Coating composition, coating method, and mold treatment method

The coating composition with silica and fluororesin particles, along with chlorine bleach, effectively addresses the adhesion and growth of mold and dust by decomposing organic contaminants, enhancing antifouling and antifungal performance and maintaining substrate stability.

WO2024247107A1PCT designated stage expired Publication Date: 2024-12-05MITSUBISHI ELECTRIC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/020094
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing coating compositions fail to effectively inhibit the adhesion and growth of mold and dust on substrates, as they do not address the decomposition of organic compounds by sodium hypochlorite, leading to instability and reduced antifouling performance.

Method used

A coating composition containing 5% or less silica particles, fluororesin particles, 0.001% to 5% chlorine bleach, and water, which forms a film that suppresses mold growth by decomposing organic contaminants and preventing dirt adhesion through electrostatic and hydrophobic properties.

Benefits of technology

The solution provides a stable coating film with improved antifouling and antifungal performance, preventing mold adhesion and growth while maintaining the substrate's design and hygiene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023020094_05122024_PF_FP_ABST
    Figure JP2023020094_05122024_PF_FP_ABST
Patent Text Reader

Abstract

This coating composition comprises 5% by mass or less of silica particles, fluororesin particles, 0.001%-5% by mass of a chlorine-based bleaching agent, and water.
Need to check novelty before this filing date? Find Prior Art

Description

Coating composition, coating method, and mold treatment method

[0001] The present disclosure relates to coating compositions for producing coatings that inhibit fouling of substrates, methods for coating substrates, and methods for treating mold on substrates.

[0002] Various types of dirt, such as dust, oily smoke, and mold, adhere to the surfaces of various items used indoors or outdoors. In particular, mold adheres to the surface of items and grows on dust and oily smoke as nutrients, causing dirt. Therefore, in order to achieve a high level of anti-fouling effect, it is necessary to inhibit the growth of mold, and there is a demand for technology that inhibits the adhesion and growth of mold.

[0003] Patent Document 1 discloses a coating composition that contains an antifungal agent and forms a film that coats a substrate, thereby inhibiting the adhesion and growth of mold on the substrate.

[0004] JP 2011-57855 A

[0005] However, Patent Document 1 does not mention any technology for inhibiting the adhesion of dust, oily smoke, mold, etc. to the surface of a coating film obtained from a coating composition. When dust, oily smoke, etc., which serve as nutrients for mold, accumulate on the surface of a coating film, mold can easily grow as it adheres to the accumulated dirt.

[0006] Furthermore, Patent Document 1 discloses sodium hypochlorite as the antibacterial agent contained in the coating composition, and discloses an organic compound as the antibacterial agent or the antifungal agent, but when the organic compound and sodium hypochlorite are contained in the coating composition, there is a possibility that the organic compound will be decomposed by the sodium hypochlorite, which may result in a decrease in the stability of the coating composition.

[0007] The present disclosure has been made to solve the above-mentioned problems, and aims to provide a coating composition that produces a coating film that is stable and has improved antifouling performance that inhibits adhesion of dirt such as dust and mold, and improved antifungal performance that inhibits the growth of mold, a method for coating a substrate, and a method for treating mold on a substrate.

[0008] The coating composition according to the present disclosure contains 5% by mass or less of silica particles, fluororesin particles, 0.001% by mass or more and 5% by mass or less of a chlorine bleaching agent, and water.

[0009] The coating method according to the present disclosure is a method for coating a substrate, which comprises applying a coating composition containing 5% by mass or less of silica particles, fluororesin particles, 0.001% by mass or more and 5% by mass or less of a chlorine-based bleaching agent, and water to the substrate, thereby forming a coating film on the surface of the substrate.

[0010] The mold treatment method according to the present disclosure involves applying to a substrate a coating composition containing 5% by mass or less of silica particles, fluororesin particles, 0.001% by mass or more and 5% by mass or less of a chlorine-based bleaching agent, and water.

[0011] According to the coating composition, coating method, and mildew treatment method of the present disclosure, it is possible to ensure the stability of the coating composition, and to obtain a coating film with improved antifouling and antifungal properties, thereby suppressing the adhesion and proliferation of mildew on a substrate.

[0012] FIG. 1 is a cross-sectional schematic diagram of a coating film obtained from a coating composition according to Embodiment 1. FIG. 2 is a top view schematic diagram illustrating a coating film obtained from a coating composition according to Embodiment 1. FIG. 3 is a top view schematic diagram illustrating a coating film in a comparative example. FIG. 4 is a cross-sectional schematic diagram illustrating a coating film formed on a substrate having water-absorbent properties, porous properties, or the like, by a coating composition according to Embodiment 2. FIG. 5 is a diagram showing several examples of the proportions of constituent elements in a coating composition according to Embodiment 1. FIG. 6 is a diagram showing evaluation results of coating compositions according to Examples 1 to 9 and Comparative Examples 1 to 3. FIG. 7 is a diagram showing several examples of the proportions of constituent elements in a coating composition according to Embodiment 2. FIG. 8 is a diagram showing evaluation results of coating compositions according to Examples 10 to 11 and Comparative Example 4. FIG. 9 is a diagram showing several examples of the proportions of constituent elements in coating compositions according to Embodiments 1 and 2. FIG. 10 is a diagram showing evaluation results of coating compositions according to Examples 12 to 14 and Comparative Examples 5 to 7.

[0013] Hereinafter, a coating composition according to an embodiment will be described with reference to the drawings. Note that in the drawings, the relative dimensional relationships and shapes of the components may differ from the actual ones. In the drawings, components with the same reference numerals are the same or correspond to each other. The components in the embodiments are merely examples and are not limited thereto.

[0014] Embodiment 1. Figure 1 is a schematic cross-sectional view of a coating film 1 obtained from a coating composition according to embodiment 1. The coating composition is applied to a substrate 4 to form the coating film 1. The coating composition according to the embodiment contains a plurality of silica particles 2, a plurality of fluororesin particles 3, and water and a chlorine bleaching agent (not shown). In the coating film 1, the plurality of silica particles 2 aggregate to form a silica film, and the plurality of fluororesin particles 3 are scattered throughout the silica film.

[0015] Chlorine bleach decomposes mold and organic contaminants. Organic contaminants include oily soot, sebum, and keratin, which serve as nutrients for mold. In the coating composition applied to the surface of the substrate 4, the chlorine bleach decomposes mold and organic contaminants attached to the surface of the substrate 4, as well as mold and organic contaminants diffused from the surface of the substrate 4 into the coating composition. The chlorine bleach also decomposes mold and organic contaminants attached to the coating composition from the ambient environment, such as the atmosphere. This provides a disinfecting effect on the surface of the substrate 4, a blocking effect on the supply of organic contaminants that serve as nutrients to mold, and an inhibitory effect on the growth of mold on the surface of the substrate 4 and within the coating film 1. Furthermore, the decomposition of mold and other contaminants on the surface of the substrate 4 by the chlorine bleach maintains or improves the adhesion of the coating film 1 to the surface of the substrate 4, and maintains the design of the substrate 4. The chlorine bleach decomposes mold and organic contaminants in the coating composition as well as mold and organic contaminants from the surrounding environment, thereby maintaining or improving the strength of the coating film 1.

[0016] The chlorine bleach is concentrated and becomes more concentrated as the water contained in the coating composition applied to the surface of the substrate 4 evaporates. As a result, the chlorine bleach naturally decomposes and is no longer contained in the coating film 1.

[0017] The content of the chlorine bleach in the coating composition is 0.001 to 5.0% by mass, preferably 0.01 to 3.0% by mass. A content within this range allows for the decomposition of mold, organic contaminants, and the like, while providing a stable coating composition. If the content of the chlorine bleach is less than 0.001% by mass, there is a risk that the mold and organic contaminants on the surface of the substrate 4 and on the surface and inside of the coating composition may not be decomposed. On the other hand, if the content of the chlorine bleach is 5.0% by mass or more, there is a risk that the dispersibility of the silica particles 2 and the fluororesin particles 3 in the coating composition may decrease, which may cause the silica particles 2 and the fluororesin particles 3 to aggregate and precipitate, resulting in a lack of stability as a coating composition.

[0018] Chlorine bleaches include hypochlorous acid, sodium hypochlorite, lithium hypochlorite, potassium hypochlorite, calcium hypochlorite, sodium dichloroisocyanurate, or potassium dichloroisocyanurate, and may be any mixture of two or more of these.

