Electrode sheet, battery cell, battery, and electric device

By setting a coating on the electrode sheet to decompose the material to form a recessed area, the problem of the expansion of the electrode assembly during the cycle charging and discharging of the battery cell is solved, and the cycling performance and reliability of the battery are improved.

WO2024244537A1PCT designated stage expired Publication Date: 2024-12-05CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/075991
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-02-05
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The expansion of the electrode assembly during the cyclic charging and discharging of existing battery cells leads to the extrusion of electrolyte, reducing the cyclic performance and increasing the risk of metal dendrites precipitation, affecting the reliability of the battery.

Method used

The coating is provided on the current collector surface of the electrode sheet. The coating contains decomposed materials such as lithium supplement material and pore-making material. After decomposition, it forms a recessed area, reserves expansion space, improves the electrolyte suction rate and liquid retention capacity, and reduces the Expansion force of the electrode assembly.

Benefits of technology

By reserving expansion space and improving the infiltration performance of the electrolyte, the cycle life of the battery is extended, the risk of metal dendrites precipitation is reduced, and the cycle performance and reliability of the battery cell are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024075991_05122024_PF_FP_ABST
    Figure CN2024075991_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to an electrode sheet, a battery cell, a battery, and an electric device. The electrode sheet comprises a current collector, a coating, and an active material layer. The coating is provided on at least one surface of the current collector. The coating comprises at least one coating area. The coating area comprises a decomposable material. The decomposable material is configured to decompose under at least one condition of charging and discharging of the battery cell. The decomposable material comprises at least one of a lithium supplementing material and a pore forming material. The lithium supplementing material comprises a lithium ion-containing compound. The active material layer is provided on at least one surface of the current collector and covers the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Electrode plates, battery cells, batteries and electrical devices

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application No. 202310651153.1 filed on June 2, 2023, entitled “Electrode Plate, Battery Cell, Battery and Electrical Device,” the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application relates to an electrode plate, a battery cell, a battery and an electrical device. Background Art

[0004] Battery cells are widely used due to their reliable performance, pollution-free operation, and zero memory effect. For example, with increasing attention paid to environmental protection and the growing popularity of new energy vehicles, the demand for power battery cells is expected to experience explosive growth.

[0005] As the requirements for battery cell performance increase, the reliability of battery cell usage becomes particularly important. Therefore, how to further improve the cycle performance of battery cells is an urgent problem that needs to be solved today.

[0006] Summary of the Invention

[0007] The present application provides an electrode plate, a battery cell, a battery and an electrical device, and the present application can improve the cycle performance of the battery cell.

[0008] In a first aspect, an embodiment of the present application proposes an electrode plate of a battery cell, wherein the electrode plate includes a current collector, a coating and an active material layer, wherein the coating is arranged on at least one surface of the current collector, the coating includes at least one coating area, the coating area includes a decomposable material, and the decomposable material is configured to decompose in at least one of charging and discharging of the battery cell, the decomposable material includes at least one of a lithium replenishing material and a pore-forming material, and the lithium replenishing material includes a compound containing lithium ions; the active material layer is arranged on at least one surface of the current collector and covers the coating.

[0009] According to the implementation mode of the present application, during the charge and discharge cycle of the battery cell, the decomposable material decomposes and the decomposable material gradually decreases. The active material layer corresponding to this position is recessed toward the current collector, and a slightly recessed area is formed on the surface of the active material layer away from the current collector, thereby reserving expansion space in the thickness direction of the electrode plate and slowing down the expansion force of the electrode assembly. The existence of this expansion space is conducive to improving the reabsorption rate of the electrolyte, improving the wetting performance of the electrolyte on the electrode assembly, and reducing the risk of local metal precipitation and metal dendrite generation in the electrode plate. The expansion space can also store electrolyte, improve the liquid retention capacity of the electrode plate, and thus improve the cycle performance of the battery cell.

[0010] The decomposable material includes at least one of a lithium-replenishing material and a pore-forming material. The lithium-replenishing material can decompose and release lithium ions during the charge and discharge process of the battery cell (for example, during the initial charge), thereby replenishing lithium in the battery system, increasing the lithium ion content in the battery system, and improving the capacity of the battery cell. The pore-forming material can decompose and release gas during the charge and discharge process of the battery cell. When the gas flows through the active material layer, it may cause a pore structure in the active material layer, thereby increasing the porosity of the active material layer, improving its liquid absorption and liquid retention capacity, and thus improving the cycle performance of the battery cell.

[0011] In some embodiments, the lithium supplement material includes one or more of lithium nitride, lithium oxide, lithium peroxide, lithium squarate, and lithium-rich lithium ferrite Li5FeO4.

[0012] In some embodiments, the pore-forming material comprises one or more of carbonates, oxalates, and metal oxides.

[0013] In some embodiments, the carbonate salt comprises one or more of ammonium carbonate, ammonium bicarbonate, and sodium bicarbonate.

[0014] In some embodiments, the oxalate salt includes one or more of ammonium oxalate, sodium oxalate, and ammonium hydrogen oxalate.

[0015] In some embodiments, the metal oxide includes one or more of zinc oxide, magnesium oxide, and aluminum oxide.

[0016] In some embodiments, the ratio of the coating weight of the active material layer to the coating weight of the coating layer is 5.2 to 150, and can optionally be 6.5 to 100. When the ratio of the coating weight of the active material layer to the coating weight is within the above range, the decomposition of the decomposable material during the cyclic charge and discharge process of the battery cell can leave sufficient space for the active material layer to expand, thereby improving the cycle performance of the battery cell.

[0017] In some embodiments, the coating weight C1 of the active material layer satisfies: 65 g / m2 ≤C1≤300g / m 2 .

[0018] In some embodiments, the coating weight C2 of the coating satisfies: 2 g / m 2 ≤C2≤20g / m 2 ; Optionally, 5g / m 2 ≤C2≤20g / m 2 .

[0019] In some embodiments, the ratio of the coating thickness to the active material layer thickness is 0.008 to 0.200; optionally, 0.015 to 0.154. When the ratio of the coating thickness to the active material layer thickness is within the above range, the decomposable material in the coating will not collapse too deeply after decomposition, thereby preventing the recessed area on the surface of the active material layer from being too deep, reducing the risk of cracks in the active material layer and facilitating the electrical performance of the active material. Furthermore, the collapse will not be too shallow, thereby preventing the recessed area on the surface of the active material layer from being too shallow, providing sufficient pre-expansion space for the electrode sheet and improving its liquid retention capacity.

[0020] In some embodiments, the coating has a thickness of 1 μm to 20 μm; optionally 5 μm to 20 μm.

[0021] In some embodiments, the active material layer has a thickness of 80 μm to 300 μm.

[0022] In some embodiments, the ratio of the width of the coating area to the width of the current collector is Y, 0.05≤Y≤0.50; optionally, 0.10≤Y≤0.50. When the ratio of the width of the coating area to the width of the active material layer is within the above range, the decomposable material in the coating will not decompose into a recessed area that is too large, thereby reducing the recessed area on the surface of the active material layer and facilitating the electrical performance of the active material. The recessed area will also not be too small, thereby reducing the recessed area on the surface of the active material layer, providing sufficient pre-expansion space for the electrode sheet and improving its liquid retention capacity.

[0023] In some embodiments, the expansion rate of the electrode plate is Z, the ratio of the width of the coating area to the width of the current collector is Y, and the electrode plate satisfies at least one of the following conditions:

[0024] (1) Z < 20%; 0.10 ≤ Y ≤ 0.50; optionally 0.10 ≤ Y ≤ 0.15;

[0025] (2) 20% ≤ Z < 25%; 0.13 ≤ Y ≤ 0.50; 0.13 ≤ Y ≤ 0.20 is optional;

[0026] (3) 25% ≤ Z < 30%; 0.15 ≤ Y ≤ 0.50; 0.15 ≤ Y ≤ 0.30 is optional;

[0027] (4) 30% ≤ Z; 0.30 ≤ Y ≤ 0.50; 0.33 ≤ Y ≤ 0.50 can be selected;

[0028] According to the embodiment of the present application, when the expansion rate of the electrode plate is large, the size of the coating is increased to provide a relatively larger recessed area for the surface of the active material layer, thereby slowing down the expansion force of the electrode assembly; when the expansion rate of the electrode plate is small, the size of the coating is reduced to make the surface of the active material layer have a relatively small recessed area, which can also play a good role in slowing down the expansion force of the electrode assembly.

