Component-normalized variable-strength dual-phase steel plate and flexible manufacturing method therefor
By controlling the specific element content and microstructure in high-strength steel and combining with flexible manufacturing methods, the shortcomings in the existing high-strength steel in terms of pore reaming performance and elongation are solved, and flexible production of steel types with multiple mechanical properties is achieved. Meet the needs of the automobile manufacturing industry.
Patent Information
- Application Number
- PCT/CN2024/096240
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-05-30
- Publication Date
- 2024-12-05
AI Technical Summary
The existing high-strength steel has shortcomings in hole reaming performance and elongation, which cannot meet the needs of the automobile manufacturing industry for multiple mechanical properties. The existing technology mainly adopts different composition designs and a single manufacturing process, making it difficult to achieve multiple strength levels of steel. flexible production.
Variable strength duplex steel designed with a single chemical composition is used to control the content of elements such as C, Si, Mn, Al, Ti, B, etc. to form a microscope of ferrite + martensite + residual austenite + nanoprecipitates. The structure, combined with flexible manufacturing methods, includes hot rolling, thermal insulation annealing, continuous annealing and tempering processes, adjusting process parameters to obtain steel types of different strength levels, ensuring the generation and distribution of martensite and nanoprecipitates.
The steel plate with tensile strength of 450-1310MPa grade has good forming performance, strong plastic accumulation is greater than 11,000, and porosity retractability is greater than 35%, solving the needs of various mechanical properties, reducing production costs and simplifying the process flow.
Smart Images

Figure PCTCN2024096240-FTAPPB-I100001 
Figure PCTCN2024096240-FTAPPB-I100002 
Figure PCTCN2024096240-FTAPPB-I100003
Abstract
Description
A normalized composition variable strength dual-phase steel plate and its flexible manufacturing method Technical Field
[0001] The present invention relates to a dual-phase steel manufacturing technology, and in particular to a normalized composition variable-strength dual-phase steel plate and a flexible manufacturing method thereof. Background Art
[0002] As the global energy crisis and environmental issues intensify, energy conservation and safety have become key development priorities for the automotive industry. Reducing vehicle weight is one of the key measures to save energy and reduce emissions. Ultra-high-strength steel, with its excellent mechanical and performance properties, is suitable for the manufacture of automotive structural components. Its widespread use can effectively reduce vehicle weight. Demand for ultra-high-strength steel in automotive applications has been increasing in recent years.
[0003] There are many varieties of ultra-high-strength steel used in automobiles. Duplex steel offers excellent strength and ductility, but its hole expansion rate (approximately 20-35%) is far lower than that of traditional mild steel used in automobiles. Bainitic and complex-phase steels, while offering high hole expansion rates, suffer from low elongation. Therefore, developing products with improved hole expansion, while maintaining an elongation no lower than that of duplex steel, should have broad application scenarios.
[0004] The body-in-white requires high-strength steel with a variety of mechanical properties, which traditionally requires different composition designs and manufacturing processes.
[0005] Chinese patent application CN103215516A discloses a high-strength hot-rolled Q&P steel and its manufacturing method. Its chemical composition is as follows: C: 0.15% to 0.40%, Si: 1.0% to 2.0%, Mn: 1.5% to 3.0%, P ≤ 0.015%, S ≤ 0.005%, Al: 0.3% to 1.0%, N ≤ 0.006%, Ti: 0.005% to 0.015%, and the remainder is Fe. The steel exhibits a yield strength ≥ 700 MPa, a tensile strength ≥ 1300 MPa, and an elongation > 10%. This invention, based on the composition of conventional C-Mn steel, increases the Si content to inhibit cementite precipitation, uses a micro-Ti treatment to refine austenite grains, and increases the Al content to accelerate the austenite transformation kinetics during air cooling. Furthermore, a hot rolling process combined with a staged cooling process is used to achieve a microstructure containing proeutectoid ferrite, martensite, and retained austenite. This significantly reduces alloy cost.
