3D printing method and device for controlling specific orientation of crystal, and 3D printing control system

By setting anisotropic regions of grain structure during the 3D printing process and using different scanning parameters to control the scanning mode of the laser beam, columnar crystals are formed, solving the problem of anisotropy control of parts in the prior art and improving the mechanical properties of parts in a specific direction.

WO2024244577A1PCT designated stage expired Publication Date: 2024-12-05AIXWAY3D (JIANGSU) CO LTD

Patent Information

Application Number
PCT/CN2024/080035
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-03-05
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing 3D printing technology has difficulty effectively controlling the anisotropy of parts without adding post-processing procedures, resulting in the mechanical properties of parts in a certain direction failing to meet actual requirements.

Method used

By setting an anisotropic grain structure region in the laser scanning path and using different scanning parameters to perform different types of scanning in the pass scanning region and the anisotropic grain structure region, the growth of the crystal structure in the xy plane and z-axis direction of the laser beam is controlled to form columnar crystals and improve the mechanical properties of the parts.

Benefits of technology

It enables efficient, personalized, and autonomous construction of parts during the 3D printing process, improves the mechanical properties of the parts, and achieves precise control over the component materials without adding post-processing procedures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024080035_05122024_PF_FP_ABST
    Figure CN2024080035_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present invention are a 3D printing method and device for controlling the specific orientation of a crystal, and a 3D printing control system. The method comprises: providing a point exposure area in a laser scanning path, so as to divide the laser scanning path into a pass scanning area and the point exposure area; controlling a laser beam to perform continuous pass scanning in an x-y plane on each layer of material corresponding to the pass scanning area, so as to construct a part main body; and controlling the laser beam to perform continuous exposure on each layer of material corresponding to the point exposure area, so as to form, in the point exposure area, a columnar crystal which grows along a z axis. By means of providing a separate exposure area, the orientation growth of crystal grains in an x-y plane during a conventional pass scanning process is blocked, such that the growth mode of the crystal grains is changed, and a micro-structure, which facilitates an improvement in the strength of the part, is provided in a specific area inside the part.
Need to check novelty before this filing date? Find Prior Art

Description

3D printing method, control system and equipment for controlling specific crystal orientation Related applications

[0001] This application claims priority to patent application 202310613608.0 filed with the China Patent Office on May 29, 2023, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present invention relates to the field of 3D printing, and in particular to a 3D printing method, a control system and equipment thereof for controlling a specific crystal orientation. Background Art

[0003] When 3D printing parts, the component is often planed into several two-dimensional structures, which are then printed layer by layer to form the final part. In particular, powder laying and sintering / melting technology involves laying down a layer of powder, then selectively sintering / melting the powder layer using a heat source (usually a laser), thereby constructing the part's structure within that layer. Layer by layer, followed by sintering / melting, the part is finally constructed.

[0004] When 3D printing parts, the layer-by-layer processing from point to line and then from line to surface often results in anisotropic properties. This anisotropy often does not align with the desired performance in all directions. To address this, existing technologies often employ post-processing to control grain orientation, thereby optimizing mechanical properties in specific directions. However, this approach increases post-processing steps and makes it difficult to achieve customized, customized mechanical properties in specific directions.

[0005] Therefore, how to effectively control the anisotropy of parts during the 3D printing process and use anisotropy to improve the performance of components is an important part of 3D printing process development. Summary of the Invention

[0006] In order to achieve excellent performance of parts in a specific direction and meet the requirements for mechanical properties of parts in a certain direction in actual use, one aspect of the present invention provides a 3D printing method, including: setting a grain structure anisotropic region in a laser scanning path to divide the laser scanning path into a pass scanning region and the grain structure anisotropic region; controlling the laser beam to use a first scanning parameter to perform continuous pass scanning in the xy plane on each layer of material corresponding to the pass scanning region to construct the part body; controlling the laser beam to use a second scanning parameter to perform exposure scanning on each layer of material corresponding to the grain structure anisotropic region to form a crystal structure with a grain orientation different from that of the pass scanning region in the grain structure anisotropic region; the combination of the part body and the crystal structure of the grain structure anisotropic region constitutes the final formed part.

[0007] Preferably, the laser beam is controlled to use a second scanning parameter to perform continuous exposure on each layer of material corresponding to the anisotropic region of the grain structure, including: crystallization: controlling the time parameter in the second scanning parameter to scan and expose on any layer of material corresponding to the anisotropic region of the grain structure, so that an exposure molten pool is generated in the anisotropic region of the grain structure, and the solidification process of the static molten pool is controlled by controlling the exposure time of the laser beam to form grains after solidification; and crystallization layer by layer to form a crystal structure with a grain orientation different from that of the grain orientation in the scanning area.

[0008] Preferably, before crystallization, the process includes: performing scanning path planning on the part, determining the pass scanning path and the scanning path of the grain structure anisotropic region according to the path planning, so that when the dynamic molten pool formed by the pass scanning moves to the grain structure anisotropic region, the output of the laser beam is interrupted, and when the laser beam is controlled to pass over the grain structure anisotropic region to re-enter the pass scanning region, the output of the laser beam is restored; and when it is determined that all scans of the current layer corresponding to the pass scanning region are completed, crystallization is entered.

[0009] Preferably, controlling the laser beam to perform scanning exposure on each layer of material corresponding to the anisotropic region of the grain structure includes: setting the offset amount and overlap rate of the anisotropic region of the grain structure on each layer of material; controlling the laser beam to perform scanning exposure after offset and overlap on each layer of material according to the offset amount and overlap rate, so as to form a crystal structure grown according to a preset angle and position in the point exposure area.

[0010] Preferably, the calculation formula of the offset is expressed as: Offset=tan(θ)*LayerThickness; wherein θ is the angle of the crystal structure, and LayerThickness is the thickness of each layer of powder; the calculation formula of the overlap rate is expressed as: Overlap=(Length-Offset) / Length*100%; wherein Length is the length of the crystal structure in each layer.

