Composite flocculant, preparation method therefor and use thereof

By using wetting agents, acids and adsorption bridge agents in the composite flocculant, the problem of the inability to effectively remove silicon powder in different silicon powder cutting fluids in the prior art is solved, and the effect of efficient flocculation precipitation and recycling is achieved.

WO2024245243A1PCT designated stage expired Publication Date: 2024-12-05TIANJIN ZHONGHUAN SEMICON CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/095825
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-28
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing flocculants cannot effectively remove silicon powder from silicon powder cutting liquids of different brands and silicon powder content, resulting in the quality of the silicon wafer being affected and may disrupt the recycling of the cutting liquid.

Method used

A composite flocculant, including wetting agent, acid and adsorption bridge agent, is used to promote flocculation and precipitation of silicon powder by reducing the surface energy and ZETA potential of the silicon powder surface, and form a bridge to achieve efficient flocculation.

Benefits of technology

It realizes efficient flocculation and precipitation of different silicon powder cutting fluids, maintains the stability of other components and indicators of the cutting fluid, facilitates recycling, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024095825_05122024_PF_FP_ABST
    Figure CN2024095825_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a composite flocculant, a preparation method therefor and a use thereof. The composite flocculant comprises a wetting agent, an acid, an adsorption bridging agent, and a solvent. The wetting agent can be in contact with silicon powder in a silicon powder cutting fluid, so that the surface energy and the interfacial tension on the surface of the silicon powder are reduced, thereby facilitating separating the silicon powder from the silicon powder cutting fluid. The acid can release hydrogen ions to act on the surface of the silicon powder, so that the ZETA potential on the surface of the silicon powder is reduced and a low pH environment is provided, thereby promoting silicon powder agglomeration. By means of electrostatic attraction, Van der Waals attractive force and hydrogen bond force, the silicon powder is bridged and connected into flocs by using the adsorption bridging agent, so that the adsorption bridging agent achieves the effect of a bridge and a link between the silicon powders, and flocculation and precipitation of the silicon powder are promoted by means of adsorption and bridging. The composite flocculant has safe ingredients, has low cost, can efficiently flocculate silicon powder in the silicon powder cutting fluid, and would not destroy other original ingredients in the silicon powder cutting fluid and impact fluctuation of indexes in the silicon powder cutting fluid, thereby facilitating cyclic utilization of the cutting fluid, and saving the cost.
Need to check novelty before this filing date? Find Prior Art

Description

Composite flocculant and its preparation method and application

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 31, 2023, with application number 202310651869.1 and application name “Composite flocculant and its preparation method and application”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to, but is not limited to, the technical field of silicon powder cutting fluid treatment, and in particular to a composite flocculant, a method for preparing the composite flocculant, and applications containing the composite flocculant. Background Art

[0003] With the widespread installation of solar panels, demand for solar silicon wafers is steadily increasing. Currently, silicon wafers are typically cut using diamond wire. At a specific linear speed, multiple diamond wires, flushed with silicon powder cutting fluid, grind away silicon material, resulting in a silicon wafer of a certain thickness. This removed silicon material remains in the cutting fluid as micron-sized silicon powder particles. As cutting continues, the silicon powder content in the cutting fluid rapidly increases, impacting wafer quality. Recycling the cutting fluid requires effective removal of the silicon powder.

[0004] Because the silicon powder in the silicon powder cutting fluid is too fine and has a certain viscosity, flocculants are used to flocculate and precipitate the silicon powder before separation. The current flocculants cannot effectively remove silicon powder from silicon powder cutting fluids of different brands, different silicon powder contents, and different indicators, and will also cause fluctuations in the original silicon powder cutting fluid indicators, affecting the recycling of the cutting fluid. Technical Solutions

[0005] In view of this, the embodiments of the present application provide a composite flocculant and a preparation method and application thereof, aiming to improve the problem that the flocculant cannot effectively flocculate and precipitate silicon powder.

[0006] An embodiment of the present application provides a composite flocculant, which includes a wetting agent, an acid, an adsorption bridging agent, and a solvent.

[0007] Optionally, in some embodiments of the present application, the wetting agent includes one or more of polyether compounds and alcohol compounds.

[0008] Optionally, in some embodiments of the present application, the acid includes one or more of hydrochloric acid, citric acid, and nitric acid.

[0009] Optionally, in some embodiments of the present application, the adsorption bridging agent includes one or more of polyquaternary ammonium salt, polyacrylamide, polyacrylic acid, polyvinyl pyrrolidone, polyvinyl alcohol, polymaleic anhydride, and polyethylene glycol; and / or

[0010] The solvent includes water.