[0029] In some embodiments, the coating layer includes multiple coating regions, which are spaced apart on the surface of the current collector and located between the current collector and the active material layer. The multiple coating regions, upon decomposition of the decomposable material, can provide multiple recessed areas for the active material layer, thereby further mitigating the expansion force of the electrode assembly and improving the liquid retention capacity of the electrode sheet.

[0030] In some embodiments, the coating is provided on both opposing surfaces of the current collector. Having the coating on both surfaces can provide multiple recessed areas for the active material layer through decomposition of the decomposable material, thereby further mitigating the expansion force of the electrode assembly and improving the liquid retention capacity of the electrode sheet.

[0031] In a second aspect, an embodiment of the present application provides a battery cell, wherein the battery cell includes an electrode assembly as described in any embodiment of the first aspect of the present application.

[0032] In some embodiments, the electrode plate includes a positive electrode plate.

[0033] In some embodiments, the electrode plate includes a negative electrode plate.

[0034] In a third aspect, an embodiment of the present application provides a battery, which includes the battery cell as described in the second aspect of the present application.

[0035] In a fourth aspect, an embodiment of the present application provides an electrical device comprising a battery as described in any embodiment of the third aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.

[0037] FIG1 is a schematic structural diagram of an electrode plate according to an embodiment of the present application.

[0038] FIG2 is a schematic structural diagram of the electrode plate shown in FIG1 at another angle.

[0039] FIG3 is a schematic cross-sectional view of the electrode sheet shown in FIG2 taken along line AA.

[0040] FIG4 is a schematic structural diagram of another embodiment of the electrode plate of the present application.

[0041] FIG5 is a schematic structural diagram of the electrode plate shown in FIG4 at another angle.

[0042] FIG6 is a schematic cross-sectional view of the electrode sheet shown in FIG5 taken along line BB.

[0043] FIG. 7 is another schematic cross-sectional view of the electrode sheet shown in FIG. 5 taken along line BB.

[0044] FIG8 is another schematic cross-sectional view of the electrode sheet shown in FIG5 taken along line BB.

[0045] FIG9 is a schematic structural diagram of a battery cell according to an embodiment of the present application.

[0046] FIG. 10 is an exploded schematic diagram of the embodiment of the battery cell of FIG. 9 .

[0047] FIG11 is a schematic structural diagram of an embodiment of a battery module of the present application.

[0048] FIG12 is a schematic structural diagram of an embodiment of a battery pack of the present application.

[0049] FIG. 13 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG. 12 .

[0050] FIG14 is a schematic structural diagram of an embodiment of an electric device including the battery cell of the present application as a power source.

[0051] The drawings are not necessarily drawn to scale.

[0052] The following are the descriptions of the reference numerals:

[0053] 1. Battery pack; 2. Upper box; 3. Lower box; 4. Battery module;

[0054] 5. Battery cell; 51. Housing; 52. Electrode assembly;

[0055] 53. Cover plate;

[0056] 6. Electrical devices;

[0057] 7. Electrode plate;

[0058] 71. Current collector; 72. Coating layer; 721. Coating area; 73. Active material layer. DETAILED DESCRIPTION

[0059] Below, the embodiments of the electrode plates, battery cells, batteries, and electrical devices of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0060] It should be noted that, unless otherwise specified, the technical terms or scientific terms used in the embodiments of this application should have the common meanings understood by technicians in the field to which the embodiments of this application belong.

[0061] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.

[0062] In addition, the technical terms "first," "second," etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. In the description of the embodiments of this application, the meaning of "plurality" is more than two, unless otherwise specifically defined.

[0063] In the description of the embodiments of this application, unless otherwise expressly specified or limited, technical terms such as "installed," "connected," "connect," and "fixed" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integration; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; and internal connections between two components or interactions between two components. Those skilled in the art will understand the specific meanings of the above terms in the embodiments of this application based on specific circumstances.

[0064] In the description of the embodiments of the present application, unless otherwise expressly specified or limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or that the first and second features are in indirect contact through an intermediate medium. Furthermore, a first feature being "above," "above," and "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is at a higher level than the second feature. A first feature being "below," "below," and "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is at a lower level than the second feature.

[0065] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0066] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0067] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0068] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0069] In this application, battery cells may include lithium-ion battery cells, lithium-ion primary battery cells, lithium-sulfur battery cells, sodium-lithium-ion battery cells, sodium-ion battery cells, or magnesium-ion battery cells, and the embodiments of this application do not limit this. Battery cells may be cylindrical, flat, rectangular, or other shapes, and the embodiments of this application do not limit this. Battery cells are generally divided into three types based on the packaging method: cylindrical battery cells, prismatic battery cells, and soft-pack battery cells, and the embodiments of this application do not limit this.

[0070] A battery cell includes an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator. The electrolyte is dispersed in the electrode assembly, so that the electrode assembly is infiltrated by the electrolyte, allowing metal ions to move between the positive electrode sheet and the negative electrode sheet through the electrolyte to work. During the cyclic charge and discharge process of the battery cell, the electrode assembly will undergo volume changes (such as volume expansion), which may squeeze the electrolyte out of the electrode assembly. The electrode assembly also absorbs the electrolyte at a slow rate, causing local liquid deficiency in the electrode assembly, which may cause local metal precipitation to produce metal dendrites, deteriorating the cycle performance of the battery cell.

[0071] In view of the above problems, the embodiment of the present application improves the electrode plate and proposes an electrode plate, which is provided with a coating on at least one surface of the current collector. The electrode plate also includes an active material layer, which is provided on at least one surface of the current collector and covers the coating; the coating includes a decomposable material, and during the charge and discharge cycle of the battery cell, the decomposable material decomposes and gradually decreases. The active material layer corresponding to this position is recessed toward the current collector, and a slight recessed area is formed on the surface of the active material layer away from the current collector, thereby reserving expansion space in the thickness direction of the electrode plate and slowing down the expansion force of the electrode assembly; and the existence of this expansion space is conducive to improving the reabsorption rate of the electrolyte, improving the wetting performance of the electrolyte on the electrode assembly, and reducing the risk of local metal precipitation of the electrode plate to produce metal dendrites; and the expansion space can also store electrolyte, improve the liquid retention capacity of the electrode plate, thereby improving the cycle performance of the battery cell.

[0072] Electrode plate

[0073] In a first aspect, an embodiment of the present application provides an electrode plate, which is applied to a battery cell.

[0074] As shown in Figures 1 to 3, the electrode plate 7 includes a current collector 71, a coating 72 and an active material layer 73. The coating 72 is arranged on at least one surface of the current collector 71, and the coating 72 includes at least one coating area 721. The coating area 721 includes a decomposable material, and the decomposable material is configured to decompose in at least one of the battery cell charging and discharging. The decomposable material includes at least one of a lithium replenishing material and a pore-forming material, and the lithium replenishing material includes a compound containing lithium ions; the active material layer 73 is arranged on at least one surface of the current collector 71 and covers the coating 72.

[0075] The active material layer 73 is provided on at least one surface of the current collector 71, and the coating layer 72 is located between the active material layer 73 and the current collector 71. During the charge and discharge cycle of the battery cell, the decomposable material decomposes and the decomposable material gradually decreases. The active material layer 73 corresponding to this position is recessed toward the current collector 71, and a slightly recessed area is formed on the surface of the active material layer 73 facing away from the current collector 71, thereby reserving expansion space in the thickness direction of the electrode plate 7 and slowing down the expansion force of the electrode assembly. The existence of this expansion space is conducive to improving the electrolyte reabsorption rate, improving the electrolyte wetting performance of the electrode assembly, and reducing the risk of metal precipitation and metal dendrite generation on the electrode plate 7. In addition, this expansion space can also store electrolyte, improving the liquid retention capacity of the electrode plate 7, thereby improving the cycle performance of the battery cell.

