Slurry composition and preparation method therefor, electron transport film layer and preparation method therefor, and perovskite solar cell and preparation method therefor

By using a slurry composition of nano-tin dioxide and amine-based ionic liquid, combined with screen printing technology, the problems of nanoparticle agglomeration and interface contact performance of the tin dioxide electron transport film layer in the prior art are solved, and high efficiency is achieved. The preparation of low-energy-consuming electron transport film layers improves the performance of perovskite solar cells.

WO2024244864A1PCT designated stage expired Publication Date: 2024-12-05TONGWEI SOLAR ENERGY (CHENGDU) CO LID
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/090411
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-04-28
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing preparation methods of tin dioxide electron transport film layer such as solution spin coating and chemical bath deposition have problems such as nanoparticle agglomeration, decreased interface contact performance, high energy consumption and difficult process control, which affects the perovskite solar cells. performance.

Method used

The slurry composition composed of nano-tin dioxide and amine-based ionic liquid is used to prepare an electron transport film layer through screen printing technology, and the hydrogen bond network is formed by using amine-tin ionic liquid and nano-tin dioxide to improve conductivity and mobility. The particle size and dispersion of nanotin dioxide are adjusted by surfactant.

Benefits of technology

The conductivity and mobility of the electron transport film layer are improved, process temperature and energy consumption are reduced, film layer defects are reduced, and the photoelectric conversion efficiency and stability of perovskite solar cells are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024090411_05122024_PF_FP_ABST
    Figure CN2024090411_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides a slurry composition and a preparation method therefor, an electron transport film layer and a preparation method therefor, and a perovskite solar cell and a preparation method therefor. The slurry composition comprises nano tin dioxide and amino ionic liquid, wherein the molar concentration ratio of the nano tin dioxide to the amino ionic liquid is (0.5-1):(0.5-2); and in the amino ionic liquid, cations are amino cations, and anions are organic acid anions.
Need to check novelty before this filing date? Find Prior Art

Description

Slurry composition and preparation method, electron transport film layer and preparation method, perovskite solar cell and preparation method

[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on May 29, 2023, with application number CN202310618942.5 and public name “Slurry composition and preparation method, electron transport film layer and preparation method, perovskite solar cell and preparation method”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present invention relates to the field of perovskite solar cells, and in particular to a slurry composition and a preparation method thereof, an electron transport film layer and a preparation method thereof, and a perovskite solar cell and a preparation method thereof. Background Art

[0003] In recent years, organic-inorganic hybrid metal halide perovskite solar cells have experienced rapid development, promising widespread application from the laboratory to the industrial sector. The electron transport layer in the NIP structure of high-efficiency perovskite solar cells is a crucial component of the cell, and its film quality directly impacts the subsequent microstructure and conductive properties of the stacked thin films, as well as the final device's photoelectric conversion efficiency.

[0004] Tin dioxide (SnO) is a wide-bandgap direct-bandgap semiconductor material with advantages such as high mobility, a wide bandgap of 3.6 eV, good light transmittance, low cost, and non-toxicity. It is currently being considered as a promising material for electron transport films. The main methods for preparing SnO2 electron transport films are solution spin coating and chemical bath deposition. However, these methods often produce defects that can degrade device performance.

[0005] Summary of the Invention

[0006] According to multiple embodiments of the present disclosure, a slurry composition is provided, comprising nano-tin dioxide and an amine-based ionic liquid, wherein the molar concentration ratio of the nano-tin dioxide to the amine-based ionic liquid is (0.5-1):(0.5-2), and the cation of the amine-based ionic liquid is an amine-based cation, and the anion is an organic acid anion.

[0007] In some embodiments of the present disclosure, the amine-based ionic liquid is one or a combination of methylamine formate, methylacetamide and methylamine acetate.

[0008] In some embodiments of the present disclosure, the particle size of the nano-tin dioxide is distributed between 5 nm and 20 nm.

[0009] In some embodiments of the present disclosure, a surfactant is added during the preparation of the nano-tin dioxide, and the surfactant molecular formula is:

[0010] Among them, the general formula of R is C n H 2n+1 , the value of n is any one of 12, 14, 16 and 18, the X - Any one of chlorine, bromine and iodine.

[0011] In some embodiments of the present disclosure, the surfactant is one or a combination of cetyltrimethylammonium bromide, octadecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, dodecyltrimethylammonium bromide, cetyltrimethylammonium chloride and cetyltrimethylammonium iodide.

[0012] In some embodiments of the present disclosure, the preparation method of the nano tin dioxide includes: uniformly mixing the surfactant with SnCl4·5H2O, alkali and a first organic solvent, reacting at a pressure of 2MPa to 5MPa and 100°C to 120°C for 20min to 50min, washing and drying to obtain the nano tin dioxide.

[0013] In some embodiments of the present disclosure, the first organic solvent is an alcohol solvent, and the alcohol solvent is one or a combination of ethylene glycol, polyethylene glycol, polypropylene alcohol, isopropyl alcohol and n-butanol.

[0014] In some embodiments of the present disclosure, the base is one or a combination of sodium hydroxide, potassium hydroxide and ammonia water.

[0015] In some embodiments of the present disclosure, the concentration of the surfactant is 0.1 mol / L to 0.3 mol / L, the concentration of the base is 1.2 mol / L to 4 mol / L, and the concentration of SnCl4·5H2O is 0.3 mol / L to 1 mol / L.

[0016] In some embodiments of the present disclosure, after the reaction for preparing the nano-tin dioxide is completed, ethanol and deionized water are used to wash and separate the precipitate.

[0017] In some embodiments of the present disclosure, the slurry composition further includes a viscosity modifier and a second organic solvent, and the viscosity of the slurry composition is 2000 cp to 7000 cp.

[0018] In some embodiments of the present disclosure, the viscosity modifier is one or a combination of methyl cellulose, ethyl cellulose and hydroxyethyl cellulose.

[0019] In some embodiments of the present disclosure, the second organic solvent is a polyol solvent, and the polyol solvent is one or a combination of ethylene glycol, propylene glycol, and polyethylene glycol.

[0020] Furthermore, according to multiple embodiments of the present disclosure, a method for preparing a slurry composition as described above is provided, comprising the following steps: mixing the nano-tin dioxide, the amine-based ionic liquid, the viscosity modifier and the second organic solvent, and stirring to obtain the slurry composition.

[0021] Furthermore, according to various embodiments of the present disclosure, an electron transport film layer is provided, which is produced by screen printing any of the above-mentioned slurry compositions.

[0022] In some embodiments of the present disclosure, the screen printing area of ​​the electron transport film layer is 25 cm 2 ~100cm 2 .

[0023] Furthermore, according to multiple embodiments of the present disclosure, a method for preparing an electron transport film layer is provided, wherein a slurry composition as described above is spread on a silk screen, the slurry composition is allowed to pass through a photosensitive resin, the slurry composition that has passed through the photosensitive resin is spread and deposited on the interface of a screen printing substrate, and the electron transport film layer is formed through heat treatment.

[0024] In some embodiments of the present disclosure, the heat treatment includes: annealing at 150° C. to 200° C. for 5 min to 10 min.

[0025] In some embodiments of the present disclosure, the heat treatment includes: first treating at 80° C. to 100° C. for 15 min to 30 min, and then annealing at 150° C. to 200° C. for 5 min to 10 min.

[0026] In some embodiments of the present disclosure, the mesh size of the silk screen is 200-500 meshes.

[0027] In some embodiments of the present disclosure, the tension of the silk screen is controlled at 25N to 30N.

[0028] In some embodiments of the present disclosure, the thickness of the photosensitive adhesive is 0.2 μm to 1 μm.