[0011] Optionally, in some embodiments of the present application, in the composite flocculant, the mass fraction of the wetting agent is from 0.03% to 0.67%; the mass fraction of the acid is from 0.05% to 0.15%; the mass fraction of the adsorption bridging agent is from 0.08% to 0.2%; and the mass fraction of the solvent is from 98.98% to 99.84%.

[0012] Optionally, in some embodiments of the present application, the wetting agent includes a polyether compound, and the mass fraction of the polyether compound in the composite flocculant is from 0.03% to 0.37%; and / or

[0013] The wetting agent includes an alcohol compound. In the composite flocculant, the mass fraction of the alcohol compound is from 0.1% to 0.3%.

[0014] Optionally, in some embodiments of the present application, the polyether compound includes one or more of acetylene glycol polyoxyethylene ether, alkylphenol polyoxyethylene ether, fatty alcohol amide polyoxyethylene ether, GP type glycerol polyether, and GPE type polyoxyethylene polyoxypropylene glycerol ether.

[0015] Optionally, in some embodiments of the present application, the alcohol compound includes one or more of 2-methyl-2,4-pentanediol, tetramethyldecynediol, and 1,2-propylene glycol.

[0016] Optionally, in some embodiments of the present application, the composite flocculant includes from 0.1% to 0.2% of 2-methyl-2,4-pentanediol, from 0.2% to 0.3% of polyether, from 0.05% to 0.1% of hydrochloric acid, from 0.1% to 0.2% of polyquaternium salt and 99.2% to 99.55% of water.

[0017] Optionally, in some embodiments of the present application, the composite flocculant includes from 0.1% to 0.3% of 2-methyl-2,4-pentanediol, from 0.23% to 0.37% of polyether, from 0.1% to 0.15% of hydrochloric acid, from 0.08% to 0.12% of polyacrylamide and from 99.06% to 99.49% of water.

[0018] Correspondingly, the present application also provides a method for preparing a composite flocculant, comprising: providing a wetting agent, an acid, an adsorption bridging agent and a solvent, and mixing them to obtain the composite flocculant.

[0019] Optionally, in some embodiments of the present application, the mass ratio of the wetting agent, the acid, the adsorption bridging agent and the solvent is 0.03-0.67:0.05-0.15:0.08-0.2:98.98-99.84.

[0020] Optionally, in some embodiments of the present application, the temperature at which the wetting agent, the acid, the adsorption bridging agent and the solvent are mixed is from 30° C. to 50° C.; and / or

[0021] The wetting agent, the acid, the adsorption bridging agent and the solvent are mixed for 2 to 3 hours; and / or

[0022] The process of mixing the wetting agent, the acid, the adsorption bridging agent and the solvent further includes performing a first stirring, and the rotation speed of the first stirring is from 500 r / min to 1000 r / min.

[0023] Accordingly, the present application also provides a method for extracting silicon powder from silicon powder cutting fluid, comprising:

[0024] Providing a silicon powder cutting fluid, wherein the silicon powder cutting fluid contains silicon powder;

[0025] Adding the composite flocculant to the silicon powder cutting fluid, mixing, and allowing to stand to obtain a layered cutting fluid comprising an upper clear liquid and a lower precipitate;

[0026] The lower layer of precipitate is taken out to obtain silicon powder.

[0027] Optionally, in some embodiments of the present application, the volume ratio of the silicon powder cutting fluid to the composite flocculant is from 1000:2.5 to 1000:0.5.

[0028] Optionally, in some embodiments of the present application, the temperature at which the silicon powder cutting fluid and the composite flocculant are mixed is from 20°C to 30°C.

[0029] Optionally, in some embodiments of the present application, the silicon powder cutting fluid and the composite flocculant are mixed for 10 hours to 20 hours.

[0030] Optionally, in some embodiments of the present application, the mixing of the silicon powder cutting fluid and the composite flocculant further includes a second stirring, and the rotation speed of the second stirring is 100 r / min to 130 r / min.

[0031] Optionally, in some embodiments of the present application, the silicon powder cutting fluid and the composite flocculant are allowed to stand for 10 to 20 minutes after mixing. Beneficial effects

[0032] The composite flocculant of the embodiment of the present application includes a wetting agent, an acid and an adsorption bridging agent. The wetting agent can contact the silicon powder in the silicon powder cutting fluid, reduce the surface energy and interfacial tension of the silicon powder surface, and help separate the silicon powder from the silicon powder cutting fluid; the acid can release hydrogen ions, act on the surface of the silicon powder, reduce the zeta potential of the silicon powder surface and provide a low pH environment, which can promote the agglomeration of the silicon powder; the adsorption bridging agent bridges the silicon powder into floccules through electrostatic attraction, van der Waals attraction and hydrogen bonding, acts as a bridge and link between silicon powder and silicon powder, and promotes the flocculation and precipitation of silicon powder through adsorption bridging; the ingredients in the composite flocculant are safe and the cost is low. Through the combined action of the wetting agent, acid and adsorption bridging agent, the silicon powder in the silicon powder cutting fluid can be efficiently flocculated without destroying the fluctuations of other original components and indicators in the silicon powder cutting fluid, thereby facilitating the recycling of the cutting fluid and saving costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. The drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0034] FIG1 is a schematic diagram of a process for extracting silicon powder from silicon powder cutting fluid according to an embodiment of the present application.

