Prismatic battery and welding method
By directly laser welding the tabs and terminals, combined with ultrasonic pre-welding and laser welding, the problems of low space utilization and thermal runaway risk in square batteries have been solved, achieving higher specific energy and weld strength.
Patent Information
- Application Number
- PCT/CN2024/086980
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2024-04-10
- Publication Date
- 2024-12-05
AI Technical Summary
In existing square batteries, the introduction of auxiliary solder pads and connecting pieces leads to low utilization of internal space, reduced specific energy, and the risk of thermal runaway.
The electrode tabs and poles are directly connected by laser welding, eliminating the need for auxiliary welding plates and connecting plates. A combination of ultrasonic pre-welding and laser welding is used to ensure a firm connection between the electrode tabs and poles.
It improves the internal space utilization and specific energy of square batteries, reduces battery temperature rise, reduces the risk of thermal runaway, and improves the strength of welding and battery yield.
Smart Images

Figure CN2024086980_05122024_PF_FP_ABST
Abstract
Description
Square battery and welding method
[0001] This application claims priority to Chinese patent applications filed with the China Patent Office on June 1, 2023, with application numbers 202310649791.X and 202321394457.6. The entire contents of the above applications are incorporated by reference into this application. Technical Field
[0002] The present application relates to the field of battery technology, and in particular to a square battery and a welding method. Background Art
[0003] In the related art, the core pack and cover plate in a prismatic battery are often connected using a core pack, auxiliary welding tabs, connecting tabs, and cover plate. The auxiliary welding tabs are used to protect the positive and negative electrode tabs on the core pack, which are then welded to the cover plate via the connecting tabs. This welding connection method not only increases the weight of the battery itself and occupies internal battery space, reducing the battery's mass-to-energy ratio and the internal space utilization rate of the prismatic battery, but also, due to the introduction of the auxiliary welding tabs and connecting tabs, the energy inside the core pack must pass through the auxiliary welding tabs and connecting tabs to be output to the charge and discharge ports on the cover plate. In this process, some energy is lost, causing a significant increase in the internal temperature of the battery, which may pose a risk of thermal runaway during long-term use of the battery. Technical issues
[0004] The present application provides a square battery and a welding method, which can improve the internal space utilization and mass-to-energy of the square battery. Technical Solutions
[0005] In a first aspect, an embodiment of the present application provides a square battery, comprising:
[0006] a cover plate, wherein the cover plate is provided with a pole;
[0007] The core package is provided with a pole ear, and the pole ear is directly connected to the pole by laser welding.
[0008] In a second aspect, an embodiment of the present application provides a welding method, comprising:
[0009] Ultrasonic pre-welding the tabs on the core pack according to a first weld print area to form ultrasonic pre-welded tabs, wherein the first weld print area is determined according to the size and shape of the pole;
[0010] Laser welding is performed on the ultrasonically pre-welded tab and the pole according to a second weld print area to complete the connection between the tab and the pole, wherein a ratio of the second weld print area to the first weld print area is less than 1. Beneficial effects
[0011] Beneficial effects of this application:
[0012] In an embodiment of the present application, a square battery includes: a cover plate, which is provided with a pole; a core pack, which is provided with a pole ear, and the pole ear is directly connected to the pole by laser welding, thereby realizing the construction of an energy transmission path of the battery and realizing the charging and discharging function of the core pack. In addition, since the pole ear of the core pack in the square battery is directly connected to the pole of the cover plate, the auxiliary welding piece and the connecting piece are eliminated, which greatly improves the internal space utilization and mass-to-energy of the square battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] FIG1 is a schematic diagram of a square battery provided in an embodiment of the present application;
[0014] FIG2 is a schematic diagram showing the relationship between the collapsed size and the thickness of the core package provided in an embodiment of the present application;
[0015] FIG3 is a schematic flow chart of an embodiment of a welding method provided in an embodiment of the present application;
[0016] FIG4 is a schematic diagram comparing the tensile strength values of two laser-welded batteries provided in an embodiment of the present application;
[0017] FIG5 is a schematic diagram showing a comparison of the internal resistance of two laser-welded batteries provided in an embodiment of the present application;
[0018] FIG6 is a schematic diagram showing a comparison of discharge temperature rises of batteries of two laser-welded shapes provided in an embodiment of the present application. Modes for Carrying Out the Invention
[0019] After research, the inventor found that the square battery of the related technology, such a welding connection method not only increases the weight of the battery itself, occupies the internal space of the battery, reduces the mass-to-energy ratio of the battery and the internal space utilization rate of the square battery, but also due to the introduction of auxiliary welding pieces and connecting pieces, the energy inside the core pack needs to pass through the auxiliary welding pieces and connecting pieces to be output to the charge and discharge ports on the cover plate. In this process, part of the energy is lost, causing the internal temperature of the battery to rise significantly. There may be a risk of thermal runaway during long-term use of the battery. The square battery has the following problems: ① The introduction of auxiliary welding pieces and connecting pieces leads to high cost and large size; ② Energy needs to be transmitted by auxiliary welding pieces and connecting pieces, so that part of the energy is lost, causing the internal temperature of the battery to rise significantly. There may be a risk of thermal runaway during long-term use of the battery.
