Structure and method for manufacturing structure

The use of metal nanoparticles in a conductive composition for electrode formation on base materials addresses the inefficiencies of conventional methods by achieving high contact ratios and porosity, resulting in economically and environmentally friendly, efficient electricity transmission at lower temperatures.

WO2024247536A1PCT designated stage expired Publication Date: 2024-12-05DAICEL CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015458
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-04-18
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Conventional conductive pastes with micro-sized metal particles for forming electrodes have poor electrical contact with base materials, leading to inefficient electricity transmission and high process temperatures, while methods like sputtering and plating are economically inefficient and environmentally detrimental.

Method used

A structure and method using a conductive composition with metal nanoparticles, preferably silver or copper, deposited on a base material, where the electrode is formed by firing the nanoparticles at a low temperature, achieving high contact ratios and porosity within specific ranges to ensure efficient electricity transmission and environmental resistance.

Benefits of technology

The method allows for economical and environmentally friendly electrode formation with high electrical efficiency, uniform contact, and reduced process temperature, avoiding the drawbacks of traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided is a structure that has excellent economical efficiency and environmental resistance and can uniformly and efficiently transmit electricity to a base material. Further provided is a method for manufacturing a structure that has excellent economical efficiency and environmental resistance and can be manufactured at a low process temperature. The structure comprises a base material and an electrode formed on the base material, the electrode having a porosity of 0.01-30%, and a contact ratio of the electrode to the base material being 70% or more. The method for manufacturing the structure provided with a base material and an electrode formed on the base material comprises: a step for attaching a conductive composition containing metal nanoparticles to the base material; and a step for forming the electrode by firing the metal nanoparticles.
Need to check novelty before this filing date? Find Prior Art

Description

Structure and method for manufacturing the structure

[0001] The present disclosure relates to a structure and a method for manufacturing the structure. More particularly, the present disclosure relates to a structure and a method for manufacturing the structure. This application claims priority from Japanese Patent Application No. 2023-086752, filed in Japan on May 26, 2023, the contents of which are incorporated herein by reference.

[0002] Transparent conductive films are used in electronic components that require transparency, such as smartphone displays, touch panels, electronic paper screens, solar cell electrodes, glass heaters, etc. Electrodes used in such transparent conductive films and piezoelectric materials are known to be formed using conductive pastes (see Patent Documents 1 to 4).

[0003] JP 2007-18226 A JP 2014-218385 A JP 2003-316517 A JP 2000-124516 A

[0004] Conventional conductive pastes for forming electrodes, such as those disclosed in Patent Documents 1 to 4, generally use compositions containing micro-sized metal particles. However, electrodes formed from conductive pastes containing micro-sized metal particles tend to have poor electrical contact with the substrate, making it difficult to uniformly and efficiently conduct electricity to the substrate, and therefore have poor performance as an electrode.

[0005] On the other hand, sputtering and plating can improve performance, but these methods have problems in terms of economic efficiency and environmental resistance, such as high costs and a large amount of waste, which has a negative impact on the environment.

[0006] Therefore, an object of the present disclosure is to provide a structure that is economical, has excellent environmental resistance, and is capable of uniformly and efficiently conducting electricity to a substrate.

[0007] Furthermore, when an electrode is formed using a conductive paste containing micro-sized metal particles, a high process temperature is required for sintering the metal particles.

[0008] Therefore, a further object of the present disclosure is to provide a method for manufacturing a structure that is economical, has excellent environmental resistance, and can be manufactured at a low process temperature.

[0009] The present disclosure provides a structure comprising a substrate and an electrode formed on the substrate, wherein the porosity of the electrode is 0.01 to 30%, and the contact rate of the electrode with respect to the substrate is 70% or more.

[0010] Preferably, the electrodes comprise silver and / or copper.

[0011] The thickness of the electrode is preferably 20 μm or less.

[0012] The ratio of the porosity (%) to the thickness (μm) of the electrode [porosity / thickness] is preferably 0.05 or more.

[0013] The content of the metal element in the electrode is preferably 60% by mass or more.

[0014] The content of glass frit in the electrode is preferably 1% by mass or less.

[0015] The substrate preferably comprises a transparent conductive material and / or a piezoelectric material.

[0016] The present disclosure also provides a method for manufacturing a structure including a substrate and an electrode formed on the substrate, the method comprising the steps of: depositing a conductive composition containing metal nanoparticles onto the substrate; and firing the metal nanoparticles to form the electrode.

[0017] The number average particle size of the metal nanoparticles is preferably 100 nm or less.

[0018] The ratio of the number average particle diameter (nm) of the metal nanoparticles to the thickness (μm) of the electrode [number average particle diameter / thickness] is preferably 4.5 or more.

[0019] Preferably, the metal nanoparticles comprise silver and / or copper.

