Separation solution for aluminum foil laminates and method for separating and recovering aluminum foil laminates using same
The use of a formic acid and carboxylic acid ester-based separation solution effectively addresses the inefficiencies in recycling aluminum foil laminates by enabling the separation of PVC and aluminum foil, enhancing the recyclability of PVC-containing materials and outperforming conventional techniques in terms of time and efficiency.
Patent Information
- Application Number
- PCT/JP2024/017260
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-09
- Publication Date
- 2024-12-05
AI Technical Summary
Current methods for recycling aluminum foil laminates, particularly those with PVC, are inefficient due to the inability to separate PVC from aluminum foil at temperatures below 100°C and under normal pressure, and existing separation technologies are not applicable to all resin types, making commercial-scale recycling impractical.
A separation solution containing formic acid, carboxylic acid ester, and water in specific ratios, along with optional additives like ketones and phosphoric acid, is used to penetrate and separate the resin layer from aluminum foil, effectively addressing the challenge of recycling PVC and other difficult-to-separate laminates.
The solution enables efficient separation of PVC and aluminum foil in a shorter time than conventional methods, facilitating the recycling of aluminum foil laminates and improving the recyclability of PVC-containing materials.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Separation solution for aluminum foil laminate and method for separating and recovering aluminum foil laminate using the same
[0001] The present invention relates to a separating solution for an aluminum foil laminate for separating an aluminum foil laminate in which a resin is laminated on at least one side of an aluminum foil into an aluminum foil and a resin, and a method for separating and recovering an aluminum foil laminate using the same.
[0002] Aluminum foil laminated with a resin on at least one side has been widely used as a packaging material for food and pharmaceutical products, where barrier properties are required to protect the contents from external environments such as oxygen, water vapor, and ultraviolet rays.In addition, for industrial purposes, aluminum foil is used in electronic materials, etc., due to its electrical properties and ease of processing.
[0003] Many resin layers have been used for lamination, including biaxially oriented polypropylene (OPP), polyethylene terephthalate (PET), epoxy, nylon, and polyvinyl chloride (PVC), due to the various performance requirements, such as heat sealability, strength, and puncture resistance. Among these, PVC, in particular, has been widely used as an aluminum foil PVC laminate for pharmaceutical packaging and industrial materials due to its mechanical and chemical properties. However, PVC generates dioxins during incineration, and hydrochloric acid is generated during incineration, damaging incinerators, a problem that has been a long-standing issue.
[0004] In recent years, recyclability has been required for resin products, but the diverse combinations of resin layers have made it difficult to recycle laminates. In particular, laminates containing aluminum foil have not been recycled because it is difficult to separate the aluminum foil from the resin layer. Furthermore, in the case of laminates in which PVC is laminated on aluminum foil (hereinafter also referred to as "aluminum foil PVC laminates"), there has been no technology that can separate PVC from aluminum foil PVC laminates at atmospheric pressure below 100°C.
[0005] To address these issues, for example, JP-A-2020-515655 (Patent Document 1) discloses a method for separating a metal layer from a resin layer by using a separation fluid containing a mixture of water and a short-chain carboxylic acid, and phosphoric acid and an alkali metal hydroxide that reduce dissolution of the metal layer.
[0006] Special Publication No. 2020-515655
[0007] However, when the present inventors verified the separability of aluminum foil PVC laminates in which various resins were laminated using the separation technique described in Patent Document 1, it was found that the PVC could not be separated from the aluminum foil PVC laminate in the combination of PVC and aluminum foil.
[0008] That is, the separation technique described in Patent Document 1 is not applicable to all types of resins, but is a technique that selects the type of laminated resin, and therefore is not applicable to PVC, which is particularly in demand for recycling as described above, and also requires a processing time of one hour or more for resins other than PVC. Therefore, the separation technique described in Patent Document 1 has the problem that it is not sufficiently satisfactory for actually implementing (putting into practical use) recycling of aluminum foil laminates on a commercial scale.
[0009] Therefore, the present invention aims to provide a separation technique that can separate PVC from an aluminum foil PVC laminate and can separate aluminum foil from other aluminum foil laminates in a shorter time than conventional techniques. An object of the present invention is to provide a separation technique that can separate PVC from an aluminum foil PVC laminate and can separate aluminum foil from other aluminum foil laminates in a shorter time than conventional techniques.
[0010] In order to solve the above problems, the present inventors have conducted extensive research into methods for separating the resin layer and the aluminum foil of an aluminum foil laminate (hereinafter also simply referred to as "laminate"). As a result, they have found that the aluminum foil laminate can be easily separated into the aluminum foil and the resin by using a solution containing formic acid, a carboxylic acid ester, and water as main components and blending each component in a specific ratio, and have completed the present invention.
