Cemented carbide and cutting tool

The cemented carbide composition, featuring tungsten carbide, cobalt, and titanium/nobium/zirconium phases, addresses the challenge of wear and fracture resistance in cutting tools, ensuring extended tool life under demanding machining conditions by optimizing Vickers hardness and cobalt content.

WO2024247221A1PCT designated stage expired Publication Date: 2024-12-05SUMITOMO ELECTRIC HARDMETAL CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/020474
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Recent advancements in cutting processes have made materials increasingly difficult to cut, necessitating improved machining efficiency with stricter conditions such as higher cutting speed, feed rate, and depth of cut, which existing cemented carbide cutting tools cannot effectively address in terms of wear resistance and tool longevity.

Method used

A cemented carbide composition comprising a first phase of tungsten carbide particles (65-85% by volume), a second phase of cobalt (3-15% by mass), and a third phase of titanium, tantalum, niobium, and zirconium, with specific Vickers hardness gradients to enhance wear resistance and fracture resistance, ensuring a longer tool life.

Benefits of technology

The cemented carbide composition provides cutting tools with excellent wear resistance and fracture resistance, maintaining tool longevity even under stringent machining conditions by optimizing Vickers hardness gradients and cobalt distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023020474_05122024_PF_FP_ABST
    Figure JP2023020474_05122024_PF_FP_ABST
Patent Text Reader

Abstract

This cemented carbide includes a first phase, a second phase, and a third phase. The first phase is composed of a plurality of tungsten carbide particles, and the content of the first phase of the cemented carbide is 65 vol.% to 85 vol.% inclusive. The second phase is composed of cobalt, and the cobalt content C5 of the cemented carbide is 3 mass% to 15 mass% inclusive. The third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium and tungsten, and at least one of carbon and nitrogen. The third phase does not contain tungsten carbide, and the total content C of titanium, tantalum, niobium, and zirconium of the cemented carbide is 2 mass% to 8 mass% inclusive. The Vickers hardness a of the cemented carbide is 12.5 GPa to 14.5 GPa inclusive, the Vickers hardness a being measured in the cemented carbide at a point P1 where the distance from the surface of the cemented carbide along a direction normal to the surface is 5 μm. The cemented carbide includes a first region sandwiched between a virtual surface Q1 having a distance of 5 μm from the surface and a virtual surface Q4 having a distance of 200 μm from the surface, the first region having a second region sandwiched between a virtual surface Q2 having a distance of 10 μm from the surface and a virtual surface Q3 having a distance of 50 μm from the surface. In the first region, a point P2 indicating a Vickers hardness b, which is the maximum value of the Vickers hardness, is present in the second region. A difference b-a between the Vickers hardness b and the Vickers hardness a is more than or equal to 1.8 GPa.
Need to check novelty before this filing date? Find Prior Art

Description

Cemented Carbide and Cutting Tools

[0001] The present disclosure relates to cemented carbides and cutting tools.

[0002] Conventionally, cemented carbide alloys having a hard phase mainly composed of tungsten carbide (WC) and a binder phase mainly composed of an iron-group element have been used as materials for cutting tools. The cemented carbide alloy described in Patent Document 1 includes, as a hard phase, a phase composed of at least one composite compound of carbide, nitride, or carbonitride containing tungsten (W) and a metal element other than tungsten, in addition to the hard phase mainly composed of WC. The cemented carbide alloy aims to improve chipping resistance by bonding WC particles with composite compound particles.

[0003] JP 2016-20541 A

[0004] The cemented carbide of the present disclosure is a cemented carbide including a first phase, a second phase, and a third phase, wherein the first phase is composed of a plurality of tungsten carbide particles, the content of the first phase in the cemented carbide is 65% by volume or more and 85% by volume or less, the second phase is composed of cobalt, and the cobalt content C5 of the cemented carbide is 3% by mass or more and 15% by mass or less, the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen, and the third phase does not contain tungsten carbide, the total content C of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more and 8% by mass or less, and the Vickers hardness a of the cemented carbide is 12.5 GPa or more and 14.5 GPa or less, The Vickers hardness a is measured at a point P1 in the cemented carbide at a distance of 5 μm from the surface of the cemented carbide in a direction normal to the surface, the cemented carbide includes a first region sandwiched between an imaginary plane Q1 at a distance of 5 μm from the surface and an imaginary plane Q4 at a distance of 200 μm from the surface, the first region having a second region sandwiched between an imaginary plane Q2 at a distance of 10 μm from the surface and an imaginary plane Q3 at a distance of 50 μm from the surface, in the first region, a point P2 exhibiting a Vickers hardness b that is the maximum value of the Vickers hardness is present in the second region, and the difference b-a between the Vickers hardness b and the Vickers hardness a is 1.8 GPa or more.

[0005] Fig. 1 is a diagram schematically showing a cross section of a cemented carbide according to embodiment 1. Fig. 2 is a graph showing an example of the relationship between the distance from the surface of the cemented carbide according to embodiment 1 and the Vickers hardness, and an example of the relationship between the distance from the surface of the cemented carbide according to embodiment 1 and the respective contents (mass%) of titanium, tantalum, niobium, and cobalt. Fig. 3 is a diagram for explaining a method for measuring the Vickers hardness of a cemented carbide.

[0006] [Problem to be Solved by the Present Disclosure] In recent years, workpiece materials have become increasingly difficult to cut in cutting processes. Furthermore, demands for improved processing efficiency have led to stricter processing conditions, such as increased cutting speeds, feed rates, and depths of cut.

[0007] Therefore, an object of the present disclosure is to provide a cemented carbide that, when used as a tool material, can provide a cutting tool that has excellent wear resistance and fracture resistance and a long tool life, and to provide a cutting tool that has a long tool life.

[0008] [Effects of the Present Disclosure] According to the present disclosure, it is possible to provide a cemented carbide that, when used as a tool material, can provide a cutting tool that has excellent wear resistance and fracture resistance and a long tool life, as well as a cutting tool that has a long tool life.

[0009] [Description of Embodiments of the Present Disclosure] First, embodiments of the present disclosure will be listed and described. (1) The cemented carbide of the present disclosure is a cemented carbide including a first phase, a second phase, and a third phase, wherein the first phase is composed of a plurality of tungsten carbide particles, the content of the first phase in the cemented carbide is 65% by volume or more and 85% by volume or less, the second phase is composed of cobalt, and the cobalt content C5 of the cemented carbide is 3% by mass or more and 15% by mass or less, the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen, and the third phase does not contain tungsten carbide, the total content C of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more and 8% by mass or less, and the Vickers hardness a of the cemented carbide is 12.5 GPa or more and 14.5 GPa or less, The Vickers hardness a is measured at a point P1 in the cemented carbide at a distance of 5 μm from the surface of the cemented carbide in a direction normal to the surface, the cemented carbide includes a first region sandwiched between an imaginary plane Q1 at a distance of 5 μm from the surface and an imaginary plane Q4 at a distance of 200 μm from the surface, the first region having a second region sandwiched between an imaginary plane Q2 at a distance of 10 μm from the surface and an imaginary plane Q3 at a distance of 50 μm from the surface, in the first region, a point P2 exhibiting a Vickers hardness b that is the maximum value of the Vickers hardness is present in the second region, and the difference b-a between the Vickers hardness b and the Vickers hardness a is 1.8 GPa or more.

[0010] When used as a tool material, the cemented carbide of the present disclosure can provide a cutting tool that has excellent wear resistance and chipping resistance and can have a long tool life.

[0011] (2) In the above (1), in the cemented carbide, a ratio C2 / C1 of a total mass-based content C2 of titanium, tantalum, niobium, and zirconium at point P2 to a total mass-based content C1 of titanium, tantalum, niobium, and zirconium at point P4, which is 200 μm away from the surface in a normal direction to the surface, may be 1.1 or more and 1.5 or less.

[0012] This indicates that the total mass content of titanium, tantalum, niobium, and zirconium is higher in areas with high Vickers hardness than in areas with low Vickers hardness. Titanium, tantalum, niobium, and zirconium can improve the oxidation resistance of cemented carbide. In cemented carbide with a ratio C2 / C1 of 1.1 or more and 1.5 or less, the region showing Vickers hardness b is presumed to have excellent oxidation resistance.