[0020] The shear rate of the conductive composition is 10 s -1 The viscosity at 1000000 mPa·s is preferably 1,000,000 mPa·s or less.

[0021] The content of the metal component in the conductive composition is preferably 1 to 90 mass %.

[0022] The content of the glass frit in the conductive composition is preferably 1% by mass or less.

[0023] The substrate preferably comprises a transparent conductive material and / or a piezoelectric material.

[0024] The structure of the present disclosure can be manufactured by a method that is economical and environmentally resistant, and can uniformly and efficiently conduct electricity to a substrate. Furthermore, the method for manufacturing a structure of the present disclosure is economical, environmentally resistant, and allows the structure to be manufactured at a low process temperature.

[0025] [Structure] The structure of the present disclosure includes a substrate and an electrode formed on the substrate.

[0026] (Substrate) The substrate (substrate) is not particularly limited as long as it has a layer capable of receiving electricity from the electrode. However, from the viewpoint of exhibiting characteristic functions, it is preferable that the substrate contains at least one or more selected from the group consisting of conductive substrates (conductors) and dielectrics, and particularly preferably contains a material such as a transparent conductive material or a piezoelectric material that has low conductivity and is difficult to receive electricity by itself. The electrode is formed on these substrates. The substrate may be a single layer or a multilayer in which multiple layers are stacked. In the case of a multilayer, it may contain one or more non-conductive substrate layers, but it contains a layer capable of receiving electricity so as to be in contact with the electrode.

[0027] Examples of the conductive substrate include metal substrates such as metal foils and metal plates formed from metals (copper, iron, alloys thereof, etc.); carbon substrates such as carbon cloth, carbon paper, and graphite; composite substrates such as conductive particle-containing films, conductive fiber-containing films, metal mesh films, metal-plated films, and optical laminates having a transparent conductive layer; resin substrates such as conductive polymer films; metal wire-containing films; and metal film laminates (printed circuit boards, etc.) having a metal (silver, copper, etc.) film on a part or all of a non-conductive substrate, and combinations of these may also be used.

[0028] Examples of materials that can form the piezoelectric material include inorganic materials such as quartz crystal, zinc oxide, and lead zirconate titanate (PZT), and organic materials such as polylactic acid, and combinations of these materials are also possible.

[0029] Examples of materials for forming the non-conductive substrate include resins, glass, ceramics, wood, paper, etc. Examples of the resin include heat-resistant plastics such as polyimide resins, polycarbonate resins, isocyanate resins, melamine resins, and glass epoxy resins, as well as polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin resins such as polyethylene and polypropylene, acrylic resins, epoxy resins, phenolic resins, and polyamide resins, as well as resins with low heat resistance such as polychlorinated biphenyl (PCB), liquid crystal polymers (LCP), vinyl chloride, molded resins, and epoxy resins, and combinations thereof may also be used.

[0030] (Electrode) The electrode contains at least a metal. Examples of the metal include conductive metals, such as gold, silver, copper, nickel, aluminum, rhodium, cobalt, ruthenium, platinum, palladium, chromium, indium, lead, and tin. Among these, silver or copper is preferred as the metal. The electrode may contain only one type of metal, or two or more types of metals.

[0031] The electrode has a porosity of 0.01 to 30% when measured by taking out a portion of the electrode. In one embodiment, the porosity is preferably 0.02 to 28%, more preferably 0.03 to 25%.

[0032] The porosity can be calculated by taking out a part of the electrode, exposing the cross section, observing the electrode cross section using a scanning electron microscope, analyzing the obtained cross-sectional image, and calculating the metal occupancy rate using the following formula: porosity [%] = 100 - occupancy rate [%]

[0033] An electrode containing voids can be produced, for example, by using a conductive composition containing metal nanoparticles and a solvent, volatilizing (evaporating) the solvent, and sintering the remaining metal nanoparticles. In this case, the surfaces of the metal nanoparticles melt, causing the metal nanoparticles to fuse together to form an electrode, but the gaps between the metal nanoparticles are not completely filled, resulting in the presence of voids in the electrode. The porosity in the electrode can be adjusted by appropriately selecting the particle size of the metal nanoparticles, the type of metal, etc.

[0034] The content of the metal element in the electrode is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, relative to 100% by mass of the total amount of the electrode. When the content is 60% by mass or more, the electrode has excellent conductivity.

[0035] The electrode preferably contains substantially no glass frit. The content of the glass frit in the electrode is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, and particularly preferably 0.1% by mass or less, relative to 100% by mass of the total amount of the electrode. The lower the content of the glass frit in the electrode, the less adverse effects caused by the glass frit will be, and the better the performance of the electrode will be.

[0036] The glass frit may be any known or commonly used glass frit, such as Bi2O3.B2O3.SiO2-based glass, PbO.SiO2-based glass, or Bi2O3.BaO.B2O3-based glass.

