bridge steel welded at a low preheat temperature and its preparation method. The chemical composition, by mass, includes: C: 0.051% to 0.091%, Si: 0.41% to 0.50%, Mn: 1.65% to 2.15%, P < 0.010%, S < 0.003%, Nb: 0.06% to 0.09%, Ti: 0.015% to 0.03%, Cr: 0.35% to 0.65%, Ca: 0.0019% to 0.0045%, Ce: 0.02% to 0.04%, with the balance being Fe and unavoidable impurities. By controlling the composition and production process, the resulting steel exhibits excellent strength, low-temperature toughness, and weldability. The preheat temperature for welding is ≤ 30°C, making it suitable for highway bridges, railway bridges, and dual-use bridges. However, the steel plate does not have a low yield strength ratio, low elongation, poor seismic performance, and no weather resistance, and its overall performance is poor.

[0009] Patent CN 108396245 A discloses a 345MPa-grade wedge-shaped steel plate with one end thinner and the other thicker. This plate is cast from two tanks of molten steel with different compositions into a continuous casting billet whose chemical composition varies along its length, followed by rolling. This allows the rolled wedge-shaped steel plate to have uniform mechanical properties. However, the process is complex and difficult to implement in actual production. Furthermore, the plate is only suitable for wedge-shaped steel plates with one end thinner and the other thicker, and its strength is only 345MPa. It lacks weather resistance and cannot meet the requirements for long-span bridge structures.

[0010] In summary, the existing technology for the research of bridge steel plates is still insufficient. At present, the main problems of bridge steel plates are as follows:

[0011] 1. A large amount of rare elements are added, making smelting difficult and the cost high.

[0012] 2. High-strength steel plates require tempering heat treatment, the production process is complex, and the production cycle is long.

[0013] 3. The steel plates are of uniform cross-section and cannot meet the actual personalized needs of users.

[0014] 4. The steel plate has low strength and poor toughness, and cannot meet the requirements of bridge projects in cold areas.

[0015] 5. The yield strength ratio of the steel plate is relatively high and the isotropy is poor, which has a certain impact on the seismic safety of the bridge.

[0016] 6. Steel plates are not weather-resistant and require painting, which is not environmentally friendly.

[0017] Summary of the Invention

[0018] The present invention aims to overcome the shortcomings of the prior art by providing an isotropic, low-yield-ratio, high-toughness bridge steel and a method for manufacturing the same. The product, produced according to the chemical composition and production process requirements of the present steel, exhibits ultra-high strength, high toughness, a low yield ratio, high plasticity, and excellent weather resistance and weldability. The performance is uniform across the entire plate, with minimal differences in transverse and longitudinal properties.

[0019] The composition design of the present invention improves the material's welding performance and toughness through low C and Mn content. Nb and Ti elements are used to inhibit austenite grain growth and promote nucleation during austenite transformation, thereby refining the grains, controlling the core structure of the steel plate thickness, and improving structural uniformity. Nb is used to inhibit austenite recrystallization, increase rolling temperatures, promote grain refinement, and ensure the steel plate's shape. Cr, Mi, Cu, and other elements are also used to improve the steel plate's weather resistance. The combined addition of Cr and Mo can also increase the steel plate's hardenability, increase the cooling rate during air or water cooling, and refine the grains, achieving increased strength and uniformity of the structure through the thickness. Combined with appropriate smelting, heating, rolling, and heat treatment processes, the steel plate achieves comprehensive properties such as multiple shapes, large thickness, high strength and toughness, a low yield ratio, excellent weather resistance, weldability, and isotropy, as well as an ideal microstructure.

[0020] In order to achieve the above object, the technical solution of the present invention is as follows:

[0021] In one aspect, the present invention provides an isotropic bridge steel with a low yield ratio and high toughness, the chemical composition of which is as follows by weight:

[0022] C: 0.02% ~ 0.05%, Si: 0.25% ~ 0.45%, Mn: 1.00% ~ 1.40%, P ≤ 0.010%, S ≤ 0.003%, Nb: 0.02% ~ 0.05%, Ni: 0.40% ~ 0.70%, Cu: 0.25% ~ 0.45%, Mo: 0.10% ~ 0.20%, Cr: 0.50 ~ 0.80%, Ti: 0.005% ~ 0.020%, B: 0.0010% ~ 0.0025%, Al: 0.01% ~ 0.04%, CEV: 0.36% ~ 0.52%, Pcm: 0.13% ~ 0.20%, atmospheric corrosion resistance index I ≥ 6.30, the balance is iron and unavoidable impurities.

[0023] In the above technical solution, further, the final microstructure of the steel plate is composed of ferrite, pearlite, and bainite; wherein, by volume percentage, ferrite is 11-28%, pearlite is 3-7%, and bainite is 69-82%.

[0024] In the above technical solution, further, the yield strength of the steel plate is ≥500MPa, the tensile strength is ≥630MPa, the elongation after fracture is ≥21%, the yield strength ratio is ≤0.83, and the impact energy at -40℃ is ≥200J; the yield strength difference between the thin and thick ends of the same plate is ≤25MPa, the tensile strength difference is ≤25MPa, the elongation difference after fracture is ≤3%, the yield strength ratio difference is ≤0.02, and the impact energy difference at -40℃ is ≤30J; the tensile strength ratio between the transverse and longitudinal directions at the same position is ≤5%, and the impact energy ratio is ≤5%.