[0020] In order to solve the above problems, as shown in FIG1 , this embodiment provides a square battery 100 , which includes a cover plate 110 , on which a pole is provided; and a core pack 120 , on which a tab is provided, which is directly connected to the pole by laser welding.
[0021] The square battery 100 provided in this embodiment includes a cover plate 110, which is provided with a pole; a core pack 120 is provided with a tab, and the tab and the pole are directly connected by laser welding; the construction of the battery's energy transmission path is realized, and the charging and discharging functions of the core pack are realized. At the same time, because the tab and the pole are welded by laser, the strength of the welding between the tab and the pole is improved compared to ultrasonic welding. Furthermore, the square battery eliminates auxiliary welding tabs and connecting tabs, thereby improving the internal space utilization and mass-to-energy of the battery. In some embodiments, the pole includes a positive pole and a negative pole; the tab includes a positive tab and a negative pole; the positive tab is directly connected to the positive pole by laser welding; and / or the negative tab is directly connected to the negative pole by laser welding.
[0022] As shown in FIG1 , the electrode column includes a positive electrode column 1101 and a negative electrode column 1102; the electrode tab includes a positive electrode tab 1201 and a negative electrode tab 1202; the positive electrode tab 1201 is directly connected to the positive electrode column 1101 by laser welding; and / or the negative electrode tab 1202 is directly connected to the negative electrode column 1102 by laser welding, that is, the positive electrode tab 1201 is connected to the positive electrode column 1101 by laser welding, and / or the negative electrode tab 1202 is connected to the negative electrode column 1102 by laser welding. The direct connection with the positive electrode column 1101, and / or the direct connection of the negative electrode ear 1202 with the electrode column 1101, realizes the construction of the energy transmission path of the battery and realizes the charging and discharging function of the core pack. At the same time, since the positive electrode ear 1201 and the positive electrode column 1101, and / or the negative electrode ear 1202 and the negative electrode column 1102 are laser welded, the firmness of the welding between the electrode ear and the electrode column is improved compared with ultrasonic welding. Furthermore, the square battery eliminates the auxiliary welding piece and the connecting piece, thereby improving the internal space utilization and mass-to-energy of the square battery.
[0023] In some embodiments, the positive electrode tab has multiple layers of positive electrode tabs, and the multiple layers of positive electrode tabs are compacted. The negative electrode tab has multiple layers of negative electrode tabs, and the multiple layers of negative electrode tabs are compacted. The ratio of the compacted size of the multiple layers of positive electrode tabs to the thickness of the core package is less than or equal to 1, and the ratio of the compacted size of the multiple layers of negative electrode tabs to the thickness of the core package is less than or equal to 1, wherein the compacted size is the positioning size of the fixture when the multiple layers of tabs are closed.
[0024] Specifically, the collapsed dimension H of the tab 收拢 It can be the thickness of the core package H 芯厚 1 / 4-5 / 7 of the size. Preferably, the folded size H 收拢 =H 芯厚*1 / 4, and makes the first layer of tabs more spacious. After the tabs are folded according to this formula, the edges of the weld marks will not be damaged due to the pulling of the tabs during the subsequent laser welding process, thereby improving the yield of the tabs.
[0025] In some embodiments, the thickness of the core package is 1mm-700mm, the collapsed size of the multi-layer positive electrode tabs is 1mm-500mm, and the collapsed size of the multi-layer negative electrode tabs is 1mm-500mm.
[0026] Specifically, H 芯厚 The size range is 1mm-700mm, and the folded size is H 收拢 The size range is 1mm-500mm. For example, H 芯厚 When the folded size is 1mm, the folded size H 收拢 If the first layer of tabs is 1mm, then the first layer of tabs is generally spacious. 芯厚 When the folded size is 700mm, 收拢 The first layer of tabs is relatively spacious. As shown in Figure 2, the folded size H 收拢 The thickness of the core package H 芯厚 The diagram shows the relationship between the dimensions of the core package. The retraction dimensions are determined based on the thickness of the core package, fully considering the impact of the core package thickness on the subsequent tab welding yield, and preventing the tab from pulling and causing damage to the weld edge. As can be seen from the core package thickness and the retraction dimensions of the positive and negative tabs, limiting the retraction dimensions of the positive and negative tabs can prevent damage to the weld edge caused by pulling on the tabs, thereby ensuring a more reliable connection between the tabs and the electrode.
[0027] In some embodiments, the positive electrode tab is formed by ultrasonic pre-welding the multi-layer positive electrode tab; and / or the negative electrode tab is formed by ultrasonic pre-welding the multi-layer negative electrode tab.
[0028] Specifically, in one embodiment, multiple layers of positive electrode tabs are ultrasonically pre-welded to form positive electrode tabs; in another embodiment, multiple layers of negative electrode tabs are ultrasonically pre-welded to form negative electrode tabs; in yet another embodiment, multiple layers of positive electrode tabs are ultrasonically pre-welded to form positive electrode tabs, and at the same time, multiple layers of negative electrode tabs are ultrasonically pre-welded to form negative electrode tabs. Since the laser beam is sensitive to the gaps between welding material layers, as the number of tab layers increases, the larger the gap between the bottom layers, the more difficult it is for the laser to penetrate, which can easily cause cold welding. The tighter the gap between the tab layers, the better the fusion of the substrate, which is less likely to cause cold welding. Therefore, the use of ultrasonic pre-welding can reduce the layer gap between the tabs, making the tabs a tight whole, and reducing abnormalities such as cold welding that may occur during laser welding.