[0037] The thickness of the electrode is preferably 20 μm or less (for example, 0.05 to 20 μm), more preferably 0.1 to 10 μm. When the thickness of the electrode is 20 μm or less, cracks are less likely to occur in the electrode. When the thickness is 0.05 μm or more, electrical contact resistance is likely to be low.

[0038] The ratio of the porosity (%) to the thickness (μm) of the electrode [porosity / thickness] is preferably 0.05 or more (e.g., 0.05 to 600). In one embodiment, the ratio is preferably 0.06 to 300, more preferably 0.07 to 5.5. When the ratio is 0.05 or more, the electrode has excellent crack resistance. When the ratio is 600 or less, the electrode has excellent conductivity and is more likely to conduct electricity to the substrate.

[0039] The above structure can be applied to, for example, electrical and electronic devices such as electromagnetic wave control materials, circuit boards, antennas, heat sinks, liquid crystal displays, organic EL displays, field emission displays (FEDs), signage, IC cards, IC tags, solar cells, LED elements, piezoelectric elements, artificial muscles, heaters, organic transistors, condensers (capacitors), inductors, electronic paper, flexible batteries, flexible sensors, membrane switches, touch panels, and electromagnetic wave shields.

[0040] In the structure, the contact rate of the electrode to the substrate is 70% or more, preferably 80% or more, more preferably 85% or more, even more preferably 90% or more, and particularly preferably 95% or more. A contact rate of 70% or more allows for uniform and efficient electrical conduction from the electrode to the substrate. The contact rate may be 100% or 99.9% or less.

[0041] [Method for manufacturing a structure] The method for manufacturing a structure according to the present disclosure is a method for manufacturing a structure including a substrate and an electrode formed on the substrate, and can manufacture the structure according to the present disclosure. The method includes at least a step of adhering a conductive composition containing metal nanoparticles onto the substrate (adhering step), and a step of firing the metal nanoparticles to form the electrode (firing step).

[0042] The conductive composition forms an electrode in the structure. The conductive composition can take various forms without any particular limitation. For example, a conductive composition called a metal ink can be prepared by dispersing metal nanoparticles in a suspension state in an appropriate solvent (dispersion medium, particularly an organic solvent). Alternatively, a conductive composition called a metal paste can be prepared by dispersing metal nanoparticles in a kneaded state in a solvent. Only one type of metal nanoparticle can be used, or two or more types (e.g., metal nanoparticles having different constituent metals or metal nanoparticles with different number-average particle diameters) can be used.

[0043] The conductive composition contains metal nanoparticles. The number-average particle size of the metal nanoparticles is preferably 100 nm or less, more preferably 60 nm or less, even more preferably 50 nm or less, and particularly preferably 40 nm or less. The number-average particle size is the size excluding the protective agent coating the surface (i.e., the size of the metal nanoparticles themselves). The number-average particle size is determined, for example, based on particle sizes determined by transmission electron microscope (TEM) observation. Only one type of metal nanoparticle may be used, or two or more types may be used. When two or more types of metal nanoparticles are contained, the average particle size refers to the average particle size of all the metal nanoparticles.

[0044] The ratio of the number-average particle size (nm) of the metal nanoparticles to the thickness (μm) of the electrode [number-average particle size / thickness] is preferably 4.5 or more, more preferably 5 or more, and even more preferably 10 or more. When the ratio is 4.5 or more, cracks are less likely to occur in the electrode during the firing process. The ratio is preferably 2000 or less, more preferably 1000 or less, even more preferably 200 or less, and particularly preferably 100 or less. The smaller the ratio, the more uniform and efficient electricity can be transmitted to the substrate.

[0045] Examples of metals constituting metal nanoparticles include conductive metals, such as gold, silver, copper, nickel, aluminum, rhodium, cobalt, ruthenium, platinum, palladium, chromium, indium, etc. Among these, silver particles (i.e., silver nanoparticles) or copper particles (i.e., copper nanoparticles) are preferred as the metal nanoparticles, since they can be fused to each other at a temperature of about 100°C and form connecting members for electronic components and the like that are conductive even on general-purpose plastic substrates with low heat resistance.

[0046] The shape of the metal nanoparticles is not particularly limited, and examples thereof include spherical (including spherical and elliptical), flake (scale-like), dendritic, and lumpy shapes. Of these, spherical shapes are preferred.

[0047] Furthermore, surface-modified metal particles having a configuration in which the surfaces of metal nanoparticles are coated with an organic protective agent are preferred. That is, the metal nanoparticles are preferably surface-modified metal nanoparticles. Surface-modified metal nanoparticles ensure spacing between metal nanoparticles, suppress aggregation, and have excellent dispersibility in solvents.