[0025] The selection principles and content design reasons of the chemical components of the present invention are as follows:

[0026] C: The C content in this invention can strengthen the steel through interstitial solid solution and react with alloying elements such as Nb to form fine carbides. These carbides precipitate before rolling deformation or austenite transformation, hindering grain growth, increasing the nucleation rate, and refining the microstructure. However, excessive C content can lead to the formation of distinct banded structures during rolling, severely impacting the uniformity of the steel's properties in all directions. Furthermore, excessive C content increases the carbon equivalent of the steel, deteriorating its weldability and low-temperature toughness. Therefore, the C content should be kept within a range of 0.02% to 0.05%.

[0027] Si: Si is a deoxidizing element in steel and has a strong solid solution strengthening effect. It can purify ferrite and reduce the pearlite content, which helps reduce the Bauschinger effect of the base material and lower the yield ratio of the steel plate. However, excessive Si can reduce the toughness of the base material's weld heat-affected zone, deteriorating the steel's toughness and weldability. Therefore, in the present invention, the Si content is preferably controlled within a range of 0.25% to 0.45%.

[0028] Mn: Mn can be dissolved in a large amount in the Fe matrix. It is an element that expands the austenite phase region, improves the stability of austenite, inhibits the growth of phase transformation grains before accelerated cooling of the steel plate, plays a role in refining grains, and improves the strength of the steel plate. When the Mn content is less than 1.0%, it has little effect on the strength of the steel plate. However, if the Mn content is too high, it will easily inhibit the ferrite transformation, affect the yield strength of the steel, and is not conducive to reducing the yield strength ratio. Too high a Mn content will induce segregation, resulting in more banded structures, deteriorating the uniformity of the steel plate structure and the lamellar tearing performance in the thickness direction, while affecting the consistency of the isotropic properties and being not conducive to welding. The present invention believes that it is more appropriate to control the Mn content within 1.00% to 1.40%.

[0029] P and S: P and S are harmful impurity elements in this invention; the lower their content, the better. Excessive P content can lead to structural segregation, significantly adversely affecting isotropy and low-temperature toughness. This invention limits P to ≤ 0.010%. Increased S content promotes the formation and growth of inclusions, deteriorating low-temperature and through-thickness properties. Therefore, S is ≤ 0.003%.

[0030] Nb: The functions of Nb in this invention include: (1) precipitation during rolling, pinning grain boundaries, promoting nucleation, and effectively refining grains, thereby increasing strength and improving toughness; (2) lowering the austenite transformation temperature, which can increase the recrystallization temperature, refine grains under high-temperature rolling, improve steel plate strength, and facilitate plate shape control; (3) during tempering, some Nb forms carbon and nitrogen compounds, ensuring steel plate strength. However, excessive Nb content can degrade the toughness of the weld and heat-affected zone and increase costs. The present invention considers that a Nb content of 0.02% to 0.05% is more suitable.

[0031] Cr: Cr is the main element for improving the weather resistance of the steel plate in the present invention. Cr element is enriched in the rust layer and can also promote the 3+ The reduction reaction forms iron-chromium-copper multi-alloy oxides, which refine the rust particles and hinder the Cl - Cr can also improve the hardenability of steel plates, refine grains, increase tensile strength, and reduce yield ratio. However, excessive Cr content can easily cause carbide precipitation, affecting the toughness of the steel. Considering the economy, weldability, and toughness, the present invention believes that it is more appropriate to control the Cr content to 0.50% to 0.80%.

[0032] Mo: Mo can improve the hardenability of steel, inhibit the segregation of impurity elements such as P and S at grain boundaries, and reduce temper brittleness. Mo also plays a unique role in stabilizing the rust layer and improving weather resistance. An appropriate amount of Mo can also reduce the yield strength ratio and improve the seismic performance of the steel plate. When Mo and Nb are added simultaneously, it can also promote the precipitation of fine Nb carbonitrides with high high-temperature stability, thereby further improving the strength of the steel plate. However, too much Mo will combine with C to reduce the plasticity and low-temperature toughness of the steel plate, and the cost is relatively high. The present invention believes that it is more appropriate to control the Mo content to 0.10% to 0.20%.

[0033] Cu: Cu improves the hardenability of steel and significantly increases the core strength of thick steel plates. It is also an important element for improving weather resistance. During the slow cooling process of thick steel plates, an appropriate amount of Cu can precipitate ε-Cu through auto-tempering, thereby improving the steel plate's strength. Excessive Cu content can cause hot cracking in the steel plate and reduce its plasticity. The present invention considers that a Cu content of 0.25% to 0.45% is more suitable.

[0034] Ni: Ni can effectively improve the low-temperature toughness of steel, inhibit chloride ion corrosion of steel, and improve the hot brittleness caused by copper in steel. Ni can also improve the isotropy of steel plates after heat treatment. However, nickel is a precious metal, and adding large amounts will significantly increase costs and affect welding performance. Therefore, an appropriate amount is added according to performance requirements. In the present invention, the Ni content is controlled at 0.40% to 0.70%.

[0035] Ti: Ti binds nitrogen, forming a precipitate primarily composed of TiN. This inhibits austenite grain growth at high temperatures and improves the toughness of the heat-affected zone (HAZ) after welding. During welding, TiN particles prevent grain growth in the heat-affected coarse-grained zone, enhancing the low-temperature toughness of the welded joint. Furthermore, due to its low solid solubility, Ti readily forms interphase precipitations during the austenite-to-ferrite transformation, enhancing strength. However, excessive Ti content can reduce the toughness of the steel. The present invention proposes that a Ti content of 0.005% to 0.020% is more suitable.