[0019] Before application of the coating composition, the substrate 4 is contaminated with mold, organic contaminants, and the like. Mold adheres to the surface of the substrate 4 as spores or hyphae. Mold and organic contaminants adhering to the surface of the substrate 4 not only impair the hygiene and cleanliness of the article, but also discolor the article due to the pigments they contain, impairing the design of the article. Mold grows in soil and plants around the world and releases spores into the air. Therefore, articles placed outdoors are exposed to airborne spores. Meanwhile, indoor articles are exposed to spores due to the movement of humans, pets, and other living creatures, as well as the movement of articles. Mold propagates when spores adhering to the surface of the substrate 4 germinate and mycelia grow. Mold also propagates by the growth of mycelia from mold-containing dirt adhering to the substrate 4. Organic contaminants, which serve as nutrients for mold, also adhere to the surface of the substrate 4. The organic contaminants adhering to the substrate 4 provide nutrients for mold growth. Therefore, to inhibit mold growth, it is necessary to remove the mold and organic contaminants.

[0020] When the coating composition is applied to the substrate 4, the chlorine bleach functions as an oxidizing agent, decomposing and removing mold and organic contaminants. The chlorine bleach is dispersed in the coating composition applied to the substrate 4. When the chlorine bleach reaches mold, it alters and decomposes its cell walls, cell membranes, cytoplasm, and enzymes, thereby removing and decomposing the mold. The chlorine bleach also alters and decomposes the organic components that make up the organic contaminants, thereby removing and decomposing the organic contaminants. While decomposing and removing the mold and organic contaminants, the chlorine bleach also decomposes the pigments contained in the mold and organic contaminants, thereby achieving a bleaching effect. As the moisture contained in the coating composition evaporates, the concentration of the chlorine bleach increases, further enhancing its performance as an oxidizing agent that decomposes mold and organic contaminants. Furthermore, as the concentration of the chlorine bleach increases, the natural decomposition rate of the chlorine bleach also increases, leading to its disappearance from the coating film 1.

[0021] The silica film in the coating film 1 of the embodiment is a dense film with fine voids because the silica particles 2 are fine particles with a large surface area per unit volume. The silica film suppresses the adhesion and fixation of dirt such as dust due to electrostatic charge. In particular, the silica particles 2 are hydrophilic, making it difficult for hydrophobic dirt to adhere and fix. In the coating film 1 of the embodiment, the fluororesin particles 3 scattered throughout the silica film are hydrophobic, making it difficult for hydrophilic dirt to adhere and fix.

[0022] The coating film 1 is obtained by volatilizing water contained in a coating composition applied to the surface of the substrate 4. The coating film 1 can obtain antifouling properties that make it difficult for mold, organic contaminants, etc. to adhere and adhere due to the silica particles 2 and fluororesin particles 3. In addition to the antifouling properties, the coating film 1 can also obtain antifungal properties due to the decomposition effect of the chlorine bleach on mold, organic contaminants, etc.

[0023] The silica particles 2 are a stable inorganic component and are therefore not decomposed by chlorine bleaching agents. The fluororesin particles 3 are a stable organic component with chemical resistance and are therefore not decomposed by chlorine bleaching agents. Therefore, the coating composition according to the first embodiment has excellent stability.

[0024] As shown in FIG. 1 , the silica particles 2 in the first embodiment are spherical. Furthermore, the average particle size of the silica particles 2 in the first embodiment is 4 nm or more and 25 nm or less, as measured by a light scattering method. Preferably, the average particle size of the silica particles 2 is 4 nm to 15 nm. By incorporating silica particles 2 having an average particle size in this range into the coating composition, the silica particles are more likely to aggregate together when dried, facilitating solidification of the coating composition. Furthermore, since the number of silica particles 2 dissolved in equilibrium in the coating composition increases, a coating film 1 with relatively high strength can be obtained without incorporating a special binder. Furthermore, since light scattering of the silica particles 2 is reduced, the transparency of the coating film 1 is improved, and changes in the color tone and texture of the surface of the article on which the coating film 1 is formed can be suppressed. Note that if the average particle size of the silica particles 2 is greater than 25 nm, the coating film 1 may not have sufficient strength. Furthermore, if the average particle size of the silica particles 2 is less than 4 nm, the stability of the coating composition may be reduced, and the strength and antifouling properties of the coating film 1 may be reduced.

[0025] The mass of silica particles 2 contained in the coating composition according to embodiment 1 is 0.1 to 5.0% of the total mass of the coating composition. Preferably, the mass of silica particles 2 contained in the coating composition is 0.3 to 2.5% of the total mass of the coating composition. When the content of silica particles 2 is 0.1 to 5.0%, a uniform and thin coating film can be formed without impairing the color tone and texture of the article surface. When the content of silica particles 2 is less than 0.1% by mass, the resulting coating film becomes too thin, making it difficult to achieve the desired antifouling properties. On the other hand, when the content of silica particles 2 exceeds 5% by mass, the coating film becomes non-uniform and cloudy, causing cracks and making it prone to peeling.

[0026] Examples of the fluororesin particles 3 in the first embodiment include PTFE (polytetrafluoroethylene), FEP (tetrafluoroethylene hexafluoropropylene copolymer), PFA (tetrafluoroethylene perfluoroalkyl vinyl ether copolymer), ETFE (ethylene tetrafluoroethylene copolymer), ECTFE (ethylene chlorotrifluoroethylene copolymer), PVDF (polyvinylidene fluoride), PCTFE (polychlorotrifluoroethylene), and PVF (polyvinyl fluoride). The fluororesin particles 3 may be a copolymer or mixture of these, or may be a mixture of these fluororesins with other resins. Of the above, PTFE and FEP are preferred as the fluororesin particles 3 because of their excellent stability and high hydrophobicity.

[0027] The average particle size of the fluororesin particles 3 is not particularly limited, but is preferably 50 nm to 10,000 nm, and more preferably 100 nm to 5,000 nm, as measured by a light scattering method. By incorporating fluororesin particles 3 having an average particle size within this range into the coating composition, the fluororesin particles 3 are adequately dispersed within the coating film 1 and are easily exposed to the surface of the coating film 1, thereby achieving good antifouling performance. If the average particle size of the fluororesin particles 3 is less than 50 nm, the coating composition may not be stable, and the fluororesin particles 3 may be less easily exposed to the surface of the coating film 1, making it possible to fail to achieve the desired antifouling performance. On the other hand, if the average particle size of the fluororesin particles 3 exceeds 10,000 nm, the hydrophobic regions in the resulting coating film 1 may become large, resulting in excessive unevenness in the coating film 1, which may prevent the desired antifouling performance from being achieved.

[0028] The mass ratio of the silica particles 2 to the fluororesin particles 3 contained in the coating composition according to embodiment 1 is 40:60 to 95:5, and more preferably 50:50 to 90:10. When the mass ratio of the silica particles 22 to the fluororesin particles 3 is 40:60 to 95:5, a coating film 1 having a well-balanced mixture of hydrophilic portions originating from the silica particles 2 and hydrophobic portions originating from the fluororesin particles 3 can be obtained by drying at room temperature, and the coating film 1 has good antifouling performance.

[0029] FIG. 2 is a top view schematic diagram illustrating a coating film 1 obtained from the coating composition according to embodiment 1. The mass ratio of silica particles 2 to fluororesin particles 3 contained in the coating film 1 in FIG. 2 is 75:25. As shown in FIG. 2, the fluororesin particles 3 are scattered across a silica film formed by aggregation of a plurality of silica particles 2. On the surface of the coating film 1 shown in FIG. 2, the area of ​​the silica film, which is the hydrophilic portion, is sufficiently larger than the area of ​​the fluororesin particles 3, which are the hydrophobic portion, and therefore the film as a whole is hydrophilic. The hydrophilic portions on the surface of the coating film 1 play an important role in improving antifungal performance. The antifungal performance provided by the hydrophilic portions on the surface of the coating film 1 will be described in detail below.