[0035] Implementation Methods of the Application

[0036] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. The described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of this application. In addition, it should be understood that the specific embodiments described herein are only used to illustrate and explain the present application and are not intended to limit the present application.

[0037] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be construed as a hard limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numbers within the range. For example, the description of a range from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0038] The technical solution of this application is as follows:

[0039] In a first aspect, an embodiment of the present application provides a composite flocculant, which is mainly used for flocculating and precipitating silicon powder in a silicon powder cutting fluid. The composite flocculant includes a wetting agent, an acid, an adsorption bridging agent, and a solvent.

[0040] The composite flocculant of the present application includes a wetting agent, an acid, an adsorption bridging agent and a solvent. The wetting agent can contact with the silicon powder in the silicon powder cutting fluid, reduce the surface energy and interfacial tension of the silicon powder surface, and help separate the silicon powder from the silicon powder cutting fluid; the acid can release hydrogen ions, act on the surface of the silicon powder, reduce the zeta potential of the silicon powder surface and provide a low pH environment, which can promote the agglomeration of the silicon powder; the adsorption bridging agent bridges the silicon powder into floccules through electrostatic attraction, van der Waals attraction and hydrogen bonding force, acts as a bridge and link between silicon powder and silicon powder, and promotes the flocculation and precipitation of silicon powder through adsorption bridging; the ingredients in the composite flocculant are safe and the cost is low. Through the combined action of the wetting agent, acid and adsorption bridging agent, the silicon powder in the silicon powder cutting fluid can be efficiently flocculated without destroying the fluctuations of other original components and indicators in the silicon powder cutting fluid, thereby facilitating the recycling of the cutting fluid and saving costs.

[0041] In some embodiments, in the composite flocculant, the wetting agent includes one or more of polyether compounds and alcohol compounds.

[0042] In some embodiments, the polyether compound includes one or more of acetylene glycol polyoxyethylene ether, alkylphenol polyoxyethylene ether, fatty alcohol amide polyoxyethylene ether, GP-type glycerol polyether, and GPE-type polyoxyethylene polyoxypropylene glycerol ether. The polyether compound can lubricate the silicon powder in the silicon powder cutting fluid.

[0043] In some embodiments, the alcohol compound includes one or more of 2-methyl-2,4-pentanediol, tetramethyldecynediol, and 1,2-propylene glycol. The alcohol compound can wet and penetrate the silicon powder in the silicon powder cutting fluid. In some embodiments, the acid includes one or more of hydrochloric acid, citric acid, and nitric acid.

[0044] In some embodiments, the adsorbent bridging agent comprises a water-soluble chain polymer.

[0045] In some embodiments, the adsorption bridging agent includes one or more of polyquaternary ammonium salt, polyacrylamide, polyacrylic acid, polyvinyl pyrrolidone, polyvinyl alcohol, polymaleic anhydride, and polyethylene glycol.

[0046] In some embodiments, the solvent comprises water.

[0047] In the composite flocculant, the mass fraction of the wetting agent is from 0.03% to 0.67%, the mass fraction of the adsorption bridging agent is from 0.08% to 0.2%, the mass fraction of the acid is from 0.05% to 0.15%, and the mass fraction of the solvent is from 98.98% to 99.84%.

[0048] The composite flocculant with a matching ratio can efficiently flocculate the silicon powder in the silicon powder cutting fluid without destroying the original other components and index fluctuations in the silicon powder cutting fluid, making it convenient for the recycling of the cutting fluid and saving costs.

[0049] In some embodiments, the mass fraction of the wetting agent in the composite flocculant is from 0.03% to 0.67%, for example, from 0.07% to 0.6%, from 0.1% to 0.55%, from 0.2% to 0.5%, from 0.3% to 0.45%, from 0.35% to 0.38%, etc. Within the above mass fraction range, the separation of silicon powder from the silicon powder cutting fluid is facilitated.

[0050] In some embodiments, the mass fraction of the adsorbent bridging agent in the composite flocculant is from 0.08% to 0.2%, for example, from 0.09% to 0.19%, from 0.1% to 0.18%, from 0.11% to 0.17%, from 0.12% to 0.16%, from 0.13% to 0.15%, etc. Within the above mass fraction range, the adsorbent bridging agent can be adsorbed onto the silicon powder in the silicon powder cutting fluid, causing bridges to form between the silicon powder particles to form large aggregates, thereby achieving flocculation and precipitation of the silicon powder.