[0029] In some embodiments, the positive electrode tab after ultrasonic pre-welding is connected to the positive electrode column by laser final welding; and / or the negative electrode tab after ultrasonic pre-welding is connected to the negative electrode column by laser final welding.
[0030] In one embodiment, the positive electrode tab after ultrasonic pre-welding is connected to the positive electrode post by laser final welding; in another embodiment, the negative electrode tab after ultrasonic pre-welding is connected to the negative electrode post by laser final welding; in yet another embodiment, the positive electrode tab after ultrasonic pre-welding is connected to the positive electrode post by laser final welding, and the negative electrode tab after ultrasonic pre-welding is connected to the negative electrode post by laser final welding. In this embodiment, by laser welding the positive electrode tab after ultrasonic pre-welding and the positive electrode post, and / or laser welding the negative electrode tab after ultrasonic pre-welding and the negative electrode post, the possibility of cold welds during laser welding is reduced, and laser welding is used for the final welding, so that the connection between the positive electrode tab and the positive electrode post and / or the connection between the negative electrode tab and the negative electrode post is more secure.
[0031] In some embodiments, the ratio of the area of the final laser weld to the area of the ultrasonic pre-weld is less than 1.
[0032] Specifically, the area of the laser final weld is smaller than the area of the ultrasonic pre-weld. For example, the area of the laser final weld is 0.6-0.8 times the area of the ultrasonic pre-weld. For example, the area of the ultrasonic pre-weld is greater than 2 mm. 2 And no more than 600mm 2 , the area of laser final welding is not less than 2mm 2 and no larger than 540mm 2 If the ultrasonic pre-welding area is 10mm 2 , the area of laser final welding can be set to 7mm 2 , it is sufficient that the area of the final laser weld is smaller than the area of the ultrasonic pre-weld. By setting the ratio between the area of the final laser weld and the area of the ultrasonic pre-weld, the tab is firmly welded to the pole through pre-weld and final weld.
[0033] In some embodiments, the shape of the laser final weld is at least one of an ellipse, a circle, or a polygon, and the shape of the ultrasonic pre-weld is at least one of an ellipse, a circle, or a polygon.
[0034] Specifically, the laser final weld shape is preset to be at least one of a square, an ellipse, a circle, or a five-pointed star. It is worth noting that due to the single regular shape, the area of the laser final weld is simpler and more convenient to design. Therefore, as a preferred embodiment of the present invention, the laser final weld shape is selected to be a regular shape, such as an ellipse, a square, etc. For example, the polygon can be a square, a five-pointed star, etc.
[0035] Specifically, the shape of the ultrasonic pre-weld is at least one of an ellipse, a circle, or a polygon. It is worth noting that due to the single regular shape, the area design of the ultrasonic pre-weld is simpler and more convenient. Therefore, as a preferred embodiment of the present invention, the shape of the ultrasonic pre-weld is a regular shape, such as an ellipse, a square, etc. For example, the polygon can be a square, a five-pointed star, etc.
[0036] In some embodiments, a ratio of the area of the ultrasonic pre-weld to the area of the pole is greater than or equal to 0.32 and less than or equal to 0.81.
[0037] Specifically, the overcurrent and temperature rise of the battery are closely related to the area of the laser final weld. When the area of the laser final weld is larger, the overcurrent capacity is better and the temperature rise is also better. However, the larger the area of the laser final weld is, the lower its processing and manufacturability are. Since the laser final weld is performed on the basis of ultrasonic pre-welding, the area of the laser final weld is smaller than the area of the ultrasonic pre-welding, and the setting of the area of the laser final weld needs to be set according to the area of the ultrasonic pre-welding. When the pole is square and the shape of the laser final weld is also square, when the length of the square of the ultrasonic pre-weld is 0.8 times the length of the pole and the width is 0.4 times the width of the pole, the area of the ultrasonic pre-weld is the largest, ensuring that the area of the laser final weld, which is positively correlated with the area of the ultrasonic pre-weld, has room to increase, thereby making the processing and manufacturability of the laser final weld higher, and the overcurrent capacity and temperature rise control better. At this time, the ratio of the area of the ultrasonic pre-weld to the area of the pole is 0.32; when the pole is elliptical and the shape of the laser final weld is also elliptical, when the major semi-axis of the ellipse of the ultrasonic pre-weld is 0.9 times the major semi-axis of the pole and the minor semi-axis is 0.9 times the minor semi-axis of the pole, the area of the ultrasonic pre-weld is the largest, ensuring that the area of the laser final weld, which is positively correlated with the area of the ultrasonic pre-weld, has room to increase, thereby making the processing and manufacturability of the laser final weld higher, and the overcurrent capacity and temperature rise control better. At this time, the ratio of the area of the ultrasonic pre-weld to the area of the pole is 0.81. Exemplarily, the shapes of the pole and the ultrasonic pre-weld are both elliptical, the short semi-axis of the pole's ellipse is b, the long semi-axis is a, the area of the pole is S1 = π*a*b, the short semi-axis of the ultrasonic pre-weld's ellipse is 0.8b, the long semi-axis is 0.4a, and the area of the ultrasonic pre-weld is S2 = π*0.8a*0.4b, wherein the size range of a is 1mm-500mm, and the size range of b is 1mm-400mm.