[0006] Chinese patent application CN104451436A discloses a bainite-martensite-austenite multiphase wear-resistant steel plate and its manufacturing method. The chemical composition of the steel plate, by weight, is as follows: C: 0.20-0.40; Mn: 0.30-1.50; Si: 0.80-1.20; Cr: 0.60-1.00; Ni: 0.20-0.60; Mo: 0.20-0.40; Cu: 0.20-0.50; B: 0.0005-0.003; S ≤ 0.010, P ≤ 0.015, with the remainder being Fe and unavoidable impurities. The rolled product can obtain a bainite-martensite-retained austenite complex phase structure with a retained austenite volume fraction of 5-15%. The yield strength of the material is greater than 1000MPa, the tensile strength is greater than 1300MPa, the elongation is greater than 15%, the hardness is HB420-500, and the machining and welding properties meet the equipment manufacturing requirements; the abrasive wear resistance is more than 1.3 times that of Hardox450, and more than 1.5 times that of Hardox450 under weakly acidic environment conditions.
[0007] Chinese patent application CN102776438A discloses a niobium-lanthanum microalloyed Mn-B ultra-high-strength steel plate and its heat treatment process, belonging to the technical field of heat treatment of steel materials. The chemical composition and content (by weight percentage) of the steel plate are: C 0.14%-0.35%, Mn 1.5%-2.0%, Si 0.6%-1.0%, P ≤ 0.015%, S ≤ 0.002%, Nb 0.01%-0.06%, B 0.0005%-0.0040%, La 0.001%-0.5%, with the balance being Fe and unavoidable impurities. The heat treatment process includes an austenitizing temperature of 880-940°C for a holding time of 0.5-5 hours, followed by water quenching; and a tempering temperature of 190-250°C for a holding time of 1-15 hours. The steel plates produced by this heat treatment process have excellent mechanical properties, with a tensile strength of 1200-1400MPa, a yield strength of 1000-1300MPa, and an elongation of 6-15%. It has the characteristics of low production cost and can be industrially produced with a thickness of 5-25mm.
[0008] Chinese patent application CN102321841A discloses a track shoe steel with a tensile strength of 1300 MPa. Its chemical composition, by weight, is as follows: C: 0.20-0.30%, Mn: 0.80-1.40%, Si: 0.15-0.35%, P: 0-0.015%, S: 0-0.016%, Cr: 0-0.30%, Ni: 0-0.25%, Cu: 0-0.30%, Ti: 0.01-0.02%, Al: 0.02-0.06%, B: 0.0005-0.0035%, with the remainder being Fe and unavoidable impurities. This track shoe steel boasts a tensile strength exceeding 1340 MPa and an elongation below 12%. The steel's U-notch impact energy absorption exceeds 72 J, demonstrating high strength, minimal quenching cracking and internal cracking, and a long service life.
[0009] It can be seen from the above patent applications that existing high-strength steels all have a single composition design and a corresponding single manufacturing process design.
[0010] The technical solutions described in Chinese patent applications CN103215516A and CN104451436A are to obtain sufficient retained austenite by adding high amounts of Si and Al, and to obtain high elongation by the TRIP effect of the retained austenite, without considering the hole expansion performance.
[0011] The ultra-high strength steels described in Chinese patent applications CN102776438A and CN102321841A respectively achieve good mechanical properties by adding microalloys such as niobium, lanthanum, nickel, cadmium, and copper, but they cannot achieve high elongation and high hole expansion performance indicators.
[0012] Summary of the Invention
[0013] The present invention aims to provide a normalized composition variable-strength dual-phase steel sheet and a flexible manufacturing method thereof. Using a single chemical composition, the steel can be produced to meet the multiple strength levels required for a body-in-white (BIW) structure. The sheet can flexibly achieve a tensile strength of 450-1310 MPa, exhibit good formability, a strength-ductility product greater than 11,000, and a hole expansion ratio greater than 35%. The microstructure of the dual-phase steel comprises ferrite + martensite + retained austenite + nano-precipitates, wherein martensite accounts for more than 30% by volume, and a sufficient amount of retained austenite (greater than 3%) and a sufficient amount of nano-precipitates (nano-precipitates with a size less than 50 nm accounting for greater than 8% by mass of the total precipitates).
[0014] To achieve the above object, the technical solution of the present invention is:
[0015] A duplex steel having the following chemical composition by mass percentage: C: 0.06-0.08%, Si: 0.4-0.6%, Mn: 2.4-2.6%, Al: 0.01-0.05%, Ti: 0.02-0.04%, B: 0.0015-0.0025%, P≤0.015%, S≤0.003%, N≤0.005%, and the balance consisting of Fe and unavoidable impurities;
[0016] The microstructure of the dual-phase steel of the present invention comprises ferrite + martensite + retained austenite + nano-precipitates, wherein the martensite accounts for more than 30% of the volume fraction;
[0017] The dual-phase steel of the present invention has a tensile strength of 450-1310 MPa, a strength-ductility product greater than 11000%, and a hole expansion rate greater than 35%.