[0051] In some embodiments, the mass fraction of the acid in the composite flocculant is from 0.05% to 0.15%, for example, from 0.06% to 0.14%, from 0.07% to 0.13%, from 0.08% to 0.12%, from 0.09% to 0.11%, 0.1%, etc. Within the above mass fraction range, the acid is conducive to releasing hydrogen ions, which act on the surface of the silicon powder, reduce the zeta potential of the silicon powder surface, provide a low pH environment, and promote silicon powder agglomeration.

[0052] When the wetting agent includes a polyether compound, the mass fraction of the polyether compound in the composite flocculant is from 0.03% to 0.37%, for example, from 0.05% to 0.35%, from 0.07% to 0.3%, from 0.1% to 0.27%, from 0.15% to 0.26%, from 0.18% to 0.2%, etc.

[0053] In some embodiments, when the wetting agent includes an alcohol compound, the mass fraction of the alcohol compound in the composite flocculant is from 0.1% to 0.3%, for example, from 0.11% to 0.28%, from 0.12% to 0.26%, from 0.13% to 0.24%, from 0.14% to 0.22%, from 0.16% to 0.2%, etc.

[0054] In at least one embodiment, the wetting agent includes both a polyether compound and an alcohol compound. In other words, the wetting agent is a composite wetting agent formed by a polyether compound and an alcohol compound.

[0055] In some embodiments, the composite flocculant includes from 0.1% to 0.2% 2-methyl-2,4-pentanediol, from 0.2% to 0.3% polyether, from 0.05% to 0.1% hydrochloric acid, from 0.1% to 0.2% polyquaternium salt, and from 99.2% to 99.55% water.

[0056] In other embodiments, the composite flocculant includes from 0.1% to 0.3% 2-methyl-2,4-pentanediol, from 0.23% to 0.37% polyether, from 0.1% to 0.15% hydrochloric acid, from 0.08% to 0.12% polyacrylamide, and from 99.06% to 99.49% water.

[0057] In a second aspect, the present invention also provides a method for preparing a composite flocculant, comprising:

[0058] A wetting agent, an acid, an adsorption bridging agent and a solvent are provided and mixed to obtain a composite flocculant.

[0059] In some embodiments, the mass ratio of the wetting agent, the acid, the adsorption bridging agent and the solvent is:

[0060] 0.03-0.67:0.05-0.15:0.08-0.2:98.98-99.84.

[0061] Within the above-mentioned mass ratio range, the wetting agent, acid and adsorption bridging agent can work together to promote the flocculation and precipitation of silicon powder in the silicon powder cutting fluid.

[0062] In some embodiments, the mass ratio of the wetting agent, the acid, the adsorption bridging agent and the solvent is:

[0063] 0.1-0.5:0.05-0.15:0.08-0.2:98.98-99.84.

[0064] In some embodiments, the mass ratio of the wetting agent, the acid, the adsorption bridging agent and the solvent is:

[0065] 0.03-0.67:0.08-0.1:0.08-0.2:98.98-99.84.

[0066] In some embodiments, the mass ratio of the wetting agent, the acid, the adsorption bridging agent and the solvent is:

[0067] 0.03-0.67:0.05-0.15:0.1-0.15:98.98-99.84.

[0068] In some embodiments, the mass ratio of the wetting agent, the acid, the adsorption bridging agent and the solvent is:

[0069] 0.03-0.67:0.05-0.15:0.08-0.2:99-99.5.

[0070] In some embodiments, the mass ratio of the wetting agent, the acid, the adsorption bridging agent and the solvent is:

[0071] 0.2-0.4:0.05-0.15:0.08-0.2:98.98-99.84.

[0072] In some embodiments, the temperature of the mixture of the wetting agent, acid, adsorption bridging agent and solvent is from 30°C to 50°C, for example, from 32°C to 48°C, from 33°C to 46°C, from 35°C to 44°C, from 36°C to 42°C, from 38 to 40°C, etc.

[0073] In some embodiments, the mixing time of the wetting agent, acid, adsorption bridging agent and solvent is 2 to 3 hours, for example, 2.1 to 2.9 hours, 2.2 to 2.8 hours, 2.3 to 2.7 hours, 2.4 to 2.6 hours, 2.5 hours, etc.

[0074] In some embodiments, the process of mixing the wetting agent, acid, adsorption bridging agent and solvent also includes a first stirring, and the rotation speed of the first stirring is from 500r / min to 1000r / min, for example, from 520r / min to 980r / min, from 550r / min to 950r / min, from 580r / min to 920r / min, 600r / min to 900r / min, 700r / min to 800r / min, etc.