[0036] B: The B element can improve the hardenability of the steel plate. A trace amount of the B element can significantly improve the hardenability and ensure the strength of the steel plate. However, when the B element is excessive, the brittleness of the steel plate increases and the tendency of welding cracks increases. Therefore, the present invention controls the B element to 0.001% to 0.0025%.

[0037] Al: Al is a strong deoxidizing element and can also combine with nitrogen to form AlN, which can refine grains, improve low-temperature impact toughness, and lower the brittle transition temperature of steel. If AlN is formed, it also refines the structure. When the Al content exceeds 0.040%, excessive aluminum oxide inclusions will reduce the cleanliness of the steel. If the Al content is too low, deoxidation is insufficient, and easily oxidizable elements such as Ti will form oxides. The present invention believes that the Al content should be controlled between 0.010% and 0.040%.

[0038] Another aspect of the present invention provides a method for manufacturing the above-mentioned isotropic low yield ratio and high toughness bridge steel, comprising: rolling, cooling, straightening, and heat treatment. The specific steps are as follows:

[0039] (1) Rolling: The continuous casting billet is loaded into the heating furnace when the furnace temperature is 650-750℃, so that the internal and external temperatures of the billet are kept consistent in the low temperature stage, so as to prepare for the uniform structure in the high temperature stage; the temperature of the continuous casting billet heating section is 1120-1230℃, the temperature of the soaking section is 1110-1220℃, and the soaking section holding time is 3.7-5.3h, so that C and N compounds are fully dissolved, especially the solid solution of Nb and Mo elements, to avoid abnormal growth of the cast structure; at the same time, the austenite grains are fully grown to provide sufficient deformation power for the austenite deformation; in addition, the billet size should be designed to ensure that the billet width after steel transfer does not exceed the length of the rolling mill roller; the rough rolling stage adopts the longitudinal-transverse rolling process, and the rough rolling start temperature is 1000-1100℃. The cumulative reduction rate of longitudinal rolling is 20-30%, the cumulative reduction rate of transverse rolling is 20-40%, the rough rolling finish temperature is 950-1050°C, and the cumulative reduction rate in the rough rolling stage is ≥60%. The purpose of adopting longitudinal-transverse rolling is to improve the banded structure and texture orientation generated within the steel plate during the rolling process, weaken the influence of the rolled structure on the transverse and longitudinal mechanical properties, and prepare the structure for subsequent heat treatment. The high-temperature transverse rolling can improve the as-cast structure of the slab. The rolling temperature and deformation process in the rough rolling stage recrystallize the austenite grains and inhibit grain growth. The superposition effect of multiple high-reduction deformations is utilized to promote the recrystallization of austenite and achieve the goal of grain refinement. This is suitable for the production of isotropic low-yield-to-strength ratio and high-toughness bridge steel plates of the present invention.

[0040] The finishing rolling stage adopts longitudinal variable thickness rolling. The relationship between the finishing rolling parameters and the thickness of the finished steel plate is as follows:

[0041] The thickness of the thick end of the finished steel plate is ≤20mm, the thickness of the intermediate billet is 5-9t, where t is the thickness of the thick end of the finished steel plate, the starting temperature of the finishing rolling is 920-970℃, the finishing temperature of the finishing rolling is 850-890℃, and the deformation rate of the thick end of the steel plate in a single pass is not less than 15%;

[0042] 20mm<thickness of finished steel plate at thick end≤30mm, intermediate billet thickness is 3~6t, where t is thickness of finished steel plate at thick end, finishing rolling start temperature is 890~960℃, finishing rolling finish temperature is 840~880℃, and deformation rate of single pass at thick end of steel plate is not less than 13%;

[0043] 30mm<thickness of finished steel plate at thick end≤50mm, intermediate billet thickness is 2.5~4.0t, where t is the thickness of finished steel plate at thick end, finishing rolling start temperature is 880~940℃, finishing rolling finish temperature is 820~860℃, and the deformation rate of single pass at thick end of steel plate is not less than 12%;

[0044] 50mm<thickness of finished steel plate at thick end≤60mm, intermediate billet thickness is 2.0~3.5t, where t is the thickness of finished steel plate at thick end, finishing rolling start temperature is 860~900℃, finishing rolling finish temperature is 800~840℃, and the deformation rate of single pass at thick end of steel plate is not less than 10%;

[0045] The appropriate intermediate billet thickness can not only meet the requirements of austenite deformation and deformation energy accumulation in the non-recrystallized zone, but also ensure that a sufficient deformation rate is obtained in the rough rolling stage under the condition of a certain thickness of the original ingot, thereby achieving the purpose of grain refinement; the large single-pass reduction in the non-recrystallized zone further promotes the refinement of austenite, improves the fine defects inside the ingot, and enhances the isotropy and toughness of the steel plate; the higher rolling and red-hot temperatures can reduce the load of the rolling mill during the rolling of longitudinally variable thickness steel plates, ensuring accurate control of the steel plate shape;

[0046] (2) Cooling: After rolling, water cooling is used for cooling. The relationship between cooling parameters and the thickness of the finished steel plate is as follows:

[0047] The thickness of the finished steel plate at the thick end is ≤20mm, the cooling temperature is 750~780℃, and the red-hot temperature is 580~650℃;

[0048] 20mm<The thickness of the finished steel plate is ≤30mm, the cooling temperature is 740~770℃, and the red-returning temperature is 500~600℃;

[0049] 30mm<thickness of finished steel plate at the end ≤50mm, cooling temperature is 710~740℃, and returning to red temperature is 480~550℃;

[0050] 50mm<The thickness of the finished steel plate is ≤60mm, and the cooling temperature is 690~720℃;

[0051] Control the start-of-cooling temperature. In this temperature range, the steel plate will generate a large amount of ferrite structure, ensuring that the steel plate has high plasticity and toughness. Accelerated cooling can further refine the austenite grain structure and improve the strength of the steel plate. Control the red-hot temperature. In this temperature range, the steel plate can form partial bainite structure and improve the matrix strength. The appropriate red-hot temperature provides a suitable temperature for subsequent straightening, avoiding excessive straightening force during straightening, resulting in poor plate shape.