[0029] In some embodiments of the present disclosure, the screen printing pressure is 0.06 mPa to 0.1 mPa.

[0030] In some embodiments of the present disclosure, the screen printing speed is 5 cm / s to 25 cm / s.

[0031] In some embodiments of the present disclosure, the distance between the screen plate and the screen printing substrate is adjusted to 0.2 mm to 0.6 mm.

[0032] In some embodiments of the present disclosure, before preparing the electron transport film layer, the screen printing substrate is cleaned with deionized water, dried, and subjected to ultraviolet-ozone treatment.

[0033] Furthermore, according to multiple embodiments of the present disclosure, a perovskite solar cell is provided, comprising a glass substrate or silicon base cell, a first conductive film layer, an electron transport film layer, an interface passivation layer, a perovskite film layer, a hole transport layer, a second conductive film layer and an anti-reflection film layer stacked in sequence, wherein the electron transport film layer is an electron transport film layer as described in any of the above or is prepared by any of the preparation methods described in the above.

[0034] In some embodiments of the present disclosure, the glass substrate is a glass substrate with a temperature resistance of 150° C. to 200° C.

[0035] In some embodiments of the present disclosure, the silicon-based battery is any one of the silicon-based battery with a resistivity of 0.5Ω.cm to 10Ω.cm, the silicon-based battery with a thickness of 80μm to 250μm, the silicon-based battery with an intrinsic layer symmetrically deposited on the front and back surfaces, and the silicon-based battery with an amorphous silicon doped layer coated on the front and back surfaces.

[0036] In some embodiments of the present disclosure, the first conductive film layer and the second conductive film layer are any one of indium tin oxide, antimony-doped tin oxide, and fluorine-doped tin oxide, and each of the first conductive film layer and the second conductive film layer has a visible light transmittance of ≥90% or a sheet resistance of between 6Ω / □ and 8Ω / □.

[0037] In some embodiments of the present disclosure, the thickness of the electron transport film layer is 50 nm to 300 nm.

[0038] In some embodiments of the present disclosure, the thickness of the perovskite thin film layer is 300 nm to 500 nm.

[0039] In some embodiments of the present disclosure, the hole transport layer is NiO x , with a thickness of 20nm to 50nm.

[0040] In some embodiments of the present disclosure, the thickness of the anti-reflection film layer is 80 nm to 140 nm, and the refractive index n value is 1.4 to 1.7.

[0041] Furthermore, according to various embodiments of the present disclosure, a method for preparing a perovskite cell as described above is provided, comprising the following steps:

[0042] Provide glass substrate or silicon substrate cells;

[0043] Preparing a first conductive thin film layer on the glass substrate or silicon base cell;

[0044] preparing an electron transport film layer on the first conductive film layer, wherein the electron transport film layer is formed by screen printing the slurry composition;

[0045] preparing an interface passivation layer and a perovskite thin film layer on the electron transport film layer;

[0046] preparing a hole transport layer on the perovskite thin film layer;

[0047] preparing a second conductive thin film layer on the hole transport layer;

[0048] Preparing an anti-reflection film layer on the second conductive film layer; and,

[0049] Perform post-processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0051] FIG1 is a structural diagram of a perovskite solar cell device provided in Experimental Example 1 of the application.

[0052] FIG2 is a flow chart of a process for preparing a perovskite solar cell device provided in Experimental Example 1 of the application.

[0053] FIG3 is a SEM image of the microscopic interface of a perovskite solar cell device in the experimental comparative example 1 disclosed in the present application.

[0054] FIG4 is an enlarged SEM image of the microscopic interface of a perovskite solar cell device in the experimental comparative example 1 disclosed in the present application.

[0055] FIG5 is a SEM image of the microscopic interface of a perovskite solar cell device in Experimental Example 1 disclosed in this application.

[0056] Icons: 1. Glass substrate; 2. Conductive thin film layer; 3. Electron transport film layer; 41. Interface passivation layer; 42. Perovskite thin film layer; 5. Hole transport layer; 6. Anti-reflection film layer; 71. Conductive positive electrode; 72. Conductive negative electrode. DETAILED DESCRIPTION

[0057] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts shall fall within the scope of protection of the present invention.

[0058] Common electron transport film materials include tin dioxide, titanium dioxide and zinc oxide. Among them, perovskite solar cells prepared with zinc oxide electron transport film have the disadvantages of poor efficiency and stability. The deep energy level traps formed by the surface defects of titanium dioxide electron transport film will recombine with the holes of perovskite, reducing the performance of the device, and titanium dioxide requires high temperature sintering, generally the sintering temperature is greater than 450 ° C, resulting in the perovskite solar cells prepared with titanium dioxide electron transport film usually having a large JV hysteresis effect. Tin dioxide is a wide bandgap direct bandgap semiconductor material with a high mobility of 250cm 2 / (V·s), wide band gap of 3.6eV, good light transmittance, low cost and non-toxicity, so tin dioxide is regarded as an electron transport film material with great development potential.

[0059] Solution spin coating and chemical bath deposition are the main methods for preparing tin dioxide electron transport film layers. The technical principle of solution spin coating is to form a uniform thin film on the substrate when the centrifugal force of the rotating substrate and the viscosity of the solution are in equilibrium. The solution spin coating method has a high waste rate of precursor solution and is prone to severe agglomeration of nanoparticles, so it cannot be applied to large-sized substrates or curved substrates. It also requires annealing at temperatures above 250°C. However, thin film materials annealed at such high temperatures will suffer from problems such as reduced interface contact performance, reduced absorption intensity, accelerated solvent volatilization, and reduced device performance. At the same time, the energy consumption is too high and may also cause damage to the silicon heterojunction bottom cell.

[0060] Chemical bath deposition involves immersing the battery substrate in a solution containing metal ions and hydroxide and selenide ion sources, slowly depositing the film. However, the concentration and pH value of the solution will affect the thin film deposition effect, and it is also prone to severe agglomeration of nanoparticles. The stability and consistency of the deposited film are difficult to control, resulting in increased difficulty in the final photovoltaic device preparation and process control.

[0061] In addition, atomic layer deposition (ALD) is also used to prepare tin dioxide electron transport films. ALD primarily involves alternately introducing pulses of dimethylaminotin and hydrogen peroxide into a reaction chamber, leading to surface chemical reactions on the substrate to form a thin film. Through self-limiting alternating saturation reactions of the precursors, a thin film with highly controllable thickness, composition, morphology, and structure at the nanoscale is obtained. However, ALD is sensitive to substrate purity, and the precursors are expensive. The ALD method also suffers from relatively slow deposition rates and winding issues, making it unsuitable for rapid, large-scale industrial production.

[0062] Based on this, the present application provides a slurry composition and preparation method, an electron transport film and preparation method thereof, and a perovskite solar cell and preparation method thereof. The slurry composition incorporates an amine-based ionic liquid and nano-tin dioxide, which are key to improving the conductivity and mobility of the electron transport film.

[0063] In a first aspect, an embodiment of the present invention provides a slurry composition.

[0064] The slurry composition comprises nano-tin dioxide and amine-based ionic liquid, wherein the molar concentration ratio of the nano-tin dioxide to the amine-based ionic liquid is (0.5-1):(0.5-2), the cation of the amine-based ionic liquid is an amine-based cation, and the anion is an organic acid anion.