[0048] The organic protective agent is not particularly limited, and examples thereof include known or commonly used organic protective agents used as protective agents (stabilizers) for metal nanoparticles. Examples of the organic protective agent include organic protective agents having functional groups such as carboxyl groups, hydroxyl groups, carbonyl groups, amide groups, ether groups, amino groups, sulfo groups, sulfonyl groups, sulfinic acid groups, sulfenic acid groups, mercapto groups, phosphate groups, and phosphite groups. Among the functional groups, carboxyl groups, hydroxyl groups, amino groups, sulfo groups, and mercapto groups are preferred, and amino groups are more preferred. Only one type of organic protective agent may be used, or two or more types may be used.

[0049] The content of the metal component (particularly the metal nanoparticles) in the conductive composition is preferably 1 to 90 mass%, more preferably 5 to 80 mass%, and even more preferably 10 to 70 mass%, relative to 100 mass% of the total amount of the conductive composition.

[0050] The solvent may be any known or commonly used solvent for dispersing metal nanoparticles, and examples of such solvents include aliphatic hydrocarbons such as pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, tridecane, and tetradecane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; aromatic hydrocarbons such as toluene, xylene, and mesitylene; alcohols such as methanol, ethanol, propanol, n-butanol, n-pentanol, n-hexanol, n-heptanol, n-octanol, n-nonanol, n-decanol, and menthol; diethylene glycol dibutyl ether, diethylene glycol methyl-n-butyl ether, and diethylene glycol-n-butyl ether acetone. Examples of suitable solvents include water and organic solvents such as ethers, including glycol ethers such as ethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, dipropylene glycol methyl isopentyl ether, dipropylene glycol monobutyl ether, dipropylene glycol methyl n-propyl ether, dipropylene glycol methyl n-butyl ether, dipropylene glycol methyl cyclopentyl ether, triethylene glycol dimethyl ether, triethylene glycol methyl n-butyl ether, tripropylene glycol methyl n-propyl ether, tripropylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether. Examples of suitable solvents include terpene-based solvents such as terpineol and dihydroterpineol. The terpene-based solvents are preferably incorporated into metal pastes. The type and amount of the solvent can be determined appropriately depending on the concentration and viscosity of the desired conductive composition (metal ink, metal paste). One or more of the solvents may be used. Among these, alcohols, ethers, hydrocarbons, and terpene-based solvents are preferred.

[0051] The content of the solvent (particularly the organic solvent) in the conductive composition is preferably 0.5 to 99 mass %, more preferably 2 to 95 mass %, and even more preferably 5 to 90 mass %, relative to 100 mass % of the total amount of the conductive composition. When the content is within the above range, the dispersibility of the metal nanoparticles is superior.

[0052] The total content of the metal component and the solvent in the conductive composition is preferably 1.5% by mass or more, more preferably 50% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, relative to 100% by mass of the total amount of the conductive composition.

[0053] The conductive composition may contain other components in addition to the metal nanoparticles and the organic solvent. The conductive composition may contain a binder resin, for example, to adjust the viscosity of the conductive composition. Only one type of binder resin may be used, or two or more types may be used. Examples of the binder resin include known or commonly used binder resins that are incorporated into conductive compositions, such as vinyl chloride-vinyl acetate copolymers, polyvinyl butyral resins, polyester resins, acrylic resins, and cellulose resins (e.g., ethyl cellulose). The content of the binder resin in the conductive composition is, for example, 10% by mass or less. From the viewpoint of excellent electrode conductivity, the content is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.1% by mass or less, and particularly preferably 0.01% by mass or less.

[0054] Examples of the other components include conductive particles other than metal nanoparticles (e.g., metal nanowires, metal resinates, etc.), additives such as dispersants, surface energy adjusters, plasticizers, leveling agents, antifoaming agents, and adhesion promoters. Only one of the other components may be used, or two or more of them may be used.

[0055] The conductive composition preferably does not substantially contain metal particles having a particle diameter of 1 μm or more (e.g., metal microparticles having a particle diameter of 1 to 20 μm). The content of the metal particles having a particle diameter of 1 μm or more in the conductive composition is preferably less than 1, more preferably less than 0.5, even more preferably less than 0.1, and particularly preferably less than 0.01, per 100 total metal nanoparticles. The presence or absence of the metal particles having a particle diameter of 1 μm or more and the proportion thereof can be confirmed by the above-mentioned transmission electron microscope (TEM) observation.

[0056] The conductive composition is preferably substantially free of the glass frit, and the content of the glass frit in the conductive composition is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, and particularly preferably 0.1% by mass or less, relative to 100% by mass of the total amount of the conductive composition.

[0057] The shear rate of the conductive composition is 10 s -1 The viscosity at room temperature is preferably 1,000,000 mPa·s or less (for example, 1 to 1,000,000 mPa·s), more preferably 500,000 mPa·s or less (for example, 3 to 500,000 mPa·s), and even more preferably 150,000 mPa·s or less. The above viscosity is the viscosity at room temperature.