[0038] In some embodiments, the ratio of the perimeter of the laser final weld track to the perimeter of the ultrasonic pre-weld track is less than 1.
[0039] Among them, in order to ensure the rationality of the trajectory setting of laser final welding, the ratio between the trajectory circumference of laser final welding and the trajectory circumference of ultrasonic pre-welding is less than 1, that is, the trajectory circumference of laser final welding is smaller than the trajectory circumference of ultrasonic pre-welding, and its processing and manufacturability are high, and the current capacity and temperature rise control are better. For example, the shapes of laser final welding and ultrasonic pre-welding are both elliptical, the short semi-axis of the ellipse of ultrasonic pre-welding is b, and the long semi-axis is a, the short semi-axis of the ellipse of laser final welding is 0.32b, and the long semi-axis is 0.72a, the trajectory circumference of ultrasonic pre-welding is L1=2π*b+4(ab), and the trajectory circumference of laser final welding is L2=2π*0.32b+4(0.72a-0.32b), the size range of a is greater than 1mm and not greater than 500mm, and the size range of b is not less than 1mm and not greater than 400mm.
[0040] FIG3 is a flow chart of a welding method according to an embodiment of the present application, wherein the welding method includes:
[0041] 101. Perform ultrasonic pre-welding on the tabs on the core pack according to a first weld print area to form ultrasonic pre-welded tabs, wherein the first weld print area is determined according to the size and shape of the pole.
[0042] The welding method is used to connect the core pack and the cover plate in the battery. The battery includes a core pack and a cover plate, and the core pack has a tab, which is a multi-layer tab, and the cover plate includes a terminal. The battery in this embodiment is connected by connecting the core pack and the cover plate.
[0043] The term "electrode shape" refers to the shape of the electrode on the cover plate, which can be, for example, square, round, or oval. The term "electrode size" refers to the dimensions of the electrode on the cover plate under different shapes, such as radius, length, and width. The first weld area refers to the parameters of the weld track when ultrasonic pre-welding the tabs. Because the setting of the first weld area can affect the battery's current capacity and temperature rise, in this embodiment, the first weld area is determined by detecting the size and shape of the electrode. This takes into account the impact of the shape and related dimensions of the electrode on the cover plate on the first weld area, ensuring the rationality of the first weld area and, in turn, ensuring the accuracy of subsequent welding and avoiding poor welding.
[0044] It is worth noting that since the laser beam is sensitive to the gap between the welding material layers, the more the number of tab layers increases, the larger the gap between the bottom layers, the more difficult it is for the laser to penetrate, which can easily cause cold welding. The tighter the gap between the tab layers, the better the fusion of the base material, and the less likely it is to cause cold welding. Therefore, the use of ultrasonic pre-welding can reduce the inter-layer gap between the tabs, making the tabs a tight whole, and reducing abnormalities such as cold welding that may occur during laser welding.
[0045] Furthermore, the shape of the pole is one of square, circular or elliptical, and the corresponding dimensions of the pole are length a and width b, radius r, short semi-axis c and long semi-axis d.
[0046] Specifically, when the shape of the pole is square, the corresponding pole dimensions are length a and width b; when the shape of the pole is circular, the corresponding pole dimension is radius r; when the shape of the pole is elliptical, the corresponding pole dimensions are short semi-axis c and long semi-axis d.
[0047] Furthermore, if the shape of the pole is the square, the length a is adjusted according to the first preset adjustment coefficient λ1 to obtain an adjusted length, wherein 0<λ1<1; the width b is adjusted according to the second preset adjustment coefficient λ2 to obtain an adjusted width, wherein 0<λ2<1; and a first weld print area is determined based on the adjusted length and the adjusted width; preferably, 0.7<λ1<0.9; preferably 0.3<λ2<0.5.
[0048] Specifically, when the shape of the pole is square, the length a and width b of the pole can be adjusted according to the corresponding first preset adjustment coefficient λ1 and the second preset adjustment coefficient λ2, respectively, to obtain the adjusted length λ1*a and the adjusted width λ2*b, and the first weld print area S can be calculated according to the square area calculation formula based on the adjusted length λ1*a and the adjusted width λ2*b. 超声 =(λ1*a)*(λ2*b), and since 0.7<λ1<0.9 and 0.3<λ2<0.5, the first weld print area is smaller than the area of the pole, and under the premise of ensuring rationality, the adjustment length and adjustment width are maximized, ensuring the rationality and maximization of the first weld print area, reducing the redundancy of the tab welding of the core pack in the battery, and ensuring the safety of the core pack.
[0049] In one embodiment, λ1 = 0.8, λ2 = 0.4, then S 超声 =(0.8*a)*(0.4*b)=0.32ab. It can be understood that in this embodiment, by adjusting the length a and width b of the square pole, and for the square pole, the length a is adjusted to 0.8 times the original length and the width b is adjusted to 0.4 times the original length, compared with the traditional manual experience setting, the reasonable accuracy of the first weld print area calculation is improved, which is conducive to improving the accuracy of ultrasonic pre-welding.