[0011] Preferably, the method includes: identifying a continuous z-axis segment based on a three-dimensional model of the part; setting a corresponding target position of the crystal structure based on the identified continuous z-axis segment; and setting a corresponding anisotropic region of the grain structure based on the set target position of the crystal structure.

[0012] Preferably, the first scanning parameter and the second scanning parameter are respectively executed by different laser beams, wherein one laser beam is used to perform continuous pass scanning in the xy plane on each layer of material corresponding to the pass scanning area using the first scanning parameter, and the other laser beam is used to perform scanning exposure on each layer of material corresponding to the point exposure area using the second scanning parameter.

[0013] One aspect of the present invention provides a 3D printing control system, which is configured as the aforementioned method.

[0014] One aspect of the present invention provides a 3D printing device, comprising: a mechanical unit; an optical path unit; and the aforementioned control system.

[0015] Preferably, the optical path unit includes: a first laser for outputting a laser beam for performing continuous scanning in the xy plane on each layer of material corresponding to the layer scanning area; and a second laser for outputting a laser beam for performing exposure scanning on each layer of material corresponding to the anisotropic grain structure area.

[0016] The present invention can achieve effective control of the anisotropy of parts during the 3D printing process and improve the component performance of the parts without adding post-processing procedures. Specifically, the method of the present invention controls the laser beam based on different scanning parameters to perform different processing operations on the materials corresponding to different areas by setting anisotropic grain structure areas and pass scanning areas, thereby achieving the combined construction of the part body and crystal structure, thereby improving the mechanical properties of the part. The improvement in its mechanical properties is reflected in the fact that by setting anisotropic grain structure areas, the oriented growth of grains in the xy plane during the traditional pass scanning process is blocked, the growth mode of the grain structure is changed, and a microstructure that is conducive to its strength improvement is set in a specific area inside the part.

[0017] In addition, during the crystallization process, the solidification process of the static molten pool is adjusted by controlling the output time of the laser beam, and the grain structure orientation is further controlled, thereby achieving fine control of the component material.

[0018] Therefore, the present invention can achieve efficient, personalized and autonomous part construction in the 3D printing process, improve the mechanical properties of the parts, and achieve fine control of the construction materials without adding post-processing procedures.

[0019] The present invention can achieve thermal orientation of grain structure at different angles on the z-axis by setting the offset and overlap rate between adjacent layers, thereby achieving growth of grain structure along a specific direction and controlling the mechanical properties of the component in a specific direction.

[0020] The present invention can print a crystal structure growing along the z-axis in a part with an irregular shape / hollow segment, thereby enhancing the strength and stability of the part. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] FIG1 shows a microstructure image of an existing 3D printed part in the xy plane;

[0022] FIG2 is a schematic diagram showing a flow chart of a 3D printing method provided by one embodiment of the present invention;

[0023] Figures 3, 4, and 5 are schematic diagrams of the laser scanning process according to one embodiment of the present invention;

[0024] FIG6 is a schematic diagram showing a model of a cylindrical component provided by one embodiment of the present invention;

[0025] FIG7 is a schematic diagram of a cross section AA of a slice of the cylindrical component in FIG6 under the conventional scanning method;

[0026] FIG8 is a schematic diagram of a cross section AA of a slice of a cylindrical component in a scanning mode according to one embodiment of the present invention;

[0027] FIG9 is a schematic diagram showing a model of columnar crystals formed in a cylindrical member;

[0028] FIG10 is a schematic diagram showing two lasers scanning a material layer according to one embodiment of the present invention;

[0029] FIG11 is a schematic diagram of a crystal preparation process according to one embodiment of the present invention;

[0030] FIG12 is a schematic diagram showing a cross-sectional layer and the next cross-sectional layer in a cylindrical component provided by one embodiment of the present invention;

[0031] FIG13 is a schematic diagram showing a model of columnar crystals grown along a specific direction in a cylindrical component according to one embodiment of the present invention;

[0032] FIG14 is a schematic diagram showing a process for constructing columnar crystals in a part with an irregular shape or hollowed-out sections according to one embodiment of the present invention;

[0033] FIG15 is a schematic diagram showing a model for constructing columnar crystals in a part with an irregular shape / hollow section according to one embodiment of the present invention;

[0034] FIG16 is a schematic structural diagram of a 3D printing device provided in one embodiment of the present invention. DETAILED DESCRIPTION

[0035] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions.

[0036] One aspect of the present invention provides a 3D printing device. The 3D printing device described herein preferably belongs to the 3D printing category that uses a laser beam or electron beam as an energy source. 3D printing technologies that use laser beams or electron beams as an energy source include, but are not limited to, selective laser sintering (SLS), selective laser melting (SLM), and electron beam melting (EBM). These printing technologies all use a laser beam or electron beam as an energy source, focusing energy on the material surface to melt it and then build up layers of material to form 3D printed parts. These devices are suitable for manufacturing high-density, high-precision, and high-strength metal parts and have found widespread application in industries such as aerospace, medical devices, automobiles, and shipbuilding. In summary, the basic principle of the 3D printing device involved is to use a computer to slice a 3D model of a part into a series of "slices" of varying thicknesses. Each layer is then fabricated from the bottom up by the device, and then bonded and stacked layer by layer to form a three-dimensional solid part.

[0037] Referring to FIG. 16 , in some embodiments, the 3D printing device is composed of at least a mechanical unit 10 , an optical path unit 20 , and a control system.