[0052] (3) Straightening: Straightening is performed using a hot straightening machine. The relationship between the straightening temperature and the thickness of the finished steel plate is as follows:

[0053] The thickness of the finished steel plate at the thick end is ≤20mm, and the straightening temperature is ≥550℃;

[0054] 20mm<The thickness of the finished steel plate at the thick end is ≤30mm, and the straightening temperature is ≥480℃;

[0055] 30mm<thickness of finished steel plate at thick end≤50mm, straightening temperature≥450℃;

[0056] 50mm<thickness of finished steel plate at thick end≤60mm, straightening temperature≥400℃;

[0057] (4) Heat treatment: The tempering temperature is 550-650℃, and the tempering holding time is 3-5min / mm. The purpose is to further improve the isotropy of the steel plate, reduce the residual stress of the steel plate, and thus improve the uniformity of the steel plate structure.

[0058] The steel plate produced by this manufacturing method features a uniform microstructure consisting of fine ferrite, pearlite, and bainite. A small amount of bainite further enhances the steel plate's tensile strength and reduces its yield ratio. The resulting steel plate exhibits high strength, excellent ductility, a low yield ratio, low-temperature toughness, good weather resistance, weldability, and isotropic properties, meeting the demands of various bridge projects while reducing the total amount of steel used in bridge construction.

[0059] In the above technical solution, further, in step (1), the method for preparing the continuous casting billet includes the following steps:

[0060] a. After pretreatment of the molten iron, it is subjected to converter smelting and off-furnace refining. In the LF refining treatment, the net argon blowing time is ≥5min, the RH vacuum degassing, and the molten steel is subjected to Ca treatment and micro-Ti treatment, with a net cycle time ≥5min. The refining and degassing treatment can effectively reduce impurity elements;

[0061] b. The target superheat of the continuous casting tundish is ≤30°C. Protect the casting process and apply soft reduction to control the continuous casting billet thickness / finished steel plate maximum thickness to ≥6.0. Controlling the casting superheat and soft reduction can effectively reduce billet quality defects; increasing the compression ratio from the continuous casting billet to the finished steel plate can effectively control the grain size.

[0062] In the above technical solution, further, in step (1), the continuous casting billet is heated at a rate of 4 to 6°C / min to avoid uneven heating inside the billet due to excessive heating of the billet.

[0063] In the above technical solution, further, in step (1), the relationship between the rolling speed in the finishing rolling stage and the thickness of the finished steel plate at the thick end is as follows:

[0064] The thickness of the finished steel plate at the thick end is ≤20mm, and the rolling speed is 1.3~2.7m / s;

[0065] 20mm<thickness of finished steel plate at the thick end≤30mm, rolling speed 1.2~2.6m / s;

[0066] 30mm<thickness of finished steel plate at the thick end≤50mm, rolling speed 1.1~2.4m / s;

[0067] 50mm<thickness of finished steel plate at the thick end≤60mm, rolling speed 0.9~1.8m / s;

[0068] In the above technical solution, further, in step (2), the relationship between the cooling rate and the thickness of the finished steel plate at the thick end is as follows:

[0069] The thickness of the finished steel plate at the thick end is ≤20mm, and the cooling rate is 3~10℃ / s;

[0070] 20mm<thickness of finished steel plate at the thick end≤30mm, cooling rate is 6~14℃ / s;

[0071] 30mm<thickness of finished steel plate at the thick end≤50mm, cooling rate is 10~18℃ / s;

[0072] 50mm<thickness of finished steel plate at thick end≤60mm, cooling rate is 12~20℃ / s.

[0073] In the above technical solution, further, in step (3), the straightening speed of the parallel section is 0.2-0.4 m / s, and the straightening speed of the variable thickness section is 0.1-0.20 m / s; according to the thickness specification of the steel plate, when the straightening enters the variable thickness section, the straightening roller gap is uniformly increased / decreased, and the upper straightening roller is linked to rise / fall, wherein the rising / falling roller speed calculation formula is:

[0074] Ascending / descending roller speed = variable thickness × straightening speed / horizontal length of variable thickness section

[0075] The variable thickness of the steel plate is ≤50mm to ensure the temperature uniformity of the entire steel plate and a good plate shape; wherein, the variable thickness of the steel plate = the thickness of the thick end of the steel plate - the thickness of the thin end of the steel plate.

[0076] FIG1 shows a schematic diagram of three types of LP steel plates. As shown in the figure, the thick end, thin end, parallel section, and thickened section of the steel plate in the present invention have the following meanings:

[0077] In 01 steel plate, h1 is the thin end, h2 is the thick end, and L1 is the thickened section;

[0078] In 02 steel plate, h'1 is the thin end, h'2 is the thick end, L'1 is the thickened section, and L'2 is the parallel section;

[0079] In 03 steel plate, h”1 is the thin end, h”2 is the thick end, L”1 is the parallel section, L”2 is the thickened section, and L”3 is the parallel section.