[0030] On the surface of the coating film 1, the hydrophilic portions are continuous without being interrupted by hydrophobic portions. Therefore, when water droplets, such as condensed water, adhere to the surface of the coating film 1, the water droplets flow through the hydrophilic portions as flow paths and are easily discharged from the surface of the coating film 1. Furthermore, water droplets that adhere to the surface of the coating film 1 tend to spread thinly over the entire coating film 1, which allows the water droplets to volatilize easily. Generally, the surface of an article with continuous water droplets adhering thereto is an environment conducive to mold growth. However, the coating film 1 of embodiment 1 has the property that water droplets that adhere to the surface are easily discharged and volatilized, thereby improving its mold-proofing performance. Furthermore, the property of droplets easily spreading over the entire coating film 1 allows hydrophilic or hydrophobic contaminants that adhere to the surface of the coating film 1 to be removed by the flow of water droplets or to be less likely to adhere. In particular, dirt on the surface of the coating film 1 is easily removed during condensation, rain, cleaning, etc. Furthermore, because the coating film 1 of embodiment 1 is mainly composed of a continuous silica film, it is also possible to suppress electrostatic charge on the film surface, which causes dirt to be adsorbed. Furthermore, because both the silica film and the fluororesin particles 3 of the coating film 1 are oil-repellent, oil droplets are less likely to adhere to the coating film 1.

[0031] On the other hand, if the ratio of silica particles 2 is greater than the above-mentioned range, the coating film 1 can effectively prevent the adhesion of hydrophobic contaminants such as oily soot or carbon, but is susceptible to the adhesion of hydrophilic contaminants such as sand dust or dirt. Also, if the ratio of silica particles 2 does not reach the above-mentioned range, the coating film 1 can effectively prevent the adhesion of hydrophilic contaminants such as sand dust or dirt, but is susceptible to the adhesion of hydrophobic contaminants such as oily soot or carbon. Mold and organic contaminants contained in oily soot, carbon, sand dust, or dirt adhere to the coating film 1, creating a mold habitat, resulting in a decrease in antifungal performance.

[0032] Here, an example in which the mass ratio of silica particles 2 to fluororesin particles 3 contained in the coating film 1 is outside the above-mentioned range will be described with reference to FIG. 3 . FIG. 3 is a top view schematic diagram showing the coating film 1 of a comparative example. In FIG. 3 , the mass ratio of silica particles 2 to fluororesin particles 3 contained in the coating film 1 is 25:75. In the coating film 1 shown in FIG. 3 , the ratio of fluororesin particles 3 to silica particles 2 is high, resulting in a large number of hydrophobic portions and the hydrophilic portions being separated by the hydrophobic portions. Therefore, when water droplets adhere to the coating film 1, the flow of the water droplets is hindered by the hydrophobic portions, and the water droplets cannot flow out using the hydrophilic portions as a flow path, remaining on the surface of the coating film 1. Furthermore, water droplets adhered to the surface of the coating film 1 are difficult to spread thinly over the entire coating film 1, which increases the time required for evaporation. Therefore, the coating film 1 illustrated in FIG. 3 does not achieve high antifungal performance or good antifouling performance.

[0033] Mold that arrives on the coating film 1 from the surrounding environment includes mold that floats in the air as spores and mold that is mixed in with hydrophilic or hydrophobic dirt as spores and hyphae. Generally, mold spores have a hydrophilic surface and adhere to objects through electrostatic bonding between hydrophilic groups, liquid bridges with water, or intermolecular forces. Mold spores are minute particles with a diameter of 2 μm to 10 μm. To prevent the adhesion of mold spores, it is necessary to form a coating film 1 that does not have hydrophilic portions large enough to allow hydrophilic dirt to adhere. Meanwhile, mold hyphae generally have lengths of tens of μm to several mm. Therefore, hydrophilic or hydrophobic dirt mixed with mold is a particle with a size of tens of μm to several mm. To prevent the adhesion of hydrophilic dirt mixed with mold, it is necessary to form a coating film 1 that does not have hydrophilic portions large enough to allow hydrophilic dirt to adhere. In order to prevent adhesion of hydrophobic stains including mold, it is necessary to form a coating film 1 that does not have hydrophobic portions large enough to allow adhesion of hydrophobic stains.

[0034] Furthermore, hydrophilic contaminants such as sand and dust generally adhere to objects through electrostatic bonding between hydrophilic groups, liquid bridges with water, or intermolecular forces. Sand and dust are minute particles with diameters ranging from several μm to several tens of μm, while dust is much larger. To prevent the adhesion of hydrophilic contaminants due to electrostatic bonding between hydrophilic groups, it is necessary to form a coating film 1 that does not have hydrophilic portions large enough for hydrophilic contaminants to adhere to.

[0035] Furthermore, hydrophobic dirt such as oily smoke, carbon, sebum, or keratin generally adheres to an object through intermolecular forces or hydrophobic bonds in the presence of water. Hydrophobic dirt is generally made up of minute particles with a diameter of 1 μm or less, with most particles having a diameter of 0.3 μm or less. If the surface of the coating film 1 is hydrophobic, hydrophobic dirt will easily adhere to it. Furthermore, when the hydrophobic surface is covered with condensed water or the like and is in contact with hydrophobic dirt, the cohesive force of water may create a hydrophobic bond between the surface and the hydrophobic dirt, causing the hydrophobic dirt to adhere to the surface of the coating film 1.

[0036] In embodiment 1, by setting the mass ratio of silica particles 2 to fluororesin particles 3 contained in the coating composition within the above-mentioned range, a coating film 1 can be obtained in which hydrophobic portions are appropriately dispersed within hydrophilic portions, as shown in Figure 2. As a result, the hydrophilic and hydrophobic portions in the coating film 1 of embodiment 1 are sized to prevent the adhesion of mold spores and mold-containing dirt. Therefore, the coating film 1 of embodiment 1 can suppress the adhesion of mold spores and mold-containing dirt due to electrostatic bonding between hydrophilic groups or between hydrophobic groups. Therefore, mold growth on the surface of the coating film 1 can be suppressed, and excellent antifungal performance can be obtained.

[0037] Furthermore, in the first embodiment, by setting the mass ratio of the silica particles 2 to the fluororesin particles 3 contained in the coating composition within the above-mentioned range, the hydrophobic portions are adequately dispersed among the hydrophilic portions, forming a coating film 1 with almost no hydrophilic portions large enough to allow stable adhesion of hydrophilic contaminants. This makes it possible to suppress adhesion of hydrophilic contaminants due to electrostatic bonding between hydrophilic groups on the surface of the coating film 1. Furthermore, in the coating film 1 of the first embodiment, even if hydrophilic contaminants adhere to the hydrophilic portions, the hydrophilic contaminants are prevented from sufficiently adhering to the hydrophilic portions due to physical obstruction by the surfaces of the hydrophobic portions adjacent to the hydrophilic portions or by protrusions on the hydrophobic portions. Therefore, the hydrophilic contaminants are less likely to adhere to the surface of the coating film 1. Furthermore, because the coating film 1 of the first embodiment is a porous coating film 1 composed of the silica particles 2 and the fluororesin particles 3, even if liquid bridging due to water or the like occurs, the water between the silica particles 2 is easily and rapidly removed from the surface of the silica film during the drying process.

[0038] Furthermore, because the coating composition according to embodiment 1 does not contain a binder or organic polymer as a constituent, the state of the surface of the coating film 1 is not changed by, for example, the precipitation of the binder or organic polymer on the surface of the coating film 1 after the liquid bridge is dissolved. Furthermore, because the coating film 1 of embodiment 1 has extremely small voids and is a film with a low density, it is possible to suppress the adhesion of hydrophilic dirt due to intermolecular forces. Furthermore, by suppressing the adhesion of hydrophilic dirt, the coating film 1 of embodiment 1 also suppresses the adhesion of nutrients necessary for mold growth, thereby inhibiting mold growth.

[0039] In the first embodiment, the coating film 1 is obtained in which hydrophobic portions are appropriately dispersed among hydrophilic portions, and therefore adhesion of hydrophobic dirt can be suppressed by the hydrophilic groups on the surface of the coating film 1 or the presence of water adsorbed on the surface. Furthermore, by suppressing adhesion of hydrophobic dirt, the coating film 1 of the first embodiment suppresses the adhesion of nutrients necessary for mold growth, thereby inhibiting mold growth.

[0040] Furthermore, since the coating film 1 of embodiment 1 is composed of chemically stable silica particles 2 and fluororesin particles 3, it can maintain its antifouling performance for a long period of time, and therefore can obtain sustained antifungal performance.