[0038] (Mechanical unit 10)

[0039] The mechanical unit primarily consists of a powder spreading roller 11, powder supply bins 12 and 13, a build chamber 14 (with a build platform 15), and auxiliary equipment. The powder supply bins 12 and 13 store and provide powder for 3D printing and are driven up and down by powder supply elevators 121 and 131. The powder spreading roller 11 is a rotating drum that spreads powder from the powder supply bins 12 and 13 onto the build platform 15 of the build chamber 14. The powder spreading roller 11 is typically made of metal or plastic, and its surface often features fine grooves or serrations to evenly compress and spread the powder, thereby evenly depositing it on the build platform 15. The build chamber 14 is used for part construction, where the final build of the part is completed. The distance the build chamber 14 descends each time is the layer thickness. After part construction is complete, the build chamber 14 rises to facilitate part removal and prepare for the next build. The build chamber 14 is raised and lowered by the build elevator 141. During the part construction process, powder is deposited layer by layer on top of the build chamber 14, also known as the build platform 15, forming a powder bed. Auxiliary equipment (not shown), such as a powder recovery system, powder handling equipment, and a gas shielding system, is used to recover and process excess metal powder and protect the metal powder from external factors such as oxidation during the printing process.

[0040] (Optical path unit 20)

[0041] The optical path unit 20 consists of a laser, a galvanometer, and a focusing lens. The laser is the core component of the optical path unit 20. It generates a laser beam and is usually a high-power, high-energy-density light source. It emits a beam to the galvanometer assembly to activate the printing material and melt or sinter it. For example, a CO2 laser or a fiber laser is usually used as an energy source. The galvanometer is a key component in the optical path unit 20 and is usually composed of two coplanar reflectors. The galvanometer can change the propagation direction and angle of the laser beam so that it can accurately irradiate the printing material and control the printing speed and shape. The focusing lens is an optical element, usually made of high-quality optical glass with high transparency and optical performance. It can minimize optical loss and scattering when the laser beam passes through. It combines the functions of focusing and lens. Unlike ordinary lenses, the main function of the focusing lens is to accurately focus the laser beam on the printing material to control the energy density and focal length of the laser, so that the printing material can be melted or sintered in a specific area. In addition to the above main components, the optical path unit 20 may also include other optical elements, such as optical fibers, reflectors, filters, etc., for optimizing parameters such as the quality, power, and color of the laser beam.

[0042] (Control System)

[0043] The control system is the core of the entire printing process, including printing parameter setting, laser scanning path planning, and build platform motion control. The control system typically consists of two parts: an optical control system and a mechanical control system. Specifically, within the control logic, the control system controls both the mechanical unit 10 and the optical unit 20.

[0044] In a specific spatial arrangement, the optical path unit 20 can be arranged above the mechanical unit 10, or it can be arranged based on the core invention points taught in this application according to the actual structural design.

[0045] In the existing 3D printing scanning process, the laser beam irradiates the material, forming the spot from a point to a line, and then from a line to a surface. This forming method often forms columnar crystals composed of grains in the direction of the molten pool's movement due to thermal factors, which degrades the part's strength in the z-axis. If the part requires higher strength in the z-axis than in the xy-axis, further heat treatment is required to change the part's material microstructure. For example, Figure 1 shows the microstructure of a 3D-printed part in the xy plane, showing that the microstructure of the part surface tends to grow along the xy plane.

[0046] To put it another way, during the metal powder 3D printing process, due to the point-by-line forming method, the internal microstructure of the component formed by scanning the current layer often exhibits a specific, consistent grain orientation due to the regular thermal gradient. This consistent grain orientation often exhibits better mechanical properties in a certain direction, which is the anisotropy of the material. If the direction of better mechanical properties coincides with the actual demand, the demand can be met. If the direction of better mechanical properties coincides with the actual demand, the material's performance cannot be fully utilized. Therefore, in practice, especially in 3D printed parts, it is desirable to be able to manually adjust the orientation of the material's internal grains to meet performance requirements.

[0047] Therefore, one aspect of the present invention proposes a 3D printing method, which uses point scanning to preferentially form a crystal structure with a specific orientation in the direction required by the part, thereby improving the overall performance of the part.

[0048] Preferably, during actual implementation, the 3D printing method of the present invention is executed by the aforementioned control system. For example, the method can be designed into a computer-readable language format (e.g., a computer program) and stored in a memory, so that it can be called and executed by the control system during the 3D printing process.

[0049] The 3D printing method of the present invention changes the scanning mode of conventional laser forming, and realizes the control of the microstructure in the tiny area of ​​the part by adding point exposure in the grain structure anisotropic area. Specifically, the composition of the 3D printing method of the present invention includes: setting the grain structure anisotropic area in the laser scanning path to divide the laser scanning path into the pass scanning area and the grain structure anisotropic area; controlling the laser beam to use the first scanning parameter to perform continuous pass scanning in the xy plane on each layer of material corresponding to the pass scanning area to construct the part body; and controlling the laser beam to use the second scanning parameter to perform exposure scanning on each layer of material corresponding to the grain structure anisotropic area to form a crystal structure with a grain orientation different from that of the grain in the pass scanning area in the grain structure anisotropic area; the part body is combined with the crystal structure of the grain structure anisotropic area to form the final formed part.

[0050] Among them, point exposure is preferably used for exposure scanning in the anisotropic grain structure area, so the anisotropic grain structure area can be not limited as a point exposure area. The crystal structure of the anisotropic grain structure area is preferably presented in a columnar form, that is, columnar crystals are formed as a form of the crystal structure.

[0051] The grain structure in the pass scanning area tends to grow along the xy plane, while the grain structure in the anisotropic grain structure area provided in the present application is controlled to tend to grow along the z axis, for example.