[0011] That is, according to the present invention, there is provided a separation solution for an aluminum foil laminate, which contains 1 wt% to 98 wt% of formic acid, 1 wt% to 98 wt% of a carboxylic acid ester consisting of a formic acid ester having 9 or less carbon atoms and / or an acetic acid ester having 9 or less carbon atoms, and 1 wt% to 90 wt% of water, and the sum of the contents of the formic acid and the carboxylic acid ester is 10 wt% to 99 wt%, and the sum of the contents of the formic acid, the carboxylic acid ester, and the water is 100 wt% or less.
[0012] Further, according to the present invention, as a method for separating a resin layer and an aluminum foil using the above-mentioned aluminum foil laminate separation solution, a step of crushing a laminate containing aluminum foil and a resin into sizes of 1 mm to 70 mm using a crusher, A step of impregnating the crushed material with the above-mentioned aluminum foil laminate separation solution, and a step of leaving or stirring for 1 minute to 72 hours under temperature conditions of 20 ° C. to 99 ° C. to peel and separate the aluminum foil and the resin are provided.
[0013] In the separation solution of the present invention, the carboxylic acid ester plays a role in penetrating into the resin layer in the laminate, and assists the separation of the resin layer by the formic acid, making it possible to easily separate even resin layers that are difficult to separate, such as PVC.
[0014] Furthermore, in order to suitably mix, for example, the carboxylic acid ester and formic acid in the separation solution, the separation solution of the present invention preferably further contains, as a solvent, 1 wt % to 89 wt % of one or more additives selected from the group consisting of ketones, ethers, alkylbenzenes, dioxolanes, and cycloalkanes, and the sum of the contents of the additives, formic acid, carboxylic acid ester, and water is preferably 100 wt % or less.
[0015] The separation solution of the present invention may further contain phosphoric acid and an alkali metal hydroxide for the purposes of adjusting the pH of the solution and adjusting the passivation of the aluminum foil in the laminate.
[0016] According to the separation solution for aluminum foil laminates and the method for separating and recovering aluminum foil laminates using the same of the present invention, the carboxylic acid ester plays a role in penetrating the resin layer in the laminate and assists in the separation of the resin layer by formic acid. By doing so, even resin layers that are difficult to separate, such as PVC, can be easily separated.
[0017] Hereinafter, a separation solution for an aluminum foil laminate according to one embodiment of the present invention and a method for separating and recovering an aluminum foil laminate using the same will be described in detail. Note that the present invention is not limited to the following examples, and various modifications are possible within the scope of the technical concept of the present invention.
[0018] <Aluminum foil laminate separation solution> The aluminum foil laminate separation solution of the present invention contains 1 wt% to 98 wt% of formic acid, 1 wt% to 98 wt% of a carboxylic acid ester consisting of a formic acid ester having 9 or less carbon atoms and / or an acetate ester having 9 or less carbon atoms, and 1 wt% to 90 wt% of water, wherein the sum of the contents of the formic acid and the carboxylic acid ester is 10 wt% to 99 wt%, and the sum of the contents of the formic acid, the carboxylic acid ester, and the water is 100 wt% or less. Hereinafter, each component of the aluminum foil laminate separation solution of the present invention will be described in detail.
[0019] <Formic Acid> Formic acid is a type of carboxylic acid, which is an organic acid. Unlike strong acids such as hydrochloric acid and nitric acid, carboxylic acids react violently with aluminum foil and are not lost during separation from the resin layer. On the other hand, formic acid exhibits the strongest acidity among monovalent aliphatic carboxylic acids, with an acidity constant K of 1.8×10 -4 For example, the acidity constant Ka of acetic acid is 1.8 x 10 -5 Since the Ka of formic acid is 10 times larger, it cuts the adhesion at the aluminum interface and the resin layer interface, further promoting separation of the aluminum foil and the resin layer.
[0020] However, unlike strong acids such as hydrochloric acid, formic acid does not ionize most monovalent aliphatic carboxylic acids. Therefore, in order to promote the separation of the aluminum laminate by formic acid, it is important, based on Le Chatelier's principle, to (a) increase the concentration on the formic acid side to shift the reaction equilibrium toward the side that causes the separation, (b) increase the amount of carboxylic acid that ionizes in the reaction field, and, as a physical action, (c) penetrate the resin to facilitate the infiltration of formic acid into the interface where the laminate is bonded.
[0021] The separation solution of the present invention must contain 1 wt% to 98 wt% formic acid, and the sum of the content of formic acid and the content of the carboxylic acid ester described below must be 10 wt% to 99 wt%. If the formic acid content is less than 1 wt%, the separation effect will not work sufficiently due to Le Chatelier's principle. On the other hand, if only formic acid is used, i.e., if the formic acid content is 100 wt% and no carboxylic acid ester is included, the physical penetration into the resin layer will be insufficient as described above, and the resin layer will not be sufficiently separated.