[0058] The method for applying the conductive composition in the application step is not particularly limited, and any known or commonly used application method can be used, such as spin coating, inkjet printing, screen printing, spray printing, dispense printing, relief printing (flexographic printing), dye-sublimation printing, offset printing, laser printer printing (toner printing), intaglio printing (gravure printing), contact printing, microcontact printing, ultra-precise deposition (UPD), electrohydrodynamic printing (EHD printing), laser-induced forward transfer (LIFT), aerosol jet printing, etc. Only one of the above application methods may be used, or two or more may be used in combination.

[0059] In the firing step, the metal composition constituting the metal film obtained through the deposition step is fired, and through the firing step, the solvent in the metal composition is volatilized (evaporated) and the metal nanoparticles are sintered together to form an electrode.

[0060] The baking method includes thermal baking (IH, etc.), light baking (UV irradiation, etc.), reduced pressure baking, etc. The baking methods may be used alone or in combination of two or more.

[0061] The temperature (baking temperature) during the baking can be, for example, 1500°C or less, preferably 900°C or less, more preferably 200°C or less, even more preferably room temperature (e.g., 25°C) to 150°C, and particularly preferably room temperature (e.g., 25°C) to 120°C. If the baking temperature is 200°C or less (particularly, 180°C or less), this can be suppressed even when the substrate is a material that is prone to thermal deformation, such as an organic substance. In particular, if it is desired to complete the baking of the metal by short-term baking, it is good to perform the baking at, for example, 60 to 200°C, preferably 70 to 180°C, more preferably 80 to 150°C, and even more preferably 90 to 120°C. The baking time can be appropriately determined taking into account the type of conductive composition, the amount of adhesion, the baking temperature, etc., and is, for example, within several hours (e.g., within 40 seconds to 33 hours), preferably within 1 hour, more preferably within 50 minutes, even more preferably 10 to 40 minutes, and particularly preferably 15 to 30 minutes.

[0062] In the method for manufacturing a structure of the present disclosure, the combination of the deposition step and the firing step may be performed only once, or may be repeated two or more times. By repeating the combination of the deposition step and the firing step two or more times, a thick film electrode can be formed. Furthermore, when the combination is repeated two or more times, only one type of conductive composition may be used (i.e., the same conductive composition may be used), or two or more types may be used.

[0063] In addition, in the method for manufacturing a structure of the present disclosure, the firing step may be performed after the deposition step is performed multiple times. For example, it is possible to use conductive compositions with different compositions suitable for each shape, such as thin lines, thick lines, and solid paint. In such cases, the deposition step can be performed by changing the printing method and type of ink according to the printing location and printing pattern, and multiple metal films can be fired at once in a single firing step to form an electrode. The conductive compositions used in the multiple deposition steps may be only one type (i.e., the same conductive composition) or two or more types (i.e., different conductive compositions).

[0064] The structure of the present disclosure can be manufactured economically and environmentally resistant without employing methods such as plating or sputtering because the porosity is within a specific range. Furthermore, the high contact rate of the electrodes with the substrate allows for uniform and efficient electrical conduction to the substrate. Furthermore, the manufacturing method of the structure of the present disclosure is economical and environmentally resistant, and the use of metal nanoparticles allows for the structure to be manufactured at a low process temperature. Furthermore, glass frit is often used with piezoelectric materials to improve bonding with electrodes, which can result in deterioration of various properties such as the electromechanical coupling constant. However, when the structure of the present disclosure is used with piezoelectric materials, the use of glass frit is not necessary, and these problems are expected to be resolved.

[0065] Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. Each configuration and combination thereof in each embodiment is an example, and addition, omission, substitution, and other modifications of configurations are possible as appropriate within the scope of the present disclosure. Furthermore, each invention according to this disclosure is not limited by the embodiments or the following examples, but is limited only by the scope of the claims.

[0066] Hereinafter, one embodiment of the present disclosure will be described in more detail based on examples.

[0067] The conductive ink compositions used in the examples and comparative examples are as follows: Ink 1: Silver nanoparticle ink, trade name "Picosil DNS351", manufactured by Daicel Corporation, number average particle diameter 50 nm Ink 2: Silver nanoparticle ink, trade name "Picosil DNS409", manufactured by Daicel Corporation, number average particle diameter 50 nm Ink 3: Silver particle ink, trade name "XA-3512 Dotite", manufactured by Fujikura Kasei Co., Ltd., number average particle diameter 1000 nm Ink 4: Silver nanoparticle ink, trade name "DNS-0169I", manufactured by Daicel Corporation, number average particle diameter 20 nm

[0068] The number-average particle diameter of the silver particles was measured by dropping the ink onto a copper mesh and observing it using a transmission electron microscope (trade name "JEM-1200EXII", manufactured by JEOL Ltd.) in a standard manner. 300 silver particles were randomly selected from the obtained image, and the particle diameters of each were measured. The average value of these measurements was calculated as the average primary particle diameter.