[0065] The amine-based ionic liquid and nano-tin dioxide are combined in the above-mentioned concentration ratio. The amine-based ionic liquid has high surface activity and can evenly disperse the nano-tin dioxide in the above-mentioned slurry composition. A huge hydrogen bond network can be formed between the amine-based ionic liquids and the amine-based ionic liquids, and the amine-based ionic liquids are fully connected with the nano-tin dioxide through the hydrogen bond network. At the same time, the oxygen vacancy defects in the nano-tin dioxide are removed. Therefore, the tin dioxide electron transport film layer made from the above-mentioned slurry composition has the advantages of high conductivity, high charge mobility, low work function and high stability, and can improve the photoelectric conversion efficiency of perovskite solar cells.

[0066] For example, the amine-based ionic liquid can be one or more of methylamine formate (C3H7NO2), methylacetamide (C3H9NO2), and methylamine acetate (CH3COONH3). The concentration of nano-tin dioxide can be 0.5mol / L, 0.6mol / L, 0.7mol / L, 0.8mol / L, 0.9mol / L, 1mol / L, etc., and the concentration of the amine-based ionic liquid can be 0.5mol / L, 0.8mol / L, 1mol / L, 1.5mol / L, 2mol / L, etc.

[0067] In some embodiments, the particle size of nano-tin dioxide is distributed between 5 nm and 20 nm.

[0068] The nano-tin dioxide particles are very small, and the slurry composition prepared from them can effectively meet the needs of screen-printing electron transport membranes. Furthermore, nano-tin dioxide of this particle size can fully contact with the amine-based ionic liquid, forming excellent hydrogen bonding with the amine-based ionic liquid, which helps improve transport conductivity and mobility, thereby enhancing the overall performance of battery devices. For example, the particle size of the nano-tin dioxide can be 5nm, 8nm, 10nm, 13nm, 16nm, 18nm, 20nm, etc.

[0069] In some embodiments, a surfactant is added during the preparation of nano-tin dioxide, and the surfactant molecular formula is:

[0070] Among them, the general formula of R is C n H 2n+1 , n can be any of 12, 14, 16 and 18, X - Any one of chlorine, bromine and iodine.

[0071] Since nano-tin dioxide has a large specific surface area and high surface energy, it is in an energy unstable state, and it is easy for particles to agglomerate and aggregate. In order to solve the problem of easy agglomeration of nano-tin dioxide particles, the present application introduces a surfactant of the above structure when preparing nano-tin dioxide, which can produce monodisperse nano-tin dioxide with a particle size as low as 5nm to 20nm, high particle uniformity and excellent dispersibility. This is because nano-tin dioxide is negatively charged during the nucleation process, and the positively charged long-chain alkyl groups in the surfactant of the above structure are easily adsorbed onto the nano-tin dioxide particles to form micelles, which can inhibit the growth of the crystal nucleus and control the morphology of the nano-tin dioxide. Therefore, the nano-tin dioxide particle size obtained after the reaction is lower, at 5nm to 20nm. At the same time, due to the positive charge repulsion effect on the surface of the modified nano-tin dioxide particles, the nano-tin dioxide particles are not easily dispersed and aggregated, the agglomeration problem is greatly improved, and the particle size distribution uniformity and dispersibility are significantly improved. Illustratively, the surfactant is one or a combination of cetyltrimethylammonium bromide, octadecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, dodecyltrimethylammonium bromide, cetyltrimethylammonium chloride, and cetyltrimethylammonium iodide.

[0072] The preparation method of nano tin dioxide is as follows: a surfactant is uniformly mixed with SnCl4·5H2O, an alkali and a first organic solvent, reacted at a pressure of 2MPa to 5MPa and 100°C to 120°C for 20min to 50min, washed and dried to obtain nano tin dioxide.

[0073] Currently, nano-tin dioxide is generally prepared under normal pressure and below 100°C. The reaction for preparing nano-tin dioxide in this application is carried out under conditions of pressure of 2MPa to 5MPa and 100°C to 120°C, which are significantly higher temperatures and pressures. Under these temperatures and pressures, the nano-tin dioxide not only reacts quickly and fully, but the positively charged long-chain alkyl groups in the surfactant can produce an optimal adsorption effect with the negatively charged nano-tin dioxide in the nucleated state, forming micelles, thereby producing nano-tin dioxide with a relatively low particle size, a highly uniform particle size distribution, and excellent dispersibility. After the reaction, the surfactant can be removed by washing to obtain the nano-tin dioxide. For example, the reaction pressure can be 2MPa, 3MPa, 4MPa, or 5MPa; the reaction temperature can be 100°C, 105°C, 110°C, 115°C, or 120°C; and the reaction time can be 20min, 25min, 30min, 35min, 40min, 45min, or 50min. This embodiment does not specifically limit the above process parameters.

[0074] In some embodiments, the first organic solvent is an alcohol solvent, and one or more of ethylene glycol, polyethylene glycol, polypropylene alcohol, isopropyl alcohol, and n-butanol can be selected. The above-mentioned surfactant has a better dissolution effect in alcohol solvents, which is beneficial for controlling the morphology of nano-tin dioxide and preparing nano-tin dioxide particles of uniform size.

[0075] In some embodiments, the base is sodium hydroxide, potassium hydroxide, ammonia water, etc., preferably ammonia water. Sodium hydroxide is a strong alkaline substance. During the dropwise mixing and stirring process, a reaction will occur at room temperature. Subsequent placement in an autoclave system will result in larger nano-tin dioxide particles, which are prone to unevenness. Ammonia water is a weak alkaline substance. The reaction does not readily occur at room temperature. Subsequent placement in an autoclave system and heating to 100°C to 120°C will initiate the reaction. The nano-tin dioxide particles prepared under these conditions have a high degree of uniformity in size.

[0076] In some embodiments, the concentration of the surfactant is 0.1 mol / L to 0.3 mol / L, the concentration of the ammonia water is 1.2 mol / L to 4 mol / L, and the concentration of SnCl4·5H2O is 0.3 mol / L to 1 mol / L. For example, the concentration of the surfactant may be 0.1 mol / L, 0.18 mol / L, 0.21 mol / L, 0.26 mol / L, 0.3 mol / L, etc., the concentration of the ammonia water may be 1.2 mol / L, 1.6 mol / L, 2 mol / L, 2.5 mol / L, 3.2 mol / L, 3.6 mol / L, 4 mol / L, etc., and the concentration of SnCl4·5H2O may be 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, etc. At the above concentration, it is conducive to the reaction of SnCl4·5H2O and ammonia water to form nano-tin dioxide, and it is also conducive to the adsorption of surfactant on the surface of nano-tin dioxide to form micelles, ultimately obtaining nano-tin dioxide with small particle size, uniform particle size distribution and excellent dispersibility.

[0077] In some embodiments, after the reaction is completed, the precipitate is washed and separated using ethanol and then deionized water. This sequential washing with ethanol and deionized water effectively removes surfactants and impurities attached to the surface of the nano-tin dioxide, thereby increasing the purity of the nano-tin dioxide. This facilitates hydrogen bonding between the nano-tin dioxide and the amine-based ionic liquid after subsequent slurrying, thereby improving transmission conductivity and mobility.

[0078] In some embodiments, a viscosity modifier and a second organic solvent are added to the slurry composition, and the viscosity of the slurry composition is 2000cp to 7000cp. For example, the viscosity of the slurry composition can be 2000cp, 3000cp, 4000cp, 5000cp, 6000cp, 7000cp, etc. The viscosity modifier is preferably a cellulose viscosity modifier. For example, the cellulose viscosity modifier can be one or more combinations of methyl cellulose, ethyl cellulose and hydroxyethyl cellulose. Methyl cellulose, ethyl cellulose and hydroxyethyl cellulose have excellent stability, are not likely to cause changes in the acidity and alkalinity of the electron transport film layer slurry composition, and have a more significant effect on increasing the viscosity. The viscosity regulation effect is better, which is conducive to preparing a slurry composition that better meets the viscosity requirements of screen printing.