[0052] More specifically, referring to FIG2 , the 3D printing method of the present invention is composed of the following steps: S101. Setting a point exposure area in a laser scanning path to divide the laser scanning path into a pass scanning area and a point exposure area; S102. Controlling the laser beam to use a first scanning parameter to perform continuous pass scanning in the xy plane on each layer of material corresponding to the pass scanning area to construct the part body; and S103. Controlling the laser beam to use a second scanning parameter to perform continuous exposure on each layer of material corresponding to the point exposure area to form columnar crystals growing along the z-axis in the point exposure area; wherein the combination of the part body and the columnar crystals constitutes the final formed part.

[0053] It should be understood that the step numbers provided here are used as identifiers of the corresponding steps and do not limit the order of the steps in the specific implementation process. For example, the execution order of S102 can be before / after S103, or can be performed synchronously or semi-synchronously with S103.

[0054] Before 3D printing, the first step is to select the appropriate material based on the desired part requirements, such as metal powder materials like NiTi alloy and stainless steel. Next, design the part model and convert it into a printable file, such as an STL file. The STL file is then imported into the 3D printing software, and the printing parameters are set based on the desired part size, layer thickness, and print speed. Furthermore, appropriate laser scanning parameters, such as laser power, scan speed, laser focal length, and a pre-set scan path, are selected based on the desired part's geometry and material properties.

[0055] In some embodiments, the present invention sets the size and shape of the spot exposure area within the laser scanning path. Typically, the size and shape of the spot exposure area need to be determined based on the characteristics of the printing material and the required performance of the part. For example, the spot exposure area can be set to a circular or square shape by controlling the laser beam's scanning range and scanning speed. In some 3D printing devices, the shape of the spot exposure area can also be adjusted by adjusting the laser beam's focus and offset. It should be noted that the size and shape of the spot exposure area have a significant impact on both print quality and printing speed. A smaller spot exposure area can improve printing accuracy but reduce printing speed. Conversely, a larger spot exposure area can increase printing speed but reduce printing accuracy. Therefore, in actual operation, adjustments need to be made based on specific needs. The diameter / length of the spot exposure area is typically set to 30μm-3mm, and in the present invention, it is preferably set to 45-100μm.

[0056] In some embodiments, the present invention sets the position of the point exposure area in the laser scanning path. The position of the point exposure area can be automatically generated by the slicing software or can be set manually. In the former case, for example, in the case where multiple point exposure areas may be distributed on the cross section of a part, the slicing software can automatically calculate the position of the appropriate point exposure area based on the geometric shape and / or support structure of each layer, and add it to the laser scanning path to ensure that each point exposure area can be fully exposed. This automatic calculation method can simplify the printing process and improve the efficiency and accuracy of printing. In the latter case, for example, the function of manually setting the point exposure area can be provided to the user in the visual interface of the slicing software to meet the need of manually setting the point exposure area.

[0057] It should be understood that after removing the designated spot exposure area from the cross-section of a part, the remaining area can be set as the pass scanning area. Since the laser beam scans along a pre-set laser scanning path, the laser scanning path after removing the spot exposure area is set as the pass scanning area. In other words, only the spot exposure area needs to be set within the laser scanning path; the remaining area is automatically classified as the pass scanning area. This can be understood as dividing the laser scanning path into the pass scanning area and the spot exposure area by setting the spot exposure area within the laser scanning path.

[0058] After the point exposure area is set, the part construction work can be carried out, which includes executing the above-mentioned S102 and S103.

[0059] More specifically, S103 is crystallization: controlling the time parameter in the second scanning parameter to scan and expose on any layer of material corresponding to the point exposure area, so that an exposure molten pool is generated in the point exposure area, and controlling the solidification process of the exposure molten pool by controlling the exposure time of the laser beam to form grains after solidification; and crystallization layer by layer to form columnar crystals.

[0060] After entering the crystallization stage, the laser scanning path needs to be adjusted to ensure continuous laser output on any layer of material corresponding to the spot exposure area, generating a static exposure pool in that area. This static exposure pool refers to the process of scanning the material during the spot exposure. This means that during the spot exposure scan, the relative movement speed of the melt pool is much slower than the speed of the pass scan, resulting in a microstructure with a different grain orientation in the spot exposure area than in the pass scan area. Specifically, the corresponding laser scanning path needs to be calculated based on the position and shape of the spot exposure area and input into the 3D printing device's control system. Furthermore, the laser beam spot needs to be aligned with the spot exposure area of ​​the current layer, and the laser beam output power and scanning speed are controlled to ensure continuous laser output in the spot exposure area, generating a static molten pool in the spot exposure area. After the static molten pool is generated in the spot exposure area, the laser beam exposure time needs to be controlled to control the solidification process of the static molten pool. For example, by controlling the laser beam output power and scanning speed, the solidification rate of the static molten pool can be controlled to form grains after solidification. The above crystallization process is repeated for each layer of material. When controlling the laser beam exposure time, it is also necessary to determine the optimal exposure time for each exposure area based on the material characteristics and printing parameters to ensure the quality and accuracy of grain formation. Typically, adjusting the exposure time requires multiple trials and optimizations to find the optimal parameter combination.

[0061] Ultimately, during the layer-by-layer crystallization process, the grains grow along the direction (z-axis) perpendicular to the manufacturing direction (xy-axis) and form columnar crystals. That is, after the crystallization of all layers is completed, a series of columnar crystals extending along the z-axis will be formed within the part.

[0062] Among them, the continuous scanning of the pass scanning area and the continuous exposure of the point exposure area are both controlled by the laser beam, but they are different:

[0063] Continuous pass scanning is the process of scanning and moving the laser beam on the powder bed. During this process, the laser beam scans along a preset path and moves the light spot to the desired position to build the part body and control the quality and accuracy of the part body surface.

[0064] Laser exposure refers to the process of directly irradiating a material with a laser beam. During this process, the laser beam irradiates the material surface, causing a physical or chemical reaction. For example, a laser beam can directly irradiate powder, causing it to melt or sinter into a solid component. The laser exposure process controls the morphology and properties of the component by controlling parameters such as laser power, exposure time, and exposure position.

