Composite current collector and manufacturing method therefor and application thereof
By using composite current collectors in sodium ion batteries, combining conductive bottom layer and conductive water-resistant layer, the problem of poor water resistance performance of the negative electrode current collector of sodium ion batteries is solved, high water resistance and conductivity are achieved, extending battery life and reducing costs .
Patent Information
- Application Number
- PCT/CN2023/102097
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2023-06-25
- Publication Date
- 2024-12-05
AI Technical Summary
The water resistance of the negative current collector of existing sodium ion batteries is poor, which affects the peeling performance of the electrode material and the current collector, resulting in poor electrode effect.
The composite liquid collector includes a conductive bottom layer and a conductive water-resistant layer. The conductive bottom layer contains conductive agent A and a conductive agent B. The conductive water-resistant layer contains conductive agent A, conductive agent B, crosslinking agent and binder. The coating is reduced by laminated structure. Inside tiny channels improve water resistance while maintaining conductivity and bonding properties.
High water resistance, conductivity and safety are achieved, the contact resistance between the electrode material and the current collector is reduced, the battery life is extended, and the production cost is reduced.
Smart Images

Figure PCTCN2023102097-FTAPPB-I100001
Abstract
Description
A composite current collector and its preparation method and application
[0001] This application claims priority to the Chinese patent application number 202310637831.9 filed with the China Patent Office on May 31, 2023. The entire contents of the above application are incorporated by reference into this application. Technical Field
[0002] The present application belongs to the field of sodium ion battery technology, for example, a composite current collector and its preparation method and application. Background Art
[0003] Sodium-ion batteries have gradually begun to be used in consumer electronics, electric vehicles and other fields, and the market has also put forward higher requirements on the energy density, cycle life, and safety of use of sodium-ion batteries.
[0004] The current collector conductive primer technology can effectively reduce the contact resistance between the electrode material and the current collector, increase the adhesion between the electrode material and the current collector, reduce the internal resistance of the battery, and extend the battery life.
[0005] In related technologies, aluminum foil is commonly used as the current collector material for the positive and negative electrodes of sodium-ion batteries. For the positive electrode, the nano-conductive-coated aluminum current collector has the same requirements during preparation as lithium-ion batteries, requiring good resistance to NMP and electrolyte. However, for the negative electrode, the use of positive nano-conductive-coated aluminum current collectors can lead to decreased adhesion and coating shedding. The main reason is that the negative electrode material is also mostly water-based, while the nano-conductive-coated aluminum current collectors usually use water-based binders. During the curing process, the coating forms many penetrating and non-penetrating microchannels due to the volatilization of water, resulting in poor water resistance, which affects the peeling performance between the negative electrode material and the current collector, thereby affecting the overall performance of the electrode.
[0006] CN114243027A discloses a sodium ion battery negative electrode current collector, a preparation method thereof, and a sodium ion battery, wherein the sodium ion battery negative electrode current collector comprises aluminum foil, the surface of which is provided with a nanosheet array.
[0007] CN217387216U discloses a negative electrode current collector, a negative electrode sheet and a battery, wherein the negative electrode current collector comprises: an aluminum conductive layer; a conductive functional layer, wherein the conductive functional layer covers the surface of the aluminum conductive layer and separates the aluminum conductive layer and the electrolyte, and the conductive functional layer is used to prevent ions in the electrolyte from contacting the aluminum conductive layer.
[0008] The current collector described in the above solution has the problem of poor water resistance, which affects the peeling performance between the electrode material and the current collector, thereby affecting the overall effect of the electrode.
[0009] Summary of the Invention
[0010] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0011] The purpose of this application is to provide a composite current collector and its preparation method and application. The composite current collector described in this application has not only high water resistance, but also high conductivity and safety, low production cost and simple method. It improves the water resistance of the current collector without affecting the overall conductivity of the current collector and the bonding performance of the electrode material.
[0012] To achieve this goal, this application adopts the following technical solutions:
[0013] In the first aspect, an embodiment of the present application provides a composite current collector, which includes a substrate and a conductive bottom layer and a conductive water-resistant layer stacked in sequence on at least one side surface of the substrate, the conductive bottom layer contains a conductive agent A, a conductive agent B and a binder, and the conductive water-resistant layer contains a conductive agent A, a conductive agent B, a cross-linking agent and a binder.