[0022] Therefore, the content of formic acid in the separation solution is not particularly limited as long as the sum of the contents of formic acid and carboxylic acid ester is 10 wt % or more and 99 wt % or less, but is preferably 9 wt % or more and 98 wt % or less, more preferably 15 wt % or more and 80 wt % or less, and even more preferably 35 wt % or more and 55 wt % or less.
[0023] The sum of the contents of formic acid and carboxylic acid ester in the separation solution is preferably 10 wt% to 99 wt%, more preferably 30 wt% to 99 wt%, and even more preferably 40 wt% to 85 wt%. If the sum of the contents of formic acid and carboxylic acid ester exceeds 99 wt%, the remaining water will be less than 1 wt%, making it difficult to obtain the hydrolysis effect described below. On the other hand, if the sum of the contents of formic acid and carboxylic acid ester is less than 10 wt%, the laminate separation effect due to formic acid and carboxylic acid ester cannot be obtained.
[0024] The separation solution of the present invention contains formic acid in an amount of 1 wt% to 98 wt% and the sum of the contents of formic acid and carboxylic acid ester is 10 wt% to 99 wt%. It may further contain acids other than formic acid to the extent that they do not affect the aluminum foil. For example, mixing formic acid with acetic acid or 10 wt% or less dilute sulfuric acid further promotes the separation effect of the laminate by formic acid. Examples of such acids other than formic acid include carboxylic acids such as acetic acid, propionic acid, citric acid, and oxalic acid, and 10 wt% or less dilute sulfuric acid. As long as the separation solution contains formic acid in an amount of 1 wt% to 98 wt% and the sum of the contents of formic acid and carboxylic acid ester is 10 wt% to 99 wt%, the content of carboxylic acids other than formic acid in the separation solution is not particularly limited, but is preferably 69 wt% or less, and more preferably 22.5 wt% or less.
[0025] <Carboxylic Acid Ester> In the present invention, the carboxylic acid ester is not limited as long as it is a formic acid ester having 9 or less carbon atoms and / or an acetic acid ester having 9 or less carbon atoms, and is, for example, one or more selected from the group consisting of methyl formate, ethyl formate, propyl formate, butyl formate, pentyl formate, hexyl formate, heptyl formate, octyl formate, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, pentyl acetate, hexyl acetate, and heptyl acetate. The carboxylic acid ester penetrates a resin layer of PVC, OPP, or the like, swelling the resin layer and promoting separation from the aluminum foil.
[0026] The separation solution preferably contains 1 wt% to 98 wt% of carboxylic acid ester, and the sum of the content of carboxylic acid ester and formic acid is preferably 10 wt% to 99 wt%. If the separation solution does not contain carboxylic acid ester, formic acid will not sufficiently penetrate the resin layer, and the resin layer of PVC, OPP, etc. will not be sufficiently separated. On the other hand, if the separation solution of the present invention contains at least 1 wt% of formic acid, and the content of carboxylic acid ester is greater than 98 wt%, the remaining water content excluding formic acid will be less than 1 wt% at most, making it difficult to obtain the effect of water (due to hydrolysis) described below.
[0027] Furthermore, the content of the carboxylic acid ester in the separation solution is more preferably 5 wt % to 65 wt %, and even more preferably 20 wt % to 65 wt %, in addition to the above range. This is because an aqueous solution containing a carboxylic acid such as formic acid or acetic acid is miscible with esters that are normally immiscible in water up to a maximum of 9 carbon atoms, but when the carbon number exceeds 9, the aqueous solution becomes less miscible, and when the water and the carboxylic acid ester separate, it becomes difficult for the ester to function as a separation solution for the laminate.
[0028] <Water> In the present invention, the separation solution contains 1 wt % to 90 wt % water. However, the sum of the contents of formic acid, carboxylic acid ester, and water is 100 wt % or less. When water is present in the separation solution, a small portion of the carboxylic acid ester is hydrolyzed in the separation solution under the acidic conditions of formic acid to form formic acid and acetic acid, allowing the separation action of the laminate to be maintained for a long period of time. However, since the hydrolysis of ordinary carboxylic acid esters requires an acid catalyst such as a strong acid such as nitric acid or hydrochloric acid, the hydrolysis does not proceed sufficiently with water alone.
[0029] Therefore, in the separation solution of the present invention, although the equilibrium shifts toward the ionization of formic acid due to hydrolysis of the carboxylic acid ester in the presence of water, promoting the separation action of the laminate, the carboxylic acid ester is hardly lost in the reaction. Therefore, in the present invention, a separation solution in which formic acid, carboxylic acid ester, and water are present in appropriate amounts is preferred, and more specifically, the water content is more preferably 5 wt % to 50 wt %, and even more preferably 5 wt % to 35 wt %, in addition to the above range.