[0013] (3) In the above (1) or (2), in the cemented carbide, a ratio C4 / C3 of the mass-based cobalt content C4 at point P1 to the mass-based cobalt content C3 at point P4, which is 200 μm away from the surface in the normal direction of the surface, may be 1.1 or more and 2.0 or less.

[0014] According to this, point P1, which is 5 μm away from the surface of the cemented carbide, has a higher cobalt content by mass than point P4, which is 200 μm away from the surface of the cemented carbide. A higher cobalt content tends to improve toughness. It is presumed that cemented carbide with a ratio C4 / C3 of 1.1 or more and 2.0 or less has excellent toughness on the surface side due to the high cobalt content on the surface side.

[0015] (4) In any one of the above (1) to (3), the cobalt content C5 of the cemented carbide may be 4% by mass or more and 11% by mass or less, thereby further improving the tool life.

[0016] (5) In any of the above (1) to (4), the difference b-c between the Vickers hardness b and the Vickers hardness c at a point P4 in the cemented carbide that is 200 μm away from the surface along the normal direction of the surface may be 0.3 GPa or more and 1.0 GPa or less.

[0017] According to this, Vickers hardness c is greater than Vickers hardness a and less than Vickers hardness b. A cutting tool including this cemented carbide has an excellent balance between wear resistance and chipping resistance, and can maintain stable cutting performance, even when wear progresses from the surface side of the cutting tool during cutting.

[0018] (6) In any of the above (1) to (5), in the cemented carbide, the difference c-a between the Vickers hardness c at a point P4, which is 200 μm away from the surface along the normal direction of the surface, and the Vickers hardness a may be 1.2 GPa or more.

[0019] As a result, even if wear progresses from the surface side of the cutting tool as cutting proceeds, the cutting tool can have an excellent balance between wear resistance and chipping resistance and can maintain stable cutting performance.

[0020] (7) A cutting tool according to the present disclosure is a cutting tool including the cemented carbide according to any one of (1) to (6) above. The cutting tool according to the present disclosure has excellent wear resistance and chipping resistance and can have a long tool life.

[0021] [Details of the Embodiments of the Present Disclosure] The cemented carbide and cutting tool of the present disclosure will be described below with reference to the drawings. In the drawings of the present disclosure, the same reference numerals represent the same or corresponding parts. Furthermore, dimensional relationships such as length, width, thickness, and depth have been appropriately changed for clarity and simplification of the drawings, and do not necessarily represent actual dimensional relationships.

[0022] In the present disclosure, the notation in the form of "A to B" means the upper and lower limits of a range (i.e., A or more and B or less), and when no unit is specified for A and a unit is specified only for B, the units of A and B are the same.

[0023] In the present disclosure, when a compound or the like is represented by a chemical formula, unless the atomic ratio is particularly limited, it is intended to include any conventionally known atomic ratio, and should not necessarily be limited to only those within the stoichiometric range.

[0024] In the present disclosure, when one or more numerical values ​​are recited as the lower limit and the upper limit of a numerical range, a combination of any one numerical value recited as the lower limit and any one numerical value recited as the upper limit is also considered to be disclosed. For example, when a1 or more, b1 or more, and c1 or more are recited as the lower limit and a2 or less, b2 or less, and c2 or less are recited as the upper limit, a1 or more and a2 or less, a1 or more and b2 or less, a1 or more and c2 or less, b1 or more and a2 or less, b1 or more and b2 or less, b1 or more and c2 or less, c1 or more and a2 or less, c1 or more and b2 or less, and c1 or more and c2 or less are considered to be disclosed.

[0025] [Embodiment 1: Cemented Carbide] A cemented carbide according to one embodiment of the present disclosure (hereinafter also referred to as "Embodiment 1") is a cemented carbide including a first phase, a second phase, and a third phase, wherein the first phase is composed of a plurality of tungsten carbide particles, the content of the first phase in the cemented carbide is 65% by volume or more and 85% by volume or less, the second phase is composed of cobalt, and the cobalt content C5 of the cemented carbide is 3% by mass or more and 15% by mass or less, the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen, and the third phase does not contain tungsten carbide, and the total content C of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more and 8% by mass or less, The cemented carbide has a Vickers hardness a of 12.5 GPa or more and 14.5 GPa or less, the Vickers hardness a is measured at a point P1 in the cemented carbide that is 5 μm away from the surface of the cemented carbide in a direction normal to the surface, the cemented carbide includes a first region sandwiched between an imaginary plane Q1 that is 5 μm away from the surface and an imaginary plane Q4 that is 200 μm away from the surface, the first region has a second region sandwiched between an imaginary plane Q2 that is 10 μm away from the surface and an imaginary plane Q3 that is 50 μm away from the surface, in the first region, a point P2 showing a Vickers hardness b that is the maximum value of the Vickers hardness is located in the second region, and the difference b-a between the Vickers hardness b and the Vickers hardness a is 1.8 GPa or more.

[0026] When used as a tool material, the cemented carbide of the present disclosure can provide a cutting tool that has excellent wear resistance and fracture resistance and can have a long tool life. The reason for this is not clear, but is presumed to be as follows.

[0027] (i) The cemented carbide of the present disclosure contains 65% by volume or more and 85% by volume or less of a first phase consisting of a plurality of tungsten carbide particles (hereinafter also referred to as "WC particles"). The tungsten carbide particles have high hardness and high thermal conductivity. Therefore, the cemented carbide of the present disclosure also has high hardness and high thermal conductivity, and cutting tools including the cemented carbide can have excellent wear resistance.

[0028] (ii) The cemented carbide of the present disclosure contains 3% by mass or more and 15% by mass or less of cobalt. Cobalt has high toughness. Therefore, the cemented carbide of the present disclosure also has high toughness, and cutting tools including the cemented carbide can have excellent chipping resistance.

[0029] (iii) The cemented carbide of the present disclosure includes a third phase consisting of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen. The third phase can improve the reactivity and oxidation resistance of the cemented carbide. Therefore, a cutting tool including the cemented carbide has improved reactivity and oxidation resistance, which in turn improves wear resistance.

[0030] (iv) The cemented carbide of the present disclosure has a Vickers hardness a of 12.5 GPa to 14.5 GPa at a point P1, which is 5 μm away from the surface. The surface side of the cemented carbide has a relatively low hardness and adequate toughness, so that a tool including the cemented carbide is prevented from chipping in the early stage of cutting.

[0031] (v) In the cemented carbide of the present disclosure, point P2 exhibiting the maximum Vickers hardness value b in the first region is located in the second region at a distance of 10 μm or more and 50 μm or less from the surface. Furthermore, the difference b - a between Vickers hardness b and Vickers hardness a is 1.8 GPa or more.

[0032] In this cemented carbide, a region exists in the second region, which is 10 μm or more and 50 μm or less from the surface, that exhibits a hardness that is 1.8 GPa or more higher than the hardness at point P1, which is further on the surface side than the second region. Even if the surface of the cemented carbide is worn away at the beginning of cutting, a cutting tool including this cemented carbide can have excellent wear resistance due to the region in the second region that is harder than the surface side.

[0033] <First Phase> <Composition of First Phase> In the cemented carbide of the first embodiment, the first phase is composed of a plurality of tungsten carbide particles. Here, the tungsten carbide particles include not only "pure WC particles (including WC containing no impurity elements and WC with impurity elements below the detection limit)" but also "WC particles containing impurities therein, as long as the effects of the present disclosure are not impaired." Examples of impurities include iron (Fe), molybdenum (Mo), and sulfur (S).