[0069] [Formation of an electrode on a transparent conductive film] Example 1 A silver nanowire-containing transparent conductive film (main substrate: PET, surface resistance: 30 Ω / □, light transmittance: >90%) was used as the substrate. Ink 1 was applied to a rectangular shape (5 mm x 20 mm) on the substrate cut into a rectangular shape (80 mm x 30 mm) by a dispense printing method, and the substrate was heated at 120°C for 30 minutes to bake the silver nanoparticles, forming an electrode and producing a structure. The electrode thickness was 10 μm. The electrode thickness was measured by SEM observation.

[0070] Examples 2 to 3, Comparative Examples 1 to 4 Structures were produced by forming electrodes on transparent conductive films in the same manner as in Example 1, except that the ink, electrode thickness, and firing conditions were changed as shown in Table 1 and the printing method was changed to screen printing. In Comparative Example 1, ink 2 and ink 3 were mixed and used so that the number average particle diameter was 500 μm.

[0071] [Formation of electrodes on piezoelectric material] Example 4 A PZT piezoelectric material (product name "3Z5*10R-S(C-6)" manufactured by Fuji Ceramics Co., Ltd.) was used as the substrate. Ink 4 was applied to the entire surface of a rectangular substrate (10 mm x 5 mm) by spray printing, and the substrate was heated at 120°C for 30 minutes to sinter the silver nanoparticles, forming an electrode to produce a structure. The electrode thickness was 1 μm. The electrode thickness was measured by SEM observation.

[0072] Example 5, Comparative Example 5 Electrodes were formed on piezoelectric materials to prepare structures in the same manner as in Example 4, except that the thickness of the electrodes and the firing conditions were changed as shown in Table 2.

[0073] [Preparation of Conductive Structure] Reference Example 1 First, copper foil (t = 35 μm) was bonded to an FR4 substrate (t = 1 mm), and three types of copper wiring were prepared by etching (length 100 mm, width 0.25 mm, 0.5 mm, 1 mm). Then, a resist was applied to each copper wiring, and the wiring was processed so that 1 mm of copper was exposed every 10 mm, thereby preparing a conductive substrate. The surface roughness Ra of the copper wiring was 0.22 μm. Ink 4 was applied to the conductive substrate by spray printing, and the substrate was heated at 200 ° C. for 30 minutes to sinter the silver nanoparticles, forming a conductive layer to prepare a structure. The thickness of the conductive layer was 0.4 μm. The thickness of the conductive layer was measured by SEM observation.

[0074] Reference Example 2 A conductive layer was formed on a substrate to produce a structure in the same manner as in Reference Example 1, except that the thicknesses of the ink and conductive layer were changed as shown in Table 3 and the printing method was changed to a dispense printing method.

[0075] Reference Example 3 A conductive layer was formed on a substrate to produce a structure in the same manner as in Reference Example 1, except that the ink and the thickness of the conductive layer were changed as shown in Table 3 and the printing method was changed to screen printing.

[0076] <Evaluation> The structures obtained in the Examples, Comparative Examples, and Reference Examples were evaluated as follows. The results are shown in Tables 1 to 3.

[0077] (1) Contact rate with the substrate The laminated portion of the substrate and electrode (conductive layer) in the structure was cut using a microtome in a direction perpendicular to the surface direction, and the cross section was processed by ion milling to expose the cross section. SEM observation was performed using a scanning electron microscope (product name "JSM-6700F", manufactured by JEOL Ltd.). For the electron microscope photographs subjected to cross-sectional observation, image processing software (product name "ImageJ", manufactured by Wayne Rasband) was used to binarize the contact portion between the substrate and the electrode (conductive layer), and the actual contact length (the length of the portion where the substrate and the sintered metal particles in the electrode (conductive layer) are in contact) and the total contact length (the length of the portion where the substrate and the electrode (conductive layer) are in contact) were read, and the value obtained by dividing the actual contact length by the total contact length was used to calculate the contact rate at the cut surface, which was then used as the contact rate.

[0078] (2) Porosity of the electrode (conductive layer) For the structure, the electrode (conductive layer) was cut using a microtome, processed by ion milling to expose the cross section, and the cross section was observed using a scanning electron microscope (product name "JSM-6700F", manufactured by JEOL Ltd.). The electron microscope photographs from which the cross section was observed were binarized using image processing software (product name "ImageJ", manufactured by Wayne Rasband) for the voids and solid portions on the cut surface, and the area of ​​the voids was divided by the total area to calculate the porosity. In addition, in Comparative Example 5, cracks occurred in the electrode, so the porosity of the crack-free region was measured. In addition, EDS analysis was performed using a scanning electron microscope for the solid portions of the examples, reference examples, and comparative examples, and elements were identified by element mapping. Since it was determined that the solid portions were composed almost entirely of metal, the porosity was calculated assuming that the solid portions were all metal components.