[0080] The beneficial effects of the present invention are:

[0081] (1) The composition of the present invention improves the toughness of the material by designing low C and low Mn, and utilizes Nb and Ti elements to inhibit the growth of austenite grains and promote nucleation during the austenite transformation to refine the grains, increase the recrystallization temperature, and ensure the uniformity of the steel plate's structure at high temperatures. The low-cost Cr element is added to improve the hardenability of the steel plate, thereby further improving the strength of the steel plate.

[0082] (2) The present invention adds appropriate amounts of weather-resistant elements such as Ni, Cu, and Mo, and the atmospheric corrosion resistance index I is greater than or equal to 6.3. This greatly improves the weather resistance of the steel plate while improving the hardenability of the steel plate, reduces the painting of bridge projects, and even eliminates the need for painting, thus saving resources and being environmentally friendly.

[0083] (3) The steel plate of the present invention has a CEV of 0.36 to 0.52 and a Pcm of 0.13 to 0.20, and has excellent welding performance, which can improve component processing efficiency.

[0084] (4) The present invention, combined with a corresponding unique production process, solves the comprehensive problems of poor shape control stability and poor weather resistance of high-strength bridge steel plates; the use of TMCP+tempering rolling process can further improve production efficiency, and can produce LP steel plates of various shapes, reduce the overall structural weight of bridge projects, and improve the construction efficiency and overall safety of bridge structure projects.

[0085] (5) The present invention improves the banded structure and texture orientation generated inside the steel plate during the rolling process through a longitudinal-transverse-longitudinal alternating rolling process, and further eliminates the influence of the banded austenite grains on the transverse and longitudinal impact toughness of the steel plate through subsequent tempering treatment.

[0086] (6) The maximum thickness of the thick end of the steel plate produced by the present invention is 60 mm, and the maximum variable thickness is 50 mm. A variety of variable thickness specifications and sizes can be produced to meet the needs of various shapes of longitudinal variable thickness bridge steel.

[0087] (7) The yield strength of the steel plate is ≥500MPa, the tensile strength is ≥630MPa, the elongation after fracture is ≥21%, the yield strength ratio is ≤0.83, the impact energy at -40℃ is ≥200J, and the performance of the same plate is uniform: the strength difference between the thin and thick ends of the same plate is ≤25MPa, the elongation difference after fracture is ≤3%, the yield strength ratio difference is ≤0.02, the impact energy difference is ≤30J, the strength and impact energy difference in the transverse and longitudinal directions at the same position is ≤5%, and the steel plate structure is fine ferrite + pearlite + bainite. BRIEF DESCRIPTION OF THE DRAWINGS

[0088] Figure 1 is a schematic diagram of the types of LP steel plates;

[0089] FIG2 is the metallographic structure of Example 5 of the present invention. DETAILED DESCRIPTION

[0090] To make the objectives, technical solutions, and advantages of the embodiments of the present invention more clear, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts shall fall within the scope of protection of the present invention.

[0091] Examples 1-10

[0092] The chemical compositions of the steels of Examples 1-10 of the present invention are shown in Table 1;

[0093] Table 1 Chemical composition of steels of Examples 1-10 (wt%)

[0094] CEV(%)=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15

[0095] Pcm(%)=C+Si / 30+Mn / 20+Cu / 20+Ni / 60+Cr / 20+Mo / 15+V / 10+5B

[0096] Atmospheric corrosion resistance index I = 26.01 (% Cu) + 3.88 (% Ni) + 1.20 (% Cr) + 1.49 (% Si) + 17.28 (% P) - 7.29 (% Cu) (% Ni) - 9.10 (% Ni) (% P) - 33.39 (% Cu) 2

[0097] The CEV, Pcm, and I values ​​of the steels of Examples 1-10 of the present invention are shown in Table 2.

[0098] Table 2 CEV, Pcm, I values ​​of steels in Examples 1-10

[0099] The manufacturing method of the above-mentioned isotropic low-yield-to-strength ratio high-toughness bridge steel includes: smelting, continuous casting, rolling, cooling, straightening, and heat treatment. The specific steps are as follows:

[0100] (1) Smelting and continuous casting: After pretreatment of molten iron, converter smelting and off-furnace refining are carried out. In the LF refining treatment, the net argon blowing time is ≥5 min, and the RH vacuum degassing is carried out. The molten steel is treated with Ca and micro-Ti, and the net cycle time is ≥5 min. Refining and degassing can effectively reduce impurity elements.

[0101] (2) Continuous casting and continuous casting billet heating: The target superheat of the continuous casting tundish is ≤30℃, and the casting is protected throughout the process. Soft pressure is applied to control the thickness of the continuous casting billet / the maximum thickness of the finished steel plate is ≥6.0; the control of the casting superheat and soft pressure can effectively reduce the quality defects of the casting billet; increasing the compression ratio from the continuous casting billet to the finished steel plate can effectively control the grain size; the continuous casting billet is loaded into the heating furnace when the furnace temperature is 650-750℃, in order to keep the internal and external temperatures of the billet consistent in the low temperature stage, so as to prepare for the uniform structure in the high temperature stage; the subsequent heating rate is 4 The temperature of the continuous casting billet should be kept at 1120-1230℃, the soaking zone at 1110-1220℃, and the soaking zone at 3.7-5.3h. This allows the carbon and nitrogen compounds to be fully dissolved, especially the solid solution of Nb and Mo elements, to avoid abnormal growth of the as-cast structure. At the same time, it ensures that the austenite grains grow fully, providing sufficient deformation power for austenite deformation. In addition, the billet size should be designed to ensure that the width of the billet after steel transfer does not exceed the length of the rolling mill roll.