[0018] Furthermore, the balance is Fe and inevitable impurities.
[0019] In some embodiments, the dual phase steel of the present invention is a normalized composition variable strength dual phase steel.
[0020] In some embodiments, the nano-precipitates in the dual phase steel of the present invention are ε carbides.
[0021] In some embodiments, the volume fraction of retained austenite in the dual phase steel of the present invention is greater than 3%.
[0022] In some embodiments, the mass fraction of nano-precipitates with a size less than 50 nm in the dual-phase steel of the present invention is greater than 8% of the total precipitates.
[0023] In some embodiments, the yield strength of the dual-phase steel of the present invention is 310 to 1200 MPa.
[0024] In some embodiments, the hole expansion ratio of the dual-phase steel of the present invention is 36-55%.
[0025] In some embodiments, the tensile strength of the dual-phase steel of the present invention is 450-590 MPa, preferably 470-590 MPa, the yield strength is 310-370 MPa, the strength-ductility product is between 12000-14500%, and the hole expansion ratio is 36-40%.
[0026] In some embodiments, the tensile strength of the dual-phase steel of the present invention is 591-980 MPa, preferably 650-980 MPa, the yield strength is 360-580 MPa, the strength-ductility product is between 12500-14700%, and the hole expansion ratio is 45-55%.
[0027] In some embodiments, the tensile strength of the dual-phase steel of the present invention is 981-1310 MPa, preferably 1000-1310 MPa, the yield strength is 600-1200 MPa, the strength-ductility product is between 11500-16000%, and the hole expansion ratio is 40-50%.
[0028] In some embodiments, in the microstructure of the dual-phase steel of the present invention, the volume fraction of martensite is 32-91%, the volume fraction of retained austenite is 4-15%, and the volume fraction of ferrite is 2-65%.
[0029] In some embodiments, the nano-precipitates with a size less than 50 nm account for 9 to 30% of the total precipitates in the dual-phase steel of the present invention. In some embodiments, the nano-precipitates with a size less than 50 nm account for 9 to 28% of the total precipitates in the dual-phase steel of the present invention.
[0030] In the composition design of the variable strength dual phase steel of the present invention:
[0031] C: The addition of C increases steel strength and ensures martensitic transformation. The present invention controls the C content to between 0.06% and 0.08%. This is because when the C content is less than 0.06%, sufficient martensite cannot be generated during annealing, affecting the strength of the steel sheet. When the C content is greater than 0.08%, peritectic reactions occur during continuous casting, making it unsuitable for high-speed continuous casting.
[0032] Si: It has a solid solution strengthening effect, improving the tempering resistance of martensite and inhibiting the precipitation and growth of Fe3C. Especially at high tempering temperatures, Si forms ε carbides, inhibiting Fe3C precipitation. However, it has a negative impact on the steel plate surface. The control range for Si is 0.4-0.6%. If it is less than 0.4%, it is not conducive to inhibiting the precipitation and growth of Fe3C during tempering. If it is above 0.6%, it will easily affect the surface quality.
[0033] Mn: Adding Mn improves the hardenability of steel and effectively increases the strength of the steel plate. The present invention controls the Mn content to 2.4-2.6% because, during the hot-rolled heat preservation hood annealing process, a large amount of carbides is produced, resulting in insufficient carbon equivalent in the matrix structure. When the mass percentage of Mn is less than 2.4%, the insufficient carbon equivalent leads to insufficient hardenability, and sufficient martensite cannot be produced during the annealing process, resulting in insufficient strength of the steel plate. When the mass percentage of Mn exceeds 2.6%, the carbon equivalent increases significantly, negatively affecting welding performance and delayed cracking resistance. Therefore, the Mn content in the present invention is controlled to 2.4-2.6%.
[0034] Al: Adding Al has the effect of deoxidation and grain refinement. Therefore, the content of Al is controlled to be 0.01-0.05% in the present invention.
[0035] Ti: 0.02-0.04% Ti is added because it is the primary compounding element in precipitates and, at high temperatures, strongly inhibits austenite grain growth, thereby refining the grains. However, excessive amounts of carbonitride-forming elements like Nb and Ti in low-carbon steel can affect subsequent phase transformations, so the upper limit of the alloying element content must be controlled.