[0041] The coating composition according to the first embodiment contains water as a solvent, which is a volatile component. Here, if the amount of minerals contained in the water is large, it may become impossible to control the aggregation of the silica particles 2. Specifically, if the concentration of ionic impurities in the water exceeds 200 ppm, the silica particles 2 may aggregate and precipitate. This may result in a decrease in the strength or transparency of the coating film 1. Therefore, from the viewpoint of the dispersion stability of the silica particles 2, it is preferable that the water in the coating composition contains a small amount of divalent or higher ionic impurities, such as calcium ions or magnesium ions. Specifically, the water contained in the coating composition according to the first embodiment is preferably deionized water, but may also be water containing ionic impurities. In this case, the concentration of the ionic impurities is preferably 200 ppm or less, and more preferably 50 ppm or less.

[0042] The water content in the coating composition is not particularly limited, but is, for example, 30 to 99.8% by mass. However, the water content is preferably 50% by mass or more and 99.5% by mass or less, and more preferably 60% by mass or more and 99% by mass or less. The coating composition may contain an organic solvent or the like to adjust the stability, coatability, and drying properties of the coating composition.

[0043] In the first embodiment, when preparing a coating composition by blending chlorine bleach, silica particles 2, fluororesin particles 3, etc., the solution or dispersion of chlorine bleach, silica particles 2, fluororesin particles 3, etc. before blending may be prevented from being a combination of a basic liquid having a pH of 8 or higher and an acidic liquid having a pH of 6 or lower. This can prevent aggregation or precipitation in the coating composition. Therefore, the coating film 1 obtained after drying of the coating composition applied to the substrate 4 is homogeneous. Furthermore, decomposition of the chlorine bleach before application of the coating composition can be prevented.

[0044] The coating composition according to the first embodiment may contain various components known in the coating technical field, provided that the above-described effects are not impaired. Examples of such components include surfactants, coupling agents, silane compounds, and antifungal agents. The amounts of these components are not particularly limited as long as the above-described effects are not impaired, and may be adjusted appropriately depending on the types of components.

[0045] The method for producing the coating composition according to the first embodiment is not particularly limited and may be based on a method known in the technical field of coating. For example, the coating composition according to the first embodiment can be produced by mixing a dispersion of silica particles 2, a dispersion of fluororesin particles 3, and a chlorine-based bleaching agent.

[0046] The method for producing a coating composition according to the first embodiment may include a method for preparing a coating composition by redispersing the aggregates or precipitates using a homogenizer or a high-pressure dispersion treatment device when aggregation or precipitation of components occurs due to the mixing of multiple liquids. To prevent re-aggregation, a surfactant, an inorganic dispersant, or a high-viscosity solvent such as ethylene glycol may be added to the mixed liquid during initial mixing or re-dispersion. Mixing materials in multiple stages in this manner enables a wide range of material combinations when producing a coating composition, and by achieving an appropriate aggregation state, the fluidity of the coating composition can be improved, or the density or smoothness of the resulting coating film 1 can be optimized.

[0047] The coating composition may be obtained by mixing all of the components at once, in which case it is stored in a container until use and applied to the substrate 4 without any processing. Alternatively, the coating composition may be obtained by mixing two or more pre-prepared liquids immediately before use. In the latter case, a method is exemplified in which only the chlorine bleach, which is particularly susceptible to decomposition, is mixed with the other components of the coating composition immediately before use. This allows the effects of the chlorine bleach and other ingredients in the coating composition to be maintained even after long-term storage.

[0048] Examples of methods for applying the coating composition according to embodiment 1 to the substrate 4 include spray application, application using a brush or roller bucket, and dipping. Spray application methods include a method in which a pre-mixed coating composition is sprayed from a spray nozzle, and a method in which two or more liquids for obtaining the coating composition are sprayed from separate spray nozzles and mixed onto the surface of the substrate 4 or just before reaching the substrate 4. Brush or roller bucket application methods include a method in which two or more liquids are applied in layers using separate application tools. Dipping application methods include a method in which two or more liquids are dipped in multiple stages.

[0049] According to the method of applying the coating composition to the substrate 4 of the first embodiment, the silica particles 2 are solidified by drying alone, and therefore heating or the like is not required, making it possible to fix the fluororesin particles 3 to the silica film. Here, when drying the coating composition, excess coating composition may be removed from the substrate 4 by an airflow. In particular, by removing excess coating composition by an airflow, a thin coating film 1 in which the fluororesin particles 3 are uniformly dispersed in the silica film can be rapidly obtained.

[0050] A preferred method for applying the coating composition to the substrate 4 is to mix two or more liquids for obtaining the coating composition during the application process and prepare the coating composition on the surface of the substrate 4. That is, a preferred method is to apply each of the two or more liquids for obtaining the coating composition to the surface of the substrate 4, mix the two or more liquids on the surface of the substrate 4, and generate the coating composition on the surface of the substrate 4. This method of forming a liquid film of the coating composition on the surface of the substrate 4 and drying the liquid film to obtain the coating film 1 can suppress the decomposition of chlorine bleach, which is prone to decomposition. It also makes it possible to form the coating film 1 using a combination of coating compositions that cannot exist stably as a liquid due to factors such as aggregation when mixed. It also reduces the labor required. The coating film 1 obtained in this manner can have little organic contamination and an appropriate porosity.

[0051] The formation of the coating film 1 containing the silica particles 2 and the fluororesin particles 3 and the decomposition of mold and organic matter by the chlorine bleach may be carried out separately. That is, the chlorine bleach may be applied to the surface of the substrate 4 before or after the coating composition or two or more liquids constituting the coating composition are applied to the substrate 4.

[0052] The article serving as the substrate 4 to which the coating composition is applied is not particularly limited, and examples thereof include various articles used indoors or outdoors that are prone to adhesion of various hydrophilic or hydrophobic stains such as dust, oily smoke, mold, or organic contaminants. Depending on the article to which the coating film 1 is applied, the surface of the article may be subjected to pretreatment such as cleaning with a detergent or alcohol, corona treatment, or UV treatment, in order to improve the wettability of the coating composition and the adhesion of the coating film 1. Furthermore, articles that are significantly contaminated with mold or organic contaminants may be subjected to pretreatment such as sterilization with a chlorine bleach.

[0053] The surface of the substrate 4 to which the coating composition is applied is not limited to a specific surface such as the top surface of the substrate 4, and the coating composition may be applied to the side or back surface of the substrate 4, or to multiple surfaces.

[0054] Embodiment 2. A coating composition according to embodiment 2 will be described below. In embodiment 2, the same components as those in embodiment 1 are denoted by the same reference numerals. In embodiment 2, the same configurations as those in embodiment 1 and the same functions as those in embodiment 1 will not be described unless there are special circumstances.

[0055] In the first embodiment, the silica particles 2 contained in the coating composition are spherical, but in the second embodiment, the silica particles 2 contained in the coating composition have irregular shapes such as needles, scales, chains, beads, or pearl necklaces. This makes it easier to form a coating film 1 with excellent antifouling properties even on the surface of a substrate 4 that is water-absorbent or porous, on which it is difficult to form a coating film 1.

[0056] Fig. 4 is a cross-sectional schematic diagram illustrating a coating film 1 formed on a substrate 4 having water-absorbent properties or porous properties by the coating composition according to embodiment 2. As shown in Fig. 4, the coating film 1 formed from the coating composition according to embodiment 2 contains a silica film in which silica particles 2 are adhered, and fluororesin particles 3 dispersed in the silica film.

[0057] When the coating composition of embodiment 2 is applied to a substrate 4 having water absorption or porous properties, a portion of the water and a portion of the chlorine bleaching agent in the coating composition flow from the surface to the interior of the substrate 4 due to capillary action in the pores 5 of the substrate 4. Meanwhile, among the components contained in the coating composition, the fluororesin particles 3 and the silica particles 2 have particle sizes sufficient to block the pores 5 of the substrate 4 and are therefore less likely to penetrate into the interior of the substrate 4. Therefore, the ratio of silica particles 2 to fluororesin particles 3 in the coating film 1 is maintained substantially the same as the ratio of silica particles 2 to fluororesin particles 3 in the coating composition before application. Therefore, by adjusting the ratio of silica particles 2 to fluororesin particles 3 in the coating composition, excellent antifouling performance can be obtained. Note that the blockage of the pores 5 by the fluororesin particles 3 and the silica particles 2 refers to the inability of the fluororesin particles 3 and the silica particles 2 to pass through the pores 5, whereas water, chlorine bleaching agent, air, and the like can pass through the fine voids in the silica film.