[0034] <First Phase Content of Cemented Carbide> In the cemented carbide of embodiment 1, the first phase content of the cemented carbide is 65 vol% or more and 85 vol% or less. From the viewpoint of improving hardness, the lower limit of the first phase content of the cemented carbide is 65 vol% or more, or may be 66 vol% or more, 70 vol% or more, 72 vol% or more, or 75 vol% or more. From the viewpoint of improving toughness, the upper limit of the first phase content of the cemented carbide is 85 vol% or less, or may be 84 vol% or less, 80 vol% or less, or may be 78 vol% or less. The first phase content of the cemented carbide may be 70 vol% or more and 84 vol% or less, or may be 72 vol% or more and 80 vol% or less.

[0035] In the present disclosure, the content of the first phase in a cemented carbide is measured by the following procedure: (A1) A surface or cross section of the cemented carbide is subjected to mirror finishing. Examples of mirror finishing methods include polishing with diamond paste, using a focused ion beam (FIB) device, using a cross-section polisher (CP) device, and a combination of these methods.

[0036] (B1) The processed surface of the cemented carbide is photographed using a scanning electron microscope ("S-3400N" manufactured by Hitachi High-Technologies Corporation) to obtain a backscattered electron image. Six backscattered electron images are prepared. Each of the six backscattered electron images has a different photographed area. The photographed location can be set arbitrarily. The observation conditions are a magnification of 5000x and an accelerating voltage of 10 kV.

[0037] (C1) The six backscattered electron images obtained in (B1) above are imported into a computer using image analysis software (ImageJ, version 1.51j8: https: / / imagej.nih.gov / ij / ), and binarized to obtain six binarized images. The binarization is performed under conditions preset in the image analysis software by clicking the "Make Binary" button on the computer screen after importing the images. In the binarized image, the first region consisting of the first phase and the second region consisting of the second and third phases can be distinguished by their shades of color. For example, in the binarized image, the first phase is shown as a black region, and the second and third phases are shown as white regions.

[0038] (D1) In each of the six binarized images, a rectangular measurement field of 25.3 μm in length and 17.6 μm in width is set. Using the image analysis software, the area percentage (area %) of the first phase is measured in each of the six measurement fields, with the entire measurement field being used as the denominator.

[0039] (E1) Calculating the average area percentage (area %) of the first phase obtained in the six measurement fields. In the present disclosure, the average area percentage (area %) of the first phase obtained in the six measurement fields is defined as the content (volume %) of the first phase in the cemented carbide.

[0040] As far as the applicant has measured, it has been confirmed that, as long as measurements are made on the same sample, even if the above measurement is performed multiple times by changing the selected location of the measurement field, there is little variation in the measurement results, and that setting the measurement field arbitrarily will not be arbitrary.

[0041] <Average particle size of tungsten carbide particles> In the cemented carbide alloy of embodiment 1, the average particle size of the tungsten carbide particles is not particularly limited and may be any conventionally known average particle size used in cemented carbides. The average particle size of the tungsten carbide particles may be, for example, 0.5 μm or more and 2.0 μm or less, or 0.7 μm or more and 1.7 μm or less.

[0042] In the present disclosure, the average particle size of tungsten carbide particles is measured by the following procedure: (A2) Six images after binarization are obtained by the same method as (A1) to (C1) described in the method for measuring the content of the first phase in cemented carbide.

[0043] (B2) A rectangular measurement field of view measuring 25.3 μm in height and 17.6 μm in width was set in each of the six binarized images obtained. Using image analysis software (ImageJ, version 1.51j8: https: / / imagej.nih.gov / ij / ), the circle-equivalent diameter (Heywood diameter: diameter equivalent to a circle with equal area) of each of the tungsten carbide particles (first phase) in the six measurement fields was measured.

[0044] (C2) Calculate the number-based arithmetic mean of the circle-equivalent diameters of all tungsten carbide particles in the six measurement fields, excluding those with a circle-equivalent diameter of 0.22 μm or less. In the present disclosure, this arithmetic mean corresponds to the average particle size of the WC particles. The reason for excluding tungsten carbide particles with a circle-equivalent diameter of 0.22 μm or less when calculating the average particle size is that the inventors have confirmed, through measurements, that particles with a circle-equivalent diameter of 0.22 μm or less often correspond to noise that is erroneously detected as tungsten carbide particles in image analysis.

[0045] As far as the applicant has measured, it has been confirmed that, as long as measurements are made on the same sample, even if the above measurement is performed multiple times by changing the selected location of the measurement field, there is little variation in the measurement results, and that setting the measurement field arbitrarily will not be arbitrary.

[0046] <Second Phase> <Composition of Second Phase> In the cemented carbide of embodiment 1, the second phase is made of cobalt. The second phase is a binder phase that bonds the tungsten carbide particles that make up the first phase together.

[0047] In the present disclosure, the phrase "the second phase is composed of cobalt (Co)" also includes the case where "the second phase contains impurities together with cobalt, as long as the effects of the present disclosure are not impaired." Examples of impurities include manganese (Mn), magnesium (Mg), calcium (Ca), molybdenum (Mo), sulfur (S), and aluminum (Al).

[0048] <Cobalt Content of Cemented Carbide> In the cemented carbide of embodiment 1, the cobalt content C5 of the cemented carbide is 3% by mass or more and 15% by mass or less. From the viewpoint of improving toughness, the lower limit of the cobalt content C5 of the cemented carbide is 3% by mass or more, or may be 4% by mass or more, 5% by mass or more, or 6% by mass or more. From the viewpoint of improving hardness, the upper limit of the cobalt content C5 of the cemented carbide is 15% by mass or less, or may be 11% by mass or less, or may be 9% by mass or less. The cobalt content of the cemented carbide may be 4% by mass or more and 11% by mass or less, or may be 5% by mass or more and 9% by mass or less.

[0049] In this disclosure, the cobalt content C5 of cemented carbide is measured by cobalt titration. The cobalt titration is performed in accordance with the Japan Machine Tool Manufacturers' Association standard (TAS0054:2017) or ISO3909:1976. Specifically, the procedure is as follows: A cemented carbide sample is pulverized and passed through a 49-mesh sieve. The sample is dissolved in nitric acid and hydrofluoric acid, and ammonium citrate and aqueous ammonia are added. Potentiometric titration is then performed with potassium ferricyanide (red ferricyanide) using platinum and saturated calomel (tungsten) electrodes. The measurement device used is an "AUT-501" manufactured by DKK-TOA Corporation.

[0050] <Third Phase> <Composition of Third Phase> In the cemented carbide of embodiment 1, the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen. The third phase does not contain tungsten carbide. The third phase can improve the reactivity resistance and oxidation resistance of the cemented carbide. Therefore, a cutting tool including the cemented carbide has improved reactivity resistance and oxidation resistance.

[0051] In the present disclosure, the phrase "the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen" also includes the case where "the third phase contains impurities as long as the effects of the present disclosure are not impaired." Examples of impurities include manganese (Mn), magnesium (Mg), calcium (Ca), molybdenum (Mo), sulfur (S), and aluminum (Al).

[0052] The third phase may contain at least two elements selected from the group consisting of titanium, tantalum, niobium, zirconium and tungsten.

[0053] The third phase may include at least one selected from the group consisting of titanium carbide (TiC), tantalum carbide (TaC), niobium carbide (NbC), titanium nitride (TiN), titanium carbonitride (TiCN), zirconium carbonitride (ZrCN), zirconium carbide (ZrC), and solid solutions derived from these compounds. Examples of the solid solutions include WTiCN, WTiTaCN, and WTiTaNbZrCN.

[0054] In the present disclosure, it is confirmed by the following procedure that the third phase comprises at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen, and that the third phase does not contain tungsten carbide.

[0055] (A3) An arbitrary position of the cemented carbide is thinned using an ion slicer (apparatus: IB09060CIS (trademark) manufactured by JEOL Ltd.) to prepare a sample with a thickness of 30 to 100 nm. The acceleration voltage of the ion slicer is 6 kV for thinning and 2 kV for finishing.

[0056] (B3) The sample is observed at 50,000x magnification using a scanning transmission electron microscope (STEM) (apparatus: JFM-ARM300F (trademark) manufactured by JEOL Ltd.) to obtain a STEM-HAADF (high-angle annular dark field scanning transmission electron microscope) image. The imaging area of ​​the STEM-HAADF image is set to the center of the sample, that is, a position that does not include areas with properties that are clearly different from the bulk portion, such as the surface vicinity of the cemented carbide (a position where the imaging area is entirely the bulk portion of the cemented carbide). The measurement condition is an acceleration voltage of 200 kV.