[0079] In some embodiments, the second organic solvent is a polyol solvent, which may be one or more of ethylene glycol, propylene glycol, and polyethylene glycol. Polyol solvents such as ethylene glycol, propylene glycol, and polyethylene glycol are all relatively viscous liquids. Furthermore, these polyol solvents can effectively dissolve cellulose-based viscosity modifiers. Therefore, combining a polyol solvent with a cellulose-based viscosity modifier can better control the viscosity of the slurry composition according to screen printing requirements.

[0080] In a second aspect, the present invention further discloses a method for preparing the slurry composition according to the first aspect:

[0081] The preparation method of the slurry composition comprises the following steps: mixing nano-tin dioxide, an amine-based ionic liquid, a viscosity regulator and a first solvent, and stirring them uniformly to obtain the slurry composition.

[0082] The preparation method of the slurry composition of the present application is simple, requiring only simple mixing to ensure uniformity, is easy to operate, and is unlikely to affect the activity of the slurry composition, thus being conducive to industrial production.

[0083] In a third aspect, the present invention also discloses an electron transport film layer.

[0084] The electron transport film layer is prepared by screen printing the above-mentioned slurry composition, and the printing area of ​​the electron transport film layer is 25 cm 2 ~100cm 2 .

[0085] The screen printing process has the advantages of flexible pattern design, high production efficiency and fast printing film forming speed. The thickness of the tin oxide film layer can be accurately adjusted by adjusting the printing process parameters, and the size of the tin oxide film can be adjusted to 25cm. 2 ~100cm 2 The electron transport film layer is prepared on a substrate for large-area screen printing, thereby realizing large-area printing of the electron transport film layer, which is suitable for industrialization.

[0086] By screen printing the above-mentioned slurry composition, the obtained electron transport film layer has better thickness uniformity and higher density, and it can be observed through SEM images that the defects of the microscopic interface of the electron transport film layer are significantly reduced, which is beneficial to improving the electron transport efficiency and photoelectric conversion efficiency of perovskite solar cells.

[0087] In a fourth aspect, the present invention also discloses a method for preparing an electron transport film layer.

[0088] The preparation method of the electron transport film layer comprises the following steps: spreading a slurry composition on a silk screen, allowing the slurry composition to pass through a photosensitive adhesive, spreading and depositing the slurry composition that has passed through the photosensitive adhesive on the interface of a silk screen printing substrate, and forming an electron transport film layer through heat treatment.

[0089] In some embodiments, the heat treatment is annealing at 150° C. to 200° C. for 5 min to 10 min.

[0090] The annealing temperature for preparing the electron transport film layer in the present application is lower than 200°C, while the annealing temperature for preparing the electron transport film layer by the current solution spin coating method is generally above 250°C. It can be seen that the annealing temperature for preparing the electron transport film layer in the present application is significantly lower. Therefore, compared with the solution spin coating method for preparing the electron transport film layer, the present application has the advantages of energy saving and environmental protection. In addition, the electron transport film layer prepared by annealing at less than 200°C in the present application can reduce the defects caused by the annealing temperature being too high on the electron transport film layer. Therefore, the electron transport film layer in the present application has better interface contact and conductivity characteristics, which is beneficial to the improvement of the interface passivation of the perovskite thin film layer in contact with the surface of the electron transport film layer.

[0091] In addition, when the heterojunction silicon base cell is used as a crystalline silicon base cell, the heterojunction silicon base cell uses a silicon-based thin film to form a pn junction. The formation temperature of the silicon-based thin film is 200°C. The maximum process temperature of the film layer subsequently superimposed on the heterojunction silicon base cell exceeds the formation temperature of the silicon-based thin film, and the silicon-based thin film is easily damaged. The annealing temperature of the electron transport film layer of the present application is lower than 200°C, so the heterojunction silicon base cell is not easily damaged or deformed by heat. At the same time, at the annealing temperature of the electron transport film layer, it is beneficial for the heterojunction silicon base cell film to further exert its passivation performance and reduce the interface and internal defects of the heterojunction silicon base cell. Moreover, since the above-mentioned annealing temperature is low, it is not easy to destroy the stability of the crystalline silicon base cell. Therefore, the present application is also suitable for thin crystalline silicon base cells as substrates, which is beneficial to reduce material costs.

[0092] In some embodiments, the heat treatment is a treatment at 80°C to 100°C for 15min to 30min, and then annealing at 150°C to 200°C for 5min to 10min. When treated at 80°C to 100°C for 15min to 30min, the second organic solvent in the slurry composition can be fully volatilized and the volatilization rate is relatively fast, which is conducive to the rapid printing of the electron transport film layer and the acquisition of an electron transport film layer without solvent residue. Exemplarily, the heat treatment temperature can be 80°C, 85°C, 90°C, 95°C, 100°C, and the heat treatment time can be 15min, 20min, 25min, 30min. This embodiment does not specifically limit the above process parameters.

[0093] In some embodiments, the mesh size of the silk screen is 200-500 mesh, and / or the tension of the silk screen is controlled at 25N-30N, and / or the thickness of the photosensitive resin is 0.2μm-1μm, and / or the silk screen printing pressure is controlled at 0.06mPa-0.1mPa, and / or the silk screen printing speed is 5cm / s-25cm / s, and / or the distance between the silk screen and the silk screen printing substrate is adjusted to 0.2mm-0.6mm.

[0094] The electron transport film layer requires a nanometer-level thickness of 50nm to 300nm. To achieve this thickness requirement, the distance between the screen and the screen printing substrate is adjusted and the thickness of the photoresist is reduced. To improve the uniformity of the printed film thickness, a relatively slow printing speed and low printing pressure are adopted. By controlling the mesh size and tension of the screen and the hardness of the squeegee, the thickness of the electron transport film can be better controlled, achieving improved uniformity and stability.

[0095] For example, the screen can be 200 mesh, 300 mesh, 400 mesh, or 500 mesh; the screen tension can be 25N, 26N, 27N, 28N, 29N, or 30N; the photosensitive resin thickness can be 0.2 μm, 0.3 μm, 0.4 μm, 0.6 μm, 0.8 μm, or 1 μm; the scraper hardness can be 55HS, 58HS, 62HS, 65HS, 67HS, or 70HS; and the screen printing pressure can be 0.0 The pressure can be 6mPa, 0.07mPa, 0.08mPa, 0.09mPa, 0.1mPa, the screen printing speed can be 5cm / s, 8cm / s, 10cm / s, 12cm / s, 15cm / s, 18cm / s, 20cm / s, 22cm / s, 25cm / s, and the distance between the screen and the conductive film layer can be 0.2mm, 0.3mm, 0.4mm, 0.5mm, 0.6mm. This embodiment does not specifically limit the above process parameters.

[0096] In some embodiments, before screen printing the electron transport film layer, the screen printing substrate needs to be cleaned with deionized water, dried, and subjected to UV-ozone treatment.

[0097] Deionized water washing and drying treatment can effectively reduce surface pollutants and solid attachments on the screen printing substrate. Ultraviolet irradiation decomposition can remove surface organic impurities, physically adsorbed and chemically adsorbed pollutants to a certain extent, obtaining a low-defect conductive layer and interface contact layer, greatly reducing contact interface contamination. The amino ions in the slurry composition are not easy to lose their activity, and the impurity recombination centers are reduced, which is conducive to the deposition of the slurry composition to form a low-defect thin film, thereby improving the efficiency of perovskite solar cell devices and ensuring process repeatability.