[0076] The coating 72 includes at least one coated region 721, which includes a decomposable material capable of decomposing during at least one of the conditions of charging and discharging the battery cell. This can be understood as the decomposable material being capable of decomposing during the cycling of the battery cell. For example, the battery cell generates heat during cycling, causing the temperature within the battery cell to rise. When the temperature is relatively high (reaching a preset temperature, such as 110°C), the decomposable material may decompose. For another example, after the battery cell is injected with electrolyte, the electrolyte diffuses into the electrode plate 7 and comes into contact with the decomposable material. The decomposable material dissolves in the electrolyte and may undergo a chemical reaction, causing the decomposable material to decompose. For another example, during cycling, the battery cell has a certain operating voltage, and the decomposable material decomposes under the operating voltage. Based on this, it can be considered that the decomposable material decomposes when a preset condition is met, which can be the preset temperature mentioned above, or when the decomposable material dissolves in the electrolyte, or under the operating voltage system. FIG2 and FIG3 show that the coating layer 72 includes four coating regions 721 . Of course, the number of coating regions 721 may be relatively less or relatively more.

[0077] In some embodiments, the decomposable material includes a lithium-replenishing material, which includes a compound containing lithium ions. Since the battery cell can form a solid electrolyte interphase (SEI) film during the formation process, and the formation of the SEI film is a process that consumes active lithium ions, the capacity of the battery cell is reduced. The lithium-replenishing material can decompose and release lithium ions during the charge and discharge process of the battery cell (for example, during the first charge process), thereby replenishing the lithium of the battery system, increasing the content of lithium ions in the battery system, and improving the capacity of the battery cell. As the lithium-replenishing material decomposes, the coating 72 gradually collapses, and the active material layer 73 corresponding to the coating 72 is recessed toward the current collector 71, forming a local recessed area on the surface of the active material layer 73. The active material layer 73 corresponding to the coating 72 can be understood as the overlap of the projection surface of the coating 72 and the projection surface of part of the active material layer 73 in the thickness direction of the electrode plate 7. This part of the active material layer 73 is the active material layer 73 corresponding to the coating 72.

[0078] For example, the lithium supplement material may include one or more of lithium nitride, lithium oxide, lithium peroxide, lithium quartz, and lithium-rich lithium ferrite Li5FeO4. The above lithium supplement material is configured to decompose under the operating voltage of the battery cell.

[0079] It can replenish lithium for the battery system during the cycle charge and discharge process of the battery cell, and as the lithium replenishing material decomposes, the active material layer 73 correspondingly becomes concave, leaving expansion space for the electrode plate 7, which is beneficial to improving the cycle performance of the battery cell.

[0080] In some embodiments, the decomposable material includes a pore-forming material. The pore-forming material is configured to decompose and release gas during the charge and discharge process of the battery cell. When the gas flows through the active material layer 73, a pore structure may be generated in the active material layer 73, thereby increasing the porosity of the active material layer 73, improving its liquid absorption and liquid retention capabilities, and thus improving the cycle performance of the battery cell. As the pore-forming material decomposes, the coating 72 gradually collapses, and the active material layer 73 corresponding to the coating 72 is recessed toward the current collector 71, forming a local recessed area on the surface of the active material layer 73. The active material layer 73 corresponding to the coating 72 can be understood as the projection surface of the coating 72 overlapping with the projection surface of part of the active material layer 73 in the thickness direction of the electrode plate 7. This part of the active material layer 73 is the active material layer 73 corresponding to the coating 72.

[0081] For example, the pore-forming material may include one or more of carbonates, oxalates, and metal oxides. These pore-forming materials are capable of decomposing during the battery cell's charge and discharge cycles. For example, oxalates and metal oxides are capable of decomposing at the battery cell's operating voltage, while carbonates are capable of decomposing when the battery cell reaches a preset temperature.

[0082] For example, the carbonate includes one or more of ammonium carbonate, ammonium bicarbonate, and sodium bicarbonate.

[0083] For example, the oxalate includes one or more of ammonium oxalate, sodium oxalate, and ammonium hydrogen oxalate.

[0084] For example, the metal oxide includes one or more of zinc oxide, magnesium oxide, and aluminum oxide.

[0085] In some embodiments, the decomposable material comprises 80% or more by weight of the coating 72. Within this range, the decomposable material can provide a recessed area for the active material layer 73 during decomposition, mitigating the expansion force of the electrode assembly. Furthermore, the decomposable material can improve the capacity and cycle performance of the battery cell.

[0086] Illustratively, the mass percentage of the decomposable material can be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 88%, 90%, 92%, 94%, 95% or a range consisting of any two of the above values.

[0087] In some embodiments, the coating layer 72 may further include a binder. The binder can enhance the bonding strength between the coating layer 72 and the current collector 71 , and can enhance the bonding strength between the coating layer 72 and the active material layer 73 .

[0088] In some embodiments, the binder may comprise 1% to 5% by mass based on the total mass of the coating layer 72 .

[0089] Illustratively, the mass percentage of the binder may be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or a range consisting of any two of the above values.

[0090] Illustratively, the binder includes one or more of polyvinylidene fluoride, polymethyl acrylate, styrene-butadiene rubber, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, polyvinyl alcohol, and polyurethane.

[0091] In some embodiments, the coating 72 may further include a conductive agent, which can improve the conductivity of the coating 72 and thus improve the conductivity of the electrode plate 7 as a whole.

[0092] In some embodiments, the conductive agent may comprise 1% to 5% by mass based on the total mass of the coating layer 72 .

[0093] Illustratively, the mass percentage of the conductive agent may be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or a range consisting of any two of the above values.

[0094] Exemplarily, the conductive agent includes one or more of activated carbon, carbon black, graphite, carbon nanotubes and carbon fibers.

[0095] In some embodiments, the ratio of the thickness of the coating layer 72 to the thickness of the active material layer 73 is 0.008 to 0.200; optionally, 0.015 to 0.154. When the ratio of the thickness of the coating layer 72 to the thickness of the active material layer 73 is within the above range, the decomposable material in the coating layer 72 will not collapse too deeply after decomposition, thereby preventing the recessed area on the surface of the active material layer 73 from being too deep, reducing the risk of cracks in the active material layer 73 and facilitating the electrical performance of the active material. The collapse will also not be too shallow, thereby preventing the recessed area on the surface of the active material layer 73 from being too shallow, providing sufficient pre-expansion space for the electrode plate 7 and improving its liquid retention capacity. It should be noted that the thickness of the coating 72 can be an average thickness, for example, measurements are taken at multiple locations on the coating 72, and the average value of the measured values ​​is calculated. When the coating 72 includes multiple coating areas 721, the thickness of the coating 72 can be the average value of the thicknesses of the multiple coating areas 721; the thickness of the active material layer 73 can also be an average thickness, for example, measurements are taken at multiple locations on the active material layer 73, and the average value of the measured values ​​is calculated.

[0096] For example, the ratio of the thickness of the coating layer 72 to the thickness of the active material layer 73 may be 0.008, 0.009, 0.010, 0.012, 0.015, 0.018, 0.020, 0.022, 0.025, 0.028, 0.030, 0.032, 0.035, 0.038, 0.040, 0.042, 0.045, 0.048, 0.050, 0.052, 0.05 5. 0.058, 0.060, 0.062, 0.065, 0.068, 0.070, 0.075, 0.078, 0.080, 0.090, 0.100, 0.110, 0.120, 0.130, 0.140, 0.150, 0.154, 0.155, 0.160, 0.170, 0.180, 0.190, 0.200, or a range consisting of any two of the above values.

[0097] As some examples, the thickness of the coating 72 may be 1 μm to 20 μm, optionally 5 μm to 20 μm, and further optionally 5 μm to 10 μm. For example, the thickness of the coating 72 may be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, or a range consisting of any two of the foregoing values.

[0098] As some examples, the thickness of the active material layer 73 is 80 μm to 300 μm. For example, the thickness of the active material layer 73 can be 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 270 μm, 280 μm, 290 μm, 300 μm, or a range consisting of any two of the above values.

[0099] In the embodiments of the present application, the thicknesses of the coating layer 72 and the active material layer 73 are well known in the art and can be measured using equipment and methods well known in the art. For example, the thickness of the coating layer 72 and the thickness of the active material layer 73 can be measured by scanning a cross section of the electrode plate 7 using a scanning electron microscope (SEM). H1 shown in FIG3 represents the thickness of the coating layer 72, and H2 represents the thickness of the active material layer 73.