[0057] (C3) A spot analysis is performed on a third phase present in a STEM-HAADF image using EDX (STEM-EDX) attached to the STEM, and the elements constituting the third phase are quantified. The spot size is set for each third phase to a range that includes only the third phase. When the quantification of the constituent elements satisfies the following conditions (a) and (b), it is confirmed that the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen. (a) The third phase contains at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen. (b) No impurity elements other than titanium, tantalum, niobium, zirconium, tungsten, carbon, and nitrogen are confirmed in the third phase, or the content of these impurity elements is less than 0.1 mass%.

[0058] When spot analysis of the third phase by EDX (STEM-EDX) detects only tungsten and carbon, and the carbon content relative to the total mass of tungsten and carbon is approximately 6.1 mass%, the third phase is determined to contain tungsten carbide. In other words, when spot analysis of the third phase by EDX (STEM-EDX) detects elements other than tungsten and carbon, the third phase is determined to not contain tungsten carbide.

[0059] <<Total Content C of Titanium, Tantalum, Niobium, and Zirconium in the Cemented Carbide>> In the cemented carbide of embodiment 1, the total content C of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more and 8% by mass or less. From the viewpoint of improving reactivity resistance and oxidation resistance, the lower limit of the total content C of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more, or may be 3% by mass or more, or 4% by mass or more. From the viewpoint of improving the thermal conductivity of the cemented carbide, the upper limit of the total content C of titanium, tantalum, niobium, and zirconium in the cemented carbide is 8% by mass or less, or may be 7% by mass or less, or may be 6% by mass or less. The total content C of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more and 8% by mass or less, or may be 3% by mass or more and 7% by mass or less, or may be 4% by mass or more and 6% by mass or less. Here, the third phase may contain at least two elements selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten. In the present disclosure, the total content C of titanium, tantalum, niobium, and zirconium in the cemented carbide means the total content of all of these elements when the cemented carbide contains all of titanium, tantalum, niobium, and zirconium, and when the cemented carbide contains one or more and three or less elements selected from the group consisting of titanium, tantalum, niobium, and zirconium, it means the total content of the contained elements.

[0060] In the present disclosure, the total content C of titanium, tantalum, niobium and zirconium of the cemented carbide is measured by ICP atomic emission spectrometry.

[0061] <Vickers Hardness> The Vickers hardness of the cemented carbide of embodiment 1 will be described with reference to FIGS. 1 and 2. FIG. 1 is a schematic diagram showing a cross section of the cemented carbide of embodiment 1. FIG. 2 is a graph showing an example of the relationship between the distance from the surface of the cemented carbide of embodiment 1 and the Vickers hardness. In the graph of FIG. 2, the X-axis represents the distance from the surface of the cemented carbide (unit: μm), and the Y-axis on the left represents the Vickers hardness (unit: GPa). Here, "distance from the surface of the cemented carbide" is synonymous with the distance from the surface of the cemented carbide to the interior (unit: μm) along the normal direction of the surface of the cemented carbide. FIG. 2 also shows an example of the relationship between the distance from the surface of the cemented carbide of embodiment 1 and the respective contents (mass%) of titanium, tantalum, niobium, and cobalt. In this case, in the graph of FIG. 2, the X-axis represents the distance from the surface of the cemented carbide (unit: μm), and the Y-axis on the right represents the content (mass%) of each element.

[0062] The cemented carbide of embodiment 1 has a Vickers hardness a of 12.5 GPa or more and 14.5 GPa or less at point P1, which is 5 μm away from surface S1 along the normal direction of surface S1. In Fig. 1 , point P1 is located on imaginary plane Q1, which is 5 μm away from surface S1 toward the interior of the cemented carbide. The surface side of the cemented carbide has a relatively low hardness and moderate toughness, so that a tool including the cemented carbide is prevented from chipping in the early stage of cutting.

[0063] 1 , the cemented carbide of the first embodiment includes a first region A1 sandwiched between an imaginary plane Q1 that is 5 μm away from the surface S1 toward the interior of the cemented carbide and an imaginary plane Q4 that is 200 μm away from the surface S1 toward the interior of the cemented carbide. The first region A1 includes a second region A2 sandwiched between an imaginary plane Q2 that is 10 μm away from the surface S1 of the cemented carbide toward the interior of the cemented carbide and an imaginary plane Q3 that is 50 μm away from the surface S1 toward the interior of the cemented carbide.

[0064] In the first region A1, point P2 exhibiting the maximum Vickers hardness, Vickers hardness b, is present in the second region A2. In this cemented carbide, a region exists in the second region, which is 10 μm or more and 50 μm from the surface, exhibiting a hardness 1.8 GPa or more higher than the hardness of point P1, which is closer to the surface than the first region A1. Therefore, even if the surface of the cemented carbide is worn away at the beginning of cutting, a cutting tool including this cemented carbide can have excellent wear resistance due to the region in the second region that is harder than the surface.

[0065] If the position showing Vickers hardness b is within a region less than 10 μm away from the surface of the substrate, the region near the surface of the substrate that has a relatively low hardness and adequate toughness will become smaller, and the effect of suppressing chipping in the initial stage of cutting will tend to decrease.If the position showing Vickers hardness b is within a region more than 50 μm away from the surface of the substrate, the region with a relatively low hardness will become larger, and the wear resistance of the cutting tool will tend to decrease.

[0066] In the cemented carbide of embodiment 1, the lower limit of the Vickers hardness a is 12.5 GPa or more, 12.6 GPa or more, 12.9 GPa or more, or 13.0 GPa or more from the viewpoint of suppressing the occurrence of excessive wear. The upper limit of the Vickers hardness a is 14.5 GPa or less, 14.4 GPa or less, 14.2 GPa or less, 14.1 GPa or less, or 14.0 GPa or less from the viewpoint of improving fracture resistance. The Vickers hardness a may be 12.6 GPa or more and 14.4 GPa or less, 12.9 GPa or more and 14.2 GPa or less, or 13.0 GPa or more and 14.0 GPa or less.

[0067] In the cemented carbide of embodiment 1, the lower limit of the difference b-a between the Vickers hardness b and the Vickers hardness a is 1.8 GPa or more, or may be 2.0 GPa or more, 2.1 GPa or more, 2.3 GPa or more, or 2.6 GPa or more, from the viewpoint of increasing the hardness near the surface of the cemented carbide and improving the wear resistance of the cemented carbide. The upper limit of the difference b-a may be 3.5 GPa or less, 3.4 GPa or less, 3.3 GPa or less, 3.2 GPa or less, or 3.1 GPa or less. The difference b-a may be 1.8 GPa or more and 3.5 GPa or less, 2.0 GPa or more and 3.4 GPa or less, 2.1 GPa or more and 3.3 GPa or less, 2.3 GPa or more and 3.2 GPa or less, or 2.6 GPa or more and 3.1 GPa or less.

[0068] In the cemented carbide of embodiment 1, the lower limit of the Vickers hardness b may be 14.0 GPa or more, 14.3 GPa or more, more than 14.5 GPa, 14.6 GPa or more, or 14.8 GPa or more from the viewpoint of improving wear resistance. The upper limit of the Vickers hardness b may be 18.0 GPa or less, 17.9 GPa or less, or 17.8 GPa or less from the viewpoint of improving fracture resistance. The Vickers hardness b may be 14.0 GPa or more and 18.0 GPa or less, 14.3 GPa or more and 17.9 GPa or less, more than 14.5 GPa and 17.8 GPa or less, 14.6 GPa or more and 17.7 GPa or less, or 14.8 GPa or more and 17.6 GPa or less.

[0069] In the cemented carbide of embodiment 1, the difference b-c between the Vickers hardness b and the Vickers hardness c at point P4, where the distance from the surface of the cemented carbide to the interior of the cemented carbide along the normal direction of the surface is 200 μm, may be 0.3 GPa or more and 1.0 GPa or less.