[0098] In a fifth aspect, the present invention also discloses a perovskite solar cell.

[0099] The perovskite solar cell comprises: a glass substrate or silicon base cell, a first conductive film layer, the electron transport film layer, an interface passivation layer, a perovskite film layer, a hole transport layer, a second conductive film layer and an anti-reflection film layer stacked in sequence.

[0100] The electron transport film layer contains an amine-based ionic liquid component, which can form a coordination effect with the subsequently deposited perovskite film layer. The amine-based ionic liquid reacts with the iodide ions of the perovskite film layer by chelation, and the acid anions react with lead, thereby forming an interface passivation layer at the contact interface between the electron transport film layer and the perovskite film layer. This interface passivation layer serves as a growth substrate for the subsequent perovskite film layer, effectively regulating the perovskite crystallization kinetics, slowing down the perovskite crystallization rate, and promoting the grain growth of the perovskite film layer, thereby obtaining a perovskite film layer with good crystallization quality, a smooth surface, low defect density, and excellent electron generation and transport performance, which is beneficial to improving the device's interface passivation and transport capabilities. In addition, the electron transport film layer with uniform thickness and excellent density has good interface contact performance with the first conductive film layer and the perovskite film layer, which is beneficial to electron transport, improving the photoelectric conversion efficiency and the overall performance of the battery device.

[0101] In some embodiments, the glass substrate is a glass substrate with a temperature resistance of 150°C to 200°C, and / or the silicon-based battery is any one of a silicon-based battery with a resistivity of 0.5Ω.cm to 10Ω.cm, a silicon-based battery with a thickness of 80μm to 250μm, a silicon-based battery with an intrinsic layer symmetrically deposited on the front and back sides, and a silicon-based battery with an amorphous silicon doped layer coated on the front and back sides, and / or the first conductive film layer and the second conductive film layer are any one of indium tin oxide, antimony-doped tin oxide and fluorine-doped tin oxide, and the visible light transmittance of the first conductive film layer and the second conductive film layer is ≥90% or the square resistance is between 6Ω / □ and 8Ω / □, and / or the thickness of the electron transport film layer is 50nm to 300nm, and / or the thickness of the perovskite film layer is 300nm to 500nm, and / or the hole transport layer is NiO x , the thickness is 20nm~50nm, and / or the thickness of the anti-reflection film layer is 80nm~140nm, and the refractive index n value is 1.4~1.7.

[0102] In a sixth aspect, the present invention further discloses a method for preparing a perovskite solar cell as in the fifth aspect:

[0103] The preparation method of perovskite solar cell comprises the following steps:

[0104] Provide glass substrate or silicon substrate cells;

[0105] Preparing a first conductive thin film layer on a glass substrate or a silicon substrate cell;

[0106] preparing the electron transport film layer on the first conductive film layer;

[0107] co-preparing an interface passivation layer and a perovskite thin film layer on the electron transport film layer;

[0108] preparing a hole transport layer on the perovskite thin film layer;

[0109] preparing a second conductive thin film layer on the hole transport layer;

[0110] preparing an anti-reflection film layer on the second conductive film layer;

[0111] Post-processing is performed to obtain perovskite solar cells.

[0112] In some embodiments, the method of jointly preparing an interface passivation layer and a perovskite thin film layer includes: spin-coating lead iodide and methylamine iodide onto the electron transport film layer, and annealing to obtain the interface passivation layer and the perovskite thin film layer.

[0113] Specifically, lead iodide and methylamine iodide are first configured into a methylamine lead iodine-based perovskite precursor solution with a concentration of 0.8 mol / L, and then a spin coating deposition operation is performed, with the molar ratio of lead iodide to methylamine iodine being 1:1.

[0114] In some embodiments, the conductive positive electrode and the conductive negative electrode are prepared by evaporation or screen printing.

[0115] The conductive positive electrode and the conductive negative electrode can be deposited by evaporation, but this method has a long evaporation time and high cost when used for deposition on large-area substrates.

[0116] The conductive positive electrode and the conductive negative electrode can also be prepared by screen printing. The preparation of the conductive positive electrode by screen printing includes the following steps:

[0117] According to the designed electrode pattern, a conductive positive electrode slurry for screen printing is printed on the second conductive film layer, and cured at a curing temperature of 100°C to 180°C for 1h to 4h to obtain a conductive positive electrode;

[0118] The method for preparing a conductive negative electrode by screen printing comprises the following steps:

[0119] According to the designed electrode pattern, the conductive negative electrode slurry for screen printing is printed on the first conductive film, and the conductive negative electrode is obtained by curing at a curing molding temperature of 100° C. to 180° C. for 1 hour to 4 hours.

[0120] In some embodiments, the conductive positive electrode paste for screen printing is a silver paste with a temperature below 220°C or a silver-clad copper paste with a temperature below 220°C, and / or the conductive negative electrode paste for screen printing is a silver paste with a temperature below 220°C or a silver-clad copper paste with a temperature below 220°C, and / or the screen printing screen uses a stainless steel screen, a nylon screen or a polyurethane screen, and / or the mesh number of the screen plate is 250 mesh to 500 mesh, and / or the screen printing film layer thickness of the conductive positive electrode and / or the conductive negative electrode is 2μm to 12μm, and / or the grid line width of the conductive positive electrode and / or the conductive negative electrode is 0.02mm to 0.2mm.

[0121] In some embodiments, a first conductive thin film layer is deposited on a glass substrate or a silicon-based battery by physical vapor deposition; and / or, an electron transport film layer is screen-printed on the first conductive thin film layer; and / or, a hole transport layer is magnetron sputtered on the perovskite thin film layer; and / or, a second conductive thin film layer is deposited on the hole transport layer by physical vapor deposition; and / or, an anti-reflection film layer is evaporated on the second conductive thin film layer.

[0122] The technical solution of the present invention will be further described below in conjunction with embodiments and drawings.

[0123] Example 1

[0124] Example 1 of the present application provides a slurry composition comprising nano-tin dioxide, methylammonium formate ionic liquid, methylcellulose, and glycerol, wherein the concentration of nano-tin dioxide is 0.8 mol / L, the concentration of methylammonium formate ionic liquid is 1 mol / L, and the concentration of methylcellulose is 0.2 mol / L.

[0125] Nano-tin dioxide is a monodisperse nano-tin dioxide with a particle size distribution of 5nm to 20nm, which is prepared by the following preparation method:

[0126] SnCl4·5H2O was dissolved in polyethylene glycol, and ammonia water was slowly added dropwise, followed by the addition of cetyltrimethylammonium bromide. The mixture was stirred at room temperature and a rotation speed of 200 rpm for 1 hour to obtain a mixed solution with a SnCl4 concentration of 0.5 mol / L, an ammonia concentration of 2 mol / L, and a cetyltrimethylammonium bromide concentration of 0.2 mol / L. The mixed solution was transferred to an autoclave, the pressure was controlled to 3.5 MPa, and the reaction was carried out at 110°C for 35 minutes. The reaction was then cooled to room temperature, and the separated precipitate was washed with ethanol and deionized water in sequence, and the precipitate was dried in a vacuum atmosphere to obtain nano-tin dioxide.

[0127] A method for preparing a slurry composition comprises dissolving nano-tin dioxide in glycerol, adding methylammonium formate ionic liquid, and then adding methyl cellulose, and continuously stirring at 500 rpm for 6 hours to prepare a slurry composition with a viscosity of 6000 cp.

[0128] Example 2

[0129] Example 2 of the present application provides a slurry composition. Compared with Example 1, the concentration of nano-tin dioxide is 0.5 mol / L, and the concentration of methylammonium formate ionic liquid is 0.5 mol / L.