[0030] <Remainder> The separation solution of the present invention may contain, as the remainder in addition to the above-mentioned components, one or more additives (solvents) selected from the group consisting of ketones, ethers, alkylbenzenes, dioxolanes, and cycloalkanes. In particular, since the separation solution of the present invention contains water, the separation solution may separate into two layers depending on the ratio of carboxylic acid ester to formic acid. Therefore, the above-mentioned solvents may be added as needed to favorably mix the separation solution. Furthermore, although ketones, ethers, aromatic hydrocarbons, and heterocyclic compounds do not have the same effect as carboxylic acid esters, they still have the effect of penetrating into the resin layer, so it is more preferable to add the above-mentioned solvents to the remainder.
[0031] Examples of ketones that can be used in the present invention include acetone, methyl ethyl ketone, diethyl ketone, methyl propyl ketone, methyl isobutyl ketone, methyl amyl ketone, cyclohexanone, isophorone, acetophenone, and benzophenone. Of these, methyl ethyl ketone is often used as a true solvent for resin coating agents and is preferred from the viewpoint of solubility.
[0032] Examples of the ether include dimethyl ether, ethyl methyl ether, diethyl ether, diphenyl ether, ethylene oxide, tetrahydrofuran (THF), furan, 1,4-dioxane, anisole, benzofuran, dibenzofuran, and crown ether. Taking into consideration miscibility with water, tetrahydrofuran (THF), furan, and 1,4-dioxane are preferred.
[0033] As the alkylbenzene, xylene or toluene can be added as appropriate. Dioxolane is preferred because it has good miscibility with water and penetrates well into the resin layer. As the cycloalkane, cyclohexane, cycloheptane, cyclooctane, etc. can be used.
[0034] When the separation solution of the present invention contains an additive such as a ketone, an ether, an alkylbenzene, a dioxolane, or a cycloalkane as described above, the content of the additive is preferably 1 wt % or more and 89 wt % or less, and more preferably 16.7 wt % or more and 50 wt % or less.
[0035] <Other Additives> The separation solution of the present invention may contain additives such as buffer solutions to the extent that the effect of separating the laminate is not impaired. For example, a buffer solution composed of phosphoric acid and an alkali metal hydroxide has the effect of stabilizing the pH of the separation solution, but adding an excessive amount of additives may slow down the reaction that promotes the separation of the laminate. Therefore, in the present invention, the amount of additive added is preferably 3 wt % or less.
[0036] Separation solutions according to examples of the present invention and separation solutions according to comparative examples were prepared and evaluated, and will be described in detail below.
[0037] 1. Preparation of Separation Solutions in Examples and Comparative Examples [Example 1] To a 100 mL glass bottle were added 45 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 20 g of butyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 25 g of purified water (ASSWS-20, AS ONE Corporation), and 10 g of methyl ethyl ketone (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), and the mixture was stirred at room temperature for 10 minutes to prepare the separation solution of Example 1.
[0038] Example 2 To a 100 mL glass bottle were added 22.5 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 22.5 g of acetic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 20 g of butyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), and 35 g of purified water (ASSWS-20, AS ONE Corporation), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 2.
[0039] Example 3 To a 100 mL glass bottle were added 80 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 5 g of butyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 5 g of purified water (AS ONE Corporation, ASSWS-20), and 10 g of methyl ethyl ketone (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 3.
[0040] Example 4 To a 100 mL glass bottle were added 65 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 20 g of butyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 5 g of purified water (ASSWS-20, AS ONE Corporation), and 10 g of methyl ethyl ketone (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 4.
[0041] Example 5 To a 100 mL glass bottle were added 45 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 40 g of butyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 5 g of purified water (AS ONE Corporation, ASSWS-20), and 10 g of methyl ethyl ketone (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 5.
[0042] Example 6 To a 100 mL glass bottle were added 20 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 65 g of butyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 5 g of purified water (ASSWS-20, AS ONE Corporation), and 10 g of methyl ethyl ketone (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 6.
[0043] Example 7 To a 100 mL glass bottle were added 20 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 20 g of butyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 10 g of purified water (ASSWS-20, AS ONE Corporation), and 50 g of methyl ethyl ketone (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 7.
[0044] Example 8 To a 100 mL glass bottle were added 45 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent), 5 g of butyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent), and 50 g of purified water (AS ONE Corporation, ASSWS-20), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 8.
[0045] Example 9 To a 100 mL glass bottle were added 15 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 15 g of butyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 1 g of purified water (ASSWS-20, AS ONE Corporation), and 69 g of methyl ethyl ketone (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 9.
[0046] Example 10 To a 100 mL glass bottle were added 29 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 1 g of hexyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 1 g of purified water (AS ONE Corporation, ASSWS-20), and 69 g of methyl ethyl ketone (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 10.