[0058] Furthermore, the silica particles 2 in the coating film 1 formed from the coating composition of embodiment 2 are irregularly shaped particles, and therefore have a large surface area per unit volume. Therefore, the silica film formed by the silica particles 2 has very small voids and a low density, which reduces adhesion of dirt to the coating film 1 due to intermolecular forces.

[0059] The silica particles 2 in the second embodiment may be particles of irregular shapes such as needles, scales, chains, beads, or pearl necklaces, or may be a mixture of particles of two or more of the needles, scales, chains, beads, and pearl necklaces. The average particle size of the silica particles 2 in the second embodiment is 50 nm or more and 500 nm or less, preferably 50 nm to 300 nm, as measured by a light scattering method. By including irregularly shaped silica particles 2 having an average particle size of 500 nm or less in a coating composition, the silica particles 2 are more likely to remain on the surface of a substrate 4 that has water absorption or porosity, and thus the coating film 1 is more likely to be formed. Furthermore, a silica film formed by irregularly shaped silica particles 2 having an average particle size of 500 nm or less has very small voids and a low density, and therefore is less susceptible to adhesion of dirt due to intermolecular forces. Furthermore, since the irregularly shaped silica particles 2 having an average particle size of 500 nm or less have a large surface area per unit volume, the area where the silica particles 2 adhere to each other in the silica film becomes large, resulting in a coating film 1 with sufficient strength. Also, in a silica film made of irregularly shaped silica particles 2 having an average particle size of 500 nm or less, the irregularly shaped silica particles 2 are folded and entangled to adhere to each other, resulting in a coating film 1 with sufficient strength.

[0060] Here, if the average particle size of the silica particles 2 in the coating composition is less than 50 nm, when the coating composition is applied to a substrate 4 having water absorption properties, porous properties, or the like, the silica particles 2 will easily penetrate into the substrate 4 due to capillary action. As a result, it may become impossible to control the ratio of the silica particles 2 to the fluororesin particles 3 in the coating film 1 on the surface of the substrate 4, which may make it difficult to maintain high antifouling performance. On the other hand, if the average particle size of the irregularly shaped silica particles 2 is longer than 500 nm, the silica particles 2 will be less likely to entangle with each other in the silica film, and the voids in the silica film will become coarse, which may reduce the strength of the coating film 1. Furthermore, the coating film 1 will have excessively large irregularities, which may make it easier for hydrophilic stains to adhere, and may prevent the desired antifouling performance from being obtained.

[0061] If the coating composition contains spherical silica particles 2 having an average particle size longer than 50 nm, there is a risk that the coating film 1 will not have sufficient strength. Furthermore, spherical silica particles 2 having an average particle size longer than 50 nm have a smaller surface area per unit volume than irregularly shaped silica particles 2 having a similar average particle size, which increases the density of the silica film and may increase the adhesion of dirt due to intermolecular forces.

[0062] The substrate 4, which has water-absorbent or porous properties, is contaminated with mold or organic contaminants before the coating composition is applied. The mold adheres to the surface of the substrate 4 and the wall surfaces of the pores 5 as spores or hyphae. The humidity inside the substrate 4 is easily maintained constant, creating an environment conducive to mold growth. Furthermore, in a substrate 4 on which mold has grown, simply sterilizing the surface of the substrate 4 will result in the mold remaining inside the substrate 4, leading to recurrence of mold growth. Furthermore, organic contaminants, which serve as nutrients for mold, also adhere to the surface of the substrate 4 and the wall surfaces of the pores 5. The organic contaminants attached to the substrate 4 serve as nutrients for mold growth. For these reasons, in order to inhibit mold growth, it is necessary to remove the mold and organic contaminants attached to the surface of the substrate 4 and the wall surfaces of the pores 5 inside the substrate 4.

[0063] When the coating composition of the second embodiment is applied to the substrate 4, the chlorine bleach decomposes and removes mold, organic contaminants, and the like attached to the surface of the substrate 4 and the wall surfaces of the pores 5. That is, the chlorine bleach that penetrates into the interior of the substrate 4 due to capillary action in the pores 5 of the substrate 4 decomposes and removes mold, organic contaminants, and the like attached to the interior of the substrate 4. Furthermore, the chlorine bleach that does not penetrate into the interior of the substrate 4 remains on the surface of the substrate 4 together with the silica particles 2 and the fluororesin particles 3, thereby decomposing and removing mold, organic contaminants, and the like attached to the surface of the substrate 4.

[0064] The water contained in the coating composition gradually volatilizes upon contact with air. The coating composition comes into contact with air at the surface of the substrate 4 to which the coating composition is applied and at the pores 5 inside the substrate 4 into which the coating composition has permeated. Here, the chlorine bleach on the surface of the substrate 4 decomposes along with mold, organic contaminants, and the like as the water on the surface of the substrate 4 volatilizes. As the water on the surface of the substrate 4 volatilizes, the silica particles 2 and fluororesin particles 3 on the surface of the substrate 4 become more cohesive, forming a coating film 1. Meanwhile, the water that has permeated the pores 5 volatilizes on the surface of the coating film 1 through the fine voids in the coating film 1.

[0065] Note that air flow is more restricted in the pores 5 inside the substrate 4 than on the surface of the substrate 4. Furthermore, the contact area between the liquid that has penetrated into the pores 5 and the air is often smaller than the contact area between the liquid and the air on the surface of the substrate 4. Therefore, the volatilization rate of the liquid in the pores 5 may be slower than the volatilization rate of the liquid on the surface of the substrate 4. As a result, mold, organic contaminants, etc. in the pores 5 inside the substrate 4 are exposed to the aqueous solution of chlorine bleach for a long period of time. This allows excellent mold prevention performance to be exhibited not only on the surface of the substrate 4 but also inside.

[0066] Examples of the coating compositions according to Embodiments 1 and 2 will be described below. FIG. 5 is a diagram showing several examples of the proportions of the components in the coating composition according to Embodiment 1. Note that FIG. 5 shows the several examples in a table format. FIG. 5 also shows the proportions of the components in each of the coating compositions according to several comparative examples.

[0067] The coating compositions of Examples 1 to 9 in Figure 5 contain sodium hypochlorite as a chlorine bleaching agent. The coating compositions of Examples 1 to 3 contain 1.0 mass% silica particles 2 and 0.8 mass% fluororesin particles 3. The coating composition of Example 1 contains 1.000 mass% sodium hypochlorite, the coating composition of Example 2 contains 0.001 mass% sodium hypochlorite, and the coating composition of Example 3 contains 4.000 mass% sodium hypochlorite. The silica particles 2 contained in the coating compositions of Examples 1 to 3 are spherical and have an average particle size of 6 nm. The fluororesin particles 3 contained in the coating compositions of Examples 1 to 3 are PTFE particles with an average particle size of 250 nm. The coating compositions according to Examples 1 to 3 were prepared by stirring and mixing pure water, colloidal silica containing the silica particles 2, and a PTFE dispersion containing the PTFE particles, and then further adding an aqueous sodium hypochlorite solution containing sodium hypochlorite and stirring and mixing the mixture.

[0068] The coating composition of Example 4 contains 1.0 mass% silica particles 2, 0.8 mass% fluororesin particles 3, and 0.500 mass% sodium hypochlorite. The coating composition of Example 5 contains 0.2 mass% silica particles 2, 0.1 mass% fluororesin particles 3, and 0.500 mass% sodium hypochlorite. The coating composition of Example 6 contains 4.0 mass% silica particles 2, 3.2 mass% fluororesin particles 3, and 2.000 mass% sodium hypochlorite. The silica particles 2 contained in the coating compositions of Examples 4 to 6 are spherical and have an average particle size of 20 nm. The fluororesin particles 3 contained in the coating compositions of Examples 4 to 6 are PTFE particles with an average particle size of 1000 nm. The coating compositions according to Examples 4 to 6 were prepared by stirring and mixing pure water, colloidal silica containing the silica particles 2, and a PTFE dispersion containing the PTFE particles, and then further adding an aqueous sodium hypochlorite solution containing sodium hypochlorite and stirring and mixing the mixture.