[0100] In some embodiments, the ratio of the width of the coating area 721 to the width of the current collector 71 is Y, 0.05≤Y≤0.50. When the ratio of the width of the coating area 721 to the width of the active material layer 73 is within the above range, after the decomposable material in the coating 72 decomposes, the depressed area will not be too large, so that the depressed area on the surface of the active material layer 73 will not be too large, and it is beneficial to the electrical properties of the active material; and the depressed area will not be too small, so that the depressed area on the surface of the active material layer 73 will not be too small, providing sufficient pre-expansion space for the electrode plate 7 and improving its liquid retention capacity. In an embodiment of the present application, for example, the length of the coating area 721 can be the same as the length of the active material layer 73, or the length of the coating area 721 can be less than the length of the active material layer 73. It should be noted that the width of the coating area 721 can be an average width, for example, measurements are taken at multiple locations in the coating area 721, and the average value of the measured values ​​is calculated; the width of the active material layer 73 can also be an average width, for example, measurements are taken at multiple locations in the active material layer 73, and the average value of the measured values ​​is calculated.

[0101] Optionally, 0.10≤Y≤0.50; further optionally, 0.11≤Y≤0.33; further optionally, 0.11≤Y≤0.23. When Y is within the above range, the cycle performance of the battery cell can be further improved.

[0102] For example, the ratio Y of the width of the coating area 721 to the width of the current collector 71 can be 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.18, 0.20, 0.22, 0.25, 0.26, 0.28, 0.30, 0.33, 0.35, 0.38, 0.40, 0.42, 0.45, 0.46, 0.48, 0.50 or a range consisting of any two of the above values.

[0103] In the embodiment of the present application, the width direction of the current collector 71 is perpendicular to the thickness direction of the electrode plate 7, and the width direction of the current collector 71 can also be considered to be parallel to the direction from the area of ​​the current collector 71 not coated with active material (for example, the corresponding tab area) to the area of ​​the current collector 71 coated with active material (corresponding to the active material layer 73).

[0104] In some embodiments, the width of the coating area 721 may be 5 mm to 50 mm. Alternatively, it may be 16 mm to 35 mm. For example, the width of the coating area 721 may be 5 mm, 6 mm, 8 mm, 10 mm, 12 mm, 15 mm, 16 mm, 18 mm, 20 mm, 22 mm, 25 mm, 28 mm, 30 mm, 32 mm, 35 mm, 38 mm, 40 mm, 42 mm, 45 mm, 48 mm, 50 mm, or a range consisting of any two of the above values.

[0105] In some embodiments, the width of the active material layer 73 may be 60 mm to 300 mm.

[0106] For example, the width of the active material layer 73 can be 60 mm, 65 mm, 70 mm, 75 mm, 80 mm, 85 mm, 90 mm, 95 mm, 100 mm, 105 mm, 110 mm, 115 mm, 120 mm, 125 mm, 130 mm, 135 mm, 140 mm, 145 mm, 150 mm, 155 mm, 160 mm, 165 mm, 170 mm, 175 mm, 180 mm, 185 mm, 190 mm, 195 mm, 200 mm, 205 mm, 210 mm, 215 mm, 220 mm, 225 mm, 230 mm, 235 mm, 240mm, 245mm, 250mm, 255mm, 260mm, 265mm, 270mm, 275mm, 280mm, 285mm, 290mm, 295mm, 300mm, or a range consisting of any two of the above values.

[0107] In the embodiment of the present application, the widths of the coating region 721 and the active material layer 73 are well known in the art and can be measured using equipment and methods well known in the art. For example, the widths of the coating region 721 and the active material layer 73 can be measured by scanning a cross section of the electrode sheet 7 using a scanning electron microscope (SEM). W1 shown in FIG. 2 represents the width of the coating region 721, and W2 represents the width of the active material layer 73.

[0108] The electrode plate 7 includes an active material layer 73 containing an active material. Active materials of different types or contents expand to different degrees during the charge and discharge process of the battery cell. In order to better adapt to the active material of the electrode plate 7, the size of the coating 72 can be adjusted. For example, when the expansion rate of the electrode plate 7 is large, the size of the coating 72 is increased to provide a relatively larger recessed area for the surface of the active material layer 73, thereby slowing down the expansion force of the electrode assembly; when the expansion rate of the electrode plate 7 is small, the size of the coating 72 is reduced so that the surface of the active material layer 73 has a relatively small recessed area, which can also play a good role in slowing down the expansion force of the electrode assembly.

[0109] The expansion rate Z of the electrode plate 7 = [(the thickness of the electrode plate 7 after expansion - the initial thickness of the electrode plate 7) / the initial thickness]*100%.

[0110] The initial thickness refers to the thickness of the electrode plate 7 in a fresh battery cell. A fresh battery cell can be understood as a battery cell with a cycle number of less than or equal to 10 cycles.

[0111] The thickness after expansion refers to the thickness of the electrode plate 7 of the battery cell after 500 cycles of charge and discharge at a 1C rate.

[0112] In an embodiment of the present application, the expansion rate of the electrode plate 7 can be detected by the following method. For example, 10 battery cells from the same batch are used as measurement samples, and the electrode plates 7 in 5 battery cells are taken out. The electrode plates 7 are cleaned in deionized water and dried at 85°C for 4 hours. The thickness of the electrode plates 7 is measured, and the average thickness is calculated and recorded as the initial thickness; the remaining 5 batteries are cyclically charged and discharged (1C rate). After 500 cycles, the electrode plates 7 in the battery cells are taken out, the electrode plates 7 are cleaned in deionized water and dried at 85°C for 4 hours, the thickness of the electrode plates 7 is measured, and the average thickness is calculated and recorded as the thickness after expansion, thereby calculating the expansion rate of the electrode plates 7.

[0113] In some embodiments, Z < 20%; 0.10 ≤ Y ≤ 0.50; optionally, 0.10 ≤ Y ≤ 0.15. For example, Z can be 6%, 7%, 8%, 10%, 11%, 12%, 12%, 15%, 16%, 17%, 18%, 19%, 19.5%, or a range consisting of any two of the above values. Y can be 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.18, 0.20, 0.22, 0.25, 0.26, 0.28, 0.30, 0.33, 0.35, 0.38, 0.40, 0.42, 0.45, 0.46, 0.48, 0.50, or a range consisting of any two of the above values.

[0114] In some embodiments, 20% ≤ Z < 25%; 0.13 ≤ Y ≤ 0.50; optionally, 0.13 ≤ Y ≤ 0.20. For example, Z can be 20%, 21%, 22%, 23%, 24%, 24.5%, or a range consisting of any two of the above values. Y can be 0.13, 0.14, 0.15, 0.16, 0.18, 0.20, 0.22, 0.25, 0.26, 0.28, 0.30, 0.33, 0.35, 0.38, 0.40, 0.42, 0.45, 0.46, 0.48, 0.50, or a range consisting of any two of the above values.

[0115] In some embodiments, 25% ≤ Z < 30%; 0.15 ≤ Y ≤ 0.50; optionally, 0.15 ≤ Y ≤ 0.30. For example, Z can be 25%, 26%, 27%, 28%, 29%, 29.5%, or a range consisting of any two of the above values. Y can be 0.15, 0.16, 0.18, 0.20, 0.22, 0.25, 0.26, 0.28, 0.30, 0.33, 0.35, 0.38, 0.40, 0.42, 0.45, 0.46, 0.48, 0.50, or a range consisting of any two of the above values.

[0116] In some embodiments, 30% ≤ Z; 0.30 ≤ Y ≤ 0.50; optionally, 0.33 ≤ Y ≤ 0.50. For example, Z can be 30%, 32%, 33%, 35%, 36%, 38%, 39%, 40%, 42%, 45%, or a range consisting of any two of the foregoing values. Y can be 0.30, 0.31, 0.32, 0.33, 0.35, 0.38, 0.40, 0.42, 0.45, 0.46, 0.48, 0.50, or a range consisting of any two of the foregoing values.