[0050] Furthermore, if the shape of the pole is the circle, the radius r is adjusted according to a third preset adjustment coefficient λ3 to obtain an adjusted radius, wherein 0<λ3<1; the first weld print area is determined according to the adjusted radius; preferably, 0.75<λ3<0.9.
[0051] Specifically, when the shape of the pole is circular, the radius r of the pole can be adjusted according to the third preset adjustment coefficient λ3 to obtain the adjusted radius λ3*r. According to the adjusted radius λ3*r, the first weld print area S can be calculated according to the area calculation formula of the circle. 超声 =π*(λ3*r)*(λ3*r), and since 0.75<λ3<0.9, the first weld print area is smaller than the area of the pole, and under the premise of ensuring rationality, the adjustment radius is maximized, ensuring the rationality and maximization of the first weld print area, reducing the welding redundancy of the tab of the core pack in the battery, and ensuring the safety of the core pack.
[0052] In one embodiment, λ3 = 0.8, then S 超声 =π*(0.8*r)*(0.8*r)=0.64π*r 2 It can be understood that in this embodiment, by adjusting the radius r of the circular pole, and for the circular pole, the radius r is adjusted to 0.8 times the original value, compared with the traditional manual experience setting, the reasonable accuracy of the first weld print area calculation is improved, which is conducive to improving the accuracy of ultrasonic pre-welding.
[0053] Furthermore, if the shape of the pole is the ellipse, the minor semi-axis c is adjusted according to the fourth preset adjustment coefficient λ4 to obtain an adjusted minor semi-axis, wherein 0<λ4<1; the major semi-axis d is adjusted according to the fifth preset adjustment coefficient λ5 to obtain an adjusted major semi-axis, wherein 0<λ5<1; the first weld print area is determined based on the adjusted minor semi-axis and the adjusted major semi-axis; preferably, 0.85<λ4<0.95; preferably, 0.85<λ5<0.95.
[0054] Specifically, when the shape of the pole is an ellipse, the short semi-axis c and the long semi-axis d of the pole can be adjusted according to the corresponding fourth preset adjustment coefficient λ4 and the fifth preset adjustment coefficient λ5, respectively, to obtain the adjusted short semi-axis λ4*c and the adjusted long semi-axis λ5*d. According to the adjusted short semi-axis λ4*c and the adjusted long semi-axis λ5*d, the first weld print area S can be calculated according to the area calculation formula of the ellipse. 超声 =π*(λ4*c)*(λ5*d), and since 0.85<λ4<0.95 and 0.85<λ5<0.95, the first weld print area is smaller than the area of the pole, and under the premise of ensuring rationality, the adjustment length and adjustment width are maximized, ensuring the rationality and maximization of the first weld print area, reducing the welding redundancy of the tab of the core pack in the battery, and ensuring the safety of the core pack.
[0055] In one embodiment, λ4=0.9, λ5=0.9, then S 超声=π*(λ4*c)*(λ5*d)=0.81*π*c*d. It can be understood that in this embodiment, by adjusting the semi-minor axis c and the semi-major axis d of the elliptical pole, and for the elliptical pole, the semi-minor axis c is adjusted to 0.9 times the original value, and the semi-major axis d is adjusted to 0.9 times the original value, compared with the traditional manual experience setting, the reasonable accuracy of the first weld print area calculation is improved, which is conducive to improving the accuracy of ultrasonic pre-welding.
[0056] 102. Laser weld the ultrasonically pre-welded tab and the pole according to a second weld print area to complete the connection between the tab and the pole, wherein a ratio of the second weld print area to the first weld print area is less than 1.
[0057] Among them, the second weld mark area refers to the parameter of a weld mark trajectory when the ultrasonic pre-welded tab and the pole are subjected to laser final welding. Since it is difficult to ensure the stability of welding by ultrasonic pre-welding alone, there may be cold welds or poor weld marks. Therefore, in this embodiment, on the basis of ultrasonic pre-welding, laser welding is continued to be performed on the ultrasonic pre-welded tab and the pole to form a complete path between the tab and the pole to realize current charging and discharging.
[0058] Specifically, the ratio of the second weld print area to the first weld print area is less than 1, that is, the second weld print area is smaller than the first weld print area. The influence of the first weld print area on the laser welding area is taken into consideration, and the rationality of the second weld print area is ensured, thereby ensuring the accuracy of laser welding and avoiding poor welding.
[0059] Furthermore, a ratio of the second weld print area to the first weld print area is μ, and 0.6<μ<0.8.
[0060] Specifically, as the connection formed by the tab and the cover plate becomes sparser, the number of pathways for energy transmission and transmission inside the battery increases, thereby improving the energy transmission capacity and effectively improving the flow capacity. At the same time, due to the increase in pathways, the energy is no longer concentrated, and the battery temperature rise can also be effectively reduced. Because a reasonable laser weld area needs to be set, the flow capacity and temperature rise of the battery are closely related to the second weld area. When the second weld area is larger, the flow capacity is better and the temperature rise is also better. However, the larger the second weld area, the lower its processing and manufacturability. When the second weld area is 0.6 to 0.8 times the ultrasonic pre-welding area, its processing and manufacturability are higher, and the flow capacity and temperature rise control are better. Therefore, in this embodiment, the second weld area is adjusted to 0.6-0.8 times the first weld area. As the preferred embodiment of this embodiment, the laser weld area S 激光 =0.8S 超声 , so as to maximize the second weld print area and improve the rationality and accuracy of the second weld print area.