[0075] Thus, within the above-mentioned mixing temperature range, mixing time range and first stirring speed range, the components are fully and evenly mixed, thereby promoting the flocculation of silicon powder.

[0076] The wetting agent, acid, adsorption bridging agent and solvent are mentioned above and will not be described in detail here.

[0077] The preparation method of the composite flocculant of the present application is simple to operate, convenient and efficient, and is conducive to large-scale preparation and application. The prepared composite flocculant has a good flocculation effect on silicon powder in silicon powder cutting fluid, will not affect other components and indicators in the silicon powder cutting fluid, improves the efficiency of flocculating silicon powder, and saves production costs.

[0078] In a third aspect, an embodiment of the present application further provides an application of a composite flocculant in extracting silicon powder from a silicon powder cutting fluid. Referring to FIG. 1 , the method for extracting silicon powder from a silicon powder cutting fluid includes:

[0079] S11, providing a silicon powder cutting fluid, wherein the silicon powder cutting fluid contains silicon powder;

[0080] S12, adding the composite flocculant to the silicon powder cutting fluid, mixing, and allowing to stand to obtain a layered cutting fluid, the layered cutting fluid comprising an upper clear liquid and a lower sediment;

[0081] S13. Take out the lower layer of precipitate to obtain silicon powder.

[0082] In some embodiments, the volume ratio of the silicon powder cutting fluid to the composite flocculant is from 1000:2.5 to 1000:0.5. Within the above volume ratio range, the silicon powder in the silicon powder cutting fluid is effectively flocculated and precipitated.

[0083] In some embodiments, the volume ratio of the silicon powder cutting fluid to the composite flocculant is from 1000:2.4 to 1000:0.6.

[0084] In some embodiments, the volume ratio of the silicon powder cutting fluid to the composite flocculant is from 1000:2.2 to 1000:0.8.

[0085] In some embodiments, the volume ratio of the silicon powder cutting fluid to the composite flocculant is from 1000:2 to 1000:1.

[0086] In some embodiments, the volume ratio of the silicon powder cutting fluid to the composite flocculant is from 1000:1.8 to 1000:1.2.

[0087] In some embodiments, the volume ratio of the silicon powder cutting fluid to the composite flocculant is from 1000:1.6 to 1000:1.4.

[0088] In some embodiments, the temperature of the silicon powder cutting fluid and the composite flocculant is mixed at a temperature of from 20°C to 30°C.

[0089] In some embodiments, the temperature at which the silicon powder cutting fluid and the composite flocculant are mixed is from 21°C to 29°C.

[0090] In some embodiments, the temperature of the silicon powder cutting fluid and the composite flocculant when mixed is from 22°C to 28°C.

[0091] In some embodiments, the temperature of the silicon powder cutting fluid and the composite flocculant when mixed is from 23°C to 27°C.

[0092] In some embodiments, the temperature of the silicon powder cutting fluid and the composite flocculant when mixed is from 24°C to 26°C.

[0093] In some embodiments, the temperature at which the silicon powder cutting fluid and the composite flocculant are mixed is 25°C.

[0094] In some embodiments, the silicon powder cutting fluid and the composite flocculant are mixed for 10 to 20 minutes.

[0095] In some embodiments, the silicon powder cutting fluid and the composite flocculant are mixed for a time ranging from 11 minutes to 19 minutes.

[0096] In some embodiments, the silicon powder cutting fluid and the composite flocculant are mixed for 12 minutes to 18 minutes.

[0097] In some embodiments, the silicon powder cutting fluid and the composite flocculant are mixed for a time ranging from 13 minutes to 17 minutes.

[0098] In some embodiments, the mixing time of the silicon powder cutting fluid and the composite flocculant is from 14 min to 16 min, 15 min.

[0099] In some embodiments, the mixing of the silicon powder cutting fluid and the composite flocculant further includes performing a second stirring, and the rotation speed of the second stirring is from 100 r / min to 130 r / min.

[0100] In this way, within the temperature range of the mixing of the silicon powder cutting liquid and the composite flocculant, the time range of the mixing of the silicon powder cutting liquid and the composite flocculant, and the speed range of the second stirring, it is beneficial for the composite flocculant to fully mix and contact with the silicon powder cutting liquid, effectively act on the silicon powder in the silicon powder cutting liquid, and thus promote the flocculation of the silicon powder.

[0101] In some embodiments, the second stirring speed is from 102 rpm to 128 rpm.

[0102] In some embodiments, the second stirring speed is from 105 rpm to 125 rpm.

[0103] In some embodiments, the second stirring speed is from 108 rpm to 122 rpm.

[0104] In some embodiments, the second stirring speed is from 110 r / min to 120 r / min.

[0105] In some embodiments, the second stirring speed is from 112 rpm to 118 rpm.