[0036] Boron (B): Boron is an element that significantly improves hardenability. Adding boron promotes martensite formation, ensuring the strength of martensitic steel. However, after grain boundary defects are completely filled, adding more boron can cause precipitation of "boron phase" at the grain boundaries, reducing plasticity. In the present invention, 0.0015-0.0025% B is added. Below 0.0015% B has insufficient effect, while above 0.0025% B is detrimental to the steel's plasticity.
[0037] In the technical solution described in the present invention, the impurity elements include P, N, and S. The lower the impurity content is controlled, the better the implementation effect is. The P content is controlled at P≤0.015%; MnS formed by S seriously affects the forming performance, so the S content is controlled at S≤0.003%; since N easily causes cracks or bubbles on the surface of the slab, the present invention controls the N content to ≤0.005%.
[0038] The flexible manufacturing method of dual-phase steel according to the present invention comprises the following steps:
[0039] 1) Smelting and casting
[0040] Smelt according to the above ingredients and cast into billets;
[0041] 2) Hot rolling
[0042] When preparing dual-phase steel with a tensile strength of 450-590 MPa, the ingot is heated to 1100-1250°C and kept warm for more than 0.5 hours; the final rolling temperature is controlled at 860-900°C, and the coiling temperature is 231-260°C;
[0043] When preparing dual-phase steel with a tensile strength of 591-980 MPa, the ingot is heated to 1100-1250°C and kept warm for more than 0.5 hours; the final rolling temperature is controlled at 860-900°C, and the coiling temperature is 201-230°C;
[0044] When preparing dual-phase steel with a tensile strength of 981-1310 MPa, the ingot is heated to 1100-1250°C and kept warm for more than 0.5 hours; the final rolling temperature is controlled at 860-900°C, and the coiling temperature is 160-200°C;
[0045] 3) Annealing of hot coil insulation cover
[0046] When preparing duplex steel with a tensile strength of 450-590 MPa, after coiling, a heat preservation cover annealing is used for 0.5-2 hours. The heat preservation cover utilizes the internal heat of the steel coil, and the temperature drop rate per hour is less than 6°C / s.
[0047] When preparing duplex steel with a tensile strength of 591-980 MPa, after coiling, a heat preservation hood annealing is used for 2.1-4 hours. The heat preservation hood utilizes the internal heat of the steel coil, and the temperature drop rate per hour is less than 6°C / s.
[0048] When preparing duplex steel with a tensile strength of 981-1310 MPa, after coiling, a heat preservation hood annealing is used for 4.1-6 hours. The heat preservation hood utilizes the internal heat of the steel coil, and the temperature drop rate per hour is less than 6°C / s.
[0049] 4) Cold rolling, controlling the cold rolling reduction rate to 0-50%;
[0050] 5) Continuous annealing
[0051] When preparing a dual-phase steel with a tensile strength of 450-590 MPa, the annealing temperature is 760-820°C, and the holding time is 50-100 seconds; then the steel is cooled at a rate of 3-10°C / s to the rapid cooling start temperature, which is 660-760°C, and then cooled to room temperature at a rate of 50-150°C / s;
[0052] When preparing a dual-phase steel with a tensile strength of 591-980 MPa, the annealing temperature is 760-820°C, and the holding time is 50-100 seconds; then the steel is cooled at a rate of 3-10°C / s to the rapid cooling start temperature, which is 660-760°C, and then cooled to room temperature at a rate of 151-350°C / s;
[0053] When preparing a dual-phase steel with a tensile strength of 981-1310 MPa, the annealing temperature is 760-820°C, and the holding time is 50-100 seconds; then the steel is cooled at a rate of 3-10°C / s to the rapid cooling start temperature, which is 660-760°C, and then cooled to room temperature at a rate of 351-600°C / s;
[0054] 6) Tempering
[0055] When preparing dual-phase steel with a tensile strength of 450-590 MPa, the tempering temperature is 160-260°C and the tempering time is 0.5-3 h;
[0056] When preparing dual-phase steel with a tensile strength of 591-980 MPa, the tempering temperature is 160-260°C and the tempering time is 2-6 hours;
[0057] When preparing dual-phase steel with a tensile strength of 981 to 1310 MPa, the tempering temperature is 160 to 260°C and the tempering time is 2 to 4 hours;
[0058] 7) Smoothing: using a smoothing rate of 0 to 0.3%.