[0047] Example 11 A 100 mL glass bottle was charged with 98 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent), 1 g of hexyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent), and 1 g of purified water (AS ONE Corporation, ASSWS-20), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution for Example 11.
[0048] Example 12 To a 100 mL glass bottle were added 15 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent), 84 g of butyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent), and 1 g of purified water (AS ONE Corporation, ASSWS-20), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution for Example 12.
[0049] Example 13 To a 100 mL glass bottle were added 15 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent), 15 g of ethyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent), and 70 g of purified water (AS ONE Corporation, ASSWS-20), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution for Example 13.
[0050] Example 14 To a 100 mL glass bottle were added 45 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 20 g of methyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 25 g of purified water (ASSWS-20, AS ONE Corporation), and 10 g of methyl ethyl ketone (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 14.
[0051] Example 15: 33 g of sodium hydroxide (Fujifilm Wako Pure Chemical Industries, Ltd., granular, special reagent grade) and 77 g of purified water (AS ONE Corporation, ASSWS-20) were placed in a 100 mL PE container and stirred at room temperature for 30 minutes to prepare a 33 wt% aqueous sodium hydroxide solution. Subsequently, 30 g of phosphoric acid (Fujifilm Wako Pure Chemical Industries, Ltd., Wako Grade 1) and 70 g of purified water (AS ONE Corporation, ASSWS-20) were placed in another 100 mL PE container and stirred at room temperature for 30 minutes to prepare a 30 wt% aqueous phosphoric acid solution. Next, 2.5 g of 30 wt% aqueous phosphoric acid solution (0.8 g solids) was added dropwise to 5.3 g of the 33 wt% aqueous sodium hydroxide solution (1.7 g solids) in a 100 mL glass bottle while stirring at room temperature, and the mixture was further stirred for 30 minutes to prepare 7.8 g of a phosphoric acid-sodium hydroxide buffer solution. Furthermore, 38 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 17 g of butyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 20.5 g of purified water (ASSWS-20, AS ONE Corporation) (a total of 25.8 g of purified water including the purified water content of the buffer solution), and 16.7 g of methyl ethyl ketone (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade) were added to the glass bottle containing the buffer solution, and the mixture was stirred at room temperature for 30 minutes to prepare a separation solution of Example 15.
[0052] Example 16 To a 100 mL glass bottle were added 9 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 1 g of octyl formate (Inoue Fragrance Manufacturing Co., Ltd., octyl formate), 1 g of purified water (AS ONE Corporation, ASSWS-20), and 89 g of methyl ethyl ketone (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 16.
[0053] Example 17 To a 100 mL glass bottle were added 1 g of formic acid (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), 9 g of isoamyl formate (Tokyo Chemical Industry Co., Ltd., purity 95% or higher), 1 g of purified water (AS ONE Corporation, ASSWS-20), and 89 g of methyl ethyl ketone (Fujifilm Wako Pure Chemical Industries, Ltd., special reagent grade), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 17.
[0054] Example 18 To a 100 mL glass bottle were added 98 g of formic acid (special grade reagent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 1 g of methyl formate (purity of 95% or higher, manufactured by Tokyo Chemical Industry Co., Ltd.), and 1 g of purified water (AS ONE Corporation, ASSWS-20), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution of Example 18.
[0055] Example 19 To a 100 mL glass bottle were added 1 g of formic acid (special grade reagent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 98 g of isoamyl formate (purity of 95% or higher, manufactured by Tokyo Chemical Industry Co., Ltd.), and 1 g of purified water (AS ONE Corporation, ASSWS-20), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution for Example 19.
[0056] Example 20 5 g of formic acid (special grade reagent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 5 g of isoamyl formate (purity of 95% or higher, manufactured by Tokyo Chemical Industry Co., Ltd.), and 90 g of purified water (AS ONE Corporation, ASSWS-20) were added to a 100 mL glass bottle and stirred at room temperature for 10 minutes to prepare the separation solution of Example 19.
[0057] Comparative Example 1: 33 g of sodium hydroxide (Fujifilm Wako Pure Chemical Industries, Ltd., granular, special reagent grade) and 77 g of purified water (AS ONE Corporation, ASSWS-20) were placed in a 100 mL PE container and stirred at room temperature for 30 minutes to prepare a 33 wt% aqueous sodium hydroxide solution. Subsequently, 30 g of phosphoric acid (Fujifilm Wako Pure Chemical Industries, Ltd., Wako Grade 1) and 70 g of purified water (AS ONE Corporation, ASSWS-20) were placed in another 100 mL PE container and stirred at room temperature for 30 minutes to prepare a 30 wt% aqueous phosphoric acid solution. Next, 3.0 g of 30 wt% aqueous phosphoric acid solution (0.9 g solids) was added dropwise to 6.3 g of the 33 wt% aqueous sodium hydroxide solution (2.1 g solids) in a 100 mL glass bottle while stirring at room temperature, and the mixture was further stirred for 30 minutes to prepare 9.3 g of a phosphoric acid-sodium hydroxide buffer solution. Furthermore, 45 g of formic acid (special grade reagent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 45.7 g of purified water (ASSWS-20, manufactured by AS ONE Corporation) (52 g in total of purified water including the purified water content of the buffer solution) were added to the glass bottle containing the buffer solution, and the mixture was stirred at room temperature for 30 minutes to prepare a separation solution of composition 2 described in Patent Document 1, which is the current technology, as a separation solution of Comparative Example 1.