[0069] The coating composition of Example 7 contains 2.0 mass% silica particles 2, 2.0 mass% fluororesin particles 3, and 1.000 mass% sodium hypochlorite. The coating composition of Example 8 contains 1.0 mass% silica particles 2, 1.5 mass% fluororesin particles 3, and 1.000 mass% sodium hypochlorite. The coating composition of Example 9 contains 1.0 mass% silica particles 2, 0.3 mass% fluororesin particles 3, and 1.000 mass% sodium hypochlorite. The silica particles 2 contained in the coating compositions of Examples 7 to 9 are spherical and have an average particle size of 6 nm. The fluororesin particles 3 contained in the coating compositions of Examples 7 to 9 are PTFE particles with an average particle size of 8,000 nm. The coating compositions according to Examples 7 to 9 were prepared by stirring and mixing pure water, colloidal silica containing the silica particles 2, and a PTFE dispersion containing the PTFE particles, and then further adding an aqueous sodium hypochlorite solution containing sodium hypochlorite and stirring and mixing the mixture.

[0070] The coating composition according to Comparative Example 1 shown in the table of Fig. 5 contains PTFE particles having an average particle size of 20,000 nm as the fluororesin particles 3. The coating composition according to Comparative Example 1 was prepared by stirring and mixing pure water and a PTFE dispersion containing the PTFE particles. The coating composition of Comparative Example 1 contains 0.8 mass% of the fluororesin particles 3.

[0071] The coating composition of Comparative Example 2 shown in the table of Figure 5 contains PTFE particles with an average particle size of 250 nm as fluororesin particles 3 and sodium hypochlorite as a chlorine bleaching agent. The silica particles 2 contained in the coating composition of Comparative Example 2 are spherical and have an average particle size of 10 nm. The coating composition of Comparative Example 2 was prepared by stirring and mixing pure water, colloidal silica containing the silica particles, and a PTFE dispersion containing the PTFE particles, and then further adding and stirring an aqueous sodium hypochlorite solution containing sodium hypochlorite. The coating composition of Comparative Example 2 contains 1.0 mass% silica particles 2, 1.0 mass% fluororesin particles 3, and 10.000 mass% sodium hypochlorite.

[0072] The coating composition according to Comparative Example 3 shown in the table of Figure 5 contains sodium hypochlorite as a chlorine bleaching agent. The silica particles 2 contained in the coating composition according to Comparative Example 3 are spherical and have an average particle size of 30 nm. The coating composition according to Comparative Example 3 was prepared by stirring and mixing pure water and colloidal silica containing the silica particles 2, and then further adding and stirring an aqueous sodium hypochlorite solution containing sodium hypochlorite. The coating composition according to Comparative Example 3 contains 10.0 mass% of silica particles 2 and 1.000 mass% of sodium hypochlorite.

[0073] An experiment to evaluate the liquid stability was carried out for the coating compositions of Examples 1 to 9 and Comparative Examples 1 to 3. In addition, the coating compositions of Examples 1 to 9 and Comparative Examples 1 to 3 were applied to a substrate 4 by dipping, and then the substrate 4 after application of the coating composition was placed on a sample stand and allowed to dry naturally at room temperature for about 10 minutes, thereby forming a coating film 1 on the substrate 4. In this experiment, a polypropylene substrate was used as the substrate 4.

[0074] Hereinafter, the evaluation results of the liquid stability of the coating compositions of Examples 1 to 9 and Comparative Examples 1 to 3, and the evaluation results of the properties, antifouling performance, weather resistance, and antifungal performance of the coating films 1 obtained from the coating compositions will be described with reference to Fig. 6. Fig. 6 is a diagram illustrating the evaluation results of the coating compositions of Examples 1 to 9 and Comparative Examples 1 to 3. Fig. 6 shows the evaluation results of Examples 1 to 9 and Comparative Examples 1 to 3 in a table format.

[0075] The liquid stability of the coating composition was evaluated by visual observation, and the properties of the coating film 1 were evaluated by visual observation and observation using an existing scanning electron microscope (SU3800, manufactured by Hitachi High-Tech Corporation).

[0076] In Figure 6, the antifouling performance is shown by sand and dust adhesion. Sand and dust adhesion corresponds to the adhesion of hydrophilic dirt. Sand and dust adhesion was evaluated as follows: a predetermined amount of Kanto loam dust was blown onto the surface of the coating film 1 with air, and the discoloration caused by the adhesion of the Kanto loam dust was visually observed and evaluated on a five-point scale. In this five-point scale evaluation, the greater the amount of Kanto loam dust adhesion, the higher the number, with 1 indicating almost no adhesion of Kanto loam dust and 5 indicating a large amount of adhesion of Kanto loam dust.

[0077] Dust adhesion corresponds to the adhesion of hydrophobic dirt. The dust adhesion was evaluated as follows: a predetermined amount of carbon black was sprayed onto the surface of the coating film 1 with air, and the coloration due to the adhesion of the carbon black was visually observed and evaluated on a 5-point scale. In the 5-point scale evaluation, the greater the amount of carbon black adhesion, the higher the number, with 1 indicating almost no adhesion of carbon black and 5 indicating heavy adhesion of carbon black.

[0078] Weather resistance was evaluated as follows: Using an existing highly accelerated weather resistance tester (Iwasaki Electric Co., Ltd.; XER-W83), the coating film 1 was exposed to a light source for 100 hours, and discoloration was visually observed and rated on a 5-point scale. In this 5-point scale, the greater the degree of discoloration, the higher the number. Using the color of the substrate 4 on which the coating film 1 is not formed as the standard, a score of 1 indicates that there is almost no difference in color from the standard, and a score of 5 indicates that there is significant discoloration and that the color is significantly different from the standard.

[0079] The antifungal performance was evaluated as follows. Each of the coating compositions of Examples 1 to 9 and Comparative Examples 1 to 3 was applied to a substrate 4 by dipping. The substrate 4 after application of the coating composition was then placed on a sample stand and allowed to air dry at room temperature for approximately 10 minutes, forming a coating film 1 on the substrate 4. The coating film 1 was then exposed to soil dust containing molds such as Aspergillus niger, Penicillium spp., and Trichoderma niger, and the molds were cultured for 168 hours at a temperature of 35°C and a humidity of 90%. The state of mold growth on the surface of the coating film 1 was then evaluated visually and using an existing optical microscope (DSX1000, manufactured by Olympus Corporation) on a five-point scale. In this five-point scale, the greater the degree of mold growth, the higher the value, with 1 representing the minimum degree of mold growth and 5 representing the maximum degree of mold growth.

[0080] 6, it was confirmed that each of the coating compositions of Examples 1 to 9 and Comparative Examples 1 and 3 had high stability as a liquid formulation without causing aggregation or precipitation. In contrast, the coating composition of Comparative Example 2 contained an excessive amount of sodium hypochlorite, which caused aggregation and precipitation, making it impossible to ensure stability as a liquid formulation.

[0081] With each of the coating compositions of Examples 1 to 9 and Comparative Example 1, a uniform coating film 1 could be formed on the substrate 4. In contrast, with the coating composition of Comparative Example 2, aggregation and precipitation occurred in the liquid, and therefore a film could not be formed on the substrate 4. Furthermore, with the coating composition of Comparative Example 3, the silica particles 2 were coarse spherical particles with an average particle size exceeding 25 nm, and therefore a non-uniform coating film 1 was formed on the substrate 4. As a result, the obtained coating film 1 was prone to cracking and peeling.

[0082] The coating films 1 obtained from the coating compositions of Examples 1 to 9 had smaller values ​​in the evaluation of sand and dust adhesion resistance, dust adhesion resistance, and antifungal performance than the coating films 1 obtained from the coating compositions of Comparative Examples 1 and 3. That is, the coating films 1 obtained from the coating compositions of Examples 1 to 9 had better antifouling performance and antifungal performance than the coating films 1 obtained from the coating compositions of Comparative Examples 1 and 3. In particular, the coating film 1 obtained from the coating composition of Example 1 had the best sand and dust adhesion resistance, dust adhesion resistance, and antifungal performance.

[0083] The weather resistance of the coating films 1 obtained from the coating compositions of Examples 1 to 9 was evaluated to have a value of 1, which was good.

[0084] Next, examples of the coating composition according to the second embodiment will be described with reference to FIG. 7. FIG. 7 is a diagram showing several examples of the proportions of the components in the coating composition according to the second embodiment. Note that FIG. 7 also shows the several examples in a table format. In addition, FIG. 7 also shows the proportions of the components in the coating composition according to Example 1 for comparison between the first embodiment and the second embodiment. In addition, FIG. 7 also shows the proportions of the components in the coating composition according to Comparative Example 4.