[0102] Table 3 Continuous casting and continuous casting slab heating process parameters of Examples 1-10 steel

[0103] (3) Rolling: The longitudinal-transverse rolling process is adopted in the rough rolling stage, the rough rolling start temperature is 1000-1100℃, the longitudinal rolling cumulative reduction rate is 20-30%, the transverse rolling cumulative reduction rate is 20-40%, the rough rolling final rolling temperature is 950-1050℃, and the rough rolling stage cumulative reduction rate is ≥60%; the purpose of adopting the longitudinal-transverse rolling process is to improve the banded structure and texture orientation generated inside the steel plate during the rolling process, weaken the influence of the rolling structure on the transverse and longitudinal mechanical properties, and prepare the structure for subsequent heat treatment; high-temperature transverse rolling can improve the as-cast structure of the slab, the rolling temperature and deformation process in the rough rolling stage recrystallize the austenite grains and inhibit grain growth, and utilize the superposition effect of multiple high-reduction deformation to promote the recrystallization of austenite and achieve the goal of grain refinement, which is suitable for the production of the isotropic low-yield-to-strength high-toughness bridge steel plate of the present invention;

[0104] Table 4 Rough rolling process parameters of steels of Examples 1-10

[0105] The finishing rolling stage adopts longitudinal variable thickness rolling. The relationship between the finishing rolling parameters and the thickness of the finished steel plate is as follows:

[0106] The thickness of the thick end of the finished steel plate is ≤20mm, the thickness of the intermediate billet is 5-9t, where t is the thickness of the thick end of the finished steel plate. The starting temperature of the finishing rolling is 920-970℃, the finishing temperature of the finishing rolling is 850-890℃, the deformation rate of the thick end of the steel plate in a single pass is not less than 15%, and the rolling speed is 1.3-2.7m / s;

[0107] 20mm<thickness of finished steel plate at thick end≤30mm, intermediate billet thickness is 3~6t, where t is thickness of finished steel plate at thick end, finishing rolling start temperature is 890~960℃, finishing rolling finish temperature is 840~880℃, deformation rate of single pass at thick end of steel plate is not less than 13%, rolling speed is 1.2~2.6m / s;

[0108] 30mm<thickness of finished steel plate at thick end≤50mm, intermediate billet thickness is 2.5~4.0t, where t is the thickness of finished steel plate at thick end, finishing rolling start temperature is 880~940℃, finishing rolling finish temperature is 820~860℃, deformation rate of single pass at thick end of steel plate is not less than 12%, rolling speed is 1.1~2.4m / s;

[0109] 50mm<thickness of finished steel plate at thick end≤60mm, intermediate billet thickness is 2.0~3.5t, where t is the thickness of finished steel plate at thick end, finishing rolling start temperature is 860~900℃, finishing rolling finish temperature is 800~840℃, deformation rate of single pass at thick end of steel plate is not less than 10%, rolling speed is 0.9~1.8m / s;

[0110] The appropriate intermediate billet thickness can not only meet the requirements of austenite deformation and deformation energy accumulation in the non-recrystallized zone, but also ensure that a sufficient deformation rate is obtained in the rough rolling stage under the condition of a certain thickness of the original ingot, thereby achieving the purpose of grain refinement; the large single-pass reduction in the non-recrystallized zone further promotes the refinement of austenite, improves the fine defects inside the ingot, and enhances the isotropy and toughness of the steel plate; the higher rolling and red-hot temperatures can reduce the load of the rolling mill during the rolling of longitudinally variable thickness steel plates, ensuring accurate control of the steel plate shape;

[0111] Table 5 Finishing rolling process parameters of steels in Examples 1-10

[0112] (4) Cooling: After rolling, water cooling is used for cooling. The relationship between cooling parameters and the thickness of the finished steel plate is as follows:

[0113] The thickness of the finished steel plate at the thick end is ≤20mm, the cooling temperature is 750-780℃, the red-hot temperature is 580-650℃, and the cooling rate is 3-10℃ / s;

[0114] 20mm<thickness of finished steel plate end≤30mm, cooling temperature is 740~770℃, red-return temperature is 500~600℃, cooling rate is 6~14℃ / s;

[0115] 30mm<thickness of finished steel plate at the thick end≤50mm, cooling temperature is 710~740℃, red-return temperature is 480~550℃, cooling rate is 10~18℃ / s;

[0116] 50mm<thickness of finished steel plate at the thick end≤60mm, cooling temperature is 690~720℃, cooling rate is 12~20℃ / s;

[0117] Control the start-of-cooling temperature. In this temperature range, the steel plate will generate a large amount of ferrite structure, ensuring that the steel plate has high plasticity and toughness. Accelerated cooling can further refine the austenite grain structure and improve the strength of the steel plate. Control the red-hot temperature. In this temperature range, the steel plate can form partial bainite structure and improve the matrix strength. The appropriate red-hot temperature provides a suitable temperature for subsequent straightening, avoiding excessive straightening force during straightening, resulting in poor plate shape.