[0130] Example 3

[0131] Example 3 of the present application provides a slurry composition. Compared with Example 1, the concentration of nano-tin dioxide is 1 mol / L, and the concentration of methylammonium formate ionic liquid is 2 mol / L.

[0132] Example 4

[0133] Example 4 of the present application provides a slurry composition. Compared with Example 1, during the preparation process of nano-tin dioxide in this example, the pressure is normal pressure and the temperature is 110°C.

[0134] Example 5

[0135] Example 5 of the present application provides a slurry composition. Compared with Example 1, during the preparation of nano-tin dioxide in this example, the pressure is controlled to be 3.5 MPa and the temperature is controlled to be 75°C.

[0136] Example 6

[0137] Example 6 of the present application provides a slurry composition. Compared with Example 1, during the preparation of nano-tin dioxide in this example, the pressure is controlled to be 3.5 MPa and the temperature is controlled to be 120°C.

[0138] Experimental Example 7

[0139] Example 7 of the present application provides a slurry composition. Compared with Example 1, commercially available nano-tin dioxide with an average particle size of 120 nm is used to replace the nano-tin dioxide in Example 1.

[0140] Comparative Example 1

[0141] The comparative example of the present application provides a slurry composition. Compared with Example 1, the concentration of nano-tin dioxide is 1.2 mol / L, and the concentration of methylammonium formate ionic liquid is 0.3 mol / L.

[0142] Application Example 1

[0143] This application example 1 provides an electron transport film layer, and the preparation method of the electron transport film layer includes the following steps:

[0144] The silk screen screen uses 300 mesh, the silk screen screen tension is controlled at 28N, the photosensitive resin thickness is controlled at 0.5μm, the slurry composition of Example 1 is poured into the silk screen screen, and the slurry is spread on the screen using a scraper with a hardness of 65HS. The silk screen printing pressure is controlled at 0.08mPa, the printing speed is 15cm / s, and the spacing between the silk screen and the silk screen printing substrate is adjusted to 0.4mm. The scraper is dragged from the top to the bottom of the conductive film layer at a constant speed to drive the conductive paste through the photosensitive resin, and the slurry composition is spread and deposited on the interface of the silk screen printing substrate. It is then transferred to a 90°C oven for heat treatment for 22min. The printing substrate coated with the electron transport film layer after heat treatment is placed in an annealing furnace at 150°C and annealed for 5min under a nitrogen protective gas atmosphere to form a 180nm thick tin dioxide electron transport film layer with an amino ionic liquid modified on the surface.

[0145] Application Example 2

[0146] This application example 2 provides an electron transport film layer, which differs from the application example 1 in that the slurry composition prepared in example 1 is replaced by the slurry composition prepared in example 2.

[0147] Application Example 3

[0148] This application example three provides an electron transport film layer, which differs from the application example one in that the slurry composition prepared in example three is used to replace the slurry composition prepared in example one.

[0149] Application Example 4

[0150] This application example 4 provides an electron transport film layer, which differs from the application example 1 in that the slurry composition prepared in Example 4 is used to replace the slurry composition prepared in Example 1.

[0151] Application Example 5

[0152] This application example 5 provides an electron transport film layer, which differs from the application example 1 in that the slurry composition prepared in example 5 is used to replace the slurry composition prepared in example 1.

[0153] Application Example 6

[0154] This application example 6 provides an electron transport film layer, which differs from the application example 1 in that the slurry composition prepared in example 6 is used to replace the slurry composition prepared in example 1.

[0155] Application Example 7

[0156] This application example 7 provides an electron transport film layer, which differs from the application example 1 in that the slurry composition prepared in Example 7 is used to replace the slurry composition prepared in Example 1.

[0157] Application Comparative Example 1

[0158] Comparative Example 1 of this application provides an electron transport film layer prepared by spin coating a nano-tin dioxide solution. The method comprises the following steps: dispersing the nano-tin dioxide particles of Example 1 in an ethanol solvent to form a solution with a nano-tin dioxide concentration of 0.8 mol / L. The solution is then spin-coated on a spin coater to produce an electron transport film layer having a thickness of 180 nm. After spin coating, the solution is annealed at 200°C for 30 minutes and cooled to room temperature to obtain the tin dioxide electron transport film layer.

[0159] Application Comparative Example 2

[0160] Comparative Example 2 of this application provides an electron transport film layer. Compared with Application Example 1, the slurry composition of Comparative Example 1 is used to replace the slurry composition of Application Example 1.

[0161] Experimental Example 1

[0162] This experimental example 1 provides a perovskite solar cell, with reference to FIG1 , and a method for preparing the perovskite solar cell includes the following steps, with reference to FIG2 :

[0163] Provide glass substrate with temperature resistance of 150℃;

[0164] On a glass substrate, a double-sided indium tin oxide conductive film layer with a visible light transmittance of ≥90% and a sheet resistance of 6Ω / □ is deposited by physical vapor deposition;

[0165] Preparation of a tin dioxide electron transport film layer on the indium tin oxide conductive film layer:

[0166] To screen-print large-area, flat films, cut the glass substrate into equal-length sizes. Avoid damaging the surface and edge conductive film layers of the glass or silicon substrate, as well as the internal membrane structure, during the cutting process. Gently wipe the edges of the cut glass substrates with a dust-free cloth moistened with anhydrous ethanol. Then, rinse them with deionized water. After rinsing, blow dry the glass substrate with an N2 air gun and place it in a clean container until ready for use. Place the glass substrate in a UV-ozone cleaner, with the conductive surface facing up, for ozone treatment, where the screen-printed ETL electron transport film will be printed.

[0167] An electron transport film layer is prepared by using the preparation method of the electron transport film layer in Application Example 1;

[0168] Preparation of a perovskite thin film layer on the electron transport film layer: In a glove box, 26.7 g of lead iodide (PbI2) and 9.2 g of methylamine iodide (MA) in a molar ratio of 1:1 were weighed and dissolved in 60 ml of dimethylformamide (DMF) solution. The mixture was stirred with a magnetic stirrer at 60°C for more than 4 hours until the solid powder was completely dissolved to obtain a transparent precursor solution of methylamine lead iodide-based perovskite (MAPbI3 / DMF) solution with a concentration of 0.8 mol / L. The precursor solution was then spin-coated onto the electron transport film layer of tin oxide at a speed of 20 mm / s and annealed at 90°C for 10 minutes to form an interface passivation layer and a perovskite thin film layer with a film thickness of 400 nm.

[0169] 35nm NiO was prepared by magnetron sputtering on the perovskite film layer. x hole transport layer;

[0170] Depositing an indium tin oxide conductive film layer with a visible light transmittance of ≥90% and a sheet resistance of 7Ω / □ on the hole transport layer by physical vapor deposition;

[0171] A conductive positive electrode and a conductive negative electrode are prepared on the conductive film layer by using an evaporation process;

[0172] An anti-reflection film layer is prepared on the conductive positive electrode by using an evaporation process. The material of the anti-reflection film layer is MgF2, the thickness is 110 nm, and the refractive index n value is 1.55.

[0173] Experimental Example 2

[0174] This experimental example provides a perovskite solar cell. Compared with the experimental example 1, the electron transport film layer of the application example 2 is used to replace the electron transport film layer of the application example 1.

[0175] Experimental Example 3

[0176] This experimental example provides a perovskite solar cell. Compared with the experimental example 1, the electron transport film layer of the application example 3 is used to replace the electron transport film layer of the application example 1.