[0106] In some embodiments, the silicon powder cutting fluid and the composite flocculant are allowed to stand for 10 to 20 minutes after mixing.

[0107] In some embodiments, the silicon powder cutting fluid and the composite flocculant are allowed to stand for 11 to 19 minutes after mixing.

[0108] In some embodiments, the silicon powder cutting fluid and the composite flocculant are allowed to stand for 12 to 18 minutes after mixing.

[0109] In some embodiments, the silicon powder cutting fluid and the composite flocculant are allowed to stand for 13 to 17 minutes after mixing.

[0110] In some embodiments, the silicon powder cutting fluid and the composite flocculant are allowed to stand for 14 to 16 minutes after mixing.

[0111] In some embodiments, the silicon powder cutting fluid and the composite flocculant are allowed to stand for 15 minutes after mixing.

[0112] The method for extracting silicon powder from silicon powder cutting fluid in the present application is simple to operate, can effectively flocculate and precipitate the silicon powder in the silicon powder cutting fluid, and will not destroy the original cutting fluid components in the silicon powder cutting fluid, which is conducive to the recycling of the cutting fluid.

[0113] The present application will be described in detail below through specific examples. The following examples are only some examples of the present application and are not limitations of the present application.

[0114] Example 1

[0115] This embodiment provides a composite flocculant, comprising 2-methyl-2,4-pentanediol, alkylphenol polyoxyethylene ether, hydrochloric acid, polyquaternary ammonium salt, and water. The preparation method thereof is as follows:

[0116] 1 g of 2-methyl-2,4-pentanediol, 2 g of alkylphenol polyoxyethylene ether, 0.5 g of hydrochloric acid, 1 g of polyquaternium salt and 996.5 g of deionized water were weighed and mixed, and stirred at 30° C. and 500 r / min for 2 h to obtain a composite flocculant.

[0117] Example 2

[0118] This embodiment provides a composite flocculant, including 2-methyl-2,4-pentanediol, acetylene glycol polyoxyethylene ether, polyacrylamide, fatty alcohol amide polyoxyethylene ether, and hydrochloric acid. The preparation method is as follows:

[0119] 1 g of 2-methyl-2,4-pentanediol, 0.3 g of acetylene glycol polyoxyethylene ether, 0.8 g of polyacrylamide, 2 g of fatty alcohol amide polyoxyethylene ether, 1 g of hydrochloric acid and 994.9 g of deionized water were weighed and mixed, and stirred at 30° C. and 500 r / min for 2 h to obtain a composite flocculant.

[0120] Example 3

[0121] This embodiment is basically the same as Example 1, except that the composite flocculant in this embodiment does not contain 2-methyl-2,4-pentanediol.

[0122] Example 4

[0123] This embodiment is basically the same as embodiment 1, except that the composite flocculant in this embodiment does not contain alkylphenol polyoxyethylene ether.

[0124] Example 5

[0125] This embodiment is substantially the same as embodiment 1, except that 2-methyl-2,4-pentanediol is replaced with 1,2-propylene glycol in this embodiment.

[0126] Example 6

[0127] This embodiment is basically the same as Example 1, except that, in this embodiment, the alkylphenol polyoxyethylene ether is replaced by GPE type polyoxyethylene polyoxypropylene glycerol ether.

[0128] Example 7

[0129] This embodiment is substantially the same as embodiment 1, except that hydrochloric acid is replaced by citric acid in this embodiment.

[0130] Example 8

[0131] This embodiment is substantially the same as embodiment 1, except that the polyquaternium salt is replaced with polyvinylpyrrolidone in this embodiment.

[0132] Example 9

[0133] This embodiment is substantially the same as embodiment 1, except that, in this embodiment, 2 g of 2-methyl-2,4-pentanediol and 995.5 g of deionized water are weighed.

[0134] Example 10

[0135] This embodiment is substantially the same as embodiment 1, except that, in this embodiment, 3 g of 2-methyl-2,4-pentanediol and 994.5 g of deionized water are weighed.

[0136] Example 11

[0137] This embodiment is substantially the same as embodiment 1, except that 0.3 g of alkylphenol polyoxyethylene ether and 998.2 g of deionized water are weighed in this embodiment.

[0138] Example 12

[0139] This embodiment is substantially the same as embodiment 1, except that 3.7 g of alkylphenol polyoxyethylene ether and 994.8 g of deionized water are weighed in this embodiment.

[0140] Example 13

[0141] This embodiment is substantially the same as embodiment 1, except that 1 g of hydrochloric acid and 996 g of deionized water are weighed in this embodiment.

[0142] Example 14

[0143] This embodiment is substantially the same as embodiment 1, except that 1.5 g of hydrochloric acid and 995.5 g of deionized water are weighed in this embodiment.