[0065] Referring to FIG3 , in one example performed according to the working sequence, the 3D printing method of the present invention comprises the following steps:

[0066] S201. Set the laser scanning path;

[0067] S202. Setting a point exposure area in the laser scanning path;

[0068] S203. Control the laser beam to perform continuous scans on the xy plane on the corresponding layer of material in the scan area;

[0069] The control system controls the laser beam to perform continuous passes in the xy plane on the corresponding layer of material in the pass scanning area to process the material. At the same time, the position information of the laser beam at each time point is recorded to facilitate the subsequent determination of the position of the dynamic melt pool.

[0070] During this process, the laser beam is focused into a spot to irradiate the corresponding material in the pass scanning area. After the laser beam hits the material surface, it causes the material surface to melt to form a molten pool; then it moves along the xy axis on the forming platform (current powder layer) to form a dynamic molten pool, which sequentially melts and solidifies the current layer of material corresponding to the pass scanning area.

[0071] S204. Obtaining the real-time position of the dynamic molten pool formed on the material corresponding to the light spot in the pass scanning area;

[0072] The control system is used to obtain the real-time position of the dynamic molten pool formed by the laser beam spot on the material corresponding to the pass scanning area, so as to subsequently determine whether it moves to the point exposure area.

[0073] The diameter of the laser spot typically depends on factors such as the optical design of the laser system, the laser wavelength, and the parameters of the focusing lens. Generally speaking, the diameter of the laser spot can range from a few microns to tens of millimeters. This diameter can, to a certain extent, control the melting and solidification processes of the printing material, thereby affecting print quality. In the present invention, the diameter of the laser spot is preferably set at 30 μm.

[0074] S205. Determine whether the dynamic molten pool moves to the point exposure area; if so, execute S206;

[0075] The control system analyzes and compares the dynamic molten pool position information to determine whether the dynamic molten pool has moved to the set point exposure area. If so, execute S206.

[0076] S206. Interrupt laser output;

[0077] S207. Control the laser beam to cross the point exposure area to re-enter the pass scanning area, return to execute S203, and synchronously execute S208;

[0078] The control system interrupts the laser beam output, causing it to stop irradiating. During the 3D printing process, the movement of the laser beam is controlled by the control system. When it is necessary to interrupt the laser beam output in a certain area, the control system sends a command to the laser to stop output and simultaneously moves the laser beam to the new target position. It should be noted that even if the laser output stops, the control system can still control the position movement of the laser beam. This is because the position control of the laser beam and the output of the laser are controlled separately. The lasers used in 3D printers are typically gas lasers or semiconductor lasers. Their output is controlled by a controller and circuit, while the position of the laser beam is constrained by the optical path unit.

[0079] The control system is used to control the laser beam to pass through the point exposure area to re-enter the pass scanning area, and return to execute S203 to continue processing the material, and simultaneously execute S208.

[0080] S208. Determine whether all scans of the pass scanning area corresponding to the current layer are completed; if so, execute S209;

[0081] S209. Crystal preparation.

[0082] During the 3D printing process, the control system will determine whether the entire scan of the current layer corresponding to the pass scanning area has been completed to determine whether laser exposure needs to continue, that is, return to each point exposure area to continue exposure (crystal preparation) for the point exposure area.

[0083] If the entire scan of the current layer (including continuous scans and continuous exposure of the spot exposure area) is complete, the following steps are performed: Determine whether the entire model has been scanned. If so, the entire 3D printing process ends. If not, scan the next layer. Repeat steps S201-S209 until the entire model is scanned. During S208, the control system monitors various parameters during the laser scanning process in real time to ensure that the scanning quality and speed of each layer are controlled and optimized. Furthermore, the control system records and processes data to facilitate subsequent process analysis and optimization.

[0084] Referring to FIG4 , in one example performed according to the working sequence, the 3D printing method of the present invention comprises the following steps:

[0085] S301. Set the laser scanning path;

[0086] S302. Setting a point exposure area in the laser scanning path;

[0087] S303. Control the laser beam to perform continuous scans on the xy plane on the corresponding layer of material in the scan area;

[0088] S304. Obtaining the real-time position of the dynamic molten pool formed on the material corresponding to the light spot in the pass scanning area;

[0089] S305. Determine whether the dynamic molten pool moves to the point exposure area; if so, execute S306;

[0090] S306. Crystallization;

[0091] S307. Control the laser beam to cross the point exposure area to re-enter the pass scanning area, return to execute S203, and synchronously execute S308;

[0092] S308. Determine whether all scans of the current layer corresponding to the pass scanning area are completed; if so, end the current process.

[0093] The difference between this example and S201-S209 is that in S201-S209, when the laser beam encounters a spot exposure area, it interrupts the laser output and controls the laser beam to continue scanning across the spot exposure area until the continuous scan of the entire layer of the scan area is completed. The laser beam then returns to the spot exposure area and begins spot exposure to form crystals. This means that spot exposure is performed after all scans are completed. In this example, when the laser beam encounters a spot exposure area, it first performs spot exposure on the spot exposure area to form crystals, then moves to the next scan area for continuous scans, and repeats this process until the scan of the entire layer is completed. This means that spot exposure and continuous scans are performed alternately. This scanning method can reduce the distance the laser jumps and improve printing efficiency.

[0094] Therefore, the main difference between the two examples is the order in which spot exposure and pass scanning are performed, resulting in a different printing order for the entire layer. In S201-S209, pass scanning is performed first, followed by spot exposure; in this example, spot exposure and pass scanning are performed alternately.