[0070] In the cemented carbide of embodiment 1, the lower limit of the difference b-c between the Vickers hardness b and the Vickers hardness c may be 0.1 GPa or more, and from the viewpoint of the balance between wear resistance and fracture resistance inside the cemented carbide, it may be 0.3 GPa or more, 0.4 GPa or more, or 0.5 GPa or more. The upper limit of the difference b-c may be 1.5 GPa or less, and from the viewpoint of the balance between wear resistance and fracture resistance inside the cemented carbide, it may be 1.0 GPa or less, 0.9 GPa or less, or 0.8 GPa or less. The difference b-c may be 0.3 GPa or more and 1.0 GPa or less, 0.4 GPa or more and 0.9 GPa or less, or 0.5 GPa or more and 0.8 GPa or less.

[0071] In the cemented carbide of embodiment 1, the difference c-a between the Vickers hardness c and the Vickers hardness a at point P4, where the distance from the surface of the cemented carbide to the interior of the cemented carbide along the normal direction of the surface is 200 μm, may be 1.2 GPa or more. The lower limit of the difference c-a may be 0.6 GPa or more, and from the viewpoint of the balance between wear resistance and fracture resistance inside the cemented carbide, it may be 1.2 GPa or more, 1.5 GPa or more, 1.6 GPa or more, or 1.7 GPa or more. The upper limit of the difference c-a is not particularly limited, but may be, for example, 2.8 GPa or less. The difference c-a may be 1.2 GPa or more and 2.8 GPa or less, or 1.5 GPa or more and 2.6 GPa or less.

[0072] In the cemented carbide of embodiment 1, the lower limit of the Vickers hardness c may be 14.0 GPa or more, 14.2 GPa or more, more than 14.5 GPa, 14.6 GPa or more, or 14.8 GPa or more from the viewpoint of improving wear resistance. The upper limit of the Vickers hardness b may be 18.0 GPa or less, 17.9 GPa or less, or 17.8 GPa or less from the viewpoint of improving fracture resistance. The Vickers hardness b may be 14.0 GPa or more and 18.0 GPa or less, 14.3 GPa or more and 17.9 GPa or less, more than 14.5 GPa and 17.8 GPa or less, 14.6 GPa or more and 17.7 GPa or less, or 14.8 GPa or more and 17.6 GPa or less.

[0073] In the present disclosure, the Vickers hardness of cemented carbide is measured using a micro Vickers hardness tester (FM810 (trademark) manufactured by FutureTech Co., Ltd.) under the following measurement conditions: test load 500 g, load holding time 10 seconds, and measurement temperature 18°C ​​or higher and 28°C or lower.

[0074] In the present disclosure, the Vickers hardness of a cemented carbide is measured according to the following procedure. A cemented carbide is embedded in resin and polished with diamond paste to expose a cross section S2 at an angle θ of 5.7° with respect to the surface S1 of the cemented carbide, as shown in FIG. 3 . When an arbitrary point B1 is set on the cross section S2 of the measurement sample, the shortest distance L2 between the surface S1 of the cemented carbide and point B1 along the cross section S2 is 10 times the distance L1 between a virtual plane S11 on the same plane as the surface S1 and point B1 along the normal direction of the surface S1. Based on this relationship, the Vickers hardness of the cemented carbide can be measured on the cross section S2 to obtain the Vickers hardness at a predetermined distance from the surface S1 of the cemented carbide.

[0075] In measuring Vickers hardness, an indenter is pressed in a direction perpendicular to the cross section S2. The measurement position is set on an imaginary straight line that intersects with the surface S2 provided on the cross section S2. The following points (a) and (b) are set on the straight line, and Vickers hardness is measured at each point. (a) A point that is 5 μm away from the imaginary surface S11 along the normal direction to the surface S1. (b) A point that is 10 μm or more and 200 μm away from the imaginary surface S11 along the normal direction to the surface S1, and is located at 10 μm intervals along the normal direction. This includes points that are 10 μm away from the imaginary surface S11 and points that are 200 μm away from the imaginary surface S11.

[0076] The above measurement is performed on each of three different imaginary straight lines. In the present disclosure, the average of the measured values ​​of the Vickers hardness of the cemented carbide at three points at the same distance L from the imaginary surface S11 corresponds to the Vickers hardness at the point at the distance L from the surface S1 of the cemented carbide.

[0077] As far as the applicant has been able to measure, it has been confirmed that there is almost no variation in the measurement results even when the Vickers hardness is measured multiple times on the same sample at different measurement positions.

[0078] <Total Mass Content of Titanium, Tantalum, Niobium, and Zirconium> The total mass content of titanium (Ti), tantalum (Ta), niobium (Ni), and zirconium (Zr) in the cemented carbide of embodiment 1 will be described with reference to FIGS. 1 and 2. FIG. 2 is a graph showing an example of the relationship between the distance from the surface of the cemented carbide of embodiment 1 and the respective contents (mass%) of titanium, tantalum, niobium, and cobalt. FIG. 2 shows a case where the cemented carbide contains titanium, tantalum, and niobium, but does not contain zirconium, among titanium, tantalum, niobium, and zirconium. The cemented carbide of embodiment 1 can contain at least one element from titanium, tantalum, niobium, and zirconium.

[0079] In the cemented carbide of embodiment 1, the ratio C2 / C1 of the total mass content C2 of titanium, tantalum, niobium, and zirconium at point P2 exhibiting a Vickers hardness b to the total mass content C1 of titanium, tantalum, niobium, and zirconium at point P4, a distance of 200 μm from the surface of the cemented carbide toward the interior of the cemented carbide along the normal direction of the surface. This indicates that the total mass content of titanium, tantalum, niobium, and zirconium is higher at locations with higher Vickers hardness than at locations with lower Vickers hardness. Titanium, tantalum, niobium, and zirconium can improve the oxidation resistance of the cemented carbide. In a cemented carbide with a ratio C2 / C1 of 1.1 to 1.5, the region exhibiting a Vickers hardness b is presumed to have excellent oxidation resistance.

[0080] In the first embodiment, the lower limit of the ratio C2 / C1 may be 1.0 or more, and from the viewpoint of the balance between the wear resistance and the fracture resistance inside the cemented carbide, it may be 1.1 or more, or 1.2 or more. The upper limit of the ratio C2 / C1 may be 2.0 or less, and from the viewpoint of the balance between the wear resistance and the fracture resistance inside the cemented carbide, it may be 1.5 or less, or 1.4 or less. The ratio C2 / C1 may be 1.1 or more and 1.5 or less, or 1.2 or more and 1.4 or less.

[0081] For example, in the cemented carbide shown in Fig. 2, at point P4, the Ti content is 2.6 mass%, the Ta content is 3.3 mass%, and the Nb content is 0.7 mass%, and the total content C1 of Ti, Ta, and Nb is 6.6 mass%. In Fig. 2, at point P2, the Ti content is 2.8 mass%, the Ta content is 4.1 mass%, and the Nb content is 0.9 mass%, and the total content C2 of Ti, Ta, and Nb is 7.8 mass%. For the cemented carbide shown in Fig. 2, the C2 / C1 ratio is 1.2.

[0082] In embodiment 1, the lower limit of the total content C1 may be 2.0% by mass or more, 3.0% by mass or more, or 4.0% by mass or more. The upper limit of the total content C1 may be 8.0% by mass or less, 7.1% by mass or less, or 6.0% by mass or less. The total content C1 may be 2.0% by mass or more and 8.0% by mass or less, 3.0% by mass or more and 7.1% by mass or less, or 4.0% by mass or more and 6.0% by mass or less.

[0083] In embodiment 1, the lower limit of the total content C2 may be 2.0% by mass or more, 2.2% by mass or more, 2.4% by mass or more, 3.6% by mass or more, or 4.8% by mass or more. The upper limit of the total content C2 may be 16.0% by mass or less, 12.0% by mass or less, 11.0% by mass or less, or 10.0% by mass or less. The total content C2 may be 2.0% by mass or more and 16.0% by mass or less, 3.6% by mass or more and 12.0% by mass or less, or 4.8% by mass or more and 11.0% by mass or less.