[0144] Example 15

[0145] This embodiment is substantially the same as embodiment 1, except that 0.8 g of polyquaternium salt and 996.7 g of deionized water are weighed in this embodiment.

[0146] Example 16

[0147] This embodiment is substantially the same as embodiment 1, except that 2 g of polyquaternium salt and 995.5 g of deionized water are weighed in this embodiment.

[0148] Application Example 1

[0149] This application example provides a method for flocculating silicon powder. 1000 mL of silicon powder cutting fluid and 0.5 mL of the composite flocculant of Example 1 are mixed, stirred at 100 rpm for 10 min at 25° C., and allowed to stand for 15 min to obtain a layered cutting fluid.

[0150] Application Examples 2 to 16

[0151] Application Examples 2 to 16 are basically the same as Application Example 1, except that the composite flocculants of Examples 2 to 16 are used respectively.

[0152] Application Example 17

[0153] This application example is basically the same as application example 1, except that in this application example, 1000 mL of silicon powder cutting fluid and 1.5 mL of the composite flocculant of example 1 are mixed.

[0154] Application Example 18

[0155] This application example is basically the same as application example 1, except that in this application example, 1000 mL of silicon powder cutting fluid and 2.5 mL of the composite flocculant of example 1 are mixed.

[0156] The thickness of the supernatant liquid of Application Examples 1 to 18 and the silicon powder cutting fluid after standing was measured, and the height of the supernatant liquid was obtained, as shown in Table 1.

[0157] Table 1:

[0158] From Table 1 we can see that:

[0159] The silicon powder cutting fluid without adding the composite flocculant had no stratification, and no supernatant and silicon powder precipitation appeared; while after adding the composite flocculant in Application Examples 1 to 18, supernatant and lower precipitation appeared; it can be seen from Application Examples 3 and 4 that the wetting effect of polyether compounds on silicon powder in silicon powder cutting fluid is better than that of alcohol compounds; it can be seen from Application Examples 1 and 5 to 8 that within the provided material selection range, after replacing the alcohol compound, polyether compound, acid and adsorption bridging agent, the height of the supernatant is not much different, and there is no significant difference in the flocculation effect on silicon powder; it can be seen from Application Examples 1, 5 to 8 that the supernatant has a similar height after replacing the alcohol compound, polyether compound, acid and adsorption bridging agent within the provided material selection range. It can be seen from Application Examples 9 to 16 that, within the provided material dosage range, by using different contents of alcohol compounds, polyether compounds, acids and adsorption bridging agents, the height of the supernatant is ≥9.8 mm, which can effectively flocculate silicon powder; from Application Examples 1, 17 to 18, it can be seen that, within the provided volume ratio range of silicon powder cutting fluid and composite flocculant, the more the composite flocculant is added, the better the flocculation effect on the silicon powder. When the volume ratio of silicon powder cutting fluid and composite flocculant reaches 1000:2.5, the supernatant reaches 30.6 mm, indicating that the composite flocculant effectively flocculates the silicon powder.

[0160] The basic concepts have been described above. For those skilled in the art, the detailed disclosure above is merely illustrative and does not limit the present application. Although not explicitly stated herein, those skilled in the art may make various modifications, improvements, and amendments to the present application. Such modifications, improvements, and amendments are suggested in the present application and remain within the spirit and scope of the exemplary embodiments of the present application.

[0161] It should be noted that, in order to simplify the description of this application and thus facilitate understanding of one or more embodiments, the foregoing descriptions of the embodiments of this application sometimes combine multiple features into a single embodiment, figure, or description thereof. However, this disclosure method does not mean that the subject matter of this application requires more features than those recited in the claims. In fact, the features of an embodiment may be fewer than all the features of a single embodiment disclosed above.

[0162] Each patent, patent application, patent application publication, and other materials, such as articles, books, specifications, publications, and documents, cited in this application is hereby incorporated by reference in its entirety, except for any application history that is inconsistent with or conflicts with this application, and any document (currently or subsequently appended to this application) that limits the broadest scope of the claims of this application. It should be noted that if the descriptions, definitions, and / or terminology used in the accompanying materials are inconsistent with or conflict with the content of this application, the descriptions, definitions, and / or terminology used in this application will control.

Claims

1. A composite flocculant, comprising a wetting agent, an acid, an adsorption bridging agent and a solvent.

2. The composite flocculant according to claim 1, wherein The wetting agent includes one or more of polyether compounds and alcohol compounds.

3. The composite flocculant according to claim 1, wherein The acid includes one or more of hydrochloric acid, citric acid and nitric acid.

4. The composite flocculant according to claim 1, wherein The adsorption bridging agent includes one or more of polyquaternary ammonium salt, polyacrylamide, polyacrylic acid, polyvinyl pyrrolidone, polyvinyl alcohol, polymaleic anhydride, and polyethylene glycol; and / or The solvent includes water.