[0117] It should be noted here that when the electrode plate 7 is a positive electrode plate, its expansion rate and Y value range satisfy the above ranges; when the electrode plate 7 is a negative electrode plate, its expansion rate and Y value range satisfy the above ranges; however, the selection of the Y values ​​of the positive electrode plate and the negative electrode plate may not interfere with each other.

[0118] In some embodiments, the ratio of the coating weight of the active material layer 73 to the coating weight of the coating layer 72 is 5.2 to 200; optionally, 6.5 to 100.

[0119] When the ratio of the coating weight of the active material layer 73 to the coating weight of the coating layer 72 is within the above range, the decomposition of the decomposable material during the battery cell charge and discharge cycle can leave sufficient expansion space for the active material layer 73, thereby improving the cycle performance of the battery cell.

[0120] Exemplarily, the ratio of the coating weight of the active material layer 73 to the coating weight of the coating layer 72 can be 5.2, 6, 6.5, 8, 10, 12, 13, 15, 16, 18, 20, 22, 25, 28, 30, 32, 35, 38, 40, 42, 45, 50, 55, 58, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, 130, 135, 140, 145, 150 or a range consisting of any two of the above values.

[0121] In some embodiments, the coating weight C1 of the active material layer 73 satisfies: 65 g / m 2 ≤C1≤300g / m 2 When the coating weight of the active material layer 73 is within the above range, the energy density of the battery cell can be increased.

[0122] For example, the coating weight C1 of the active material layer 73 may be 65 g / m 2 , 68g / m 2 , 70g / m 2 , 72g / m 2 , 75g / m 2 , 78g / m 2 , 80g / m 2 , 85g / m 2 , 90g / m 2 , 95g / m 2 , 100g / m 2 , 105g / m 2 , 110g / m 2 , 115g / m 2 , 120g / m 2 , 125g / m 2 , 130g / m 2 , 135g / m 2 , 140g / m 2 , 150g / m 2 , 155g / m 2 , 160g / m 2 , 165g / m 2 , 170g / m 2 , 180g / m 2 , 190g / m 2 , 200g / m 2 , 210g / m 2 , 220g / m 2 , 230g / m 2 , 240g / m 2 , 250g / m 2, 260g / m 2 , 270g / m 2 , 280g / m 2 , 290g / m 2 , 300g / m 2 Or a range consisting of any two of the above values.

[0123] In some embodiments, the coating weight C2 of the coating layer 72 satisfies: 2 g / m 2 ≤C2≤20g / m 2 ; Optionally, 5g / m 2 ≤C2≤20g / m 2 When the coating weight of the coating layer 72 is within the above range, it can provide a reserved expansion space for the active material layer 73, thereby improving the cycle performance of the battery cell.

[0124] For example, the coating weight C2 of the coating layer 72 may be 2 g / m 2 , 3g / m 2 , 4g / m 2 , 5g / m 2 , 6g / m 2 , 7g / m 2 , 8g / m 2 , 9g / m 2 , 10g / m 2 , 11g / m 2 , 12g / m 2 , 13g / m 2 , 14g / m 2 , 15g / m 2 , 16g / m 2 , 17g / m 2 , 18g / m 2 , 19g / m 2 , 20g / m 2 Or a range consisting of any two of the above values.

[0125] In the embodiment of the present application, the coating weight of the active material layer 73 and the coating 72 has a meaning well known in the art and can be measured using instruments and methods well known in the art. For example, take an electrode plate 7 that is coated on one side and cold pressed (if it is an electrode plate coated on both sides, the active material layer 73 and the coating 72 on one side can be wiped off first), punch it into small discs with an area of ​​S1, weigh it, and record it as M1. Then wipe off the active material layer 73 of the electrode plate 7 after weighing, weigh the weight of the current collector 71 and the coating 72, and record it as M0. The coating weight of the active material layer 73 = (the weight of the electrode plate 7 M1 - the weight of the current collector 71 and the coating 72 M0) / S1. Wipe off the coating 72, weigh the weight of the current collector 71 as M2, and the coating weight of the coating 72 = (the weight of the current collector 71 and the coating 72 M0 - the weight of the current collector 71 M2) / S1.

[0126] The parameters mentioned in the embodiments of this application refer to the parameter ranges of the single-sided coating 72 or active material layer 73. When the coating 72 or active material layer 73 is provided on both surfaces of the current collector 71, the parameters of the coating 72 or active material layer 73 on either surface meet the requirements of this application and are considered to fall within the scope of protection of this application.

[0127] The coating layer 72 includes at least one coating region 721. The coating region 721 may be one or more. When there are multiple coating regions 721, there may be two, three, four, etc. The multiple coating regions 721 may be spaced apart on the surface of the current collector 71 and located between the current collector 71 and the active material layer 73. The multiple coating regions 721 can provide multiple recessed areas for the active material layer 73 through the decomposition of the decomposable material, thereby further mitigating the expansion force of the electrode assembly and improving the liquid retention capacity of the electrode plate 7.

[0128] The projection profile of the coating area 721 in the thickness direction can be a regular geometric shape or an irregular geometric shape. The regular geometric shape can be a triangle, quadrilateral, pentagon, hexagon, octagon, circle, ellipse, etc.; at least part of the irregular geometric shape can be an arc, etc.

[0129] The current collector 71 includes two surfaces opposite to each other along its own thickness direction, and the coating 72 is provided on at least one surface of the current collector 71 . For example, the coating 72 can be provided on one of the surfaces of the current collector 71 , or the coating 72 can be provided on both surfaces of the current collector 71 .

[0130] As shown in Figures 4 to 7, when the coating 72 is provided on both surfaces of the current collector 71, the structure of the electrode plate 7 may include an active material layer 73, a coating 72, a current collector 71, a coating 72, and an active material layer 73 arranged in sequence along the thickness direction. The coatings 72 on the two surfaces may be arranged completely symmetrically; or they may be arranged asymmetrically, for example, the coatings 72 on the two surfaces may be staggered, that is, the projections of the coatings 72 on the two surfaces in the thickness direction may overlap or not overlap. Figure 6 shows a schematic diagram of the basically symmetrical arrangement of the coatings 72 on the two surfaces of the electrode plate 7. Figure 7 shows a schematic diagram of the asymmetrical arrangement of the coatings 72 on the two surfaces of the electrode plate 7.

[0131] The coating amounts of the coating layers 72 on the two surfaces may be different or the same. The coating shapes of the coating layers 72 on the two surfaces may be different or the same.

[0132] When the coating 72 is provided on one surface of the current collector 71, the structure of the electrode plate 7 may include the current collector 71, the coating 72 and the active material layer 73 arranged in sequence along the thickness direction; or, as shown in FIG8 , the structure of the electrode plate 7 may include the active material layer 73, the current collector 71, the coating 72 and the active material layer 73 arranged in sequence along the thickness direction.

[0133] In some embodiments, the active material layer 73 includes a positive electrode active material. In this case, the electrode plate 7 is a positive electrode plate, the active material layer 73 is a positive electrode active material layer, and the current collector 71 is a positive electrode current collector.

[0134] In some embodiments, the active material layer 73 includes a negative electrode active material. In this case, the electrode plate 7 is a negative electrode plate, the active material layer 73 is a negative electrode active material layer, and the current collector 71 is a negative electrode current collector.

[0135] [Positive electrode]

[0136] In some embodiments, the positive electrode plate is the electrode plate described above. The positive electrode plate includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector and including a positive electrode active material. The positive electrode plate also includes a coating disposed on at least one surface of the positive electrode current collector and covered by the positive electrode active material layer.

[0137] For example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is provided on either or both of the two facing surfaces of the positive electrode current collector.

[0138] When the battery cell of the present application is a lithium-ion battery, the positive electrode active material may include, but is not limited to, at least one of a lithium-containing transition metal oxide, a lithium-containing phosphate, and their respective modified compounds. Examples of the lithium transition metal oxide may include, but are not limited to, at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of the lithium-containing phosphate may include, but are not limited to, at least one of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds.

[0139] In some embodiments, in order to further improve the energy density of the battery cell, the positive electrode active material for the lithium ion battery may include a general formula of Li a Ni b Co c M d O e A f At least one of a lithium transition metal oxide and a modified compound thereof. 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M comprises at least one of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, and B, and A comprises at least one of N, F, S, and Cl.