[0085] 7 contains sodium hypochlorite as a chlorine bleaching agent. Each of the coating compositions of Examples 10 to 11 and Comparative Example 4 contains 1.0 mass% of silica particles 2 and 0.8 mass% of fluororesin particles 3. The coating composition of Example 10 contains 1.000 mass% of sodium hypochlorite, and each of the coating compositions of Example 11 and Comparative Example 4 contains 2.000 mass% of sodium hypochlorite.

[0086] The silica particles 2 contained in the coating composition of Example 10 are acicular and have an average particle size of 100 nm. The fluororesin particles 3 contained in the coating composition of Example 10 are PTFE particles with an average particle size of 250 nm. The coating composition of Example 10 is prepared by stirring and mixing pure water, colloidal silica containing the silica particles, and a PTFE dispersion containing the PTFE particles, and then further adding and stirring an aqueous sodium hypochlorite solution containing sodium hypochlorite.

[0087] The silica particles 2 contained in the coating composition of Example 11 are beaded and have an average particle size of 400 nm. The fluororesin particles 3 contained in the coating composition of Example 11 are PTFE particles with an average particle size of 250 nm. The coating composition of Example 11 is prepared by stirring and mixing pure water, colloidal silica containing the silica particles, and a PTFE dispersion containing the PTFE particles, and then further adding an aqueous sodium hypochlorite solution containing sodium hypochlorite and stirring and mixing.

[0088] The silica particles 2 contained in the coating composition of Comparative Example 4 are scaly and have an average particle size of 1000 nm. The fluororesin particles 3 contained in the coating composition of Comparative Example 4 are PTFE particles with an average particle size of 250 nm. The coating composition of Comparative Example 4 is prepared by stirring and mixing pure water, colloidal silica containing the silica particles, and a PTFE dispersion containing the PTFE particles, and then further adding an aqueous sodium hypochlorite solution containing sodium hypochlorite and stirring and mixing.

[0089] An experiment to evaluate the liquid stability was carried out for the coating compositions of Examples 10 to 11 and Comparative Example 4. In addition, the coating compositions of Examples 10 to 11 and Comparative Example 4 were applied to a substrate 4 by dipping, and then the substrate 4 after application of the coating composition was placed on a sample stand and allowed to dry naturally at room temperature for about 10 minutes, thereby forming a coating film 1 on the substrate 4. In this experiment, a polypropylene substrate was used as the substrate 4.

[0090] Hereinafter, the evaluation results of the liquid stability of the coating compositions of Examples 10 to 11 and Comparative Example 4, and the evaluation results of the properties, antifouling performance, weather resistance, and antifungal performance of the coating films 1 obtained from the coating compositions will be described with reference to Fig. 8. Fig. 8 is a diagram illustrating the evaluation results of the coating compositions of Examples 10 to 11 and Comparative Example 4. For comparison, Fig. 8 also shows the evaluation results of Example 1. Fig. 8 also shows the evaluation results of Example 1, Examples 10 to 11, and Comparative Example 4 in a table format.

[0091] As shown in Figure 8, similar to Example 1, the coating compositions of Examples 10 to 11 and Comparative Example 4 were confirmed to be highly stable as liquid formulations without causing aggregation or precipitation. Furthermore, similar to Example 1, a uniform coating film 1 was obtained on a substrate 4 using the coating compositions of Examples 10 to 11. On the other hand, in Comparative Example 4, the silica particles 2 in the coating composition were coarse, irregularly shaped particles with an average particle size exceeding 500 nm, and therefore a non-uniform coating film 1 was formed on the substrate 4, and cracks occurred in the coating film 1, causing some of the coarse particles to fall off from the surface.

[0092] As shown in Figure 8, the coating films 1 obtained from the coating compositions of Examples 10 and 11 had smaller values ​​in the evaluation of sand and dust adhesion, dust adhesion, and antifungal performance, and had better antifouling and antifungal performance, compared to the coating film 1 obtained from the coating composition of Comparative Example 4. In addition, the weather resistance of the coating films obtained from the coating compositions of Examples 10 and 11 was also good.

[0093] Other examples of the coating compositions according to Embodiments 1 and 2 will be described below with reference to Fig. 9. Fig. 9 is a diagram showing several examples of the proportions of the components in the coating compositions according to Embodiments 1 and 2. Note that Fig. 9 also shows the several examples in a table format. Fig. 9 also shows the proportions of the components in the coating compositions according to Comparative Examples 5 to 7.

[0094] 9 , the coating compositions of Examples 12 to 14 and Comparative Examples 5 to 7 contain sodium hypochlorite as a chlorine bleaching agent. The coating compositions of Examples 12, 14, and Comparative Examples 5 to 7 contain 1.000 mass% sodium hypochlorite, and the coating composition of Example 13 contains 2.000 mass% sodium hypochlorite. The coating composition of Example 12 contains 4.0 mass% silica particles 2 and 0.4 mass% fluororesin particles 3. The coating compositions of Examples 13 and 14 contain 2.0 mass% silica particles 2 and 1.6 mass% fluororesin particles 3. The coating compositions of Comparative Examples 5 to 7 contain 1.0 mass% silica particles 2 and 0.8 mass% fluororesin particles 3.

[0095] The silica particles 2 contained in the coating composition of Example 12 are spherical and have an average particle size of 20 nm. The fluororesin particles 3 contained in the coating composition of Example 12 are PTFE particles with an average particle size of 1000 nm. The coating composition of Example 12 is prepared by stirring and mixing pure water, colloidal silica containing the silica particles, and a PTFE dispersion containing the PTFE particles, and then further adding and stirring an aqueous sodium hypochlorite solution containing sodium hypochlorite.

[0096] The silica particles 2 contained in the coating composition of Example 13 are acicular and have an average particle size of 100 nm. The fluororesin particles 3 contained in the coating composition of Example 12 are PTFE particles with an average particle size of 250 nm. The coating composition of Example 13 is prepared by stirring and mixing pure water, colloidal silica containing the silica particles, and a PTFE dispersion containing the PTFE particles, and then further adding and stirring an aqueous sodium hypochlorite solution containing sodium hypochlorite.

[0097] The silica particles 2 contained in the coating composition of Example 14 are beaded and have an average particle size of 400 nm. The fluororesin particles 3 contained in the coating composition of Example 14 are PTFE particles with an average particle size of 250 nm. The coating composition of Example 14 is prepared by stirring and mixing pure water, colloidal silica containing the silica particles, and a PTFE dispersion containing the PTFE particles, and then further adding an aqueous sodium hypochlorite solution containing sodium hypochlorite and stirring and mixing.

[0098] The silica particles 2 contained in the coating composition of Comparative Example 5 are spherical and have an average particle size of 30 nm. The fluororesin particles 3 contained in the coating composition of Comparative Example 5 are PTFE particles with an average particle size of 250 nm. The coating composition of Comparative Example 5 is prepared by stirring and mixing pure water, colloidal silica containing the silica particles, and a PTFE dispersion containing the PTFE particles, and then further adding an aqueous sodium hypochlorite solution containing sodium hypochlorite and stirring and mixing.

[0099] The silica particles 2 contained in the coating composition of Comparative Example 6 are spherical and have an average particle size of 100 nm. The fluororesin particles 3 contained in the coating composition of Comparative Example 6 are PTFE particles with an average particle size of 250 nm. The coating composition of Comparative Example 6 is prepared by stirring and mixing pure water, colloidal silica containing the silica particles, and a PTFE dispersion containing the PTFE particles, and then further adding an aqueous sodium hypochlorite solution containing sodium hypochlorite and stirring and mixing.

[0100] The silica particles 2 contained in the coating composition of Comparative Example 7 are acicular and have an average particle size of 1000 nm. The fluororesin particles 3 contained in the coating composition of Comparative Example 7 are PTFE particles with an average particle size of 250 nm. The coating composition of Comparative Example 7 is prepared by stirring and mixing pure water, colloidal silica containing the silica particles, and a PTFE dispersion containing the PTFE particles, and then further adding an aqueous sodium hypochlorite solution containing sodium hypochlorite and stirring and mixing.

[0101] An experiment to evaluate the liquid stability was carried out for the coating compositions of Examples 12 to 14 and Comparative Examples 5 to 7. The coating compositions of Examples 12 to 14 and Comparative Examples 5 to 7 were applied to a substrate 4 by dipping, and then the substrate 4 after application of the coating composition was set up on a sample stand and allowed to dry naturally, thereby forming a coating film 1 on the substrate 4. In this experiment, a gypsum board substrate, which is a porous substrate, was used as the substrate 4.