5. The composite flocculant according to claim 1, wherein In the composite flocculant, the mass fraction of the wetting agent is from 0.03% to 0.67%; The mass fraction of the acid is from 0.05% to 0.15%; The mass fraction of the adsorption bridging agent is from 0.08% to 0.2%; The mass fraction of the solvent is from 98.98% to 99.84%.

6. The composite flocculant according to claim 1, wherein The wetting agent comprises a polyether compound, and in the composite flocculant, the mass fraction of the polyether compound is from 0.03% to 0.37%; and / or The wetting agent includes an alcohol compound. In the composite flocculant, the mass fraction of the alcohol compound is from 0.1% to 0.3%.

7. The composite flocculant according to claim 2 or 6, wherein The polyether compound includes one or more of acetylene glycol polyoxyethylene ether, alkylphenol polyoxyethylene ether, fatty alcohol amide polyoxyethylene ether, GP type glycerol polyether, and GPE type polyoxyethylene polyoxypropylene glycerol ether.

8. The composite flocculant according to claim 2 or 6, wherein The alcohol compound includes one or more of 2-methyl-2,4-pentanediol, tetramethyldecynediol, and 1,2-propylene glycol.

9. The composite flocculant according to claim 1, wherein The composite flocculant comprises from 0.1% to 0.2% of 2-methyl-2,4-pentanediol, from 0.2% to 0.3% of polyether, from 0.05% to 0.1% of hydrochloric acid, from 0.1% to 0.2% of polyquaternary ammonium salt and from 99.2% to 99.55% of water.

10. The composite flocculant according to claim 1, wherein The composite flocculant comprises 0.1% to 0.3% of 2-methyl-2,4-pentanediol, 0.23% to 0.37% of polyether, 0.1% to 0.15% of hydrochloric acid, 0.08% to 0.12% of polyacrylamide and 99.06% to 99.49% of water.

11. A method for preparing a composite flocculant, comprising: A wetting agent, an acid, an adsorption bridging agent and a solvent are provided and mixed to obtain a composite flocculant.

12. The preparation method according to claim 11, wherein The mass ratio of the wetting agent, the acid, the adsorption bridging agent and the solvent is 0.03-0.67:0.05-0.15:0.08-0.2:98.98-99.

84.

13. The preparation method according to claim 11, wherein The temperature at which the wetting agent, the acid, the adsorption bridging agent and the solvent are mixed is from 30° C. to 50° C.; and / or The wetting agent, the acid, the adsorption bridging agent and the solvent are mixed for 2 hours to 3 hours; and / or The process of mixing the wetting agent, the acid, the adsorption bridging agent and the solvent also includes a first stirring, and the rotation speed of the first stirring is from 500 r / min to 1000 r / min.

14. A method for extracting silicon powder from silicon powder cutting fluid, comprising: Providing a silicon powder cutting fluid, wherein the silicon powder cutting fluid contains silicon powder; Adding the composite flocculant according to any one of claims 1 to 10 to the silicon powder cutting liquid, mixing, and standing to obtain a layered cutting liquid, wherein the layered cutting liquid includes an upper clear liquid and a lower precipitate; The lower layer of precipitate is taken out to obtain silicon powder.

15. The method for extracting silicon powder from silicon powder cutting fluid according to claim 14, wherein: The volume ratio of the silicon powder cutting fluid to the composite flocculant is from 1000:2.5 to 1000:0.

5.

16. The method for extracting silicon powder from silicon powder cutting fluid according to claim 14, wherein: The temperature at which the silicon powder cutting fluid and the composite flocculant are mixed is from 20°C to 30°C.

17. The method for extracting silicon powder from silicon powder cutting fluid according to claim 14, wherein: The silicon powder cutting fluid and the composite flocculant are mixed for 10 hours to 20 hours.

18. The method for extracting silicon powder from silicon powder cutting fluid according to claim 14, wherein: The silicon powder cutting fluid and the composite flocculant are mixed together and a second stirring is performed. The rotation speed of the second stirring is from 100 r / min to 130 r / min.

19. The method for extracting silicon powder from silicon powder cutting fluid according to claim 14, wherein: The silicon powder cutting fluid and the composite flocculant are allowed to stand for 10 to 20 minutes after being mixed.

Citation Information

Patent Citations

  • Method of recycling cutting suspension

    CN101032806A

  • Method for preparing flocculating agent for red mud precipitation

    CN101544454A

  • Recovery method for cutting fluid

    CN102071093A

  • Method for nuisanceless resourceful treatment of waste mortar from silicon chip cutting

    CN102167968A

  • Method for purifying silica micropowder through selective flocculation

    CN102211774A