[0079] (3) Electrode Surface Resistance For the structures obtained in Examples 1 to 3 and Comparative Examples 1 to 4, the electrode surface resistance was measured by a four-terminal method using a resistance measuring device (product name “MCP-T610”, manufactured by Mitsubishi Chemical Corporation).

[0080] (4) Thermography Analysis The structures obtained in Examples 1 to 3 and Comparative Examples 1 to 4 were connected to a stabilized power supply (trade name "PSP-2010", manufactured by GOODWILL INSTRUMENT CO., LTD.) using alligator clips, and a current of 0.2 mA was applied to the electrodes. The central temperature A of the transparent conductive film and the minimum temperature B within a radius of 1 cm from the center were measured using a thermograph (trade name "FLIR C5", manufactured by FLIR Systems Japan Inc.) when the current was applied. Note that "Temperature Unevenness" in Table 1 was evaluated as follows: ⊚ when A-B was less than 3.5°C, ◯ when it was 3.5°C or more and less than 4.5°C, △ when it was 4.5°C or more and less than 5.0°C, and × when it was 5.0°C or more.

[0081] (5) Electrical Contact Resistance The electrical contact resistance of the structures produced in the reference examples was measured by the TLM method using a digital multimeter (product name "VOAC7602", manufactured by IWATSU Corporation).

[0082]

[0083]

[0084]

[0085] As shown in Table 1, the structures of Examples 1 to 3 were evaluated as having small temperature unevenness in the transparent conductive film and being able to uniformly and efficiently conduct electricity to the substrate. On the other hand, in Comparative Examples 1 to 4, in which the porosity of the electrode exceeded 30% and the contact rate with the substrate was less than 70%, the temperature unevenness in the transparent conductive film was large and it was evaluated as not being able to uniformly and efficiently conduct electricity to the substrate.

[0086] Comparing Example 1 in Table 1 with Reference Example 2 in Table 3, although the inks and substrates used are different, the number-average particle size of the silver nanoparticles, the thickness of the electrode (conductive layer), the contact rate with the substrate, and the porosity of the electrode (conductive layer) are similar. Furthermore, the electrical contact resistance (the electrical resistance that occurs when current flows through the contact surfaces of two objects) of Reference Example 2 is sufficiently low, and the temperature unevenness in Example 1 was small. Comparing Comparative Example 2 in Table 1 with Reference Example 3 in Table 3, although the substrates used are different, the number-average particle size of the silver nanoparticles, the thickness of the electrode (conductive layer), the contact rate with the substrate, and the porosity of the electrode (conductive layer) are similar. Furthermore, the electrical contact resistance of Reference Example 3 is sufficiently higher than that of Reference Examples 1 and 2, and the temperature unevenness in Comparative Example 2 was large. Therefore, comparing Example 1 with Reference Example 2 and Comparative Example 2 with Reference Example 3, it is clear that there is a correlation between electrical contact resistance and the uniformity and efficiency of conduction to the substrate, and that low electrical contact resistance can be evaluated as enabling uniform and efficient conduction of electricity to the substrate. It can also be determined that even when the ink and substrate used are different, the electrical contact resistance can be determined to be similar if the contact rate with the substrate and the porosity of the electrode (conductive layer) are similar. Furthermore, comparing Examples 4 and 5 in Table 2 with Reference Example 1 in Table 3, although different substrates were used, the number-average particle size of the silver nanoparticles, the thickness of the electrode (conductive layer), the contact rate with the substrate, and the porosity of the electrode (conductive layer) are similar, and the electrical contact resistance of Reference Example 1 is significantly lower than that of Reference Example 2. Therefore, it is presumed that the structures of Examples 4 and 5 can conduct electricity to the substrate uniformly and efficiently. Furthermore, as is clear from Reference Examples 1, 2, and 3, there is a correlation between contact resistance and contact rate in principle, and the higher the contact rate, the lower the contact resistance. Therefore, it can be determined that Example 5, which has a large contact ratio, has a small contact resistance, and can transmit electricity uniformly and efficiently to the substrate.

[0087] Furthermore, the structures of the examples do not employ sputtering or plating, and therefore are economical and environmentally resistant. Furthermore, because metal nanoparticles are used as the material for forming the electrodes, the electrodes can be formed at low process temperatures. In all examples, reference examples, and comparative examples, glass frit is not actively added, and therefore the glass frit content in the electrodes or conductive layers is 0.1 mass% or less, meaning that glass frit is essentially absent.