[0095] Referring to FIG5 , in one example performed according to the working sequence, the 3D printing method of the present invention comprises the following steps:

[0096] S401. Set the laser scanning path;

[0097] S402. Setting a point exposure area in the laser scanning path;

[0098] S403. Control the first laser beam to perform continuous scans in the xy plane on the layer of material corresponding to the scanned area; S413. Control the second laser beam to perform continuous exposure (crystallization) on the layer of material corresponding to the point exposure area; wherein S403 and S413 are performed simultaneously;

[0099] After S403, the process proceeds to S404 to obtain the real-time position of the dynamic molten pool formed by the light spot on the material corresponding to the pass scanning area;

[0100] S405. Determine whether the dynamic molten pool moves to the point exposure area; if so, execute S406;

[0101] S406. Interrupt laser output;

[0102] S407. Control the laser beam to cross the point exposure area to re-enter the pass scanning area, return to execute S403, and synchronously execute S408;

[0103] S408. Determine whether all scans of the current layer corresponding to the pass scanning area are completed; if so, end the process;

[0104] After S413 , the process proceeds to S414 . It is determined whether all exposures of the point exposure area corresponding to the current layer are completed; if so, the process ends.

[0105] This example differs from S201-S209 in that different laser beams are used to control continuous pass scanning and continuous exposure. Specifically, different laser beams control the first and second scanning parameters. One laser beam (the first laser beam) uses the first scanning parameters to perform continuous pass scanning in the xy plane on each layer of material corresponding to the pass scanning area, while the other laser beam (the second laser beam) uses the second scanning parameters to perform exposure scanning on each layer of material corresponding to the point exposure area. This synchronized dual laser beam operation further improves scanning efficiency.

[0106] In some embodiments, as shown in FIG10 , the aforementioned optical path unit 20 has two lasers, namely a first laser 21 and a second laser 22, wherein the first laser 21 is used to output a laser beam for continuous pass scanning in the xy plane on each layer of material corresponding to the pass scanning area; the second laser 22 is used to output a laser beam for continuous exposure on each layer of material corresponding to the point exposure area.

[0107] In order to facilitate a clearer understanding of the present invention, the 3D printing method of the present invention is described in detail below using a cylindrical part as a printing example.

[0108] As shown in Figure 6, the printing goal is to process a cylindrical component and hope that the component has higher mechanical properties in the z-axis direction perpendicular to the radial direction.

[0109] As shown in Figure 7, for section AA of a slice of the cylindrical component in Figure 6, assume the laser scanning path is a1-a26. Traditional 3D printing methods, due to the continuous scanning process in the xy plane, result in a strong grain orientation in the xy plane for the cylindrical component. This grain orientation is detrimental to the strength in the z-axis, which reduces the interlayer bonding strength in the z-axis, resulting in lower tensile strength and yield strength in the z-axis.

[0110] As shown in Figure 8, for section AA of a slice of the cylindrical component in Figure 6, let the laser scanning path be a1-a26. The present invention divides the laser scanning path into a combination of point exposure areas b1-b7 and a pass scanning area by setting point exposure areas b1-b6 within a1-a26. The remaining path of the laser scanning path after deducting point exposure areas b1-b7 constitutes the pass scanning area. Based on this arrangement, the 3D printing method of the present invention changes the pass scanning method used in traditional component forming by setting point exposure areas at preset positions along the scanning path. By controlling the scanning method of the point exposure areas, it is possible to achieve directional growth of the microstructure in this area in the z-axis direction, forming columnar crystals c1-c7 as shown in Figure 9, thereby improving the z-axis strength.

[0111] In one scanning method, a control system controls the laser beam, starting at position a1, to continuously scan the pass scanning area in the xy plane along a scanning path from a1 to a26, completing the entire scan of the current layer within the pass scanning area. During the scanning process, the position of the dynamic molten pool formed by the laser beam spot on the material corresponding to the pass scanning area is determined in real time. Laser output is interrupted when the dynamic molten pool moves to the spot exposure areas b1-b7, and the laser beam is controlled to pass through the spot exposure areas b1-b7 to scan the pass scanning area along the preset scanning path. After completing the entire scan of the current layer within the pass scanning area, the laser beam is then controlled to continuously expose the material corresponding to the spot exposure areas b1-b7 in sequence to form a crystal.

[0112] In one scanning method, a control system controls the laser beam, starting at position a1, to continuously scan the pass scanning area in the xy plane along a scanning path from a1 to a26, completing a complete scan of the current layer within the pass scanning area. During the scanning process, the position of the dynamic melt pool formed by the laser beam spot on the corresponding material in the pass scanning area is determined in real time. When the dynamic melt pool moves to the point exposure area b1-b7, the laser beam is first controlled to continuously expose the point exposure area b1-b7 to form a crystal. After crystal formation is completed, the laser beam is controlled to continue scanning along the preset scanning path. In other words, the current layer is completely scanned by alternating point exposure and pass scanning.

[0113] In one scanning method, the control system controls the laser beam, starting at position a1, to continuously scan the pass scanning area in the xy plane along a scanning path from a1 to a26, completing the entire scan of the current layer in the pass scanning area. During the scanning process, the controller controls the first laser beam to continuously scan the material layer corresponding to the pass scanning area in the xy plane, while simultaneously controlling the second laser beam to continuously expose the material layer corresponding to the spot exposure area.

[0114] Regardless of which of the above scanning methods is used, after completing the entire scan of the current layer (point exposure + pass scanning), the forming platform is controlled to descend a layer thickness, and the powder roller is controlled to lay a new layer of powder on the processed current layer. The equipment is transferred to the next layer for processing, and the scanning is repeated layer by layer until the entire cylindrical component is manufactured. Then, columnar crystals generated along the z-axis are formed in the point exposure area, namely columnar crystals c1-c7 as shown in Figure 9.