[0059] Preferably, step 1) is performed by a thin slab continuous casting process.
[0060] Herein, when the cold rolling reduction ratio is 0%, it means that the cold rolling step is not performed.
[0061] In some embodiments, when preparing dual-phase steel with a tensile strength of 450-590 MPa, the holding time in the hot rolling step is 0.5-3.5 hours. When preparing dual-phase steel with a tensile strength of 450-590 MPa, the coiling temperature in the hot rolling step is 232-260°C.
[0062] In some embodiments, when preparing dual-phase steel with a tensile strength of 591-980 MPa, the holding time in the hot rolling step is 0.5-2.5 hours. When preparing dual-phase steel with a tensile strength of 591-980 MPa, the coiling temperature in the hot rolling step is 203-228°C.
[0063] In some embodiments, when preparing a dual-phase steel having a tensile strength of 981 to 1310 MPa, the holding time in the hot rolling step is 1.2 to 3.2 hours.
[0064] In some embodiments, in the hot coil insulation cover annealing step, when preparing a dual-phase steel with a tensile strength of 450 to 590 MPa, the annealing time is 0.5 to 2 hours; when preparing a dual-phase steel with a tensile strength of 591 to 980 MPa, the annealing time is 2.2 to 4 hours; when preparing a dual-phase steel with a tensile strength of 981 to 1310 MPa, the annealing time is 4.3 to 6 hours.
[0065] In some embodiments, in the continuous annealing step, when preparing a dual-phase steel with a tensile strength of 450 to 590 MPa, the steel is cooled to room temperature at a rate of 50 to 150°C / s; when preparing a dual-phase steel with a tensile strength of 591 to 980 MPa, the steel is cooled to room temperature at a rate of 160 to 350°C / s; when preparing a dual-phase steel with a tensile strength of 981 to 1310 MPa, the steel is cooled to room temperature at a rate of 360 to 600°C / s.
[0066] In the manufacturing method of the present invention:
[0067] The present invention adopts a flexible manufacturing process, designs different components of dual-phase steels with different strengths, and adjusts different process controls to obtain required mechanical properties.
[0068] The main changes of the flexible process of the present invention for different strengths are as follows:
[0069] Adjustment of hot rolling coiling temperature parameters: For higher strength steel grades, a lower hot rolling coiling temperature, and therefore a lower hood annealing temperature, is required to prevent precipitates from growing and achieve a better precipitation strengthening effect.
[0070] Adjustment of insulation hood annealing parameters: For higher strength steel grades, longer insulation time is required to obtain more precipitates.
[0071] Adjusting continuous annealing parameters: For higher-strength steel grades, faster cooling rates are required to achieve higher strength. Flexible control of cooling rates can control the amount of martensite obtained, resulting in different strength levels in the final product.
[0072] Adjusting the Tempering Holding Time Parameters: During the tempering process, higher-strength steel grades require longer holding times to obtain more retained austenite and nano-precipitates. However, excessive holding times can reduce the strength of the finished annealed steel. Therefore, for different strength ranges, it is necessary to specify a reasonable holding time range to ensure both strength and sufficient retained austenite and nano-precipitates.
[0073] Flexible control of the insulation cover annealing process parameters, annealing process parameters, and tempering process parameters can be used to control the amount and size of retained austenite and fine dispersed precipitates, ensuring that the retained austenite content is greater than 3% and that the mass fraction of nano-precipitates less than 50nm in the final microstructure exceeds 8%. This allows for the production of different strength levels and comprehensive performance. The duplex steel has a tensile strength of 450-1310MPa, a strength-ductility product greater than 11,000, and a hole expansion ratio greater than 35%.
[0074] Compared with the prior art, the present invention has the following beneficial effects:
[0075] The present invention adopts a normalized component design, combines flexible manufacturing technology, and sets different hot coil heat preservation cover annealing, heat preservation cover annealing, continuous annealing and tempering processes to obtain a dual-phase steel with a tensile strength of 450-1310 MPa.
[0076] The development and application of numerous high-performance steels with varying compositions and mechanical properties has enabled safe and lightweight body-in-white (BIW) construction. However, this multi-steel approach presents numerous challenges, including resistance spot welding of dissimilar steels, process optimization, and recycling. This invention addresses this challenge by utilizing a single chemical composition to produce the multiple strength grades required for BIW.