[0088] Variations of the invention according to the present disclosure are described below. [Appendix 1] A structure comprising a substrate and an electrode formed on the substrate, wherein the porosity of the electrode is 0.01 to 30%, and the contact rate of the electrode to the substrate is 70% or more. [Appendix 2] The structure according to Appendices 1, wherein the electrode contains silver and / or copper. [Appendix 3] The structure according to Appendices 1 or 2, wherein the thickness of the electrode is 20 μm or less. [Appendix 4] The structure according to any one of Appendices 1 to 3, wherein the ratio of the porosity (%) to the thickness (μm) of the electrode [porosity / thickness] is 0.05 or more. [Appendix 5] The structure according to any one of Appendices 1 to 4, wherein the content of metal elements in the electrode is 60% by mass or more. [Appendix 6] The structure according to any one of Appendices 1 to 5, wherein the content of glass frit in the electrode is 1% by mass or less. [Appendix 7] The structure according to any one of Appendices 1 to 6, wherein the substrate contains a transparent conductive material and / or a piezoelectric material. [Appendix 8] A method for producing a structure comprising a substrate and an electrode formed on the substrate, the method comprising the steps of: adhering a conductive composition containing metal nanoparticles onto the substrate; and firing the metal nanoparticles to form the electrode. [Appendix 9] A method for producing a structure according to Appendices 8, wherein the number-average particle size of the metal nanoparticles is 100 nm or less. [Appendix 10] A method for producing a structure according to Appendices 8 or 9, wherein the ratio of the number-average particle size (nm) of the metal nanoparticles to the thickness (μm) of the electrode [number-average particle size / thickness] is 4.5 or more. [Appendix 11] A method for producing a structure according to any one of Appendices 8 to 10, wherein the metal nanoparticles contain silver and / or copper. [Appendix 12] A method for producing a structure according to any one of Appendices 8 to 10, wherein the conductive composition is heated at a shear rate of 10 s -1[Appendix 13] A method for producing a structure according to any one of Appendices 8 to 12, wherein the conductive composition has a metal component content of 1 to 90 mass %. [Appendix 14] A method for producing a structure according to any one of Appendices 8 to 13, wherein the conductive composition has a glass frit content of 1 mass % or less. [Appendix 15] A method for producing a structure according to any one of Appendices 8 to 14, wherein the substrate contains a transparent conductive material and / or a piezoelectric material.

Claims

1. A structure comprising a substrate and an electrode formed on the substrate, the electrode having a porosity of 0.01 to 30%, and a contact rate of the electrode with respect to the substrate of 70% or more.

2. The structure of claim 1, wherein said electrodes comprise silver and / or copper.

3. The structure according to claim 1 or 2, wherein the thickness of said electrode is 20 μm or less.

4. The structure according to claim 1 or 2, wherein the ratio of the porosity (%) to the thickness (μm) of the electrode [porosity / thickness] is 0.05 or more.

5. The structure according to claim 1 or 2, wherein the content of the metal element in the electrode is 60 mass % or more.

6. The structure according to claim 1 or 2, wherein the glass frit content in the electrode is 1 mass % or less.

7. The structure according to claim 1 or 2, wherein the substrate comprises a transparent conductive material and / or a piezoelectric material.

8. A method for producing a structure comprising a substrate and an electrode formed on the substrate, the method comprising the steps of: depositing a conductive composition containing metal nanoparticles onto the substrate; and firing the metal nanoparticles to form the electrode.

9. The method for producing a structure according to claim 8, wherein the number average particle size of the metal nanoparticles is 100 nm or less.

10. A method for producing the structure described in claim 8 or 9, wherein the ratio [number average particle diameter / thickness] of the number average particle diameter (nm) of the metal nanoparticles to the thickness (μm) of the electrode is 4.5 or more.

11. The method for producing a structure according to claim 8 or 9, wherein the metal nanoparticles contain silver and / or copper.

12. The shear rate of the conductive composition is 10 s -1 10. The method for producing a structure according to claim 8, wherein the viscosity of the solution is 1,000,000 mPa·s or less.

13. The method for producing a structure according to claim 8 or 9, wherein the content of the metal component in the conductive composition is 1 to 90 mass %.

14. The method for producing a structure according to claim 8 or 9, wherein the content of glass frit in the conductive composition is 1 mass % or less.

15. The method for producing a structure according to claim 8 or 9, wherein the substrate contains a transparent conductive material and / or a piezoelectric material.

Citation Information

Patent Citations

  • Method for producing dense metallic copper film, liquid composition used for the same, dense metallic copper film obtained by the same, conductor wiring, heat conduction passage and assembly

    JP2011238737A

  • Liquid composition, metal film, conductive wiring line, and method for producing metal film

    WO2013145953A1

  • Conductive ink

    WO2019225271A1