[0115] The present invention can achieve effective control of the anisotropy of parts during the 3D printing process and improve the construction performance of parts without adding post-processing procedures. Specifically, the method of the present invention controls the laser beam to perform different processing operations on the materials corresponding to different areas by setting point exposure areas and pass scanning areas, thereby achieving the combined construction of the part body and columnar crystals, thereby improving the mechanical properties of the part. The improvement in its mechanical properties is reflected in the setting of a separate exposure area to block the oriented growth of grains in the xy plane during the traditional pass scanning process, thereby changing the growth mode of the grains and setting a microstructure in a specific area inside the part that is conducive to its strength improvement.

[0116] In addition, during the crystallization process, the solidification process of the static molten pool is adjusted by controlling the output time of the laser beam, and the grain orientation is further controlled, thereby achieving fine control of the construction material.

[0117] Therefore, the present invention can achieve efficient, personalized and autonomous part construction in the 3D printing process, improve the mechanical properties of the parts, and achieve fine control of the construction materials without adding post-processing procedures.

[0118] Referring to Figure 11, in some embodiments, the aforementioned S103 can also be composed of the following steps: S501. Setting the offset and overlap rate of the point exposure area on each layer of material; and S502. Controlling the laser beam to continuously expose after offset and overlap on each layer of material according to the offset and overlap rate, so as to form columnar crystals grown at a predetermined angle and position in the point exposure area.

[0119] In a specific embodiment, a 3D model containing columnar crystals is designed using drawing software. The model should include information such as the shape of the part and the position, shape, and angle of the internal columnar crystals. Then, a corresponding G code is generated based on the designed 3D model. The code contains commands and instructions that the 3D printer needs to execute to control parameters such as the laser scanning path and the height of the printing layer. When writing the G code, it is necessary to take into account information such as the position and angle of the columnar crystals, and set parameters such as the offset and overlap rate of the point exposure area when printing each layer. When continuously exposing the point exposure area, the laser beam is controlled to offset and overlap between different layers according to preset parameters so that the columnar crystals gradually grow according to the predetermined angle and position.

[0120] Each layer of printing requires consideration of parameters such as the offset and overlap of the exposure area, ensuring that the grains gradually grow into columnar crystals at the desired angles and positions. Specifically, the angle and position of the columnar crystals within the component must be determined to determine parameters such as the offset and overlap. These parameters should be selected based on the desired structural strength and mechanical properties to ensure that the printed columnar crystals possess the desired properties.

[0121] Specifically, the offset should be selected according to the position and angle of the columnar crystals and adjusted when printing each layer. If the offset is set incorrectly, the columnar crystals may break or deviate from the expected position. While setting the offset, it is also necessary to set the overlap rate of the point exposure area of ​​each layer to ensure that the columnar crystals between adjacent layers can be properly docked. The overlap rate should be selected according to the position and angle of the columnar crystals and adjusted when printing each layer. If the overlap rate is set incorrectly, the columnar crystals may have defects or gaps. During the printing process, it is also necessary to continuously adjust the parameters to ensure that the columnar crystals gradually grow according to the expected position and angle.

[0122] In one embodiment, the calculation formula of the offset is expressed as:

[0123] Offset=tan(θ)*LayerThickness;

[0124] Where θ is the angle of the columnar crystal, and LayerThickness is the thickness of each layer of powder;

[0125] Offset can be understood as a displacement in the z-axis direction. This offset ensures that the columnar crystals grow in the desired direction within the component. During the printing process, the laser beam's exposure area for each layer is composed of a series of continuous contour lines. These contour lines accumulate in the longitudinal direction, creating a certain degree of error, which can cause the columnar crystals to deviate from the desired direction in the z-axis. To address this issue, the columnar crystals can be fine-tuned in each layer to align with the desired direction, achieving a more precise reinforcement effect.

[0126] In one embodiment, the calculation formula of the overlap ratio is expressed as:

[0127] Overlap=(Length-Offset) / Length*100%;

[0128] Where Length is the length of the columnar crystal in each layer.

[0129] S501 and S502 primarily illustrate how to create a scanning method that forms a specific angle along the z-axis within a component. Figure 12 shows a cross-sectional layer n and the next cross-sectional layer n+1 within a cylindrical component. After completing the scan (spot exposure + pass scanning) of cross-sectional layer n, when scanning the next cross-sectional layer n+1, it is necessary to obtain the offset and overlap ratio of the set spot exposure area, and use this as a basis for controlling the scan of cross-sectional layer n+1. As shown in Figure 13, d1-d3 are columnar crystals constructed within a cylindrical component that grow along a specific direction. By setting the offset and overlap ratio between adjacent layers, thermal orientation of grains at different angles along the z-axis can be achieved, thereby enabling grain growth along a specific direction and controlling the mechanical properties of the component in that specific direction.

[0130] By setting the offset and overlap ratio of each layer of columnar crystals in the printing software, the columnar crystals can be grown along a specific direction within the cylindrical component.

[0131] It should be noted that these parameter examples are only used to illustrate the calculation method of the offset formula and the overlap rate formula. The specific parameter settings should be adjusted and optimized according to the actual situation.

[0132] Referring to FIG14 , in some embodiments, the 3D printing method provided by the present invention may also be composed of the following steps:

[0133] S601. Identify a continuous z-axis segment based on the three-dimensional model of the part; S602. Set the corresponding target position of the columnar crystal based on the identified continuous z-axis segment; and S603. Set the corresponding point exposure area based on the set target position of the columnar crystal.

[0134] First, based on the part's 3D model, the part's z-segments must be determined through calculation and analysis. A continuous z-segment is one without interruptions or missing parts along the z-axis. This can be determined by calculating features such as the model's volume, surface area, and shape. Graphics processing algorithms, such as contour tracing, can also be used to extract the outline of each z-segment. By comparing the distances between adjacent contours, it's possible to determine which contours are continuous, thereby identifying continuous z-segments.