[0102] Hereinafter, the evaluation results of the liquid stability of the coating compositions of Examples 12 to 14 and Comparative Examples 5 to 7, and the evaluation results of the properties, antifouling performance, weather resistance, and antifungal performance of the coating films 1 obtained from the coating compositions will be described with reference to Fig. 10. Fig. 10 is a diagram illustrating the evaluation results of the coating compositions of Examples 12 to 14 and Comparative Examples 5 to 7. Note that Fig. 10 also shows the evaluation results of Examples 12 to 14 and Comparative Examples 5 to 7 in a table format.

[0103] 10, it was confirmed that the coating compositions of Examples 12 to 14 and Comparative Examples 5 to 7 did not undergo aggregation or precipitation and were highly stable as liquid formulations. Furthermore, the coating compositions of Examples 12 to 14 were able to form a uniform coating film 1 on the gypsum board substrate.

[0104] On the other hand, in Comparative Examples 5 and 6, the silica particles 2 in the coating composition were coarse, spherical particles with an average particle size exceeding 25 nm, and therefore a non-uniform coating film 1 was formed on the gypsum board substrate. Cracks occurred in the coating film 1, and it easily peeled off. In Comparative Example 7, the silica particles 2 in the coating composition were coarse, irregularly shaped particles with an average particle size exceeding 500 nm, and therefore a non-uniform coating film 1 was formed on the gypsum board substrate. As a result, cracks occurred in the coating film 1, and some of the coarse particles fell off from the surface.

[0105] The coating films 1 obtained from the coating compositions of Examples 12 to 14 had lower values ​​in the evaluation of sand and dust adhesion, dust adhesion, and antifungal performance, and had better antifouling and antifungal performance, compared to the coating films 1 obtained from the coating compositions of Comparative Examples 5 to 7. In particular, the coating composition of Example 13 had the best sand and dust adhesion, dust adhesion, and antifungal performance. Furthermore, the weather resistance of the coating films 1 obtained from the coating compositions of Examples 12 to 14 was good.

[0106] The following describes the effects of the coating composition, coating method, and mildew treatment method according to Embodiments 1 and 2. The coating composition according to Embodiments 1 and 2 contains 5% by mass or less of a plurality of silica particles 2, a plurality of fluororesin particles 3, 0.001% by mass or more and 5% by mass or less of a chlorine-based bleaching agent, and water.

[0107] According to the above configuration, the plurality of silica particles 2 and the plurality of fluororesin particles 3 contained in the coating composition are not decomposed by the chlorine bleach, thereby ensuring the stability of the coating composition. Furthermore, since the proportion of the chlorine bleach in the coating composition is 5% by mass or less, precipitation due to aggregation of two or more fluororesin particles 3 is unlikely to occur, ensuring the stability of the coating composition. Furthermore, since the silica particles 2 are hydrophilic, hydrophobic stains are less likely to adhere to the coating film 1, and since the fluororesin particles 3 are hydrophobic, hydrophilic stains are less likely to adhere to the coating film 1. Furthermore, since the coating composition contains 0.001% by mass or more of the chlorine bleach, it is possible to decompose mold, organic contaminants, etc. on the surface of the substrate 4 to be coated and on the surface and interior of the coating film 1. Therefore, the plurality of silica particles 2, the plurality of fluororesin particles 3, and the chlorine bleach provide high antifouling performance, thereby improving antifungal performance. Furthermore, because the content of the plurality of silica particles 2 in the coating composition is 5 mass% or less, peeling of the coating film 1 is suppressed, and antifouling and antifungal properties are maintained. Thus, the coating compositions and coating methods according to Embodiments 1 and 2 ensure the stability of the coating composition and enable the production of a coating film 1 having high antifouling and antifungal properties. Furthermore, since the coating film 1 contains silica particles 2 with low light scattering, the transparency of the coating film 1 is improved, and even when the coating film 1 is applied to a substrate 4, changes in the color tone and texture of the substrate 4 can be suppressed. Therefore, the designability of the substrate 4 is ensured by the maintenance of the color tone and texture of the substrate 4 due to the transparency of the coating film 1, the suppression of pigmentation due to the above-mentioned high antifungal properties, the suppression of peeling of the coating film 1, and the high weather resistance of the coating film 1.

[0108] The plurality of silica particles 2 according to the first embodiment have an average particle size of 25 nm or less, and each of the plurality of silica particles 2 is a spherical particle. Because the average particle size of the silica particles 2 in the coating composition is 25 nm or less, the silica particles 2 tend to aggregate easily when the coating film 1 is formed by drying, facilitating solidification of the coating composition. Furthermore, compared to when the average particle size of the silica particles 2 is greater than 25 nm, more silica particles 2 are dissolved in equilibrium in the coating composition, making it possible to form a uniform, high-strength coating film 1 that is inhibited from cracking and peeling.

[0109] In the second embodiment, the plurality of silica particles 2 have an average particle size of 50 nm or more and 1000 nm or less, and each of the plurality of silica particles 2 is an irregularly shaped particle having a needle-like, scale-like, chain-like, bead-like, or pearl necklace-like shape. Because the average particle size of the silica particles 2 is 50 nm or more, the silica particles 2 in the substrate 4, which has water-absorbent or porous properties, are prevented from penetrating into the substrate 4 by capillary action. This makes it possible to control the ratio of silica particles 2 to fluororesin particles 3 on the surface of the substrate 4, allowing the coating film 1 to maintain high antifouling performance. Furthermore, the irregularly shaped silica particles 2 in the coating film 1 are folded, entangled, and adhered to each other, resulting in a coating film 1 with sufficient strength.

[0110] The average particle size of the plurality of fluororesin particles 3 according to the first and second embodiments is 50 nm or more and 10,000 nm or less. This allows the fluororesin particles 3 to be appropriately dispersed in the coating composition, resulting in a stable coating composition. In addition, the fluororesin particles 3 are easily exposed on the surface of the coating film 1, resulting in good antifouling performance.

[0111] In the first and second embodiments, the mass ratio of the plurality of silica particles 2 to the plurality of fluororesin particles 3 is in the range of 40:60 to 95:5. As a result, a coating film 1 having a good antifouling performance and a well-balanced mixture of hydrophilic portions originating from the silica particles 2 and hydrophobic portions originating from the fluororesin particles 3 can be obtained by drying at room temperature.

[0112] Although the embodiments have been described above, the contents of the present disclosure are not limited to the embodiments and include conceivable equivalents. Furthermore, the configurations described in the first and second embodiments and their modifications can be combined with each other as long as the functions and operations are not impaired.

[0113] 1 Coating film, 2 Silica particles, 3 Fluororesin particles, 4 Substrate, 5 Pores

Claims

1. A coating composition comprising: 5% by mass or less of silica particles; fluororesin particles; 0.001% by mass or more and 5% by mass or less of a chlorine bleaching agent; and water.

2. The coating composition according to claim 1, wherein the silica particles have an average particle size of 25 nm or less and are spherical particles.

3. The coating composition according to claim 1, wherein the silica particles have an average particle size of 50 nm or more and 1000 nm or less, and the silica particles are irregularly shaped particles in the form of needles, scales, chains, beads, or pearl necklaces.

4. The coating composition according to any one of claims 1 to 3, wherein the average particle size of the fluororesin particles is 50 nm or more and 10,000 nm or less.

5. The coating composition according to any one of claims 1 to 4, wherein the mass ratio of the silica particles to the fluororesin particles is in the range of 40:60 to 95:

5.

6. A method for coating a substrate, comprising applying a coating composition containing 5% by mass or less of silica particles, fluororesin particles, 0.001% by mass or more and 5% by mass or less of a chlorine-based bleaching agent, and water to the substrate to form a coating film on the surface of the substrate.

7. A method for treating mold, comprising applying to a substrate a coating composition containing 5% by mass or less of silica particles, fluororesin particles, 0.001% by mass or more and 5% by mass or less of a chlorine bleach, and water.

Citation Information

Patent Citations

  • Mildew-proof coating and production process thereof

    CN110643211A

  • Efficient mildew removing and preventing agent for treating mildew and spots on wall surface

    CN113480885A

  • Water-based environment-friendly antibacterial paint and preparation method thereof

    CN114507464A

  • Air conditioner and coating composition

    JP2010096437A

  • Water-based coating composition and coating method using the same

    JP2012001586A