[0061] Furthermore, the laser welding of the ultrasonic pre-welded tab and the pole according to the second weld print area includes: obtaining a preset welding shape for laser welding; determining a laser welding trajectory according to the second weld print area and the preset welding shape; and laser welding the ultrasonic pre-welded tab and the pole according to the laser welding trajectory.
[0062] The preset welding shape of laser welding is a pre-set shape for laser welding. For example, the preset welding shape is a five-pointed star, a triangle, a polygon or an irregular shape.
[0063] Specifically, the preset welding shape is a five-pointed star, a triangle, a polygon or an irregular shape. It is worth noting that due to the regular shape, the design of the second welding print area is simpler and more convenient. Therefore, as a preference of this embodiment, the preset welding shape selects a regular shape, such as an ellipse, a square, etc.
[0064] Specifically, a laser weld with a preset welding shape and an area of the second weld print area is performed between the ultrasonic pre-welded tab and the pole, completing the laser weld of the ultrasonic pre-welded tab and the pole. More specifically, the size of the preset welding shape is calculated based on the second weld print area and the preset welding shape, and the laser welding trajectory is calculated based on the size and the preset welding shape. Laser final welding is performed between the ultrasonic pre-welded tab and the pole according to the laser welding trajectory, thereby realizing the welding of the tab and the pole in the battery. Since the second weld print area is reasonable and accurate, the battery yield is improved.
[0065] Furthermore, before ultrasonically pre-welding the tabs on the core package according to the first weld print area, the method further includes: determining a folding size of the tabs according to the thickness of the core package; and folding and compacting the tabs according to the folding size.
[0066] Among them, the folded size is the positioning size of the fixture when the tab is closed.
[0067] Specifically, the tabs can be assembled after the tabs are slit and die-cut, wherein the assembly method includes but is not limited to lamination or winding. Then, the thickness H of the core package is obtained according to the model of the core package or the parameter information of the core package. 芯厚 The collapsing dimensions of the positive and negative tabs within the core pack are determined based on the core pack thickness to ensure sufficient tightness between the tabs during ultrasonic pre-welding of the assembled core pack. As can be appreciated, in this embodiment, the collapsing dimensions are determined based on the core pack thickness, fully accounting for the impact of the core pack thickness on the subsequent tab welding yield and preventing damage to the weld edges due to tab pulling.
[0068] Furthermore, the thickness of the core package is 1mm-700mm, and the collapsed size is 1mm-500mm;
[0069] Alternatively, the collapsed size is less than or equal to the thickness of the core package; preferably, the ratio of the collapsed size to the thickness of the core package is 1 / 5 to 1; preferably, the ratio of the collapsed size to the thickness of the core package is 1 / 4 to 5 / 7.
[0070] Specifically, the collapsed dimension H of the tab 收拢 It can be the thickness of the core package H 芯厚 1 / 4-5 / 7 of the size. Preferably, the folded size H 收拢 =H 芯厚 *1 / 4, and make the first layer of tabs more spacious. According to this formula, the tabs after being gathered will not be damaged by the tab pulling during the subsequent laser welding process, thus improving the yield of the tabs. As shown in Figure 2, the gathered size H 收拢 The thickness of the core package H 芯厚 Schematic diagram of the size relationship.
[0071] In one example, H 芯厚 The size range is 1mm-700mm, and the folded size is H 收拢 The size range is 1mm-500mm. For example, H 芯厚 When the folded size is 1mm, the folded size H 收拢 If the first layer of tabs is 1mm, then the first layer of tabs is generally spacious. 芯厚 When the folded size is 700mm, 收拢 It is 500mm, and the first layer of tabs is relatively spacious.
[0072] Furthermore, the ratio of the first weld mark area to the area of the pole is greater than or equal to 0.32 and less than or equal to 0.81; and / or the ratio of the trajectory circumference corresponding to the laser welding to the trajectory circumference corresponding to the ultrasonic pre-welding is less than 1.
[0073] Specifically, the overcurrent and temperature rise of the battery are closely related to the area of the laser final weld. When the area of the laser final weld is larger, the overcurrent capacity is better and the temperature rise is also better. However, the larger the area of the laser final weld is, the lower its processing and manufacturability are. Since the laser final weld is performed on the basis of ultrasonic pre-welding, the area of the laser final weld is smaller than the area of the ultrasonic pre-welding, that is, the area of the second weld print is smaller than the area of the first weld print, and the setting of the area of the laser final weld needs to be set according to the area of the ultrasonic pre-welding. When the pole is square and the shape of the laser final weld is also square, when the length of the square of the ultrasonic pre-weld is 0.8 times the length of the pole and the width is 0.4 times the width of the pole, the area of the ultrasonic pre-weld is the largest, ensuring that the area of the laser final weld, which is positively correlated with the area of the ultrasonic pre-weld, has room to increase, thereby making the processing and manufacturability of the laser final weld higher, and the overcurrent capacity and temperature rise control better. At this time, the ratio of the area of the ultrasonic pre-weld to the area of the pole is 0.32; when the pole is elliptical and the shape of the laser final weld is also elliptical, when the major semi-axis of the ellipse of the ultrasonic pre-weld is 0.9 times the major semi-axis of the pole and the minor semi-axis is 0.9 times the minor semi-axis of the pole, the area of the ultrasonic pre-weld is the largest, ensuring that the area of the laser final weld, which is positively correlated with the area of the ultrasonic pre-weld, has room to increase, thereby making the processing and manufacturability of the laser final weld higher, and the overcurrent capacity and temperature rise control better. At this time, the ratio of the area of the ultrasonic pre-weld to the area of the pole is 0.81. Exemplarily, the shapes of the pole and the ultrasonic pre-weld are both elliptical, the short semi-axis of the pole's ellipse is b, the long semi-axis is a, the area of the pole is S1 = π*a*b, the short semi-axis of the ultrasonic pre-weld's ellipse is 0.8b, the long semi-axis is 0.4a, and the area of the ultrasonic pre-weld is S2 = π*0.8a*0.4b, wherein the size range of a is 1mm-500mm, and the size range of b is 1mm-400mm.