[0084] In the present disclosure, the total mass content C1 of titanium, tantalum, niobium, and zirconium at point P4 and the total mass content C2 of titanium, tantalum, niobium, and zirconium at point P2 are measured on the same cross section S2 of the cemented carbide as that used to measure Vickers hardness using an energy dispersive X-ray spectrometer (SEM-EDX, Oxford Instruments' "EMAX-ACT") attached to a scanning electron microscope. The EDX measurement conditions are an observation magnification of 3000x and an acceleration voltage of 15 kV. The total content C1 and the total content C2 are measured on the same cross section of the cemented carbide as that used to measure Vickers hardness.

[0085] The procedure for measuring the total content C1 is as follows: In the cross section S2 of the cemented carbide, the total contents of titanium, tantalum, niobium, and zirconium are measured at three non-overlapping positions at a distance of 200 μm from the surface of the cemented carbide toward the interior of the cemented carbide along the normal direction of the surface, and the average of the total contents at the three positions is calculated. This average corresponds to the total content C1.

[0086] The procedure for measuring the total content C2 is as follows: The total content of titanium, tantalum, niobium, and zirconium is measured at one location within 200 μm of the outer edge of the indentation (indentation) made by the indenter at the point where the Vickers hardness b was measured on the cross section S2 of the cemented carbide. The measurement is performed at locations within 200 μm of the outer edge of each of three indentations, and the average of the total contents at the three locations is calculated. This average corresponds to the total content C2.

[0087] <Cobalt Content> The mass-based cobalt (Co) content in the cemented carbide of embodiment 1 will be described with reference to FIGS. 1 and 2. In the cemented carbide of embodiment 1, the ratio C4 / C3 of the mass-based cobalt content C4 at the surface S1 of the cemented carbide to the mass-based cobalt content C3 at a point P4, which is 200 μm from the surface S1 of the cemented carbide toward the interior of the cemented carbide along the normal direction of the surface S1, may be 1.1 or more and 2.0 or less. The mass-based cobalt content at the surface of the cemented carbide is higher than that at a point 200 μm away from the surface of the cemented carbide. A high cobalt content tends to improve toughness. It is presumed that a cemented carbide having a ratio C4 / C3 of 1.1 or more and 2.0 or less has excellent toughness at the surface due to the high cobalt content at the surface.

[0088] In the cemented carbide of embodiment 1, the lower limit of the ratio C4 / C3 may be 1.1 or more, 1.2 or more, or 1.3 or more, from the viewpoint of improving chipping resistance at the initial stage of cutting. The upper limit of the ratio C4 / C3 may be 2.0 or less, or 1.9 or less, from the viewpoint of balancing wear resistance and chipping resistance inside the cemented carbide. The ratio C4 / C3 may be 1.2 or more and 1.9 or less, or 1.3 or more and 1.8 or less.

[0089] For example, in the cemented carbide shown in FIG. 2, the Co content C3 at point P4 is 6.2 mass %, the Co content C4 at the surface is 9.4 mass %, and C4 / C3 is 1.5.

[0090] In the first embodiment, the lower limit of the cobalt content C3 may be 3% by mass or more, or 4% by mass or more. The upper limit of the cobalt content C3 may be 15% by mass or less, or 14% by mass or less. The cobalt content C3 may be 3% by mass or more and 15% by mass or less, or 4% by mass or more and 14% by mass or less.

[0091] In the first embodiment, the lower limit of the cobalt content C4 may be 3.9% by mass or more, 4% by mass or more, or 5% by mass or more. The upper limit of the cobalt content C4 may be 30% by mass or less, or 20% by mass or less. The cobalt content C4 may be 4% by mass or more and 30% by mass or less, or 5% by mass or more and 20% by mass or less.

[0092] <Zirconium Content> The cemented carbide of embodiment 1 may contain zirconium (Zr). Zirconium has the effect of improving the high-temperature hardness of the cemented carbide. In the cemented carbide, the percentage of the mass of zirconium relative to the mass of cobalt may be 0% or more and 6% or less. This improves the high-temperature hardness of the cemented carbide, thereby improving the tool life. In the cemented carbide, if the percentage of the mass of zirconium relative to the mass of cobalt exceeds 6%, the solid solubility limit of zirconium in cobalt is exceeded, and zirconium precipitates in the cemented carbide in the form of carbide, etc., which tends to deteriorate the chipping resistance of the cemented carbide.

[0093] In the cemented carbide, the upper limit of the percentage of the mass of zirconium relative to the mass of cobalt may be 6% or less, 5% or less, or 4% or less, from the viewpoint of a balance between fracture resistance and improved high-temperature hardness. In the cemented carbide, the lower limit of the percentage of the mass of zirconium relative to the mass of cobalt may be 1% or more, or 2% or more, from the viewpoint of improved high-temperature hardness. In the cemented carbide, the percentage of the mass of zirconium relative to the mass of cobalt may be 1% or more and 5% or less, or 2% or more and 4% or less.

[0094] The zirconium content of the cemented carbide is measured by ICP emission spectroscopy.

[0095] <Composition of Cemented Carbide> The cemented carbide of embodiment 1 includes a first phase, a second phase, and a third phase. The cemented carbide of embodiment 1 may also include the first phase, the second phase, and the third phase. The cemented carbide of embodiment 1 may include other phases in addition to the first, second, and third phases, as long as the effects of the present disclosure are not impaired. Examples of other phases include chromium carbides. The cemented carbide of embodiment 1 may include impurities in addition to the first, second, and third phases, as long as the effects of the present disclosure are not impaired. Examples of impurities include iron (Fe), molybdenum (Mo), sulfur (S), manganese (Mn), magnesium (Mg), calcium (Ca), and aluminum (Al). The impurity content of the cemented carbide (when two or more elements constitute the impurities, the total concentration of these elements) may be less than 0.1% by mass. The impurity content of the cemented carbide can be measured by ICP atomic emission spectroscopy.

[0096] <Method for manufacturing cemented carbide> The cemented carbide of embodiment 1 can be manufactured by, for example, carrying out a raw material powder preparation step, a mixing step, a molding step, a sintering step, and a cooling step in the above order. Each step will be described below.

[0097] <<Raw Material Powder Preparation Step>> In the raw material powder preparation step, raw material powders of all materials constituting the cemented carbide are prepared. As raw material powders, tungsten carbide powder as a raw material for the first phase, cobalt (Co) powder as a raw material for the second phase, titanium carbide (TiC) powder, titanium nitride (TiN) powder, tantalum carbide (TaC) powder, niobium carbide (NbN) powder, and zirconium carbide (ZrC) powder (hereinafter also referred to as "third phase raw material powder") are prepared. Chromium carbide (Cr) may be added as a grain growth inhibitor, if necessary. 3 C 2 ) powders can be prepared. These raw material powders can be commercially available.

[0098] The average particle size of the tungsten carbide powder (hereinafter also referred to as "WC powder") may be 1.5 μm or more and 6.0 μm or less. The average particle size of the cobalt powder may be 0.5 μm or more and 3.0 μm or less. The average particle size of the third phase raw material powder may be 0.5 μm or more and 4.0 μm or less. The average particle size of the chromium carbide powder may be 1.0 μm or more and 2.0 μm or less. In the present disclosure, the average particle size of these powders refers to the average particle size measured by the FSSS (Fisher Sub-Sieve Sizer) method. The average particle size is measured using a "Sub-Sieve Sizer Model 95" (trademark) manufactured by Fisher Scientific.

[0099] In the mixing step, the raw material powders prepared in the preparation step are mixed to obtain a mixed powder. The content of each raw material powder in the mixed powder is appropriately adjusted taking into consideration the content of each component of the first, second, and third phases of the cemented carbide.

[0100] The mixing method is not particularly limited, and conventionally known methods such as a ball mill or an attritor can be used. The mixing conditions are also not particularly limited, and conventionally known conditions can be used.