[0058] Comparative Example 2: 33 g of sodium hydroxide (Fujifilm Wako Pure Chemical Industries, Ltd., granular, special reagent grade) and 77 g of purified water (AS ONE Corporation, ASSWS-20) were placed in a 100 mL PE container and stirred at room temperature for 30 minutes to prepare a 33 wt% aqueous sodium hydroxide solution. Subsequently, 30 g of phosphoric acid (Fujifilm Wako Pure Chemical Industries, Ltd., Wako Grade 1) and 70 g of purified water (AS ONE Corporation, ASSWS-20) were placed in another 100 mL PE container and stirred at room temperature for 30 minutes to prepare a 30 wt% aqueous phosphoric acid solution. Next, 3.0 g of 30 wt% aqueous phosphoric acid solution (0.9 g solids) was added dropwise to 6.3 g of the 33 wt% aqueous sodium hydroxide solution (2.1 g solids) in a 100 mL glass bottle while stirring at room temperature, and the mixture was further stirred for 30 minutes to prepare 9.3 g of a phosphoric acid-sodium hydroxide buffer solution. Furthermore, 45 g of glacial acetic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 99.7%+%) and 45.7 g of purified water (manufactured by AS ONE Corporation, ASSWS-20) (52 g in total of purified water including the purified water content of the buffer solution) were added to the glass bottle containing the buffer solution, and the mixture was stirred at room temperature for 30 minutes to prepare a separation solution of Composition 1 described in Patent Document 1, which is the current technology, as a separation solution of Comparative Example 2.
[0059] Comparative Example 3 A separation solution for Comparative Example 3 was prepared by adding 100 g of formic acid (special grade reagent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) to a 100 mL glass bottle.
[0060] Comparative Example 4 A 100 mL glass bottle was charged with 90 g of formic acid (special grade reagent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 10 g of purified water (AS ONE Corporation, ASSWS-20), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution for Comparative Example 4.
[0061] Comparative Example 5 A 100 mL glass bottle was charged with 8 g of formic acid (special grade reagent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 1 g of octyl formate (octyl formate, manufactured by Inoue Fragrance Manufacturing Co., Ltd.), and 91 g of purified water (AS ONE Corporation, ASSWS-20), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution for Comparative Example 5.
[0062] Comparative Example 6 To a 100 mL glass bottle were added 1 g of formic acid (special grade reagent, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 8 g of octyl formate (octyl formate, manufactured by Inoue Fragrance Manufacturing Co., Ltd.), and 91 g of purified water (AS ONE Corporation, ASSWS-20), and the mixture was stirred at room temperature for 10 minutes to prepare a separation solution for Comparative Example 6.
[0063] 2. Evaluation of Separation Solutions in Examples and Comparative Examples <Evaluation Test 1> (1) Preparation of Test Specimen 1 (PVC Configuration) For the aluminum foil, 45 μm 8021 material (manufactured by Toyo Aluminum Co., Ltd.) was used. Subsequently, a urethane adhesive was used as the adhesive, and a base agent (manufactured by Toyo Ink Co., Ltd.: base agent TMK-55, solid content 30% by mass) and a curing agent (CAT56-3K, solid content 70% by mass) were prepared. 100 parts by weight, 10 parts by weight, and 40 parts by weight of the base agent, curing agent, and ethyl acetate were mixed until the color was uniform, and a 25% by mass urethane resin solution was prepared. The coating liquid was mixed just before coating, and the weight after drying with a bar coater #16 in a mixed state was 5.0 g / m 2 The adhesive was applied to the glossy side of the aluminum foil so that the adhesive was applied, and dried at 100 ° C. for 40 seconds. Next, a 60 μm thick hard vinyl chloride film (Sumitomo Bakelite Co., Ltd.: VSS-6702) was attached using a small laminator at a nip temperature of 90 ° C. and a speed of 5 m / min. Furthermore, a urethane adhesive was applied to the matte side of the aluminum foil in the same manner as the glossy side, and then dried. A 60 μm thick hard vinyl chloride film (Sumitomo Bakelite Co., Ltd.: VSS-6702) was attached, and aged at 40 ° C. for 4 days to prepare a test specimen 1 (laminate) for evaluating the separation solution of the examples and comparative examples.