[0074] Specifically, in order to ensure the rationality of the trajectory setting of laser final welding, the ratio between the trajectory circumference of laser final welding and the trajectory circumference of ultrasonic pre-welding is less than 1, that is, the trajectory circumference of laser final welding is smaller than the trajectory circumference of ultrasonic pre-welding. Its processing and manufacturability are high, and the current capacity and temperature rise control are better. For example, the shapes of laser final welding and ultrasonic pre-welding are both elliptical, the short semi-axis of the ellipse of ultrasonic pre-welding is b, and the long semi-axis is a, the short semi-axis of the ellipse of laser final welding is 0.32b, and the long semi-axis is 0.72a, the trajectory circumference of ultrasonic pre-welding is L1=2π*b+4(ab), and the trajectory circumference of laser final welding is L2=2π*0.32b+4(0.72a-0.32b), the size range of a is greater than 1mm and not greater than 500mm, and the size range of b is not less than 1mm and not greater than 400mm.
[0075] In this embodiment, the first weld print area is determined according to the size and shape of the pole to ensure the rationality of the first weld print area. According to the first weld print area, the pole tabs on the core package are ultrasonically pre-welded according to the first weld print area, which reduces the layer gap between the pole tabs, makes the pole tabs a tight whole, and reduces abnormalities such as cold welding that may occur during laser welding. The ultrasonically pre-welded pole tabs and the pole are laser welded according to the second weld print area. Since the second weld print area is smaller than the first weld print area, it can ensure that the pole tab is completely attached to the pole post. Under the premise of achieving welding stability, the overcurrent capacity of the pole tab is guaranteed, ensuring the rationality and maximization of the second weld print area, effectively improving the overcurrent capacity at the connection between the pole tab and the pole, and reducing the temperature rise. In addition, the laser welding method forms a complete passage between the pole tab and the pole, which greatly improves the battery yield.
[0076] In one example, Figure 4 shows a comparison of the tensile strength values of two laser-welded battery shapes. The experimental group used the elliptical shape of this embodiment, while the control group used a double-line shape, Type II. The welding energy was 3900W, the welding speed was 200mm / s, and the number of layers was 70. Figure 4 clearly shows that the peel strength of the experimental group was higher than that of the control group, and the welds in the experimental group were superior to those in the control group.
[0077] In one example, as shown in FIG5 , there is a schematic diagram comparing the tested internal resistance (ACR1) of batteries of two laser-welded shapes, wherein the experimental group has the shape of the present embodiment, i.e., an elliptical shape, and the control group has a double-line shape. As can be seen from FIG5 , the ACR1 of the experimental group decreased by 0.0276 milliohms compared with the control group, with a decrease percentage of 11.42%.
[0078] In one example, as shown in FIG6 , which is a schematic diagram comparing the discharge temperature rise of batteries with two laser-welded shapes, the experimental group is the shape of the present embodiment, i.e., an elliptical shape, and the control group is a double-line shape, i.e., type II. The welding energy is 3900 W, the welding speed is 200 mm / s, and the number of layers is 70. As can be seen from FIG6 , the discharge temperature rise of the experimental group is 1°C-1.5°C better than that of the control group.
Claims
1. A square battery, comprising: A cover plate, wherein the cover plate is provided with a pole; The core package is provided with a pole ear, and the pole ear is directly connected to the pole by laser welding.
2. The square battery according to claim 1, wherein: The poles include a positive pole and a negative pole; The tabs include a positive tab and a negative tab; The positive electrode tab is directly connected to the positive electrode column by laser welding; and / or the negative electrode tab is directly connected to the negative electrode column by laser welding.
3. The square battery according to claim 2, wherein: The positive electrode ear has multiple layers of positive electrode ears, and the multiple layers of positive electrode ears are compressed. The negative electrode ear has multiple layers of negative electrode ears, and the multiple layers of negative electrode ears are compressed. The ratio of the compressed size of the multiple layers of positive electrode ears to the thickness of the core package is less than or equal to 1, and the ratio of the compressed size of the multiple layers of negative electrode ears to the thickness of the core package is less than or equal to 1, wherein the compressed size is the positioning size of the fixture when the multiple layers of the ears are closed.