[0101] After the mixing step, the mixed powder may be granulated as necessary. Granulating the mixed powder makes it easier to fill the mixed powder into a die or mold during the molding step described below. A known granulation method can be applied to the granulation, and for example, a commercially available granulator such as a spray dryer can be used.

[0102] <<Forming Step>> The forming step is a step of forming the mixed powder obtained in the mixing step into a predetermined shape to obtain a molded body. The forming method and forming conditions in the forming step are not particularly limited, and general methods and conditions may be used. An example of the predetermined shape is a cutting tool shape.

[0103] <Sintering Process> In the sintering process, the compact obtained in the molding process is sintered to obtain a cemented carbide. First, when heating from the start of sintering to a temperature before the appearance of a liquid phase (e.g., 1300°C), heating is performed under conditions of a low vacuum in the sintering furnace (e.g., 2 kPaG to 10 kPaG by introducing argon). Under these conditions, the raw material powder is heated while suppressing denitrification from the raw material powder. Then, while maintaining the same pressure conditions, the temperature is heated to around 1450°C (1400°C to 1450°C). When the temperature reaches around 1450°C, the sintering furnace is evacuated (pressure 0.1 kPaG) in a short time (e.g., within 300 seconds). This operation rapidly denitrifies the powder in a short time, making it difficult for titanium, tantalum, niobium, and zirconium present on the surface side of the cemented carbide to migrate toward the interior of the cemented carbide, thereby forming a region with high concentrations of titanium, tantalum, niobium, and zirconium in the surface region of the cemented carbide. This state is maintained for 20 minutes to 40 minutes, and the compact is sintered to obtain a cemented carbide.

[0104] <<Cooling Step>> The cooling step is a step of cooling the cemented carbide after sintering is completed. The cooling rate to 1300°C is set to a gentle condition (for example, -2°C / min). This allows cobalt to easily migrate to the surface of the cemented carbide, and a region with a high cobalt concentration can be formed on the surface of the cemented carbide.

[0105] [Embodiment 2: Cutting Tool] The cutting tool of embodiment 2 includes the cemented carbide of embodiment 1. The cutting tool of embodiment 2 can include a cutting edge made of at least the cemented carbide of embodiment 1. In the present disclosure, the cutting edge refers to the portion involved in cutting, and in the cemented carbide, refers to the cutting edge ridge and the region of the cemented carbide that is within 0.5 mm of the cutting edge ridge toward the cemented carbide.

[0106] Examples of cutting tools include cutting tools, drills, end mills, indexable cutting tips for milling, indexable cutting tips for turning, metal saws, gear cutting tools, reamers, taps, and the like.

[0107] The cemented carbide of the second embodiment may constitute the entire tool or a part of the tool. Here, "constitute a part" refers to a mode in which the cemented carbide of the second embodiment is brazed to a predetermined position of any substrate to form a cutting edge.

[0108] The cutting tool of the second embodiment may further include a hard film that covers at least a part of the surface of the substrate made of cemented carbide. Examples of the hard film include diamond-like carbon, diamond, and Al. 2 O 3 Alternatively, a film made of TiCN can be used.The hard film may be a CVD film formed by chemical vapor deposition (CVD).

[0109] The present embodiment will be described in more detail with reference to examples, although the present embodiment is not limited to these examples.

[0110] <Production of cemented carbide> <Step of preparing raw material powders> Powders having the compositions shown in the "Raw Material" column of Table 1 were prepared as raw material powders. The tungsten carbide (WC) powder had an average particle size of 3.2 μm, the cobalt (Co) powder had an average particle size of 1.2 μm, and the chromium carbide (Cr 3 C 2 ) powder has an average particle size of 1.5 μm, titanium carbide (TiC) powder has an average particle size of 1.5 μm, titanium nitride (TiN) powder has an average particle size of 2.0 μm, tantalum carbide (TaC) powder has an average particle size of 1.0 μm, niobium carbide (NbC) powder has an average particle size of 1.1 μm, and zirconium carbide (ZrC) powder has an average particle size of 1.5 μm.

[0111] <Mixing Step> Each raw material powder was mixed in the blending amount shown in the "Content (mass%)" column of "Raw Material" in Table 1 to prepare a mixed powder. The "mass%" in the "Raw Material" column of Table 1 indicates the percentage of the mass of each raw material powder with respect to the total mass of the raw material powders. Mixing was carried out using an attritor. The mixing time was 8 hours. The obtained mixed powder was spray-dried to obtain a granulated powder.

[0112] <<Molding Step>> The obtained granulated powder was press-molded to prepare a chip-shaped compact.

[0113] <Sintering step> The compact was placed in a sintering furnace and heated to sinter. The pressure inside the sintering furnace when heating from the start of sintering to 1300°C was as shown in the "Pressure up to 1300°C" column under "Sintering" in Table 2. Thereafter, the temperature was increased to 1450°C while maintaining the same pressure conditions.

[0114] For the samples marked with "Yes" in the "Vacuuming" column of "Sintering" in Table 2, the sintering furnace was evacuated to a vacuum (pressure of 0.1 kPaG) within 300 seconds when the temperature reached 1450°C. This state was maintained for 20 to 40 minutes, and the compact was sintered to obtain a cemented carbide.

[0115] For the samples in which "None" is written in the "Vacuuming" column of "Sintering" in Table 2, the pressure inside the sintering furnace was set to 1 kPaG when the temperature reached 1,450°C, and this state was maintained for 20 minutes to 40 minutes, thereby sintering the compacted body and obtaining a cemented carbide.

[0116] <<Cooling Step>> After sintering was completed, the samples were slowly cooled in an argon (Ar) gas atmosphere to obtain cemented carbide. The cooling rate to 1300°C for each sample is shown in the "Cooling Rate" column of Table 2.

[0117]

[0118]

[0119] <Evaluation of Cemented Carbide> <Composition of Cemented Carbide> For each sample of cemented carbide, the first phase content of the cemented carbide, the cobalt content C5 of the cemented carbide, and the total content C of titanium, tantalum, niobium, and zirconium of the cemented carbide were measured. Here, the cobalt content C5 of the cemented carbide means the cobalt content in the entire cemented carbide, and the total content C of titanium, tantalum, niobium, and zirconium of the cemented carbide means the total content C of titanium, tantalum, niobium, and zirconium in the entire cemented carbide. Specific measurement methods are as described in embodiment 1. The results are shown in the "First Phase Content" and "C5 (Total)" columns of "Co Content" in Table 3 and the "C (Total)" column of "Total Content of Ti, Ta, Zr, and Nb" in Table 4. The term "Ti, Ta, Zr, and Nb Content" does not necessarily indicate that each sample contains all of Ti, Ta, Zr, and Nb.

[0120] <Average Particle Size of Tungsten Carbide Particles> It was confirmed that the average particle size of the tungsten carbide particles was 0.5 μm or more and 2.0 μm or less in all samples.

[0121] <<Composition of the Second Phase>> In all samples, the second phase was confirmed to consist of cobalt.

[0122] <<Composition of Third Phase>> In each sample, the elements contained in the third phase were identified by STEM-EDX. The specific identification method is as described in embodiment 1. The results are shown in the "Composition" column of "Third Phase" in Table 3. In all samples, it was confirmed that the third phase was composed of the elements listed in Table 3 and that the third phase did not contain tungsten carbide.

[0123] <Vickers Hardness> For each cemented carbide sample, the Vickers hardness was measured in a first region sandwiched between an imaginary plane Q1 at a distance of 5 μm from the surface of the cemented carbide and an imaginary plane Q4 at a distance of 200 μm from the surface. The specific measurement method is as described in embodiment 1. The Vickers hardness a at point P1, which is 5 μm from the surface, is shown in the "a (P1)" column of "Vickers hardness" under "Cemented Carbide" in Table 5. The Vickers hardness c at point P4, which is 200 μm from the surface of the cemented carbide along the normal direction of the surface to the interior of the cemented carbide, is shown in the "c (P4)" column of "Vickers hardness" under "Cemented Carbide" in Table 5.