[0064] (2) Evaluation test of separation solution 100 g of the separation solution prepared in each example and each comparative example was placed in a 100 mL glass bottle (mouth inner diameter x body diameter x height: φ31.9 x φ48.5 x 87 mm). Next, one rotor (As One Corporation, tapered shape, length 25 mm, diameter 8 mm, material PTFE) was placed inside, and the lid was covered with aluminum foil to prevent the separation solution from volatilizing. Furthermore, the glass bottle containing the separation solution was placed in a 6-channel heating and stirring dry bath (As One Corporation: HDBS-6) and heated while stirring at 200 rpm until the temperature reached 60 ° C. After confirming with a thermometer that the separation solution had reached 60 ° C, test specimen 1 was cut into 2 mm x 10 mm, the lid was removed, and test specimen 1 was submerged in each separation solution and the lid was replaced. The samples were evaluated as follows: those in which the PVC peeled off in the separation solution within 1 hour were rated "A", those in which the PVC peeled off in the separation solution within 5 hours were rated "B", those in which the PVC peeled off in the separation solution within 24 hours were rated "C", and those in which the PVC did not peel off in the separation solution even after 24 hours were rated "F".
[0065] <Evaluation Test 2> (1) Preparation of Test Specimen 2 (OPP Configuration) For the aluminum foil, 20 μm 1N30 material (manufactured by Toyo Aluminum Co., Ltd.) was used. Subsequently, a urethane adhesive was used as the adhesive, and a base agent (manufactured by Rock Paint Co., Ltd.: base agent RU-77, solid content 60% by mass) and a curing agent (H-5, solid content 75% by mass) were prepared. 150 parts by weight of the base agent, 15 parts by weight, and 80 parts by weight of ethyl acetate were mixed until the color was uniform, and a 41% by mass urethane resin solution was prepared. The coating liquid was mixed just before coating, and the weight after drying with a bar coater #12 in a mixed state was 3.0 g / m 2 The solution was applied to the glossy side of aluminum foil so that the thickness was 100°C, and then dried for 40 seconds at 100°C. Next, a 20 μm thick OPP (P2102 manufactured by Toyobo Co., Ltd.) was attached using a small laminator at a nip temperature of 60°C and a speed of 5 m / min. After that, the solution was aged at 40°C for 2 days to prepare test specimen 2 (laminate) for evaluating the separation solution of the examples and comparative examples.
[0066] (2) Evaluation test of separation solution 100 g of the separation solution prepared in each example and each comparative example was placed in a 100 mL glass bottle (mouth inner diameter x body diameter x height: φ31.9 x φ48.5 x 87 mm). Next, one rotor (As One Corporation, tapered shape, length 25 mm, diameter 8 mm, material PTFE) was placed inside, and the lid was covered with aluminum foil to prevent the separation solution from volatilizing. Furthermore, the glass bottle containing the separation solution was placed in a 6-channel heating and stirring dry bath (As One Corporation: HDBS-6) and heated while stirring at 200 rpm until the temperature reached 60 ° C. After confirming with a thermometer that the separation solution had reached 60 ° C, test specimen 2 was cut into 10 mm x 10 mm, the lid was removed, and test specimen 2 was submerged in each separation solution and the lid was replaced. The OPP that peeled off in the separation solution within 30 minutes was rated as "A", the OPP that peeled off in the separation solution within 45 minutes was rated as "B", the OPP that peeled off in the separation solution within 60 minutes was rated as "C", and the OPP that did not peel off in the separation solution even after 60 minutes was rated as "F".
[0067] <Evaluation Test 3> <Evaluation Test of Separation Solution> A commercially available PVC PTP sheet (Mevalotin Tablet 5, manufactured by Daiichi Sankyo Co., Ltd.) was used as test specimen 3. 100 g of the separation solution prepared in each example and each comparative example was placed in a 100 mL glass bottle (mouth inner diameter x body diameter x height: φ31.9 x φ48.5 x 87 mm). Next, one rotor (As One Corporation, tapered shape, length 25 mm, diameter 8 mm, material PTFE) was placed in the bottle and the lid was closed with aluminum foil to prevent the separation solution from volatilizing. Furthermore, the glass bottle containing the separation solution was placed in a 6-channel heating and stirring dry bath (As One Corporation: HDBS-6) and heated to 95 ° C. while stirring at 200 rpm. After confirming with a thermometer that the separation solution had reached 95 ° C., test specimen 3 was cut into 10 mm x 10 mm pieces, the lid was removed, and test specimen 3 was submerged in each separation solution and the lid was replaced. The samples were rated as follows: those in which the PVC peeled off in the separation solution within 15 minutes were rated "A"; those in which the PVC peeled off in the separation solution within 30 minutes were rated "B"; those in which the PVC peeled off in the separation solution within 60 minutes were rated "C"; and those in which the PVC did not peel off in the separation solution even after 60 minutes were rated "F".