[0014] The composite current collector described in the embodiment of the present application includes a conductive bottom layer and a conductive water-resistant layer. The conductive water-resistant layer is located on the surface of the conductive bottom layer, reducing the number of tiny penetrating channels inside the coating and reducing the ability of water to penetrate the coating film, thereby improving the water resistance of the conductive coating without affecting the overall conductivity of the current collector and its adhesion performance with the electrode material.
[0015] In one embodiment, the substrate comprises a current collector.
[0016] In one embodiment, the conductive agent A is a flake-shaped conductive agent.
[0017] In one embodiment, the conductive agent A includes conductive graphite and / or graphene.
[0018] In one embodiment, the particle size of the conductive agent A is 1-3 μm, for example, 1 μm, 1.5 μm, 2 μm, 2.5 μm or 3 μm.
[0019] In one embodiment, the conductive agent B includes conductive carbon black and / or carbon nanotubes.
[0020] In one embodiment, the particle size of the conductive agent B is 200-600 nm, for example, 200 nm, 300 nm, 400 nm, 500 nm, or 600 nm.
[0021] In the embodiment of the present application, different conductive agents A and conductive agents B are added to the conductive base layer and the conductive water-resistant layer, respectively. The conductive agent A has a layered structure, has good conductivity and has a certain shielding effect; the conductive agent B has better ionic and electronic conductivity and a larger specific surface area, which is conducive to the adsorption of electrolytes and improves the ionic conductivity and rate performance.
[0022] In one embodiment, the crosslinking agent includes any one of isocyanate, aziridine-type curing crosslinking agent, or epoxy-type curing crosslinking agent, or a combination of at least two thereof.
[0023] In one embodiment, the adhesive comprises a modified polyacrylic acid adhesive and / or a polyacrylic acid adhesive.
[0024] In the conductive water-resistant layer of the composite current collector described in the embodiment of the present application, the binder and the cross-linking agent are mixed and heated to cross-link, thereby effectively improving the water resistance.
[0025] In one embodiment, in the conductive base layer, the mass ratio of the conductive agent B to the conductive agent A is (10-20):1, for example: 10:1, 12:1, 15:1, 18:1 or 20:1.
[0026] The content of the conductive agent B in the conductive bottom layer described in the embodiment of the present application is higher than that of the conductive agent A. The conductive agent B is conductive carbon black and / or carbon nanotubes, which has excellent conductive properties and can take into account the conductive properties of the nano-coating current collector.
[0027] In one embodiment, in the conductive base layer, the mass ratio of the conductive agent B to the binder is (1-2):1, for example: 1:1, 1.2:1, 1.5:1, 1.8:1 or 2:1.
[0028] In one embodiment, in the conductive water-resistant layer, the mass ratio of the conductive agent A to the conductive agent B is (10-20):1, for example: 10:1, 12:1, 15:1, 18:1 or 20:1.
[0029] In the conductive water-resistant layer described in the embodiment of the present application, the content of conductive agent B is lower than that of conductive agent A. Conductive agent A is a flaky conductive agent with large particle size and has excellent shielding effect. The addition of a cross-linking agent can further enhance the water resistance of the coating.
[0030] In the composite current collector described in the examples of this application, the conductive bottom layer comprises a high proportion of nano-conductive particles (conductive agent B), resulting in better mixing and conductivity. The conductive water-resistant layer comprises a high proportion of flaky micron-sized particles (conductive agent A), effectively reducing the specific surface area of the outer layer and the formation of penetrating and non-penetrating microchannels.
[0031] In one embodiment, in the conductive water-resistant layer, the mass ratio of the conductive agent A to the binder is (1-2):1, for example: 1:1, 1.2:1, 1.5:1, 1.8:1 or 2:1.
[0032] In one embodiment, in the conductive water-resistant layer, the mass ratio of the binder to the cross-linking agent is (80-200):1, for example: 80:1, 100:1, 120:1, 150:1 or 200:1.
[0033] In one embodiment, the thickness of the conductive bottom layer is 0.2-0.4 μm, for example, 0.2 μm, 0.25 μm, 0.3 μm or 0.4 μm.
[0034] In one embodiment, the thickness of the conductive water-resistant layer is 0.3-0.8 μm, for example, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm or 0.8 μm.