[0140] As an example, the positive active material for lithium ion batteries may include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM333),LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523),LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622),LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.85 Co 0.15 Al 0.05 At least one of O2, LiFePO4, and LiMnPO4.

[0141] When the battery cell of the present application is a sodium ion battery, the positive electrode active material may include but is not limited to at least one of sodium-containing transition metal oxides, polyanion materials (such as phosphates, fluorophosphates, pyrophosphates, sulfates, etc.), and Prussian blue materials.

[0142] As an example, the positive active material for sodium ion batteries may include NaFeO2, NaCoO2, NaCrO2, NaMnO2, NaNiO2, NaNi 1 / 2 Ti 1 / 2 O2、NaNi 1 / 2 Mn 1 / 2 O2、Na 2 / 3 Fe 1 / 3 Mn 2 / 3 O2、NaNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, NaFePO4, NaMnPO4, NaCoPO4, Prussian blue materials, general formula X p M' q (PO4) r O x Y 3-x At least one of the materials. p M' q (PO4) r O x Y 3-x , 0<p≤4, 0<q≤2, 1≤r≤3, 0≤x≤2, X includes H + 、Li + 、Na + , K + and NH4 + At least one of , M' is a transition metal cation, optionally at least one of V, Ti, Mn, Fe, Co, Ni, Cu and Zn, and Y is a halogen anion, optionally at least one of F, Cl and Br.

[0143] In the present application, the modified compounds of the above-mentioned positive electrode active materials may be the positive electrode active materials subjected to doping modification and / or surface coating modification.

[0144] In some embodiments, the positive electrode active material layer may further optionally include a positive electrode conductive agent. The present application does not particularly limit the type of the positive electrode conductive agent. By way of example, the positive electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the positive electrode conductive agent is ≤5% based on the total mass of the positive electrode active material layer.

[0145] In some embodiments, the positive electrode active material layer may further optionally include a positive electrode binder. This application does not particularly limit the type of the positive electrode binder. As an example, the positive electrode binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylic resin. In some embodiments, based on the total mass of the positive electrode active material layer, the mass percentage of the positive electrode binder is ≤5%.

[0146] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0147] The positive electrode active material layer is typically formed by coating a positive electrode slurry onto a positive electrode current collector, followed by drying and cold pressing. The positive electrode slurry is typically formed by dispersing the positive electrode active material, an optional conductive agent, an optional binder, and any other components in a solvent and stirring them uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP).

[0148] [Negative electrode]

[0149] In some embodiments, the negative electrode plate is the electrode plate described above. The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector and including a negative electrode active material. The negative electrode plate also includes a coating disposed on at least one surface of the negative electrode current collector and covered by the negative electrode active material layer.

[0150] The negative electrode active material can be any negative electrode active material known in the art for use in battery cells. For example, the negative electrode active material may include, but is not limited to, at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. The silicon-based material may include at least one of elemental silicon, silicon oxide, a silicon-carbon composite, a silicon-nitrogen composite, and a silicon alloy. The tin-based material may include at least one of elemental tin, tin oxide, and a tin alloy.

[0151] In some embodiments, the negative electrode active material layer may further optionally include a negative electrode conductive agent. The present application does not particularly limit the type of the negative electrode conductive agent. For example, the negative electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the negative electrode conductive agent is ≤5 wt % based on the total weight of the negative electrode active material layer.

[0152] In some embodiments, the negative electrode active material layer may further optionally include a negative electrode binder. The present application embodiment does not particularly limit the type of the negative electrode binder. As an example, the negative electrode binder may include at least one of styrene-butadiene rubber (SBR), a water-soluble unsaturated resin SR-1B, a water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). In some embodiments, the mass percentage of the negative electrode binder is ≤5 wt% based on the total weight of the negative electrode active material layer.

[0153] In some embodiments, the negative electrode active material layer may optionally include other additives. For example, the other additives may include thickeners, such as sodium carboxymethyl cellulose (CMC-Na), PTC thermistor materials, and the like. In some embodiments, the weight percentage of the other additives is ≤ 2 wt % based on the total weight of the negative electrode active material layer.

[0154] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include at least one of copper, a copper alloy, nickel, a nickel alloy, titanium, a titanium alloy, silver, and a silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0155] The negative electrode active material layer is typically formed by coating a negative electrode slurry onto a negative electrode current collector, followed by drying and cold pressing. The negative electrode slurry is typically formed by dispersing the negative electrode active material, an optional conductive agent, an optional binder, and other optional additives in a solvent and stirring until uniformly mixed. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.

[0156] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode active material layer. For example, in some embodiments, the negative electrode plate described in the embodiments of the present application further includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode active material layer and disposed on the surface of the negative electrode current collector. In other embodiments, the negative electrode plate described in the embodiments of the present application further includes a protective layer covering the surface of the negative electrode active material layer.

[0157] battery cells

[0158] Secondly, embodiments of the present application also provide a battery cell. A battery cell, also known as a rechargeable battery or storage battery, refers to a battery that can be recharged to activate the active material after discharge for continued use. Typically, a battery cell includes an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator. The separator is disposed between the positive and negative electrode sheets and primarily prevents short circuits between the positive and negative electrodes while allowing active ions to pass through.

[0159] The present application has no particular limitation on the type of battery cells. For example, the battery cells may be lithium-ion batteries, sodium-ion batteries, etc. In particular, the battery cells may be lithium-ion battery cells.

[0160] In some embodiments, the positive electrode sheet may be the positive electrode sheet of any embodiment of the first aspect of the present application, and the negative electrode sheet may be a conventional negative electrode sheet, which may not include a coating.

[0161] In other embodiments, the negative electrode plate may be the negative electrode plate of any embodiment of the first aspect of the present application, and the positive electrode plate may be a conventional positive electrode plate, which may not include a coating.

[0162] In some further embodiments, the positive electrode sheet may be the positive electrode sheet of any embodiment of the first aspect of the present application, and the negative electrode sheet may be the negative electrode sheet of any embodiment of the first aspect of the present application.

[0163] [Electrolyte]

[0164] The battery cells also include an electrolyte.

[0165] During the charge and discharge process of a battery cell, active ions are embedded and released back and forth between the positive and negative electrodes, and the electrolyte conducts the active ions between the positive and negative electrodes. The present application embodiment does not specifically limit the type of electrolyte, and the electrolyte can be selected based on actual needs.

[0166] The electrolyte solution includes an electrolyte salt and a solvent. The types of the electrolyte salt and the solvent are not particularly limited and can be selected according to actual needs.

[0167] When the battery cell of the present application is a lithium-ion battery, as an example, the electrolyte salt may include but is not limited to at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0168] When the battery cell of the present application is a sodium ion battery, as an example, the electrolyte salt may include but is not limited to at least one of sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalatoborate (NaDFOB), sodium dioxalatoborate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorobis(oxalatophosphate) (NaDFOP) and sodium tetrafluorooxalatophosphate (NaTFOP).

[0169] As an example, the solvent may include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0170] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature power performance.

[0171] [Isolation film]

[0172] The battery cell also includes a separator.

[0173] In some embodiments, the battery cell further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0174] In some embodiments, the material of the separator may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.

[0175] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet may be formed into an electrode assembly through a winding process and / or a lamination process.

[0176] In some embodiments, the battery cell may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0177] In some embodiments, the outer packaging of the battery cell may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the battery cell may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0178] The present application has no particular limitation on the shape of the battery cell, which can be cylindrical, square, or any other shape. FIG9 shows a battery cell 5 with a square structure as an example.

[0179] In some embodiments, as shown in FIG10 , the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the separator may be formed into an electrode assembly 52 through a winding process and / or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 may be one or more, which can be adjusted according to demand.

[0180] The preparation method of the battery cell of the present application is well known. In some embodiments, a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte can be assembled to form a battery cell. As an example, the positive electrode sheet, separator, and negative electrode sheet can be wound and / or laminated to form an electrode assembly. The electrode assembly is placed in an outer packaging, dried, and then injected with electrolyte. The battery cell is then vacuum packaged, allowed to stand, formed, and shaped.

[0181] In some embodiments of the present application, the battery cells according to the present application can be assembled into a battery module. The battery module can contain multiple battery cells, and the specific number can be adjusted according to the application and capacity of the battery module.