[0068] <Evaluation Test 4> <Evaluation Test of Separation Solution> A commercially available NYCPP component (manufactured by Dai Nippon Printing Co., Ltd., Al laminate film D-EL40H (3) 200 mm x 100 m, 25 μm nylon film / adhesive / 40 μm corrosion-resistant aluminum / 60 μm polypropylene coating) was used as test specimen 4. 100 g of the separation solution prepared in each example and each comparative example was placed in a 100 mL glass bottle (mouth inner diameter x body diameter x height: φ31.9 x φ48.5 x 87 mm). Next, one rotor (As One Corporation, shape tapered, length 25 mm, diameter 8 mm, material PTFE) was placed inside, and the lid was covered with aluminum foil to prevent the separation solution from volatilizing. Furthermore, the glass bottle containing the separation solution was placed in a 6-channel heating and stirring dry bath (As One Corporation: HDBS-6) and heated to 95 ° C while stirring at 200 rpm. After confirming with a thermometer that the separation solution had reached 95°C, test specimen 4 was cut into a 10 mm x 10 mm piece, the lid was removed, test specimen 4 was submerged in each separation solution, and the lid was replaced. The evaluation was carried out by assigning "A" to specimens in which the CPP peeled off in the separation solution within 15 minutes, "B" to specimens in which the CPP peeled off in the separation solution within 30 minutes, "C" to specimens in which the CPP peeled off in the separation solution within 60 minutes, and "F" to specimens in which the CPP did not peel off in the separation solution even after 60 minutes.
[0069] Table 1 shows the compositions of the separation solutions of Examples 1 to 20 and Comparative Examples 1 to 6, and the evaluation results of Evaluation Tests 1 to 4 using the separation solutions of the Examples and Comparative Examples.
[0070] <Discussion> Comparing the separation solutions of Examples 1 to 20 shown in Table 1 with the separation solutions of Comparative Examples 1 to 6, the separation solutions of Examples 1 to 20 contain formic acid at 1 wt% or more and 98 wt% or less, a carboxylic acid ester having 9 or less carbon atoms at 1 wt% or more and 98 wt% or less, and water at 1 wt% or more and 90 wt% or less, and the sum of the contents of the formic acid and the carboxylic acid ester is 10 wt% or more and 99 wt% or less, and the sum of the contents of the formic acid, the carboxylic acid ester, and the water is 100 wt% or less. As a result, it was found that excellent separation effect of the aluminum foil laminate was exhibited in Evaluation Tests 1 to 4.
[0071] As a result, the separation solution for aluminum foil laminates of the present invention can separate PVC and aluminum foil as shown in Table 1, and it has been found that the aluminum foil can be separated from other aluminum foil laminates in a shorter time than with conventional techniques.
Claims
1. A separation solution for aluminum foil laminates, comprising 1 wt% or more and 98 wt% or less of formic acid, 1 wt% or more and 98 wt% or less of a carboxylate ester consisting of a formic acid ester having 9 or less carbon atoms and / or an acetate ester having 9 or less carbon atoms, and 1 wt% or more and 90 wt% or less of water, wherein the sum of the contents of the formic acid and the carboxylate ester is 10 wt% or more and 99 wt% or less, and the sum of the contents of the formic acid, the carboxylate ester and the water is 100 wt% or less.
2. The separation solution for aluminum foil laminates according to claim 1, further comprising 1 wt% or more and 89 wt% or less of one or more additives selected from the group consisting of ketones, ethers, alkylbenzenes, dioxolanes and cycloalkanes, and the sum of the contents of the additives, the formic acid, the carboxylic acid ester and water is 100 wt% or less.
3. The separating solution for aluminum foil laminates according to claim 1, further comprising phosphoric acid and an alkali metal hydroxide.
4. A method for separating and recovering an aluminum foil laminate, comprising the steps of: crushing a laminate containing aluminum foil and resin into pieces having a size of 1 mm or more and 70 mm or less using a crusher; immersing the crushed pieces in a separating solution for aluminum foil laminates described in any one of claims 1 to 3; and leaving or stirring the solution at a temperature of 20°C to 99°C for 1 minute to 72 hours to peel off and separate the aluminum foil and the resin.
Citation Information
Patent Citations
Treatment of shredder dust and device
JP1999057651A
Method for recovering amphoteric metal and method for producing regenerated amphoteric metal
JP2020040302A
Method and apparatus for recycling packaging materials
JP2020515655A
Separation fluid, method and apparatus for recycling multilayer materials using passivation agents - Patents.com