[0124] In all samples, it was confirmed that point P2, which exhibits the maximum Vickers hardness value b, is located in a second region sandwiched between an imaginary plane Q2, which is 10 μm from the surface of the cemented carbide to the interior of the cemented carbide, and an imaginary plane Q3, which is 50 μm from the surface to the interior of the cemented carbide. The Vickers hardness b is shown in the "b (P2)" column of "Vickers hardness" under "Cemented Carbide" in Table 5. Based on the obtained "a," "b," and "c," "ba," "bc," and "ca" were calculated. The results are shown in Table 5.

[0125] <<Total Mass Content of Titanium, Tantalum, Niobium, and Zirconium>> For each cemented carbide sample, the total mass content C1 of titanium, tantalum, niobium, and zirconium at point P4, a distance of 200 μm from the surface of the cemented carbide to the interior of the cemented carbide along the normal direction of the surface, and the total mass content C2 of titanium, tantalum, niobium, and zirconium at point P2, which indicates Vickers hardness b, were measured. Specific measurement methods are as described in embodiment 1. The results are shown in the "C1 (P4)" and "C2 (P2)" columns of "Total Content of Ti, Ta, NiZr" in Table 3. Based on the obtained "C1" and "C2," "C2 / C1" was calculated. The results are shown in the "C2 / C1" column of Table 4.

[0126] <<Cobalt Content by Mass>> For each cemented carbide sample, the cobalt content by mass C3 at point P4, which was 200 μm from the surface of the cemented carbide toward the interior of the cemented carbide along the normal direction of the surface, and the total cobalt content by mass C4 at point P1, which was 5 μm from the surface of the cemented carbide along the normal direction of the surface, were measured. Specific measurement methods were as described in embodiment 1. The results are shown in the "C3 (P4)" and "C4 (P1)" columns of "Co content" in Table 3. "C4 / C3" was calculated based on the obtained "C3" and "C4". The results are shown in the "C4 / C3" column of Table 3.

[0127]

[0128]

[0129]

[0130] <Cutting Test 1> Turning was performed under the following conditions using a cutting tool (tool model number: CNMG120408N-GU (manufactured by Sumitomo Electric Hardmetal Corporation)) for each sample, and the average wear volume Vb (mm) on the flank side of the cutting tool after 15 minutes of cutting was measured. The smaller the average wear volume Vb (mm), the better the wear resistance and the longer the tool life. In Cutting Test 1, when the average wear volume Vb (mm) is 0.40 mm or less, it is judged that the wear resistance is excellent and the tool life is long. The results are shown in the "Cutting Test 1" column in Table 6.

[0131] <Cutting conditions> Workpiece: S45C Processing: External turning of round bar Cutting speed: 350 m / min Feed rate: 0.25 mm / rev Depth of cut: 2.0 mm Cutting fluid: Water-soluble cutting oil The above cutting conditions correspond to high-speed processing.

[0132] <Cutting Test 2> Twenty cutting tools (tool model number: CNMG120408N-GU (manufactured by Sumitomo Electric Hardmetal Corporation)) for each sample were prepared, and turning was performed using these under the following conditions, and the breakage rate (%) after 20 seconds of cutting was measured. A smaller breakage rate indicates better fracture resistance and a longer tool life. In Cutting Test 2, a breakage rate of 25% or less was considered to indicate a long tool life. The results are shown in the "Cutting Test 2" column in Table 6.

[0133] <Cutting conditions> Workpiece: SCM440 (grooved round bar) Processing: Intermittent turning of grooved round bar Cutting speed: 120 m / min Feed rate: 0.15 mm / rev Depth of cut: 2.0 mm Cutting fluid: None

[0134] In this example, if the average wear amount Vb is 0.40 mm or less in cutting test 1 and the breakage rate is 25% or less in cutting test 2, the tool life is determined to be long.

[0135]

[0136] <Discussion> The cemented carbide alloys and cutting tools of Samples 1 to 17 correspond to Examples. The cemented carbide alloys and cutting tools of Samples 101 to 113 correspond to Comparative Examples. Samples 1 to 17 had excellent wear resistance and fracture resistance, and exhibited long tool life in both Cutting Test 1 and Cutting Test 2. Samples 101, 104, and 107 had insufficient wear resistance and insufficient tool life in Cutting Test 1. Samples 102, 103, 105, 106, and 108 to 113 had insufficient fracture resistance and insufficient tool life in Cutting Test 2.

[0137] Although the embodiments and examples of the present disclosure have been described above, it is intended from the beginning that the configurations of the above-described embodiments and examples may be appropriately combined and modified in various ways. The embodiments and examples disclosed herein are illustrative in all respects and should not be considered limiting. The scope of the present invention is defined by the claims, not by the above-described embodiments and examples, and is intended to include meanings equivalent to the claims and all modifications within the scope of the claims.

[0138] A1: first region; A2: second region; S1: surface of cemented carbide; Q1, Q2, Q3, Q4: virtual surfaces.

Claims

1. A cemented carbide including a first phase, a second phase, and a third phase, wherein the first phase is composed of a plurality of tungsten carbide particles, the content of the first phase in the cemented carbide is 65% by volume or more and 85% by volume or less, the second phase is composed of cobalt, and the cobalt content C5 of the cemented carbide is 3% by mass or more and 15% by mass or less, the third phase is composed of at least one element selected from the group consisting of titanium, tantalum, niobium, zirconium, and tungsten, and at least one of carbon and nitrogen, the third phase does not contain tungsten carbide, the total content C of titanium, tantalum, niobium, and zirconium in the cemented carbide is 2% by mass or more and 8% by mass or less, and the Vickers hardness a of the cemented carbide is 12.5 GPa or more and 14.5 GPa or less, the Vickers hardness a is measured at a point P1 in the cemented carbide at a distance of 5 μm from the surface of the cemented carbide in a normal direction to the surface, the cemented carbide includes a first region sandwiched between an imaginary plane Q1 at a distance of 5 μm from the surface and an imaginary plane Q4 at a distance of 200 μm from the surface, the first region having a second region sandwiched between an imaginary plane Q2 at a distance of 10 μm from the surface and an imaginary plane Q3 at a distance of 50 μm from the surface, in the first region, a point P2 exhibiting a Vickers hardness b that is the maximum value of the Vickers hardness is present in the second region, and a difference b-a between the Vickers hardness b and the Vickers hardness a is 1.8 GPa or more.

2. The cemented carbide according to claim 1, wherein a ratio C2 / C1 of a total content C2 of titanium, tantalum, niobium and zirconium on a mass basis at point P2 to a total content C1 of titanium, tantalum, niobium and zirconium on a mass basis at point P4, which is 200 μm away from the surface in a normal direction to the surface, is 1.1 or more and 1.5 or less.

3. The cemented carbide according to claim 1 or claim 2, wherein a ratio C4 / C3 of the cobalt content C4 on a mass basis at point P1 to the cobalt content C3 on a mass basis at point P4, which is 200 μm away from the surface in a normal direction to the surface, is 1.1 or more and 2.0 or less.

4. The cemented carbide according to any one of claims 1 to 3, wherein the cobalt content C5 of the cemented carbide is greater than or equal to 4 mass% and less than or equal to 11 mass%.

5. The cemented carbide according to any one of claims 1 to 4, wherein a difference b-c between the Vickers hardness b and a Vickers hardness c at a point P4 in the cemented carbide that is 200 μm away from the surface in the normal direction to the surface is 0.3 GPa or more and 1.0 GPa or less.

6. The cemented carbide according to any one of claims 1 to 5, wherein the difference c-a between the Vickers hardness c at a point P4, which is 200 μm away from the surface in the normal direction to the surface, and the Vickers hardness a, is 1.2 GPa or more.

7. A cutting tool comprising the cemented carbide according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Super hard alloy and cutting tool

    JP2016020541A

  • Preparation of coated surface cutting tool made of sintered hard alloy

    JP1984006304A

  • Cutting tool made of abrasion resistant cermet excelling in chipping resistance

    JP1990131803A

  • Cemented carbide cutter

    JP2022136020A

  • Hard alloy and cutting tool

    WO2013002270A1