[0035] In one embodiment, the total thickness of the conductive base layer and the conductive water-resistant layer is 0.5-1.2 μm, for example, 0.5 μm, 0.6 μm, 0.8 μm, 1 μm or 1.2 μm.
[0036] In a second aspect, an embodiment of the present application provides a method for preparing the composite current collector as described in the first aspect, the preparation method comprising the following steps:
[0037] (1) mixing and dispersing the conductive agent A, the conductive agent B and the binder to obtain a bottom conductive paste, and mixing and dispersing the conductive agent A, the conductive agent B, the crosslinking agent and the binder to obtain a water-resistant conductive paste;
[0038] (2) coating the bottom conductive paste on the surface of the substrate to obtain a conductive bottom layer, coating the water-resistant conductive paste on the surface of the conductive bottom layer to form a conductive water-resistant layer, and obtaining the composite current collector.
[0039] In a third aspect, an embodiment of the present application provides a pole piece, which comprises the composite current collector as described in the first aspect.
[0040] In a fourth aspect, an embodiment of the present application provides a sodium ion battery, wherein the sodium ion battery comprises the electrode as described in the third aspect.
[0041] Compared with the related art, this application has the following beneficial effects:
[0042] (1) The composite current collector described in the present application has high water resistance, high conductivity and safety, low production cost and simple method, and improves the water resistance of the current collector without affecting the overall conductivity of the current collector and the bonding performance with the electrode material.
[0043] (2) The water drop angle of the composite current collector described in the present application can reach more than 30°, the water content can reach less than 200 ppm, it shows high water resistance, and the electrode resistance can reach less than 2.53 mΩ. DETAILED DESCRIPTION
[0044] The technical solution of the present application is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present application and should not be regarded as specific limitations of the present application.
[0045] Example 1
[0046] This embodiment provides a composite current collector, and the preparation method of the composite current collector is as follows:
[0047] (1) 10 kg of conductive carbon black with a particle size of 200 nm as conductive agent B, 1 kg of conductive graphite with a particle size of 2 μm as conductive agent A, and 40 kg of modified polyacrylic acid binder (content 25 wt%) were mixed and dispersed to obtain a bottom conductive paste, and 1 kg of conductive carbon black with a particle size of 200 nm as conductive agent B, 10 kg of conductive graphite with a particle size of 2 μm as conductive agent A, 40 kg of modified polyacrylic acid binder (content 25 wt%), and 0.08 kg of isocyanate were mixed and dispersed to obtain a water-resistant conductive paste;
[0048] (2) The bottom conductive paste is coated on the surface of an aluminum current collector with a thickness of 12 μm to obtain a conductive bottom layer, and the water-resistant conductive paste is coated on the surface of the conductive bottom layer to obtain the composite current collector, wherein the thickness of the conductive water-resistant layer is 0.5 μm, the thickness of the conductive bottom layer is 0.2 μm, and the total thickness of the conductive bottom layer and the conductive water-resistant layer is 0.7 μm.
[0049] Example 2
[0050] This embodiment provides a composite current collector, and the preparation method of the composite current collector is as follows:
[0051] (1) 15 kg of carbon nanotubes with a particle size of 200 nm as conductive agent B, 1 kg of graphene with a particle size of 2.2 μm as conductive agent A, and 40 kg of modified polyacrylic acid binder (content 25 wt%) were mixed and dispersed to obtain a bottom conductive paste, and 1 kg of carbon nanotubes with a particle size of 200 nm as conductive agent B, 14 kg of graphene with a particle size of 2.2 μm as conductive agent A, 40 kg of modified polyacrylic acid binder (content 25 wt%), and 0.1 kg of isocyanate were mixed and dispersed to obtain a water-resistant conductive paste;
[0052] (2) The bottom conductive paste is coated on the surface of an aluminum current collector with a thickness of 12 μm to obtain a conductive bottom layer, and the water-resistant conductive paste is coated on the surface of the conductive bottom layer to obtain the composite current collector, wherein the thickness of the conductive water-resistant layer is 0.5 μm, the thickness of the conductive bottom layer is 0.2 μm, and the total thickness of the conductive bottom layer and the conductive water-resistant layer is 0.7 μm.