4. The square battery according to claim 3, wherein: The thickness of the core package is 1mm-700mm, the compacted size of the multi-layer positive electrode tabs is 1mm-500mm; the compacted size of the multi-layer negative electrode tabs is 1mm-500mm.
5. The square battery according to claim 4, wherein: The gathered size is 1 / 4-5 / 7 of the thickness of the core package.
6. The square battery according to claim 3, wherein: The positive electrode tab is formed by ultrasonic pre-welding the multiple layers of positive electrode tabs that are compressed and held together; and / or, the negative electrode tab is formed by ultrasonic pre-welding the multiple layers of negative electrode tabs that are compressed and held together.
7. The square battery according to claim 6, wherein: The positive electrode tab after ultrasonic pre-welding is connected to the positive electrode column by laser final welding; and / or the negative electrode tab after ultrasonic pre-welding is connected to the negative electrode column by laser final welding.
8. The square battery according to claim 7, wherein: The ratio between the area of the laser final weld and the area of the ultrasonic pre-weld is less than 1.
9. The square battery according to claim 7, wherein: The shape of the laser final weld is at least one of an ellipse, a circle or a polygon, and / or the shape of the ultrasonic pre-weld is at least one of an ellipse, a circle or a polygon.
10. The square battery according to any one of claims 6 to 9, wherein: The ratio of the area of the ultrasonic pre-welding to the area of the pole is greater than or equal to 0.32 and less than or equal to 0.
81.
11. The square battery according to claim 7, wherein: The ratio between the perimeter of the laser final welding track and the perimeter of the ultrasonic pre-welding track is less than 1.
12. A welding method, the method comprising: Performing ultrasonic pre-welding on the tabs on the core pack according to a first weld print area to form ultrasonic pre-welded tabs, wherein the first weld print area is determined according to the size and shape of the pole; The ultrasonic pre-welded pole tab and the pole are laser welded according to a second weld print area to complete the connection between the pole tab and the pole, wherein the ratio of the second weld print area to the first weld print area is less than 1.
13. The welding method according to claim 12, wherein: The shape of the pole is one of square, round or elliptical, and the corresponding dimensions of the pole are length a, width b, radius r, short semi-axis c and long semi-axis d.
14. The welding method according to claim 13, wherein: include: If the shape of the pole is the square, the length a is adjusted according to the first preset adjustment coefficient λ1 to obtain an adjusted length, wherein 0<λ1<1; The width b is adjusted according to a second preset adjustment coefficient λ2 to obtain an adjusted width, wherein 0<λ2<1; Determine a first weld print area according to the adjusted length and the adjusted width; Preferably, 0.7<λ1<0.9; Preferably, 0.3<λ2<0.
5.
15. The welding method according to claim 13, wherein: include: If the shape of the pole is the circle, the radius r is adjusted according to a third preset adjustment coefficient λ3 to obtain an adjusted radius, wherein 0<λ3<1; Determine the first weld area according to the adjustment radius; Preferably, 0.75<λ3<0.
9.
16. The welding method according to claim 13, wherein: include: If the shape of the pole is the ellipse, the minor semi-axis c is adjusted according to a fourth preset adjustment coefficient λ4 to obtain an adjusted minor semi-axis, wherein 0<λ4<1; The major semi-axis d is adjusted according to a fifth preset adjustment coefficient λ5 to obtain an adjusted major semi-axis, wherein 0<λ5<1; Determine a first weld print area according to the adjusted minor semi-axis and the adjusted major semi-axis; Preferably, 0.85<λ4<0.95; Preferably, 0.85<λ5<0.
95.
17. The welding method according to any one of claims 12 to 16, wherein: The ratio of the second weld print area to the first weld print area is μ, and 0.6<μ<0.
8.
18. The welding method according to any one of claims 12 to 16, before ultrasonically pre-welding the tabs on the core package according to the first weld print area, further comprising: Determining the folded size of the tab according to the thickness of the core package; The tabs are folded and compacted according to the folded size.
19. The welding method according to claim 18, wherein: The thickness of the core package is 1mm-700mm, and the collapsed size is 1mm-500mm; or, The collapsed size is less than or equal to the thickness of the core package; Preferably, the ratio of the collapsed size to the thickness of the core package is 1 / 5 to 1; Preferably, the ratio of the collapsed size to the thickness of the core package is 1 / 4 to 5 / 7.
20. The welding method according to any one of claims 12 to 16, wherein: The laser welding of the ultrasonic pre-welded tab and the pole according to the second weld print area includes: Obtaining a preset welding shape for laser welding; Determining a laser welding trajectory according to the second weld print area and the preset welding shape; The ultrasonic pre-welded pole lug and the pole are laser welded according to the laser welding trajectory.
21. The welding method according to any one of claims 12 to 16, wherein: The ratio of the first weld area to the area of the pole is greater than or equal to 0.32 and less than or equal to 0.81; And / or, the ratio between the circumference of the trajectory corresponding to the laser welding and the circumference of the trajectory corresponding to the ultrasonic pre-welding is less than 1.
Citation Information
Patent Citations
Welding method and welding structure of battery tab and pole
CN114976510A
Laser welding method for aluminum foil pole lug and pole post after ultrasonic welding
CN115283868A
Welding method and battery
CN116551183A
Power battery structure
CN217544862U