[0077] After coiling, the hot coil is quickly annealed under a heat shield. Combined with the rational design of the composition and process, a long-term heat-hold annealing at a relatively low temperature produces finely dispersed ε carbides. This finely dispersed ε carbide is then inherited into the final continuously annealed product through rational process design. The fine dispersed precipitates in the annealed product enhance overall strength, reduce strength differences between phases, reduce strength differences between grain boundaries and within grains, and strengthen grain boundaries during deformation, thereby enhancing both strength and hole expansion. Flexible hot coiling temperatures and heat-holding times control the quantity and size of the fine dispersed precipitates, ensuring that nano-precipitates smaller than 50 nm account for greater than 8% of the total precipitate mass, enabling the product to achieve varying strength levels and overall performance.
[0078] Another feature of this invention is the use of discontinuous, ultra-low-temperature, long-term tempering, aimed at regenerating fine, dispersed ε carbides while preventing the martensitic structure from losing strength due to over-tempering. Simultaneously, the untransformed austenite is carbon-enriched, resulting in a sufficient amount of retained austenite (greater than 3%) and nano-precipitates (ensuring that the mass fraction of nano-precipitates less than 50 nm in the final structure exceeds 8%) after cooling. This significantly contributes to both strength and elongation. Flexible tempering temperatures and times can be used to control the amount and size of the fine, dispersed precipitates, enabling the product to achieve different strength levels and overall performance.
[0079] Compared with the existing technology, the technical solutions described in Chinese patent applications CN103215516A and CN104451436A are to obtain sufficient retained austenite by adding high Si and Al, and to obtain high elongation by the TRIP effect of the retained austenite, without considering the hole expansion performance, which is different from the idea of the present invention.
[0080] The ultra-high strength steels described in Chinese patent applications CN102776438A and CN102321841A respectively achieve good mechanical properties by adding microalloys such as niobium, lanthanum, nickel, cadmium, and copper, but they cannot achieve the high elongation and high hole expansion performance indicators covered by the present invention. DETAILED DESCRIPTION
[0081] The present invention will be further explained and illustrated below in conjunction with specific embodiments. However, such explanation and illustration do not constitute an improper limitation on the technical solution of the present invention.
[0082] The composition of the steel examples of the present invention is shown in Table 1, with the remainder consisting of Fe and other unavoidable impurities excluding P, S, and N. Table 2 lists the manufacturing process parameters for the steel plates of the present invention examples. Table 3 lists the microstructure ratios of the steel plates of the present invention examples. Table 4 lists the relevant performance parameters of the steel plates of the present invention examples.
[0083] The flexible processes are as follows:
[0084] Flexible process 1: When the tensile strength of duplex steel is 450-590 MPa, the hot rolling coiling temperature is 231-260°C; the heat preservation hood annealing time is 0.5-2 hours; continuous annealing is performed at a cooling rate of 50-150°C / s to room temperature; and the tempering time is 0.5-3 hours.
[0085] Flexible process 2: When the tensile strength of dual-phase steel is 591-980 MPa, the hot rolling coiling temperature is 201-230°C; the heat preservation hood annealing time is 2.1-4 hours; the continuous annealing is cooled to room temperature at a rate of 151-350°C / s; the tempering time is 2-6 hours;
[0086] Flexible process 3: When the tensile strength of dual-phase steel is 981-1310 MPa, the hot rolling coiling temperature is 160-200°C; the heat preservation hood annealing time is 4.1-6 hours; the continuous annealing is cooled to room temperature at a rate of 351-600°C / s; and the tempering time is 2-6 hours.
[0087] As can be seen from Table 3, the microstructure of the dual-phase steel of the present invention includes ferrite + martensite + retained austenite + nano-precipitates, wherein martensite accounts for more than 30% by volume, the volume fraction of retained austenite is greater than 3%, and the mass fraction of nano-precipitates with a size less than 50 nm accounts for more than 8% of the total precipitates.
[0088] As can be seen from Table 4, the present invention adopts a uniform composition design in combination with a flexible manufacturing method. By adjusting parameters such as the continuous annealing and tempering processes, a martensitic steel with a tensile strength of 450-1310 MPa can be obtained. The product steel plate has good formability and delayed cracking resistance, a strength-ductility product greater than 11,000, and a hole expansion rate greater than 35%.