[0053] Example 3
[0054] The only difference between this embodiment and embodiment 1 is that the mass ratio of the conductive agent A to the conductive agent B in the conductive base layer is 10:1, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0055] Example 4
[0056] The only difference between this embodiment and embodiment 1 is that in the conductive water-resistant layer, the mass ratio of the conductive agent B to the conductive agent A is 10:1, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0057] Example 5
[0058] The only difference between this embodiment and embodiment 1 is that the thickness of the conductive water-resistant layer is 0.2 μm, and other conditions and parameters are exactly the same as those in embodiment 1.
[0059] Example 6
[0060] The only difference between this embodiment and embodiment 1 is that the thickness of the conductive water-resistant layer is 1 μm, and other conditions and parameters are exactly the same as those in embodiment 1.
[0061] Example 7
[0062] The only difference between this embodiment and embodiment 1 is that the thickness of the conductive bottom layer is 0.1 μm, and other conditions and parameters are exactly the same as those in embodiment 1.
[0063] Example 8
[0064] The only difference between this embodiment and embodiment 1 is that the thickness of the conductive bottom layer is 0.5 μm, and other conditions and parameters are exactly the same as those in embodiment 1.
[0065] Comparative Example 1
[0066] The only difference between this comparative example and Example 1 is that no conductive water-resistant layer is provided, and other conditions and parameters are exactly the same as those in Example 1.
[0067] Comparative Example 2
[0068] The only difference between this comparative example and Example 1 is that the conductive water-resistant layer is provided in the lower layer, and the other conditions and parameters are exactly the same as those in Example 1.
[0069] Comparative Example 3
[0070] The only difference between this comparative example and Example 1 is that no cross-linking agent is added to the conductive water-resistant layer, and other conditions and parameters are exactly the same as those in Example 1.
[0071] Performance testing:
[0072] Water drop angle test: The contact angles measured are the contact angles 10 seconds after the liquid (water) is dropped. Ten points are measured for each sample, and the average value is taken.
[0073] Water content test: Under a relative humidity of 20%, install the bottle liner in the bottle cap in advance, heat the solid sample at 220°C, use a gas flow rate of 50 ml / min, extract for 180 seconds, and use a relative drift value of 20 μg / min.
[0074] Electrode resistance test: The solid sample is balanced under 40% humidity for 72 hours, and the penetration resistance is tested using an electrode resistance meter with a pressure of 0.3t and a pressure holding time of 5s.
[0075] The test results are shown in Table 1:
[0076] Table 1
[0077] As can be seen from Table 1, from Examples 1-2, the water drop angle of the composite current collector described in the present application can reach more than 30°, the water content can reach less than 200 ppm, showing high water resistance, and the electrode sheet resistance can reach less than 2.53 mΩ.
[0078] By comparing Example 1 and Examples 3-4, it can be seen that in the conductive bottom layer of the composite current collector described in the present application, the added amount of conductive agent A is less than that of conductive agent B. Conductive agent B is conductive carbon black and / or carbon nanotubes, which has excellent conductive properties and can take into account the conductive properties of the nano-coating current collector. In the conductive water-resistant layer, the content of conductive agent B is lower than that of conductive agent A. Conductive agent A is a flaky conductive agent with a large particle size and has an excellent shielding effect. The addition of a cross-linking agent can further enhance the water resistance of the coating.
[0079] By comparing Example 1 with Examples 5-6, it can be seen that in the composite current collector described in the present application, the thickness of the conductive water-resistant layer will affect its performance. When the thickness of the conductive water-resistant layer is controlled at 0.3 to 0.8 μm, the performance of the composite current collector is better. If the thickness of the conductive water-resistant layer is too large, the conductive performance deteriorates. If the thickness of the conductive water-resistant layer is too small, the water-resistant performance deteriorates.
[0080] By comparing Example 1 with Examples 7-8, it can be seen that in the composite current collector described in this application, the thickness of the conductive bottom layer will affect its performance. When the thickness of the conductive bottom layer is controlled at 0.2 to 0.4 μm, the performance of the composite current collector is better. If the thickness of the conductive bottom layer is too large, the water resistance will deteriorate and the conductive performance will also be reduced. If the thickness of the conductive bottom layer is too small, the conductive performance will also be affected due to the reduction in the amount of conductive substance in the bottom layer.