[0135] Secondly, after identifying the continuous z-axis segments, the target positions of the corresponding columnar crystals need to be set according to the preset columnar crystal design requirements. For example, if a columnar crystal is set along the z-axis within a cylindrical component, the offset and overlap ratio of the columnar crystals in each layer can be calculated, and the target position of the columnar crystals in each layer can be calculated based on this.

[0136] Finally, based on the target location of the columnar crystal, a corresponding spot exposure area needs to be set at that location. A spot exposure area is an exposure process performed at a specific location within each layer to achieve a specific shape and structure. During this process, the size, shape, and position of the spot exposure area can be adjusted as needed to ensure the perfect control and realization of the columnar crystal's shape and structure.

[0137] As shown in Figure 15, columns e1-e11 are columnar crystals constructed within a part with an irregular shape or hollow sections. It should be noted that the columnar crystals e1-e11 shown in the figure are only for the purpose of illustrating their distribution along the z-axis within the part and do not represent their actual placement. In reality, the columnar crystals are located within the part and, at micron-scale, are not visible from the outside. This allows columnar crystals to be printed along the z-axis within parts with irregular shapes or hollow sections, thereby enhancing the part's strength and stability.

Claims

1. A 3D printing method, characterized in that: include: Setting a grain structure anisotropic region in a laser scanning path to divide the laser scanning path into a pass scanning region and the grain structure anisotropic region; Controlling the laser beam to perform continuous pass scanning in the xy plane on each layer of material corresponding to the pass scanning area using a first scanning parameter to construct a part body; as well as The laser beam is controlled to use a second scanning parameter to perform exposure scanning on each layer of material corresponding to the grain structure anisotropic region, so as to form a crystal structure in the grain structure anisotropic region that is different from the grain orientation in the pass scanning region; wherein the part body is combined with the crystal structure in the grain structure anisotropic region to form a finally formed part.

2. The 3D printing method according to claim 1, characterized in that: Controlling the laser beam to perform exposure scanning on each layer of material corresponding to the anisotropic region of the grain structure using a second scanning parameter includes: Crystal making: controlling the time parameter in the second scanning parameter to scan and expose on any layer of material corresponding to the anisotropic region of the grain structure, so that an exposure molten pool is generated in the anisotropic region of the grain structure, and controlling the solidification process of the exposure molten pool by controlling the exposure time of the laser beam to form grains after solidification; and The crystal structure is formed layer by layer to form a crystal structure having a grain orientation different from that in the pass scanning area.

3. The 3D printing method according to claim 2, characterized in that: Before crystallization, including: Performing scanning path planning on the part, determining the pass scanning path and the scanning path of the grain structure anisotropic region according to the scanning path planning, so that when the dynamic molten pool formed by the pass scanning moves to the grain structure anisotropic region, the output of the laser beam is interrupted, and when the laser beam is controlled to cross the grain structure anisotropic region to re-enter the pass scanning region, the output of the laser beam is resumed; as well as When it is determined that all scans of the pass scanning area corresponding to the current layer are completed, the crystal making process is started.

4. The 3D printing method according to claim 1, characterized in that: Controlling the laser beam to perform scanning exposure on each layer of material corresponding to the anisotropic region of the grain structure includes: Setting the offset and overlap rate of the anisotropic region of the grain structure on each layer of material; The laser beam is controlled to perform scanning exposure after offset and overlap on each layer of material according to the offset amount and overlap rate, so as to form a crystal structure grown at a preset angle and position in the anisotropic region of the grain structure.

5. The 3D printing method according to claim 4, characterized in that: The calculation formula of the offset is expressed as: Offset=tan(θ)*LayerThickness; Among them, θ is the angle of the crystal structure, and LayerThickness is the thickness of each layer of powder; The calculation formula of the overlap ratio is expressed as: Overlap=(Length-Offset) / Length*100%; Among them, Length is the length of the crystal structure in each layer.

6. The 3D printing method according to claim 1, characterized in that: include: Identify the z-axis segments with continuity based on the three-dimensional model of the part; Setting a target position of the corresponding crystal tissue according to the identified continuous z-axis segment; as well as The corresponding grain structure anisotropic region is set according to the set target position of the crystal structure.

7. The 3D printing method according to claim 1, characterized in that: The first scanning parameter and the second scanning parameter are respectively executed by different laser beams, wherein one laser beam is used to perform continuous pass scanning in the xy plane on each layer of material corresponding to the pass scanning area using the first scanning parameter, and the other laser beam is used to perform scanning exposure on each layer of material corresponding to the grain anisotropic area using the second scanning parameter.

8. A 3D printing control system, characterized in that: The control system is configured to execute the method according to any one of claims 1-7.

9. A 3D printing device, characterized in that: include: Mechanical unit; Optical path unit; as well as Includes the control system described in claim 8.

10. The 3D printing device according to claim 9, characterized in that: The optical path unit comprises: A first laser is used to output a laser beam for performing continuous pass scanning in an xy plane on each layer of material corresponding to the pass scanning area; and The second laser is used to output a laser beam for performing exposure scanning on each layer of material corresponding to the anisotropic region of the grain structure.

Citation Information

Patent Citations

  • Regulation and control method for grain orientation distribution of Inconel 939 nickel-based high-temperature alloy in additive manufacturing

    CN114959332A

  • Additive manufacturing method and apparatus for forming objects from nickel-based superaloy in

    CN115702052A

  • 3D printing method, control system and equipment for controlling specific orientation of crystal

    CN116786842A

  • 3-Dimensional manufacturing method for the metallic materials using 3D printing with controlling the microstructure

    KR1020170068014A

  • Turbine component having multiple controlled metallic grain orientations, apparatus and manufacturing method thereof

    US20180202293A1

Cited By

  • LPBF metal 3D printing method and system based on discrete point dynamic regulation and control

    CN121017575A

  • Preparation method of laser cladding heterostructure stainless steel

    CN121042563A