[0177] Experimental Example 4

[0178] This experimental example provides a perovskite solar cell. Compared with Experimental Example 1, the electron transport film layer of Application Example 4 is used to replace the electron transport film layer of Application Example 1.

[0179] Experimental Example 5

[0180] This experimental example provides a perovskite solar cell. Compared with Experimental Example 1, the electron transport film layer of Application Example 5 is used to replace the electron transport film layer of Application Example 1.

[0181] Experimental Example 6

[0182] This experimental example provides a perovskite solar cell. Compared with Experimental Example 1, the electron transport film layer of Application Example 6 is used to replace the electron transport film layer of Application Example 1.

[0183] Experimental Example 7

[0184] This experimental example provides a perovskite solar cell. Compared with Experimental Example 1, the electron transport film layer of Application Example 7 is used to replace the electron transport film layer of Application Example 1.

[0185] Experimental Example 8

[0186] This experimental example provides a perovskite solar cell. Compared to Experimental Example 1, a conductive positive electrode and a conductive negative electrode are prepared on a conductive film layer using screen printing. A stainless steel screen is used for screen printing according to the designed electrode pattern. The screen mesh is 350 mesh, the screen-printed film layer thickness is 7μm, and Ag with a grid line width of 0.1mm serves as the conductive positive and negative electrodes. The printed conductive electrodes are formed and cured at a temperature of 150°C for 2 hours. The conductive positive electrode forms an ohmic contact with the indium tin oxide conductive film layer of the perovskite solar cell's positive electrode, and the conductive negative electrode forms an ohmic contact with the indium tin oxide conductive film layer of the perovskite solar cell's negative electrode.

[0187] Comparative Example 1

[0188] This experimental example provides a perovskite solar cell. Compared with Experimental Example 1, the electron transport film layer of Application Example 1 is replaced by the electron transport film layer of Application Example 1.

[0189] Comparative Example 2

[0190] This experimental example provides a perovskite solar cell. Compared with the experimental example 1, the electron transport film layer of the comparative example 2 is used to replace the electron transport film layer of the application example 1.

[0191] Experiment 1

[0192] The surface morphology of the perovskite solar cells of Experimental Example 1 and Comparative Example 1 was characterized using a scanning electron microscope. The test details are shown in Figures 3 to 5.

[0193] As can be seen from Figure 5, the surface density of the electron transport film layer prepared in Experimental Example 1 is good and there are no pinhole defects. Combined with Figure 3, it can be seen that the surface of the electron transport film layer prepared in Experimental Comparative Example 1 has obviously more defect pinholes of different sizes. The density in the field of view in the figure represents the number of defects contained in one square centimeter, and the density in the field of view is 11000 / cm 2, it can be seen that the number of defects in the electron transport film layer of experimental comparative example 1 is very large. Figure 4 is an enlarged partial area view of Figure 3. By observing Figure 4, it can be seen that the surface of the electron transport film layer has obvious white hole defects and even smaller impurity defects. This proves that compared with the traditional solution spin coating method for preparing electron transport film layers, the number of defects in the electron transport film layer prepared by screen printing the slurry composition is significantly reduced, which is conducive to the preparation of electron transport film layers with uniform thickness and flatness, thereby improving the performance and contact performance of the electron transport film layer itself, and thus improving the photoelectric conversion efficiency of perovskite solar cells.

[0194] Experiment 2

[0195] The open circuit voltage (Voc), short circuit current density (Jsc), fill factor (FF), and photoelectric conversion efficiency (Eff) of the perovskite solar cells prepared in the above experimental examples and comparative examples were measured using a Halm test and sorting device. The test results are detailed in Table 1.

[0196] Table 1

[0197] It can be concluded from Table 1 that the perovskite solar cell prepared in Experimental Example 1 has an open circuit voltage Voc 4.4% higher, a short circuit current density Jsc 4.9% higher, a fill factor FF 4.6% higher, and a photoelectric conversion efficiency Eff 14.3% higher than that of the comparative example 1, which proves that compared with the electron transport film layer prepared by solution spin coating, the electron transport film layer prepared by screen printing in this application has fewer defects and the photoelectric conversion efficiency of the perovskite solar cell is higher.

[0198] Combined with Figure 5, it can be seen that the surface density of the electron transport film layer prepared in Experimental Example 1 is good and there are no pinhole defects. Combined with Figure 3, it can be seen that the surface of the electron transport film layer prepared in Experimental Comparative Example 1 has obviously more defect pinholes of different sizes. The density in the field of view in the figure represents the number of defects contained in one square centimeter, and the density in the field of view is 11000 / cm 2 , it can be seen that the number of defects in the electron transport film layer of experimental comparative example 1 is very large. Figure 4 is an enlarged partial area view of Figure 3. By observing Figure 4, it can be seen that the surface of the electron transport film layer has obvious white hole defects and even smaller impurity defects. This proves that compared with the traditional solution spin coating method for preparing electron transport films, the number of defects in the electron transport film layer prepared by screen printing the slurry composition is significantly reduced, which is conducive to the preparation of a uniform and flat electron transport film layer, thereby improving the performance of the electron transport film layer itself and the contact performance, thereby improving the photoelectric conversion efficiency of the perovskite solar cell.

[0199] The perovskite solar cell prepared in Experimental Example 1 has an open circuit voltage Voc 3.6% higher, a short circuit current density Jsc 5.3% higher, a fill factor FF 4.4% higher, and a photoelectric conversion efficiency Eff 13.9% higher than that of the experimental comparative example 2, which proves that controlling the dosage ratio of nano-tin dioxide and amine-based ionic liquid has a significant influence on the connection effect between the hydrogen bonds formed by nano-tin dioxide and amine-based ionic liquid, which is the key to improving the transmission conductivity and mobility of the electron transport film layer, thereby helping to improve the performance of perovskite solar cells.

[0200] The perovskite solar cell prepared in Experimental Example 1 has an open circuit voltage 0.71% higher, a short circuit current density Jsc 0.73% higher, a fill factor FF 0.57% higher, and a photoelectric conversion efficiency Eff 2.04% higher than that of Experimental Example 4. The perovskite solar cell prepared in Experimental Example 1 has an open circuit voltage 0.08% higher, a short circuit current density Jsc 0.26% higher, a fill factor FF 0.89% higher, and a photoelectric conversion efficiency Eff 1.27% higher than that of Experimental Example 5. The perovskite solar cell prepared in Experimental Example 1 has an open circuit voltage 0.08% higher, a short circuit current density Jsc 0.26% higher, a fill factor FF 0.89% higher, and a photoelectric conversion efficiency Eff 1.27% higher than that of Experimental Example 7. 55%, the short-circuit current density Jsc is 2.82% higher, the fill factor FF is 1.3% higher, and the photoelectric conversion efficiency Eff is 4.73% higher. It can be seen that the nano-tin dioxide prepared under higher temperature and higher pressure conditions has a smaller particle size, higher uniformity, and better dispersion. This proves that the hydrogen bond network connection effect formed by the nano-tin dioxide prepared under the conditions of higher temperature and pressure and the amino-based ionic liquid is better, the transmission conductivity and mobility of the electron transport film layer are improved, and it is more beneficial to improving the performance of perovskite solar cells.

[0201] The above is a detailed introduction to the slurry composition and preparation method, electron transport film layer and preparation method, perovskite solar cell and preparation method disclosed in the embodiments of the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the slurry composition and preparation method, electron transport film layer and preparation method, perovskite solar cell and preparation method and their core ideas of the present invention: At the same time, for those skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A slurry composition comprising nano-tin dioxide and an amine-based ionic liquid, wherein: The molar concentration ratio of the nano-tin dioxide to the amine-based ionic liquid is (0.5-1):(0.5-2), and the cation of the amine-based ionic liquid is an amine-based cation, and the anion is an organic acid radical anion.