[0089] Table 1 (Unit: weight percentage)
[0090] Table 3 Note: The volume fraction and mass fraction of microstructure are tested according to GB / T 13298.
[0091] Table 4 Note: Yield strength, tensile strength and elongation are tested according to GB / T 228.1, and hole expansion is tested according to GB / T 24524.
Claims
1. A dual-phase steel, the chemical composition of which is as follows by mass percentage: C: 0.06-0.08%, Si: 0.4-0.6%, Mn: 2.4-2.6%, Al: 0.01-0.05%, Ti: 0.02-0.04%, B: 0.0015-0.0025%, P≤0.015%, S≤0.003%, N≤0.005%, the balance comprising Fe and other unavoidable impurities; The microstructure of the dual-phase steel includes ferrite+martensite+retained austenite+nanoprecipitates. in, Martensite accounts for more than 30% volume fraction, retained austenite is greater than 3% volume fraction, and nano-precipitates with a size less than 50nm account for more than 8% of the total precipitates mass fraction; The tensile strength of the dual-phase steel is 450-1310 MPa, the strength-ductility product is greater than 11000%, and the hole expansion rate is greater than 35%.
2. The dual-phase steel according to claim 1, Its characteristics are: The balance is Fe and other inevitable impurities.
3. The dual-phase steel according to claim 1 or 2, Its characteristics are: The nano-precipitates are ε carbides.
4. The dual-phase steel according to claim 1 or 2, Its characteristics are The volume fraction of martensite is 32-91%, the volume fraction of retained austenite is 4-15%, and the volume fraction of ferrite is 2-65%; and / or the mass fraction of nano-precipitates with a size less than 50nm accounts for 9-30% of the total precipitates, such as 9-28%.
5. The dual-phase steel according to any one of claims 1 to 4, Its characteristics are: The yield strength of the dual-phase steel is 310-1200 MPa.
6. The dual-phase steel according to any one of claims 1 to 5, Its characteristics are: The hole expansion ratio of the dual-phase steel of the present invention is 36-55%.
7. The dual-phase steel according to any one of claims 1 to 4, Its characteristics are: The tensile strength of the dual-phase steel is 450-590MPa, preferably 470-590MPa, the yield strength is 310-370MPa, the strength-plasticity product is 12000-14500%, and the hole expansion rate is 36-40%; or the tensile strength of the dual-phase steel is 591-980MPa, preferably 650-980MPa, the yield strength is 360-580MPa, the strength-plasticity product is 12500-14700%, and the hole expansion rate is 45-55%; or the tensile strength of the dual-phase steel is 981-1310MPa, preferably 1000-1310MPa, the yield strength is 600-1200MPa, the strength-plasticity product is 11500-16000%, and the hole expansion rate is 40-50%.
8. The method for producing dual-phase steel according to any one of claims 1 to 7, Its characteristics are: The steps include: 1) Smelting and casting Smelting according to the composition of claim 1 or 2, and casting into a billet; 2) Hot rolling When preparing dual-phase steel with a tensile strength of 450-590 MPa, the ingot is heated to 1100-1250°C and kept warm for more than 0.5 hours; the final rolling temperature is controlled at 860-900°C and the coiling temperature is 231-260°C; When preparing dual-phase steel with a tensile strength of 591-980 MPa, the ingot is heated to 1100-1250°C and kept warm for more than 0.5 hours; the final rolling temperature is controlled at 860-900°C and the coiling temperature is 201-230°C; When preparing dual-phase steel with a tensile strength of 981-1310 MPa, the ingot is heated to 1100-1250°C and kept warm for more than 0.5 hours; the final rolling temperature is controlled at 860-900°C and the coiling temperature is 160-200°C; 3) Annealing of hot coil insulation cover When preparing dual-phase steel with a tensile strength of 450-590 MPa, after coiling, a heat preservation hood is used for annealing, and the annealing time is 0.5-2 hours. The heat preservation hood utilizes the internal heat of the steel coil, and the temperature drop rate per hour is less than 6°C / s; When preparing dual-phase steel with a tensile strength of 591-980 MPa, after coiling, a heat preservation hood is used for annealing, and the annealing time is 2.1-4 hours. The heat preservation hood utilizes the internal heat of the steel coil, and the temperature drop rate per hour is less than 6°C / s; When preparing dual-phase steel with a tensile strength of 981-1310 MPa, after coiling, a heat preservation hood is used for annealing, and