[0118] Table 6 Cooling process parameters of steels in Examples 1-10

[0119] (5) Straightening: Straightening is performed using a hot straightening machine. The relationship between the straightening temperature and the thickness of the finished steel plate is as follows:

[0120] The thickness of the finished steel plate at the thick end is ≤20mm, and the straightening temperature is ≥550℃;

[0121] 20mm<The thickness of the finished steel plate at the thick end is ≤30mm, and the straightening temperature is ≥480℃;

[0122] 30mm<thickness of finished steel plate at thick end≤50mm, straightening temperature≥450℃;

[0123] 50mm<thickness of finished steel plate at thick end≤60mm, straightening temperature≥400℃;

[0124] The straightening speed in the parallel section is 0.2-0.4 m / s, and the straightening speed in the variable thickness section is 0.1-0.20 m / s. According to the thickness specifications of the steel plate, the straightening roller gap is uniformly increased / decreased when the straightening enters the variable thickness section, and the upper straightening roller rises / falls in conjunction. The calculation formula for the rising / falling roller speed is: rising / falling roller speed = variable thickness × straightening speed / horizontal length of the variable thickness section

[0125] The variable thickness of the steel plate is ≤50mm to ensure the temperature uniformity and good plate shape of the entire steel plate; the variable thickness of the steel plate = the thickness of the thick end of the steel plate - the thickness of the thin end;

[0126] Table 7 Straightening process parameters of steels of Examples 1-10

[0127] (6) Heat treatment: The tempering temperature is 550-650℃, and the tempering holding time is 3-5min / mm. The purpose is to further improve the isotropy of the steel plate, reduce the residual stress of the steel plate, and thus improve the uniformity of the steel plate structure.

[0128] Table 8 Heat treatment process parameters of steels in Examples 1-10

[0129] The mechanical properties of the thick end of the steel of Examples 1-10 of the present invention are shown in Table 9, and the mechanical properties of the thin end are shown in Table 10.

[0130] Table 9 Mechanical properties of thick end of steel of Examples 1-10

[0131] Table 10 Mechanical properties of thin end of steel of Examples 1-10

[0132] The final microstructure of the steel of Examples 1-10 of the present invention is composed of ferrite, pearlite, and bainite, and the proportions are shown in Table 11.

[0133] Table 11 Microstructure ratio of steels in Examples 1-10

[0134] The above embodiments are merely preferred embodiments of the present invention and are not intended to limit the scope of implementation. The scope of protection of the present invention shall be determined by the scope defined in the claims. Other variations or modifications may be made based on the above description. Obvious variations or modifications derived therefrom remain within the scope of protection of the present invention.

Claims

1. An isotropic bridge steel with low yield strength ratio and high toughness, It is characterized in that Its chemical composition weight percentage is: C: 0.02% ~ 0.05%, Si: 0.25% ~ 0.45%, Mn: 1.00% ~ 1.40%, P ≤ 0.010%, S ≤ 0.003%, Nb: 0.02% ~ 0.05%, Ni: 0.40% ~ 0.70%, Cu: 0.25% ~ 0.45%, Mo: 0.10% ~ 0.20%, Cr: 0.50% ~ 0.80%, Ti: 0.005% ~ 0.020%, B: 0.0010% ~ 0.0025%, Al: 0.01% ~ 0.04%, the balance is iron and unavoidable impurities; The steel has a CEV of 0.36% to 0.52%, a Pcm of 0.13% to 0.20%, and an atmospheric corrosion resistance index I of ≥6.

30.

2. The isotropic low yield strength ratio high toughness bridge steel according to claim 1, It is characterized in that The final microstructure of the steel plate is composed of ferrite, pearlite and bainite; wherein, by volume percentage, ferrite is 11-28%, pearlite is 3-7%, and bainite is 69-82%.

3. The isotropic low yield strength ratio high toughness bridge steel according to claim 1, It is characterized in that The yield strength of the steel plate is ≥500MPa, the tensile strength is ≥630MPa, the elongation after fracture is ≥21%, the yield strength ratio is ≤0.83, and the impact energy at -40℃ is ≥200J; the yield strength difference between the thin and thick ends of the same plate is ≤25MPa, the tensile strength difference is ≤25MPa, the elongation difference after fracture is ≤3%, the yield strength ratio difference is ≤0.02, and the impact energy difference at -40℃ is ≤30J; the tensile strength ratio between the transverse and longitudinal directions at the same position is ≤5%, and the impact energy ratio is ≤5%.