[0081] By comparing Example 1 and Comparative Examples 1-2, it can be seen that the conductive water-resistant layer described in the present application is located on the surface of the conductive bottom layer, reducing the number of penetrating micro-channels inside the coating and reducing the ability of water to penetrate the coating film, thereby improving the water resistance of the nano-conductive coating without affecting the overall conductivity of the current collector and its adhesion performance with the electrode material.
[0082] From the comparison between Example 1 and Comparative Example 3, it can be seen that adding a cross-linking agent to the conductive water-resistant layer described in the present application can further enhance the water resistance of the coating.
[0083] The applicant declares that the above is only a specific implementation method of the present application, but the protection scope of the present application is not limited thereto. Technical personnel in the relevant technical field should understand that any changes or substitutions that can be easily thought of by technical personnel in the relevant technical field within the technical scope disclosed in this application fall within the protection scope and disclosure scope of this application.
Claims
1. A composite current collector, comprising a substrate and a conductive bottom layer and a conductive water-resistant layer stacked in sequence on at least one side surface of the substrate, wherein the conductive bottom layer comprises a conductive agent A, a conductive agent B and a binder, and the conductive water-resistant layer comprises a conductive agent A, a conductive agent B, a cross-linking agent and a binder.
2. The composite current collector according to claim 1, wherein: The substrate includes a current collector.
3. The composite current collector according to claim 1 or 2, wherein: The conductive agent A is a flake conductive agent; Optionally, the conductive agent A includes conductive graphite and / or graphene; Optionally, the particle size of the conductive agent A is 1 to 3 μm.
4. The composite current collector according to any one of claims 1 to 3, wherein: The conductive agent B includes conductive carbon black and / or carbon nanotubes; Optionally, the particle size of the conductive agent B is 200-600 nm.
5. The composite current collector according to any one of claims 1 to 4, wherein: The cross-linking agent includes any one of isocyanate, aziridine type curing cross-linking agent or epoxy type curing cross-linking agent or a combination of at least two thereof; Optionally, the adhesive includes a modified polyacrylic acid adhesive and / or a polyacrylic acid adhesive.
6. The composite current collector according to any one of claims 1 to 5, wherein: In the conductive bottom layer, the mass ratio of the conductive agent B to the conductive agent A is (10-20):1; Optionally, the mass ratio of the conductive agent B to the binder is (1-2):
1.
7. The composite current collector according to any one of claims 1 to 6, wherein: The mass ratio of the conductive agent A to the conductive agent B in the conductive water-resistant layer is (10-20):1; Optionally, the mass ratio of the conductive agent A to the binder is (1-2):1; Optionally, the mass ratio of the binder to the cross-linking agent is (80-200):
1.
8. The composite current collector according to any one of claims 1 to 7, wherein: The thickness of the conductive bottom layer is 0.2 to 0.4 μm; Optionally, the thickness of the conductive water-resistant layer is 0.3-0.8 μm.
9. The composite current collector according to any one of claims 1 to 8, wherein: The total thickness of the conductive bottom layer and the conductive water-resistant layer is 0.5-1.2 μm.
10. A method for preparing the composite current collector according to any one of claims 1 to 9, the method comprising the following steps: (1) mixing and dispersing the conductive agent A, the conductive agent B and the binder to obtain a bottom conductive paste, and mixing and dispersing the conductive agent A, the conductive agent B, the crosslinking agent and the binder to obtain a water-resistant conductive paste; (2) coating the bottom conductive paste on the surface of the substrate to obtain a conductive bottom layer, coating the water-resistant conductive paste on the surface of the conductive bottom layer to form a conductive water-resistant layer, and obtaining the composite current collector.
11. A pole piece, wherein: The pole piece comprises the composite current collector as described in any one of claims 1 to 9.
12. A sodium ion battery, wherein: The sodium ion battery comprises the pole piece as claimed in claim 11.
Citation Information
Patent Citations
Dual-layer method of fabricating ultracapacitor current collectors
CN103098161A
Current collector, preparation method of current collector and lithium ion battery comprising current collector
CN105375035A
Composite current collector of lithium ion battery and manufacturing method of composite current collector
CN105762366A
Carbon-coated aluminum foil, preparation method and application
CN106602076A
Negative electrode current collector and negative electrode
CN114843520A