2. The slurry composition according to claim 1, wherein the amine-based ionic liquid is one or a combination of methylamine formate, methylamine acetate and methylamine acetate. 3 . The slurry composition according to claim 1 , wherein the particle size of the nano-tin dioxide is distributed between 5 nm and 20 nm.

4. According to any one of claims 1 to 3, a surfactant is added during the preparation of the nano-tin dioxide, and the surfactant molecular formula is: in, The general formula of R is C n H 2n+1 , the value of n is any one of 12, 14, 16 and 18, the value of X - Any one of chlorine, bromine and iodine.

5. The slurry composition according to claim 4, wherein the surfactant is one or a combination of cetyltrimethylammonium bromide, octadecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, dodecyltrimethylammonium bromide, cetyltrimethylammonium chloride and cetyltrimethylammonium iodide.

6. The slurry composition according to claim 4, wherein the preparation method of the nano tin dioxide comprises: The surfactant is mixed evenly with SnCl4·5H2O, alkali and the first organic solvent, reacted at a pressure of 2MPa-5MPa and 100°C-120°C for 20min-50min, washed and dried to obtain the nano-tin dioxide. 7 . The slurry composition according to claim 6 , wherein the first organic solvent is an alcohol solvent, and the alcohol solvent is one or a combination of ethylene glycol, polyethylene glycol, polypropylene alcohol, isopropyl alcohol and n-butyl alcohol.

8. The slurry composition according to any one of claims 6 to 7, wherein the alkali is one or a combination of sodium hydroxide, potassium hydroxide and ammonia water.

9. According to the slurry composition according to any one of claims 6 to 8, the concentration of the surfactant is 0.1 mol / L to 0.3 mol / L, the concentration of the alkali is 1.2 mol / L to 4 mol / L, and the concentration of SnCl4·5H2O is 0.3 mol / L to 1 mol / L. 10 . The slurry composition according to claim 6 , wherein after the reaction for preparing the nano-tin dioxide is completed, ethanol and deionized water are used to wash and separate the precipitate. 11 . The slurry composition according to claim 1 , further comprising a viscosity modifier and a second organic solvent, and the viscosity of the slurry composition is 2000 cp to 7000 cp. 12 . The slurry composition according to claim 11 , wherein the viscosity modifier is one or a combination of methyl cellulose, ethyl cellulose and hydroxyethyl cellulose. 13 . The slurry composition according to claim 11 , wherein the second organic solvent is a polyol solvent, and the polyol solvent is one or a combination of ethylene glycol, propylene glycol and polyethylene glycol.

14. A method for preparing the slurry composition according to any one of claims 1 to 13, comprising the following steps: The nano-tin dioxide, the amine-based ionic liquid, the viscosity modifier and the second organic solvent are mixed and stirred to obtain the slurry composition.

15. An electron transport film layer, prepared by screen printing the slurry composition according to any one of claims 1 to 13.

16. The electron transport film according to claim 15, wherein the screen printing area of ​​the electron transport film is 25 cm 2 ~100cm 2 .

17. A method for preparing an electron transport film layer, comprising spreading the slurry composition as described in any one of claims 1 to 13 on a silk screen, allowing the slurry composition to pass through a photosensitive resin, spreading and depositing the slurry composition that has passed through the photosensitive resin on the interface of a screen printing substrate, and forming the electron transport film layer through heat treatment.

18. The preparation method according to claim 17, wherein the heat treatment comprises: Anneal at 150℃~200℃ for 5min~10min.

19. The preparation method according to claim 17, wherein the heat treatment comprises: First treat at 80℃~100℃ for 15min~30min, and then anneal at 150℃~200℃ for 5min~10min.

20. The preparation method according to any one of claims 17 to 19, wherein the mesh size of the silk screen is 200 to 500 meshes.

21. The preparation method according to any one of claims 17 to 20, wherein the tension of the silk screen is controlled at 25N to 30N.

22. The preparation method according to any one of claims 17 to 21, wherein the thickness of the photosensitive resin is 0.2 μm to 1 μm.

23. The preparation method according to any one of claims 17 to 22, wherein the screen printing pressure is 0.06 mPa to 0.1 mPa.

24. The preparation method according to any one of claims 17 to 23, wherein the screen printing speed is 5 cm / s to 25 cm / s. 25 . The preparation method according to claim 17 , wherein the distance between the screen plate and the screen printing substrate is adjusted to 0.2 mm to 0.6 mm. 26 . The preparation method according to claim 17 , wherein before preparing the electron transport film layer, the screen printing substrate is cleaned with deionized water, dried and subjected to ultraviolet-ozone treatment.

27. A perovskite solar cell, comprising a glass substrate or silicon base cell, a first conductive film layer, an electron transport film layer, an interface passivation layer, a perovskite film layer, a hole transport layer, a second conductive film layer and an anti-reflection film layer stacked in sequence, wherein the electron transport film layer is the electron transport film layer as described in any one of claims 15 to 16 or is prepared by the preparation method as described in any one of claims 17 to 25.

28. The perovskite solar cell according to claim 27, wherein the glass substrate is a glass substrate with a temperature resistance of 150°C to 200°C.

29. The perovskite solar cell according to any one of claims 27 to 28, wherein the silicon-based cell is any one of the silicon-based cell with a resistivity of 0.5Ω.cm to 10Ω.cm, the silicon-based cell with a thickness of 80μm to 250μm, the silicon-based cell with an intrinsic layer symmetrically deposited on the front and back surfaces, and the silicon-based cell with an amorphous silicon doped layer coated on the front and back surfaces.

30. According to the perovskite solar cell according to any one of claims 27 to 29, the first conductive film layer and the second conductive film layer are any one of indium tin oxide, antimony-doped tin oxide and fluorine-doped tin oxide, and the visible light transmittance of the first conductive film layer and the second conductive film layer is ≥90% or the sheet resistance is between 6Ω / □ and 8Ω / □.

31. The perovskite solar cell according to any one of claims 27 to 30, wherein the thickness of the electron transport film layer is 50 nm to 300 nm.

32. The perovskite solar cell according to any one of claims 27 to 31, wherein the thickness of the perovskite thin film layer is 300 nm to 500 nm.

33. The perovskite solar cell according to any one of claims 27 to 32, wherein the hole transport layer is NiO x , thickness is 20nm~50nm.

34. The perovskite solar cell according to any one of claims 27 to 33, wherein the thickness of the anti-reflection film layer is 80 nm to 140 nm, and the refractive index n value is 1.4 to 1.

7.

35. A method for preparing a perovskite battery according to any one of claims 27 to 34, comprising the following steps: Provide glass substrate or silicon substrate cells; Preparing a first conductive film layer on the glass substrate or silicon substrate cell; preparing an electron transport film layer on the first conductive film layer, wherein the electron transport film layer is made by screen printing the slurry composition; Co-preparing an interface passivation layer and a perovskite film layer on the electron transport film layer; preparing a hole transport layer on the perovskite thin film layer; preparing a second conductive film layer on the hole transport layer; Preparing an anti-reflection film layer on the second conductive film layer; and, Perform post-processing.

Citation Information

Patent Citations

  • SnO2-doped slurry, preparation method and application thereof

    CN109932401A

  • Slurry composition and preparation method thereof, electron transport film layer and preparation method thereof, perovskite solar cell and preparation method thereof

    CN116634781A

  • Metal complexes based on a bis(2-pyridylmethyl)amine-based scaffold and methods of making the same

    US20170240569A1