[0182] Figure 11 is a schematic diagram of an exemplary battery module 4. As shown in Figure 11 , within the battery module 4, multiple battery cells 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple battery cells 5 may be secured together using fasteners.

[0183] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.

[0184] In some embodiments, the battery modules 4 may be assembled into a battery pack, and the number of battery modules 4 included in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0185] Figures 12 and 13 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 12 and 13, the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 covers the lower case 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the battery box.

[0186] In the embodiments of the present application, a battery cell, a battery module, and a battery pack may all be used as examples of batteries.

[0187] Electrical devices

[0188] The third aspect of the embodiments of the present application provides an electric device, which includes at least one of the battery cells, battery modules or battery packs of the present application. The battery cells, battery modules or battery packs can be used as the power source of the electric device, and can also be used as the energy storage unit of the electric device. The electric device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0189] The electrical device may select a battery cell, a battery module or a battery pack according to its usage requirements.

[0190] FIG14 is a schematic diagram of an exemplary electric device 6. The electric device 6 is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the electric device 6, a battery pack or battery module may be used.

[0191] As another example, an electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a battery cell as a power source.

[0192] Example

[0193] The following examples describe the present disclosure in more detail. These examples are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing. The instruments used in the examples are commercially available.

[0194] Example 1

[0195] 1. Preparation of positive electrode sheet

[0196] Aluminum foil with a thickness of 12 μm was used as the positive electrode current collector.

[0197] The lithium nitride lithium supplement material, the conductive agent carbon black, and the binder polyvinylidene fluoride (PVDF) are added to the solvent N-methylpyrrolidone (NMP) in a mass ratio of 90:5:5 and stirred thoroughly to form a uniform functional slurry; the functional slurry is evenly coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a coating is obtained.

[0198] The positive electrode active material LiNi 0.8 Co0.1 Mn 0.1 O2 (NCM811), conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in an appropriate amount of solvent N-methylpyrrolidone NMP in a weight ratio of 97.5:1.4:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is evenly coated on the surface of the positive electrode collector aluminum foil, and after drying and cold pressing, a positive electrode sheet containing a positive electrode active material layer is obtained, wherein the positive electrode active material layer is covered with a coating, and the positive electrode sheet includes a positive electrode active material layer, a coating, a positive electrode collector, a coating and a positive electrode active material layer arranged in sequence along the thickness direction.

[0199] 2. Preparation of negative electrode sheet

[0200] A copper foil with a thickness of 8 μm was used as the negative electrode current collector.

[0201] The lithium nitride lithium supplement material, the conductive agent carbon black (Super P), and the binder polyvinylidene fluoride (PVDF) are added to the solvent N-methylpyrrolidone NMP in a mass ratio of 90:5:5 and stirred thoroughly to form a uniform functional slurry; the functional slurry is evenly coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a coating is obtained.

[0202] The negative electrode active material graphite (95% artificial graphite and 5% natural graphite), binder styrene-butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC-Na), and conductive agent carbon black (Super P) are fully stirred and mixed in an appropriate amount of solvent deionized water in a weight ratio of 96.2:1.8:1.2:0.8 to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on the surface of the negative electrode collector copper foil, and after drying and cold pressing, a negative electrode active material layer is obtained, wherein the negative electrode active material layer covers the coating, and the negative electrode plate includes a negative electrode active material layer, a coating, a negative electrode collector, a coating and a negative electrode active material layer arranged in sequence along the thickness direction.

[0203] 3. Isolation film

[0204] A porous polyethylene (PE) film is used as the separator.

[0205] 4. Preparation of electrolyte

[0206] In an environment with a water content of less than 10 ppm, non-aqueous organic solvents ethylene carbonate EC and diethyl carbonate DMC are mixed in a volume ratio of 1:1 to obtain an electrolyte solvent, and then lithium salt lithium hexafluorophosphate and the mixed electrolyte solvent are mixed to prepare an electrolyte with a lithium salt concentration of 1 mol / L.

[0207] 5. Preparation of battery cells

[0208] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive electrode sheet and the negative electrode sheet to serve as an isolation, and then wound to obtain an electrode assembly; the electrode assembly is placed in an outer packaging shell, dried, and then injected with electrolyte, and after vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.

[0209] Comparative Example 1

[0210] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, the preparation method of the positive electrode sheet of Comparative Example 1 is as follows:

[0211] Aluminum foil with a thickness of 12 μm was used as the positive electrode current collector.

[0212] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in an appropriate amount of solvent N-methylpyrrolidone NMP in a weight ratio of 97.5:1.4:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is evenly coated on the surface of the positive electrode collector aluminum foil, and after drying and cold pressing, a positive electrode sheet containing a positive electrode active material layer is obtained. The positive electrode sheet includes a positive electrode active material layer, a positive electrode collector and a positive electrode active material layer arranged in sequence along the thickness direction. The width of the positive electrode active material layer is 180 mm, the thickness is 130 μm, and the coating weight is 200 g / m 2 .

[0213] The preparation method of the negative electrode sheet is as follows:

[0214] A copper foil with a thickness of 8 μm was used as the negative electrode current collector.

[0215] The negative electrode active material graphite (artificial graphite 95% and natural graphite 5%), the binder styrene-butadiene rubber (SBR), the thickener sodium carboxymethyl cellulose (CMC-Na), and the conductive agent carbon black (Super P) are fully stirred and mixed in an appropriate amount of solvent deionized water at a weight ratio of 96.2:1.8:1.2:0.8 to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on the surface of the negative electrode collector copper foil, and after drying and cold pressing, a negative electrode plate is obtained. The negative electrode plate includes a negative electrode active material layer, a negative electrode collector and a negative electrode active material layer arranged in sequence along the thickness direction. The negative electrode active material layer has a width of 190 mm and a thickness of 150 μm, and a coating weight of 130 g / m 2 .

[0216] Example 2

[0217] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, the negative electrode of Example 2 was not coated. The preparation method was as follows:

[0218] A copper foil with a thickness of 8 μm was used as the negative electrode current collector.

[0219] The negative electrode active material graphite (95% artificial graphite and 5% natural graphite), binder styrene-butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC-Na), and conductive agent carbon black (Super P) are fully stirred and mixed in an appropriate amount of solvent deionized water in a weight ratio of 96.2:1.8:1.2:0.8 to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet is obtained. The negative electrode sheet includes a negative electrode active material layer, a negative electrode current collector, and a negative electrode active material layer arranged in sequence along the thickness direction.

[0220] Example 3

[0221] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, the positive electrode sheet of Example 3 was not provided with a coating. The preparation method was as follows:

[0222] Aluminum foil with a thickness of 12 μm was used as the positive electrode current collector.

[0223] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in an appropriate amount of solvent N-methylpyrrolidone NMP in a weight ratio of 97.5:1.4:1.1 to form a uniform positive electrode slurry; the positive electrode slurry is evenly coated on the surface of the positive electrode collector aluminum foil, and after drying and cold pressing, a positive electrode sheet containing a positive electrode active material layer is obtained. The positive electrode sheet includes a positive electrode active material layer, a positive electrode collector and a positive electrode active material layer arranged in sequence along the thickness direction.

[0224] Example 4 to Example 6

[0225] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, Examples 4 to 6 adjusted the negative electrode active material and coating size, as follows:

[0226] The negative electrode active material of Example 4 includes 95% artificial graphite and 5% silicon.

[0227] The negative electrode active material of Example 5 includes 98.5% artificial graphite and 1.5% silicon.

[0228] The negative electrode active material of Example 6 includes 90% artificial graphite and 10% natural graphite.

[0229] Example 7

[0230] A lithium-ion battery was prepared using a method similar to that of Example 1. The difference from Example 1 was that the positive electrode active material in Example 7 was adjusted. The positive electrode active material in Example 7 was lithium iron phosphate LiFePO4.

[0231] Example 8 to Example 13

[0232] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, the types of decomposable materials in the coatings were adjusted in Examples 8 to 13.

[0233] Example 14 to Example 19

[0234] A lithium-ion battery was prepared using a method similar to that of Example 1. Unlike Example 1, Examples 14 to 19 adjusted the coating thickness of at least one of the positive electrode sheet and the negative electrode sheet.