4. A method for manufacturing the isotropic low yield ratio and high toughness bridge steel according to any one of claims 1 to 3, It is characterized in that include: Rolling, cooling, straightening, heat treatment, the specific steps are as follows: (1) Rolling: The continuous casting billet is loaded into the heating furnace when the furnace temperature is 650-750°C. The temperature of the continuous casting billet heating section is 1120-1230°C, the temperature of the soaking section is 1110-1220°C, the soaking section holding time is 3.7-5.3h, the longitudinal-transverse rolling process is adopted in the rough rolling stage, the rough rolling start temperature is 1000-1100°C, the longitudinal rolling cumulative reduction rate is 20%-30%, the transverse rolling cumulative reduction rate is 20%-40%, the rough rolling final rolling temperature is 950-1050°C, and the cumulative reduction rate in the rough rolling stage is ≥60%; The finishing rolling stage adopts longitudinal variable thickness rolling. The relationship between the finishing rolling parameters and the thickness of the finished steel plate at the thick end is as follows: The thickness of the thick end of the finished steel plate is ≤20mm, the thickness of the intermediate billet is 5-9t, where t is the thickness of the thick end of the finished steel plate, the start rolling temperature of the finishing rolling is 920-970℃, the final rolling temperature of the finishing rolling is 850-890℃, and the deformation rate of the thick end of the steel plate in a single pass is not less than 15%; 20mm<thickness of finished steel plate at thick end≤30mm, intermediate billet thickness is 3~6t, where t is the thickness of finished steel plate at thick end, finishing rolling start temperature is 890~960℃, finishing rolling final rolling temperature is 840~880℃, and the deformation rate of single pass at thick end of steel plate is not less than 13%; 30mm<thickness of finished steel plate at thick end≤50mm, intermediate billet thickness is 2.5~4.0t, where t is the thickness of finished steel plate at thick end, finishing rolling start temperature is 880~940℃, finishing rolling final rolling temperature is 820~860℃, single pass of thick end of steel plate The deformation rate is not less than 12%; 50mm<thickness of finished steel plate at thick end≤60mm, intermediate billet thickness is 2.0~3.5t, where t is the thickness of finished steel plate at thick end, finishing rolling start temperature is 860~900℃, finishing rolling final rolling temperature is 800~840℃, and the deformation rate of single pass at thick end of steel plate is not less than 10%; (2) Cooling: After rolling, water cooling is used for cooling. The relationship between cooling parameters and the thickness of the finished steel plate is as follows: The thickness of the finished steel plate at the thick end is ≤20mm, the cooling temperature is 750~780℃, and the red-returning temperature is 580~650℃; 20mm<The thickness of the finished steel plate is ≤30mm, the cooling temperature is 740~770℃, and the red-returning temperature is 500~600℃; 30mm<The thickness of the finished steel plate is ≤50mm, the cooling temperature is 710~740℃, and the red-returning temperature is 480~550℃; 50mm<The thickness of the finished steel plate is ≤60mm, the cooling temperature is 690~720℃, and the red-returning temperature is 450~500℃; (3) Straightening: Straightening is performed by a hot straightening machine. The relationship between the straightening temperature and the thickness of the finished steel plate at the thick end is as follows: The thickness of the finished steel plate at the thick end is ≤20mm, and the straightening temperature is ≥550℃; 20mm<The thickness of the finished steel plate at the thick end is ≤30mm, and the straightening temperature is ≥480℃; 30mm<thickness of finished steel plate at thick end≤50mm, straightening temperature≥450℃; 50mm<The thickness of the finished steel plate at the thick end is ≤60mm, and the straightening temperature is ≥400℃; (4) Heat treatment: The tempering temperature is 550-650°C, and the tempering holding time is 3-5 min / mm.

5. The manufacturing method according to claim 4, It is characterized in that In step (1), the method for preparing the continuous casting billet comprises the following steps: a. Smelting: After the molten iron is pretreated, it is subjected to converter smelting and refining outside the furnace. In the LF refining treatment, the net argon blowing time is ≥5min, and the RH vacuum degassing, the net cycle time is ≥5min; b. Continuous casting: The target superheat of the continuous casting tundish is ≤30℃, the pouring is protected throughout the whole process, and light pressure is applied to control the thickness of the continuous casting billet / the maximum thickness of the finished steel plate is ≥6.

0.

6. The manufacturing method according to claim 4, It is characterized in that In step (1), the continuous casting billet is heated at a rate of 4 to 6°C / min.

7. The manufacturing method according to claim 4, It is characterized in that In step (1), the relationship between the rolling speed in the finishing rolling stage and the thickness of the finished steel plate at the thick end is as follows: The thickness of the finished steel plate at the thick end is ≤20mm, and the rolling speed is 1.3~2.7m / s; 20mm<The thickness of the finished steel plate is ≤30mm, and the rolling speed is 1.2~2.6m / s; 30mm<The thickness of the finished steel plate is ≤50mm, and the rolling speed is 1.1~2.4m / s; 50mm<The thickness of the finished steel plate at the thick end is ≤60mm, and the rolling speed is 0.9~1.8m / s; 8. The manufacturing method according to claim 4, It is characterized in that In step (2), the relationship between the cooling rate and the thickness of the finished steel plate at the thick end is as follows: The thickness of the finished steel plate at the thick end is ≤20mm, and the cooling rate is 3~10℃ / s; 20mm<The thickness of the finished steel plate is ≤30mm, and the cooling rate is 6~14℃ / s; 30mm<The thickness of the finished steel plate is ≤50mm, and the cooling rate is 10~18℃ / s; 50mm<The thickness of the finished steel plate at the thick end is ≤60mm, and the cooling rate is 12~20℃ / s.

9. The manufacturing method according to claim 4, It is characterized in that In step (3), the straightening speed of the parallel section is 0.2-0.4 m / s, and the straightening speed of the variable thickness section is 0.1-0.20 m / s; The variable thickness of the steel plate is ≤50mm, wherein the variable thickness of the steel plate = the thickness of the thick end of the steel plate - the thickness of the thin end of the steel plate.

Citation Information

Patent Citations

  • Thick high-strength steel plate and process for producing the same

    CN101622370A

  • Weather resistant steel plate and manufacturing method thereof

    CN102168229A

  • High-performance bridge weathering steel containing Mo and preparation method thereof

    CN102534417A

  • 420 MPa-level LP steel plate and production method thereof

    CN108396241A

  • Longitudinal special-shaped fracture surface steel plate and production method thereof

    CN108397682A