the annealing time is 4.1-6 hours. The heat preservation hood utilizes the internal heat of the steel coil, and the temperature drop rate per hour is less than 6°C / s; 4) Cold rolling, controlling the cold rolling reduction rate to 0-50%; 5) Continuous annealing When preparing a dual-phase steel with a tensile strength of 450-590 MPa, the annealing temperature is 760-820°C, and the holding time is 50-100 seconds; then the steel is cooled at a rate of 3-10°C / s to the rapid cooling start temperature, which is 660-760°C, and then cooled to room temperature at a rate of 50-150°C / s; When preparing a dual-phase steel with a tensile strength of 591-980 MPa, the annealing temperature is 760-820°C, and the holding time is 50-100 seconds; then the steel is cooled at a rate of 3-10°C / s to a rapid cooling start temperature of 660-760°C, and then cooled to room temperature at a rate of 151-350°C / s; When preparing a dual-phase steel with a tensile strength of 981-1310 MPa, the annealing temperature is 760-820°C, and the holding time is 50-100 seconds; then the steel is cooled at a rate of 3-10°C / s to a rapid cooling start temperature of 660-760°C, and then cooled to room temperature at a rate of 351-600°C / s; 6) Tempering When preparing dual-phase steel with a tensile strength of 450-590 MPa, the tempering temperature is 160-260°C and the tempering time is 0.5-3 h; When preparing dual-phase steel with a tensile strength of 591 to 980 MPa, the tempering temperature is 160 to 260 ° C and the tempering time is 2 to 6 hours; When preparing dual-phase steel with a tensile strength of 981 to 1310 MPa, the tempering temperature is 160 to 260 ° C and the tempering time is 2 to 6 hours; 7) Smoothing: use a smoothing rate of 0 to 0.3%.
9. The method for producing dual-phase steel according to claim 8, Its characteristics are: Step 1) Casting adopts thin slab continuous casting process.
10. The method for producing dual-phase steel according to claim 8, Its characteristics are: When preparing dual-phase steel with a tensile strength of 450-590 MPa, the holding time in the hot rolling step is 0.5-3.5 hours; when preparing dual-phase steel with a tensile strength of 450-590 MPa, the coiling temperature in the hot rolling step is 232-260°C.
11. The method for producing dual-phase steel according to claim 8, Its characteristics are: When preparing dual-phase steel with a tensile strength of 591 to 980 MPa, the holding time in the hot rolling step is 0.5 to 2.5 hours; when preparing dual-phase steel with a tensile strength of 591 to 980 MPa, the coiling temperature in the hot rolling step is 203 to 228°C.
12. The method for producing dual-phase steel according to claim 8, Its characteristics are: When preparing dual-phase steel with a tensile strength of 981 to 1310 MPa, the holding time in the hot rolling step is 1.2 to 3.2 hours.
13. The method for producing dual-phase steel according to claim 8, Its characteristics are: In the hot coil insulation cover annealing step, when preparing a dual-phase steel with a tensile strength of 450-590 MPa, the annealing time is 0.5-2 hours; when preparing a dual-phase steel with a tensile strength of 591-980 MPa, the annealing time is 2.2-4 hours; when preparing a dual-phase steel with a tensile strength of 981-1310 MPa, the annealing time is 4.3-6 hours.
14. The method for producing dual-phase steel according to claim 8, Its characteristics are: In the continuous annealing step, when preparing a dual-phase steel with a tensile strength of 450 to 590 MPa, cooling to room temperature is performed at a rate of 50 to 150°C / s; when preparing a dual-phase steel with a tensile strength of 591 to 980 MPa, cooling to room temperature is performed at a rate of 160 to 350°C / s; when preparing a dual-phase steel with a tensile strength of 981 to 1310 MPa, cooling to room temperature is performed at a rate of 360 to 600°C / s.
Citation Information
Patent Citations
Track shoe steel with tensile strength of up to 1300 MPa and manufacturing method thereof
CN102321841A
Niobium-lanthanum microalloying Mn-B series superstrength steel plate and heat treatment technology thereof
CN102776438A
700MPa high strength hot rolling Q&P steel and manufacturing method thereof
CN103215516A
Bainite-martensite-austenite multi-phase wear-resistant steel plate and manufacturing method thereof
CN104451436A
High-strength hot-dip zinc plated steel sheet excellent in workability and process for manufacturing the same
CN101821419A