[0235] Test section

[0236] 1. Test of the initial capacity of the electrode plate

[0237] The positive electrode sheets prepared in the above embodiments and comparative examples were taken and formed into a counter electrode with a metal lithium sheet. A polyethylene (PE) film was used as an isolation membrane. A few drops of the same electrolyte as the battery cell in Example 1 were dripped into the cells, and the cells were assembled into CR2430 button cells in an argon-protected glove box.

[0238] After the button cell was left to stand for 12 h, it was charged and discharged three times at a constant current of 0.1C / 0.1C at 25°C, and the discharge capacity was recorded. The third discharge capacity was taken as the initial capacity value.

[0239] Correspondingly, the initial gram capacity of the negative electrode active material can also be calculated according to the above method.

[0240] 2. Test method for cycle residual capacity and retention rate

[0241] The lithium-ion batteries prepared in the above examples and comparative examples were tested with a three-piece aluminum plate fixture and a sensor, with an initial fixture force of 3000N. A 1C / 1C cycle retention rate test was performed using a constant temperature chamber at 25°C, and the expansion force data was recorded in real time until 3000 cycles, and the capacity retention rate was recorded.

[0242] 3. Electrode plate interface state

[0243] The lithium-ion batteries prepared in the above examples and comparative examples were subjected to three charge-discharge activation tests at 0.5C / 0.5C, followed by a 2-hour rest period. The batteries were then subjected to three charge-discharge cycles at 2C / 0.5C, and disassembled after full charge. If the interface had different color regions, such as off-white, the off-white region was considered to be a lithium deposition region, while no obvious off-white region indicated no lithium deposition.

[0244] Test results

[0245] The test results are shown in Table 1 and Table 2.

[0246] Table 1

[0247] Table 2

[0248] It can be seen from Table 1 and Table 2 that during the cyclic charge and discharge process of the lithium-ion battery of Comparative Example 1, the volume expansion of the electrode plate is large, which may cause the electrolyte to be squeezed out, resulting in poor cycle performance and easy precipitation of lithium dendrites.

[0249] Compared to Comparative Example 1, the present embodiment of the present application includes a coating on both the positive and negative electrode sheets. During the charge and discharge cycle of the lithium-ion battery, the decomposable material in the coating can decompose, causing the active material layer corresponding to the decomposable material to sag, thereby reducing the expansion rate of the electrode sheet and improving the cycle performance of the lithium-ion battery. It can also reduce the risk of lithium dendrite precipitation and improve the reliability of the lithium-ion battery. Moreover, the coating provided in the present embodiment of the application does not substantially reduce the initial capacity of the lithium-ion battery, and if the coating contains a lithium-supplementing material, it may also have the function of increasing the initial capacity.

[0250] Through experiments, it was found that only providing a coating in the positive electrode sheet or the negative electrode sheet can also improve the cycle performance and reliability of lithium-ion batteries to a certain extent. The coating is suitable for negative electrode active material systems of different materials (corresponding to different expansion rates), and positive electrode active material systems of different materials (corresponding to different expansion rates). The coating size specifications (such as thickness and / or width) can be adjusted to suit different material systems. And through test examples, it was found that when the ratio of the coating weight of the active material layer to the coating weight of the coating is 5.2 to 200; when it is optionally 6.5 to 100, the effect of improving the cycle performance of the lithium-ion battery is better; when the coating weight C2 of the coating satisfies: 2g / m 2 ≤C2≤20g / m 2 ; Optional 5g / m 2 ≤C2≤20g / m 2 Under these circumstances, the effect of improving the cycle performance of lithium-ion batteries is better.

[0251] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions, and modifications may be made to the embodiments without departing from the spirit, principles, and scope of the present application.

Claims

1. An electrode plate of a battery cell, comprising: current collector; a coating disposed on at least one surface of the current collector, the coating comprising at least one coating region, the coating region comprising a decomposable material, the decomposable material being configured to decompose in at least one of charging and discharging of the battery cell, the decomposable material comprising at least one of a lithium replenishing material and a pore-forming material, the lithium replenishing material comprising a compound containing lithium ions; and The active material layer is disposed on at least one surface of the current collector and covers the coating layer.

2. The electrode plate according to claim 1, wherein: The lithium supplement material includes one or more of lithium nitride, lithium oxide, lithium peroxide, lithium squarate and lithium-rich lithium ferrite Li5FeO4.

3. The electrode plate according to claim 1 or 2, wherein: The pore-forming material includes one or more of carbonate, oxalate and metal oxide.

4. The electrode plate according to claim 3, wherein: The carbonate comprises one or more of ammonium carbonate, ammonium bicarbonate and sodium bicarbonate; and / or The oxalate comprises one or more of ammonium oxalate, sodium oxalate and ammonium hydrogen oxalate; and / or The metal oxide includes one or more of zinc oxide, magnesium oxide and aluminum oxide.

5. The electrode sheet according to any one of claims 1 to 4, wherein: The ratio of the coating weight of the active material layer to the coating weight of the coating layer is 5.2 to 200.

6. The electrode plate according to claim 5, wherein: The ratio of the coating weight of the active material layer to the coating weight of the coating layer is 6.5 to 100.

7. The electrode sheet according to any one of claims 1 to 6, wherein: The coating weight C1 of the active material layer satisfies: 65 g / m 2 ≤C1≤300g / m 2 ; and / or The coating weight C2 of the coating satisfies: 2g / m 2 ≤C2≤20g / m 2 .

8. The electrode sheet according to any one of claims 1 to 7, wherein: The ratio of the thickness of the coating layer to the thickness of the active material layer is 0.008 to 0.

200.

9. The electrode plate according to claim 8, wherein: The ratio of the thickness of the coating layer to the thickness of the active material layer is 0.015 to 0.

154.

10. The electrode plate according to claim 8 or 9, wherein: The coating has a thickness of 1 μm to 20 μm; or The active material layer has a thickness of 80 μm to 300 μm.

11. The electrode sheet according to any one of claims 1 to 10, wherein: The ratio of the width of the coating area to the width of the current collector is Y, and 0.05≤Y≤0.

50.

12. The electrode sheet according to any one of claims 1 to 11, wherein: The expansion rate of the electrode plate is Z, the ratio of the width of the coating area to the width of the current collector is Y, The electrode plate satisfies at least one of the following conditions: (1)Z<20%; 0.10≤Y≤0.50; (2) 20% ≤ Z < 25%; 0.13 ≤ Y ≤ 0.50; (3) 25% ≤ Z < 30%; 0.15 ≤ Y ≤ 0.50; (4) 30%≤Z; 0.30≤Y≤0.

50.

13. The electrode plate according to claim 12, wherein: The electrode plate satisfies at least one of the following conditions: (1)Z<20%; 0.10≤Y≤0.15; (2) 20% ≤ Z < 25%; 0.13 ≤ Y ≤ 0.20; (3) 25% ≤ Z < 30%; 0.15 ≤ Y ≤ 0.30; (4) 30%≤Z; 0.33≤Y≤0.

50.

14. The electrode sheet according to any one of claims 1 to 13, wherein: The coating layer includes a plurality of coating regions, and the plurality of coating regions are arranged at intervals on the surface of the current collector and are located between the current collector and the active material layer.

15. The electrode sheet according to any one of claims 1 to 14, wherein: The coating is disposed on two surfaces of the current collector facing each other.

16. A battery cell comprising the electrode sheet according to any one of claims 1 to 15. The battery cell according to claim 16 , wherein the electrode sheet comprises a positive electrode sheet. The battery cell according to claim 16 , wherein the electrode sheet comprises a negative electrode sheet.

19. A battery comprising the battery cell according to any one of claims 16 to 18.

20. An electrical device comprising the battery according to claim 19.

Citation Information

Patent Citations

  • Positive electrode and preparation method therefor, and lithium secondary battery

    CN105702913A

  • Lithium supplement safety coating, positive pole piece and lithium ion battery

    CN114335420A

  • Current collector with pore-forming functional coating, pole piece and lithium ion battery

    CN114464816A

  • Positive plate, secondary battery, battery module, battery pack and electric device

    CN115842097A

  • Lithium supplement positive electrode, preparation method thereof and lithium ion secondary battery

    CN116154100A